Adsorbent for oil adsorption and method for manufacturing adsorbent for oil adsorption

A cellulose-based adsorbent with a small amount of water repellent ensures efficient oil adsorption and easy recovery by floating on water, addressing the cost and efficiency issues of previous wax-coated cardboard adsorbents.

JP7560913B1Active Publication Date: 2024-10-03CELL MAP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024065110
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-10-03
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

Existing oil adsorbents made from coated cardboard require a large amount of wax, which increases costs and can lead to wax peeling, reducing adsorption efficiency and making recovery difficult, especially when submerged in water.

Method used

An adsorbent comprising cellulose material with a water repellent, excluding wax and silicone-based compounds, is impregnated with a small amount (0.2-5.0 wt%) to ensure floatation and efficient oil adsorption without water absorption.

Benefits of technology

The adsorbent effectively adsorbs large amounts of oil while floating on water, facilitating easy recovery by preventing sinking, even under water pressure, and maintaining adsorption efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560913000001
    Figure 0007560913000001
  • Figure 0007560913000002
    Figure 0007560913000002
  • Figure 0007560913000003
    Figure 0007560913000003
Patent Text Reader

Abstract

The present invention provides an adsorbent for oil adsorption that floats on water and can sufficiently adsorb oil by using a relatively small amount of a specified compound, and a method for manufacturing the adsorbent for oil adsorption. [Solution] A water-floating adsorbent for absorbing oil comprises a cellulosic material and a water repellent agent contained in the cellulosic material, the cellulosic material being 95 wt% or more and the water repellent agent being 0.2 wt% or more and 5.0 wt% or less inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an oil absorbing sorbent and a method for manufacturing the oil absorbing sorbent, in particular to a water-floating oil absorbing sorbent and a method for manufacturing the oil absorbing sorbent. [Background technology]

[0002] Various technologies have been developed that use waste paper containing natural fibers as a raw material for oil adsorbents, with the aim of recovering waste oil discharged from restaurants, commercial facilities, food processing facilities, etc. For example, a method for manufacturing an oil adsorbent is known in which cardboard coated with wax over almost the entire outer surface is crushed into fibers to produce an oil adsorbent (see, for example, Patent Document 1). The oil adsorbent described in Patent Document 1 can adsorb a large amount of oil. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-165914 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the oil adsorbent described in Patent Document 1, when coating the cardboard with wax, a large amount of wax, 20% by weight or more of the cardboard, is required, making it difficult to reduce the manufacturing cost. In addition, since the oil adsorbent described in Patent Document 1 is simply a coating of wax on the cardboard surface, the wax is likely to peel off from the cardboard surface, which may reduce the oil adsorbing effect, or the oil adsorbent may sink in water after floating on the water surface for a certain period of time. If the oil adsorbent sinks in water, it becomes difficult to recover the oil adsorbent that has adsorbed oil.

[0005] Therefore, an object of the present invention is to provide an adsorbent for oil adsorption that floats on water and can sufficiently adsorb oil by using a relatively small amount of a specified compound, and a method for manufacturing the adsorbent for oil adsorption. [Means for solving the problem]

[0006] In order to achieve the above object, the present invention provides a water-floating adsorbent for adsorbing oil, the adsorbent comprising a cellulose-based material and a water-repellent agent contained in the cellulose-based material. Water repellent agents other than wax-based water repellent agents and silicone-based water repellent agents The present invention provides an adsorbent for adsorbing oil, which has a cellulosic material content of 95 wt % or more and a water repellent agent content of 0.2 wt % or more and 5.0 wt % or less, in terms of external proportion.

[0007] In order to achieve the above object, the present invention also provides a method for producing an adsorbent for adsorbing oil that floats on water, the method comprising: Excluding wax-based and silicone-based water repellents The present invention provides a method for manufacturing an adsorbent for oil adsorption, comprising a preparation step of preparing an aqueous solution of a water repellent by diluting the water repellent with water, and an impregnation step of impregnating a defibrated cellulosic material with the aqueous solution of the water repellent, the method comprising the steps of: (a) preparing an aqueous solution of the water repellent by diluting the water repellent with water; and (b) impregnating a defibrated cellulosic material with the aqueous solution of the water repellent, the method comprising the steps of: Effect of the Invention

