Surface-metallized, calibrated composite solder balls for electronic board assembly

Surface-metalized composite solder balls with EPS cores and metal coatings address manufacturing and thermal issues, enhancing cost-effectiveness and mechanical stability in electronic board assembly.

JP7560543B2Active Publication Date: 2024-10-02アンスティテュート デ レシェルシュ アン アンジニアリ ドゥ サーフェス
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022515075
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-12
Filing Date
2020-09-11
Publication Date
2024-10-02
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Current flexible balls used in electronic board assembly have manufacturing costs, calibration issues, and are prone to differential thermal foaming due to dense polymeric cores and metal shells, which affect their density and mechanical stress sensitivity.

Method used

Manufacture surface-metalized and calibrated composite solder balls with a core of expanded polystyrene (EPS) having at least 50% intergranular porosity, coated with copper, nickel, and gold layers, using autocatalytic chemical deposition and granulometric sorting to achieve specific diameters and thicknesses.

Benefits of technology

The solution reduces production costs, improves thermal stability, and maintains mechanical integrity by allowing controlled interconnections between components, reducing mechanical stress and thermal deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560543000002
    Figure 0007560543000002
  • Figure 0007560543000003
    Figure 0007560543000003
  • Figure 0007560543000004
    Figure 0007560543000004
Patent Text Reader

Abstract

The present invention relates to a method for producing composite solder balls with metallized surfaces, the balls comprising a core consisting of spherical support particles of diameter D0 made of expanded polystyrene and having an intergranular porosity of at least 50%, and a shell covering the support particles and formed by a plurality of metallic surface layers. The present invention also relates to the balls obtainable by the method according to the invention, as well as to their use for the assembly of electronic substrates.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to the manufacture of composite solder balls and their use as interconnect solutions for the assembly of electronic boards.

[0002] The search for technologies for the assembly of increasingly miniaturized, lead-free electronic boards is increasingly prompting industry players in this field to seek innovative solutions for implementing the interconnections between components that are sensitive to mechanical stresses, such as ball matrices of the CBGA type ("ceramic ball grid array"), or electromechanical microsystems (traditionally referred to by the acronym MEMS for "microelectromechanical systems").

[0003] Flexible balls (shown in Figure 1) are one of the technologies used to implement systems in packages, commonly referred to by the acronym SiP ("System in Package"). They contain contacts that are soldered, allowing their easy assembly within the package.

[0004] However, currently, the flexible balls currently used in this field have the drawback of being formed from a high density core of polymeric material, which has a negative impact on the manufacturing costs associated with the output of the manufacturing process and the initial ball calibration, as well as the final density of the ball. Furthermore, the problem of differential thermal foaming can be faced between the particle core and the metal shell during the subsequent brazing operation.

[0005] To overcome this drawback, the applicant has developed a method for manufacturing composite solder balls, metallized on the surface, which balls have a core made of spherical support particles of diameter D0, made of expanded polystyrene (EPS) and having an intergranular porosity of at least 50%, and a sphere covering the support particles, the final particles having a diameter D f In particular, the thickness E cu Copper coating, thickness E Niand at least one nickel layer of thickness E au and a shell formed by a plurality of metallic surface layers including a gold topcoat of 1000 .mu.m.

[0006] According to the invention, the method comprises the following steps: A) a first step of providing support particles, followed by B) D0=D f- 2*(E Ni +E cu +E Au a first step of granulometric sorting of the support particles, consisting of a step of physical and / or mechanical separation of support particles having a diameter D0 with a tolerance of + / - 5% such that D0 is between 200 μm and 1000 μm; C) a step of activation treatment of the thus selected support particles to obtain activated support particles; D) a first step of metallization of the activated support particles by autocatalytic chemical deposition of one or more copper layers, said step being carried out to a copper layer thickness E of 15 to 35 μm in order to obtain copper-coated support particles. cu a first step, which is repeated until E) a second step of metallization of the copper-coated support particles by autocatalytic chemical deposition of at least one nickel layer alloyed with phosphorus NiP having a mass percentage of 7-10% phosphorus relative to the total weight of the NiP layer, said step being performed by depositing a chemical nickel layer thickness E of 4 μm to 7 μm in order to obtain chemical nickel-coated support particles. Ni a second step, which is performed until F) Thickness E of 0.05μm~0.12μm Au The surface is metallized and a third step of chemical metallization of the support particles coated with nickel, consisting of a step of gold deposition by the method of galvanic displacement implemented by immersion in an aqueous solution containing gold ions (typically implemented according to the prior art) so as to obtain coated composite solder balls; G) Surface metallized to a tolerance of + / - 5% for diameter D f and a second step of granular sorting of the particles thus metallized to select and select composite solder balls (1) having the above formula (1).

