Dust suppression processing method
A non-melt flowable TFE copolymer with controlled sedimentation and low perfluorooctanoic acid content addresses the issues of sedimentation and environmental impact in dust suppression, ensuring effective and economical dust control.
Patent Information
- Application Number
- JP2023529124
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2022-12-06
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Existing dust suppression methods using TFE polymers face issues with sedimentation and difficulty in redispersion, leading to reduced dust suppression effectiveness and environmental concerns due to high perfluorooctanoic acid content.
A non-melt flowable TFE copolymer with a redispersion sedimentation rate of 60% or less, combined with low perfluorooctanoic acid and salt content, is used to create a dust suppression treatment agent that maintains effectiveness and environmental safety by preventing solidification and enhancing redispersibility.
The method effectively suppresses dust generation from substances by maintaining the copolymer's ability to disperse uniformly, reducing sedimentation, and minimizing environmental impact through low perfluorooctanoic acid content, thus ensuring efficient and economical dust control.
Smart Images

Figure 0007560839000007 
Figure 0007560839000008 
Figure 0007560839000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a dust-suppressing treatment method using a dust-suppressing treatment composition that has excellent performance in suppressing dust from dust-generating substances and also has excellent re-dispersibility, and more specifically, to a dust-suppressing treatment method for dust-generating substances using a dust-suppressing treatment composition that is composed of a non-melt-flowable aqueous dispersion of tetrafluoroethylene (hereinafter referred to as TFE) copolymer, the re-dispersion sedimentation rate of the TFE copolymer being 60% or less, and the content of perfluorooctanoic acid and its salts being less than 10 ppb. [Background technology]
[0002] Technology for suppressing dust from dust-emitting substances is important for daily life and industry due to health, safety, environmental and other requirements. As such a dust suppression technique, Patent Document 1 below proposes a method in which PTFE (TFE polymer) is mixed with a powdery substance and the mixture is subjected to a compression-shear action at a temperature of about 20 to 200°C to fibrillate the TFE polymer and suppress the generation of dust from the powdery substance.
[0003] The TFE polymers described in Patent Document 1 listed below include Teflon (registered trademark) 6 and Teflon (registered trademark) 30, which are TFE homopolymers in terms of composition and in the form of fine powder or emulsion, and Teflon (registered trademark) 6C, which is a modified TFE polymer in terms of composition and in the form of fine powder.
[0004] Also, the following Patent Document 2 proposes a dust suppression method using a stable aqueous emulsion containing 1.0 mass % or more of a hydrocarbon-based anionic surfactant relative to a TFE homopolymer (TFE polymer), and shows that the method has a dust suppression effect for powdery substances. According to this Patent Document 2, TFE polymer particles are produced in the form of an aqueous emulsion by the emulsion polymerization method disclosed in the following Patent Documents 3 and 4, that is, by pressing and polymerizing TFE into an aqueous medium containing a water-soluble polymerization initiator and an anionic surfactant having a fluoroalkyl group as a hydrophobic group (hereinafter referred to as a fluorine-containing emulsifier) as an emulsifier, and an emulsion stabilizer is further added to increase stability.
[0005] Furthermore, Patent Document 5 listed below describes a method for suppressing dust by using a dust-suppressing treatment composition comprising a fluorinated polymer aqueous dispersion having a fluorinated emulsifier content of 50 ppm or less, which has a dust-suppressing effect and can suppress dust without worrying about the impact on the environment.
[0006] However, the TFE polymer aqueous dispersion used as the dust-suppressing treatment composition in these methods is prone to settling when left standing for a long period of time, and the TFE polymer that has once settled has the problem of being strongly solidified and difficult to redisperse. In addition, there is a risk that the dust-suppressing effect inherent to the TFE polymer cannot be fully exhibited depending on the conditions of use, for example, causing a decrease in the TFE polymer concentration in the TFE polymer aqueous dispersion. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 52-32877 [Patent Document 2] Japanese Patent Application Publication No. 8-20767 [Patent Document 3] Special table 2010-509441 publication [Patent Document 4] Special Publication No. 2010-509442 [Patent Document 5] International Publication No. WO2007 / 000812 Summary of the Invention [Problem to be solved by the invention]
[0008] That is, the present invention aims to provide a dust suppression treatment method using a dust suppression treatment composition which has an excellent dust suppression effect, is excellent in redispersibility of the non-melt-flowable TFE copolymer, which is the solid content in the dust suppression treatment composition after being left to stand for a long period of time, and is also excellent in environmental performance. [Means for solving the problem]
[0009] The present invention relates to a non-melt-flowable aqueous dispersion of a tetrafluoroethylene copolymer, the particle size (d84) of which is 50 to 84% when the cumulative volume percentage of the copolymer is 84%. 185 nm, and the non-melt-flowable tetrafluoroethylene copolymer is tetrafluoroethylene and the comonomer H Hexafluoropropylene And The present invention provides a dust-suppressive treatment method for a dust-generating substance, comprising mixing the dust-suppressive treatment composition with a dust-generating substance and subjecting the mixture to a compression-shear action under a temperature condition of 20 to 200°C to fibrillate the tetrafluoroethylene copolymer and suppress the generation of dust from the dust-generating substance, using a dust-suppressive treatment composition in which the copolymer has a redispersion sedimentation rate of 60% or less, as represented by the following formula:
[0010] Redispersion sedimentation rate (%) = X3 / X2 × 100 (1) During the ceremony, X2: 15 g of an aqueous dispersion of TFE polymer having the same concentration as the copolymer is added at a temperature of 2 Centrifuge at 0°C for 30 minutes at 3000 rpm. After the core separation, the redispersion is expressed by the following formula (2): Percentage of solids settling after dispersion (%) X3: 15 g of the copolymer aqueous dispersion was mixed at a temperature of 20° C. and a rotation speed of 3000 After centrifugation at 400 rpm for 30 minutes, the mixture was redispersed. The solid sedimentation ratio after redispersion is expressed by the following formula (2) (%) Percentage of solids settling after redispersion (%) = (Solid sedimentation amount after redispersion) / (Solid amount before centrifugation) × 100 (2)
[0011] In a preferred embodiment of the present invention, the content of the perfluorooctanoic acid and salts thereof in the aqueous dispersion is less than 5 ppb.
[0014] In a preferred embodiment of the present invention, the perfluoroalkyl group in the (perfluoroalkyl)ethylene is a perfluoroalkyl group having 1 to 10 carbon atoms.
[0015] In a preferred embodiment of the present invention, the (perfluoroalkyl)ethylene is at least one selected from (perfluoroethyl)ethylene, (perfluorobutyl)ethylene, (perfluorohexyl)ethylene, and (perfluorooctyl)ethylene.
[0018] The comonomer is 0.01 to 1.0% by weight based on tetrafluoroethylene. 0.30 It is a preferred embodiment of the present invention that the content is in an amount of % by mass.
[0020] The copolymer is contained in a dust suppressant treatment composition. 20 In a preferred embodiment of the present invention, the content is in an amount of up to 80% by mass.
[0021] In a preferred embodiment of the present invention, the specific gravity (SSG) of the copolymer is 2.27 or less.
[0022] The present invention also provides a method for suppressing dust generation of a dust-generating substance by using a dust-suppressing treatment powder obtained by granulating the above dust-suppressing treatment composition and then drying the granulated powder.