[0008] According to the oil adsorbent and the manufacturing method of the oil adsorbent of the present invention, it is possible to provide an oil adsorbent that floats on water and can sufficiently adsorb oil by using a relatively small amount of a specified compound, and a manufacturing method of the oil adsorbent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Embodiment Mode] <Outline of oil adsorbent> The adsorbent for absorbing oil that floats on water according to an embodiment of the present invention is composed of a cellulosic material and a water repellent agent contained in the cellulosic material. That is, the adsorbent for absorbing oil that floats on water (hereinafter, sometimes simply referred to as an "adsorbent for absorbing oil" or an "adsorbent") has a cellulosic material and a water repellent agent, and the water repellent agent is impregnated or absorbed into the cellulosic material from the surface thereof. The adsorbent for absorbing oil is manufactured by adding a small amount (about several wt%) of the water repellent agent to the cellulosic material.

[0010] In this way, an oil adsorbent having a cellulosic material impregnated with a water repellent can adsorb a large amount of oil without sinking when placed in water that contains oil, even though only a small amount of water repellent has been added. Therefore, the oil adsorbent according to this embodiment can adsorb a large amount of oil simply by being placed in wastewater containing waste oil, and since it does not sink in the water even after adsorbing the oil (it does not sink in the water even when subjected to the water pressure from the flow of the wastewater), the oil adsorbent can be extremely easily recovered after adsorbing the oil.

[0011] <Details of oil adsorbent> The adsorbent for oil adsorption according to this embodiment is an adsorbent for oil adsorption that floats on water. The adsorbent for oil adsorption has a cellulosic material and a water repellent contained in the cellulosic material, and the cellulosic material is 95 wt% or more and the water repellent is 0.2 wt% or more and 5.0 wt% or less. The proportion of the water repellent added in this embodiment is calculated by an external ratio. For example, the ratio of the external ratio means a value expressed in wt% of the amount of the water repellent present in the cellulosic material when the mass of the cellulosic material is 100 wt%.

[0012] (Cellulosic materials) The cellulose-based material is a cellulose-based material having water absorption properties. Specifically, the cellulose-based material may be one or more types of cellulose fibers selected from plant-derived cellulose fibers, animal-derived cellulose fibers (e.g., cellulose fibers isolated from sea squirts, seaweed, etc.), and microorganism-derived cellulose fibers (e.g., cellulose fibers produced by acetic acid bacteria, etc.). Note that the cellulose-based material may be a material that has been previously impregnated with paraffin or the like and that has been discarded after being used for a specific purpose.

[0013] Examples of raw materials for plant-derived cellulose fibers include plant fibers such as pulp obtained from natural plant raw materials such as wood, bamboo, hemp, Manila hemp, sisal, jute, kenaf, cotton, beet, agricultural waste, and cloth. Examples of raw materials for cellulose fibers include paper (craft paper, copy paper, etc.), waste paper (newspaper waste, cardboard waste, magazine waste, copy paper waste, etc.), recycled paper, coated paper, craft paper, cardboard, waste cardboard, used tea leaves, coffee husks, cotton linters, and / or hemp bags. Examples of wood include cedar, cypress, eucalyptus, and acacia. The raw materials for cellulose fibers can be used alone or in combination of two or more.

[0014] In addition, the cellulose-based material is preferably a fibrous cellulose-based material obtained by subjecting a raw material to a defibration treatment, that is, a cellulose-containing material containing cellulose fibers. From the viewpoint of appropriately incorporating a water repellent into the cellulose-based material, the fiber length of the cellulose fiber obtained by subjecting the raw material to a defibration treatment is, for example, preferably 0.5 mm or more, preferably 1.0 mm or more, preferably 10.0 mm or less, preferably 5.0 mm or less, and preferably 2.5 mm or less. Similarly, the fiber width of the cellulose fiber obtained by subjecting the raw material to a defibration treatment is, for example, preferably 1 μm or more, preferably 10 μm or more, preferably 20 μm or more, preferably 200 μm or less, preferably 100 μm or less, preferably 50 μm or less, and preferably 30 μm or less.

[0015] (Amount of cellulosic material) The amount of cellulose-based material in the adsorbent for oil adsorption in this embodiment is 90 wt% or more, preferably 95 wt% or more, also preferably 98 wt% or more, and may be 99 wt% or more.