[0007] Balls made of expanded polystyrene (EPS) have the advantage that they can be reduced in size when heated, thus offering the possibility of being calibrated by heat treatment.

[0008] In the sense of the present invention, intergranular porosity means the internal porosity of the support particle, where it is possible to observe different types of pore-channels, networks, "pockets", blind pores and surface roughness at the surface and / or within the support particle, which can be measured, for example, by helium pycnometry.

[0009] The first step of the method according to the invention is providing support particles (Step A).

[0010] Advantageously, it is possible to use balls of expanded polystyrene (EPS) having a level of intergranular porosity of more than 90%.

[0011] In the method according to the invention, first a first granulometric sorting (step B) of the support particles (10) is carried out, which consists of a step of physical and / or mechanical separation of said support particles having a diameter D0 selected to be between 200 μm and 1000 μm. According to an advantageous embodiment of the method according to the invention, step B) of the granulometric sorting of the support particles can consist of a mechanical sieving to sort and select the support particles having a diameter D0 selected to be between 200 μm and 1000 μm. In practice, support particles with a size corresponding to the target value D0 + / - 5% will be selected.

[0012] If expanded polystyrene (EPS) balls are used as support particles, step B) of the granular sorting of the support particles may consist of a mechanical sieving of the support particles. It may then be advantageously completed by a heat treatment at a temperature of 100°C to 120°C, and preferably 110°C to 120°C, of ​​the upper slice of the thus treated particles (i.e. particles with a size larger than D0+5%), in order to increase the calibration output of the initial population of balls. Indeed, given that the diameter of the expanded polystyrene (EPS) balls decreases when heated, when mechanical sieving is combined with heating, the oversized diameter of the sieving of the upper slice of the previously sorted balls may thus be reduced so that the initially rejected balls reach the required diameter D0+ / -5%. This makes it particularly possible to significantly reduce the production costs by increasing the output of the number of balls with diameter D0. This step of heat treatment may advantageously be carried out in a fluidized bed, by gas or by liquid, in order to preserve the initial spherical nature of the balls.

[0013] At the end of the size-based selection step B), an activation treatment (step C) of the previously selected support particles is carried out in order to obtain activated support particles.

[0014] In the sense of the present invention, an activation treatment means a treatment consisting of activating the surface of the support particles in order to allow good adhesion of a subsequent metallization treatment.

[0015] A first advantageous embodiment of the activation treatment is, for example, the application of a fluorine-containing compound to the surface of the previously selected support particles. It may consist in depositing silver seeds by reduction of silver ions in solution, the silver deposition being achieved by germination growth. This operation may be carried out, for example, by reduction of ammoniacal silver nitrate in a glycolic solution.

[0016] Another advantageous embodiment of the activation treatment may also consist in depositing, by physical vapour deposition (PVD), a thin layer of copper, less than 1 μm, on the surface of the previously selected support particles.

[0017] Once the support particles are activated, the actual metallization of the particles takes place (steps D-F).

[0018] The first step (step D) of metallizing the activated support particles is the autocatalytic chemical deposition of one or more copper layers, which is performed to obtain copper-coated support particles with a copper layer thickness E of 15 μm to 35 μm. cu is obtained. Multiple successive metallization operations may be necessary to obtain the desired copper thickness.

[0019] If it is desired that the solder balls are hollow or semi-hollow, it is possible to carry out either partial or complete dissolution, or partial or complete pyrolysis, of the expanded polystyrene (EPS) of the support particles during the metallization steps D to E. To achieve this, the copper layer then formed in step E must be sufficiently fine or sufficiently porous to allow the dissipation of the EPS.

[0020] The second step of metallization (step E) consists of metallizing the copper-coated support particles obtained at the end of step D) (optionally converted into hollow or quasi-hollow balls) by autocatalytic chemical deposition of at least one nickel layer alloyed with phosphorus NiP, with a mass percentage of phosphorus of 7-10% relative to the total weight of the NiP (or chemical nickel) layer. Said step E) comprises the deposition of a chemical nickel layer (111) of thickness E of 4 μm to 7 μm, in order to obtain chemical nickel-coated support particles. Ni This is carried out until

[0021] The third step of metallization (step F) is a thin film of thickness E from 0.05 μm to 0.12 μm. au The method comprises the metallization of the chemically nickel-coated support particles by immersion in a solution containing gold ions to obtain composite solder balls that are superficially metallized and coated with a gold topcoat.