[0023] The dust-suppressing treatment method of the present invention can be suitably used for dust-generating powdery substances as the dust-generating substances. Effect of the Invention
[0024] The present invention provides a dust-suppressing treatment method for dust-generating substances using a dust-suppressing treatment composition which has excellent performance in suppressing dust from dust-generating substances, excellent redispersibility of non-melt-flowable TFE copolymer particles, which are the solid content in the dust-suppressing treatment composition, even after being left to stand for a long period of time, and excellent environmental performance. [Brief description of the drawings]
[0025] [Figure 1] FIG. 2 is a graph showing the results of a centrifugation sedimentation test and a centrifugation sedimentation redispersion test for Examples 1 to 3 and Comparative Example 1. [Diagram 2] FIG. 2 is a diagram showing the results of a static sedimentation test and a static sedimentation redispersion test for Examples 1 and 2 and Comparative Example 1. [Diagram 3] Photographs of Example 2 and Comparative Example 1 after standing for 90 days. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The dust-suppressing treatment method for a dust-generating substance of the present invention is characterized in that it uses a dust-suppressing treatment composition comprising a non-melt-flowable TFE copolymer aqueous dispersion, in which the redispersion sedimentation rate of the copolymer represented by the above formula (1) is 60% or less, and the content of perfluorooctanoic acid and its salts in the aqueous dispersion is less than 10 ppb, mixes the dust-suppressing treatment composition with a dust-generating substance, and subjects the mixture to a compression-shear action at a temperature of about 20 to 200°C, thereby fibrillating the non-melt-flowable TFE copolymer and suppressing the generation of dust from the dust-generating substance. As mentioned above, the TFE polymer particles, which are solids in the dust suppressive treatment composition, tend to settle, so that when the TFE polymer aqueous dispersion is left standing for a long period of time, the TFE polymer particles settle, and the settled TFE polymer particles solidify and are difficult to redisperse by stirring or the like. However, in the dust suppressive treatment composition used in the present invention, by using a dust suppressive treatment composition having a redispersion settling rate of the non-melt-flowable TFE copolymer aqueous dispersion of 60% or less, it is possible to suppress the settled non-melt-flowable TFE copolymer particles from solidifying, and to significantly improve redispersibility. As a result, in the dust suppressive treatment method of the present invention, a small amount of the dust suppressive treatment composition can be mixed uniformly with the dust-generating substance, so that it is possible to efficiently suppress the generation of dust from the dust-generating substance. Furthermore, since the content of the persistently decomposable perfluorooctanoic acid and its salt is less than 10 ppb, it is also excellent in environmental performance.
[0027] The dust suppressant treatment composition used in the present invention has excellent re-dispersibility in addition to dust suppression performance, as is clear from the results of the centrifugation sedimentation test, centrifugation re-dispersion test, static sedimentation test, static sedimentation re-dispersion test, and falling dust test in the Examples described below.
[0028] (Redispersion Sedimentation Rate) As is clear from FIG. 1 showing the results of the centrifugal separation sedimentation test and the centrifugal separation sedimentation redispersion test, the dust suppressant treatment composition having a redispersion sedimentation rate of 60% or less of the non-melt flowable TFE copolymer aqueous dispersion used in the present invention has a reduced amount of sedimentation compared to the TFE polymer aqueous dispersion having a redispersion sedimentation rate of more than 60%. As shown in Examples 1 to 3 described later, the dust-suppressing treatment method of the present invention clearly enables good redispersion by setting the redispersion sedimentation rate, as shown by the above formula (1), of the non-melt-flowable TFE copolymer aqueous dispersion in the dust-suppressing treatment composition used to be 60% or less, preferably 50% or less, and more preferably 30% or less. Furthermore, the non-melt-flowable TFE copolymer in the dust-suppressing treatment composition used in the present invention is considered to have excellent sedimentation stability because it contains few rod-shaped particles that are prone to sedimentation.
[0029] When the redispersion sedimentation rate shown by the above formula (1) exceeds 60%, the sedimented non-melt-flowable TFE copolymer particles are solidified, making it difficult to redisperse. In addition, as a result of the sedimentation of the solid non-melt-flowable TFE copolymer particles, the non-melt-flowable TFE copolymer particles dispersed in the dust suppression treatment composition are reduced, and in order to maintain the performance of suppressing dust from dust-generating substances equivalent to that before sedimentation, more non-melt-flowable TFE copolymer aqueous dispersion is required. Furthermore, the solidified non-melt-flowable TFE copolymer cannot be used as a dust suppression treatment, so it must be discarded, which wastes much of the non-melt-flowable TFE copolymer, which is a useful resource, and also generates disposal costs, which is undesirable from the economic point of view.
[0030] (Non-melt flowable TFE copolymer) The non-melt-flowable TFE copolymer of the present invention is preferably a non-melt-flowable copolymer of tetrafluoroethylene and at least one comonomer selected from perfluoro(alkyl vinyl ether), (perfluoroalkyl)ethylene, and hexafluoropropylene.
[0031] The (perfluoroalkyl)ethylene preferably has a perfluoroalkyl group having 1 to 10 carbon atoms, more preferably at least one selected from (perfluoroethyl)ethylene, (perfluorobutyl)ethylene, (perfluorohexyl)ethylene, and (perfluorooctyl)ethylene, and further preferably (perfluorobutyl)ethylene.
[0032] The perfluoro(alkyl vinyl ether) preferably has a perfluoroalkyl group having 1 to 10 carbon atoms, and more preferably at least one selected from perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether), and perfluoro(propyl vinyl ether).
[0033] The comonomer in the non-melt-flowable TFE copolymer used in the present invention is contained in an amount of 0.01 to 1.00% by mass, preferably 0.01 to 0.50% by mass, more preferably 0.01 to 0.30% by mass, based on TFE. When the content of the comonomer is 0.01 to 1.00% by mass, the stability of the aqueous dispersion is improved because there are few rod-shaped particles that tend to settle in the solid content. On the other hand, when the content of the comonomer exceeds 1.00% by mass, it is not preferable because it becomes difficult to fibrillate and the thermal stability is reduced. Also, when the content of the comonomer is less than 0.01% by mass, the effect of the comonomer cannot be expected and the redispersion sedimentation rate is poor, which is not preferable.
[0034] The melting point of the non-melt flowable TFE copolymer used in the present invention is 320 to 350° C., preferably 334 to 342° C. If the melting point is less than 320° C., the comonomer content in the non-melt flowable TFE copolymer increases, making it difficult to fibrillate, which is not preferred. The non-melt flowable TFE copolymer used in the present invention is a copolymer that does not exhibit melt moldability at temperatures above its melting point, and is preferably a copolymer whose MFR cannot be measured at temperatures above its melting point according to ASTM D1238 (372°C, load 5 kg). Such a non-melt flowable TFE copolymer is different from a TFE copolymer that has melt flowability and is melt moldable.
[0035] The specific gravity (SSG) of the non-melt-flowable TFE copolymer is desirably 2.27 or less, preferably 2.22 or less, and more desirably 2.20 or less. The larger the SSG value, the smaller the molecular weight, and vice versa. Therefore, the smaller the SSG value, i.e., the higher the molecular weight, the easier it is to fibrillate with a small shear force, and when mixed with a dust-generating substance, fibrils are easily generated and a high dust-suppressing effect can be obtained. On the other hand, the larger the SSG value (over 2.27), i.e., the smaller the molecular weight, the harder it is to fibrillate, and the effect of suppressing dust from the dust-generating substance is inferior, which is not preferable.
