Magnetic layered building surface material
The magnetic layer-equipped architectural facing material addresses the limitations of conventional building materials by enabling easy cutting and magnet attachment, ensuring adhesion and non-flammability, suitable for building applications.
Patent Information
- Application Number
- JP2020550228
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-05
- Filing Date
- 2019-09-05
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2039-09-05
AI Technical Summary
Conventional building materials with iron plates on their surfaces cannot be easily cut or processed, and construction methods that involve fixing steel plates on site increase man-hours, making them impractical for flexible use.
A magnetic layer-equipped architectural facing material containing a magnetic material and an inorganic binder, allowing for easy cutting and attachment of magnets, while maintaining non-combustibility and adhesion properties.
The material can attract magnets, be easily cut into any shape, and ensures high adhesion with wallpaper or paint, while providing improved non-flammability and stability, suitable for various building applications.
Smart Images

Figure 0007560819000007 
Figure 0007560819000008 
Figure 0007560819000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a building surface material with a magnetic layer. [Background technology]
[0002] Conventionally, there has been a need to fix printed matter, etc., to walls, etc., using magnetic materials such as magnets in, for example, school buildings, commercial facilities, etc. For this reason, there has been a demand for building materials that can attract magnets as building materials to be used when forming walls, etc.
[0003] A building material with thin steel plates on its surface was known to be capable of attracting magnets.
[0004] Furthermore, for example, Patent Document 1 discloses a bulletin board wall in which a thin iron plate is interposed between wallpaper and a base material, and which is capable of holding items by utilizing the attractive force of magnets. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japan Utility Model Publication No. 6-78983 Summary of the Invention [Problem to be solved by the invention]
[0006] However, building materials with steel plates arranged and fixed on their surfaces cannot be processed, for example by cutting.
[0007] One of the major advantages of architectural surface materials is that they can be easily cut or processed using a cutter or circular saw, etc., and can be cut into the desired shape at the construction site. However, there was a problem with building materials that have steel plates on the surface, in that this advantage was lost.
[0008] Furthermore, in the case of the bulletin board wall disclosed in Patent Document 1, construction work such as attaching a steel plate to the surface of the base material must be carried out on-site, but such construction work increases the number of labor hours required, which is problematic.
[0009] In view of the problems with the prior art described above, one aspect of the present invention aims to provide a building surface material with a magnetic layer that can attract magnets and can be easily cut into any shape. [Means for solving the problem]
[0010] In order to solve the above problems, according to one aspect of the present invention, a building surface material and and a magnetic layer covering at least a portion of the surface of the architectural facing material. The magnetic layer provides a building surface material with a magnetic layer, which contains a magnetic material and an inorganic binder. Effect of the Invention
[0011] According to one aspect of the present invention, it is possible to provide a building surface material with a magnetic layer that can attract a magnet and can be easily cut into any shape. [Brief description of the drawings]
[0012] [Figure 1] 1 is a perspective view of a building surface material with a magnetic layer according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of a magnet attraction test of a building surface material with a magnetic layer according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view of a wall structure according to an embodiment of the present invention. [Figure 4] FIG. 1 is a perspective view of a wall structure according to an embodiment of the present invention. [Diagram 5] FIG. 1 is an explanatory diagram of a method for evaluating the adhesive force of a magnet used in Experimental Example 1 to a 1 mm iron plate. [Figure 6] FIG. 2 is an explanatory diagram of a specimen for an adhesion test prepared in an adhesion test in Experimental Example 2. [Figure 7] FIG. 13 is an explanatory diagram for evaluation of rust occurrence in Experimental Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the form for carrying out the present invention will be described with reference to the drawings. However, the present invention is not limited to the following embodiment, and various modifications and substitutions can be made to the following embodiment without departing from the scope of the present invention. [Magnetic layered building surface material] An example of the configuration of the building surface material with a magnetic layer of this embodiment will be described.
[0014] The architectural facing material with a magnetic layer of this embodiment can have an architectural facing material and a magnetic layer covering at least a part of the surface of the architectural facing material. The magnetic layer can contain a magnetic material and an inorganic binder.
[0015] An example of the configuration of the building surface material with a magnetic layer of this embodiment will be specifically described below.
[0016] As shown in FIG. 1, a building surface material 10 with a magnetic layer of this embodiment can have a building surface material 11 and a magnetic layer 12 that covers at least a portion of the surface of the building surface material 11.
[0017] In the architectural surface material 10 with a magnetic layer shown in FIG. 1, an example is shown in which the magnetic layer 12 is formed on the entire surface of one main surface 11a of the architectural surface material 11, but the magnetic layer may be formed on a portion required to attract a magnetic body such as a magnet, and is not limited to this form. For example, the magnetic layer may be formed so as to cover a portion of the one main surface 11a. Also, the magnetic layer may be disposed not only on the one main surface 11a, but also on a portion or all of the other main surface 11b, or on a portion or all of the side surface.
[0018] The shape of the magnetic layer does not need to be a continuous surface shape, and may be, for example, a linear shape, a dot shape, etc. The architectural surface material with a magnetic layer of this embodiment may also have multiple discontinuous magnetic layers.
[0019] Each of the components contained in the building surface material with a magnetic layer of this embodiment will be described below.
[0020] The architectural surface material 11 is not particularly limited, and various architectural surface materials can be used. For example, fiber-reinforced cement board, glass mat gypsum board, glass fiber nonwoven fabric containing gypsum board, glass fiber mixed cement board, fiber mixed calcium silicate board, gypsum board specified by JIS A 6901 (2014), gypsum board that is lighter or heavier than the gypsum board specified by JIS A 6901 (2014) (hereinafter, the gypsum board specified by the above JIS and the gypsum board that is lighter or heavier than the gypsum board specified by JIS are also collectively referred to as "gypsum board"), gypsum board, slag gypsum board, and resin board. For this reason, the architectural surface material 11 is preferably, for example, a fiber-reinforced cement board, glass mat gypsum board, glass fiber nonwoven fabric containing gypsum board, glass fiber mixed cement board, fiber mixed calcium silicate board, gypsum board, gypsum board, slag gypsum board, or resin board.
[0021] The architectural surface material with a magnetic layer of this embodiment can be preferably used as a material for forming the walls of buildings. Since it is widely used as a wall material, the architectural surface material is preferably a gypsum board. The gypsum board here means a gypsum board defined in JIS A 6901 (2014) as described above, or a gypsum board that is lighter or heavier than the gypsum board defined in JIS A 6901 (2014). It is preferable that the gypsum board that is lighter than the gypsum board defined in JIS A 6901 (2014) has a specific gravity of 0.3 or more and less than 0.65.
[0022] The magnetic layer 12 can contain a magnetic material and an inorganic binder.
[0023] The magnetic layer 12 is a layer provided so as to be able to attract a magnetic body such as a magnet, and by containing a magnetic material, it is possible to attract a magnetic body such as a magnet.
[0024] The type of magnetic material contained in the magnetic layer 12 is not particularly limited, and various magnetic materials capable of attracting magnetic bodies such as magnets by magnetic force can be used. The magnetic material is preferably a material that can strongly attract magnetic bodies such as magnets with a small amount of addition, and is preferably a material that exhibits ferromagnetism at least at the environmental temperature when the architectural surface material with a magnetic layer is used. The environmental temperature when the architectural surface material with a magnetic layer is used can be, for example, a temperature range of -20°C to 50°C. The material exhibiting ferromagnetism here means a material (substance) that has a magnetic moment as a whole, and means a material that has spontaneous magnetization even in an environment without an external magnetic field. For this reason, the material exhibiting ferromagnetism also includes ferrimagnetic materials and the like.
[0025] As the magnetic material, iron powder is particularly preferred because it is particularly low cost and has excellent stability. The type of iron powder is not particularly limited, but for example, one or more types selected from iron oxide powder, reduced iron powder, and atomized iron powder can be suitably used. In particular, when iron powder is used as the magnetic material, it is preferable that the magnetic material contains atomized iron powder.
