Molded Articles Containing Zeolite Materials Having Framework-Type MFI
Patent Information
- Application Number
- JP2021519721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-09
- Filing Date
- 2019-10-09
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-10-09
AI Technical Summary
Existing catalysts for propylene epoxidation, such as titanium silicalite-1, suffer from irregular cavities and poor selectivity and catalyst life, leading to inefficient production of propylene oxide and high by-product formation.
A molded article comprising a zeolite material with skeletal MFI structure, composed of Ti, Si, and H, and a silica binder, is prepared through specific post-treatments including hydrothermal conditions and calcination, resulting in a structured catalyst with improved pore volume and selectivity for propylene oxide production.
The structured catalyst exhibits enhanced propylene oxide selectivity and yield, with reduced by-product formation, and maintains high activity over extended periods, demonstrating improved catalytic performance in propylene epoxidation reactions.
Smart Images

Figure 0007560452000005 
Figure 0007560452000006 
Figure 0007560452000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a molded article comprising a zeolitic material having a framework MFI, a method for preparing the same and a method for using the same, wherein 98-100% by mass of the zeolitic material consists of Ti, Si, O and H. [Background technology]
[0002] Titanium-containing zeolitic materials of structure type MFI are known to be efficient catalysts, including, for example, epoxidation reactions. In industrial-scale processes, typically carried out in a continuous mode, the zeolitic materials are usually employed in the form of shaped articles that contain a suitable binder in addition to the catalytically active zeolitic material.
[0003] M. Liu et al. in "Green and efficient preparation of hollow titanium silicalite-1 by using recycled mother liquid" disclose the preparation of hollow titanium silicalite-1 (hollow TS-1, HTS-1) by using recycled mother liquor for post-synthesis treatment. In this regard, the starting material of titanium silicalite-1 was hydrothermally treated with different bases to form hollow voids in the material. The resulting hollow TS-1 showed better catalytic activity in propylene epoxidation than the starting material.
[0004] J. Xu et al., "Effect of triethylamine treatment of titanium silicalite-1 on propylene epoxidation", Frontiers of Chemical Science and Engineering, disclose titanium silicalite-1 treated with triethylamine solution under different conditions. It has been shown that the crystals of TS-1 have many irregular cavities due to random dissolution of framework silicon. Samples of the modified TS-1 showed more or less improved catalyst life when used for propylene epoxidation in a fixed-bed reactor.
[0005] M. Liu et al., in "Highly Selective Epoxidation of Propylene in a Low-Pressure Continuous Slurry Reactor and the Regeneration of Catalyst", disclose the epoxidation of propylene to propylene oxide with hydrogen peroxide using micron-sized TS-1 catalyst with a hollow structure.
[0006] CN108250161A relates to a method for oxidizing allyl alcohol using titanium silicalite as a catalyst. The titanium silicalite is at least partially modified titanium silicalite, and the modification process includes contacting titanium silicon molecular sieve as raw material with a liquid containing nitric acid and peroxide.
[0007] CN103708493A relates to a titanium silicon molecular sieve with framework structure MFI and its preparation method. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] CN108250161A [Patent Document 2] CN103708493A [Non-patent literature]
[0009] [Non-Patent Document 1] M. Liu et al., “Green and efficient preparation of hollow titanium silicalite-1 by using recycled mother liquid” [Non-Patent Document 2] J. Xu et al., "Effect of triethylamine treatment of titanium silicalite-1 on propylene epoxidation", Frontiers of Chemical Science and Engineering [Non-Patent Document 3] M. Liu et al., “Highly Selective Epoxidation of Propylene in a Low-Pressure Continuous Slurry Reactor and the Regeneration of Catalyst” Summary of the Invention [Problem to be solved by the invention]
[0010] The object of the present invention is to provide novel molded articles comprising zeolitic materials with framework type MFI, in particular hollow TS-1 zeolites, which have advantageous properties, in particular improved propylene oxide selectivity, when used as catalysts or catalyst components, in particular in the epoxidation reaction of propene to propylene oxide. A further object of the present invention is to provide a process for the preparation of such molded articles, in particular a process which gives rise to molded articles having advantageous properties, in particular when used preferably as catalysts or catalyst components, in particular in oxidation or epoxidation reactions. A further object of the present invention is to provide an improved process for the epoxidation of propene with hydrogen peroxide as oxidant, which allows a very high propylene selectivity while showing a very low selectivity with respect to by-products and by-products of the epoxidation reaction.
[0011] Surprisingly, it has been found that such mouldings exhibiting said advantageous properties can be provided when a given moulding comprising hollow TS-1 zeolite is subjected to a specific post-treatment, as a result of which a moulding is obtained which exhibits, inter alia, a specific minimum pore volume as determined by mercury intrusion porosimetry as described herein.In particular, it has been found that, surprisingly, mouldings can be provided which, when used as catalysts in the epoxidation reaction of propene to propylene oxide, and which, when compared to prior art mouldings comprising HTS-1 or TS-1, exhibit a significant improvement in propylene oxide selectivity and yield, and further exhibit excellent life properties. [Means for solving the problem]
[0012] The present invention thus relates to a shaped article comprising a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and wherein the zeolitic material having a framework-type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1, the shaped article further comprising a silica binder, and the shaped article has a pore volume of at least 0.8 mL / g as determined by Hg porosimetry as described in Reference Example 2.
[0013] Furthermore, the present invention relates to a method for preparing a shaped article comprising a zeolitic material having a framework MFI and a silica binder, preferably such a shaped article, which method comprises the steps of: (i) providing a mixture comprising a silica binder precursor and a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1; (ii) shaping the mixture obtained from (i) to obtain a precursor of a molded article; (iii) preparing a mixture comprising the precursor of the molded article obtained from (ii) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the molded article; (iv) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain a molded article. Includes.
[0014] Furthermore, the present invention relates to a shaped article, preferably as defined above, obtainable or obtained by the process as defined above.
[0015] Furthermore, the present invention relates to the use of said shaped articles as adsorbents, absorbents, catalysts or catalyst components, preferably as catalysts or as catalyst components. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 shows the catalytic performance of the inventive molded article according to example 1.2 (solid line) versus the molded article of comparative example 3 (dotted line). [Diagram 2] FIG. 2 shows the catalytic performance of the inventive molded article according to Example 1.2 (solid line) versus the molded article of Comparative Example 3 (dotted line). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] It is preferred that the zeolitic material having framework-type MFI contains hollow voids having diameters greater than 5.5 Angstroms, preferably in the range of greater than 5.5 Angstroms and less than the size of the crystallites of the zeolitic material, as determined by TEM as described in Reference Example 3.
[0018] It is preferred that 99 to 100 mass %, more preferably 99.5 to 100 mass %, and even more preferably 99.9 to 100 mass % of the zeolite material having a framework MFI is composed of Ti, Si, O and H.
[0019] The zeolitic material having a framework MFI preferably has a sodium content, calculated as Na2O, in the range of 0-0.1% by mass, more preferably 0-0.07% by mass, more preferably 0-0.05% by mass, based on the mass of the zeolitic material. It is also preferred that the zeolitic material having a framework MFI has an iron content, calculated as Fe2O3, in the range of 0-0.1% by mass, more preferably 0-0.07% by mass, more preferably 0-0.05% by mass, based on the mass of the zeolitic material.
[0020] Typically, the zeolitic material contained in the molded article of the present invention is in the form of a powder which, with regard to its particle size distribution, can be prepared, for example, by a specific synthesis process resulting in the desired particle size distribution, or by grinding a given zeolitic material, or by spray drying a suspension comprising the zeolitic material, or by spray granulating a suspension comprising the zeolitic material, or by flash drying a suspension comprising the zeolitic material, or by microwave drying a suspension comprising the zeolitic material.
[0021] The zeolitic material having a framework-type MFI may preferably have a volume-based particle size distribution characterized by a Dv90 value in the range of 80 to 200 micrometers, more preferably in the range of 90 to 175 micrometers, more preferably in the range of 100 to 150 micrometers, determined as described in Reference Example 5. Furthermore, the zeolitic material having a framework-type MFI may preferably have a volume-based particle size distribution characterized by a Dv50 value in the range of 30 to 75 micrometers, more preferably in the range of 35 to 65 micrometers, more preferably in the range of 40 to 55 micrometers, determined as described in Reference Example 5. Furthermore, the zeolitic material having a framework-type MFI may preferably have a volume-based particle size distribution characterized by a Dv10 value in the range of 1 to 25 micrometers, preferably in the range of 3 to 20 micrometers, more preferably in the range of 5 to 15 micrometers, determined as described in Reference Example 5.
[0022] There is no specific restriction regarding the Ti content of the zeolitic material having a framework MFI. It is preferred that the zeolitic material having a framework MFI has a Ti content, calculated as elemental Ti, in the range of 1.3-2.1% by mass, more preferably in the range of 1.5-1.9% by mass, more preferably in the range of 1.6-1.8% by mass, based on the mass of the zeolitic material.
[0023] Zeolitic materials having framework type MFI, determined as described in Reference Example 9, have a major resonance in the range of -108 to -120 ppm, and more preferably a minor resonance in the range of -95 to -107 ppm. 29 It is preferable to show a Si solid-state NMR spectrum.
[0024] With the total pore volume of the molded article being at least 0.8 mL / g, it is preferred that this is in the range of 0.8 to 1.5 mL / g, more preferably in the range of 0.9 to 1.4 mL / g, and more preferably in the range of 1.0 to 1.3 mL / g.
[0025] Furthermore, no particular restrictions are applied with respect to the shaped shape of the molded article. The molded article is preferably in the form of a strand, more preferably the strand has a hexagonal, rectangular, quadratic, triangular, elliptical or circular cross section, more preferably a circular cross section. Preferably, the cross section has a diameter in the range of 0.1 to 10 mm, more preferably in the range of 0.2 to 7 mm, more preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm, more preferably in the range of 1.6 to 1.8 mm.
[0026] Preferably, the moulded article exhibits a hardness, determined as described in Reference Example 4, of at least 4N, more preferably in the range of 4-20N, more preferably in the range of 6-15N, more preferably in the range of 8-10N.
[0027] There is no particular limitation regarding the mass ratio of the zeolite material having a framework MFI to the silica binder in the molded article. The mass ratio of the zeolite material having a framework MFI to the silica binder calculated as SiO2, MFI:SiO2, is preferably in the range of 0.5:1 to 10:1, more preferably in the range of 1:1 to 5:1, more preferably in the range of 1.5:1 to 4:1, more preferably in the range of 2:1 to 3:1.
[0028] In general, the molded article of the present invention may contain, in addition to the zeolite material and the silica binder, one or more further components, for example, one or more zeolite materials other than the zeolite material having a framework MFI, and / or one or more binders other than the silica binder, for example, an alumina binder, a zirconium binder, a ceria binder, a titania binder, etc. It is preferred that 99 to 100% by mass, more preferably 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the molded article is composed of the zeolite material having a framework MFI and the silica binder.
[0029] The molded article has a thickness of 300-400 mm, as determined in Example 6. 2 / g, more preferably 325 to 365 m 2 / g, more preferably 340 to 350 m 2 It is preferred that the carbon black has a BET specific surface area in the range of 1 / g.
[0030] It is preferred that 50 to 100% by mass, and more preferably 60 to 100% by mass, of the molded article is present in a crystalline form.
[0031] In particular, the molded articles disclosed herein exhibit particular properties when used in the catalytic epoxidation of propylene, specifically as described in Reference Example 10. It is preferred that the molded articles exhibit a pressure drop rate, determined as described in Reference Example 10, in the range of 0.012-0.030 bar(abs) / min, more preferably in the range of 0.015-0.025 bar(abs) / min, more preferably in the range of 0.016-0.020 bar(abs) / min. Furthermore, it is preferred that the molded articles exhibit a propylene oxide activity, determined as described in Reference Example 10, of at least 4.5 wt.%, more preferably in the range of 4.5-7 wt.%, more preferably in the range of 5-6 wt.%.
[0032] Furthermore, the molded article exhibits particular properties when used in the catalytic epoxidation of propylene, in particular as described in Reference Example 11. It is preferred that the molded article exhibits a propylene oxide over propylene selectivity, determined in a continuous epoxidation reaction as described in Reference Example 11, in the range of 96-100%, preferably in the range of 96.5-100%, more preferably in the range of 97-100%. In this regard, it is preferred that the molded article exhibits a hydrogen peroxide conversion in the range of 85-95%, more preferably in the range of 87-93%, more preferably in the range of 88-92%, and more preferably said selectivity is determined at 200 hours time-on-stream, preferably at 200 and 300 hours time-on-stream, more preferably at 200, 300 and 400 hours time-on-stream, more preferably at 200, 300, 400 and 500 hours time-on-stream, more preferably at 200, 300, 400, 500 and 600 hours time-on-stream, more preferably at 200, 300, 400, 500, 600 and 700 hours time-on-stream, wherein the term "time-on-stream" refers to the duration of continuous epoxidation reaction without catalyst regeneration.
