Carbon material filler for electromagnetic wave shielding, electromagnetic wave shielding material, and carbon material-containing compact for electromagnetic wave shielding
A lightweight, easily graphitizable carbon material with controlled crystal structure addresses the limitations of existing carbon materials by providing high electromagnetic shielding in a single component, suitable for resin-based applications.
Patent Information
- Application Number
- JP2021057699
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-30
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing carbon materials for electromagnetic shielding are either heavy, costly, or require multiple materials to achieve sufficient shielding properties, making them impractical for many applications.
A lightweight, easily graphitizable carbon material with controlled crystal structure is developed, characterized by specific X-ray diffraction parameters and particle size, which can be used alone for high electromagnetic shielding.
The carbon material achieves high electromagnetic shielding properties while maintaining lightness and cost-effectiveness, suitable for various resin-based applications.
Smart Images

Figure 0007561078000003 
Figure 0007561078000004 
Figure 0007561078000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon filler for electromagnetic shielding, and an object of the present invention is to provide a carbon material filler for electromagnetic shielding made of an easily graphitizable carbon material that has light weight not possible with conventional electromagnetic shielding materials and is capable of exhibiting high electromagnetic shielding properties. [Background technology]
[0002] In recent years, various systems using mobile communications, sensors using radio waves, and monitoring devices have evolved and spread remarkably, and are now widely installed in everyday devices in our daily lives.
[0003] However, in our daily lives, when communication systems are used extensively, it has been pointed out that in devices that use similar frequencies between different systems, the original systems may be affected by other communication radio waves and malfunction. In fact, system failures due to sensor malfunctions have been confirmed.
[0004] Furthermore, when strong radio waves are used at similar frequencies in wireless or radio systems, noise can occur, rendering the system unusable.
[0005] To deal with such cases, electromagnetic shielding materials made of conductive iron foil, wire mesh, or thin copper fibers, as well as conductive paints with electromagnetic shielding properties, have traditionally been used.
[0006] In particular, in the case of resin molded products, because resin is not conductive, efforts have been made to impart electromagnetic wave shielding properties by blending conductive metal fillers or metal fibers, or various carbon materials or carbon fibers, to create conductive resin compositions.
[0007] Among these, carbon materials have attracted attention as fillers for resin compositions having electromagnetic wave shielding properties because of their low specific gravity compared to metallic inorganic materials, and various development examples have been reported.
[0008] Patent Documents 1 to 4 are documents relating to various carbon materials used in resin compositions having electromagnetic wave shielding properties. Patent Document 1 proposes that carbon black and graphite can be used in combination with characteristic particle sizes to achieve high electromagnetic wave shielding properties. In addition, Patent Document 2 proposes a combination of expanded graphite and carbon fiber, and Patent Document 3 proposes a combination of furnace black and short carbon fiber. Furthermore, Patent Document 4 proposes blending carbon nanotubes, carbon black, and carbon fiber.
[0009] However, these carbon materials are insufficient to provide sufficient electromagnetic wave shielding properties. Therefore, Patent Documents 5 to 7 propose that metallic and inorganic conductive fillers be added to the combination of these various carbon materials to obtain even higher electromagnetic shielding properties.
[0010] Patent Document 5 proposes a carbon black composition that uses carbon black in combination with a metal component such as Ni. Patent Document 6 proposes the combined addition of an inorganic filler, carbon black, and stainless steel fiber. Patent Document 7 proposes a material that uses a combination of metal-coated carbon fiber and graphite. Patent Document 8 proposes the use of a conductive powder material that uses heat-treated coal coke powder in combination with carbon (graphite) or a metal-based flake filler as an electromagnetic wave shielding material.
[0011] However, although these proposed examples have high electromagnetic wave shielding properties, they are not necessarily preferable as practical electromagnetic wave shielding materials because they require a combination of multiple materials, the use of metal-based materials in combination increases the specific gravity, and the use of carbon fiber increases the material costs. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2003-258491 A [Patent Document 2] JP 2000-95947 A [Patent Document 3] Japanese Patent Application Publication No. 8-172292 [Patent Document 4] JP 2014-133842 A [Patent Document 5] Special Publication No. 2006-513120 [Patent Document 6] Japanese Patent Application Publication No. 6-73248 [Patent Document 7] JP 2005-298653 A [Patent Document 8] Japanese Patent Publication No. H6-251620 Summary of the Invention [Problem to be solved by the invention]
[0013] As mentioned above, various materials with electromagnetic wave shielding properties have been proposed, but there are no examples yet of a material that has high electromagnetic wave shielding properties, is low cost, and is lightweight, all of which can be achieved using carbon materials alone. An object of the present invention is to provide a carbon material filler for electromagnetic shielding, which is made of an easily graphitizable carbon material and has light weight that has not been achieved with conventional electromagnetic shielding materials, and which is capable of exhibiting high electromagnetic shielding properties. [Means for solving the problem]
[0014] As a result of intensive research by the present inventors to improve these drawbacks, they focused on the relationship between the crystal structure of a carbon material and the electromagnetic shielding property, and by controlling the crystal structure of an easily graphitizable carbon material, the crystal structure of which can be controlled and prepared relatively freely, they realized an easily graphitizable carbon material that exhibits high electromagnetic shielding property while maintaining the light weight characteristic of carbon materials. That is, the present inventors have completed the present invention by specifying the composition ratio of the main crystal face and the secondary crystal face to be within a certain range in an easily graphitizable carbon material, the crystal structure of which can be controlled and prepared relatively freely.