[0026] The particle size of the magnetic material is not particularly limited, and any particle size of magnetic material can be used. For the magnetic layer of the magnetic layer-attached architectural surface material of this embodiment, it is preferable to use a magnetic material with a particle size that is generally used, and for example, a magnetic material with an average particle size of 20 μm or more and 200 μm or less can be suitably used.
[0027] In this specification, the average particle size refers to the particle size at an integrated value of 50% in the particle size distribution determined by a laser diffraction / scattering method, and is the average particle size on a volume basis, that is, the volume average particle size.
[0028] The ratio of the magnetic material contained in the magnetic layer is not particularly limited, and can be selected arbitrarily depending on, for example, the magnetic property of the magnetic material and the magnetic body adsorption ability required for the architectural surface material with a magnetic layer. For example, the magnetic layer has a magnetic material content per unit area of 0.3 kg / m 2 This means that the content of the magnetic material in the magnetic layer per unit area is preferably 0.3 kg / m or more. 2 By setting the content of the magnetic material in the magnetic layer to 0.8 kg / m or more, it is possible to make the magnetic material such as a magnet adhere to the surface of the architectural surface material with a magnetic layer with sufficient adhesion. In particular, from the viewpoint of increasing the adhesion of the magnetic material such as a magnet, the content of the magnetic material in the magnetic layer per unit area is set to 0.8 kg / m or more. 2 More preferably, it is 1.0 kg / m or more. 2 More preferably, it is equal to or greater than this.
[0029] The upper limit of the content per unit area of the magnetic material in the magnetic layer is not particularly limited, and can be arbitrarily selected depending on, for example, the magnetic property of the magnetic material, the adhesive force required for the architectural surface material with a magnetic layer, the cost, etc. The content per unit area of the magnetic material in the magnetic layer is, for example, 10 kg / m 2 It is preferable that:
[0030] In addition, in the content per unit area of the magnetic material in the magnetic layer, the unit area refers to the unit area of the surface of magnetic layer 12 opposite the surface facing building surface material 11.
[0031] The density of the magnetic layer is 2.0 g / cm 3 It is preferable that the content is 2.5 g / cm or more. 3 This is more preferable when the density of the magnetic layer is 2.0 g / cm or more. 3 By setting the above, the magnetic attraction force can be particularly increased, and the magnetic layer can more reliably attract magnetic material such as a magnet.
[0032] The upper limit of the density of the magnetic layer is not particularly limited, and can be selected as desired depending on, for example, the adhesive force and cost required for the architectural surface material with a magnetic layer. The density of the magnetic layer is, for example, 5.0 g / cm 3 It is preferable that:
[0033] The inorganic binder contained in the magnetic layer is not particularly limited, and various inorganic binders can be used. By using an inorganic binder, it is possible to improve non-combustibility compared to the case of using an organic binder. Therefore, for example, the architectural surface material with a magnetic layer of this embodiment can satisfy the non-combustibility performance by providing only one magnetic layer. In addition, by using an inorganic binder, it is possible to suppress oxidation of the magnetic material and increase the stability of the magnetic material.
[0034] As the inorganic binder, for example, one or more types selected from inorganic silicate-based, phosphate-based, silica sol-based, and the like can be preferably used.
[0035] As described above, by using an inorganic binder in the magnetic layer, the non-combustibility of the architectural surface material with a magnetic layer can be improved compared to the case of using an organic binder. For this reason, it is preferable not to use an organic binder as the binder of the magnetic layer, and it is preferable that the magnetic layer does not contain an organic binder. Among inorganic binders, inorganic silicate-based binders also function as flame retardant materials, so inorganic silicate-based binders can be preferably used in applications where increased non-combustibility is particularly required. As the inorganic silicate-based binder, for example, an alkali metal silicate-based binder can be preferably used.
[0036] The content of the inorganic binder contained in the magnetic layer is not particularly limited and can be selected as desired depending on the strength required of the magnetic layer, etc. The magnetic layer preferably contains the inorganic binder in an amount of 1 part by mass to 35 parts by mass, and more preferably contains the inorganic binder in an amount of 1 part by mass to 15 parts by mass, per 100 parts by mass of the magnetic material.
[0037] This is because by making the content of the inorganic binder 1 part by mass or more per 100 parts by mass of the magnetic material, the magnetic layer can be made into a uniform film shape, and furthermore, the adhesion with the underlying architectural surface material can be improved. Also, by making the content of the inorganic binder 35 parts by mass or less per 100 parts by mass of the magnetic material, the occurrence of cracks in the magnetic layer can be suppressed. Although the cause of the occurrence of cracks in the magnetic layer is not clear, it is presumed that if the content ratio of the inorganic binder becomes too high, the shrinkage amount of the entire magnetic layer increases when the magnetic material-containing coating material, which is the raw material of the magnetic layer, hardens.
[0038] The magnetic layer may contain any optional components in addition to the magnetic material and inorganic binder.
[0039] The magnetic layer may also contain, for example, further inorganic additives.
[0040] The inorganic additive is preferably one or more selected from talc, gypsum, calcium carbonate, magnesium oxide, magnesium hydroxide, aluminum oxide, barium sulfate, kaolin, and the like.
[0041] By adding inorganic additives, the fluidity of the coating material containing magnetic material used when forming the magnetic layer can be increased, and the surface of the magnetic layer can be made particularly smooth. In addition, since the inorganic additives exemplified above are all white-colored materials, by containing the inorganic additives in the magnetic layer, or by further containing the pigment described below, the magnetic layer surface of the architectural surface material with magnetic layer can be made closer to white.
[0042] The particle size of the inorganic additive used is not particularly limited, but for example, the average particle size is preferably from 0.1 μm to 50 μm, and more preferably from 1 μm to 30 μm.
[0043] When an inorganic additive is added, the amount of the inorganic additive contained in the magnetic layer can be selected according to the type of inorganic additive used, particle size, etc., and is not particularly limited. When the magnetic layer contains an inorganic additive, for example, the inorganic additive is preferably contained in a ratio of 0.5 parts by mass to 30 parts by mass to 100 parts by mass of the magnetic material, more preferably 1 part by mass to 20 parts by mass to 100 parts by mass of the magnetic material, and even more preferably 5 parts by mass to 10 parts by mass to 10 parts by mass to 100 parts by mass of the magnetic material. If the content of the inorganic additive is less than 0.5 parts by mass or more than 30 parts by mass to 100 parts by mass of the magnetic material, the fluidity of the magnetic material-containing coating material used to form the magnetic layer may decrease. If the fluidity of the magnetic material-containing coating material decreases, pinholes, which are traces of air bubbles, may occur in the magnetic layer. Even if pinholes occur in the magnetic layer, there is no change in the magnetic attraction force of the magnetic layer, but there is a risk of impairing the aesthetic appearance when the surface is finished with paint. On the other hand, by setting the content of the inorganic additive to 0.5 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the magnetic material as described above, the occurrence of pinholes in the magnetic layer can be particularly suppressed, which is preferable.
[0044] The magnetic layer may also contain an anti-rust agent, which can particularly prevent the magnetic material contained in the magnetic layer from being oxidized and discolored, or prevent changes in the adsorptive power of magnetic bodies such as magnets.
[0045] If the magnetic layer contains a rust inhibitor, its content is not particularly limited; however, depending on the components of the rust inhibitor and the amount added, it may react with the inorganic binder and gel, so it is preferable to add it within a range that does not affect other components.
[0046] When the magnetic layer contains a rust inhibitor, the magnetic layer preferably contains the rust inhibitor in a proportion of 0.1% by mass or more, and more preferably 0.3% by mass or more, relative to the magnetic material.
[0047] When the magnetic layer contains a rust inhibitor, the upper limit of its content is not particularly limited, but adding an excessive amount does not significantly change the rust-preventing effect and may reduce the strength of the magnetic layer. For this reason, it is preferable that the magnetic layer contains the rust inhibitor in a proportion of, for example, 20% by mass or less relative to the magnetic material.
[0048] The type of rust inhibitor is not particularly limited, but it is preferable that the rust inhibitor includes at least one type selected from, for example, water-soluble or emulsion organic acid-based rust inhibitors, chelate-based rust inhibitors, organic acid amine-based rust inhibitors, fatty acid-based rust inhibitors, and nitrite-based rust inhibitors.