[0016] (Water repellent) As the water repellent, a compound that imparts water resistance to paper or the like can be used. Specifically, it is preferable to use a cationic or anionic sizing agent as the water repellent. As the sizing agent, a rosin-based sizing agent mainly composed of rosin, an alkylketene (AKD)-based sizing agent mainly composed of alkylketene dimer, an alkenylsuccinic anhydride-based sizing agent mainly composed of alkenylsuccinic anhydride, a styrene acrylate-based sizing agent mainly composed of synthetic resin, etc. can be used. From the viewpoint of making it easy to spray onto the cellulose-based material, the viscosity of these sizing agents at 25°C is 300 mPa·s or less, may be 200 mPa·s or less, may be 150 mPa·s or less, may be 100 mPa·s or less, or may be 50 mPa·s or less. In this embodiment, the water repellent agent does not include wax (wax-based water repellent), silicone-based water repellent, and / or zirconium-based water repellent.

[0017] (Water repellent content) In the adsorbent for adsorbing oil according to this embodiment, the blending amount of the water repellent is, by external percentage, 0.1 wt% or more, optionally 0.2 wt% or more, optionally 0.4 wt% or more, optionally 5.0 wt% or less, optionally 1.0 wt% or less, or optionally 2.0 wt% or less. Note that, relative to 100 parts by mass of the cellulose-based material, the blending amount of the water repellent may be 0.2 parts by mass or more, optionally 0.4 parts by mass or more, optionally 5.0 parts by mass or less, or optionally 2.0 parts by mass or less.

[0018] (Other additives) Various additives such as property adjusters, reinforcing agents, colorants, flame retardants, antioxidants, antiaging agents, antistatic agents, UV absorbers, UV dispersants, solvents, fragrances, deodorants, pigments, dyes, fillers, and talc may be added to the adsorbent for adsorbing oil according to this embodiment as necessary within the scope of not impairing the physical properties, etc., of the adsorbent for adsorbing oil.

[0019] (Water absorption of oil adsorbent) The adsorbent for adsorbing oil according to this embodiment is an adsorbent that floats on water. Specifically, when the adsorbent for adsorbing oil is placed in water, it floats on water for at least 24 hours or more from the time of placement. In addition, the adsorbent floats on water even after it has adsorbed oil.

[0020] (Ratio of oil absorption to the amount of water repellent added in an oil adsorbent) The oil adsorbent according to the present embodiment is manufactured so that the ratio of the oil absorption of the oil adsorbent to the amount of water repellent added during the manufacture of the oil adsorbent is equal to or greater than a predetermined value. For example, suppose that an oil adsorbent x (g) is put into water containing oil, and the oil adsorbent adsorbs y (g) of oil. Also, suppose that the amount of water repellent added during the manufacture of this oil adsorbent is a (wt%). In this case, the amount of water repellent in the oil adsorbent used to adsorb the oil is A = (a x) / 100 (g). Therefore, the ratio of the oil absorption to the amount of water repellent added (hereinafter, this ratio may be expressed as "B") is expressed as y / A (g / g).

[0021] In this embodiment, B is 100 or more, and may be 200 or more, 1,000 or more, 3,000 or more, or 5,000 or more.

[0022] <Other uses> The adsorbent according to this embodiment hardly absorbs water (that is, it does not absorb moisture), and therefore can be used for the following purposes.

[0023] (a) Anti-mold materials A mold-preventing member, A cellulosic material; A water repellent agent contained in the cellulosic material; having The cellulosic material is 95 wt% or more, The antifungal member has a water repellent agent content of 0.2 wt % or more and 5.0 wt % or less by external ratio.

[0024] The cellulosic material has a surface that contains a water repellent, which prevents moisture in the air from being absorbed into the cellulosic material, thereby preventing mold from growing on the mold-resistant component.

[0025] (b) Thermal insulation materials A thermal insulation member, A cellulosic material; A water repellent agent contained in the cellulosic material; having The cellulosic material is 95 wt% or more, The water repellent agent is contained in an amount of 0.2 wt % or more and 5.0 wt % or less by weight.

[0026] The cellulose-based material may be a cellulose-based material obtained by defibrating. This allows the cellulose-based material to be configured with voids, and the air contained in these voids provides heat insulation performance. In addition, the surface of the cellulose-based material contains a water repellent, which can prevent mold from growing on the heat-insulating member.

[0027] In addition, the respective components of the antifungal member and / or the heat insulating member may be the same as some or all of the components of the adsorbent for absorbing oil according to this embodiment.