[0015] The present invention relates to a filler made of an easily graphitizable carbon material that is blended with a resin material in order to absorb electromagnetic waves, and is a carbon material filler for electromagnetic wave shielding that satisfies the following (1) to (3). (1) The lattice spacing d 002 of the 002 plane of the graphitizable carbon material as measured by X-ray diffraction (XRD) is 0.338 nm or more. (2) When the graphitizable carbon material is measured by X-ray diffraction (XRD), the relative intensity ratio (A / B) of the peak intensity (A) of the "002 plane" detected therein to the higher peak intensity (B) selected from the "100 plane" and the "004 plane" is 2.5 or more and less than 27. (3) It is in powder form and the average particle diameter D50 is 1 μm or more and 5 mm or less.
[0016] In the carbon material filler for electromagnetic wave shielding of the present invention, the raw material of the graphitizable carbon material is preferably coal and / or heavy oil derived from petroleum, and further preferably is in the form of powder having an average particle size D50 of 5 μm or more and 3 mm or less.
[0017] The present invention provides an electromagnetic wave shielding material, characterized in that the above-mentioned electromagnetic wave shielding carbon material filler is blended with a molding material selected from a thermoplastic resin, a thermosetting resin, or a binder pitch. The present invention relates to an electromagnetic wave shielding carbon material-containing molded body, which is characterized by being prepared by blending the above-mentioned electromagnetic wave shielding carbon material filler with a molding material selected from a thermoplastic resin, a thermosetting resin, or a binder pitch, and solidifying the mixture. Effect of the Invention
[0018] According to the present invention, by using a specific graphitizable carbon material filler as an electromagnetic wave shielding carbon material filler, high electromagnetic wave shielding properties can be achieved even with a single filler. A composition containing this graphitizable carbon material filler in a resin material or binder pitch is useful as an electromagnetic wave shielding material, and by molding and solidifying this electromagnetic wave shielding material, it is possible to provide a carbon material-containing molded body for electromagnetic wave shielding that is lightweight and easily processed into various shapes. [Brief description of the drawings]
[0019] [Figure 1] 1 is an XRD chart of Example 1 (electromagnetic wave shielding: 62 dB). [Diagram 2] 1 is an XRD chart of Comparative Example 1 (electromagnetic wave shielding: 11 dB). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described in detail below.
[0021] There are many types of carbon materials, from graphite, coal, charcoal, and carbon black to graphitizable and non-graphitizable carbon, but the carbon material used as the carbon material filler for electromagnetic shielding in the present invention is required to be a graphitizable carbon material. Here, a graphitizable carbon material is a carbon material whose crystal structure easily changes depending on the heat treatment temperature and history time, and can ultimately have a graphite structure by heat treatment at 2500°C or higher. More specifically, the graphitizable carbon, which is the carbon material of the present invention, is a carbon material having a lattice spacing d002 of 002 planes of 0.338 nm or more as measured by an X-ray diffractometer (XRD), preferably in the range of 0.343 to 0.360 nm. If d002 is less than 0.338 nm, the carbon material will be graphitized too much, and will become flaky when crushed, resulting in an excessively large specific surface area that makes it difficult to fill resins, or will deviate from the crystal structure with high electromagnetic wave shielding properties described below, making it unsuitable.
[0022] The graphitizable carbon material as the electromagnetic wave shielding carbon material filler of the present invention preferably has a relative intensity ratio α (=A / B) value between the peak intensity (A) of the "002 plane" detected in X-ray diffraction measurement (XRD) and a higher peak intensity (B) selected from the "100 plane" and the "004 plane" of the main crystal plane constituting the carbon material and that is 2.5 or more and less than 27, more preferably 16.0 or more and less than 26.5, and most preferably 19.0 or more and less than 26.0. In the present invention, these peak heights (intensities) were measured, and the peak of the "002 plane" having the highest peak height was defined as the first peak intensity (A), and either the "100 plane" or the "004 plane" having a higher peak height than the other was defined as the second peak intensity (B), and the relative intensity ratio (A / B) of these peaks was calculated. By setting the composition ratio of the main crystal face (002 face) to the secondary crystal face (100 face or 004 face) within the above-mentioned predetermined range, high electromagnetic wave shielding properties can be achieved. The peak intensity of the main crystal plane (002 plane) is preferably 1000 cps or more, more preferably 5000 cps or more, and further preferably 10000 cps or more. The upper limit is preferably 13000 cps or less, and more preferably 12000 cps or less. The peak intensity of the secondary crystal plane (100 plane or 004 plane) is preferably 100 cps or more, more preferably 200 cps or more. The upper limit is preferably 1000 cps or less, more preferably 700 cps or less.