[0022] Finally, the second step (step G) of the method according to the invention is to metallize the surface and to obtain a diameter D f This is the second step of granular sorting of the particles thus metallized to select and select the composite solder balls having

[0023] The invention also relates to solder balls obtainable by the manufacturing method according to the invention.

[0024] According to a first particularly advantageous embodiment of the invention, the solder balls may have the following characteristics: - diameter D0 of about 630 μm + / - 5%; - copper layer thickness Ecu of about 30 μm, - NiP layer thickness E of about 5 μm Ni , - Gold layer thickness E of 0.05μm to 0.12μm Au , - Diameter Df of approximately 700μm + / - 5%.

[0025] According to a second particularly advantageous embodiment of the invention, the solder balls may have the following characteristics: - diameter D0 of about 350 μm + / - 5% μm, - copper layer thickness Ecu of about 20 μm, - NiP layer thickness E of about 5 μm Ni , - Gold layer thickness E of approximately 0.1 μm Au , - Diameter Df of approximately 400μm + / - 5%.

[0026] Advantageously, the solder ball according to the invention may be a hollow (or semi-hollow) ball comprising a core made of more than 50% by volume of polymer material, if it is expanded polystyrene (EPS). Such a solder ball is obtained using a method according to the invention, which method comprises, in steps D) to E), a partial or complete melting step or a partial or complete pyrolysis step of the expanded polystyrene (EPS) creating the initial support particles.

[0027] The invention also relates to the use of the balls according to the invention for the assembly of electronic substrates. Indeed, the structure of the balls according to the invention makes it possible to implement interconnections between components that are sensitive to mechanical stresses (CBGA, MEMS, etc.). They have the further advantage of being able to maintain a controlled position and limit the mechanical stresses in the interconnections between the substrate and the components.

[0028] Other characteristics and advantages of the invention will become apparent from the following description, given by way of non-limiting example and with reference to the attached drawings, in which: [Brief description of the drawings]

[0029] [Figure 1] 1 is a schematic diagram of an example of a flexible ball known from the prior art, which includes contacts that are soldered for its assembly in an integrated circuit housing; [Diagram 2] 1 is a schematic diagram of an example of a flexible ball according to the present invention. [Diagram 3] 1 is a schematic diagram of an example of a flexible ball according to the present invention, with the gold surface layer not shown for clarity. [Figure 4] FIG. 3 is a photograph of an activated EPS ball (coated with a thin layer of silver) obtained at the end of activation step C) of the method according to the invention. [Diagram 5] 5 is a photograph of an activated EPS ball coated with a copper layer obtained at the end of copper metallization step D) of the method according to the invention. [Figure 6] FIG. 3 is a photograph of an activated EPS ball successively coated with copper and chemical nickel (NiP) layers obtained at the end of step E) of metallization with chemical nickel of the method according to the invention. [Figure 7] FIG. 3 is a photograph of a solder ball according to the invention, consisting of an activated EPS ball coated successively with copper, chemical nickel (NiP) and gold layers, obtained at the end of step F) of metallization with chemical nickel of the method according to the invention. [Figure 8]1 is an optical microscope image of a cross section of a ball according to the invention, showing the EPS support ball obtained at the end of a first embodiment of the method according to the invention, and successive layers of copper, chemical nickel, and gold (EPS ball with a diameter of about 655 μm and a copper layer thickness of 17 μm). [Figure 9] 1 shows a first optical microscope image (A) of a cross-section of a copper-coated EPS ball obtained at the end of step D) of a second embodiment of the method according to the invention (EPS ball with a diameter of 660 μm and a copper layer thickness of 15 μm) and a second optical microscope image (B) of a cross-section of a copper-coated EPS ball obtained at the end of step D) of a third embodiment of the method according to the invention (EPS ball with a diameter of 630 μm and a copper layer thickness of 31 μm). [Figure 10] Shown is a first optical microscope image A showing EPS-supported balls 10 having a size distribution D0 of 0.5 to 1 mm, and a second optical microscope image B showing EPS-supported balls 10 obtained after granulometric sorting selecting diameters of 0.63 to 0.66 mm. [Figure 11] Shown is a metallized ball 1 according to the invention, having a diameter of about 400 μm + / - 5%. [Figure 12] FIG. 1 is an SEM image showing a metallized ball 1 according to the present invention before heat treatment at 360° C. (A), and the SEM image shows a metallized ball 1 according to the present invention that has undergone a subsequent heat treatment at 360° C. for 20 minutes to verify the heat resistance of the ball (B). [Figure 13] FIG. 1 is an SEM image showing a ball with a high density polystyrene core that was metallized according to steps A-G of the method of the present invention and subjected to a subsequent heat treatment at 360° C. for 20 minutes to verify the heat resistance of the ball (B).