[0033] Furthermore, the present invention relates to a method for preparing a shaped article, preferably as disclosed herein, comprising a zeolitic material having a framework MFI and a silica binder, the method comprising the steps of: (i) providing a mixture comprising a silica binder precursor and a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1; (ii) shaping the mixture obtained from (i) to obtain a precursor of a molded article; (iii) preparing a mixture comprising the precursor of the molded article obtained from (ii) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the molded article; (iv) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain a molded article. Includes.
[0034] It is preferred that the zeolitic material having framework-type MFI comprises hollow voids having diameters greater than 5.5 Angstroms, more preferably in the range of greater than 5.5 Angstroms and less than the size of the crystallites of the zeolitic material, as determined by TEM as described in Reference Example 3.
[0035] Regarding the preparation of the zeolitic material having a framework-type MFI according to (i), there is no particular limitation. A preferred method for preparing the zeolitic material having a framework-type MFI according to (i) may comprise the following steps: (a) providing a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a type I nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1; (b) preparing an aqueous mixture comprising the zeolitic material provided in (i) and a zeolitic framework-based MFI structure directing agent; (c) subjecting the mixture resulting from step (b) to hydrothermal conditions under autogenous pressure, preferably in an autoclave, to obtain a suspension comprising a precursor of the zeolitic material having framework type MFI according to (i) and separating said precursor from the suspension, (d) optionally, calcining the precursor in a gas atmosphere; (e) subjecting the precursor obtained from step (c) or (d) to an acid treatment and preferably drying the acid-treated precursor in a gas atmosphere; (f) calcining the acid-treated precursor to obtain the zeolitic material having framework-type MFI according to (i).
[0036] Preferably, the zeolite framework type MFI structure directing agent according to step (a) comprises a tetraalkylammonium salt, preferably a tetraalkylammonium hydroxide. In the mixture according to step (b), the mass ratio of the zeolite framework type MFI structure directing agent to the zeolite material provided in (i), SDA:MFI, is in the range of 1:4 to 3:1, more preferably in the range of 1:2 to 1.5:1, more preferably in the range of 0.8:1 to 0.9:1. Preferably, the hydrothermal conditions according to step (c) comprise a temperature of the mixture in the range of 150 to 190°C, more preferably in the range of 160 to 180°C, more preferably in the range of 165 to 175°C. Subjecting the mixture obtained from step (b) to the hydrothermal conditions according to step (c) may be preferably performed for 5 to 50 hours, preferably 10 to 30 hours, more preferably 20 to 25 hours. Preferably, the separation according to step (c) comprises subjecting the suspension to filtration or centrifugation, more preferably the separation further comprises washing the zeolitic material having framework type MFI at least once with a liquid solvent system, the liquid solvent system preferably comprising one or more of water, alcohol and mixtures of two or more thereof, more preferably water. Preferably, the separation according to step (c) further comprises drying the precursor, preferably the washed precursor, in a gas atmosphere. Preferably, the drying is carried out at a temperature of the gas atmosphere in the range of 40-80°C, more preferably in the range of 50-70°C, more preferably in the range of 55-65°C. Preferably, the gas atmosphere comprises nitrogen, oxygen or a mixture thereof, more preferably the gas atmosphere is oxygen, air or lean air. If carried out, the calcination of the precursor according to step (d) is preferably carried out at a temperature of the gas atmosphere in the range of 450-550°C, more preferably in the range of 475-525°C, more preferably in the range of 490-510°C. Preferably, the gas atmosphere comprises nitrogen, oxygen, or a mixture thereof, more preferably the gas atmosphere is oxygen, air, or lean air.
[0037] Preferably, the acid treatment according to step (e) comprises preparing an aqueous mixture of the precursor obtained from step (c) or (d) and an acid, respectively, and heating the resulting mixture. There is no particular limitation regarding the chemical nature of the acid. Preferably, the acid is one or more of nitric acid, sulfuric acid, and acetic acid, more preferably nitrile acid. In this aqueous mixture, the mass ratio of the acid to the precursor obtained from step (c) or (d) is preferably in the range of 1:2 to 5:1, preferably in the range of 1:1 to 3:1, more preferably in the range of 1.5:1 to 2.5:1. Preferably, the aqueous mixture is heated under reflux, preferably for example, for 0.5 to 1.5 hours, more preferably for 0.75 to 1.25 hours. When the acid-treated precursor is dried in a gas atmosphere according to step (d), the drying is preferably performed at a temperature of the gas atmosphere in the range of 100 to 140°C, more preferably in the range of 110 to 130°C. Preferably, the gas atmosphere used for drying comprises nitrogen, oxygen or a mixture thereof, more preferably the gas atmosphere is oxygen, air or lean air. Preferably, the drying may be carried out for 2 to 6 hours, more preferably 3 to 5 hours. According to step (f), the calcination is preferably carried out at a gas atmosphere temperature in the range of 450 to 550°C, more preferably in the range of 475 to 525°C, more preferably in the range of 490 to 520°C. The calcination may be preferably carried out for 3 to 10 hours, more preferably 5 to 8 hours. Preferably, the gas atmosphere used for calcination comprises nitrogen, oxygen or a mixture thereof, more preferably the gas atmosphere is oxygen, air or lean air.
[0038] The present invention also relates to a zeolitic material having framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and wherein the zeolitic material having framework-type MFI exhibits a type IV nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1, and which is obtainable or obtained by a process comprising, preferably consisting of, steps (a) to (f).
[0039] The present invention therefore also relates to a method for preparing the above-mentioned moulded article, said method comprising a method for preparing a zeolitic material with framework type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O and H, and the zeolitic material with framework type MFI exhibits a nitrogen adsorption / desorption isotherm of type IV, determined as described in Reference Example 1, said method comprising the steps of: (a) providing a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a type I nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1; (b) preparing an aqueous mixture comprising the zeolitic material provided in (i) and a zeolitic framework-based MFI structure directing agent; (c) subjecting the mixture resulting from step (b) to hydrothermal conditions under autogenous pressure, preferably in an autoclave, to obtain a suspension comprising a precursor of the zeolitic material having framework type MFI according to (i) and separating said precursor from the suspension, (d) optionally, calcining the precursor in a gas atmosphere; (e) subjecting the precursor obtained from step (c) or (d) to an acid treatment and preferably drying the acid-treated precursor; (f) calcining the acid-treated precursor to obtain the zeolitic material having framework-type MFI according to (i). wherein the method further comprises: (i) preparing a mixture comprising a silica binder precursor and a zeolitic material obtained from step (f) or obtainable or obtained by a process comprising steps (a) to (c); (ii) shaping the mixture obtained from (i) to obtain a precursor of a molded article; (iii) preparing a mixture comprising the precursor of the molded article obtained from (ii) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the molded article; (iv) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain a molded article. Includes.
[0040] As mentioned above, 98-100% by weight of the zeolitic material having framework type MFI contained in the mixture provided in (i) consists of Ti, Si, O and H. The zeolitic material may therefore generally comprise one or more further elements of the periodic system of elements. It is preferred that 99-100% by weight, more preferably 99.5-100% by weight, more preferably 99.9-100% by weight of the zeolitic material having framework type MFI consists of Ti, Si, O and H.
[0041] The zeolitic material having a framework MFI according to (i) preferably has a sodium content, calculated as Na2O, in the range of 0 to 0.1% by weight, more preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material. The zeolitic material having a framework MFI preferably has an iron content, calculated as Fe2O3, in the range of 0 to 0.1% by weight, more preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0042] Typically the zeolitic material according to (i) is in the form of a powder which, with regard to its particle size distribution, can be prepared, for example, by a specific synthesis process resulting in the desired particle size distribution, or by grinding a given zeolitic material, or by spray drying a suspension comprising the zeolitic material, or by spray granulating a suspension comprising the zeolitic material, or by flash drying a suspension comprising the zeolitic material, or by microwave drying a suspension comprising the zeolitic material.
[0043] The zeolitic material according to (i) may preferably have a volume-based particle size distribution characterized by a Dv90 value, determined as described in Reference Example 5, in the range of 80 to 200 micrometers, more preferably in the range of 90 to 175 micrometers, more preferably in the range of 100 to 150 micrometers. Furthermore, the zeolitic material having a framework-type MFI may preferably have a volume-based particle size distribution characterized by a Dv50 value, determined as described in Reference Example 5, in the range of 30 to 75 micrometers, more preferably in the range of 35 to 65 micrometers, more preferably in the range of 40 to 55 micrometers. Furthermore, the zeolitic material having a framework-type MFI may preferably have a volume-based particle size distribution characterized by a Dv10 value, determined as described in Reference Example 5, in the range of 1 to 25 micrometers, preferably in the range of 3 to 20 micrometers, more preferably in the range of 5 to 15 micrometers.
[0044] There is no specific restriction regarding the Ti content of the zeolitic material having a framework-type MFI according to (i). It is preferred that the zeolitic material having a framework-type MFI has a Ti content, calculated as elemental Ti, in the range of 1.3-2.1 wt.%, more preferably in the range of 1.5-1.9 wt.%, more preferably in the range of 1.6-1.8 wt.%, based on the mass of the zeolitic material.
[0045] Zeolitic materials having framework type MFI according to (i), determined as described in Reference Example 9, have a major resonance in the range of -108 to -120 ppm, and more preferably a minor resonance in the range of -95 to -107 ppm. 29 It is preferable to show a Si solid-state NMR spectrum.
[0046] Preferably, the zeolitic material according to (i) has a molecular weight of at least 300 m, determined as described in Reference Example 6. 2 / g, more preferably 350 to 500m 2 / g, preferably 375 to 450 m 2 / g, more preferably 390 to 410 m2 / g.
[0047] The silica binder precursor is preferably selected from the group consisting of silica sol, colloidal silica, wet-process silica, dry-process silica, and mixtures of two or more thereof, and more preferably the silica binder precursor is colloidal silica. In this context, both colloidal silica and so-called "wet-process" silica and so-called "dry-process" silica can be used. Colloidal silica is preferably commercially available as an alkaline and / or ammoniacal solution, more preferably as an ammoniacal solution, for example as Ludox®, Syton®, Nalco® or Snowtex®, among others. "Wet-process" silica is commercially available, for example as Hi-Sil®, Ultrasil®, Vulcasil®, Santocel®, Valron-Estersil®, Tokusil® or Nipsil®, among others. "Dry process" silicas are commercially available, for example as Aerosil®, Reolosil®, Cab-O-Sil®, Fransil® or ArcSilica®, among others. According to the invention, ammoniacal solutions of colloidal silica are preferred.
[0048] No particular restrictions apply with regard to the physical or chemical properties of the mixture provided in (i). It is preferred that in the mixture according to (i) the mass ratio of the zeolitic material to the Si contained in the silica binder precursor, calculated as SiO2, is in the range of 0.5:1 to 10:1, more preferably in the range of 1:1 to 5:1, more preferably in the range of 1.5:1 to 4:1, more preferably in the range of 2:1 to 3:1.
[0049] Preferably, the mixture provided in (i) comprises, in addition to the zeolitic material and the silica binder precursor, one or more further components. More preferably, the mixture according to (i) further comprises one or more viscosity modifiers, or one or more pore formers, preferably more mesopore formers, or one or more viscosity modifiers and one or more pore formers, preferably mesopore formers.
[0050] The one or more agents are preferably selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof, where the organic polymer is more preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof, where the organic polymer is more preferably selected from the group consisting of cellulose derivatives, polyalkylene oxides, polystyrene, and mixtures of two or more thereof, where the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof, where the one or more agents more preferably include water, carboxymethylcellulose, polyethylene oxide, and polystyrene. More preferably, the one or more agents consist of water, carboxymethylcellulose, polyethylene oxide, and polystyrene.
[0051] When the mixture prepared according to (i) comprises one or more viscosity modifiers and / or mesopore formers, the mass ratio of zeolitic material to the one or more agents, i.e. to any of these agents, is preferably in the range of 1:1 to 5:1, preferably in the range of 2.5:1 to 4:1, more preferably in the range of 3:1 to 3.5:1.
[0052] There are no particular limitations regarding the method of providing the mixture (i), i.e., preparing the mixture. It is preferred to prepare the mixture by suitable mixing of the components, preferably by mixing in a kneader or mix-muller.
[0053] Depending on the mass of the mixture, the mixing or kneading time should be adjusted. By way of example only, the mixture may be mixed or kneaded for 15 to 60 minutes, preferably 30 to 55 minutes, more preferably 40 to 50 minutes.
[0054] No particular restrictions apply to shaping the mixture obtained in (i) by (ii), as long as a precursor of a molded article can be obtained. Thus, the mixture obtained from (i) can be shaped into any conceivable form. It is preferred to shape the mixture in (ii) into strands, more preferably into strands having a circular cross section.
[0055] When the mixture is shaped into strands having a circular cross section by (ii), no particular restrictions apply with respect to the diameter of the circular cross section. The strands having a circular cross section preferably have a diameter in the range of 0.1 to 10 mm, more preferably in the range of 0.2 to 7 mm, more preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm, more preferably in the range of 1.6 to 1.8 mm.
[0056] There is no particular restriction as to the shaping of (ii), and the shaping may be carried out by any conceivable means. In (ii), the shaping preferably comprises extruding the mixture.