[0049] However, the magnetic layer-attached architectural surface material of this embodiment can suppress oxidation of the magnetic material and increase the stability of the magnetic material by using an inorganic binder as described above, so the magnetic layer of the magnetic layer-attached architectural surface material of this embodiment does not need to contain a rust inhibitor.
[0050] The magnetic layer may also contain any other additives, such as a thickener, an antifoaming agent, one or more pigments selected from titanium oxide, white lead, zinc oxide, lithopone, etc., to adjust the color of the magnetic layer, and a filler (bulking material).
[0051] If the Hunter whiteness (Wb) of the surface of the magnetic layer measured by a color difference meter exceeds 25, for example, when wallpaper is placed on the surface of a building surface material with a magnetic layer to give a wallpaper finish or paint is applied to give a paint finish, the color of the magnetic layer is less likely to show through the surface of the finishing material, which is preferable. For this reason, it is preferable to adjust the color of the magnetic layer by adding, for example, the inorganic additives already described, or, in some cases, the pigments described above, so that the Hunter whiteness (Wb) of the surface of the magnetic layer is greater than 25. In particular, when iron powder is used as the magnetic material and the magnetic layer does not contain inorganic additives or pigments, the Hunter whiteness (Wb) of the magnetic layer surface is about 3, so it is preferable to add inorganic additives or pigments to the magnetic layer to adjust the color, as described above. According to the study by the inventors of the present invention, for example, when 0.5 parts by mass of talc, which is an inorganic additive, and 2 parts by mass of titanium oxide, which is a pigment, are added to 100 parts by mass of iron powder contained in the magnetic layer, the Hunter whiteness (Wb) is about 30. For this reason, when the magnetic layer contains iron powder, it preferably contains 0.5 parts by mass or more of an inorganic additive such as talc and 2 parts by mass or more of a pigment such as titanium oxide per 100 parts by mass of iron powder.
[0052] As described above, the magnetic layer of the architectural surface material with a magnetic layer of this embodiment can contain any additive, but from the viewpoint of enhancing the non-combustibility of the architectural surface material with a magnetic layer of this embodiment, it is preferable to suppress the content of organic compounds in the magnetic layer. However, according to the study by the inventors of the present invention, if the content ratio of the organic compound in the magnetic layer to 100 parts by mass of the magnetic material is up to about 5 parts by mass, there is almost no change in the heat value of the architectural surface material with a magnetic layer, and the non-combustibility is not affected. For this reason, the content ratio of the organic compound in the magnetic layer is preferably 5 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, to 100 parts by mass of the magnetic material.
[0053] The organic compound contained in the magnetic layer is derived from any additive added to the magnetic layer. Therefore, the content ratio of the organic compound contained in the magnetic layer can be adjusted to a desired range by adjusting the content ratio of the organic compound in the additive added to the magnetic material-containing coating material used to form the magnetic layer.
[0054] The thickness of the magnetic layer 12 is not particularly limited, but is preferably, for example, 0.1 mm or more, and more preferably 0.3 mm or more.
[0055] There is no particular upper limit to the thickness of the magnetic layer 12, but it is preferable that the thickness be, for example, 5.0 mm or less, and more preferably 2.0 mm or less.
[0056] In the architectural facing material with a magnetic layer of this embodiment, the surface opposite to the surface of the magnetic layer facing the architectural facing material is preferably exposed. In other words, the surface opposite to the surface of the magnetic layer facing the architectural facing material preferably does not have any other layers, including a layer that enhances non-combustibility. This is because the architectural facing material with a magnetic layer of this embodiment has sufficiently enhanced non-combustibility due to the magnetic layer containing an inorganic binder. Therefore, there is no need to provide various layers to further enhance non-combustibility.
[0057] In addition, when using the architectural surface material with a magnetic layer of this embodiment to form a wall or the like, finishing materials such as wallpaper that are placed on the surface of the magnetic layer are not included in the other layers described above. Therefore, when these finishing materials are excluded, it is preferable that the architectural surface material with a magnetic layer of this embodiment has an exposed surface on the opposite side to the surface of the magnetic layer that faces the architectural surface material.
[0058] So far, the components contained in the architectural surface material with a magnetic layer of this embodiment have been described. Below, the characteristics of the architectural surface material with a magnetic layer of this embodiment will be described.
[0059] The building surface material with a magnetic layer of this embodiment preferably has a smooth surface.
[0060] Here, the surface (main surface) of the architectural surface material with a magnetic layer in this embodiment being smooth means that when the thickness of the architectural surface material with a magnetic layer is measured at multiple points, the thickness variation is 500 μm or less.
[0061] The thickness of the magnetic layered architectural surface material can be measured in the same manner as specified in "a) Thickness" of "7.3.1 Dimensions" of JIS A 6901 (2014). Specifically, the thickness can be measured at six equally spaced measurement positions within 25 mm from the end face of the magnetic layered architectural surface material sample and at least 80 mm inward from both sides. Therefore, if the variation in thickness at the six measured positions is 500 μm or less, the surface can be said to be smooth.
[0062] A smooth surface of the architectural surface material with a magnetic layer is preferable because it can form a flat wall when used as a wall material, for example. In addition, a smooth surface of the architectural surface material with a magnetic layer makes it easy to perform wallpapering (wallpaper finish) by sticking wallpaper, painting finish by applying paint, decorative finish such as lamination, decorative magnet finish by arranging decorative magnets, etc. Note that decorative magnet finish refers to finishing the surface of a wall by adhering wallpaper, decorative board, or decorative paper with a magnet arranged on one main surface to the architectural surface material with a magnetic layer with the magnet.
[0063] Moreover, the architectural surface material with a magnetic layer of this embodiment preferably has a thickness t that satisfies the standard JIS A 6901 (2014).
[0064] Meeting the JIS A 6901 (2014) standard means that the thickness of the architectural surface material with a magnetic layer falls within one of the following ranges: 9.5mm or more and 10.0mm or less, 12.5mm or more and 13.0mm or less, 15.0mm or more and 15.5mm or less, 16.0mm or more and 16.5mm or less, 18.0mm or more and 18.5mm or less, 21.0mm or more and 21.5mm or less, or 25.0mm or more and 25.5mm or less.
[0065] This is because, when the thickness t of the architectural surface material with a magnetic layer meets the standard of JIS A 6901 (2014), the thickness of the architectural surface material with a magnetic layer meets the same standard as the thickness of a normally used architectural surface material. For this reason, even if a wall or the like is formed by simultaneously using the architectural surface material with a magnetic layer of this embodiment and a normal architectural surface material, it is possible to easily form a flush wall without unevenness due to the type of architectural surface material used, that is, a flat wall, without adjusting the thickness, which is preferable.
[0066] It is more preferable that the thickness t of the architectural surface material with a magnetic layer, like more commonly used architectural surface materials, falls within any of the following ranges: 9.5 mm or more and 10.0 mm or less, 12.5 mm or more and 13.0 mm or less, 15.0 mm or more and 15.5 mm or less, or 21.0 mm or more and 21.5 mm or less.
[0067] The thickness t of the architectural surface material with a magnetic layer referred to here means the thickness of the entire architectural surface material with a magnetic layer, as shown in Fig. 1. For example, when the architectural surface material with a magnetic layer is composed of architectural surface material 11 and magnetic layer 12, such as architectural surface material with a magnetic layer 10 shown in Fig. 1, the sum of the thicknesses of architectural surface material 11 and magnetic layer 12 is the thickness t of the architectural surface material with a magnetic layer 10.
[0068] The thickness of architectural surface materials with a magnetic layer can be evaluated using the method specified in JIS A 6901 (2014).
[0069] The architectural surface material with a magnetic layer of this embodiment preferably meets the performance of quasi-noncombustible. That is, the architectural surface material with a magnetic layer of this embodiment is preferably recognized as a quasi-noncombustible material. The term "quasi-noncombustible" is defined in Article 1, item 5 of the Enforcement Order of the Building Standards Act. In order to be recognized as a quasi-noncombustible material, it is required that when exposed to heat from a normal fire, the material does not burn for 10 minutes after heating begins, that it does not cause deformation, melting, cracks or other damage that is harmful to fire prevention, and that it does not generate smoke or gas that is harmful to evacuation.