[0036] The non-melt-flowable TFE copolymer aqueous dispersion of the present invention is an aqueous dispersion in which fine particles (colloidal particles) of a high-molecular-weight non-melt-flowable TFE copolymer are dispersed. The non-melt-flowable TFE copolymer fine particles in the aqueous dispersion are desirably fine particles having a particle size (d84) at a cumulative volume percentage of 84% of 250 nm or less, preferably 50 to 250 nm, and more preferably 50 to 225 nm. If d84 is smaller than 50 nm, the effect of suppressing dust from dust-generating substances may be reduced compared to when it is within the above range, while if d84 exceeds 250 nm, sedimentation stability (dispersion stability) is reduced, which is undesirable. A particle size (d84) of 250 nm or less means that, unlike a particle size (d50) of 250 nm or less, there are no extremely large primary particles, and this means that the aqueous dispersion has excellent sedimentation stability.
[0037] In the present invention, the concentration of the non-melt-flowable TFE copolymer in the non-melt-flowable TFE copolymer aqueous dispersion is not particularly limited, but is in the range of 10 to 80 mass%, preferably 15 to 80 mass%, and more preferably 20 to 80 mass%. In order to enhance the dispersion effect of the non-melt-fluid TFE copolymer in dust-generating materials, the lower the concentration of the non-melt-fluid TFE copolymer, the better; a high concentration of the non-melt-fluid TFE copolymer is undesirable because it may impair sedimentation stability (dispersion stability). On the other hand, when transporting the non-melt-fluid TFE copolymer aqueous dispersion, the higher the concentration, the more the transportation cost can be saved. Therefore, the concentration of the non-melt-fluid TFE copolymer in the dust suppression treatment composition used in the present invention is preferably 10% by mass or more, particularly in the range of 20 to 80% by mass. In addition, when mixing with a dust-generating substance, in order to enhance the dispersing effect of the non-melt-flowable TFE copolymer in the dust-suppressing treatment composition used in the present invention, the dust-suppressing treatment composition can be diluted with water so that the concentration of the non-melt-flowable TFE copolymer is 5 mass % or less.
[0038] The content of perfluorooctanoic acid and its salts in the non-melt flowable TFE copolymer aqueous dispersion used in the present invention is preferably less than 10 ppb, more preferably less than 5 ppb, more preferably 0 ppb, based on the mass of the aqueous dispersion. Since perfluorooctanoic acid and its salts are difficult to decompose and are of concern for their impact on the environment, it is desirable that their content be as low as possible. The concentration of perfluorooctanoic acid and its salts in the non-melt fluidity TFE copolymer aqueous dispersion can be calculated by freezing 10 ml of the non-melt fluidity TFE copolymer aqueous dispersion in a polyethylene container in a -20°C freezer, flocculating the non-melt fluidity TFE copolymer and separating it from the water, transferring the entire contents of the polyethylene container to a Soxhlet extractor and extracting with approximately 80 ml of methanol for 7 hours, and measuring the measured sample liquid by liquid chromatography to calculate the concentration of perfluorooctanoic acid and its salts in the non-melt fluidity TFE copolymer aqueous dispersion.
[0039] There is no particular limitation on the method for preparing a non-melt-flowable aqueous dispersion of a TFE copolymer having a content of perfluorooctanoic acid and its salts of less than 10 ppb. The following method can be exemplified. For example, as disclosed in the above-mentioned Patent Documents 3 and 4, there is a method in which perfluorooctanoic acid and its salts are not used as a polymerization agent during polymerization, but an ammonium salt of a fluoromonoether acid (C3F7-O-CF(CF3)COOH) and an ammonium salt of a fluoropolyether acid (C3F7-O-[CF(CF3)CF2]n-CF(CF3)COOH) are used to polymerize a TFE copolymer.
[0040] The non-melt flowable TFE copolymer in the dust suppression treatment composition used in the present invention is a non-melt flowable TFE copolymer of TFE and the comonomer, and the redispersion sedimentation rate is 60% or less, so that it can be fibrillated to obtain dust suppression effect similar to the non-melt flowable TFE polymer, and can also obtain excellent redispersion sedimentation rate.In addition, the content of perfluorooctanoic acid and its salt in the non-melt flowable TFE copolymer aqueous dispersion is less than 10ppb, so that it also has excellent environmental performance.
[0041] Furthermore, the dust suppressant treatment composition, which is a non-melt-flowable TFE copolymer aqueous dispersion used in the present invention, may contain an emulsion stabilizer to enhance the stability of the non-melt-flowable TFE copolymer aqueous dispersion. As the emulsion stabilizer, a hydrocarbon-based anionic surfactant is preferred. This surfactant essentially forms a salt that is insoluble or poorly soluble in water with calcium, aluminum, and iron, which are soil components, and therefore pollution of rivers, lakes, and groundwater caused by the surfactant can be avoided.
[0042] Examples of such hydrocarbon-based anionic surfactants include higher fatty acid salts, higher alcohol sulfate salts, liquid fatty oil sulfate salts, fatty alcohol phosphate salts, dibasic fatty acid ester sulfonates, and alkyl aryl sulfonates. In particular, Na, K, Li, and NH4 salts of polyoxyethylene alkyl phenyl ether ethylene sulfonate (polyoxyethylene n is 1 to 6, alkyl has 8 to 11 carbon atoms), alkyl benzene sulfonate (alkyl has 10 to 12 carbon atoms), dialkyl sulfosuccinate (alkyl has 8 to 10 carbon atoms), etc. can be exemplified as preferred ones because they can impart high mechanical stability to a non-melt flowable TFE copolymer aqueous dispersion and prevent aggregation of non-melt flowable TFE copolymer particles due to high speed stirring, etc.
[0043] (Dust suppression treatment method) The dust suppressant treatment method of the present invention comprises mixing the above-mentioned dust suppressant treatment composition with a dust-generating substance, and subjecting the mixture to a compression-shear action at a temperature of 20 to 200°C, preferably 50 to 150°C, to fibrillate the non-melt-flowable TFE copolymer in the composition, thereby making it possible to suppress the generation of dust from the dust-generating substance. That is, the specific non-melt-flowable TFE copolymer used in the present invention is fibrillated into spider web-like ultrafine fibers when subjected to compression-shear action under the appropriate conditions as described above, and therefore, in the dust-suppressed treated product treated using the dust-suppression treatment method of the present invention, dust-generating substances are captured and aggregated in the spider web-like fine fibers, thereby suppressing dust.
[0044] The dust-generating substance to be subjected to dust suppression treatment by the dust suppression treatment method of the present invention is an inorganic and / or organic dust-generating substance, and there is no particular limitation on the substance, shape, etc. The present invention can also be effectively applied to dust-generating powdery substances as dust-generating substances. Particularly suitable dust-generating substances include cements such as Portland cement and alumina cement, slaked lime, quicklime powder, calcium carbonate, mineral powders such as dolomite, magnesite, talc, silica stone, and fluorite, clay mineral powders such as kaolin and bentonite, slag powders by-produced in the manufacturing process of metals such as steel and non-ferrous metals, combustion ash powders such as coal and garbage, gypsum powder, powdered metals, carbon black, activated carbon powder, ceramic powders such as metal oxides, pigments, etc., that is, all dust-generating substances that scatter and float in the air as solid particulate matter to generate dust are included.