[0057] Suitable extrusion equipment is described, for example, in "Ullmann's Enzyklopaedie der Technischen Chemie", 4th edition, volume 2, p. 295 et seq., 1972. In addition to the use of extruders, extrusion presses can also be used to prepare the shaped articles. If necessary, the extruder can be suitably cooled during the extrusion process. The strands leaving the extruder through the extruder die head can be mechanically cut with a suitable wire or with a non-continuous gas stream.
[0058] There is no particular restriction regarding the shaping of (ii), and (ii) may comprise further steps, preferably (ii) further comprising drying the precursor of the shaped article in a gas atmosphere.
[0059] When the precursor of the molded article is dried in a gas atmosphere, there is no particular restriction on the drying conditions. Drying is preferably carried out at a gas atmosphere temperature in the range of 80 to 160°C, more preferably in the range of 100 to 140°C, and more preferably in the range of 110 to 130°C.
[0060] The duration of drying should be adjusted depending on the mass of the precursor of the molded article to be dried. By way of example only, the precursor of the molded article may for example be dried in a gas atmosphere for 2 to 6 hours, preferably for 3 to 5 hours, more preferably for 3.5 to 4.5 hours.
[0061] Furthermore, when the precursor of the molded article is dried in a gas atmosphere, no particular restrictions are applied with respect to the gas atmosphere for drying.The gas atmosphere preferably contains nitrogen, oxygen, or a mixture thereof, and the gas atmosphere is more preferably oxygen, air, or lean air.
[0062] As disclosed above, no particular restrictions apply with respect to the shaping of (ii), which may include further steps. It is preferred that (ii) further comprises calcining the shaped article precursor, preferably the dried shaped article precursor, in a gas atmosphere.
[0063] When the precursor of the molded article is calcined in a gas atmosphere, no particular restrictions are imposed on the calcination conditions. It is preferable to carry out the calcination at a gas atmosphere temperature in the range of 450 to 530°C, more preferably in the range of 470 to 510°C, and more preferably in the range of 480 to 500°C.
[0064] The duration of the calcination should be adjusted depending on the mass of the precursor of the shaped article to be calcined. By way of example only, the precursor of the shaped article may for example be calcined in a gas atmosphere for 3 to 7 hours, preferably for 4 to 6 hours, more preferably for 4.5 to 5.5 hours.
[0065] Furthermore, when the precursor of the shaped article is calcined in a gas atmosphere, no particular restrictions apply with respect to the gas atmosphere for calcination. It is preferred that the gas atmosphere comprises nitrogen, oxygen or a mixture thereof, and the gas atmosphere is preferably oxygen, air or lean air.
[0066] Regarding the conditions of the water treatment in (iii), no particular restrictions are applied, and any conceivable conditions may be applied, so long as the water treatment includes hydrothermal conditions and can obtain a water-treated precursor of a molded article. The water treatment according to (iii) preferably includes a temperature of the mixture in the range of 100 to 200°C, more preferably in the range of 125 to 175°C, more preferably in the range of 130 to 160°C, more preferably in the range of 135 to 155°C, and more preferably in the range of 140 to 150°C.
[0067] As disclosed above, no particular restrictions are applied with respect to the conditions of the water treatment according to (iii). It is preferred that the water treatment according to (iii) is carried out under autogenous pressure. It is particularly preferred that the water treatment according to (iii) is carried out in an autoclave.
[0068] As disclosed above, no particular restrictions are applied regarding the conditions of the water treatment by (iii). The water treatment by (iii) is preferably carried out for 6 to 10 hours, more preferably 7 to 9 hours, and more preferably 7.5 to 8.5 hours.
[0069] No particular restrictions are applied with respect to the physical or chemical properties of the mixture prepared in (iii). In the mixture prepared in (iii), it is preferred that the mass ratio of the zeolitic material to water is in the range of 1:1 to 1:10, more preferably in the range of 1:3 to 1:7, more preferably in the range of 1:4 to 1:6.
[0070] Regarding the method comprising (i), (ii), (iii) and (iv) disclosed herein, no particular restrictions are applied regarding the further method steps that may be carried out between the two steps. After (iii) and before (iv), it is preferable to separate the water-treated precursor of the shaped article from the mixture obtained from (iii), the separation preferably comprises subjecting the mixture obtained from (iii) to filtration or centrifugation, more preferably, the separation further comprises washing the water-treated precursor of the shaped article at least once with a liquid solvent system, the liquid solvent system preferably comprises one or more of water, alcohol, and mixtures of two or more thereof, and the water-treated precursor of the shaped article is more preferably washed with water.
[0071] As disclosed above, this process may include further steps. After (iii) and before (iv), the water-treated precursor of the molded article is preferably dried in a gas atmosphere, where the water-treated precursor of the molded article is preferably separated as described above. For drying, no particular restrictions are applied regarding the drying conditions. Drying is preferably carried out at a temperature of the gas atmosphere in the range of 80 to 160°C, more preferably in the range of 100 to 140°C, more preferably in the range of 110 to 130°C.
[0072] The duration of drying should be adjusted depending on the mass of the water-treated precursor of the molded article to be dried. By way of example only, the precursor of the molded article may be dried in a gas atmosphere for example for 2 to 6 hours, preferably for 3 to 5 hours, more preferably for 3.5 to 4.5 hours. Furthermore, when the water-treated precursor of the molded article or the separated water-treated precursor of the molded article is dried in a gas atmosphere, no particular restrictions are applied with respect to the gas atmosphere for drying. It is preferable that the gas atmosphere contains nitrogen, oxygen, or a mixture thereof, and the gas atmosphere is preferably oxygen, air, or lean air.
[0073] Regarding the conditions of the calcination in (iv), no particular restrictions are applied. It is preferable that the calcination in (iv) is carried out at a temperature of the gas atmosphere in the range of 400 to 490°C, more preferably in the range of 420 to 470°C, and more preferably in the range of 440 to 460°C.
[0074] The duration of calcination should be adjusted depending on the mass of the water-treated precursor of the shaped article to be calcined. By way of example only, the precursor of the shaped article may for example be calcined in a gas atmosphere for 0.5 to 5 hours, preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours.
[0075] Furthermore, no particular restrictions apply with regard to the gas atmosphere for the calcination. The gas atmosphere according to (iv) preferably comprises nitrogen, oxygen or a mixture thereof, the gas atmosphere being preferably oxygen, air or lean air.
[0076] Calcination is particularly preferably carried out in a muffle furnace, a rotary kiln and / or a belt calciner.
[0077] Furthermore, the present invention relates to a shaped article comprising a zeolitic material having framework-type MFI and a silica binder, the shaped article being obtainable or obtainable by the method described herein above.
[0078] Furthermore, the present invention relates to the use of the shaped article according to any one of the embodiments disclosed herein as an adsorbent, absorbent, catalyst or catalyst component, preferably as a catalyst or catalyst component, more preferably as a Lewis acid catalyst or Lewis acid catalyst component, as an isomerization catalyst or isomerization catalyst component, as an oxidation catalyst or oxidation catalyst component, as an aldol condensation catalyst or aldol condensation catalyst component, or as a Prins reaction catalyst or Prins reaction catalyst component, more preferably as an oxidation catalyst or oxidation catalyst component, more preferably as an epoxidation catalyst or epoxidation catalyst component, more preferably as an epoxidation catalyst.
[0079] The invention also relates to the use of said moulded articles as catalysts or catalyst components, preferably as catalyst components for the preparation of propylene oxide from propene in methanol as solvent and with hydrogen peroxide as oxidant.
[0080] According to the present invention, when hydrogen peroxide is used as oxidizing agent, it is considered that hydrogen peroxide is formed in situ during the reaction from hydrogen and oxygen or from other suitable precursors. More preferably, the term "using hydrogen peroxide as oxidizing agent" as used in the context of the present invention relates to an embodiment in which hydrogen peroxide is not formed in situ but is employed as starting material, preferably in the form of a solution, preferably at least partially aqueous, more preferably an aqueous solution, said preferably aqueous solution having a preferred hydrogen peroxide concentration in the range of 20-60% by weight, more preferably 25-55% by weight, based on the total weight of the solution.
[0081] In addition to the above, the present invention relates to a method for preparing propylene oxide, using the molded article of the present invention as a catalytic species. According to this method, propene is reacted with hydrogen peroxide in a methanol solution in the presence of the molded article disclosed herein to obtain propylene oxide. The reaction feed introduced into at least one reactor in which the continuous epoxidation process of the present invention is carried out comprises propene, methanol and hydrogen peroxide. Moreover, this reaction feed comprises a certain amount of potassium cations, and further phosphorus in the form of the anion of at least one phosphorus oxyacid.
[0082] The conversion and selectivity of the epoxidation reaction can be influenced, for example, by the temperature of the epoxidation reaction, the pH of the epoxidation reaction mixture, and / or by the addition of one or more compounds to the reaction mixture other than the reactants propene and hydrogen peroxide.
[0083] When the molded article is used as an epoxidation catalyst or as an epoxidation catalyst component for the epoxidation reaction of an organic compound, no particular restrictions apply with respect to the organic compound. It is preferred that the organic compound has at least one C-C double bond, and the organic compound is more preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably propene. It is particularly preferred that the molded article is used as an epoxidation catalyst or epoxidation catalyst component for the epoxidation of propene, more preferably for the epoxidation of propene with hydrogen peroxide as the oxidizing agent, more preferably for the epoxidation of propene with hydrogen peroxide as the oxidizing agent in a solvent containing an alcohol, preferably methanol.
[0084] According to the present invention, when hydrogen peroxide is used as oxidizing agent, it is considered that hydrogen peroxide is formed in situ during the reaction from hydrogen and oxygen or from other suitable precursors. Most preferably, however, the term "using hydrogen peroxide as oxidizing agent" as used in the context of the present invention relates to an embodiment in which hydrogen peroxide is not formed in situ but is employed as starting material, preferably in the form of a solution, preferably at least partially aqueous, more preferably an aqueous solution, said preferably aqueous solution having a preferred hydrogen peroxide concentration in the range of 20-60% by weight, more preferably 25-55% by weight, based on the total weight of the solution.
[0085] Furthermore, the present invention relates to a method for oxidizing an organic compound, the method comprising contacting an organic compound with a catalyst comprising the shaped article according to any one of the embodiments disclosed herein, preferably for the epoxidation reaction of an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably propene.
[0086] Regarding the conditions of the process for oxidizing an organic compound, no particular restrictions apply, and one or more agents may be used therein. It is preferred that the process includes the use of an oxidizing agent, more preferably hydrogen peroxide is used as the oxidizing agent, more preferably the oxidation reaction is carried out in a solvent, more preferably a solvent comprising an alcohol, preferably methanol.
[0087] Furthermore, the present invention relates to a method for preparing propylene oxide, comprising reacting propene with hydrogen peroxide in a methanol solution in the presence of a catalyst comprising the shaped article according to any one of the embodiments disclosed herein to obtain propylene oxide.
[0088] Typically, the process for preparing propylene oxide is carried out in a reactor. No particular restrictions apply with regard to the means of feeding propene, methanol and hydrogen peroxide into the reactor. It is preferred to introduce a reaction feed containing propene, methanol and hydrogen peroxide into the reactor, said reaction feed containing potassium cations (K ) in an amount of 100 to 160 micromoles per mole of hydrogen peroxide contained in the reaction feed. + ) and further contains phosphorus (P) in the form of the anion of at least one phosphorus oxyacid.
[0089] No particular restrictions apply with regard to the physical or chemical nature of the reaction feed, which may contain one or more further components. The reaction feed may contain 100 to 155 micromoles of K, more preferably 120 to 150 micromoles of K, per mole of hydrogen peroxide contained in the reaction feed. + It is preferred that the compound contains
[0090] As disclosed above, no particular restrictions are imposed on the physical and chemical properties of the reaction feed. + The molar ratio of to P is preferably in the range of 1.5:1 to 2.5:1, and more preferably in the range of 1.9:1 to 2.1:1.
[0091] As disclosed above, no particular restrictions are imposed on the physical and chemical properties of the reaction feeds. The reaction feeds are preferably derived from a hydrogen peroxide feed, a methanol feed, and a propene feed.
[0092] When the reaction feed is obtained from a hydrogen peroxide feed, a methanol feed, and a propene feed, no particular restrictions apply with respect to the physical or chemical nature of the hydrogen peroxide feed. The hydrogen peroxide feed may contain less than 110 micromoles of K, more preferably less than 70 micromoles, more preferably less than 30 micromoles, and especially less than 5 micromoles, per mole of hydrogen peroxide contained in the hydrogen peroxide feed. + It is preferred that the compound contains
[0093] Hydrogen peroxide feed less than 110 micromolar K + When the hydrogen peroxide feed contains + and P in the form of the anion of at least one phosphorus oxyacid, in an amount of K as defined in any one of the embodiments disclosed herein. + and P in the form of the anion of at least one phosphorus oxyacid are preferably added to the hydrogen peroxide feed, or to the propene feed, or to the methanol feed, or to a mixture of two or three thereof, in an amount such that the reaction feed contains
[0094] K + and P in the form of the anion of at least one phosphorus oxyacid, in an amount of K as defined in any one of the embodiments disclosed herein. + and P in the form of the anion of at least one phosphorus oxyacid are added to the hydrogen peroxide feed, or to the propene feed, or to the methanol feed, or to a mixture of two or three thereof, in such an amount that the reaction feed contains at least one solution of dipotassium hydrogen phosphate, and no particular restrictions apply as to the physical or chemical nature of the at least one solution. It is preferred that the at least one solution is an aqueous solution of dipotassium hydrogen phosphate.