[0028] <Manufacturing method 1 of oil adsorbent (sizing agent treatment method)> The adsorbent for oil adsorption that floats on water according to the present embodiment can be manufactured as follows. First, the raw material of the cellulosic material is defibrated by mechanical defibration or the like (defibration process). This results in a cellulosic material with a predetermined fiber length and a predetermined fiber width. Meanwhile, a water repellent aqueous solution is prepared by diluting a predetermined amount of a predetermined water repellent (sizing agent) with water (e.g., distilled water) (preparation process). Then, the defibrated cellulosic material obtained by the defibration process is impregnated with the water repellent aqueous solution prepared in the preparation process (impregnation process). In this case, the blending amounts of each material are adjusted so that the cellulosic material is 95 wt% or more and the water repellent is 0.2 wt% or more and 5.0 wt% or less in terms of external ratio. In the impregnation process, for example, the water repellent aqueous solution in the form of a mist is sprayed on the defibrated cellulosic material one or more times to impregnate the cellulosic material with the water repellent. This allows the water repellent to be impregnated from at least a part of the surface of the cellulosic material into the interior of the cellulosic material.

[0029] The cellulose-based material impregnated with the aqueous water repellent solution is then aged for a predetermined time in a predetermined container (aging step). After the aging step, the cellulose-based material impregnated with the aqueous water repellent solution is dried by heating or warming at a predetermined temperature for a predetermined time (drying step). This produces the adsorbent for adsorbing oil that floats on water according to the present embodiment.

[0030] <Method of manufacturing adsorbent for oil adsorption 2 (internal addition method)> The adsorbent for adsorbing oil that floats on water according to the present embodiment can also be manufactured by the following method. First, a raw material of a cellulosic material is defibrated by mechanical defibration or the like (defibration process). This results in a cellulosic material with a predetermined fiber length and a predetermined fiber width. The defibrated cellulosic material and a water repellent solution containing a predetermined amount of a predetermined water repellent are mixed in a container such as a tank to prepare a mixture (mixing process). Next, the mixed mixture is made into a sheet by papermaking through each process such as a predetermined preparation process using a wet papermaking device, a predetermined papermaking process, a predetermined sheeting process, and / or a drying process such as drying and winding. The sheet can also be wound up as a roll. The sheet is then defibrated by mechanical defibration or the like (re-defibration process) to manufacture the adsorbent for adsorbing oil that floats on water according to the present embodiment. In the mixing process, from the viewpoint of allowing the sheet obtained after each process using a wet papermaking apparatus to contain the desired concentration of water repellent (i.e., from the viewpoint of allowing the water repellent to remain at the desired concentration relative to the mass of defibrated cellulose after dehydration; specifically, from the viewpoint of allowing the cellulosic material in the sheet to be 95 wt% or more and the water repellent to be 0.2 wt% or more and 5.0 wt% or less), the concentration of the water repellent to be mixed with the cellulosic material is set to a concentration higher than the desired concentration to be contained in the sheet.

[0031] <Effects of the embodiment> The oil-adsorbing adsorbent according to the present embodiment can adsorb a large amount of oil while floating on the water, simply by incorporating a very small amount of water repellent into the cellulose-based material. As a result, the adsorbent according to the present embodiment can efficiently adsorb oil contained in wastewater from kitchens of hotels, inns, restaurants, cafeterias, and / or service areas, as well as food processing equipment. When the oil-adsorbing adsorbent according to the present embodiment is placed in a grease trap installed in a kitchen or the like, a large amount of oil can be adsorbed into the adsorbent while the adsorbent remains floating. Therefore, since the oil-adsorbing adsorbent according to the present embodiment floats on the water even when it has adsorbed a large amount of oil, it is easy to recover the adsorbent, and the work efficiency of oil recovery can be improved.

[0032] [Experimental Example] The present invention will be described in more detail below with reference to experimental examples. Note that these experimental examples are merely illustrative and should not be construed as limiting.

[0033] <Production of adsorbents for oil adsorption> (Preparation of Cellulosic Materials) The following raw materials were used as the cellulosic materials. ·cardboard ·Hemp bag Cotton linters

[0034] Each raw material was defibrated using a mechanical defibrator ("ATOMZ" manufactured by Ishikawa Soken Co., Ltd.) to obtain pass products (pass products, which are samples obtained by passing through a φ10 screen) with a screen diameter of φ10 (fiber length: 1 to 2.5 mm, fiber width: 20 to 30 μm). That is, the following pass products were obtained.