[0045] The amount of the dust-suppressing treatment composition used in the present invention to be added to a dust-generating substance can be appropriately set depending on the type of dust-generating substance, particle size distribution, specific gravity (true specific gravity, apparent specific gravity), dust-suppressing treatment temperature, the degree of compression-shear action applied, the degree of dust suppression of the resulting dust-suppressing treated product, and the like. As a guideline for the amount of addition, for example, the dust-suppressing treatment composition can be added in an amount of 0.001 to 1.0 mass %, preferably 0.005 to 0.50 mass %, calculated as the solid content of the non-melt-flowable TFE copolymer resin relative to the dust-generating substance, to suppress dust generated from the dust-generating substance.
[0046] Furthermore, the dust suppressant treatment composition for dust-generating substances used in the present invention is preferable from the economical point of view, since the non-melt-flowable TFE copolymer does not solidify strongly even after being left to stand for a long period of time, i.e., it has excellent redispersibility (low redispersion settling rate), and therefore disposal costs can be reduced.
[0047] Furthermore, by using the dust-suppressing treatment powder for dust-generating substances, which is obtained by granulating the dust-suppressing treatment composition for dust-generating substances of the present invention and then drying it, dust-prevention treatment can be performed on dust-generating substances that are sensitive to moisture due to their hygroscopicity or deliquescence, etc. For information on the dust-prevention treatment method using a powder, see, for example, JP-B-52-32877. EXAMPLES
[0048] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Examples 1 to 3, Examples 11 to 13 and Examples 32 to 35 are reference examples. In the present invention, the physical properties were measured by the following methods.
[0049] [1] Particle size at cumulative volume percentage 84% (d84) The particle size (d84) of the non-melt-flowable TFE copolymer particles or TFE polymer particles was measured using a Microtrac UPA150 Model No. 9340 (manufactured by Nikkiso Co., Ltd.).
[0050] [2] Standard specific gravity (SSG) Measured according to ASTM D-4894. A non-melt-flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion obtained by emulsion polymerization was adjusted to a concentration of 15% by mass using pure water. Then, about 750 ml of the non-melt-flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion adjusted to the above concentration was placed in a polyethylene container (500 ml capacity) and vigorously shaken by hand to aggregate and separate the solids. The separated solids were dried at 150°C for 2 hours. 12.0 g of the dried solids (resin powder) were placed in a cylindrical mold with a diameter of 2.85 cm and smoothed, and after 30 seconds, the final pressure was 350 kg / cm. 2 The pressure was gradually increased to 350 kg / cm 2 The preform thus obtained (two pieces per sample) was heated in an air furnace from 290°C to 380°C at 2°C / min, held at 380°C for 30 minutes, cooled to 294°C at 1°C / min, held at 294°C for 1 minute, removed from the furnace, and cooled to room temperature (23±1°C) to prepare a standard sample. The mass ratio of the standard sample to the mass of the same volume of water at room temperature (23±1°C) was used as the standard gravity. In this case, the average of the standard gravity of the two samples was calculated and used as the standard gravity. This standard density serves as a guide for the average molecular weight, and generally the lower the standard density, the higher the molecular weight.
[0051] [3-1] Comonomer content (perfluorobutyl ethylene (PFBE) content) Using the same method as in [2] above, 0.8±0.050 g of a non-melt flowable TFE copolymer aqueous dispersion or a dried solid (resin powder) obtained from a TFE polymer aqueous dispersion was placed in a cylindrical mold with a diameter of 2.85 cm and smoothed between aluminum foils. After 30 seconds, the final pressure was 496 kg / cm. 2 The pressure was gradually increased until the final pressure was reached, and this final pressure was maintained for 2 minutes to obtain a sample for measurement. Similarly, measurement samples were also prepared for resin powders with known PFBE contents (mass%) (two points with PFBE contents of 0 mass% and 0.03 mass%). The infrared spectra of these samples were measured, and the absorbance ratio X was calculated using the following formula (3). Absorbance ratio X=(CB) / (AB)...(3) A:936cm-1 Peak height (absorbance) B:887cm -1 Peak height (absorbance) C:875cm -1 Peak height (absorbance) A calibration curve was created from the PFBE content (mass%) and absorbance ratio X of two samples with known PFBE content (mass%), and the PFBE content (mass%) of the sample was calculated from the absorbance ratio X of the sample.
[0052] [3-2] Comonomer content (perfluoropropyl vinyl ether (PPVE) content) Using the same method as in [2] above, 1.75±0.005 g of a non-melt flowable TFE copolymer aqueous dispersion or a dried solid (resin powder) obtained from a TFE polymer aqueous dispersion was placed in a cylindrical mold with a diameter of 2.85 cm, smoothed between aluminum foils, and gradually increased pressure was applied for 30 seconds until the final pressure reached 1470 kg / cm. 2 The final pressure was applied and maintained for 2 minutes to obtain measurement sample 1. Similarly, measurement samples were also prepared for resin powders with known PPVE contents (mass%) (two points with PPVE contents of 0 mass% and 0.75 mass%). The infrared spectra of these samples were measured, and the absorbance ratio and absorbance ratio X1 were calculated using the following equations (4) and (5). Absorbance ratio X1 = (absorbance ratio of sample 1 / absorbance ratio of known resin powder) × 0.75···(4) Absorbance ratio=B1 / A1...(5) A1:936cm -1 Peak height (absorbance) B1:994cm -1 Peak height (absorbance) A calibration curve was created from the PPVE content (mass%) and absorbance ratio X1 of two samples with known PPVE contents (mass%), and the PPVE content (mass%) of the sample was calculated from the absorbance ratio X1 of the sample.
[0053] [3-3] Comonomer content (Hexafluoropropylene (HFP) content) Using the same method as described in [2] above, a 1.75±0.005 g sample of a non-melt flowable TFE copolymer aqueous dispersion or a dried solid (resin powder) obtained from a TFE polymer aqueous dispersion was placed in a cylindrical mold with a diameter of 2.85 cm, flattened between aluminum foil, and pressure was applied for 30 seconds, gradually increasing until the final pressure reached 1470 kg / cm. 2 The final pressure was applied and maintained for 2 minutes to obtain a sample for measurement. Similarly, measurement samples were prepared for resin powders with known HFP contents (mass%) (three points with HFP contents of 0.06 mass%, 0.08 mass%, and 0.12 mass%). The infrared spectra of these samples were measured, and the absorbance ratio and absorbance ratio X2 were calculated using the following formulas (6) and (7). Absorbance ratio x2 = (absorbance ratio of sample / absorbance ratio of known sample) x 0.42 (6) Absorbance ratio = B2 / A2 (7) A2:936cm -1 Peak height (absorbance) B2:983cm -1 Peak height (absorbance) A calibration curve was created from the HFP content (mass%) and absorbance ratio X2 of three samples with known HFP content (mass%), and the HFP content (mass%) of each sample was calculated from the absorbance ratio X2 of each sample.