[0095] When the reaction feed is derived from a hydrogen peroxide feed, a methanol feed, and a propene feed, no particular restrictions apply with respect to the physical or chemical nature of the hydrogen peroxide feed. The hydrogen peroxide feed is preferably an aqueous or methanolic or aqueous / methanolic, more preferably an aqueous hydrogen peroxide feed, and preferably contains hydrogen peroxide in an amount of 25-75% by weight, more preferably 30-50% by weight.
[0096] When the reaction feed is obtained from a hydrogen peroxide feed, a methanol feed, and a propene feed, no particular restrictions are applied with respect to the physical or chemical properties of the propene feed. It is preferred that the propene feed further contains propane, and the volume ratio of propene to propane is preferably in the range of 99.99:0.01 to 95:5.
[0097] No particular restrictions apply with regard to the physical or chemical nature of the reaction feed. The reaction feed may therefore consist of one or more phases. It is preferred that the reaction feed introduced into the reactor consists of one liquid phase.
[0098] No particular restrictions apply with regard to the conditions under which the process for preparing propylene oxide, which comprises reacting propene with hydrogen peroxide in a methanol solution in the presence of a catalyst comprising molded articles, is carried out in a reactor at a pressure of at least 10 bar (abs), more preferably at least 15 bar (abs), more preferably at least 20 bar (abs), more preferably in the range of 20 to 40 bar (abs).
[0099] As disclosed above, no particular restrictions are applied regarding the conditions for carrying out the process for preparing propylene oxide, which comprises reacting propene with hydrogen peroxide in a methanol solution in the presence of a catalyst comprising a molded article. It is preferable to cool the reaction mixture in the reactor externally and / or internally so that the maximum temperature of the reaction mixture in the reactor is in the range of 30-70°C.
[0100] No particular restrictions are imposed on the method of reacting propene with hydrogen peroxide in a methanol solution in the presence of a catalyst containing a molded article. The reaction of propene with hydrogen peroxide in a methanol solution in the presence of a catalyst containing a molded article is as follows: (a) reacting propene and hydrogen peroxide in methanol solution in the presence of a catalyst comprising a shaped article in at least one reactor R1, preferably operated in an isothermal mode, wherein a reaction feed comprising propene, methanol and hydrogen peroxide is introduced into R1, said reaction feed being enriched in potassium cations (K) in an amount of 100 to 160 micromoles per mole of hydrogen peroxide contained in the reaction feed; + ) and further containing phosphorus (P) in the form of the anion of at least one phosphorus oxyacid; (b) separating from the reaction mixture obtained from (a) and withdrawn from R1 a stream containing unreacted hydrogen peroxide, said separation being preferably carried out by distillation in at least one, preferably one, distillation column K1, (c) mixing a stream containing unreacted hydrogen peroxide with a stream of propene and feeding the mixed stream into at least one, preferably one, reactor R2 containing a catalyst comprising molded articles and preferably operated in an adiabatic mode, reacting propene and hydrogen peroxide in R2; wherein the conversion rate of hydrogen peroxide in R1 is preferably in the range of 85 to 95%, more preferably in the range of 87 to 93%.
[0101] The unit bar (abs) is 10 5 Refers to absolute pressure in Pa, and the unit angstrom is 10 -10 Refers to the length of m.
[0102] The present invention is further described by the following series of embodiments and combinations of embodiments resulting from the dependency and back reference as shown. In particular, in each instance where the range of embodiments is mentioned, it should be noted that in the context of a term such as "the molded article according to any one of embodiments 1 to 4", it is meant that all embodiments within this range are expressly disclosed to those skilled in the art, that is, the wording of this term is understood by those skilled in the art to be synonymous with "the molded article according to any one of embodiments 1, 2, 3 and 4".
[0103] 1. A molded article comprising a zeolitic material having a framework type MFI, wherein 98-100% by weight of said zeolitic material consists of Ti, Si, O, and H, and wherein said zeolitic material having a framework type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1, said molded article further comprising a silica binder, and said molded article has a pore volume of at least 0.8 mL / g as determined by Hg porosimetry as described in Reference Example 2.
[0104] 2. The molded article according to embodiment 1, wherein the zeolitic material having framework type MFI comprises hollow voids having diameters greater than 5.5 angstroms, preferably greater than 5.5 angstroms and smaller than the size of the crystallites of the zeolitic material, as determined by TEM as described in Reference Example 3.
[0105] 3. The molded article according to embodiment 1 or 2, wherein 99 to 100% by mass, preferably 99.5 to 100% by mass, more preferably 99.9 to 100% by mass, of the zeolitic material having framework MFI is composed of Ti, Si, O, and H.
[0106] 4. The molded article according to any one of embodiments 1 to 3, wherein the zeolitic material having framework MFI has a sodium content, calculated as Na2O, in the range of 0 to 0.1% by weight, preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0107] 5. The molded article according to any one of embodiments 1 to 4, wherein the zeolitic material having framework MFI has an iron content, calculated as Fe2O3, in the range of 0 to 0.1% by weight, preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0108] 6. The molded article according to any one of the preceding claims, wherein the zeolitic material having framework MFI preferably has a volume-based particle size distribution characterized by a Dv90 value, determined as described in Reference Example 5, in the range of 80 to 200 micrometers, preferably in the range of 90 to 175 micrometers, more preferably in the range of 100 to 150 micrometers.
[0109] 7. The molded article according to any one of the preceding claims, wherein the zeolitic material having framework MFI has a volume-based particle size distribution characterized by a Dv50 value, determined as described in Reference Example 5, in the range of 30 to 75 micrometers, preferably in the range of 35 to 65 micrometers, more preferably in the range of 40 to 55 micrometers.
[0110] 8. The molded article according to any one of the preceding claims, wherein the zeolitic material having framework MFI has a volume-based particle size distribution characterized by a Dv10 value, determined as described in Reference Example 5, in the range of 1 to 25 micrometers, preferably in the range of 3 to 20 micrometers, more preferably in the range of 5 to 15 micrometers.
[0111] 9. The molded article according to any one of embodiments 1 to 8, wherein the zeolitic material having framework MFI has a Ti content, calculated as elemental Ti, in the range of 1.3 to 2.1 mass%, preferably in the range of 1.5 to 1.9 mass%, more preferably in the range of 1.6 to 1.8 mass%, based on the mass of the zeolitic material.
[0112] 10. Zeolitic material having a framework type MFI, determined as described in Reference Example 9, has a major resonance in the range of -108 to -120 ppm, and preferably a minor resonance in the range of -95 to -107 ppm. 29 10. The molded article of any one of the preceding claims, showing a Si solid-state NMR spectrum.
[0113] 11. The molded article according to any one of embodiments 1 to 10, having a pore volume in the range of 0.8 to 1.5 mL / g, preferably in the range of 0.9 to 1.4 mL / g, and more preferably in the range of 1.0 to 1.3 mL / g.
[0114] 12. The molded article according to any one of the preceding embodiments, which is preferably a strand having a hexagonal, rectangular, quadratic, triangular, elliptical or circular cross section, more preferably a circular cross section, the cross section preferably having a diameter in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm, more preferably in the range of 1.6 to 1.8 mm.
[0115] 13. The molded article according to any one of the preceding embodiments, exhibiting a hardness, determined as described in Reference Example 4, of at least 4 N, preferably in the range of 4 to 20 N, more preferably in the range of 6 to 15 N, more preferably in the range of 8 to 10 N.
[0116] 14. The molded article according to any one of the preceding embodiments, wherein in the molded article, the mass ratio of the zeolitic material having framework MFI to the silica binder, calculated as SiO2, MFI:SiO2, is in the range of 1:1 to 5:1, preferably in the range of 1.5:1 to 4:1, more preferably in the range of 2:1 to 3:1.
[0117] 15. The molded article according to any one of embodiments 1 to 14, wherein 99 to 100% by mass, preferably 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the molded article is made of a zeolitic material having a framework MFI and a silica binder.
[0118] 16. Determined as described in Reference Example 6, 300-400 m 2 / g, preferably 325 to 365 m 2 / g, more preferably 340 to 350 m 2 16. The molded article according to any one of the preceding claims, having a BET specific surface area in the range of 1 / g.
[0119] 17. The molded article according to any one of the preceding embodiments, wherein 50-100% by mass, preferably 60-100% by mass, of the molded article is present in crystalline form.
[0120] 18. The molded article according to any one of the preceding embodiments, exhibiting a pressure drop rate, determined as described in Reference Example 10, in the range of 0.012 to 0.030 bar(abs) / min, preferably in the range of 0.015 to 0.025 bar(abs) / min, more preferably in the range of 0.016 to 0.020 bar(abs) / min.
[0121] 19. The molded article of any one of the preceding embodiments, exhibiting a propylene oxide activity, determined as described in Reference Example 10, of at least 4.5% by weight, preferably in the range of 4.5 to 7% by weight, more preferably in the range of 5 to 6% by weight.
[0122] 20. The molded article according to any one of the preceding embodiments, exhibiting a propylene oxide over propylene selectivity in the range of 96 to 100%, preferably in the range of 96.5 to 100%, more preferably in the range of 97 to 100%, as determined in a continuous epoxidation reaction as described in Reference Example 11.
[0123] 21. The molded article of embodiment 20, wherein the hydrogen peroxide conversion is in the range of 85-95%, preferably in the range of 87-93%, more preferably in the range of 88-92%, and more preferably the selectivity is determined at 200 hours time-on-stream, preferably at 200 and 300 hours time-on-stream, more preferably at 200, 300 and 400 hours time-on-stream, more preferably at 200, 300, 400 and 500 hours time-on-stream, more preferably at 200, 300, 400, 500 and 600 hours time-on-stream, more preferably at 200, 300, 400, 500, 600 and 700 hours time-on-stream, wherein the term "time-on-stream" refers to the duration of continuous epoxidation reaction without catalyst regeneration.
[0124] 22. A method for preparing a shaped article comprising a zeolitic material having a framework MFI and a silica binder, preferably as described in any one of the preceding embodiments 1 to 21, comprising: (i) providing a mixture comprising a silica binder precursor and a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1; (ii) shaping the mixture obtained from (i) to obtain a precursor of a molded article; (iii) preparing a mixture comprising the precursor of the molded article obtained from (ii) and water, and subjecting the mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the molded article; (iv) Calcining the water-treated precursor of the molded article in a gas atmosphere to obtain a molded article. The method includes:
[0125] 23. The method of embodiment 22, wherein the zeolitic material having framework-type MFI comprises hollow voids having diameters greater than 5.5 angstroms, preferably greater than 5.5 angstroms and smaller than the size of the crystallites of the zeolitic material, as determined by TEM as described in Reference Example 3.
[0126] 24. The method according to embodiment 22 or 23, wherein 99 to 100% by weight, preferably 99.5 to 100% by weight, more preferably 99.9 to 100% by weight, of the zeolitic material having framework MFI consists of Ti, Si, O and H.
[0127] 25. The method according to any one of embodiments 22 to 24, wherein the zeolitic material having framework MFI has a sodium content, calculated as Na2O, in the range of 0 to 0.1% by weight, preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0128] 26. The method according to any one of embodiments 22 to 25, wherein the zeolitic material having framework-type MFI has an iron content, calculated as Fe2O3, in the range of 0 to 0.1% by weight, preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0129] 27. The method according to any one of embodiments 22 to 26, wherein the zeolitic material having framework MFI preferably has a volume-based particle size distribution characterized by a Dv90 value in the range of 80 to 200 micrometers, preferably in the range of 90 to 175 micrometers, more preferably in the range of 100 to 150 micrometers, determined as described in Reference Example 5.
[0130] 28. The method according to any one of embodiments 22 to 27, wherein the zeolitic material having framework MFI has a volume-based particle size distribution characterized by a Dv50 value, determined as described in Reference Example 5, in the range of 30 to 75 micrometers, preferably in the range of 35 to 65 micrometers, more preferably in the range of 40 to 55 micrometers.
[0131] 29. The method according to any one of embodiments 22 to 28, wherein the zeolitic material having framework MFI has a volume-based particle size distribution characterized by a Dv10 value in the range of 1 to 25 micrometers, preferably in the range of 3 to 20 micrometers, more preferably in the range of 5 to 15 micrometers, determined as described in Reference Example 5.
[0132] 30. The method according to any one of embodiments 22 to 29, wherein the zeolitic material having framework MFI has a Ti content, calculated as elemental Ti, in the range of 1.3 to 2.1 mass%, preferably in the range of 1.5 to 1.9 mass%, more preferably in the range of 1.6 to 1.8 mass%, based on the mass of the zeolitic material.