[0035] (Pass item list) · Cardboard fiber defibration products (φ10) ·Hemp bag defibration product (φ10) · Cotton linter defibrated (φ10)

[0036] (Sizing agent) On the other hand, the following sizing agents were used as water repellents. All of the following sizing agents are manufactured by Arakawa Chemical Industries, Ltd. Furthermore, "Sizepine" is a registered trademark. Size Pine K903-20 (solid content 20wt%) An alkyl ketene dimer (AKD) emulsion sizing agent that exhibits cationic properties. Size Pine 924 (solid content 30wt%) Anionic AKD emulsion sizing agent. Size Pine N-775 (solid content 50wt%) Anionic rosin emulsion sizing agent. Size Pine E (solid content 30wt%) Anionic rosin solution (neutralized salt) sizing agent.

[0037] (Production of adsorbents for oil adsorption - Experimental Examples 1 to 18) The adsorbent according to Experimental Example 1 was manufactured so that the solid content of the sizing agent (Size Pine K903-20) was 0.20 wt% (the amount of sizing agent added was 0.20 wt%) based on the mass of the raw material, defibrated cardboard (φ10). First, the sizing agent was diluted with distilled water to a predetermined concentration (1 g of sizing agent, 199 g of distilled water, concentration 0.1 wt%) to prepare 200 g of sizing agent aqueous solution. Next, 100 g of raw material was placed in a plastic bag, and the prepared sizing agent aqueous solution was sprayed onto the raw material with a spray bottle. Then, the raw material sprayed with the sizing agent aqueous solution in the plastic bag was aged at room temperature for 24 hours to allow the sizing agent to permeate the raw material. After aging, the raw material permeated with the sizing agent was placed in a shelf-type heating vacuum dryer and dried at 120°C for 1 hour under vacuum reduced pressure. As a result, the adsorbent according to Experimental Example 1 was obtained.

[0038] In the same manner as above, the adsorbent according to Experimental Example 2 (sizing agent: Size Pine K903-20, sizing agent added amount: 0.40 wt%), the adsorbent according to Experimental Example 3 (sizing agent: Size Pine K903-20, sizing agent added amount: 0.80 wt%), the adsorbent according to Experimental Example 4 (sizing agent: Size Pine K903-20, sizing agent added amount: 2.00 wt%), the adsorbent according to Experimental Example 5 (sizing agent: Size Pine 924, sizing agent added amount: 0.20 wt%), Adsorbent according to Experimental Example 6 (sizing agent: Size Pine 924, amount of sizing agent added: 0.40 wt%), Adsorbent according to Experimental Example 7 (sizing agent: Size Pine 924, amount of sizing agent added: 0.80 wt%), Adsorbent according to Experimental Example 8 (sizing agent: Size Pine 924, amount of sizing agent added: 1.00 wt%), Adsorbent according to Experimental Example 9 (sizing agent: Size Pine 924, amount of sizing agent added: 2.00 wt%), Adsorbent according to Experimental Example 10 (sizing agent: Size Pine 924, amount of sizing agent added: 2.00 wt%), 924, amount of sizing agent added: 4.00 wt%), adsorbent according to Experimental Example 11 (sizing agent: Sizepine N-775, amount of sizing agent added: 0.40 wt%), adsorbent according to Experimental Example 12 (sizing agent: Sizepine N-775, amount of sizing agent added: 1.00 wt%), adsorbent according to Experimental Example 13 (sizing agent: Sizepine N-775, amount of sizing agent added: 2.00 wt%), adsorbent according to Experimental Example 14 (sizing agent: Sizepine N-775, amount of sizing agent added: The following were produced: an adsorbent according to Experimental Example 15 (sizing agent: Sizepine N-775, sizing agent added amount: 4.00 wt%), an adsorbent according to Experimental Example 16 (sizing agent: Sizepine E, sizing agent added amount: 0.40 wt%), an adsorbent according to Experimental Example 17 (sizing agent: Sizepine E, sizing agent added amount: 1.00 wt%), and an adsorbent according to Experimental Example 18 (sizing agent: Sizepine E, sizing agent added amount: 2.00 wt%). In addition, a blank sample containing no sizing agent was produced by treating the raw material in the same manner using 200 g of tap water instead of a sizing agent.