[0030] [Figure 1] is described in a presentation of known prior art. It shows, inter alia, a flexible ball having welded contacts 1, 2 which facilitate assembly. Figures 2 to 12 are described in more detail in the following examples, which illustrate the invention without limiting its scope. EXAMPLES

[0031] Equipment and Instruments Autocatalytic Chemical Deposition Equipment (for the deposition of copper and chemical nickel) -Mechanical screening equipment starting product -Expanded polystyrene (EPS) balls with diameters of 595μm to 665μm, - Expanded polystyrene (EPS) balls with a diameter of approximately 400 μm, - Chemical nickel (containing 7-10% by weight of P), -copper -silver nitrate, - Gold ions.

[0032] Characterization: Morphological analysis Optical microscopy observations are carried out on the surface ([Figures 4] to [Figures 7]) and cross-sections ([Figures 8] and [Figures 9]) using an optical microscope.

[0033] The observations in Figures 12 and 13 are obtained using a scanning electron microscope (SEM).

[0034] Example 1: Production of a solder ball according to the invention by a first embodiment of the method according to the invention, The solder balls according to the invention are developed from expanded polystyrene (EPS) balls according to a first embodiment of the method according to the invention. The manufacture is divided according to the following steps: -1) A first mechanical screening of the EPS balls 10 having a size distribution of 0.5 to 1 mm is carried out in order to keep only balls with a diameter of approximately 630 μm ([Figure 10]). -2) The surface of the EPS particles is then activated to allow good adhesion of the subsequent metallization treatment. Activated balls 10' are obtained by depositing silver seeds on the surface of the balls. The operation is carried out in a bath by reduction of silver nitrate. At the end of this treatment, balls 10' are obtained as shown in [Figure 4]. -3) The third step consists in carrying out a metallization process using copper. A copper layer 110 of 30 μm thickness Ecu is obtained by autocatalytic chemical deposition (see: [Fig. 2], [Fig. 3]). At the end of this process, a ball 10'' is obtained as shown in [Fig. 5] (surface view) or in part B of [Fig. 9] (cross-sectional view). The fourth step consists in depositing a 5 μm thick chemical nickel (NiP) layer 111 on the copper layer 110 (see Fig. 2, Fig. 3), and implementing said coating by autocatalytic chemical deposition. At the end of this process, a ball 10'' is obtained, as shown in Fig. 6. The final metallization layer is a gold topcoat 112 (see FIG. 2). After immersion of the chemical nickel-coated ball 10'' in a solution containing gold ions, a gold layer is thus deposited, the thickness of which is E Au is 0.05 μm to 0.12 μm (see FIG. 2). At the end of this process, a solder ball 1 as shown in FIG. 7 is obtained. - The final step is a diameter D of approximately 700 μm + / - 5% f This is a granular sorting of the balls to keep only the ball 1 according to the present invention.

[0035] Example 2: Manufacturing of the solder balls according to the invention by a second embodiment of the method according to the invention The solder balls according to the invention are formed in the same way as in Example 1, having a supporting ball of 660 μm diameter and a copper deposit of about 15-17 mm thickness (see FIGS. 8 and 9A).

[0036] Example 3: Manufacturing of solder balls according to the invention by a third embodiment of the method according to the invention The solder balls according to the invention are formed to a diameter D of about 400 μm + / - 5%. f To obtain the ball, the ball is formed in the same manner as in Examples 1 and 2 (see FIG. 12).

[0037] Example 4: Effect of heat treatment after sieving step SEM analysis (FIG. 12) shows a metallized and calibrated ball according to the present invention before (12a) and after (12b) heat treatment at 360° C. Note that the ball does not degrade / change after heat treatment, indicating its temperature stability.

[0038] Example 5 (Comparative) To establish a comparative analysis of the weight of the balls 3, a batch of balls (with diameter D0700μm+ / -5%) was formed according to steps A-G of the method according to the invention (Cu / NiP / Au metallization) and then subjected to a subsequent heat treatment (B) at 360°C for 20 minutes to verify the heat resistance of the balls. To achieve this, three different types of support balls were used: a first batch formed on the basis of expanded polystyrene balls (exhibiting a porosity of about 95%), - a second batch formed on the basis of cross-linked polystyrene balls (high density), and - The third batch formed on the basis of metal copper balls (high density).