[0133] 31. The zeolitic material having a framework type MFI, determined as described in Reference Example 9, has a major resonance in the range of -108 to -120 ppm and preferably a minor resonance in the range of -95 to -107 ppm. 29 31. The method of any one of embodiments 22 to 30, showing a Si solid state NMR spectrum.
[0134] 32. The zeolitic material having a framework MFI has a molecular weight of at least 300 m, as determined as described in Reference Example 6. 2 / g, preferably 350 to 500m 2 / g, preferably 375 to 450 m 2 / g, more preferably 390 to 410 m 2 The method according to any one of embodiments 22 to 31, having a BET specific surface area in the range of 1 / g.
[0135] 33. The method of any one of embodiments 22 to 32, wherein the silica binder precursor is selected from the group consisting of silica sol, colloidal silica, wet-process silica, dry-process silica, and mixtures of two or more thereof, and the silica binder precursor is preferably colloidal silica.
[0136] 34. The method of any one of embodiments 22 to 33, wherein in the mixture according to (i), the mass ratio of the zeolitic material to the Si contained in the silica binder precursor, calculated as SiO2, is in the range of 1:1 to 5:1, preferably in the range of 1.5:1 to 4:1, more preferably in the range of 2:1 to 3:1.
[0137] 35. The method of any one of embodiments 22 to 34, wherein the mixture prepared by (i) further comprises one or more viscosity modifiers and / or mesopore formers.
[0138] 36. The method of embodiment 35, wherein the one or more agents are selected from the group consisting of water, alcohol, organic polymers, and mixtures of two or more thereof, where the organic polymer is preferably selected from the group consisting of cellulose, cellulose derivatives, starch, polyalkylene oxides, polystyrene, polyacrylates, polymethacrylates, polyolefins, polyamides, polyesters, and mixtures of two or more thereof, where the organic polymer is more preferably selected from the group consisting of cellulose derivatives, polyalkylene oxides, polystyrene, and mixtures of two or more thereof, where the organic polymer is more preferably selected from the group consisting of methylcellulose, carboxymethylcellulose, polyethylene oxide, polystyrene, and mixtures of two or more thereof, where more preferably the one or more agents comprise water, carboxymethylcellulose, polyethylene oxide, and polystyrene.
[0139] 37. The method of embodiment 35 or 36, wherein in the mixture prepared by (i), the mass ratio of zeolite material to the one or more agents is in the range of 1:1 to 5:1, preferably in the range of 2.5:1 to 4:1, more preferably in the range of 3:1 to 3.5:1.
[0140] 38. The method according to any one of embodiments 22 to 37, wherein the mixture is mixed in a kneader or mixing muller.
[0141] 39. The method according to any one of embodiments 22 to 38, wherein in (ii), the mixture is shaped into strands, preferably strands having a circular cross-section.
[0142] 40. The method of embodiment 39, wherein the strands having a circular cross-section have a diameter in the range of 0.2 to 10 mm, preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, more preferably in the range of 1.5 to 2 mm, more preferably in the range of 1.6 to 1.8 mm.
[0143] 41. The method of any one of embodiments 22 to 40, wherein in (ii), shaping comprises extruding the mixture.
[0144] 42. The method according to any one of embodiments 22 to 41, wherein the shaping according to (ii) further comprises drying the precursor of the shaped article in a gas atmosphere.
[0145] 43. The method according to embodiment 42, wherein drying is carried out at a temperature of the gas atmosphere in the range of 80 to 160°C, preferably in the range of 100 to 140°C, more preferably in the range of 110 to 130°C.
[0146] 44. The method of embodiment 42 or 43, wherein the gas atmosphere comprises nitrogen, oxygen, or a mixture thereof, and the gas atmosphere is preferably oxygen, air, or lean air.
[0147] 45. The method according to any one of embodiments 22 to 44, preferably any one of embodiments 37 to 39, wherein the shaping according to (ii) further comprises calcining the preferably dried shaped article precursor in a gas atmosphere.
[0148] 46. The method of embodiment 45, wherein the calcination is carried out at a temperature of the gas atmosphere in the range of 450 to 530 °C, preferably in the range of 470 to 510 °C, more preferably in the range of 480 to 500 °C.
[0149] 47. The method of embodiment 45 or 46, wherein the gas atmosphere comprises nitrogen, oxygen, or a mixture thereof, and the gas atmosphere is preferably oxygen, air, or lean air.
[0150] 48. The method according to any one of embodiments 22 to 47, wherein the water treatment according to (iii) comprises a temperature of the mixture in the range of 100 to 200°C, preferably in the range of 125 to 175°C, more preferably in the range of 130 to 160°C, more preferably in the range of 135 to 155°C, more preferably in the range of 140 to 150°C.
[0151] 49. The method according to any one of embodiments 22 to 48, wherein the water treatment according to (iii) is carried out under autogenous pressure, preferably in an autoclave.
[0152] 50. The method according to any one of embodiments 22 to 49, wherein the water treatment with (iii) is carried out for 6 to 10 hours, preferably 7 to 9 hours, more preferably 7.5 to 8.5 hours.
[0153] 51. The method according to any one of embodiments 22 to 50, wherein in the mixture prepared in (iii), the mass ratio of zeolite material to water is in the range of 1:1 to 1:10, preferably in the range of 1:3 to 1:7, more preferably in the range of 1:4 to 1:6.
[0154] 52. The method according to any one of embodiments 22 to 51, wherein after (iii) and before (iv), the water-treated precursor of the shaped article is separated from the mixture obtained from (iii), the separation preferably comprises subjecting the mixture obtained from (iii) to filtration or centrifugation, more preferably the separation further comprises washing the water-treated precursor of the shaped article at least once with a liquid solvent system, the liquid solvent system preferably comprising one or more of water, alcohol, and mixtures of two or more thereof, and the water-treated precursor of the shaped article is more preferably washed with water.
[0155] 53. The method according to any one of embodiments 22 to 52, wherein after (iii) and before (iv), the separated water-treated precursor of the shaped article is preferably dried in a gas atmosphere, wherein the drying is preferably carried out at a temperature of the gas atmosphere in the range of 80 to 160°C, more preferably in the range of 100 to 140°C, more preferably in the range of 110 to 130°C, and wherein the gas atmosphere preferably comprises nitrogen, oxygen, or a mixture thereof, or the gas atmosphere is more preferably oxygen, air, or lean air.
[0156] 54. The method according to any one of embodiments 22 to 53, wherein the calcination in (iv) is carried out at a temperature of the gas atmosphere in the range of 400 to 490 °C, preferably in the range of 420 to 470 °C, more preferably in the range of 440 to 460 °C.
[0157] 55. The method according to any one of embodiments 22 to 54, wherein the gas atmosphere according to (iv) comprises nitrogen, oxygen, or a mixture thereof, the gas atmosphere being preferably oxygen, air, or lean air.
[0158] 56. The following process: (a) providing a zeolitic material having a framework-type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a type I nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1; (b) preparing an aqueous mixture comprising the zeolitic material provided in (i) and a zeolitic framework-based MFI structure directing agent; (c) subjecting the mixture resulting from step (b) to hydrothermal conditions under autogenous pressure, preferably in an autoclave, to obtain a suspension comprising a precursor of the zeolitic material having framework type MFI according to (i) and separating said precursor from the suspension, (d) optionally, calcining the precursor in a gas atmosphere; (e) subjecting the precursor obtained from step (c) or (d) to an acid treatment and preferably drying the acid-treated precursor; (f) calcining the acid-treated precursor to obtain the zeolitic material having framework-type MFI according to (i). 56. The method according to any one of embodiments 22 to 55, comprising preparation of the zeolitic material of (i) by a process comprising, preferably consisting of, the steps:
[0159] 57. A shaped article comprising a zeolitic material having framework MFI and a silica binder, the shaped article being obtainable or obtainable by the method according to any one of embodiments 22 to 56.
[0160] 58. Use of the shaped article according to any one of embodiments 1 to 21 or according to embodiment 57 as an adsorbent, absorbent, catalyst or catalyst component, preferably as a catalyst or catalyst component, more preferably as a Lewis acid catalyst or Lewis acid catalyst component, as an isomerization catalyst or as an isomerization catalyst component, as an oxidation catalyst or as an oxidation catalyst component, as an aldol condensation catalyst or as an aldol condensation catalyst component, or as a Prins reaction catalyst or as a Prins reaction catalyst component, more preferably as an oxidation catalyst or as an oxidation catalyst component, more preferably as an epoxidation catalyst or epoxidation catalyst component, more preferably as an epoxidation catalyst.
[0161] 59. The use according to embodiment 58, wherein an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably for the epoxidation reaction of propene, more preferably for the epoxidation of propene using hydrogen peroxide as an oxidant, more preferably for the epoxidation of propene using hydrogen peroxide as an oxidant in a solvent comprising an alcohol, preferably methanol.
[0162] 60. A method for oxidizing an organic compound, preferably for the epoxidation of an organic compound, more preferably for the epoxidation reaction of an organic compound having at least one C-C double bond, preferably a C2-C10 alkene, more preferably a C2-C5 alkene, more preferably a C2-C4 alkene, more preferably a C2 or C3 alkene, more preferably propene, comprising contacting the organic compound with a catalyst comprising the shaped article of any one of embodiments 1 to 21 or embodiment 57.
[0163] 61. The method of embodiment 60, wherein hydrogen peroxide is used as the oxidizing agent, and the oxidation reaction is preferably carried out in a solvent, more preferably in a solvent comprising an alcohol, preferably methanol.
[0164] 62. A method for preparing propylene oxide, comprising reacting propene with hydrogen peroxide in a methanol solution in the presence of a catalyst comprising the shaped article of any one of embodiments 1 to 21 or embodiment 57 to obtain propylene oxide.
[0165] 63. A reaction feed containing propene, methanol and hydrogen peroxide is introduced into a reactor, and the reaction feed is added with potassium cations (K cations) in an amount of 100 to 160 micromoles per mole of hydrogen peroxide contained in the reaction feed. + 63. The method of embodiment 62, further comprising phosphorus (P) in the form of the anion of at least one phosphorus oxyacid.
[0166] 64. The reaction feed contains 100 to 155 micromoles, preferably 120 to 150 micromoles, of K per mole of hydrogen peroxide contained in the reaction feed. + 64. The method of embodiment 63, comprising:
[0167] 65. In the reaction feed, K + The method according to embodiment 63 or 64, wherein the molar ratio of to P is in the range of 1.5:1 to 2.5:1, preferably in the range of 1.9:1 to 2.1:1.
[0168] 66. The method of any one of embodiments 63 to 65, wherein the reaction feed is obtained from a hydrogen peroxide feed, a methanol feed, and a propene feed.
[0169] 67. The hydrogen peroxide feed contains less than 110 micromoles, preferably less than 70 micromoles, more preferably less than 30 micromoles, and especially less than 5 micromoles of K per mole of hydrogen peroxide contained in the hydrogen peroxide feed. + 67. The method of embodiment 66, comprising:
[0170] 68. K +and P in the form of the anion of at least one phosphorus oxyacid, in an amount of K as defined in any one of embodiments 63 to 65. + and P in the form of the anion of at least one phosphorus oxyacid are added to the hydrogen peroxide feed, or to the propene feed, or to the methanol feed, or to a mixed feed of two or three thereof in an amount such that the reaction feed contains:
[0171] 69. The method of embodiment 68, wherein at least one solution is an aqueous solution of dipotassium hydrogen phosphate.
[0172] 70. The method of any one of embodiments 66 to 69, wherein the hydrogen peroxide supply is an aqueous or methanolic or aqueous / methanolic, preferably an aqueous, hydrogen peroxide supply, preferably containing hydrogen peroxide in an amount of 25 to 75% by weight, more preferably 30 to 50% by weight.
[0173] 71. The method of any one of embodiments 66 to 70, wherein the propene feed further contains propane, and the volume ratio of propene to propane is preferably in the range of 99.99:0.01 to 95:5.
[0174] 72. The method of any one of embodiments 63 to 71, wherein the reaction feed consists of one phase when introduced into the reactor.
[0175] 73. The process according to any one of embodiments 62 to 72, wherein the pressure at which the reaction of propene with hydrogen peroxide in methanol solution in the presence of a catalyst comprising a shaped article is carried out in a reactor is at least 10 bar (abs), preferably at least 15 bar (abs), more preferably at least 20 bar (abs), more preferably in the range of 20 to 40 bar (abs).
[0176] 74. The method of any one of embodiments 62 to 73, wherein the reaction mixture in the reactor is cooled externally and / or internally such that the maximum temperature of the reaction mixture in the reactor is in the range of 30 to 70°C.