[0054] [4] Solid content mass% Less than 6 g of non-melt-flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion was weighed into a tared aluminum dish, and the mass (mass before drying) of the non-melt-flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion was measured (measured to four decimal places).Then, the mixture was left to stand in a 105°C dryer for 2 hours to remove moisture, baked in a constant temperature oven at 380°C for 20 minutes, cooled to room temperature, and then the mass (mass after drying) was measured, and the solid content (mass %) was calculated using the following formula (8). Solid content mass% = [(mass after drying - tare mass of aluminum dish) / mass before drying] x 100···(8)
[0055] [5] Melting point In the same manner as in [2] above, 10.0±0.3 mg of a non-melt-flowable TFE copolymer aqueous dispersion or a dried solid (resin powder) obtained from a TFE polymer aqueous dispersion was placed in a measurement Super Clean aluminum sample pan (manufactured by PerkinElmer Japan Co., Ltd.), and then a cover was placed on it and the sample was sealed using a standard crimper press to prepare a measurement sample. The measurement sample was subjected to a power compensation type differential scanning calorimeter Diamond DSC (manufactured by PerkinElmer Japan Co., Ltd.) using an empty Super Clean aluminum sample pan as the reference material, while increasing the temperature from 200°C to 370°C at a rate of 10°C per minute, and the calorific value was measured. The temperature at the point where the endothermic peak observed as a result of the measurement was maximum was taken as the melting point of the measurement sample (resin powder).
[0056] [6] Centrifugal sedimentation test 15 g of non-melt fluid TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion having the composition shown in Table 1 was placed in a centrifuge tube (Corning, 15 ml centrifuge tube), and centrifuged for 30 minutes at 20° C. and 3000 rpm using a centrifuge (Kubota, Tabletop Cooled Centrifuge 5500, Angle Rotor RA508). After centrifugation, the solids other than the solids that had settled to the bottom of the centrifuge tube (liquid part: supernatant and solids that had not settled) were removed from the centrifuge tube, the centrifuge tube was left in an upside-down state for 30 minutes, the liquid part was further removed, and the mass (the sum of the mass of the centrifuge tube and the mass of the solids that had settled to the bottom of the centrifuge tube) was measured, and the mass obtained by subtracting the mass of the centrifuge tube from the mass was used as the amount of solids that had settled, and the solids settling ratio was calculated from the following formula (10) and the settling rate was calculated from the following formula (9).
[0057] Sedimentation rate = X1 / X0 × 100 (9) During the ceremony, X0: 15 g of the TFE polymer aqueous dispersion shown in Comparative Example 1 was stirred at a temperature of 20° C. Centrifuge at 3000 rpm for 30 minutes. After that, the liquid portion other than the solid matter that settled to the bottom of the centrifuge tube (the supernatant and the sediment) was The solid content (undissolved solid content) is calculated by the following formula (10) The sedimentation rate (%). X1: 15 g of a non-melt-flowable TFE copolymer aqueous dispersion shown in the examples, Centrifuge at 20°C and 3000 rpm for 30 minutes. After centrifugation, the solid matter that had settled to the bottom of the centrifuge tube (liquid portion: The following formula (10) is obtained when the supernatant and non-settled solids are removed: The solid sedimentation rate (%) is Solids settling rate (%) = (amount of settled solids) / (mass of solids before centrifugation) × 100 (10)
[0058] [7] Centrifugal redispersion test The mass of the centrifuge tube from which the liquid portion was removed in [6] above was measured, 10 g of pure water was added to the centrifuge tube, and the solids that had settled to the bottom of the centrifuge tube were ultrasonically dispersed at 38 kHz for 1 minute. After that, all the solids other than those that had settled to the bottom of the centrifuge tube (the liquid portion and the redispersed solids) were removed, and the centrifuge tube was left in an inverted position for 30 minutes to further remove the liquid portion. The mass (the sum of the mass of the centrifuge tube and the mass of the solids that had settled to the bottom of the centrifuge tube) was measured, and the mass obtained by subtracting the mass of the centrifuge tube from this was determined as the amount of solids that had settled after redispersion. The solids settling ratio after redispersion was calculated from the following formula (2'), and the redispersion settling rate was calculated from the following formula (1').
[0059] Redispersion sedimentation rate (%) = X3 / X2 × 100 (1') During the ceremony, X2: 15 g of the TFE polymer aqueous dispersion shown in Comparative Example 1 was added at a temperature of 20° C. Centrifuge at 3000 rpm for 30 minutes. The solid sedimentation fraction when the mixture is redispersed after the solidification is expressed by the following formula (2'): The percentage is 100%. X3: 15 g of the non-melt-flowable TFE copolymer aqueous dispersion shown in the examples Centrifuge at 20°C and 3000 rpm for 30 minutes. After centrifuging the mixture again, the mixture is dispersed in water, and the resultant mixture is then dispersed in water. The solid sedimentation rate (%). Percentage of solids settling after redispersion (%) = (Solid sedimentation amount after redispersion) / (Solid mass before centrifugation) × 100 (2')
[0060] [8] Static settling test As shown in Table 2, 15 g of non-melt fluid TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion was placed in a centrifuge tube, and after closing the mouth of the centrifuge tube, it was left standing at room temperature for 30 days, 60 days, and 90 days, respectively. After leaving it standing for 30 days, 60 days, and 90 days, the mouth of the centrifuge tube was opened, and the solids other than the settled solids (liquid part: supernatant and solids that did not settle) were removed, and the centrifuge tube was left standing for 30 minutes in an upside-down state to further remove the liquid part, and its mass (the sum of the mass of the centrifuge tube and the mass of the solids that settled at the bottom of the centrifuge tube) was measured, and the mass obtained by subtracting the mass of the centrifuge tube from the mass was regarded as the amount of settled solids after standing, and the solids settling ratio was calculated from the following formula (12) and the settling rate was calculated from the following formula (11).
[0061] Sedimentation rate=X5 / X4×100...(11) During the ceremony, X4: 15 g of the TFE polymer aqueous dispersion shown in Comparative Example 1 was placed in a centrifuge tube with the mouth closed. After that, they were left at room temperature for 30 days, 60 days, and 90 days. After that, the liquid portion other than the precipitated solids (the supernatant and the non-settled solids) Remove the solids (which may be toxic) and leave the centrifuge tube upside down for 30 minutes. The solid sedimentation ratio (% ). X5: 15 g of the non-melt-flowable TFE copolymer aqueous dispersion shown in the examples After closing the centrifuge tube, the tubes were left for 30 days, 60 days, and 90 days, respectively. After leaving it at room temperature, the precipitated solids (liquid portion: supernatant and Remove the precipitate (and any solids that have not settled) and place the centrifuge tube upside down for 30 minutes. After leaving it to stand for a while and removing the liquid portion, the amount of solids that settled after standing (mass) The solid sedimentation rate (%) is calculated based on the following formula (12). . Solids settling rate (%) = (Solid sedimentation amount after standing) / (Solid mass before standing)×100 (12)
[0062] [9] Static settling and redispersion test The mass of the test tube that was left standing in [8] above was measured, 10 g of pure water was added to the centrifuge tube, and the solids that had settled to the bottom of the centrifuge tube were ultrasonically dispersed at 38 kHz for 1 minute. After that, all the solids other than those that had settled to the bottom of the centrifuge tube (the liquid portion and the redispersed solids) were removed, and the centrifuge tube was left standing upside down for 30 minutes to further remove the liquid portion. The mass (the sum of the mass of the centrifuge tube and the mass of the solids that had settled to the bottom of the centrifuge tube) was measured, and the mass obtained by subtracting the mass of the centrifuge tube from this was regarded as the amount of solids that had settled after redispersion. The redispersed solids settling ratio was calculated from the following formula (14), and the redispersion settling rate was calculated from the following formula (13).
