Steel materials

A steel material with a tailored chemical composition and microstructure addresses the challenge of balancing cold forgeability and fatigue strength, enhancing performance in steel components through optimized VCr precipitates and structural ratios.

JP7560802B1Active Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024541958
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-04-03
Filing Date
2024-04-02
Publication Date
2024-10-03
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

Existing steel materials used for cold forging and aging heat treatment either prioritize cold forgeability or fatigue strength, but not both simultaneously, leading to suboptimal performance in complex-shaped steel parts requiring high fatigue strength.

Method used

A steel material with a specific chemical composition and microstructure, including 0.03-0.25% C, 0.05-0.50% Si, 0.70-2.50% Mn, 0.05-0.70% Cr, 0.10-0.40% V, and controlled microstructural ratios of polygonal ferrite, martensite, bainite, and pearlite, along with VCr precipitates, to enhance both cold forgeability and fatigue strength.

Benefits of technology

The steel material achieves excellent cold forgeability and fatigue strength in steel components, reducing manufacturing costs and improving shape accuracy through a balanced microstructure and precipitate distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560802000001
    Figure 0007560802000001
  • Figure 0007560802000002
    Figure 0007560802000002
  • Figure 0007560802000003
    Figure 0007560802000003
Patent Text Reader

Abstract

Provided is a steel material which has excellent cold forgeability and which, when cold forged and aging treated to form a steel part, has excellent fatigue strength. The steel material according to the present disclosure contains, by mass%, C: 0.03 to 0.25%, Si: 0.05 to 0.50%, Mn: more than 0.70 to 2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.001 to 0.100%, Cr: 0.05 to 0.70%, V: more than 0.10 to 0.40%, and N: 0.002 to 0.015%. In the microstructure, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is composed of bainite and / or pearlite. In the polygonal ferrite, the number density of VCr precipitates having a circle equivalent diameter of 5 to 100 nm is 1000 to 5000 precipitates / μm 3 It is.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a steel material, and more particularly to a steel material that can be used as a material for steel parts manufactured by cold forging and aging heat treatment. [Background technology]

[0002] Steel parts for machine structural applications, such as automobile parts, industrial machinery parts, and construction machinery parts, are required to have a shape and high fatigue strength to perform a predetermined function. Steel materials, particularly steel materials for machine structures, are widely used as materials that satisfy the requirements for shape and fatigue strength. Examples of steel materials for machine structures include carbon steel materials for machine structures and alloy steel materials for machine structures.

[0003] In the process of manufacturing steel parts of a specified shape using steel as a raw material, plastic processing and machining are carried out. In plastic processing, intermediate parts are manufactured by plastically deforming the steel material using processes such as hot forging and cold forging. In machining, unnecessary parts of the steel material are removed by cutting using a lathe or drill.

[0004] When comparing plastic processing and machining, machining has higher processing accuracy than plastic processing. Therefore, machining is used to finish the shape of steel parts. On the other hand, machining involves removing part of the steel, resulting in a lot of steel loss and significant wear on the processing tools. Therefore, machining has higher processing costs than plastic processing. If the shape accuracy of plastic processing is improved, the part of the steel that is removed in the finishing machining can be reduced. Therefore, in order to reduce the manufacturing costs of steel parts, it is necessary to improve the shape accuracy of plastic processing.

[0005] As mentioned above, plastic processing is mainly classified into hot forging and cold forging. In hot forging, steel is forged while being heated to a high austenite temperature range. The strength of steel decreases at high temperatures. Therefore, in hot forging, steel can be subjected to large plastic deformation with a low load compared to cold forging. On the other hand, in the process of cooling steel to room temperature after plastically deforming it at high temperatures, the steel thermally shrinks and changes its shape due to phase transformation. Therefore, the shape accuracy of the intermediate parts produced is low. As a result, a large portion of the steel is removed in the next machining process, which increases costs.

[0006] On the other hand, in cold forging, steel is forged at room temperature. Since cold forging is less susceptible to thermal distortion, the shape of the intermediate parts produced can be closer to the final parts. This reduces machining costs. On the other hand, since the strength of steel is high at room temperature, cold forging requires forging machines and dies that can bear high loads. Therefore, steel for cold forging is required to have low strength (deformation resistance) against plastic deformation at room temperature, that is, excellent cold forgeability.

[0007] Incidentally, in order to increase the fatigue strength of steel parts, heat treatment is sometimes performed on the raw steel material (intermediate parts after forging). As a heat treatment, there is a method of performing quenching and tempering on the intermediate parts after forging. However, quenching and tempering increase the manufacturing cost. Furthermore, since thermal strain occurs in the intermediate parts during quenching and tempering, the shape accuracy of the intermediate parts decreases, and the cost of machining increases. Therefore, if quenching and tempering are performed after cold forging, the advantage of cold forging, that is, high shape accuracy can be obtained, is offset.

[0008] Therefore, as an alternative heat treatment method to quenching and tempering, a technique has been proposed in which aging heat treatment is performed after cold forging to increase the fatigue strength of steel parts. In aging heat treatment, heat treatment is performed in a low temperature range where phase transformation does not occur to generate precipitates, and the fatigue strength of the steel parts is increased by age hardening. Therefore, when steel parts are manufactured by performing cold forging and aging heat treatment using steel as a raw material, the shape accuracy can be increased in the manufacturing process to reduce manufacturing costs, and the fatigue strength of the steel parts can also be increased by age hardening.

[0009] A steel material suitable for use as a material for steel parts manufactured by performing cold forging and aging heat treatment is proposed in JP 2019-173168 A (Patent Document 1).

[0010] The steel material of Patent Document 1 is composed of, in mass%, C: 0.02 to 0.25%, Si: 0.005 to 0.50%, Mn: over 0.70 to 2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.005 to 0.050%, Cr: 0.02 to 0.70%, V: 0.02 to 0.30%, N: 0.003 to 0.030%, Nb: 0 to 0.10%, B: 0 to 0.005%, Ca: 0 to 0.005%, Bi: 0 to 0.10%, Pb: 0 to 0.20%, and the balance: Fe and impurities, wherein the total content of Cu, Ni, and Mo in the impurities is 0.05 mass% or less, and the Ti content in the above impurities is 0.005 mass% or less, and has a chemical composition that satisfies formula (1). In addition, in formula (1), [V precipitates] / [V content]≦0.50. In this steel material, the microstructure contains polygonal ferrite, bainite and / or pearlite. The area ratio of polygonal ferrite in the microstructure is 10 to 90%.

[0011] In Patent Document 1, a steel material containing V but suppressing the precipitation of V carbides (i.e., a steel material with a large amount of dissolved V) is used as a material, and aging heat treatment is performed after cold forging. As a result, V carbides are generated in the steel part by the aging heat treatment, and the durability ratio (fatigue strength / tensile strength) of the steel part is increased by age hardening.

[0012] In Patent Document 1, the cold forgeability of the steel is emphasized, and the hardness of the steel is assumed to be low. Therefore, although the durability ratio of the steel part is high, the fatigue strength may not be so high. Therefore, the steel disclosed in Patent Document 1 is effective as a material for steel parts of complex shapes that require high cold forgeability. On the other hand, it may not be an appropriate material for steel parts of not so complex shapes that require high fatigue strength.

[0013] In addition, a steel preform that increases the strength of steel parts that have been subjected to cold forging and aging heat treatment has been proposed in International Publication No. 2021 / 210557 (Patent Document 2).

[0014] The steel material of Patent Document 2 has, in mass%, C: 0.03 to 0.25%, Si: 0.02 to 0.50%, Mn: over 0.70 to 2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.005 to 0.050%, V: over 0.10 to 0.40%, N: 0.003 to 0.030%, Cr: 0 to 0.70%, Nb: 0 to 0.100%, B: 0 to 0.0100%, Cu: 0 to 0.30%, The steel material is composed of Ni: 0-0.30%, Ca: 0-0.0050%, Bi: 0-0.10%, Pb: 0-0.090%, Mo: 0-0.50%, Ti: 0-0.005%, Zr: 0-0.010%, Se: 0-0.10%, Te: 0-0.10%, rare earth elements: 0-0.010%, Sb: 0-0.10%, Mg: 0-0.0050%, W: 0-0.0050%, and the balance: Fe and impurities. The steel material further contains fine V precipitates, and [V in precipitates] / [V]≧0.30. Furthermore, the amount of diffusible hydrogen when hydrogen is charged by a cathodic hydrogen charging method is 0.10 ppm or more. In Patent Document 2, in order to obtain such fine V precipitates, in the cold forging process, cold working is performed from a first direction such that the processing strain amount is 0.05 or more, and then cold working is performed from a second direction different from the first direction such that the processing strain amount is 0.05 or more. By performing such a cold forging process, the strength of the steel material that has been subjected to aging heat treatment after cold forging is increased.