[0177] 75. The reaction of propene with hydrogen peroxide in a methanol solution in the presence of a catalyst containing a molded article is as follows: (i) reacting propene and hydrogen peroxide in methanol solution in the presence of a catalyst comprising a moulded article in at least one reactor R1, preferably operated in an isothermal mode, wherein a reaction feed comprising propene, methanol and hydrogen peroxide is introduced into R1, said reaction feed being enriched in potassium cations (K) in an amount of 100 to 160 micromoles per mole of hydrogen peroxide contained in the reaction feed; + ) and further containing phosphorus (P) in the form of the anion of at least one phosphorus oxyacid; (ii) separating from the reaction mixture obtained from (i) and withdrawn through R1 a stream containing unreacted hydrogen peroxide, said separation being preferably carried out by distillation in at least one, preferably one, distillation column K1, (iii) mixing a stream containing unreacted hydrogen peroxide with a stream of propene and feeding the mixed stream into at least one, preferably one, reactor R2 containing a catalyst comprising molded articles and preferably operated in an adiabatic mode, reacting propene and hydrogen peroxide in R2; 75. The method of any one of embodiments 62 to 74, comprising:
[0178] According to a further aspect, the present invention relates to a zeolitic material having a framework type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, P, and H, and the zeolitic material having a framework type MFI exhibits a type IV nitrogen adsorption / desorption isotherm, determined as described in Reference Example 1. The present invention is therefore further described by the following series of embodiments and combinations of embodiments resulting from the dependencies and back references as indicated. In particular, in each instance where a range of embodiments is mentioned, it is to be noted that in the context of terms such as "the zeolitic material according to any one of the embodiments 1' to 4'", it is meant that all embodiments within this range are expressly disclosed to the skilled person, i.e., the wording of this term is understood by the skilled person to be synonymous with "the molded article according to any one of the embodiments 1', 2', 3', and 4'".
[0179] 1'. A P-containing zeolitic material having a framework type MFI, wherein 98-100% by mass of the zeolitic material consists of Ti, Si, O, P, and H, and the zeolitic material having a framework type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1.
[0180] 2'. The zeolite material according to embodiment 1', wherein 99 to 100% by mass, preferably 99.5 to 100% by mass, more preferably 99.9 to 100% by mass of the zeolite material is composed of Ti, Si, O, and H.
[0181] 3'. The zeolitic material according to embodiment 1' or 2', having a Ti content, calculated as elemental Ti, in the range of 0.5 to 3.0 mass%, preferably in the range of 1.0 to 2.0 mass%, more preferably in the range of 1.2 to 1.8 mass%, based on the mass of the zeolitic material.
[0182] 4'. The zeolitic material according to any one of embodiments 1' to 3', having a P content, calculated as elemental P, in the range of 0.5 to 6.0 mass%, preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%, based on the mass of the zeolitic material.
[0183] 5'. At least 250 m, as determined as described in Reference Example 6 2 / g, preferably 250 to 500m 2 / g, more preferably 300 to 450m 2 The zeolitic material according to any one of embodiments 1' to 4', having a BET specific surface area in the range of 1 / g.
[0184] 6'. Contains three resonances with areas of (74.5±3x)%, (23.5±2x)%, and (2.0±x)%. 29 The zeolitic material according to any one of embodiments 1' to 5', exhibiting a Si direct excitation solid-state NMR spectrum, wherein x is 2, preferably 1, more preferably 0.5.
[0185] 7'. Contains a major resonance having a peak in the range of -108 to -120 ppm with area I0, and preferably a minor resonance having a peak in the range of -95 to -108 ppm with area I1. 29 The zeolitic material according to any one of embodiments 1' to 6' exhibits a Si cross-polarized solid-state NMR spectrum, with the ratio I0:I1 preferably in the range of 0.7:1 to 1.3:1, more preferably in the range of 0.85:1 to 1.15:1, more preferably in the range of 0.9:1 to 1.1:1.
[0186] 8'. Five resonances with peaks at (-2±0.2) ppm, (-11±0.2) ppm, (-23±0.2) ppm, (-31±0.2) ppm, and (-44±0.2) ppm, and optionally additional resonances. 31The zeolitic material according to any one of embodiments 1' to 7', exhibiting a P direct excitation solid-state NMR spectrum, in which the ratio of the integral I0 over the range of +7 to -23 ppm to the integral I1 over the range of -23 to -53 ppm in the spectrum is preferably in the range of 0.5:1 to 1.1:1, more preferably in the range of 0.65:1 to 0.95:1, more preferably in the range of 0.7:1 to 0.9:1.
[0187] 9'. Five resonances with peaks at (-2±0.2) ppm, (-11±0.2) ppm, (-23±0.2) ppm, (-31±0.2) ppm, and (-44±0.2) ppm, and optionally further resonances. 31 8. The zeolitic material according to any one of embodiments 1' to 8', exhibiting a P cross-polarized solid-state NMR spectrum, in which the ratio of the integral I0 over the range from +7 to -23 ppm to the integral I1 over the range from -23 to -53 ppm is preferably in the range of 0.5:1 to 1.1:1, more preferably in the range of 0.65:1 to 0.95:1, more preferably in the range of 0.7:1 to 0.9:1.
[0188] 10'. A method for preparing a P-containing zeolitic material according to any one of embodiments 1' to 9', comprising: (i') preparing an aqueous mixture comprising a zeolitic material having a framework type MFI, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm as determined as described in Reference Example 1, the mixture further comprising a source of P. (ii') drying the mixture prepared in (i') in a gas atmosphere to obtain a precursor of the P-containing zeolite material; (iii') calcining the dried precursor of the P-containing zeolitic material to obtain the P-containing zeolitic material. The method includes:
[0189] 11. The method according to embodiment 10', wherein the zeolitic material according to (i') comprises hollow voids having diameters greater than 5.5 angstroms, preferably in the range of greater than 5.5 angstroms and smaller than the size of the crystallites of the zeolitic material, as determined by TEM as described in Reference Example 3.
[0190] 12'. The method according to embodiment 10' or 11', wherein 99 to 100% by weight, preferably 99.5 to 100% by weight, more preferably 99.9 to 100% by weight, of the zeolitic material according to (i') consists of Ti, Si, O and H.
[0191] 13'. The method according to any one of embodiments 10' to 12', wherein the zeolitic material according to (i') has a sodium content, calculated as Na2O, in the range of 0 to 0.1% by weight, preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0192] 14'. The method according to any one of embodiments 10' to 13', wherein the zeolitic material according to (i') has an iron content, calculated as Fe2O3, in the range of 0 to 0.1% by weight, preferably in the range of 0 to 0.07% by weight, more preferably in the range of 0 to 0.05% by weight, based on the weight of the zeolitic material.
[0193] 15'. The method according to any one of embodiments 10' to 14', wherein the zeolitic material according to (i') has a Ti content, calculated as elemental Ti, in the range of 1.3 to 2.1 mass%, preferably in the range of 1.5 to 1.9 mass%, more preferably in the range of 1.6 to 1.8 mass%, based on the mass of the zeolitic material.
[0194] 16'. The method of any one of embodiments 10' to 15', wherein the source of P comprises one or more phosphorus oxoacids, preferably one or more of hypophosphoric acid, hypophosphorous acid, phosphoric acid, phosphorous acid, pyrophosphoric acid, and triphosphate, more preferably phosphoric acid (H3PO4).
[0195] 17'. The method according to any one of embodiments 10' to 16', wherein the drying according to (ii') is carried out at a temperature of the gas atmosphere in the range of 50 to 150°C, preferably in the range of 70 to 140°C, more preferably in the range of 90 to 130°C, the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, more preferably the gas atmosphere being oxygen, air or lean air.
[0196] 18'. The process according to any one of embodiments 10' to 17', wherein the calcination according to (iii') is carried out at a temperature of the gas atmosphere in the range of 400 to 600°C, preferably in the range of 450 to 550°C, more preferably in the range of 475 to 525°C, the gas atmosphere preferably comprising nitrogen, oxygen or a mixture thereof, more preferably the gas atmosphere being oxygen, air or lean air.
[0197] 19'. A P-containing zeolitic material obtainable or obtained by the method according to any one of embodiments 10' to 18', preferably according to any one of embodiments 1' to 9'.
[0198] 20'. A shaped article comprising the zeolitic material according to any one of embodiments 1' to 9' and an acidic binder, said shaped article being optionally obtainable by the method according to any one of embodiments 22 to 56, in which instead of the zeolitic material according to (i) the zeolitic material according to any one of embodiments 1' to 9' is employed.
[0199] 21'. Use of the zeolitic material according to any one of embodiments 1' to 9' or embodiment 19', or of the shaped article according to embodiment 20', as an adsorbent, as an absorbent, as a catalyst or as a catalyst component.
[0200] The present invention is further illustrated by the following Examples and Reference Examples. EXAMPLES
[0201] Reference Example 1: Determination of N2 adsorption / desorption isotherms Nitrogen adsorption / desorption isotherms were determined at 77 K according to the method disclosed in DIN 66131.
[0202] Reference Example 2: Determination of the total pore volume The total pore volume was determined via mercury intrusion porosimetry according to DIN66133.
[0203] Reference Example 3: Determination of Hollow Void Size in Zeolitic Materials The size of the hollow voids in the zeolite materials was determined by TEM. Samples for transmission electron microscopy (TEM) were prepared on ultrathin carbon TEM supports. For this purpose, the powder was dispersed in ethanol. A drop of this dispersion was applied between two objective glasses and gently dispersed. A TEM support film was then immersed onto the resulting thin film. The samples were imaged by TEM using a Tecnai Osiris machine (FEI Company, Hillsboro, USA) operated at 200 keV under bright-field and high-angle annular dark-field scanning TEM (HAADF-STEM) conditions. Chemical composition maps were acquired by energy dispersive X-ray spectroscopy (EDXS). Images and elemental maps were evaluated using the iTEM (Olympus, Tokyo, Japan, version: 5.2.3554) and Esprit (Bruker, Billerica, USA, version 1.9) software packages.
[0204] Reference Example 4: Determination of Hardness The crushing strength referred to in the present invention is understood to be that determined by a crushing strength tester Z2.5 / TS1S (supplier Zwick GmbH&Co., D-89079 Ulm, Germany). For the principle of this machine and its operation, reference is made to the respective instruction manual "Register1:Betriebsanleitung / Sicherheitshandbuch für die Material-Pruefmaschine Z2.5 / TS1S", version 1.5, December 2001, Zwick GmbH&Co. Technische Dokumentation, August-Nagel-Strasse 11, D-89079 Ulm, Germany. This machine had a horizontally fixed table on which the strand was placed. The strand was actuated against the fixed table by a plunger with a diameter of 3 mm, which was freely movable in the vertical direction. The device was operated with a preload of 0.5 N, a shear rate under the preload of 10 mm / min, and a subsequent test rate of 1.6 mm / min. A vertically movable plunger, connected to a load cell for picking up the force, moves during the measurements towards a fixed turntable on which the mouldings to be investigated (strands) are placed, thus working the strand against the table. The plunger is applied perpendicular to the longitudinal axis of the strand. With the machine, increasing forces are applied via the plunger to a given strand, which will be described below, until the strand is crushed. The force which crushes the strand is called the crushing strength of the strand. A computer is used to control the experiment, to register and evaluate the measurement results. The value obtained is the average value of the measurements of 10 strands in each case.
[0205] Reference Example 5: Determination of Dv10, Dv50 and Dv90 Values Sample preparation: 1.0 g of the sample was suspended in 100 g of deionized water and stirred for 1 minute. Equipment used and respective parameters: - Mastersizer S Long Bed Version 2.15, ser.No. 33544-325; Supplier: Malvern Instruments GmbH, Herrenberg, Germany - Focal width: 300RFmm - Beam length: 10.00mm - Module: MS17 - Shadowing: 16.9% - Dispersion model: 3D - Analytical model: Polydisperse - Correction: None
[0206] Reference Example 6: Determination of the BET specific surface area The BET specific surface area was determined by nitrogen physical adsorption at 77 K according to the method disclosed in DIN 66131. For the determination of the BET specific surface area, N2 sorption isotherms were measured at the temperature of liquid nitrogen using a Micrometrics ASAP2020M and Tristar system.
[0207] Reference Example 7: Determination of Langmuir surface area The Langmuir surface area was determined by nitrogen physisorption at 77 K according to the method disclosed in DIN 66131.
[0208] Reference Example 8: Powder X-ray diffraction and crystallinity determination Powder X-ray diffraction (PXRD) data were collected using a diffractometer (D8Advance Series II, Bruker AXS GmbH) equipped with a LYNXEYE detector operated with a copper anode X-ray tube operated at 40 kV and 40 mA, with Bragg-Brentano geometry and an air scattering shield to reduce air scattering.
[0209] Crystallinity calculation: The crystallinity of the samples was determined using the software DIFFRAC.EVA from Bruker AXS GmbH, Karlsruhe. The method is described in the user manual, page 121. Default parameters were used for the calculation.
[0210] Calculation of phase composition: The phase composition was calculated on the raw data using the modeling software DIFFRAC.TOPAS provided by Bruker AXS GmbH, Karlsruhe. Using the identified crystal structures of the phases, the instrumental parameters and the crystallite sizes of the individual phases, a diffraction pattern was simulated. This was fitted to the data, and a function was added to model the background intensity.
[0211] Data collection: Samples were homogenized in a mortar and then pressed into a standard flat sample holder provided by Bruker-AXS GmbH for Bragg-Brentano topography data collection. A glass plate was used to compress and flatten the sample powder to achieve a flat surface. Data were collected in the 2θ angle range of 2-70° with a 2θ step size of 0.02° and the variable divergence slit was set at an angle of 0.1°. The crystalline content represents the intensity of the crystalline signal relative to the total scattered intensity (DIFFRAC.EVA User Manual, Bruker AXS GmbH, Karlsruhe).