[0039] Further, in the same manner as above, adsorbents according to the experimental examples were produced by applying each sizing agent to each raw material, and blank samples for each raw material were also produced. That is, adsorbents and blank samples according to experimental examples 19 to 21 were produced in the same manner as experimental examples 1 to 10, except that the raw material was a jute bag, and adsorbents and blank samples according to experimental examples 22 to 23 were produced in the same manner as experimental examples 5 to 10, except that the raw material was cotton linters. The blending amounts of the cellulose-based material and the sizing agent in each experimental example are as shown in Tables 1 to 3. Specifically, Table 1 shows the results of producing an adsorbent using a cardboard defibrated product, Table 2 shows the results of producing an adsorbent using a jute bag defibrated product, and Table 3 shows the results of producing an adsorbent using a cotton linter defibrated product.

[0040] [Table 1]

[0041] [Table 2]

[0042] [Table 3]

[0043] <Oil absorption test> The adsorbents according to the respective experimental examples and the blank sample were subjected to an oil absorption test as follows. First, the oils used in the oil absorption test were as follows.

[0044] (Oils used in oil absorption tests) Salad oil (Nisshin Oillio Group, Nisshin Canola Oil, density: 0.91g / ml) Dioctyl phthalate (Kanto Chemical Co., Ltd., Di-2-ethylhexyl Phthalate (Class 1), density: 0.95g / ml)

[0045] (Oil Absorption Test Procedure) The oil absorption test was carried out according to the following procedure. 1) Put 400cc of tap water and 110cc of oil into a 1000cc flask. 2) 10 g of the adsorbent according to Experimental Example 1 is placed in the flask prepared in 1) above. 3) After adding the adsorbent, stir at 200 rpm for 20 minutes. 4) After stirring, the floating adsorbent from Experimental Example 1 is scooped up with a net and allowed to stand on the top of the flask for 3 minutes (this allows the water adhering to the adsorbent and the oil not adsorbed by the adsorbent to be returned to the flask). 5) Transfer the water and oil remaining in the flask to a 500cc graduated cylinder and allow the phases to separate. 6) After phase separation, measure the volume (cc) of the oil layer and calculate the oil absorption (g) using the density of the oil.

[0046] The results of the oil absorption test carried out according to the above procedure are shown in Tables 4 to 6. Specifically, Table 4 shows the oil absorption test results for cardboard pulp products, Table 5 shows the oil absorption test results for hemp bag pulp products, and Table 6 shows the oil absorption test results for cotton linter pulp products. The adsorbents according to each experimental example except for the blank sample always floated on water from step 2) above to scooping with a net in step 4) above in the oil absorption test procedure. In addition, the adsorbents according to experimental examples 1 to 23 were placed in a beaker containing water and observed for 24 hours, and it was confirmed that all of the adsorbents floated on water after 24 hours had passed.

[0047] In Tables 4 to 6, the oil absorption rate of salad oil (ratio of oil absorption rate to the amount of water repellent added (g / g)) was calculated by the following formula.

[0048] Percentage of salad oil absorption = (100 x salad oil absorption (g)) / (amount of sizing agent added (wt%) x mass of adsorbent added (g))

[0049] In addition, in Tables 4 to 6, the ratio of oil absorption of dioctyl phthalate (ratio of oil absorption to the amount of water repellent added (g / g)) was calculated by the following formula.

[0050] Percentage of oil absorption of dioctyl phthalate = (100 x oil absorption of dioctyl phthalate (g)) / (amount of sizing agent added (wt%) x mass of adsorbent added (g))

[0051] [Table 4]

[0052] [Table 5]

[0053] [Table 6]

[0054] As can be seen from the results of the oil absorption test, in all of the adsorbents according to Experimental Examples 1 to 23, the ratio of the oil absorption amount to the amount of water repellent added was 100 or more, indicating that a very large amount of oil can be adsorbed by simply adding a very small amount of water repellent. It was also shown that all of the adsorbents according to Experimental Examples 1 to 23 were able to adsorb oil while floating on water.

[0055] Although the embodiments and experimental examples of the present invention have been described above, the embodiments and experimental examples described above do not limit the invention according to the claims. It should be noted that not all of the combinations of features described in the embodiments and experimental examples are essential to the means for solving the problems of the invention.