[0070] In addition, the magnetic layer-attached architectural surface material of this embodiment preferably satisfies the performance of noncombustibility. In other words, it is preferable that it is recognized as a noncombustible material. In addition, noncombustibility is stipulated in Article 2, item 9 of the Building Standards Act and Article 108, item 2 of the Enforcement Order of the Building Standards Act. In order to be recognized as a noncombustible material, it is required that when heat from a normal fire is applied, it does not burn for 20 minutes after the start of heating, that it does not cause deformation, melting, cracks or other damage that is harmful to fire prevention, and that it does not generate smoke or gas that is harmful to evacuation. The interior decoration restrictions of the Building Standards Act determine that the building materials that can be used are semi-noncombustible materials or noncombustible materials depending on the purpose and size of the building. The magnetic layer-attached architectural surface material of this embodiment can be adapted to the interior decoration restrictions required for the building in which it is used, that is, it can be a semi-noncombustible material or a noncombustible material, so it can be used in buildings of any purpose and size.
[0071] As described above, the magnetic layer-attached architectural surface material of this embodiment has enhanced non-combustibility by using an inorganic binder in the magnetic layer, but in some cases, in order to further enhance non-combustibility, a material that is less flammable can be selected for the architectural surface material and the magnetic layer material. Specifically, for example, for the architectural surface material on which the magnetic layer is arranged, an architectural surface material that satisfies semi-incombustible performance or an architectural surface material that satisfies incombustible performance can be used. By selecting these materials as necessary, an architectural surface material with a magnetic layer that satisfies semi-incombustible and incombustible performance can be obtained.
[0072] As described above, the architectural surface material with a magnetic layer of this embodiment is capable of attracting a magnetic body such as a magnet by disposing the magnetic layer. The magnetic attraction force is not particularly limited, but it is preferable that the magnetic attraction force satisfies, for example, the following magnetic attraction test characteristics.
[0073] First, as shown in Fig. 2, the architectural surface material 21 with a magnetic layer of this embodiment is set up so that the main surface 21a is vertical. Then, a single magnet 22 is used, the diameter of the magnet part being 17 mmφ, and the adhesive force to a 1 mm steel plate is 3.5 N. When a single A4 paper 23 is attached to the main surface 21a by the single magnet, it is preferable that the adhesive force is such that the A4 paper does not fall. Note that, here, setting up so that the main surface 21a is vertical means that the main surface of the architectural surface material 21 with a magnetic layer having a plate shape, i.e., the surface that attracts the magnet, is set up so that it is vertical to the horizontal direction of the ground or the like. Hereinafter, the same description has the same meaning.
[0074] It is also preferable that the architectural surface material with a magnetic layer has similar characteristics when wallpaper is placed on the main surface of the architectural surface material with a magnetic layer. That is, the architectural surface material with a magnetic layer 21 with wallpaper applied to the main surface 21a is stood so that the main surface 21a is vertical. Then, when a single magnet 22 having a diameter of 17 mmφ and an adhesive force of 3.5 N to a 1 mm steel plate is used and a single sheet of A4 paper 23 is attached to the main surface 21a with the single magnet, it is preferable that the adhesive force is such that the A4 paper 23 does not fall off.
[0075] When placing wallpaper on the main surface of the architectural surface material with a magnetic layer and carrying out a magnet adsorption test, the wallpaper may be, for example, a commonly used wallpaper with a thickness of 0.3 mm. For example, vinyl cloth or the like may be used as the wallpaper.
[0076] In addition, in all of the above magnetic adsorption tests, the thickness of A4 paper was 0.09 mm and the mass was 64 g / m 2 In this specification, not only in the present magnetic attraction test, but also in any other case, A4 paper having the above thickness and mass can be preferably used as the A4 paper.
[0077] When carrying out any of the above magnet attraction tests, the position of the magnetic layer is not particularly limited, but the architectural surface material with a magnetic layer of this embodiment exhibits sufficient attraction force to attract a magnet by providing the magnetic layer on at least a part of the surface of the architectural surface material. For this reason, it is preferable that the magnetic layer is provided at least on the part where the magnet 22 is to be placed.
[0078] In addition, the positions of the magnet 22 and the A4 paper 23 are not particularly limited, but it is preferable that the distance L between the center of the magnet 22 and the top end of the A4 paper 23 is 3 cm, and that the center of the magnet 22 is positioned in the center of the width of the A4 paper 23.
[0079] The architectural surface material with a magnetic layer of this embodiment has been described above, but the architectural surface material with a magnetic layer of this embodiment is capable of attracting magnetic bodies such as magnets by disposing a magnetic layer on at least a portion of the surface of the architectural surface material. In addition, since the magnetic layer is only disposed on at least a portion of the surface of the architectural surface material, it can be easily cut and processed into any shape.
[0080] In addition, in the case of conventional architectural facings in which an iron plate is arranged and fixed on the surface, the iron plate makes it difficult to drive in screws or nails, making it difficult to fasten the architectural facings, and there is also the problem that the adhesiveness of the wall covering or paint decreases when finishing with wallpaper or paint.
[0081] On the other hand, according to the architectural surface material with a magnetic layer of this embodiment, since the magnetic layer is only disposed on at least a part of the surface of the architectural surface material, nails, screws, etc. can be easily driven in. Furthermore, since the architectural surface material with a magnetic layer of this embodiment only has a magnetic layer disposed on at least a part of the surface of the architectural surface material as described above, it is possible to suppress the occurrence of cracks even when nails, screws, etc. are driven in. In addition, the adhesiveness to wallpaper and paint can be made sufficiently high. [Method of manufacturing architectural surface materials with magnetic layer] Next, a description will be given of one example of the method for manufacturing the architectural surface material with a magnetic layer of this embodiment. The architectural surface material with a magnetic layer described above can be manufactured by the method for manufacturing the architectural surface material with a magnetic layer of this embodiment. Therefore, some of the matters already described will be omitted.
[0082] The manufacturing method of the architectural surface material with a magnetic layer of this embodiment can include a magnetic layer formation step of applying a magnetic material-containing coating material containing a magnetic material and an inorganic binder to at least a portion of the surface of the architectural surface material to form a magnetic layer.
[0083] The magnetic material-containing coating material can be prepared by mixing the above-mentioned magnetic layer materials, specifically the magnetic material, an inorganic binder, and, if necessary, inorganic additives and optional additives such as rust inhibitors. When preparing the magnetic material-containing coating material, a dispersion medium such as water for adjusting viscosity can also be added and mixed as necessary.
[0084] The content per unit area of the magnetic material in the magnetic layer and the density of the magnetic layer can be adjusted, for example, by the particle size of the magnetic material contained in the magnetic material-containing coating material, and the content (content ratio) of various components such as the magnetic material, mixing water, and inorganic additives. In addition, when a filler (bulk-increasing material) is added to the magnetic material-containing coating material, it can also be adjusted by the amount (content) of the filler added. For example, aggregate can be used as the filler.
[0085] The raw materials used in the magnetic layer formation process and the suitable amounts of the raw materials added, the content per unit area of the magnetic material in the magnetic layer, the suitable range of density, etc. have already been described, so description thereof will be omitted.
[0086] In the magnetic layer forming process, the means and method for applying the magnetic material-containing coating material to at least a part of the surface of the architectural surface material are not particularly limited. However, it is preferable to apply the coating material so that the thickness of the magnetic layer to be formed is uniform. Therefore, in the magnetic layer forming process, it is preferable to apply the magnetic material-containing coating material to at least a part of the surface of the architectural surface material by using a roll coater, a flow coater, or a scraping method.