[0212] Reference Example 9: 29 Si solid-state NMR determination 29 Direct excitation of Si solid-state NMR was performed using a 5 μs 90° pulse, 30 ms free induction decay (FID) acquisition, and 50 kHz 1 Heteronuclear radio frequency decoupling (HPPD) at the H nutation frequency, averaging of at least 128 scans, and a recycle delay of 120 s were used. Spectra are referenced to a unified scale according to Pure Appl. Chem., Vol. 80, No. 1, pp. 59-84, 2008. 29 The Si frequency is that of Me4Si (tetramethylsilane, TMS) in CDCl3 (1% volume fraction). 29 The frequency ratio relative to Si is 19.867187%, expressed in ppm on a unified scale. Direct integration of the spectra was performed using a Bruker Topspin3.
[0213] Reference Example 10: Determination of Propylene Oxide Activity and Pressure Drop Rate (PO Test) In the PO test, a preliminary test procedure to evaluate the possible suitability of the molded articles as epoxidation catalysts for propene, the molded articles were tested in a glass autoclave by reacting propene with an aqueous hydrogen peroxide solution (30% by weight) to obtain propylene oxide. In particular, 0.5 g of the molded article was introduced together with 45 mL of methanol into a glass autoclave cooled to -25°C. 20 mL of liquid propene was forced into the glass autoclave, which was then heated to 0°C. At this temperature, 18 g of aqueous hydrogen peroxide solution (30% by weight in water) was introduced into the glass autoclave. After 5 hours of reaction at 0°C, the mixture was heated to room temperature and analyzed by gas chromatography for the propylene oxide content of the liquid phase. The propylene oxide content of the liquid phase (in % by weight) is the result of the PO test, i.e. the propylene oxide activity of the molded article.
[0214] The pressure drop rate was determined by following the pressure progression during the PO test. The pressure progression was recorded using an S-11 transmitter (Wika Alexander Wiegand SE & Co. KG) placed in the pressure line of the autoclave and a graphic plotter Buddeberg 6100A. The data obtained were read out and a pressure rise curve was plotted. The pressure drop rate (PDR) was calculated by the following formula: PDR = [p(max)-p(min)] / delta t During the ceremony, PDR / (bar / min) = Pressure Drop Rate p(max) / bar = maximum pressure at the start of the reaction p(min) / bar = minimum pressure observed during the reaction Delta t / min = the time difference between the start of the reaction and the time when p(min) is observed
[0215] Reference Example 11: Determination of the Performance of Propylene Epoxidation Catalysts In a continuous epoxidation reaction setup, a vertically arranged tubular reactor (length: 1.4 m, outer diameter 10 mm, inner diameter: 7 mm) equipped with a jacket for thermal stabilization was filled with 15 g of extrusions in the form of strands as described in the following examples. The remaining reactor volume was filled with inert material (steatite spheres with a diameter of 2 mm) up to a height of about 5 cm at the lower end of the reactor and the remainder at the upper end of the reactor. The following flow rates of starting materials were passed through the reactor: methanol (49 g / h), hydrogen peroxide (9 g / h, adopted as an aqueous hydrogen peroxide solution with a hydrogen peroxide content of 40% by weight), propylene (7 g / h, polymer grade). A cooling medium was passed through the cooling jacket to regulate the temperature of the reaction mixture so that the conversion of hydrogen peroxide, determined on the basis of the reaction mixture leaving the reactor, was essentially constant at 90%. The pressure in the reactor was kept constant at 20 bar (abs) and the reaction mixture, except for the fixed bed catalyst, consisted of a single liquid phase.
[0216] The reactor effluent downstream of the pressure control valve was collected, weighed and analyzed. The organic components were analyzed by two separate gas chromatographs. The hydrogen peroxide content was determined colorimetrically using the titanyl sulfate method. The selectivity for a given propylene oxide was determined relative to propene and hydrogen peroxide and was calculated as 100 times the ratio of the moles of propylene oxide in the effluent divided by the moles of propene or hydrogen peroxide in the feed.
[0217] Reference Example 12: Preparation of zeolitic material with framework type MFI (Hollow TS-1 (HTS-1)) Reference Example 12.1: Preparation of a zeolitic material with framework type MFI, in which 98-100% by mass of the zeolitic material consists of Ti, Si, O, and H (Titanium Silicalite-1 (TS-1) Titanium silicalite-1 (TS-1) powder was prepared according to the following recipe: TEOS (tetraethyl orthosilicate) (300 kg) was charged into a stirred tank reactor at room temperature and stirring (100 rpm) was started. In the second vessel, 60 kg TEOS and 13.5 kg TEOT (tetraethyl orthotitanate) were first mixed and then added to the TEOS in the first vessel. After that, another 360 kg TEOS was added to the mixture in the first vessel. Next, the contents of the first vessel were stirred for 10 minutes, after which 950 g TPAOH (tetrapropylammonium hydroxide) was added. Stirring was continued for 60 minutes. Ethanol released by hydrolysis was separated by distillation at a bottom temperature of 95 °C. Then, 300 kg water was added to the contents of the first vessel, and an amount of water equivalent to the amount of distillate was further added. The resulting mixture was stirred for 1 hour. Crystallization was carried out at autogenous pressure at 175 °C within 12 hours. The resulting titanium silicalite-1 crystals were separated, dried and calcined in air at a temperature of 500° C. for 6 hours.
[0218] Reference Example 12.2: Preparation of Hollow TS-1 (HTS-1) 1072 g of deionized water was placed in a beaker. Then, 424 g of tetrapropylammonium hydroxide (as an aqueous solution containing 40% by weight of tetrapropylammonium hydroxide) was added with stirring. Then, 200 g of TS-1 powder prepared according to Reference Example 12.1 was added. The mixture was homogenized for 30 minutes. The mixture was then transferred to an autoclave. The mixture was hydrothermally treated at 170° C. for 24 hours. The resulting suspension was filtered and the resulting solid residue was washed with deionized water. The resulting solid was dried at room temperature overnight. The yield was 150 g.
[0219] 3000 g of aqueous nitric acid (10% by weight HNO3 in water) was placed in a glass beaker. 150 g of dry solid was added to it while stirring. The resulting suspension (while stirring at 250 rpm) was refluxed at 100° C. for 1 h. For work-up, the suspension was filtered and the solid residue was washed with deionized water. The resulting solid was dried in air and subsequently calcined in air in an oven by the following procedure. 1. Heat to 120℃ within 1 hour 2. Dry at 120℃ for 4 hours 3. Heat up to 500℃ within 190 minutes 4. Calcinate at 500℃ for 5 hours.
[0220] The solid was then crushed. The yield was 121 g. The resulting powder had a TOC of less than 0.1 g / 100 g, a Si content of 44 g / 100 g, and a Ti content of 1.7 g / 100 g, a water adsorption / desorption of less than 8.5 at 85% relative humidity, and a pH of 453 m. 2 / g, and a BET specific surface area of 601 m 2 / g Langmuir surface area (each determined as described hereinabove). The sample consisted essentially of HTS-1 (1 wt. % crystalline anatase and 99 wt. % crystalline HTS-1) as determined by X-ray diffraction analysis.
[0221] Example 1: Preparation of a Molded Article According to the Invention Example 1.1: Shaping of HTS-1 powder 50 g of the zeolite material of Reference Example 12.2 and 2 g of Walocel™ (Walocel MW15000GB, Wolff Cellulosics GmbH&Co.KG, Germany) were placed in a kneader and kneaded for 5 minutes. Then, 50.4 g of an aqueous dispersion containing 25% by weight of polystyrene and 25% by weight of silica (colloidal Ludox® AS40 was used as the dispersion base) were added. After 10 minutes, 0.67 g of polyethylene oxide (PEO, Union Carbide, PolyOX Coagulant) was added and the mixture was kneaded. After another 10 minutes, 41.65 g of colloidal silica (Ludox® AS40) was added. Then, the addition of deionized water was started in 10 ml portions every 10 minutes, until a total of 100 ml of water was added. The total kneading time was 45 minutes. After the water addition was complete, the kneaded mass was subjected to shaping. For shaping, the kneaded mass was extruded at a pressure of 150 bar (abs) to obtain strands with a circular cross section and a diameter of 1.7 mm, which were then dried and calcined in air according to the following program: 1.Heated to 120℃ within 60 minutes 2. Maintain a temperature of 120℃ for 4 hours 3.Heated to 490℃ within 185 minutes 4. Maintain the temperature at 490℃ for 5 hours.
[0222] The yield was 55 g.
[0223] Example 1.2: Water treatment of shaped HTS-1 36 g of strands prepared according to Example 1.1 were divided into 4 portions of 9 g each and mixed with 180 g of deionized water per portion. The resulting mixture was heated in an autoclave for 8 hours at a temperature of 145 ° C. The resulting water-treated strands were then separated and sieved through a 0.8 mm sieve. The resulting strands were then washed with deionized water and pre-dried in a nitrogen stream at ambient temperature. The washed and pre-dried strands were then dried and calcined in air according to the following program: 1. Heat to 120℃ within 60 minutes 2. Maintain a temperature of 120℃ for 4 hours 3. Heat up to 450℃ within 165 minutes 4. Maintain the temperature at 450℃ for 2 hours.
[0224] The yield was 36.2 g. The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 45 g / 100 g, and a Ti content of 1.3 g / 100 g, each determined as described hereinabove. The hardness of the strands, determined as described hereinabove, was 4.3 N, and the pore volume, determined as described hereinabove, was 0.82 ml / g.
[0225] Example 2: Preparation of a molded article according to the invention Example 2.1: Shaping of HTS-1 powder 79 g of commercial HTS-1 powder (CN Titanium Silicate RT-03, Zhejiang TWRD New Material Co., Ltd., China) and 3 g of Walocel™ (Walocel MW15000GB, Wolff Cellulosics GmbH & Co. KG, Germany) were placed in a kneader and kneaded for 5 minutes. Then, 75.5 g of an aqueous dispersion containing 25% by weight of polystyrene and 25% by weight of colloidal silica (Ludox® AS40 was used as the basis for the dispersion) was added. After 10 minutes, 1.0 g of polyethylene oxide (PEO, Union Carbide, PolyOX Coagulant) was added and the mixture was kneaded. After another 10 minutes, 70 g of colloidal silica (Ludox® AS40) was added. The mass was kneaded for another 10 minutes. The total kneading time was 35 minutes. The kneaded mass was extruded at a pressure of 120 bar (abs) to obtain strands with a circular cross section with a diameter of 1.9 mm. The extruded strands were then dried and calcined in air according to the following program: 1. Heat to 120℃ within 60 minutes 2. Maintain a temperature of 120℃ for 4 hours 3.Heated to 490℃ within 185 minutes 4. Maintain the temperature at 490℃ for 5 hours.
[0226] The yield was 90 g. The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 45 g / 100 g, and a Ti content of 1.2 g / 100 g, each determined as described hereinabove. The hardness of the strands, determined as described hereinabove, was 0.85 N, and the pore volume, determined as described hereinabove, was 0.76 ml / g. The crystallinity, determined as described hereinabove, was 78%.
[0227] Example 2.2: Water treatment of shaped HTS-1 36 g of the material prepared according to Example 2.1 was divided into 4 portions of 9 g each and mixed with 180 g of deionized water per portion. The resulting mixture was heated in an autoclave at a temperature of 145 ° C for 8 hours. The strands were then sieved through a 0.8 mm sieve. The strands were washed with deionized water and pre-dried in a nitrogen stream at ambient temperature. The washed and pre-dried strands were then dried and calcined in air according to the following program: 1. Heat to 120℃ within 60 minutes 2. Maintain a temperature of 120℃ for 4 hours 3. Heat up to 450℃ within 165 minutes 4. Maintain the temperature at 450℃ for 2 hours.
[0228] The yield was 34.9 g. The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 44 g / 100 g, and a Ti content of 1.3 g / 100 g, and was weighed at 345 m. 2 The strands had a BET specific surface area of 2.0 x 100 / g, each determined as described hereinabove. The strand hardness, determined as described hereinabove, was 8.4 N, and the pore volume, determined as described hereinabove, was 1.0 ml / g.
[0229] Comparative Example: Preparation of Moldings According to the Prior Art The following comparative examples were prepared to allow a comparison between the moldings of the prior art including HTS-1 and the moldings according to the present invention, especially with regard to their catalytic performance in epoxidation reactions. The moldings according to Comparative Example 1 were prepared with reference to the above-cited prior art of Xu et al., especially using Sesbania cannbina Pers. powder. The moldings according to Comparative Example 2 were prepared based on the prior art of Liu et al., in which sepiolite was employed in the preparation process. The comparative examples are therefore carried out with particular regard to the prior art.