[0015] However, the fatigue strength of steel parts may be increased by other means than those described in Patent Document 2. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] JP 2019-173168 A [Patent Document 2] International Publication No. 2021 / 210557 Summary of the Invention [Problem to be solved by the invention]

[0017] An object of the present disclosure is to provide a steel material that has excellent cold forgeability and that has excellent fatigue strength when cold forged and subjected to aging heat treatment to form a steel part. [Means for solving the problem]

[0018] The steel material according to the present disclosure is Chemical composition, in mass%, C: 0.03-0.25%, Si: 0.05 to 0.50%, Mn: over 0.70~2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.001 to 0.100%, Cr: 0.05-0.70%, V: more than 0.10~0.40%, N: 0.002~0.015%, Nb: 0 to 0.100%, Ti: 0 to 0.050%, B: 0~0.0100%, Cu: 0-0.30%, Ni: 0-0.30%, Mo: 0-0.30%, Ca: 0 to 0.0050%, Bi: 0 to 0.100%, Pb: 0~0.090%, Zr: 0 to 0.010%, Se: 0~0.010%, Te: 0~0.010%, Rare earth elements: 0~0.010%, Mg: 0 to 0.0050%, W: 0~0.050% or less, Sn: 0 to 0.100%, and the balance being Fe and impurities, In the microstructure, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is bainite and / or pearlite, In the polygonal ferrite, the circle equivalent diameter is 5 to 100 nm, and the number density of VCr precipitates, which are precipitates containing V and Cr, is 1000 to 5000 pieces / μm 3 It is. Effect of the Invention

[0019] The steel material according to the present disclosure has excellent cold forgeability, and when subjected to cold forging and aging heat treatment to form a steel part, it has excellent fatigue strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present inventors conducted various investigations to solve the above-mentioned problems and obtained the following findings.

[0021] The present inventors first conducted a study from the viewpoint of chemical composition on a steel material that has excellent cold forgeability and has excellent fatigue strength when cold forged and aged to form a steel part as a raw material. As a result, the present inventors found that the steel material has, in mass%, C: 0.03-0.25%, Si: 0.05-0.50%, Mn: over 0.70-2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.001-0.100%, Cr: 0.05-0.70%, V: over 0.10-0.40%, N: 0.002-0.015%, Nb: 0-0.100%, Ti: 0-0.050%, B: 0-0.0100%, Cu: 0-0.30%, Ni: 0-0.30%, It was believed that excellent cold forgeability and excellent fatigue strength could be obtained with a chemical composition consisting of Mo: 0-0.30%, Ca: 0-0.0050%, Bi: 0-0.100%, Pb: 0-0.090%, Zr: 0-0.010%, Se: 0-0.010%, Te: 0-0.010%, rare earth elements (REM): 0-0.010%, Mg: 0-0.0050%, W: 0-0.050%, Sn: 0-0.100%, and the balance being Fe and impurities.

[0022] Therefore, the present inventors further investigated means for obtaining excellent cold forgeability and excellent fatigue strength from the viewpoint of the microstructure.

[0023] In order to improve the cold forgeability, it is effective to suppress the hardness of the steel material. If the area ratio of polygonal ferrite in the microstructure is high, the hardness of the steel material can be suppressed. On the other hand, if the area ratio of polygonal ferrite is too high, the hardness of the steel material becomes too low. In this case, sufficient fatigue strength cannot be obtained in the steel part after cold forging and aging heat treatment. In addition, since martensite is very hard, if martensite is generated in the microstructure, the cold forgeability is significantly reduced. On the other hand, although bainite and pearlite are hard structures, their effect on cold forgeability is low compared to martensite.

[0024] Taking the above into consideration, in the microstructure of a steel material satisfying the above-mentioned chemical composition, if the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is bainite and / or pearlite, sufficient cold forgeability can be obtained, and when the steel part is made into a steel part by cold forging and aging heat treatment, the fatigue strength of the steel part can be increased.

[0025] The present inventors further investigated factors that affect the fatigue strength of steel parts when cold forging and aging heat treatment are performed on steel materials. Fatigue strength shows a positive correlation with hardness. Therefore, it is considered that if the hardness of a steel part is high, the fatigue strength can also be increased. Therefore, factors that affect the hardness of steel parts manufactured by the above-mentioned manufacturing process were investigated. As a result, the present inventors considered that the hardness of a steel part is affected by the following three hardnesses. (1) Hardness of the steel material (2) Work hardening by cold forging (3) Age hardening by aging heat treatment

[0026] In the steel material of Patent Document 1, attention is focused on age hardening due to aging heat treatment, and the formation of V carbides in the steel material is suppressed in order to ensure the amount of V carbides formed during aging heat treatment.

[0027] On the other hand, the present inventors have considered further increasing the hardness (fatigue strength) of steel parts by utilizing not only age hardening through aging heat treatment but also work hardening through cold forging in order to increase the hardness of the steel parts.

[0028] To utilize the work hardening caused by cold forging, it is necessary to increase the dislocation density in the steel by cold forging. To increase the dislocation density, it is necessary to increase the number of sites that act as dislocation multiplication sources during cold forging. Precipitates of a certain size, such as cementite, function as dislocation multiplication sources. On the other hand, V carbide (VC) is of a very small size and does not function as a dislocation multiplication source.

[0029] Bainite and pearlite in the microstructure of the above-mentioned steel material contain cementite, which is a source of dislocation proliferation. Therefore, during cold forging, work hardening occurs in bainite and pearlite. On the other hand, polygonal ferrite does not contain cementite. Therefore, sufficient work hardening is difficult to occur.

[0030] Therefore, in this embodiment, a large number of VCr precipitates, which are precipitates containing V and Cr, are generated in the polygonal ferrite of the steel material. The VCr precipitates have a larger particle size than V carbides. If the VCr precipitates have a circle equivalent diameter of 5 to 100 nm, they function as a source of dislocation proliferation in the polygonal ferrite during cold forging. Furthermore, if VCr precipitates are used instead of V carbides, even if some VCr precipitates are generated in the steel material of the above-mentioned chemical composition, the amount of dissolved V can be secured to a certain extent. Therefore, V carbides or VCr precipitates can be generated using the dissolved V during aging heat treatment, and not only work hardening but also age hardening can be utilized.

[0031] Based on the above findings, the present inventors have investigated the appropriate amount of VCr precipitates capable of exhibiting work hardening and age hardening in the manufacturing process of the above-mentioned steel parts. As a result, in a steel material having the above-mentioned chemical composition, the number density of VCr precipitates having a circle equivalent diameter of 5 to 100 nm is set to 1000 to 5000 precipitates / μm 3 If this is the case, it has been found that in steel parts manufactured by carrying out cold forging and aging heat treatment, not only age hardening but also work hardening occurs, resulting in excellent fatigue strength.

[0032] The gist of the forged steel part according to the embodiment of the present invention, which was completed based on the above findings, is as follows.

[0033] [1] Chemical composition, in mass%, C: 0.03-0.25%, Si: 0.05 to 0.50%, Mn: over 0.70~2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.001 to 0.100%, Cr: 0.05-0.70%, V: more than 0.10~0.40%, N: 0.002~0.015%, Nb: 0 to 0.100%, Ti: 0 to 0.050%, B: 0~0.0100%, Cu: 0-0.30%, Ni: 0-0.30%, Mo: 0-0.30%, Ca: 0 to 0.0050%, Bi: 0 to 0.100%, Pb: 0~0.090%, Zr: 0 to 0.010%, Se: 0~0.010%, Te: 0~0.010%, Rare earth elements: 0~0.010%, Mg: 0 to 0.0050%, W: 0~0.050% or less, Sn: 0 to 0.100%, and the balance being Fe and impurities, In the microstructure, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is bainite and / or pearlite, In the polygonal ferrite, the circle equivalent diameter is 5 to 100 nm, and the number density of VCr precipitates, which are precipitates containing V and Cr, is 1000 to 5000 pieces / μm 3 That is, Steel material.

[0034] [2] The steel material according to [1], The chemical composition is, in mass%, Nb: 0.001 to 0.100%, Ti: 0.001 to 0.050%, B: 0.0001~0.0100%, Cu: 0.01-0.30%, Ni: 0.01 to 0.30%, Mo: 0.01 to 0.30%, Ca: 0.0001 to 0.0050%, Bi: 0.001 to 0.100%, Pb: 0.001~0.090%, Zr: 0.001 to 0.010%, Se: 0.001 to 0.010%, Te: 0.001 to 0.010%, Rare earth elements: 0.001~0.010%, Mg: 0.0001 to 0.0050%, W: 0.001 to 0.050% or less, and Sn: 0.001 to 0.100%, containing one or more selected from the group consisting of Steel material.