[0063] Redispersion sedimentation rate = X7 / X6 × 100 (13) During the ceremony, X6: 15 g of the TFE polymer aqueous dispersion shown in Comparative Example 1 was placed in a centrifuge tube with the mouth closed. After that, they were left at room temperature for 30 days, 60 days, and 90 days. After that, the liquid portion other than the precipitated solids (the supernatant and the non-settled solids) Remove the solids (which may be toxic) and leave the centrifuge tube upside down for 30 minutes. After further removing the solids, the solids are redispersed as shown in the following formula (14). The shape sedimentation rate (%). X7: 15 g of the non-melt-flowable TFE copolymer aqueous dispersion shown in the examples After closing the centrifuge tube, the tubes were left for 30 days, 60 days, and 90 days, respectively. After leaving it at room temperature, the precipitated solids (liquid portion: supernatant and Remove the precipitate (and any solids that have not settled) and place the centrifuge tube upside down for 30 minutes. After leaving the mixture to stand for a while and removing the liquid portion, the mixture was redispersed according to the following formula (14 ) is the solids settling percentage (%). Percentage of solids settling after redispersion (%) = (Solid sedimentation amount after redispersion) / (Solid mass before centrifugation) × 100 (14)
[0064]
[10] Falling dust test (amount of falling dust) 200 g of sample (dust suppression treated material) was allowed to fall naturally from the top opening of a cylindrical container with an inner diameter of 39 cm and a height of 59 cm, and the amount of suspended dust (relative concentration (CPM: counts per minute)) in the container at a position 45 cm above the bottom was measured using a scattered light type digital dust meter. The amount of suspended dust was measured by measuring 5 consecutive times for 1 minute after the sample was added, and the geometric mean value x (CPM) obtained by subtracting the measured value (dark count) before the sample was added was used as the "amount of fallen dust" for the sample. The geometric mean value x was calculated using the following formula (15): Log x=(1 / 5)×Σlog(xi‐d)···(15) In the formula, xi: individual suspended dust amount, and d: dark count. It is more preferable that the falling dust amount (CPM) is 50 or less since the dust prevention performance is more excellent.
[0065] Example 1 (Polymerization of non-melt-flowable TFE copolymers) In a 4-liter stainless steel (SUS316) autoclave equipped with a stirring blade and a temperature control jacket, 60 g of paraffin wax, 2087 ml of deionized water, 12.03 g of ammonium salt of fluoromonoether acid (formula C3F7-0-CF(CF3)COOH), 1.0 g of ammonium salt of fluoropolyether acid (C3F7-O-[CF(CF3)CF2]n-CF(CF3)COOH), and 0.01 g of polyoxyethylene alkylphenyl ether were charged, and the system was replaced with nitrogen gas three times while heating to 80°C to remove oxygen, and then vacuum was drawn. After that, 4.4 g of PFBE, 0.2 g of ammonium salt of fluoromonoether acid, and 199.8 ml of deionized water were charged, and tetrafluoroethylene (TFE) was supplied to set the internal pressure to 1.90-1.98 MPa, and the internal temperature was maintained at 80°C while stirring at 110 rpm.
[0066] Next, 100 ml of the aqueous solution was pumped from an aqueous solution of 0.12 g of ammonium persulfate dissolved in 400 ml of water. After the injection of the aqueous ammonium persulfate solution was completed, TFE was continued to be supplied so as to maintain the internal pressure at 2.0 MPa. When the consumption of TFE reached 1106.79 g, stirring was stopped. The gas in the autoclave was released to normal pressure, a vacuum was drawn, and the pressure was returned to normal pressure with nitrogen gas, after which the contents were removed and the reaction was terminated, and a non-melt flowable TFE copolymer aqueous dispersion was obtained.
[0067] The particle size (d84) at a cumulative volume percentage of 84%, SSG, PFBE content, solid mass, melting point, and perfluorooctanoic acid and its salt content were measured for the obtained non-melt flowable TFE copolymer aqueous dispersion. In addition, a centrifugal separation test and a centrifugal separation and separation redispersion test were performed. The results are shown in Table 1 and Figure 1.
[0068] (Examples 2 and 3) A non-melt-flowable TFE copolymer aqueous dispersion was obtained in the same manner as in Example 1, except that the PFBE content was set to the amount shown in Table 1. The particle size (d84) at a cumulative volume percentage of 84%, SSG, PFBE content, solid mass, melting point, and perfluorooctanoic acid and its salt content were measured for the obtained non-melt-flowable TFE copolymer aqueous dispersion. In addition, a centrifugal separation test and a centrifugal separation and redispersion test were performed. The results are shown in Table 1 and FIG. 1.
[0069] Comparative Example 1 For a TFE polymer aqueous dispersion (Teflon (registered trademark) PTFE Dispersion 312-JR, manufactured by Mitsui-Chemours Fluoroproducts Co., Ltd.), the particle size (d84) at a cumulative volume percentage of 84%, SSG, PFBE content, solid mass, and perfluorooctanoic acid and its salt content were measured. In addition, a centrifugal separation test and a centrifugal separation and redispersion test were performed. In addition, physical property analysis was performed in the same manner as in Example 1. The results are shown in Table 1 and FIG. 1.
[0070] Furthermore, a static settling test and a static settling redispersion test were carried out for Examples 1 and 2 and Comparative Example 1. The results are shown in Table 2 and Figure 2. Additionally, Figure 3 shows photographs of Example 2 and Comparative Example 1 after standing for 90 days.
[0071] (Falling dust test) (Example 4, Comparative Example 2) 1,000 g of powdered quicklime containing 95.7% CaO and 1.6% MgO (powdered quicklime that passed through a 2.0 mm standard mesh sieve, 17.3% remaining on a 1.0 mm standard mesh sieve, 18.9% remaining on a 600 μm standard mesh sieve, 18.1% remaining on a 300 μm standard mesh sieve, 14.1% remaining on a 150 μm standard mesh sieve, and 31.6% passing through a 150 μm standard mesh sieve) was placed in a small soil mixer with a volume of 5 liters and stirred at a rotation speed of 140 rpm. Alternatively, the non-melt flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion prepared in Comparative Example 1 was weighed out at a mass equivalent to 0.05 g in terms of solid content (0.005 mass% in terms of the solid content mass of the non-melt flowable TFE copolymer or TFE polymer relative to the quicklime), diluted with water so that the total amount of moisture and water contained in the non-melt flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion became 100 g, and the dispersion thus obtained was gradually added. Approximately one minute after the start of mixing, steam began to be generated due to the heat of the quicklime hydration reaction, and approximately two minutes later, all of the water was used up to produce slaked lime through the hydration of the quicklime, and steam generation ceased. Three minutes after mixing began, the mixer was stopped. The temperature at this point was measured with a thermometer and was 107°C. This dust-suppressed quicklime was a mixture of quicklime and slaked lime, including approximately 30% newly produced slaked lime through the hydration reaction. The resulting dust-suppressed The treated material was subjected to a falling dust test, and the results are shown in Table 3.