[0230] Comparative Example 1: Molding of HTS-1 powder Based on the general teaching of J.Xu et al.: "Effect of triethylamine treatment of titanium silicalite-1 on propylene epoxidation", 150g of commercial HTS-1 powder (Titanium Silicalite RT-03, Zhejiang TWRD New Material Co.,Ltd., China) and 6g of Sesbania powder were placed in a kneader and kneaded for 5 minutes. Then, 75g of colloidal silica (Ludox® AS40) was added. The mass was kneaded for another 10 minutes. Then, 40mL of water was added and the mixture was kneaded for another 5 minutes. After that, another 20mL of water was added and the mixture was kneaded for another 10 minutes. The total kneading time was 30 minutes. A part of the kneaded mass was extruded at a pressure of 150 bar (abs) to obtain strands with a circular cross section with a diameter of 1.7 mm. The remaining kneaded mass was extruded at a pressure of 205 bar (abs). The extruded strands were then dried and calcined in air according to the following program: 1. Heat to 120℃ within 60 minutes 2. Maintain a temperature of 120℃ for 6 hours 3.Heated to 550℃ within 165 minutes 4. Maintain the temperature at 550℃ for 6 hours.
[0231] The yield was 63.2 g. The resulting material had a Ti content of 1.3 g / 100 g, 369 m 2 / g, and a BET specific surface area of 495 m 2 / g Langmuir surface area, each determined as described hereinabove. The hardness of the strands, determined as described hereinabove, was 5.2 N, and the pore volume, determined as described hereinabove, was 0.45 ml / g. The crystallinity, determined as described hereinabove, was 79%.
[0232] Comparative Example 2: Shaping of HTS-1 powder Based on the general teaching of "Highly Selective Epoxidation of Propylene in a Low-Pressure Continuous Slurry Reactor and the Regeneration of Catalyst" by M. Liu et al., 54 g of commercial zeolite HTS-1 (Titanium Silicalite RT-03, Zhejiang TWRD New Material Co,Ltd., China), 36 g of meerschaum with Mg content of about 13 wt% (CAS63800-37-3, Aldrich), and 10 g of methylcellulose (Walocel MW15000GB, Wolff Cellulosics GmbH&Co.KG, Germany) were placed in a kneader and kneaded for 5 min. Then, 40 mL of water was added and the mixture was kneaded for another 15 min. After that, another 25 mL of water was added and the mixture was kneaded for another 10 min. The total kneading time was 30 min. The kneaded mass was extruded at a pressure of 150 bar (abs) to obtain strands with a circular cross section and a diameter of 1.7 mm. The extruded strands were then dried and calcined in air according to the following program: 1. Heat to 80℃ within 40 minutes 2. Maintain temperature at 80℃ for 6 hours 3.Heated to 650℃ within 265 minutes 4. Maintain the temperature at 650℃ for 6 hours.
[0233] The yield was 77.9 g. The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 40 g / 100 g, a Mg content of 5.8 g / 100 g, and a Ti content of 1.1 g / 100 g, and was 314 m. 2 The BET specific surface area was 10 N, determined as described hereinabove, and the pore volume was 0.5 ml / g, determined as described hereinabove.
[0234] For a better overview, the pore volumes of the inventive molded articles containing HTS-1 and of the prior art molded articles containing HTS-1 are given in Table 1 below.
[0235] [Table 1]
[0236] Comparative Example 3: Molding of TS-1 powder Examples 1.1 and 1.2 were repeated, but in Example 1.1, (non-hollow) TS-1 powder according to Reference Example 12.1 was employed as the zeolite material instead of HTS-1 powder according to Reference Example 12.2. Each resulting TS-1-containing strand was further treated (water treatment) as described in Example 1.2.
[0237] Example 3: Catalysis Test Example 3.1: Preliminary Test - PO Test The example mouldings were preliminarily tested for general suitability as epoxidation catalysts by the PO test described in Reference Example 10. The respective resulting values of propylene oxide activity are shown in Table 2 below.
[0238] [Table 2]
[0239] Apparently, according to the PO test, the molded article according to the present invention exhibits very good propylene oxide activity, and is a promising candidate for catalyst in industrial continuous epoxidation reaction.
[0240] Example 3.2: Catalytic properties of the molded articles in a continuous epoxidation reaction The properties of the molded articles of the present invention were compared with those of the prior art in a continuous epoxidation reaction as described in Reference Example 11. After a significant time on stream (TOS) of 200 hours, the propylene oxide selectivity (relative to hydrogen peroxide) of the molded articles according to the present invention Example 2.2 was compared with the respective molded articles according to the prior art (Comparative Examples 1 and 2). To get a complete picture, a further comparative test was carried out by subjecting a molded article containing (non-hollow) TS-1 zeolite material to exactly the same continuous epoxidation reaction conditions according to Reference Example 11 (Comparative Example 3). The following results according to Table 3 were obtained:
[0241] [Table 3]
[0242] Clearly, the molded articles according to the invention show the highest selectivity values for both hydrogen peroxide and propene when compared to the molded articles of the prior art containing HTS-1 zeolite according to Comparative Examples 1 and 2, as well as when compared to the molded articles containing (non-hollow) TS-1 zeolite. It should be noted in particular that these results are obtained on the basis of the molded articles according to Example 1.2, which according to the preliminary PO test results according to Example 3. above may appear to have a slightly inferior catalytic activity compared to the molded articles according to the invention according to Example 2.2. The excellent properties of the molded articles according to the invention are further demonstrated.
[0243] Furthermore, it was found that the molded articles of the present invention exhibit excellent stability with respect to the selectivity of propylene oxide. In this regard, when the molded articles of the present invention (according to Example 1.2) and those of Comparative Example 3 were subjected to continuous epoxidation reaction conditions according to Reference Example 11 with a TOS of more than 750 hours, it was found that the high selectivity towards hydrogen peroxide and propene even showed a tendency to increase over time. Moreover, such highly advantageous properties were not only observed for the valuable product of the epoxidation reaction (propylene oxide), but at the same time, it was found that the molded articles of the present invention also showed a significantly lower selectivity towards undesirable by-products of the epoxidation reaction, such as oxygen, hydroperoxides and methoxypropanol. The respective results are shown in Figures 1 and 2, and the values extracted from the figures are shown in Table 4 below.
[0244] [Table 4]
[0245] Clearly, the molded articles of the present invention exhibited highly advantageous improved life characteristics in a continuous epoxidation reaction, the continuous mode being the standard mode for industrial scale epoxidation processes.
[0246] Example A: Preparation of P-treated HTS-1 20 g of commercial HTS-1 powder (CN Titanium Silicate RT-03, Zhejiang TWRD New Material Co.,Ltd., China) was placed in a container. 2.31 g of orthophosphoric acid (aqueous solution, 85% by weight H3PO4) was added to the zeolite material and homogenized. The resulting mixture was dried in air at a temperature of 110°C for 12 h. The resulting dry solid material was sieved (mesh size 1.6 mm) and the resulting material was calcined in air at 500°C with a heating ramp of 2 K / min for 5 h. The yield was 20.9 g (split: 2.8 g, small particles: 18.1 g). The resulting material had a TOC of less than 0.1 g / 100 g, a Si content of 42 g / 100 g, a Ti content of 1.4 g / 100 g, and a P content of 2.7 g / 100 g.
[0247] BRIEF DESCRIPTION OF THE DRAWINGS Figure 1: Catalytic performance of the inventive molded article according to Example 1.2 (solid line) against the molded article of Comparative Example 3 (dotted line), in particular the propylene selectivity towards hydrogen peroxide (dark grey) and towards propene (light grey). The lower solid black line shows the hydrogen peroxide conversion, the upper solid black line shows the temperature of the cooling medium flowing through the jacket of the reactor.
[0248] FIG. 2: Catalytic performance of the inventive molding according to Example 1.2 (solid line) versus the molding of Comparative Example 3 (dotted line), showing in particular the selectivity towards oxygen, hydroxyacetone, hydroperoxide, 1-methoxy-2-propanol and 2-methoxy-1-propanol.
[0249] References - M. Liu et al.: "Green and efficient preparation of hollow titanium silicalite-1 by using recycled mother liquid", Chemical Engineering Journal, 2018, Vol. 331, pp. 194-202 - J. Xu et al.: "Effect of triethylamine treatment of titanium silicalite-1 on propylene epoxidation", Frontiers of Chemical Science and Engineering, 2014, Vol. 8(4), pp. 478-487 - M. Liu et al. "Highly Selective Epoxidation of Propylene in a Low-Pressure Continuous Slurry Reactor and the Regeneration of Catalyst", Industrial+Engineering Chemistry Research 2015, Vol. 54(20), pp. 5416-5426 - CN108250161A <h2 style=";text-align:left;direction:ltr">- CN103708493A
Claims
1. A molded article comprising a zeolitic material having a framework type MFI and including hollow TS-1, wherein 98-100% by weight of the zeolitic material is composed of Ti, Si, O, and H, and the zeolitic material having a framework type MFI exhibits Type IV adsorption / desorption, the molded article further comprising a silica binder, the molded article having a pore volume in the range of 0.8 mL / g to 1.5 mL / g as determined via mercury intrusion porosimetry; wherein in said molded article the mass ratio of said zeolitic material having framework MFI to said silica binder, calculated as SiO 2 , MFI:SiO 2 , is in the range of 1:1 to 5:1; The zeolitic material having framework type MFI has a Ti content, calculated as elemental Ti, in the range of 1.3 to 2.1 wt. %, based on the weight of the zeolitic material.
2. 2. The article of claim 1, wherein the zeolitic material having framework-type MFI contains hollow voids having diameters greater than 5.5 Angstroms as determined by TEM.
3. 3. The molded article according to claim 1, wherein 99 to 100% by weight of the zeolitic material having framework type MFI consists of Ti, Si, O, and H.
4. 4. The molded article according to claim 1, wherein the zeolitic material having framework type MFI has a Ti content, calculated as elemental Ti, in the range of 1.5 to 1.9% by weight, based on the weight of the zeolitic material.
5. The molded article according to any one of claims 1 to 4, wherein the pore volume is in the range of 0.9 to 1.4 mL / g.
6. In the molded article, the SiO 2 The mass ratio of the silica binder calculated as MFI:SiO 2 The molded article according to any one of claims 1 to 5, wherein the moulded article has a moulded article ratio of 1.5:1 to 4:
1.
7. 7. The molded article according to claim 1, wherein 99 to 100% by mass of the molded article consists of the zeolitic material having framework MFI and the silica binder.
8. 1. A method for preparing a molded article comprising a zeolite material having a framework type MFI and including hollow TS-1 and a silica binder, comprising: (i) providing a mixture comprising a silica binder precursor and a zeolitic material having a framework-type MFI and including hollow TS-1, wherein 98-100% by weight of the zeolitic material consists of Ti, Si, O, and H, and the zeolitic material having a framework-type MFI exhibits a Type IV nitrogen adsorption / desorption isotherm; (ii) shaping the mixture obtained from (i) to obtain a precursor of said shaped article; (iii) preparing a mixture comprising the precursor of the molded article obtained from (ii) and water, and subjecting said mixture to a water treatment under hydrothermal conditions to obtain a water-treated precursor of the molded article; (iv) calcining the water-treated precursor of the molded article in a gas atmosphere to obtain the molded article. Including, the molded article having a pore volume in the range of 0.8 mL / g to 1.5 mL / g as determined via mercury intrusion porosimetry; wherein in said molded article the mass ratio of said zeolitic material having framework MFI to said silica binder, calculated as SiO 2 , MFI:SiO 2 , is in the range of 1:1 to 5:1; The zeolitic material having framework type MFI has a Ti content, calculated as elemental Ti, in the range of 1.3 to 2.1 wt. %, based on the weight of the zeolitic material. method.
9. 9. The method of claim 8, wherein the silica binder precursor is selected from the group consisting of silica sol, colloidal silica, wet process silica, dry process silica, and mixtures of two or more thereof.
10. 10. The method of claim 8 or 9, wherein the mixture prepared by (i) further comprises one or more viscosity modifiers and / or mesopore formers.
11. 11. The method of any one of claims 8 to 10, comprising in (ii) shaping the mixture into strands.
12. 12. The method according to any one of claims 8 to 11, wherein the shaping according to (ii) further comprises drying the precursor of the shaped article in a gas atmosphere, and calcining the dried precursor of the shaped article in a gas atmosphere at a temperature of the gas atmosphere in the range of 450 to 530°C.
13. 13. The method according to any one of claims 8 to 12, wherein the water treatment according to (iii) comprises a temperature of the mixture in the range of 100 to 200°C.
14. 8. Use of the molded article according to any one of claims 1 to 7 as an adsorbent, absorbent, catalyst or catalyst component, as an isomerization catalyst or as an isomerization catalyst component, as an oxidation catalyst or as an oxidation catalyst component, as an aldol condensation catalyst or as an aldol condensation catalyst component, or as a Prins reaction catalyst or as a Prins reaction catalyst component.
Citation Information
Patent Citations
Titanium silicalite molecular sieve with MFI structure and preparation method thereof
CN103708493A
Oxidation method for allyl alcohol
CN108250161A
Titanium-silicon molecular sieve and its preparing method
CN1132699C
Method for producing zeolite and zeolite-type
JP2016529190A
Molded articles made from hydrophobic zeolite-based materials and methods for manufacturing the same
JP2016535718A