[0035] Hereinafter, the cold forging steel of this embodiment will be described in detail. Percentages relating to elements mean mass percent.

[0036] [Features of the steel material of this embodiment] The steel material of this embodiment satisfies the following characteristics 1 to 3. (Feature 1) Chemical composition, by mass%, is C: 0.03-0.25%, Si: 0.05-0.50%, Mn: over 0.70-2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.001-0.100%, Cr: 0.05-0.70%, V: over 0.10-0.40%, N: 0.002-0.015%, Nb: 0-0.100%, Ti: 0-0.050%, B: 0-0.0100%, Cu: 0- 0.30%, Ni: 0-0.30%, Mo: 0-0.30%, Ca: 0-0.0050%, Bi: 0-0.100%, Pb: 0-0.090%, Zr: 0-0.010%, Se: 0-0.010%, Te: 0-0.010%, rare earth elements (REM): 0-0.010%, Mg: 0-0.0050%, W: 0-0.050%, Sn: 0-0.100%, and the balance is Fe and impurities. (Feature 2) In the microstructure, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the balance is made up of bainite and / or pearlite. (Feature 3) In the polygonal ferrite, the circle equivalent diameter is 5 to 100 nm, and the number density of VCr precipitates, which are precipitates containing V and Cr, is 1000 to 5000 pieces / μm 3 It is. Features 1 to 3 will be explained below.

[0037] [(Feature 1) Chemical composition] The chemical composition of the steel material according to the embodiment of the present invention contains the following elements.

[0038] C: 0.03 to 0.25% Carbon (C) increases the fatigue strength of steel parts manufactured using steel as a raw material. Specifically, C generates bainite and / or pearlite, which are hard structures in the microstructure, to increase the fatigue strength of the steel parts. C also generates VCr precipitates to increase the fatigue strength of the steel parts. If the C content is less than 0.03%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the C content exceeds 0.25%, even if the contents of other elements are within the ranges of this embodiment, the strength of the steel material increases excessively and the cold forgeability decreases. Therefore, the C content is 0.03 to 0.25%. The lower limit of the C content is preferably 0.05%, more preferably 0.07%, and further preferably 0.09%. The upper limit of the C content is preferably 0.23%, more preferably 0.21%, and further preferably 0.20%.

[0039] Silicon: 0.05 to 0.50% Silicon (Si) enhances the fatigue strength of steel parts manufactured using steel as a raw material. If the Si content is less than 0.05%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Si content exceeds 0.50%, the strength of the steel material increases excessively, and therefore the cold forgeability decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Si content is 0.05 to 0.50%. The lower limit of the Si content is preferably 0.08%, more preferably 0.10%, and further preferably 0.12%. The upper limit of the Si content is preferably 0.45%, more preferably 0.43%, and further preferably 0.41%.

[0040] Mn: over 0.70~2.50% Manganese (Mn) enhances the hardenability of steel and generates bainite and pearlite, which are hard structures in the microstructure. Therefore, it enhances the fatigue strength of steel parts manufactured using the steel as a raw material. If the Mn content is 0.70% or less, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mn content exceeds 2.50%, the hardenability of the steel material becomes excessively high and martensite is formed, and in this case, even if the contents of other elements are within the ranges of this embodiment, the cold forgeability of the steel material decreases. Therefore, the Mn content is more than 0.70% to 2.50%. The lower limit of the Mn content is preferably 0.80%, more preferably 0.90%, and further preferably 1.00%. The upper limit of the Mn content is preferably 2.30%, more preferably 2.20%, and further preferably 2.10%.

[0041] P:0.035% or less Phosphorus (P) is an impurity. P segregates at grain boundaries and reduces the cold forgeability of steel. Therefore, the P content is 0.035% or less. The lower the P content, the better. However, excessive reduction in the P content increases the production cost. Therefore, in consideration of normal industrial production, the lower limit of the P content is preferably more than 0%, more preferably 0.001%, more preferably 0.005%, and even more preferably 0.010%. The upper limit of the P content is preferably 0.030%, more preferably 0.025%, and further preferably 0.020%.

[0042] S: 0.050% or less Sulfur (S) is an impurity. S combines with Mn to form MnS, which improves the machinability of steel. However, if the S content exceeds 0.050%, coarse MnS is generated. The coarse MnS reduces cold forgeability. Therefore, the S content is 0.050% or less. The S content is preferably as low as possible. However, excessive reduction in the S content increases the production cost. Therefore, in consideration of normal industrial production, the lower limit of the S content is preferably more than 0%, more preferably 0.001%, more preferably 0.005%, and even more preferably 0.010%. The upper limit of the S content is preferably 0.045%, more preferably 0.040%, further preferably 0.030%, and further preferably 0.020%.

[0043] Al: 0.001 to 0.100% Aluminum (Al) deoxidizes steel. If the Al content is less than 0.001%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Al content exceeds 0.100%, coarse Al-based inclusions such as Al oxides are formed in the steel material, and the coarse Al-based inclusions reduce the cold forgeability of the steel material. Therefore, the Al content is 0.001 to 0.100%. The lower limit of the Al content is preferably 0.005%, more preferably 0.010%, and further preferably 0.015%. The upper limit of the Al content is preferably 0.090%, more preferably 0.070%, still more preferably 0.050%, and still more preferably 0.040%. Note that, in the steel material of the present embodiment, the Al content means the total Al content.

[0044] Cr: 0.05~0.70% Chromium (Cr) improves the hardenability of steel material and promotes the formation of bainite and / or pearlite in the microstructure. Therefore, it increases the fatigue strength of steel parts manufactured using the steel material as a raw material. Cr also forms VCr precipitates in the steel material, and further forms VCr precipitates in the aging heat treatment process during the manufacturing process of the steel parts. This increases the fatigue strength of the steel parts. If the Cr content is less than 0.05%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cr content exceeds 0.70%, the hardenability of the steel material becomes excessively high, the area ratio of polygonal ferrite becomes too low, or the area ratio of martensite becomes too high, and in this case, even if the contents of other elements are within the ranges of this embodiment, the cold forgeability of the steel material decreases. Therefore, the Cr content is 0.05 to 0.70%. The lower limit of the Cr content is preferably 0.06%, more preferably 0.08%, and further preferably 0.10%. The upper limit of the Cr content is preferably 0.60%, more preferably 0.50%, and further preferably 0.30%.

[0045] V: More than 0.10~0.40% Vanadium (V) forms VCr precipitates in steel materials, and also forms VCr precipitates and / or V carbides during the aging heat treatment process in the manufacturing process of steel parts. This increases the fatigue strength of the steel parts. If the V content is 0.10% or less, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the V content exceeds 0.40%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the V content is more than 0.10% to 0.40%. The lower limit of the V content is preferably 0.12%, more preferably 0.14%, and further preferably 0.15%. The upper limit of the V content is preferably 0.38%, more preferably 0.35%, and further preferably 0.30%.

[0046] N: 0.002~0.015% Nitrogen (N) combines with V in the steel material to form V nitrides. V nitrides are thermodynamically more stable than VCr precipitates and are formed at high temperatures. Therefore, if V nitrides are formed, the amount of V available for forming VCr precipitates decreases. If the N content exceeds 0.015%, V nitrides are formed in excess. Therefore, even if the contents of other elements are within the ranges of this embodiment, the formation of VCr precipitates is insufficient, and the fatigue strength of the steel part decreases. On the other hand, a certain amount of V can dissolve in steel at high temperatures, so there is no need to reduce the N content to less than 0.002%. Therefore, the N content is 0.002 to 0.015%. The lower limit of the N content is preferably 0.003%, and more preferably 0.004%. The upper limit of the N content is preferably 0.012%, more preferably 0.010%, and further preferably 0.008%.

[0047] The balance of the chemical composition of the steel material of this embodiment is composed of Fe and impurities. Here, the impurities in the chemical composition refer to those that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, when the steel material is industrially manufactured, and are not intentionally contained, but are allowed within a range that does not adversely affect the steel material of this embodiment. The O (oxygen) content in the impurities is, for example, 0.0040% or less.

[0048] [About optional elements] The chemical composition of the steel material of this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of the following first to third groups. [Group 1] Nb: 0 to 0.100%, Ti: 0 to 0.050%, B: 0~0.0100%, Cu: 0-0.30%, Ni: 0 to 0.30%, and Mo: 0 to 0.30%, one or more selected from the group consisting of [Group 2] Ca: 0 to 0.0050%, Bi: 0 to 0.100%, and Pb: 0 to 0.090%, one or more selected from the group consisting of [Group 3] Zr: 0 to 0.010%, Se: 0~0.010%, Te: 0~0.010%, Rare earth elements: 0~0.010%, Mg: 0 to 0.0050%, W: 0 to 0.050%, and Sn: 0 to 0.100%, one or more selected from the group consisting of The first to third groups will be explained below.