[0087] Here, the roll coater is a means for applying a magnetic material-containing coating material to a rotating roller, and forming a magnetic layer on the surface of the architectural surface material by the roller. Also, the flow coater is a means for flowing a magnetic material-containing coating material from above the architectural surface material being transported onto the surface of the architectural surface material in the form of a thin film, and forming a magnetic layer on the surface of the architectural surface material. Also, the scraping method is a means (method) for scraping the magnetic material-containing coating material supplied to the surface of the architectural surface material with, for example, a blade, and spreading it to the desired thickness on the surface of the architectural surface material to form a magnetic layer.
[0088] In addition, the building surface material to be supplied to the magnetic layer forming step may be masked in advance in areas where the magnetic layer is not to be formed, so that a magnetic layer having a desired pattern can be formed.
[0089] The method for producing a building surface material with a magnetic layer of this embodiment can include any optional step in addition to the above-mentioned magnetic layer forming step.
[0090] The manufacturing method for an architectural surface material with a magnetic layer of this embodiment may further include, as necessary, a drying step for drying the formed magnetic layer, and a cutting step for cutting the architectural surface material with a magnetic layer or the raw architectural surface material to any size.
[0091] The drying temperature in the drying step is not particularly limited, but is preferably, for example, 100° C. or less, and more preferably 70° C. or less. This is because keeping the drying temperature at 100° C. or less can prevent defects such as warping of the architectural surface material with a magnetic layer and cracks in the magnetic layer.
[0092] The lower limit of the drying temperature is not particularly limited, but from the viewpoint of productivity, it is preferably 20° C. or higher, and more preferably 30° C. or higher. [Wall structure] Next, an example of the configuration of a wall structure using the architectural surface material with a magnetic layer described above will be described with reference to Figures 3 and 4. Figure 3 shows a cross-sectional view of a partition wall, which is a wall structure, taken along a plane parallel to the height direction and perpendicular to the main surface of the wall, and Figure 4 shows a perspective view of the partition wall. Note that in Figure 4, the ceiling light steel base and the like shown in Figure 3 are omitted in order to make the structure of the partition wall easier to understand.
[0093] The wall structure of this embodiment may include the above-mentioned architectural surface material with a magnetic layer. Specific configuration examples are shown below.
[0094] The partition wall 30 shown in FIG. 3 is constructed on a reinforced concrete floor slab F1. The lower end of the partition wall 30 is fixed to the floor slab F1, and the upper end of the partition wall 30 is fixed to a reinforced concrete floor slab F2 on the upper floor. The framework of the partition wall 30 is composed of steel studs 31, floor runners 321, and upper runners (ceiling runners) 322. The studs 31 are made of channel-shaped members made of light-weight steel, and the floor runners 321 and upper runners 322 are made of light-weight channel steel. The dotted lines in FIG. 3 indicate the inner walls of the studs 31. The floor runners 321 and upper runners 322 are fixed to the floor slabs F1 and F2, respectively, by fasteners 33 such as anchor bolts, and the lower and upper ends of the studs 31 are fastened to the floor runners 321 and upper runners 322, respectively. The studs 31 are aligned in the wall core direction at predetermined intervals (eg, 455 mm intervals) set to a dimension of about 300 to 600 mm, and are installed vertically between the floor slabs F1, F2.
[0095] The underlay board 34 is attached to both sides of the stud 31 with screws 35, and the overlay board 36 is fixed to the surface of the underlay board 34 with one or more fasteners 37 such as staples and adhesives. As the underlay board 34, a non-combustible building material board such as a gypsum board defined in JIS A 6901 (2014), a gypsum board that is lighter or heavier than the gypsum board, a gypsum board, a hard gypsum board, a glass fiber reinforced gypsum board, or a calcium silicate board can be suitably used. Note that in FIG. 3, the screws 35 are partially omitted for convenience of illustration.
[0096] A surface finishing material 38 such as paint or wallpaper is applied to the surface of the upper board 36.
[0097] A heat insulating material 39 such as glass wool or rock wool can be placed inside the partition wall 30. A floor finishing material 40 can be applied on the floor slab F1, and a baseboard 41 can be attached to the lower edge of the partition wall 30. As the baseboard 41, a general-purpose prefabricated baseboard, for example, a vinyl baseboard, can be used.
[0098] Furthermore, the ceiling light steel base 42 can be suspended from the floor slab F2 of the upper floor. A ceiling finishing material 43 can be placed on the surface of the ceiling light steel base 42.
[0099] The ceiling finishing material 43 is connected to the interior wall surface via a trim 44 such as a ceiling trim. As the trim 44, a prefabricated trim made of resin or metal, or a joiner or processed wood product can be used.
[0100] 4, the underlay boards 34 are installed in a horizontal laying direction, and the upper and lower underlay boards 34 are butted against each other at horizontal joints 45. The multiple horizontal joints 45 extend horizontally and parallel to each other as joints in the form of butt joints.
[0101] The top boards 36 are installed in a vertical direction and are connected to each other via vertical joints 46 of a desired joint shape such as open joints, butt joints, joint construction joints, etc. The vertical joints 46 extend vertically and parallel to each other.
[0102] The above-mentioned architectural surface material with a magnetic layer can be suitably used as the overlay board 36. The vertical joints 46 between the overlay boards 36 can be treated with a joint treatment material. Note that a part of the overlay boards 36 constituting the partition wall 30 can be made of the architectural surface material with a magnetic layer, and the remaining part can be made of a normal architectural surface material without a magnetic layer.
[0103] In this way, by using the above-mentioned architectural surface material with a magnetic layer as the top board 36, it is possible to make the partition wall, which is a wall structure, into a wall capable of attracting magnetic materials such as magnets, which is preferable.
[0104] Here, the configuration of a partition wall has been described as an example of a wall structure, but the wall structure of this embodiment is not limited to a partition wall, and includes various wall structures using the architectural surface material with a magnetic layer described above. Also, here, an example has been shown in which the architectural surface material with a magnetic layer is fixed to an underlay board, but the wall structure of this embodiment is not limited to this, and includes wall structures in which the architectural surface material with a magnetic layer described above is fixed to a stud with a screw or the like. EXAMPLES
[0105] The present invention will be described below with reference to specific examples, but is not limited to these examples. [Experimental Example 1] In Experimental Example 1, a building surface material with a magnetic layer as shown in FIG. 1 was produced, and a magnet attraction test was carried out.
[0106] First, the manufacturing conditions for the building surface material with a magnetic layer will be described.
[0107] A gypsum board measuring 12.0 mm thick x 300 mm wide x 400 mm long was prepared as the architectural surface material 11, and a magnetic layer 12 was formed over the entire surface of one of its main surfaces 11a to form a architectural surface material 10 with a magnetic layer.
[0108] The magnetic layer was formed by mixing 100 parts by mass of iron powder as a magnetic material, 5 parts by mass of an inorganic binder, an alkali metal silicate-based binder, and water to form a magnetic material-containing coating material, which was then applied to the main surface of the architectural surface material 11 by a scraping method to a thickness of 0.75 mm and dried.
[0109] As shown in Table 1, reduced iron powder was used in Experimental Examples 1-1 to 1-5, atomized iron powder was used in Experimental Examples 1-6 to 1-10, and iron oxide powder was used in Experimental Examples 1-11 to 1-15. The iron oxide powder used was triiron tetroxide powder. All iron powders had an average particle size of 50 μm.
[0110] The alkali metal silicate binder contains lithium silicate, sodium silicate, and zinc borate.
[0111] In Experimental Examples 1-1 to 1-15, the magnetic layer 12 was formed so that the content per unit area of the iron powder, which is the magnetic material, was the value shown in Table 1. Specifically, for example, in Experimental Examples 1-1, 1-6, and 1-11, the content per unit area of the iron powder, which is the magnetic material of the magnetic layer, was 0.3 kg / m 2 In forming the magnetic layer 12 of each experimental example, the amount of water added to the magnetic material-containing coating material was adjusted so that the iron powder content per unit area of the magnetic layer 12 was adjusted to a desired value for each experimental example.
[0112] It was also confirmed that the thickness of the magnetic layer was within the range of 0.75 mm±0.25 mm in all experimental examples.