[0039] For each batch, 1000 balls were removed and weighed. The following results were obtained and are summarized in Table 1 below. [Table 1]

[0040] The balls (first batch) formed according to the invention based on expanded polystyrene have a mass reduction factor of 1.7 to 9.4 compared to current solutions (high-density cores made of organic or metallic materials).

[0041] On the other hand, by using an EPS core (balls according to the invention, of the first batch) compared to balls obtained on the basis of a high density core (balls of the second and third batches), It is noted that the thermal stability of the balls improves. Indeed, it should be noted that from 360° C., the balls made on the basis of high density polystyrene (balls of the second and third batches) show behavioral defects with the appearance of “droplets” of organic material on the ball surface (FIG. 1). This phenomenon is not observed in the balls according to the invention made on the basis of expanded polystyrene (balls of the first batch).

Claims

1. Metallized on the surface, calibrated, diameter D f A method for manufacturing a composite solder ball (1) of the present invention, comprising the steps of: a core consisting of spherical support particles (10) of diameter D0 made of expanded polystyrene (EPS) and having an intergranular porosity of at least 50%; - covering said support particles (10) with a thickness E cu Copper coating, thickness E Ni and at least one nickel layer of thickness E Au and a shell (11) formed by a plurality of metal surface layers (110, 111, 112) including a gold topcoat of 1000 nm, the method comprising the steps of: A) a first step of providing support particles (10), followed by B) D 0 =D f- 2*(E Ni +E cu +E Au ) such that the diameter D 0 A first step of granulometric sorting of the support particles (10) consisting of a step of physical and / or mechanical separation of the support particles (10) having D 0 may be selected to be between 200 μm and 1000 μm; C) a step of activation treatment of the thus selected support particles (10) to obtain activated support particles (10'); D) A first step of metallization of said activated support particle (10') by autocatalytic chemical deposition of one or more copper layers, said step resulting in a copper thickness E of 15 to 30 μm to obtain a copper-coated support particle (10''). cu a first step, which is repeated until a copper coating (110) of E) a second step of metallization of said copper-coated support particle (10'') by autocatalytic chemical deposition of at least one nickel layer alloyed with phosphorus NiP having a mass percentage of phosphorus of 7-10% relative to the total weight of said NiP layer, said step being carried out until a thickness ENi of a chemical nickel layer (111) of 4 μm to 7 μm is obtained, in order to obtain a chemical nickel-coated support particle (10'''); F) Thickness E of 0.05 μm to 0.12 μm Au a third step of metallization of said support particles (10''') coated with chemical nickel, consisting of a step of gold deposition by a method of galvanic displacement implemented by immersion in an aqueous solution containing gold ions, so as to obtain composite solder balls metallized and coated on said surface with a gold topcoat of 1000 g; G) said surface is metallized and has a diameter D f a second step of granular sorting of said particles thus metallized to select and select composite solder balls (1) having

2. The step B) of granulometric selection of the support particles (10) comprises granulometric selection of the support particles (10) with a diameter D selected to be between 200 μm and 1000 μm. 0 2. The method of claim 1, further comprising mechanical sieving to screen and select said support particles (10) having

3. The mechanical sieving B) of the support particles (10) is followed by a heat treatment of the upper slices of the particles thus treated at a temperature of 100° C. to 120° C., and preferably 110° C. to 120° C., to reduce their size to the range D 0 The method of claim 2 , wherein the difference is greater than +5%.

4. 4. The method according to claim 1, wherein the activation treatment of the selected support particles (10) consists of depositing silver seeds on its surface by introduction into a bath of silver nitrate or by depositing a thin layer of copper of 1 μm or less on its surface by physical vapor deposition (PVD).

5. In steps D) to E), the expanded polystyrene (EP) used to prepare the support particles (10) is The method according to any one of claims 1 to 4, further comprising a partial or complete dissolution step of expanded polystyrene (EPS) or a partial or complete pyrolysis step of the expanded polystyrene (EPS) to produce the support particles (10).

6. A diameter D, metallized on said surface and calibrated, obtained by the method defined in any one of claims 1 to 5 for the assembly of electronic boards. f Use of the composite solder ball (10).

Citation Information

Patent Citations

  • Method of mounting conductive ball

    JP1998150263A

  • Method for plating fine particle, electrically conductive fine particle and connected structure

    JP2002322591A

  • Solder ball and component connecting structure using the same

    JP2003101207A

  • JPP6500583B