[0049] [Group 1 (Nb, Ti, B, Cu, Ni and Mo)] The steel material of this embodiment may contain, in place of a portion of Fe, one or more elements selected from the group consisting of Nb: 0-0.100%, Ti: 0-0.050%, B: 0-0.0100%, Cu: 0-0.30%, Ni: 0-0.30%, and Mo: 0-0.30%. These elements are optional elements, and all of them increase the fatigue strength of a steel part manufactured using the steel material as a material.

[0050] Nb: 0 to 0.100% Niobium (Nb) is an optional element and may not be contained, that is, the Nb content may be 0%. When Nb is contained, that is, when the Nb content is more than 0%, Nb combines with C and / or N in the steel material to form Nb precipitates. The Nb precipitates increase the fatigue strength of steel parts through precipitation strengthening. Even if even a small amount of Nb is contained, the above effect can be obtained to some extent. However, if the Nb content exceeds 0.100%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Nb content is 0 to 0.100%. The lower limit of the Nb content is preferably 0.001%, more preferably 0.010%, and further preferably 0.020%. The upper limit of the Nb content is preferably 0.080%, more preferably 0.060%, and further preferably 0.050%.

[0051] Ti: 0 to 0.050% Titanium (Ti) is an optional element and may not be contained, that is, the Ti content may be 0%. When contained, that is, when the Ti content is more than 0%, Ti combines with N or C in the steel material to form Ti precipitates, thereby increasing the fatigue strength of the steel part. Even if even a small amount of Ti is contained, the above effect can be obtained to some extent. However, if the Ti content exceeds 0.050%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ti content is 0 to 0.050%. The lower limit of the Ti content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the Ti content is preferably 0.045%, more preferably 0.040%, and further preferably 0.030%.

[0052] B: 0~0.0100% Boron (B) is an optional element and may not be contained, that is, the B content may be 0%. When contained, that is, when the B content is more than 0%, B strengthens the grain boundaries of the steel material and increases the fatigue strength of the steel part. Even if even a small amount of B is contained, the above effects can be obtained to some extent. However, if the B content exceeds 0.0100%, the above effects become saturated, and if the B content exceeds 0.0100%, the raw material cost further increases and the manufacturability also decreases. Therefore, the B content is 0 to 0.0100%. The lower limit of the B content is preferably 0.0001%, more preferably 0.0005%, still more preferably 0.0010%, and still more preferably 0.0020%. The upper limit of the B content is preferably 0.0080%, more preferably 0.0060%, and further preferably 0.0050%.

[0053] Cu: 0-0.30% Copper (Cu) is an optional element and may not be contained, that is, the Cu content may be 0%. When contained, that is, when the Cu content is more than 0%, Cu improves the hardenability of the steel material and increases the fatigue strength of the steel part. Even if even a small amount of Cu is contained, the above effects can be obtained to a certain extent. However, if the Cu content exceeds 0.30%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cu content is 0 to 0.30%. The lower limit of the Cu content is preferably 0.01%, more preferably 0.05%, and further preferably 0.10%. The upper limit of the Cu content is preferably 0.28%, more preferably 0.25%, and further preferably 0.20%.

[0054] Ni: 0 to 0.30% Nickel (Ni) is an optional element and may not be contained, that is, the Ni content may be 0%. When contained, that is, when the Ni content is more than 0%, Ni improves the hardenability of the steel material and increases the fatigue strength of the steel part. Even if even a small amount of Ni is contained, the above effects can be obtained to a certain extent. However, if the Ni content exceeds 0.30%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ni content is 0 to 0.30%. The lower limit of the Ni content is preferably 0.01%, more preferably 0.05%, and further preferably 0.10%. The upper limit of the Ni content is preferably 0.28%, more preferably 0.25%, and further preferably 0.20%.

[0055] Mo: 0 to 0.30% Molybdenum (Mo) is an optional element and may not be contained, that is, the Mo content may be 0%. When contained, that is, when the Mo content exceeds 0%, Mo improves the hardenability of the steel material and increases the fatigue strength of the steel part. Even if even a small amount of Mo is contained, the above effects can be obtained to a certain extent. However, if the Mo content exceeds 0.30%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mo content is 0 to 0.30%. The lower limit of the Mo content is preferably 0.01%, more preferably 0.05%, and further preferably 0.10%. The upper limit of the Mo content is preferably 0.28%, more preferably 0.25%, and further preferably 0.20%.

[0056] [Group 2 (Ca, Bi and Pb)] The chemical composition of the steel material of this embodiment may further contain one or more elements selected from the group consisting of Ca: 0-0.0050%, Bi: 0-0.100%, and Pb: 0-0.090%, instead of a portion of Fe. These elements are optional elements, and all of them improve the machinability of the steel material.

[0057] Ca: 0 to 0.0050% Calcium (Ca) is an optional element and may not be contained, that is, the Ca content may be 0%. When contained, that is, when the Ca content is more than 0%, Ca improves the machinability of the steel material. Even if even a small amount of Ca is contained, the above effect can be obtained to a certain extent. However, if the Ca content exceeds 0.0050%, coarse CaO is generated, and in this case, the cold forgeability of the steel material is deteriorated even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ca content is 0 to 0.0050%. The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0005%, further preferably 0.0010%, and further preferably 0.0020%. The upper limit of the Ca content is preferably 0.0048%, more preferably 0.0045%, and further preferably 0.0040%.

[0058] Bi: 0 to 0.100% Bismuth (Bi) is an optional element and may not be contained, that is, the Bi content may be 0%. When contained, that is, when the Bi content exceeds 0%, Bi improves the machinability of the steel material. Even if even a small amount of Bi is contained, the above effect can be obtained to some extent. However, if the Bi content exceeds 0.100%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Bi content is 0 to 0.100%. The lower limit of the Bi content is preferably 0.001%, more preferably 0.010%, further preferably 0.020%, and further preferably 0.030%. The upper limit of the Bi content is preferably 0.090%, more preferably 0.080%, and further preferably 0.060%.

[0059] Pb: 0~0.090% Lead (Pb) is an optional element and may not be contained, i.e., the Pb content may be 0%. When contained, that is, when the Pb content is more than 0%, Pb improves the machinability of the steel material. Even if even a small amount of Pb is contained, the above effect can be obtained to some extent. However, if the Pb content exceeds 0.090%, the cold forgeability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Pb content is 0 to 0.090%. The lower limit of the Pb content is preferably 0.001%, more preferably 0.010%, further preferably 0.020%, and further preferably 0.040%. The upper limit of the Pb content is preferably 0.080%, more preferably 0.075%, and further preferably 0.070%.

[0060] [Group 3 (Zr, Se, Te, rare earth elements (REM), Mg, W, and Sn)] The chemical composition of the steel material of this embodiment may further contain, instead of a portion of Fe, one or more elements selected from the group consisting of Zr: 0-0.010%, Se: 0-0.010%, Te: 0-0.010%, rare earth elements (REM): 0-0.010%, Mg: 0-0.0050%, W: 0-0.050%, and Sn: 0-0.100%. These elements are optional elements, and any of them may be contained in the steel material as an impurity.

[0061] Zr: 0 to 0.010% Zirconium (Zr) is an impurity and may not be contained, that is, the Zr content may be 0%. When Zr is contained, that is, when the Zr content exceeds 0%, if the Zr content exceeds 0.010%, Zr forms coarse inclusions, and in this case, the fatigue strength of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Zr content is 0 to 0.010%. The Zr content is preferably as low as possible. However, excessive reduction in the Zr content increases the production cost. Therefore, the lower limit of the Zr content is preferably 0.001%. The upper limit of the Zr content is preferably 0.008%, more preferably 0.005%, and further preferably 0.002%.

[0062] Se: 0 to 0.010% Selenium (Se) is an impurity and may not be contained, that is, the Se content may be 0%. When contained, that is, when the Sn content exceeds 0%, if the Se content exceeds 0.010%, Se embrittles the steel material and reduces the fatigue strength of the steel part even if the contents of other elements are within the range of this embodiment. Therefore, the Se content is 0 to 0.010%. The Se content is preferably as low as possible. However, excessive reduction in the Se content increases the production cost. Therefore, the lower limit of the Se content is preferably 0.001%. The upper limit of the Se content is preferably 0.008%, more preferably 0.005%, and further preferably 0.002%.

[0063] Te: 0 to 0.010% Tellurium (Te) is an impurity and may not be contained, i.e. the Te content may be 0%. When contained, that is, when the Te content exceeds 0%, if the Te content exceeds 0.010%, Te embrittles the steel material and reduces the fatigue strength of the steel part even if the contents of other elements are within the range of this embodiment. Therefore, the Te content is 0 to 0.010%. The lower the Te content, the better. However, excessive reduction in the Te content increases the production cost. Therefore, the lower limit of the Te content is preferably 0.001%. The upper limit of the Te content is preferably 0.008%, more preferably 0.005%, and further preferably 0.002%.