[0113] In the magnet attraction test, as shown in Fig. 2, first, the architectural surface material 21 with a magnetic layer produced in each experimental example was set up so that the main surface 21a was vertical. Then, a single magnet 22 with a diameter of 17 mmφ and an attraction force of 3.5 N to a 1 mm steel plate was used to attach an A4 sheet of paper 23 to the main surface 21a. The number of A4 sheets of paper 23 was then increased until the A4 sheets of paper 23 fell, and the number of A4 sheets of paper 23 minus one sheet when the A4 sheets of paper 23 fell was evaluated as the magnetic attraction force of the architectural surface material with a magnetic layer.
[0114] The magnet used in the magnet attraction test was attached to a 1 mm thick iron plate 52 as shown in Fig. 5, and a hook 511 connected to the magnet 51 was pulled up along the block arrow A at a speed of 3 mm / sec using an autograph (not shown) to measure the maximum strength. The maximum strength was defined as the attraction force to the 1 mm iron plate, and the same magnet was used in this experimental example.
[0115] In addition, when conducting the magnetic adsorption test shown in Figure 2, the distance L between the center of the magnet 22 and the top end of the A4 paper 23 was 3 cm, and the magnet was positioned so that the center of the magnet 22 was located in the center of the A4 paper 23 in the width direction.
[0116] The A4 paper 23 has a thickness of 0.09 mm and a mass of 64 g / m 2 A4 size paper was used.
[0117] The evaluation results are shown in Table 1.
[0118] In Table 1, the numbers below each experimental example number indicate the results of the magnet attraction test.
[0119] Experimental Examples 1-1 to 1-15 are all examples of the present invention.
[0120] [Table 1] From the results shown in Table 1, it was confirmed that when a magnetic layer containing a magnetic material and an inorganic binder was formed on the surface of a building surface material to form a building surface material with a magnetic layer, the building surface material with a magnetic layer had sufficient magnetic attraction. In addition, when cutting was attempted with a cutter, it was confirmed that the building surface materials with a magnetic layer of each experimental example could be easily cut into any shape. [Experimental Example 2] In Experimental Example 2, atomized iron powder was used as the magnetic material, which has the best magnetic attraction when the content per unit area of the magnetic material in the magnetic layer is the same as in Experimental Example 1. Then, architectural surface materials with a magnetic layer were produced in the same manner as in Experimental Example 1, by changing the amount of inorganic binder or using an organic binder instead of the inorganic binder.
[0121] Specifically, a gypsum board measuring 12.0 mm thick x 300 mm wide x 400 mm long was prepared as a building surface material, and a magnetic layer was formed over the entire surface of one of its main surfaces to create a building surface material with a magnetic layer.
[0122] The magnetic layer was formed by mixing 100 parts by mass of atomized iron powder, which is the magnetic material, with an inorganic or organic binder in the proportions shown in Table 2 as a binder, and water to form a magnetic material-containing coating material, which was then applied to the main surface of the architectural surface material 11 by a scraping method to a thickness of 0.75 mm and dried.
[0123] The atomized iron powder used was the same as that used in Experimental Example 1.
[0124] In Experimental Examples 2-1 to 2-7, an inorganic binder, an alkali metal silicate binder, was used as the binder. The alkali metal silicate binder used was the same as that used in Experimental Example 1. In Experimental Example 2-8, an organic binder, a vinyl acetate resin, was used as the binder.
[0125] In each of the experimental examples, the magnetic layer 12 had a content of iron powder, which is a magnetic material, of 2.0 kg / m 2 In forming the magnetic layer 12 of each experimental example, the amount of water added to the magnetic material-containing coating material was adjusted so that the iron powder content per unit area of the magnetic layer 12 was adjusted to a desired value.
[0126] It was also confirmed that the thickness of the magnetic layer was within the range of 0.75 mm±0.25 mm in all experimental examples.
[0127] The architectural facing material with a magnetic layer thus produced was subjected to a magnet attraction test, an adhesion test, an appearance test, and a heat generation test.
[0128] The magnet attraction test has already been explained in Experimental Example 1, so the explanation will be omitted here, and other evaluation methods will be explained. (Adhesion test) In carrying out the adhesion test, first, an adhesion test specimen 60 was prepared by adhering attachments 621, 622 to a magnetic layer-attached architectural surface material test piece 61, as shown in Fig. 6. Fig. 6 shows a cross-sectional view of the adhesion test specimen 60 in a plane parallel to the lamination direction of the magnetic layer-attached architectural surface material test piece 61 and the attachments 621, 622.
[0129] In preparing the adhesiveness test specimen 60, first, a magnetic layer-attached architectural surface material test piece 61 was cut out with a circular saw from the magnetic layer-attached architectural surface material prepared in each experimental example. Specifically, a cut was made perpendicular to the exposed surface of the magnetic layer, and the magnetic layer-attached architectural surface material test piece 61 was cut out so that it was a rectangular parallelepiped measuring 4 cm x 4 cm when viewed from above in the lamination direction of the magnetic layer and the architectural surface material.
[0130] Then, a pair of attachments 621, 622, each having a surface size of 4 cm x 4 cm for adhering the sample, were adhered with epoxy resin to the architectural surface material 611 and the magnetic layer 612 of the architectural surface material test piece 61 with a magnetic layer, respectively. In this way, the adhesiveness test specimen 60 was produced.
[0131] Next, one attachment 621 was fixed and the other attachment 622 was pulled upward in FIG. 6 at a speed of 2 mm / min using an autograph (AG-X plus, manufactured by Shimadzu Corporation), and the location of breakage in the architectural surface material test piece 61 with a magnetic layer was observed.
[0132] If fracture occurs between the magnetic layer of architectural surface material test piece 61 with a magnetic layer, specifically between magnetic layer 612 and architectural surface material 611, this indicates that the adhesive strength between the magnetic layer and the architectural surface material is low and the adhesion (bonding) is insufficient. If fracture occurs at architectural surface material 611 of architectural surface material test piece 61 with a magnetic layer, this indicates that the adhesive strength between the magnetic layer and the architectural surface material is high and the adhesion is sufficiently high. (Appearance test) The prepared architectural facing material with a magnetic layer was visually inspected for the presence of cracks on the surface of the magnetic layer. (Pyrogenicity test) The test was conducted in accordance with the ISO5660-1 cone calorimeter method. The test was evaluated in accordance with 6. Judgment in the Japan Research Institute's Fire Resistance Testing and Evaluation Procedure Manual, 4.10.1 Non-flammability Test Method, and 4.11.1 Semi-non-flammability Test Method.
[0133] During the evaluation of the heat generation test, the heat generation test (semi-noncombustible) indicates the total heat generation amount, maximum heat generation rate, and whether or not cracks have penetrated within 10 minutes after the start of heating, while the heat generation test (noncombustible) indicates the total heat generation amount, maximum heat generation rate, and whether or not cracks have penetrated within 20 minutes after the start of heating.
[0134] Experimental Examples 2-1 to 2-7 are working examples, and Experimental Example 2-8 is a comparative example. The evaluation results are shown in Table 2.
[0135] [Table 2] From the results shown in Table 2, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example 2-1 to Experimental Example 2-7 had sufficient magnetic attraction. In addition, when an attempt was made to cut them with a cutter, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example could be easily cut into any shape.
[0136] Furthermore, in Experimental Examples 2-1 to 2-7 in which an inorganic binder was used, it was confirmed that the total heat generation amount and the maximum heat generation rate were suppressed and non-combustibility was improved compared to Experimental Example 2-8 in which an organic binder was used.
[0137] The total heat generated in the first 10 minutes after heating was started was 8 MJ / m 2 The maximum heat generation rate is 200kw / m or less for more than 10 seconds. 2 If the heat resistance does not exceed 100%, and there are no cracks or holes that penetrate to the back surface that are harmful in terms of flame retardancy, it is recognized as a semi-noncombustible material. Also, if the same requirements as for semi-noncombustible are met for 20 minutes after heating begins, it is recognized as a noncombustible material. Therefore, it was confirmed that the architectural surface materials with magnetic layers of Experimental Examples 2-3 to 2-7 are noncombustible materials. It was also confirmed that the architectural surface materials with magnetic layers of Experimental Examples 2-2 to 2-7 are semi-noncombustible materials.