[0056] In addition, the adsorbent for absorbing oil according to this embodiment and the method for manufacturing the adsorbent for absorbing oil can also be referred to in the following appended claims, which should not be confused with the claims. (Additional note 1) An adsorbent for adsorbing oil that floats on water even after adsorbing oil, A fibrous cellulosic material; A water repellent agent impregnated (or absorbed) into the interior of the cellulosic material from the surface thereof; having The cellulosic material is 95 wt% or more, The water-floating adsorbent for adsorbing oil has a solid content of 0.1 wt% or more and 5.0 wt% or less. (Additional note 2) The adsorbent for adsorbing oil according to appended claim 1, wherein the water repellent is a sizing agent and excludes wax, silicone-based water repellent, and / or zirconium-based water repellent. (Additional note 3) The adsorbent for adsorbing oil according to claim 1, wherein the water repellent is impregnated into the interior of the cellulose-based material from at least a portion of the surface thereof. (Additional note 4) A method for producing a water-floating adsorbent for oil adsorption, comprising the steps of: A defibration step of defibrating a cellulosic material; A preparation step of preparing a water repellent aqueous solution by diluting the water repellent with water; an impregnation step of impregnating the defibrated cellulosic material with the water repellent aqueous solution; an aging step of aging the cellulose-based material impregnated with the water repellent aqueous solution; a drying step of drying the cellulose-based material impregnated with the water repellent aqueous solution after the aging step; Equipped with The cellulosic material is 95 wt% or more, A method for producing an adsorbent for adsorbing oil that floats on water, in which the water repellent is present in an amount of 0.2 wt% or more and 5.0 wt% or less.

Claims

1. A water-floating adsorbent for adsorbing oil, comprising: A cellulosic material; A water repellent agent contained in the cellulose-based material, the water repellent agent being excluding a wax-based water repellent agent and a silicone-based water repellent agent; having The cellulosic material is 95 wt % or more, The adsorbent for adsorbing oil has a water repellent content of 0.2 wt % or more and 5.0 wt % or less.

2. 2. The adsorbent for absorbing oil according to claim 1, which floats on water for at least 24 hours after being placed in water.

3. 2. The adsorbent for absorbing oil according to claim 1, wherein the ratio of the oil absorption amount of the adsorbent for absorbing oil to the amount of the water repellent added is 100 or more.

4. 2. The adsorbent for adsorbing oil according to claim 1, wherein the viscosity of the water repellent at 25° C. is 300 mPa·s or less.

5. The adsorbent for oil adsorption according to claim 1, wherein the raw material of the cellulosic material is at least one selected from the group consisting of paper, waste paper, recycled paper, coated paper, kraft paper, cardboard, waste cardboard, tea leaves, and hemp bags.

6. 2. The adsorbent for adsorbing oil according to claim 1, wherein the cellulosic material is a cellulose-containing material that has been subjected to a defibration treatment.

7. A method for producing a water-floating adsorbent for oil adsorption, comprising the steps of: A defibration step of defibrating a cellulosic material; A preparation step of preparing an aqueous solution of a water repellent by diluting a water repellent, excluding a wax-based water repellent and a silicone-based water repellent, with water; an impregnation step of impregnating the defibrated cellulosic material with the water repellent aqueous solution; Equipped with The cellulosic material is 95 wt % or more, A method for producing an adsorbent for adsorbing oil, wherein the water repellent is present in an amount of 0.2 wt % or more and 5.0 wt % or less by external ratio.

8. A method for producing a water-floating adsorbent for oil adsorption, comprising the steps of: A defibration step of defibrating a cellulosic material; a mixing step of mixing the defibrated cellulosic material with a water repellent solution containing a water repellent other than a wax-based water repellent and a silicone-based water repellent to obtain a mixture; a papermaking step of papermaking the mixture to obtain a sheet; a re-fibrillation process for defibrating the sheet; Equipped with The cellulosic material is 95 wt % or more, A method for producing an adsorbent for adsorbing oil, wherein the water repellent is present in an amount of 0.2 wt % or more and 5.0 wt % or less by external ratio.

Citation Information

Patent Citations

  • Oil adsorbent and its production

    JP1979158391A

  • Absorbent of organic liquid

    JP1985150832A

  • Manufacturing method of oil adsorbent body

    JP2009165914A

  • Liquid adsorbing material, and liquid adsorbing body obtained by using the material

    JP2016198723A

  • Sheet-like oil adsorbent comprising biodegradable fiber