[0064] Rare earth elements (REM): 0~0.010% Rare earth elements (REM) are impurities and may not be present, i.e. the REM content may be 0%. When contained, that is, when the REM content exceeds 0%, if the REM content exceeds 0.010%, REM forms coarse inclusions and reduces the fatigue strength of the steel material even if the contents of other elements are within the ranges of this embodiment. Therefore, the REM content is 0 to 0.010%. The REM content is preferably as low as possible. However, excessive reduction in the REM content increases the production cost. Therefore, the preferred lower limit of the REM content is 0.001%. The upper limit of the REM content is preferably 0.008%, more preferably 0.005%, and even more preferably 0.002%.

[0065] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc), which has atomic number 21, yttrium (Y), which has atomic number 39, and the lanthanides lanthanum (La), which has atomic number 57, to lutetium (Lu), which has atomic number 71. In this specification, the REM content refers to the total content of these elements.

[0066] Magnesium: 0 to 0.0050% Magnesium (Mg) is an impurity and may not be contained, that is, the Mg content may be 0%. When contained, that is, when the Mg content exceeds 0%, if the Mg content exceeds 0.0050%, Mg forms coarse inclusions, which reduces the fatigue strength of the steel material even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mg content is 0 to 0.0050%. The lower the Mg content, the better. However, excessive reduction in the Mg content increases the production cost. Therefore, the lower limit of the Mg content is preferably 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the Mg content is preferably 0.0040%, more preferably 0.0030%, and further preferably 0.0020%.

[0067] W: 0~0.050% Tungsten (W) is an impurity and may not be contained, that is, the W content may be 0%. When W is contained, that is, when the W content exceeds 0%, if the W content exceeds 0.050%, W reduces the cold forgeability of the steel material even if the contents of other elements are within the ranges of this embodiment. Therefore, the W content is 0 to 0.050%. The W content is preferably as low as possible. However, excessive reduction in the W content increases the production cost. Therefore, the lower limit of the W content is preferably 0.001%, more preferably 0.005%, and further preferably 0.010%. The upper limit of the W content is preferably 0.040%, more preferably 0.030%, and further preferably 0.020%.

[0068] Sn: 0 to 0.100% Tin (Sn) is an impurity and may not be contained, that is, the Sn content may be 0%. When contained, that is, when the Sn content exceeds 0%, if the Sn content exceeds 0.100%, Sn reduces the cold forgeability of the steel material even if the contents of other elements are within the ranges of this embodiment. Therefore, the Sn content is 0 to 0.100%. The Sn content is preferably as low as possible. However, excessive reduction in the Sn content increases the production cost. Therefore, the lower limit of the Sn content is preferably 0.001%, more preferably 0.005%, and even more preferably 0.010%. The upper limit of the Sn content is preferably 0.060%, more preferably 0.040%, and further preferably 0.020%.

[0069] [Feature 2: Microstructure] In the microstructure of the steel material of this embodiment, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the balance is made up of bainite and / or pearlite.

[0070] Polygonal ferrite is a soft phase and is effective for improving cold forgeability. However, there is a large difference in strength between polygonal ferrite and hard structures such as bainite and pearlite. When structures with large strength differences are mixed in the microstructure, cracks may occur during cold forging due to the strength difference. However, in the steel material of this embodiment, VCr precipitates are formed in the microstructure, and the VCr precipitates are also formed in the polygonal ferrite. Therefore, in the steel material of this embodiment, the VCr precipitates formed in the steel material can suppress the strength difference between the polygonal ferrite and the hard structure. As a result, even if the area ratio of the polygonal ferrite is high, the cold forgeability can be improved. The above effects can be sufficiently obtained if the area ratio of polygonal ferrite in the microstructure of the steel material is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is bainite and / or pearlite.

[0071] The lower limit of the area ratio of polygonal ferrite is preferably 32%, more preferably 34%, and further preferably 36%. The upper limit of the area ratio of polygonal ferrite is preferably 85%, more preferably 80%, more preferably 75%, more preferably 68%, more preferably 66%, and more preferably 64%.

[0072] In the microstructure, the remainder is bainite and / or pearlite. Bainite and pearlite have higher strength than polygonal ferrite. Therefore, bainite and pearlite increase the fatigue strength of steel parts manufactured using the steel material as a material. Furthermore, bainite and pearlite do not significantly reduce cold forgeability like martensite.

[0073] On the other hand, although martensite is a high-strength structure, as described above, it significantly reduces the cold forgeability of the steel material. Therefore, in the microstructure of this embodiment, it is preferable that the area ratio of martensite is as low as possible. Therefore, in this embodiment, the area ratio of martensite is 5% or less.

[0074] The upper limit of the area ratio of martensite is preferably 4%, more preferably 3%, more preferably 2%, more preferably 1%, and even more preferably 0%.

[0075] [Method for measuring the area ratio of each structure in a microstructure] The polygonal ferrite area ratio, the bainite area ratio and the pearlite area ratio in the microstructure of a steel material are measured by the following method.

[0076] The observation surface is a cross section parallel to the axial direction of the steel material and including the central axis of the steel material. A test piece including the observation surface is taken from the steel material. The observation surface of the test piece is mirror-polished. After mirror polishing, the observation surface is etched with 3% nital (ethanol + 3% nitric acid solution) to reveal the microstructure. Of the etched observation surface, an observation field including a R / 2 depth position from the surface of the steel material in the radial direction is observed with an optical microscope. The observation magnification is 400x, and there are five observation fields. In this specification, the R / 2 position of the steel material means the center position of the radius (=R) in the cross section (circular shape) perpendicular to the axial direction of the steel material. The center position of the radius also means a depth position from 3R / 8 to 5R / 8 from the surface of the steel material. The area of ​​each observation field is 58,800 μm 2 (280μm x 210μm).

[0077] In the observation field, polygonal ferrite has a different contrast and morphology from hard structures (bainite, pearlite, and martensite). Therefore, each structure is recognized as follows based on the contrast and morphology: White polygonal grains without internal structure are recognized as polygonal ferrite; A structure with a mixture of high-brightness white areas and low-brightness black areas in stripes is recognized as pearlite; A structure with a narrow plate-like or needle-like structure with black precipitates inside or at the boundary of the narrow plate-like or needle-like structure is recognized as bainite.

[0078] The area ratio of polygonal ferrite and the area ratios (%) of bainite and pearlite are determined in each of the five observation fields. For each structure, the arithmetic average values ​​of the five observation fields are taken as the polygonal ferrite area ratio (%), pearlite area ratio (%), and bainite area ratio (%).

[0079] In the steel material of this embodiment that satisfies Feature 1, martensite forms in gaps between bainite. Therefore, the bainite area ratio obtained by observation with an optical microscope at 400x magnification as described above also includes the area ratio of martensite, which will be described later. Therefore, the bainite area ratio (%) of the steel material of this embodiment is determined by subtracting the area ratio of martensite obtained by the method described later from the area ratio of bainite, which is the arithmetic average value of the five observation fields obtained by the above method.

[0080] Here, the area ratio of martensite in the microstructure of a steel material is measured by the following method.

[0081] The observation surface is a cross section parallel to the axial direction of the steel material and including the central axis of the steel material. A test piece including the observation surface is taken from the steel material. The observation surface of the test piece is mirror-polished. After mirror polishing, the observation surface is etched with 3% nital (ethanol + 3% nitric acid solution) to reveal the microstructure. The observation surface after etching is observed using a scanning electron microscope (SEM) equipped with a backscattered electron image detector, with an observation field including the R / 2 depth position from the surface of the steel material in the radial direction. The observation magnification is 1000 times, and there are five observation fields. The area of ​​each observation field is 10,800 μm 2 (120μm x 90μm).

[0082] Martensite is identified based on the contrast in the observation field. Specifically, in the backscattered electron image, martensite shows a brighter contrast than polygonal ferrite, bainite, and pearlite. Based on the contrast, the area ratio (%) of martensite is determined in each of the five observation fields. The arithmetic average of the area ratios of martensite in the five observation fields is defined as the area ratio (%) of martensite. As described above, the value obtained by subtracting the martensite area ratio from the bainite area ratio is defined as the bainite area ratio (%) in the microstructure of the steel material of this embodiment.

[0083] [(Feature 3) Number density of VCr precipitates] The steel material of the present embodiment further has a number density of VCr precipitates, which are precipitates containing V and Cr and have a circle equivalent diameter of 5 to 100 nm in the polygonal ferrite, of 1000 to 5000 precipitates / μm 3 It is.