[0138] In the adhesion test, in the case of Experimental Example 2-1, in which the amount of inorganic binder blended was less than 1 part by mass relative to 100 parts by mass of the magnetic material, the fracture occurred in the magnetic layer. Since the magnetic layer is thin, the fracture in the magnetic layer means that the fracture occurred between the magnetic layer and the architectural surface material, i.e., at the interface, as described above. On the other hand, in the cases of Experimental Examples 2-2 to 2-7, in which the amount of inorganic binder blended was 1 part by mass or more relative to 100 parts by mass of the magnetic material, it was confirmed that the fracture did not occur at the interface between the magnetic layer and the architectural surface material, but occurred in the gypsum core, i.e., inside the architectural surface material.
[0139] This is believed to be because in Experimental Example 2-1, the adhesive strength between the magnetic layer and the architectural facing material was lower than in Experimental Examples 2-2 to 2-7, i.e., the adhesion was low, causing the fracture at the interface. In the other Experimental Examples 2-2 to 2-7, the adhesive strength between the magnetic layer and the architectural facing material was sufficiently high, causing the fracture at the gypsum core.
[0140] However, it was confirmed that if the blended amount of inorganic binder becomes too large, cracks may occur in the magnetic layer, as in Experimental Example 2-7. [Experimental Example 3] In Experimental Example 3, atomized iron powder was used as the magnetic material, which has the best magnetic attraction when the content per unit area of the magnetic material in the magnetic layer is the same as in Experimental Example 1. Then, a magnetic layer-attached architectural surface material was produced and evaluated using the magnetic material-containing coating material obtained by further adding a predetermined amount of inorganic additive to the above magnetic material and inorganic binder.
[0141] Specifically, a gypsum board measuring 12.0 mm thick x 300 mm wide x 400 mm long was prepared as a building surface material, and a magnetic layer was formed over the entire surface of one of its main surfaces to create a building surface material with a magnetic layer.
[0142] The magnetic layer was formed by mixing 100 parts by mass of atomized iron powder (magnetic material), 5 parts by mass of an inorganic binder, an alkali metal silicate-based binder, inorganic additives in the proportions shown in Table 3, and 20 parts by mass of water to form a magnetic material-containing coating material, which was then applied to the main surface of the architectural surface material 11 by a scraping method to a thickness of 0.75 mm and dried.
[0143] The atomized iron powder and the alkali metal silicate binder used were the same as those used in Experimental Example 1.
[0144] As the inorganic additive, talc with an average particle size of 16 μm was used.
[0145] In each of the experimental examples, the magnetic layer 12 had a content of iron powder, which is a magnetic material, of 2.0 kg / m 2 The magnetic layer is formed so as to satisfy the above.
[0146] It was also confirmed that the thickness of the magnetic layer formed in each of the experimental examples was within the range of 0.75 mm±0.25 mm.
[0147] The architectural facing material with a magnetic layer thus produced was subjected to a magnet attraction test, an adhesion test, an appearance test, and a heat generation test.
[0148] The magnet attraction test, adhesiveness test, and heat generation test have already been described in Experimental Example 1 or Experimental Example 2, so the description thereof will be omitted here.
[0149] In the appearance test, the surface of the magnetic layer was evaluated for pinholes, which are traces of air bubbles. If pinholes were visually confirmed, they were rated as present, and if they were not, they were rated as absent.
[0150] Experimental Examples 3-1 to 3-6 are all examples of the present invention.
[0151] [Table 3] From the results shown in Table 3, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example 3-1 to Experimental Example 3-6 had sufficient magnetic attraction. In addition, when an attempt was made to cut them with a cutter, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example could be easily cut into any shape.
[0152] In Experimental Examples 3-1 to 3-6, when adhesion tests were conducted, it was confirmed that the material broke at the architectural facing, i.e., the plaster core, and it was confirmed that the adhesive strength between the magnetic layer and the architectural facing was sufficiently high.
[0153] In Experimental Examples 3-1 and 3-6, it was confirmed that pinholes were generated on the surface of the magnetic layer. This is thought to be because the amount of inorganic additive added was insufficient or too much, resulting in insufficient fluidity of the magnetic material-containing coating material.
[0154] It was confirmed that the architectural surface materials with a magnetic layer of Experimental Examples 3-1 to 3-6 were non-combustible materials. [Experimental Example 4] In Experimental Example 4, the type of architectural facing material was changed, and an architectural facing material with a magnetic layer as shown in FIG. 1 was produced and evaluated.
[0155] First, the manufacturing conditions for the building surface material with a magnetic layer will be described.
[0156] Various architectural facing materials shown in Table 4 were prepared as the architectural facing material 11. The dimensions of each were 12.0 mm thick x 300 mm wide x 400 mm long. A magnetic layer 12 was then formed over the entire surface of one of the main surfaces 11a to obtain an architectural facing material with a magnetic layer.
[0157] The magnetic layer was formed by mixing 100 parts by mass of atomized iron powder (magnetic material), 5 parts by mass of an inorganic binder, an alkali metal silicate-based binder, and 20 parts by mass of water, and then applying the magnetic material-containing coating material to the main surface of the architectural surface material 11 by a scraping method to a thickness of 0.75 mm and drying it.
[0158] The atomized iron powder and the alkali metal silicate binder used were the same as those used in Experimental Example 1.
[0159] In each of the experimental examples, the magnetic layer 12 had a content of iron powder, which is a magnetic material, of 2.0 kg / m 2 The magnetic layer is formed so as to satisfy the above condition.
[0160] It was also confirmed that the thickness was within the range of 0.75 mm ± 0.25 mm.
[0161] The architectural facing material with the magnetic layer thus produced was subjected to a magnet attraction test, an adhesion test, and a heat generation test.
[0162] The magnet attraction test, adhesiveness test, and heat generation test have already been described in Experimental Example 1 or Experimental Example 2, so the description thereof will be omitted here.
[0163] Experimental Examples 4-1 to 4-5 are all examples of the present invention.
[0164] [Table 4] From the results shown in Table 4, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example 4-1 to Experimental Example 4-5 had sufficient magnetic attraction. In addition, when an attempt was made to cut them with a cutter, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example could be easily cut into any shape.
[0165] In Experimental Examples 4-1 to 4-5, when adhesion tests were conducted, it was confirmed that the film broke at the architectural facing, i.e., the base material, and it was confirmed that the adhesive strength between the magnetic layer and the architectural facing was sufficiently high.
[0166] It was confirmed that the architectural surface materials with a magnetic layer of Experimental Examples 4-1 to 4-5 were non-combustible materials. [Experimental Example 5] In Experimental Example 5, the atomized iron powder was used as the magnetic material, which has the best magnetic attraction force when the content per unit area of the magnetic material in the magnetic layer is the same as in Experimental Example 1. Then, as the magnetic material-containing coating material, a predetermined amount of inorganic additive and thickener was further added to the above magnetic material and inorganic binder, and a building surface material with a magnetic layer was produced and evaluated.
[0167] Specifically, a gypsum board measuring 12.0 mm thick x 300 mm wide x 400 mm long was prepared as a building surface material, and a magnetic layer was formed over the entire surface of one of its main surfaces to create a building surface material with a magnetic layer.
[0168] The magnetic layer was formed by mixing 100 parts by mass of atomized iron powder as the magnetic material, 5 parts by mass of an inorganic binder, an alkali metal silicate binder, 5 parts by mass of an inorganic additive, a modified polyacrylic sulfonate as a thickener in the proportions shown in Table 5, and 20 parts by mass of water to form a magnetic material-containing coating material, which was then applied to the main surface of the architectural surface material 11 by a scraping method to a thickness of 0.75 mm and dried.
[0169] The atomized iron powder and the alkali metal silicate binder used were the same as those used in Experimental Example 1.
[0170] As the inorganic additive, talc with an average particle size of 16 μm was used.
[0171] In each of the experimental examples, the magnetic layer 12 had a content of iron powder, which is a magnetic material, of 2.0 kg / m 2 The magnetic layer is formed so as to satisfy the above condition.