[0072] (Examples 5 and 6, Comparative Examples 3 and 4) The non-melt-flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion prepared in Example 2 or Comparative Example 1 was weighed out in an amount equivalent to the amount added (mass % solid content relative to the dust-generating substance) shown in Table 3, diluted with water so that the total amount of water and moisture contained in the non-melt-flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion was 100 g, and a dispersion in which the composition was dispersed was used. A mixture of quicklime and slaked lime subjected to dust-suppression treatment was obtained in the same manner as in Example 4. A drop dust generation test of the obtained dust-suppression treated product was performed. The results are shown in Table 3.
[0073] Comparative Example 5 A drop dusting test was carried out on the mixture of quicklime and slaked lime obtained in the same manner as in Example 4, except that the non-melt flowable TFE copolymer aqueous dispersion or TFE polymer aqueous dispersion was not used, and 100 g of water was used instead. The results are shown in Table 3.
[0074] [Table 1]
[0075] [Table 2]
[0076] [Table 3]
[0077] (Examples 7 to 13) (Polymerization of non-melt-flowable TFE copolymers) In a 4-liter stainless steel (SUS316) autoclave equipped with a stirring blade and a temperature control jacket, 60 g of paraffin wax, 2087 ml of deionized water, 12.03 g of ammonium salt of fluoromonoether acid (formula C3F7-0-CF(CF3)COOH), 1.0 g of ammonium salt of fluoropolyether acid (C3F7-O-[CF(CF3)CF2]n-CF(CF3)COOH), and 0.01 g of polyoxyethylene alkylphenyl ether were charged, and the system was replaced with nitrogen gas three times while heating to 80°C to remove oxygen, and then vacuum was drawn. Then, comonomer (HFP or PPVE) was pumped in the amount shown in Table 4. Then, tetrafluoroethylene (TFE) was supplied to set the internal pressure to 1.90-1.98 MPa, and the internal temperature was kept at 80°C while stirring at 110 rpm.
[0078] Next, 100 ml of the aqueous solution was pumped from an aqueous solution of 0.12 g of ammonium persulfate dissolved in 400 ml of water. After the injection of the aqueous ammonium persulfate solution was completed, TFE was continued to be supplied so as to maintain the internal pressure at 2.0 MPa. When the consumption of TFE reached 1106.79 g, stirring was stopped. The gas in the autoclave was released to normal pressure, a vacuum was drawn, and the pressure was returned to normal pressure with nitrogen gas, after which the contents were removed and the reaction was terminated, and a non-melt flowable TFE copolymer aqueous dispersion was obtained.
[0079] The particle size (d84) at a cumulative volume percentage of 84%, SSG, PFBE content, solid mass, melting point, and amount of perfluorooctanoic acid and its salts were measured for the obtained non-melt flowable TFE copolymer aqueous dispersion. In addition, a centrifugal separation test and a centrifugal separation and separation redispersion test were performed. The results are shown in Table 4.
[0080] (Examples 14, 15, 21, 23, 24, 29, 30, 32 to 35) The dust-generating substance shown below and the non-melt-flowable TFE copolymer aqueous dispersions prepared in Examples 7 to 13 were weighed out in amounts equivalent to the amounts shown in Table 5 or Table 6 (% by mass of solid content relative to the dust-generating substance), and the non-melt-flowable TFE copolymer aqueous dispersion was diluted with water so that the total amount of water and moisture contained in the dispersion was 100 g, and a dust-suppressing treated product was obtained by the following method. The dust-suppressing treated product obtained was subjected to a drop dust generation test. The results are shown in Table 5 or Table 6.
[0081] (Examples 16 to 20, 22, 25 to 28, and 31) The dust-generating substance shown below and the non-melt-flowable TFE copolymer aqueous dispersions prepared in Examples 7 to 13 were weighed out in amounts equivalent to the amounts shown in Table 5 or Table 6 (% by mass of solid content relative to the dust-generating substance), and the non-melt-flowable TFE copolymer aqueous dispersion was diluted with water so that the total amount of water and moisture contained in the dispersion was 35 g, and a dust-suppressing treated product was obtained by the following method. The dust-suppressing treated product obtained was subjected to a drop dust generation test. The results are shown in Table 5 or Table 6.
[0082] <Dusting substances> Powdered quicklime (containing 96.0% CaO and 0.9% MgO) (Powdered quicklime that passed through a 2.0mm standard mesh sieve, 0.18% remained on a 1.0mm standard mesh sieve, 2.48% remained on a 600μm standard mesh sieve, 20.44% remained on a 300μm standard mesh sieve, 20.58% remained on a 150μm standard mesh sieve, and 56.32% passed through a 150μm standard mesh sieve) Dustproof treatment of powdered quicklime (Examples 14, 15, 21, 23, 24, 29, 30, 32 to 35): 1000g of powdered quicklime was weighed into the container of a mortar mixer, the container was set in the mortar mixer and stirred at a low speed, the dispersion diluted with water (mass of non-melt flowable TFE copolymer corresponding to the amount added shown in Table 5 or Table 6 + 100g of water) was added into the mortar mixer, and the stirring of the mixer was stopped 3 minutes after the start of stirring. Thereafter, the quicklime in the mortar mixer was transferred to an enamel tray and allowed to cool for about 5 minutes to obtain a dust-suppressing treated product.
[0083] Ordinary Portland cement (containing 64.3% CaO, 1.1% MgO, 20.5% SiO2, 5.1% Al2O3, 3.1% Fe2O3 and 2.0% SO3) (Ordinary Portland cement that passed completely through a 2.0 mm standard mesh sieve, a 1.0 mm standard mesh sieve, a 600 μm standard mesh sieve, a 300 μm standard mesh sieve, 0.22% remaining on a 150 μm standard mesh sieve, and 99.78% passing through a 150 μm standard mesh sieve) Dust-proofing treatment of a 9:1 mixture of ordinary Portland cement (hereinafter referred to as cement) and the powdered lime (Examples 16, 22, 25, and 31): 450g x 2 of cement was weighed out, spread evenly on an enamel tray, and heated at 105°C for one day and night. 100g of powdered quicklime was weighed into the container of a mortar mixer, and the dispersion diluted with water (mass of non-melting fluid TFE copolymer corresponding to the amount added shown in Table 5 or Table 6 + 35g of water) was added to the mortar mixer and stirred at low speed for 1 minute to obtain material A. 450g of cement heated to 105°C was added to the obtained material A, and further stirred for 1 minute to obtain material B. 450g of cement heated to 105°C was added to the obtained material B, and stirred for 3 minutes with a mortar mixer to obtain a dust-suppressing treated product.
[0084] ·Anhydrite (Anhydrous gypsum that passed completely through a 2.0 mm standard mesh sieve, completely through a 1.0 mm standard mesh sieve, 0.13% remaining on a 600 μm standard mesh sieve, 0.22% remaining on a 300 μm standard mesh sieve, 11.33% remaining on a 150 μm standard mesh sieve, and 88.31% passing through a 150 μm standard mesh sieve) Dust-proofing treatment of anhydrous gypsum (Examples 17 and 26): Anhydrous gypsum was weighed out 500g x 2, spread evenly on an enamel tray, and heated at 105 ° C for one day and night. 500g of the heated anhydrous gypsum was weighed into the container of a mortar mixer, and the above-mentioned dispersion diluted with water (mass of non-melt flowable TFE copolymer corresponding to the amount added shown in Table 5 or Table 6 + 35g of water) was put into the mortar mixer and stirred at low speed for 1 minute, and 500g of anhydrous gypsum heated to 105 ° C was added and stirred for 3 minutes, and then spread evenly on an enamel tray and heated at 105 ° C for 1 hour to obtain a mixture. About 1 kg of the mixture was put into a mortar and stirred with a pestle for 9 minutes to obtain a dust-suppressing treated product.