[0084] Generally speaking, in the microstructure of steel, cementite, which acts as a source of dislocation proliferation, exists in bainite and pearlite, but polygonal ferrite does not contain cementite as a rule. Therefore, while work hardening occurs in bainite and pearlite through processing such as cold forging, work hardening does not occur in polygonal ferrite because there is no source of dislocation proliferation.

[0085] On the other hand, as described above, in the steel material of this embodiment, VCr precipitates are generated in the polygonal ferrite in the steel material. The VCr precipitates are coarse compared to V carbides (VC). The VCr precipitates, which are coarser than V carbides, become sites of dislocation multiplication sources during processing such as cold forging. Therefore, during cold forging, work hardening is also generated in polygonal ferrite due to the presence of VCr precipitates, in addition to the occurrence of work hardening in bainite and pearlite. Therefore, when a steel part is manufactured by performing cold forging and aging heat treatment using the steel material of this embodiment as a material, two hardening mechanisms, work hardening in the cold forging process by VCr precipitates and age hardening by precipitates (VCr precipitates and / or V carbides) generated during aging heat treatment, act to increase the hardness of the steel part. As a result, excellent fatigue strength is obtained in the steel part.

[0086] Specifically, VCr precipitates having a circle equivalent diameter of 5 to 100 nm function as a source of dislocation multiplication. Here, the number density of VCr precipitates having a circle equivalent diameter of 5 to 100 nm is referred to as the VCr precipitate number density ND. When the VCr precipitate number density ND is 1000 precipitates / μm 3 If the number density ND of VCr precipitates is less than 5000 / μm, the amount of VCr precipitates generated is insufficient. In this case, a steel part manufactured by performing a cold forging process and an aging heat treatment process using the steel material as a raw material does not have sufficient fatigue strength. 3 If the density exceeds 1000 to 5000 / μm, the steel material will not have sufficient cold forgeability. 3 It is.

[0087] The preferable lower limit of the VCr precipitate number density ND is 1100 particles / μm 3 and more preferably 1200 particles / μm 3 and more preferably 1300 particles / μm 3 and more preferably 1400 particles / μm 3 and more preferably 1500 particles / μm 3 It is. The preferred upper limit of the VCr precipitate density ND is 4900 particles / μm 3and more preferably 4500 particles / μm 3 and more preferably 4000 particles / μm 3 and more preferably 3800 particles / μm 3 and more preferably 3600 particles / μm 3 It is.

[0088] [Method for measuring VCr precipitate number density ND] The number density ND of VCr precipitates in polygonal ferrite can be measured by the following method using a scanning transmission electron microscope (STEM-EDS).

[0089] The R / 2 position of the steel material is the center of the circle, and a disk test piece with a diameter of 3 mm and a thickness of approximately 2 mm is taken from the steel material. The axial direction of the disk test piece is parallel to the axial direction of the steel material. Both sides (front and back) of the disk are polished using emery paper. At this time, the disk is polished so that the front surface is parallel to the back surface. One of the front and back surfaces of the disk is used as the observation surface. The observation surface is further polished to a mirror finish. The mirror-polished observation surface is further polished using colloidal silica as an abrasive.

[0090] Electron beam backscatter diffraction (EBSD) is performed on the polished observation surface to identify the crystal orientation of the parent phase. Based on the identified crystal orientation of the parent phase, the vertical direction (observation direction) of the observation surface of the thin film is determined to be the crystal orientation of the parent phase. <001> To obtain the crystal orientation, the disk specimen is processed by focused ion beam (FIB) processing to prepare a thin film sample for STEM.

[0091] In the FIB processing, a thin film sample for STEM is prepared by the lift-out method using a gallium (Ga) ion beam with an accelerating voltage of 30 kV.

[0092] The surface layer of the STEM thin film sample prepared using an ion beam with an accelerating voltage of 30 kV contains dislocation loops and amorphous structures, making it unsuitable for observing VCr precipitates of a few nm in size. Therefore, the surface of the STEM thin film sample is polished using an ion beam with a low accelerating voltage of 1 kV or less. Through the above manufacturing process, a STEM thin film sample with a thickness of approximately 100 nm is prepared.

[0093] The prepared thin film specimen is observed with the optical system of STEM. Specifically, the crystal orientation of the polygonal ferrite parent phase in the thin film specimen for STEM is <001> The thin film sample for STEM is tilted so that the incidence is on the zone axis of the sample. The observation magnification is set to 200,000 times, and the acceleration voltage is set to 300 kV. The detector is set under known high-angle annular dark-field (HAADF) conditions, known low-angle annular dark-field (LAADF) conditions, and known bright-field (BF) conditions, and a STEM photograph image of one observation field is taken for each of any five polygonal ferrite grains (a total of five STEM photograph images of observation fields). Note that the dislocation density is different between the polygonal ferrite grains and other structures. Therefore, the polygonal ferrite grains can be easily identified in STEM observation.

[0094] The area of ​​each observation field is 1000 nm × 1000 nm. In all observation fields, the thickness of the thin film sample for STEM is measured by the log-ratio method of electron energy loss spectroscopy (EELS).

[0095] A quantitative analysis of the chemical composition of three or more representative particles in five observation fields is performed using the EDS-ZAF method. In the chemical composition of each particle, if the total content of metal elements excluding Fe is taken as 100% by mass, the V content is 20% or more by mass, the Cr content is 5% or more by mass, and the total content of V and Cr is 60% or more, then the particle is recognized as a VCr precipitate.

[0096] The contrast of particles identified as VCr precipitates is identified. Particles in the observation field of view that have the same contrast as the identified contrast are identified as VCr precipitates. The circle equivalent diameter of each identified VCr precipitate is determined using a well-known image processing method. Of the identified VCr precipitates, the number of VCr precipitates with a circle equivalent diameter of 5 to 100 nm is determined. The VCr precipitate number density (particles / μm 3The arithmetic mean value of the VCr precipitate number density obtained in each observation field was taken as the VCr precipitate number density ND (particles / μm 3 )

[0097] [Effects of the steel material of this embodiment] The steel material of this embodiment satisfies Features 1 to 3. Therefore, the steel material of this embodiment has excellent cold forgeability. Furthermore, a steel part manufactured by carrying out a cold forging process and an aging heat treatment process using the steel material as a raw material has excellent fatigue strength.

[0098] [Shape and use of the steel material according to this embodiment] The steel material of this embodiment is, for example, a steel material having a circular cross section perpendicular to the axial direction, such as a steel bar or wire rod. The steel material of this embodiment is widely applicable to applications requiring cold forgeability and fatigue strength. The steel material of this embodiment is particularly applicable as a material for steel parts manufactured by carrying out a cold forging process and an aging heat treatment process using the steel material as a material. However, the steel material of this embodiment is not limited to the above applications.

[0099] [Manufacturing method] An example of a method for manufacturing the steel material of this embodiment will be described. The method for manufacturing the steel material described below is one example for manufacturing the steel material of this embodiment. Therefore, a steel material satisfying Features 1 to 3 may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing the steel material of this embodiment.

[0100] The method for manufacturing a steel material according to this embodiment includes the following steps. (Process 1) Material preparation process (Process 2) Hot processing process Each step will be described below.

[0101] [Material preparation process] In the material preparation process, a material satisfying Feature 1 is manufactured by the following method. Specifically, molten steel satisfying Feature 1 is manufactured using a converter, an electric furnace, or the like. Blooms are manufactured using the molten steel by a continuous casting method. Alternatively, ingots are manufactured using the molten steel by an ingot casting method. Through the above steps, a material (bloom or ingot) is prepared.

[0102] [Hot processing process] In the hot working step, hot working is performed on the raw material to produce a steel material. The hot working may be, for example, hot rolling or hot forging.

[0103] When the hot working is hot rolling, the hot working process includes, for example, a rough rolling process in which a material (bloom or ingot) is roughly rolled into a billet, and a finish rolling process in which the billet is finish rolled into a steel material.

[0104] The rough rolling process may, for example, include the following steps: After heating the material, the material is bloomed using a blooming mill. If necessary, the material is further rolled using a continuous rolling mill after blooming to produce a billet. The heating temperature in the rough rolling process is a known temperature, for example, 1050 to 1300°C.

[0105] In the finish rolling process, hot rolling is performed on the billet to produce a steel material. In the finish rolling process, for example, the following steps are performed. The billet produced in the rough rolling process is charged into a heating furnace and heated. The heated billet is used to perform finish rolling (hot rolling) in a finish rolling mill to produce a steel material. The steel material after finish rolling is cooled to produce the steel material of this embodiment. The heating temperature in the finish rolling process is a known temperature, for example, 1050 to 1250°C. In addition, when the steel material temperature (surface temperature of the steel material) at the exit side of the rolling stand that lastly rolled down in the finish rolling mill row in the finish rolling process is taken as the finish rolling temperature (°C), the finish temperature is, for example, 900 to 1100°C.