[0172] It was also confirmed that the thickness of the magnetic layer formed in each of the experimental examples was within the range of 0.75 mm±0.25 mm.
[0173] The architectural facing material with the magnetic layer thus produced was subjected to a magnet attraction test, an adhesion test, and a heat generation test.
[0174] The magnet attraction test, adhesiveness test, and heat generation test have already been described in Experimental Example 1 or Experimental Example 2, so the description thereof will be omitted here.
[0175] Experimental Examples 5-1 to 5-4 are all examples of the present invention.
[0176] [Table 5] From the results shown in Table 5, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example 5-1 to Experimental Example 5-4 had sufficient magnetic attraction. In addition, when an attempt was made to cut them with a cutter, it was confirmed that all of the architectural surface materials with a magnetic layer of Experimental Example could be easily cut into any shape.
[0177] In Experimental Examples 5-1 to 5-4, when adhesion tests were conducted, it was confirmed that the material broke at the architectural facing, i.e., the plaster core, and it was confirmed that the adhesive strength between the magnetic layer and the architectural facing was sufficiently high.
[0178] It was confirmed that the magnetic layer-attached architectural surface materials of Experimental Examples 5-1 to 5-4 were non-combustible materials. In addition, it was confirmed that if the blending amount of the thickener, which is an organic compound, is about 5 parts by mass or less per 100 parts by mass of the magnetic material, there is no significant change in the total calorific value, and there is no significant effect on non-combustibility. [Experimental Example 6] In Experimental Example 6, atomized iron powder was used as the magnetic material, which has the best magnetic attraction when the content per unit area of the magnetic material in the magnetic layer is the same as in Experimental Example 1. Then, in addition to the above magnetic material as the raw material of the magnetic material-containing coating material, a predetermined amount of inorganic additive and an inorganic binder or an organic binder were used as the binder to prepare a building surface material with a magnetic layer, and evaluation was performed.
[0179] Specifically, a gypsum board measuring 12.0 mm thick x 100 mm wide x 100 mm long was prepared as a building surface material, and a magnetic layer was formed over the entire surface of one of its main surfaces to create a building surface material with a magnetic layer.
[0180] The magnetic layer was formed by mixing 100 parts by mass of atomized iron powder as the magnetic material, 5 parts by mass of talc as an inorganic additive, 5 parts by mass of an inorganic binder (Experimental Example 6-1) or an organic binder (Experimental Example 6-2) as a binder, and 20 parts by mass of water, and then applying the magnetic material-containing coating material to the main surface of the architectural surface material 11 by a scraping method to a thickness of 0.75 mm and drying it.
[0181] The atomized iron powder used was the same as that used in Experimental Example 1.
[0182] As the inorganic additive, talc with an average particle size of 16 μm was used.
[0183] In Experimental Example 6-1, an inorganic binder, an alkali metal silicate-based binder, was used as the binder. The alkali metal silicate-based binder used was the same as that used in Experimental Example 1. In Experimental Example 6-2, an organic binder, a vinyl acetate resin, was used as the binder.
[0184] In each of the experimental examples, the magnetic layer 12 had a content of iron powder, which is a magnetic material, of 2.0 kg / m 2 The magnetic layer is formed so as to satisfy the above.
[0185] It was also confirmed that the thickness of the magnetic layer formed in each of the experimental examples was within the range of 0.75 mm±0.25 mm.
[0186] The thus-produced building surface material with a magnetic layer was then evaluated for rust formation.
[0187] To evaluate the occurrence of rust, as shown in Figure 7, architectural surface material with a magnetic layer 71 of experimental example 6-1, architectural surface material with a magnetic layer 72 of experimental example 6-2, and a petri dish 73 containing 100 mL of water were placed in an airtight container 74, and the airtight container was then placed in a thermostatic chamber set at 40°C, and the occurrence of rust on the magnetic layer was visually confirmed.
[0188] The results are shown in Table 6. Note that Experimental Example 6-1 is an embodiment, and Experimental Example 6-2 is a comparative example.
[0189] [Table 6] According to the results shown in Table 6, it was confirmed that even 14 days after the start of the test, no rust occurred in the architectural surface material with a magnetic layer of Experimental Example 6-1, which used an inorganic binder. On the other hand, the occurrence of rust was confirmed on the 7th day after the start of the test in the architectural surface material with a magnetic layer of Experimental Example 6-2, which used an organic binder.
[0190] From the above results, it was confirmed that by using an inorganic binder as the binder, it is possible to prevent the magnetic material of the magnetic layer from oxidizing and causing rust, even without adding a rust inhibitor.
[0191] Although the results of the magnet attraction test are not shown, it was confirmed that both of the architectural surface materials with magnetic layers of Experimental Example 6-1 and Experimental Example 6-2 had sufficient magnet attraction. In addition, when cutting was attempted with a cutter, it was confirmed that both of the architectural surface materials with magnetic layers of Experimental Example 6-1 and Experimental Example 6-2 could be easily cut into any shape.
[0192] Although the architectural surface material with a magnetic layer has been described above in terms of the embodiments, the present invention is not limited to the above embodiments, etc. Various modifications and changes are possible within the scope of the gist of the present invention described in the claims.
[0193] This application claims priority based on Japanese Patent Application No. 2018-190511, filed with the Japan Patent Office on October 5, 2018, the entire contents of which are incorporated herein by reference. [Explanation of symbols]
[0194] 10, 21, 71 Magnetic layered building surface material 11, 611 Architectural facing materials 12, 612 magnetic layer
Claims
1. Architectural facings; and a magnetic layer covering at least a portion of the surface of the architectural facing material. The magnetic layer contains a magnetic material, an inorganic binder, and an inorganic additive, the inorganic additive is talc; The magnetic layer contains the inorganic additive in an amount of 0.5 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the magnetic material.
2. An architectural surface material with a magnetic layer as described in claim 1, in which the Hunter whiteness (Wb) of the surface of the magnetic layer measured with a color difference meter exceeds 25.
3. 3. The architectural surface material with a magnetic layer according to claim 1, wherein the magnetic layer contains the inorganic binder in an amount of 1 part by mass or more and 35 parts by mass or less per 100 parts by mass of the magnetic material.
4. The magnetic layer has a content of the magnetic material per unit area of 0.3 kg / m 2 The architectural surface material with a magnetic layer according to any one of claims 1 to 3.
5. The architectural surface material with a magnetic layer according to any one of claims 1 to 4, wherein the architectural surface material is a fiber-reinforced cement board, a glass mat gypsum board, a gypsum-containing board with glass fiber nonwoven fabric, a glass fiber mixed cement board, a fiber mixed calcium silicate board, a gypsum board, a gypsum board, a slag gypsum board, or a resin board.
6. 6. The architectural surface material with a magnetic layer according to claim 1, wherein the magnetic layer contains an organic compound in an amount of 5 parts by mass or less per 100 parts by mass of the magnetic material.
7. 7. The architectural surface material with a magnetic layer according to claim 1, wherein the surface of the magnetic layer opposite to the surface facing the architectural surface material is exposed.
8. The architectural surface material with a magnetic layer according to any one of claims 1 to 7, having a thickness of 9.5 mm or more and 10.0 mm or less, 12.5 mm or more and 13.0 mm or less, 15.0 mm or more and 15.5 mm or less, 16.0 mm or more and 16.5 mm or less, 18.0 mm or more and 18.5 mm or less, 21.0 mm or more and 21.5 mm or less, or 25.0 mm or more and 25.5 mm or less.
9. 9. A construction surface material with a magnetic layer according to any one of claims 1 to 8, which satisfies semi-incombustible performance.
10. A building surface material with a magnetic layer according to any one of claims 1 to 8, which has non-combustible properties.
Citation Information
Patent Citations
JP1986128022U
notice wall
JP1994078983U
Magnetically attractive wall
JP1997088294A
Ornamental magnet attraction non-inflammable decorative sheet
JP2016132983A
Gypsum building material having magnetic layer, magnetic joint treatment material, and method for producing gypsum building material having magnetic layer
WO2018074218A1