[0085] Granulated blast furnace slag powder (Granulated blast furnace slag that passed completely through a 2.0 mm standard mesh sieve, completely through a 1.0 mm standard mesh sieve, 0.02% remaining on a 600 μm standard mesh sieve, 0.06% remaining on a 300 μm standard mesh sieve, 0.31% remaining on a 150 μm standard mesh sieve, and 99.61% passing through a 150 μm standard mesh sieve) Dust-proofing treatment of ground granulated blast furnace slag (Examples 18 and 27): A dust-suppressed treated product was obtained in the same manner as the above-mentioned dust-proofing treatment of anhydrous gypsum, except that ground granulated blast furnace slag was used.
[0086] Dolomite (Dolomite that passed through a 2.0mm standard mesh sieve completely, 0.06% remained on a 1.0mm standard mesh sieve, 0.50% remained on a 600μm standard mesh sieve, 3.44% remained on a 300μm standard mesh sieve, 8.20% remained on a 150μm standard mesh sieve, and 87.79% passed through a 150μm standard mesh sieve) Dust-proofing of dolomite (Examples 19 and 28): Dolomite was weighed out in an amount of 500g x 2, spread evenly on an enamel tray, and heated at 105 ° C for one day and night. 500g of the heated dolomite was weighed into a mortar mixer container, and the above-mentioned water-diluted dispersion (mass of non-melt flowable TFE copolymer corresponding to the amount added shown in Table 5 or Table 6 + 35g of water) was added to the mortar mixer and stirred at low speed for 1 minute, and 500g of dolomite heated to 105 ° C was added and stirred for 3 minutes, and then the mixture was spread evenly on an enamel tray and heated at 105 ° C for 1 hour to obtain a mixture. About 1kg of the mixture was put into a mortar mixer and stirred for 3 minutes to obtain a dust-suppressing treated product.
[0087] Lignite powder (Lignite powder that passed completely through a 2.0mm standard mesh sieve, a 1.0mm standard mesh sieve, a 600μm standard mesh sieve, 0.02% retained on a 300μm standard mesh sieve, 33.03% retained on a 150μm standard mesh sieve, and 66.95% passed through a 150μm standard mesh sieve) Dust-proofing of lignite powder (Example 20): 500 g of lignite powder (hygroscopic dust-generating powder) was weighed out, spread evenly on an enamel tray, and heated at 105 ° C for one day and night. Pure water was added so that the solid content of the aqueous dispersion of Example 7 was 15%, and the mixture was put into a granulation tank equipped with a stirrer, and then stirred at 600 to 700 rpm until the powder precipitated. After the precipitate was precipitated, stirring was continued for another 3 to 5 minutes. The precipitated powder was collected with a mesh and separated from the water, then dried in an oven at 150 ° C for 2 to 15 hours until the water disappeared, and cooled to room temperature to obtain a powder consisting of the aqueous dispersion of Example 7. 5 g of the obtained powder and about 1 / 4 of the heated lignite powder were placed in a mortar and slowly mixed with a pestle. The lignite powder was further added in 1 / 4 portions in three batches and mixed, then spread evenly on an enamel tray and heated at 105 ° C for 1 hour to obtain a mixture. About 500 g of the mixture was placed in a mortar and mixed with a pestle until the non-melt-flowable TFE copolymer was sufficiently fibrillated, to obtain a dust-suppressing treated material.
[0088] [Table 4]
[0089] [Table 5]
[0090] [Table 6] [Industrial Applicability]
[0091] The dust-suppression treatment method of the present invention is suitably used for treating dust-generating substances to suppress dust to obtain dust-suppressed products of dust-generating substances in the fields of building materials, soil stabilizers, solidification materials, fertilizers, landfill disposal of incineration ash or hazardous substances, explosion protection, cosmetics, and fillers for various plastics.
Claims
1. A dust-suppressing treatment method for a dust-generating substance, comprising: a non-melt-flowable aqueous dispersion of a tetrafluoroethylene copolymer, the particle size (d84) of said copolymer being 50-185 nm when the cumulative volume percentage of said copolymer is 84%, said non-melt-flowable tetrafluoroethylene copolymer being a non-melt-flowable copolymer of tetrafluoroethylene and a comonomer, hexafluoropropylene, said copolymer having a redispersion sedimentation rate of 60% or less as represented by the following formula; and a content of perfluorooctanoic acid and its salts in said aqueous dispersion being less than 10 ppb, said dust-suppressing treatment composition being mixed with a dust-generating substance, and said mixture being subjected to a compression-shear action under a temperature condition of 20-200°C, thereby fibrillating the tetrafluoroethylene copolymer and suppressing the generation of dust from the dust-generating substance. Redispersion sedimentation rate (%) = X 3 / X 2 × 100 During the ceremony, X 2 The percentage of solids sedimented after redispersion (%) is represented by the following formula: 15 g of an aqueous dispersion containing perfluorooctanoic acid and its salts at less than 10 ppb relative to the mass of the aqueous dispersion and containing the same concentration of tetrafluoroethylene polymer as the copolymer, centrifuged at 20° C. and 3,000 rpm for 30 minutes in a centrifuge and then redispersed. X 3 The percentage of solids sedimented after redispersion (%) is calculated based on the following formula when 15 g of the aqueous copolymer dispersion is centrifuged at 20° C. and 3,000 rpm for 30 minutes and then redispersed. Percentage of solids settling after redispersion (%) = (amount of solids settling after redispersion) / (mass of solids before centrifugation) x 100
2. 2. The method for suppressing dust generation of a dust-generating substance according to claim 1, wherein the content of said perfluorooctanoic acid and its salts in said aqueous dispersion is less than 5 ppb.
3. 3. The method for suppressing dust generation of a dust-generating substance according to claim 1, wherein the comonomer is contained in an amount of 0.01 to 0.30% by mass based on the tetrafluoroethylene.
4. 3. The method for suppressive treatment of dust-generating substances according to claim 1, wherein the copolymer is contained in the dust-suppressive treatment composition in an amount of 20 to 80% by mass.
5. 3. The method for suppressing dust generation of a dust-generating substance according to claim 1, wherein the copolymer has a specific gravity (SSG) of 2.27 or less.
6. 3. The method for suppressing dust generation of a dust-generating substance according to claim 1, wherein the dust-generating substance is a dust-generating powdery substance.
7. 3. The method for suppressing dust generation of dust-generating substances according to claim 1, wherein the dust-suppressing treatment composition is granulated and then dried to obtain a powder of the dust-suppressing treatment.
Citation Information
Patent Citations
JP1975009441A
Evaporator
JP1977032877A
Method for preventing dusting
JP1996020767A
Fluororesin aqueous dispersion
JP2008037914A
Aqueous polymerization of fluorinated monomers using polymerization agents containing fluoropolyetheric acid or salt and short-chain fluorinated surfactants
JP2010509442A