[0106] [Manufacturing conditions for hot processing] In the hot working process, the cooling process of the steel material after finish rolling satisfies the following conditions. (Condition 1) After the finish rolling, the holding time t at 900 to 800°C is set to 25 to 300 seconds. (Condition 2) The average cooling rate CR at 800 to 600°C is set to 0.6 to 4.0°C / s. Each condition will be explained below.

[0107] [(Condition 1) Retention time t] The steel material after the finish rolling is cooled, and nuclei of VCr precipitates are generated in the temperature range of 900 to 800 ° C. That is, the temperature range of 900 to 800 ° C. after the finish rolling is the temperature range in which VCr precipitates are generated. Therefore, in order to obtain an appropriate number density of VCr precipitates, the steel material is held for an appropriate holding time t in the temperature range of 900 to 800 ° C. after the finish rolling (the temperature range in which VCr precipitates are generated). If the holding time t is less than 25 seconds, the nuclei of VCr precipitates are not generated sufficiently. In this case, the number density ND of VCr precipitates is not obtained sufficiently in the manufactured steel material. On the other hand, if the holding time t exceeds 300 seconds, the nuclei of VCr precipitates grow and become coarse, and as a result, the number of generated nuclei is reduced. In this case, the number density ND of VCr precipitates is not obtained sufficiently in the manufactured steel material.

[0108] If the holding time t is 25 to 300 seconds, the steel material is held for an appropriate time in the temperature range of 900 to 800°C (the temperature range in which VCr precipitates form). As a result, a sufficient amount of VCr precipitate nuclei are formed, and the number density ND of the VCr precipitates in the manufactured steel material is 1000 to 5000 particles / μm. 3 It becomes.

[0109] [(Condition 2) Average cooling rate CR] If the average cooling rate CR in the temperature range of 800 to 600°C after the holding time t is less than 0.6°C / sec, the cooling rate is too slow. In this case, the VCr precipitates become coarse. As a result, in the manufactured steel, the number density ND of VCr precipitates with a circle equivalent diameter of 5 to 100 nm is 1000 precipitates / μm 3 It will be less than.

[0110] On the other hand, if the average cooling rate CR in the temperature range of 800 to 600°C exceeds 4.0°C / sec, the cooling rate is too fast. In this case, the amount of polygonal ferrite generated may be excessively small, the amount of bainite and / or pearlite generated may be excessive, or martensite may be excessively generated. Furthermore, VCr precipitates cannot grow sufficiently, and as a result, the number density ND of VCr precipitates having a circle equivalent diameter of 5 to 100 nm in the manufactured steel material is 1000 precipitates / μm. 3 It will be less than.

[0111] If the average cooling rate CR is 0.6 to 4.0°C / sec, an appropriate amount of polygonal ferrite is formed, and an appropriate amount of bainite and / or pearlite is formed, and the formation of martensite can be sufficiently suppressed. As a result, in the microstructure of the manufactured steel material, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is bainite and / or pearlite.

[0112] In the temperature range of 800 to 600°C, the nuclei of VCr precipitates formed in the temperature range of 900 to 800°C grow. If the average cooling rate CR in the temperature range of 800 to 600°C is 0.6 to 4.0°C / sec, the VCr precipitates grow to an appropriate size. Therefore, in the manufactured steel, the number density ND of VCr precipitates with a circle equivalent diameter of 5 to 100 nm is 1000 to 5000 precipitates / μm 3 It becomes.

[0113] When the hot working is hot forging, hot forging is performed on the raw material to produce the steel material. The heating temperature in hot forging is 1050 to 1300°C. When the temperature at the end of the final working (pressing) in hot forging is the finishing temperature, the finishing temperature is 900 to 1100°C. The cooling after hot forging satisfies the above-mentioned conditions 1 and 2.

[0114] The steel material of this embodiment is manufactured by the above-described manufacturing method.

[0115] [Method of manufacturing steel parts using the steel material of this embodiment as a material] When a steel part is manufactured by carrying out a cold forging step and an aging heat treatment step using the steel material of this embodiment as a raw material, the manufacturing method of the steel part may be a well-known manufacturing method. The manufacturing method of the steel part includes a cold forging step and an aging heat treatment step.

[0116] In the cold forging process, cold forging is performed on the steel material to produce an intermediate steel material. If the steel material is a steel bar or a wire rod, wire drawing may be performed before the cold forging process. The cold forging and wire drawing may be performed under well-known conditions.

[0117] In the aging heat treatment process, heat treatment is performed on the intermediate steel material. The heat treatment temperature and holding time in the aging heat treatment process may be well-known conditions. For example, the heat treatment temperature is 550 to 700°C, and the holding time at the heat treatment temperature is 20 to 120 minutes. EXAMPLES

[0118] The effect of one aspect of the steel material of this embodiment will be described more specifically with reference to an example. The conditions in the following example are an example of conditions adopted to confirm the feasibility and effect of the steel material of this embodiment. Therefore, the steel material of this embodiment is not limited to this example of conditions.

[0119] Steel materials having the chemical compositions shown in Tables 1A to 1D were produced by the following method.

[0120] [Table 1A]

[0121] [Table 1B]

[0122] [Table 1C]

[0123] [Table 1D]

[0124] In the "Chemical Composition" columns of Tables 1B and 1D, "-" means that the content of the corresponding element was below the impurity level. In all steels with test numbers shown in the tables, the O content was 0.0040% or less.

[0125] Molten steel of each test number was produced by vacuum melting, and a 50 kg ingot was produced. The produced ingot was used to produce steel. Specifically, hot working (hot forging) was performed on the ingot. The heating temperature in hot forging was 1200°C, and the finishing temperature was 1000°C. In the cooling process of the steel after hot forging, the holding time t (seconds) at 900 to 800°C and the average cooling rate CR (°C / second) at 800 to 600°C were as shown in Tables 2A and 2B. A steel (round bar) with a diameter of 24 mm was produced by the above manufacturing process.

[0126] [Table 2A]

[0127] [Table 2B]

[0128] [Evaluation test] The following evaluation tests were carried out on the round bar material (steel material) and the steel preforms that were the raw material for the steel preforms with each test number.

[0129] (Test 1) Microstructure observation test (Test 2) VCr precipitate number density ND measurement test (Test 3) Cold forgeability evaluation test (Test 4) Vickers hardness test on steel parts Each test will be explained below.

[0130] [(Test 1) Microstructure Observation Test] For the steel material of each test number, the structure in the microstructure was identified according to the above-mentioned [Method for measuring the area ratio of each structure in the microstructure]. As a result, in all test numbers, polygonal ferrite, bainite and / or pearlite were confirmed in the microstructure. In addition, martensite was also confirmed in some test numbers. Furthermore, for each test number, the area ratio (%) of polygonal ferrite, the area ratio (%) of pearlite, the area ratio (%) of bainite and the area ratio (%) of martensite were obtained. As a result of the test, in the microstructure, in all steel materials of the test numbers, the structure other than polygonal ferrite and martensite was bainite and / or pearlite. Tables 2A and 2B show the area ratio (%) of polygonal ferrite, the area ratio (%) of martensite, and the total area ratio (%) of the remainder (bainite and pearlite).

[0131] [(Test 2) VCr precipitate number density ND measurement test] For each test number, the VCr precipitate number density ND (number / μm 3 Tables 2A and 2B show the number density of VCr precipitates, ND (particles / μm 3 ) is shown.

[0132] [(Test 3) Cold forgeability evaluation test] From the steel material of each test number, multiple cylindrical test pieces with a diameter of 14 mm and a length of 21 mm were taken. The central axis of the cylindrical test pieces was coaxial with the central axis of the steel material. A compression test (cold forging) was performed at room temperature (25 ° C.) using the cylindrical test pieces. Specifically, the compression test was performed until the processing rate defined by formula (1) reached 70%. A compression test was performed on five cylindrical test pieces for each test number. The presence or absence of cracks in the cylindrical test pieces after the test was confirmed. Generally, the processing rate of cold forging is 70% or less. Therefore, if no cracks were generated in the steel material by the compression test at a processing rate of 70%, it was determined that excellent cold forgeability was obtained. Working ratio = (1-(length of cylindrical specimen after compression test / length of cylindrical specimen before compression test)) x 100 (1)

[0133] The presence or absence of cracks in the steel material after the compression test at a processing rate of 70% was confirmed by the following method. The five cylindrical test pieces after the compression test were observed for the presence or absence of cracks using a 5x magnifying glass. If no cracks of 0.5 mm or more in length were observed in any of the five cylindrical test pieces, it was determined that excellent cold forgeability was obtained without cracks (indicated as "E (Excellent)" in the "Cold Forgeability" column in Tables 2A and 2B). On the other hand, if cracks of 0.5 mm or more in length were confirmed in any one or more of the five cylindrical test pieces, it was determined that sufficient cold forgeability was not obtained (indicated as "B (Bad)" in the "Cold Forgeability" column in Tables 2A and 2B). Note that if sufficient cold forgeability was not obtained, Test 4 was not performed (indicated as "-" in the "Steel Part Vickers Hardness (HV)" column in Tables 2A and 2B).

[0134] [(Test 4) Vickers hardness test on steel parts] The steel material having each test number was used as a raw material, and the cold forging process and the aging heat treatment process were carried out to obtain steel parts, and the Vickers hardness of the steel parts was determined by the following method. Cold drawing simulating the cold forging process was performed on the steel material with a diameter of 24 mm for each test number in the following manner. A test piece for drawing with a diameter of 20 mm and a diameter of 16 mm at the tip was prepared from the steel material. The central axis of the test piece for drawing was coaxial with the central axis of the steel material. Bonder treatment was performed on the test piece for drawing, and a zinc phosphate coating for lubrication was formed on the surface of the test piece. Then, cold drawing was performed on the test piece for drawing using a die with a diameter of 17 mm. The cold drawing was performed in one pass, and the reduction in area was 28%. Aging heat treatment was performed on the test piece after cold drawing. The heat treatment temperature in the aging heat treatment was 600 ° C, and the holding time at the heat treatment temperature was 1 hour (60 minutes). Through the above manufacturing process, steel parts were manufactured using the steel material with each test number as the material.

[0135] As a simple evaluation of the fatigue strength of steel parts, the Vickers hardness, which is positively correlated with fatigue strength, was measured. Specifically, test pieces were taken with a cross section perpendicular to the central axis of the steel part of each test number as the test surface. A Vickers hardness test in accordance with JIS Z 2244-1:2020 was performed on the test surface of the test piece. The test force was 9.8N. The measurement positions were three arbitrary points near the central axis of the test surface. The arithmetic average value of the values ​​obtained at the three measurement positions was taken as the Vickers hardness (Hv) of the steel part of that test number. The Vickers hardness (Hv) of the obtained steel parts is shown in Tables 2A and 2B. When the Vickers hardness was 265HV or more, it was considered that excellent fatigue strength was obtained. When the Vickers hardness was less than 265HV, it was considered that sufficient fatigue strength was not obtained.

[0136] [Test Results] The test results are shown in Tables 1A to 1D, 2A, and 2B. The steel materials of test numbers 1 to 44 satisfied characteristics 1 to 3. Therefore, excellent cold forgeability was obtained. Furthermore, the steel parts that were subjected to cold forging and aging heat treatment had a Vickers hardness of 265HV or more, and excellent fatigue strength was obtained.

[0137] On the other hand, in test number 45, the C content was too high, and therefore sufficient cold forgeability was not obtained.

[0138] In test number 46, the C content was too low. Therefore, the area ratio of polygonal ferrite was too high. Furthermore, the number density of VCr precipitates was too low. Therefore, the Vickers hardness of the steel part subjected to cold forging and aging heat treatment was less than 265HV, and sufficient fatigue strength was not obtained.

[0139] In test number 47, the Si content was too high, and therefore sufficient cold forgeability was not obtained.

[0140] In test number 48, the Si content was too low, so that the steel part that had been subjected to cold forging and aging heat treatment had a Vickers hardness of less than 265 HV and did not have sufficient fatigue strength.

[0141] In test number 49, the Mn content was too high. As a result, the area ratio of polygonal ferrite was less than 30% and the area ratio of martensite exceeded 5%, so sufficient cold forgeability was not obtained.

[0142] In test number 50, the Mn content was too low, so that the steel part that had been subjected to cold forging and aging heat treatment had a Vickers hardness of less than 265 HV and did not have sufficient fatigue strength.

[0143] In test number 51, the Cr content was too high, so the area ratio of polygonal ferrite was less than 30%, and therefore sufficient cold forgeability was not obtained.

[0144] In test number 52, the Cr content was too low, and therefore the number density of VCr precipitates was too low, and therefore the steel part subjected to cold forging and aging heat treatment had a Vickers hardness of less than 265 HV, and sufficient fatigue strength was not obtained.

[0145] In test number 53, the V content was too high, so sufficient cold forgeability was not obtained.

[0146] In test number 54, the V content was too low, and therefore the number density of VCr precipitates was too low, and therefore the steel part subjected to cold forging and aging heat treatment had a Vickers hardness of less than 265 HV, and sufficient fatigue strength was not obtained.

[0147] In test numbers 55 to 59, the average cooling rate CR at 800 to 600 ° C after finish rolling was too slow. As a result, the number density of VCr precipitates was too low. Therefore, in the steel parts subjected to cold forging and aging heat treatment, the Vickers hardness was less than 265 HV, and sufficient fatigue strength was not obtained.

[0148] In test numbers 60 to 62, the average cooling rate CR at 800 to 600 ° C after finish rolling was too fast. Therefore, in test numbers 60 to 62, the area ratio of polygonal ferrite was too low, and in test numbers 60 and 61, the area ratio of martensite was too high. As a result, sufficient cold forgeability was not obtained in these test numbers. Furthermore, in these test numbers, the number density of VCr precipitates was too low.

[0149] In test numbers 63 to 65, the average cooling rate CR at 800 to 600°C after finish rolling was too fast, although not as fast as in test numbers 60 to 62. Therefore, the number density of VCr precipitates was too low in test numbers 63 to 65. Therefore, the Vickers hardness of the steel parts subjected to cold forging and aging heat treatment was less than 265HV, and sufficient fatigue strength was not obtained.

[0150] In test numbers 66 and 67, the holding time t at 900 to 800 ° C after finish rolling was too short. Therefore, the number density of VCr precipitates was too small in these test numbers. Therefore, the Vickers hardness of the steel parts subjected to cold forging and aging heat treatment was less than 265 HV, and sufficient fatigue strength was not obtained.

[0151] In test numbers 68 and 69, the holding time t at 900 to 800 ° C after finish rolling was too long. Therefore, the number density of VCr precipitates was too small in these test numbers. Therefore, the Vickers hardness of the steel parts subjected to cold forging and aging heat treatment was less than 265 HV, and sufficient fatigue strength was not obtained.

[0152] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.

Claims

1. The chemical composition, in mass%, is C: 0.03-0.25%, Si: 0.05-0.50%, Mn: more than 0.70 to 2.50%, P: 0.035% or less, S: 0.050% or less, Al: 0.001-0.100%, Cr: 0.05-0.70%, V: more than 0.10 to 0.40%, N: 0.002-0.015%, Nb: 0 to 0.100%, Ti: 0 to 0.050%, B: 0 to 0.0100%, Cu: 0 to 0.30%, Ni: 0 to 0.30%, Mo: 0 to 0.30%, Ca: 0-0.0050%, Bi: 0-0.100%, Pb: 0 to 0.090%, Zr: 0 to 0.010%, Se: 0 to 0.010%, Te: 0 to 0.010%, Rare earth elements: 0 to 0.010%, Mg: 0 to 0.0050%, W: 0 to 0.050% or less, Sn: 0 to 0.100%, and The balance is Fe and impurities, In the microstructure, the area ratio of polygonal ferrite is 30 to 90%, the area ratio of martensite is 5% or less, and the remainder is composed of bainite and / or pearlite, In the polygonal ferrite, the circle equivalent diameter is 5 to 100 nm, and the number density of VCr precipitates, which are precipitates containing V and Cr, is 1000 to 5000 precipitates / μm 3 That is, Steel material.

2. The steel material according to claim 1, The chemical composition is, in mass%, Nb: 0.001 to 0.100%, Ti: 0.001 to 0.050%, B: 0.0001 to 0.0100%, Cu: 0.01-0.30%, Ni: 0.01 to 0.30%, Mo: 0.01-0.30%, Ca: 0.0001-0.0050%, Bi: 0.001-0.100%, Pb: 0.001-0.090%, Zr: 0.001 to 0.010%, Se: 0.001 to 0.010%, Te: 0.001 to 0.010%, Rare earth elements: 0.001 to 0.010%, Mg: 0.0001 to 0.0050%, W: 0.001 to 0.050% or less, and Sn: 0.001 to 0.100%; Steel material.

Citation Information

Patent Citations

  • Steel for soft-nitriding, excellent in cold forgeability and pitting resistance

    JP1998306343A

  • Spring steel and spring, and methods of producing them

    JP2016113671A

  • Hot-rolled steel sheet for tailored rolled blank, tailored rolled blank, and method for producing these

    WO2015162932A1

  • Steel near-net-shape material and method for producing same

    WO2021210577A1

  • Steel material for cold forging

    JP2019173168A