[0023] The graphitizable carbon material as the carbon material filler for electromagnetic shielding of the present invention has a volume resistivity of 2.0 mΩcm or less. It is presumed that the electromagnetic shielding property of a carbon material is due to its electrical conductivity, and when the volume resistivity is 2.0 mΩcm or less, a certain degree of electromagnetic shielding property can be exhibited even when the carbon material is used alone.
[0024] The carbonaceous filler for electromagnetic shielding of the present invention is desirably in the form of a powder having an average particle diameter D50 of 1 μm or more and 5.0 mm or less. The particle diameter D50 is more preferably 5.0 μm to 3.0 mm, and most preferably 10.0 μm to 2.5 mm. Even if the particle diameter D50 is 5.0 mm or more, the electromagnetic shielding property is sufficiently exhibited, but handling during kneading and molding is difficult, and it is difficult to prepare a shape with a desired strength due to the generation of voids, etc.
[0025] The carbon material filler preferably has an ellipse long-to-short ratio of 0.1 to 0.5, more preferably 0.2 to 0.4. Since the shape of the carbon material filler is affected by the degree of growth of the carbon crystals, a ratio of ellipse long-to-short in the above range can achieve a balance between compoundability as a filler and electromagnetic wave shielding performance. The ellipse long / short ratio is a value obtained by observing a cross section of a carbon material filler embedded in a resin or the like using a SEM or other method to determine the ellipse-equivalent minor axis length (La) and ellipse-equivalent major axis length (Lb), calculating the (La) / (Lb) ratio, and then averaging the results for several tens of particles or more. Specifically, particle images observed using a SEM or other method can be analyzed using image analysis software (WinROOF, manufactured by Mitani Shoji Co., Ltd.) or the like.
[0026] The raw material for the easily graphitizable carbon material to be used as the carbon material filler for electromagnetic shielding of the present invention can be petroleum- or coal-based heavy oil, synthetic resin, or the like. However, heavy oil derived from coal or petroleum is preferable. It is particularly preferable to use coal-based heavy oil, which is rich in aromatic properties and therefore provides a good yield of carbon material, has a low corrosive sulfur (S) content, and is low in impurities such as vanadium (V) and iron (Fe), as well as volatile matter. Examples of petroleum heavy oils include petroleum pitch, asphalt, heavy oils, heavy crude oil, etc., and examples of coal heavy oils include coal tar, tar heavy oil, tar pitch, etc., which are by-produced in coke ovens when producing coke for steelmaking used in blast furnaces. These may be hydrogenated, or a blend of coal heavy oil and petroleum heavy oil may be used.
[0027] The method for producing the graphitizable carbon material is not particularly limited in the present invention as long as it is a generally known method, but it is preferable to use the delayed coking method from the viewpoint of mass production.
[0028] Hereinafter, the production of the carbon material filler of the present invention using the delayed coking method will be described, but it should be noted in advance that the method is not limited to the described method, and the carbon material filler of the present invention can also be obtained by methods other than the delayed coking method.
[0029] The delayed coking method for producing graphitizable carbon materials from coal-based heavy oil involves first obtaining a carbonized product from the raw material heavy oil by carrying out thermal decomposition and polycondensation reactions of the raw material coal-based heavy oil in a delayed coker or the like at a maximum temperature of about 400°C to 700°C for about 24 hours.
[0030] Next, the above-mentioned carbide is coarsely crushed and fired in a rotary kiln at a maximum temperature of 800°C to 1500°C in a low-oxygen atmosphere, thereby adjusting the crystal structure of the graphitizable carbon material so that it exhibits XRD parameters suitable for use as the carbon material filler for electromagnetic wave shielding of the present invention. The calcination treatment removes moisture and volatile matter in the carbonized material and converts the remaining hydrocarbons as polymer components into carbon to promote crystal growth. The calcination temperature is preferably in the range of 700 to 2000°C, more preferably 900 to 1500°C. For the calcination of carbides, equipment capable of large-scale heat treatment, such as lead hammer furnaces, shuttle furnaces, tunnel furnaces, roller hearth kilns, and microwaves, other than rotary kilns, can be used, but is not limited to these. Furthermore, these calcination equipment may be either continuous or batch type.
[0031] The coal-based raw coke or calcined coke obtained above is cooled, pulverized and classified by a jet mill or the like to adjust the particle size to a desired size, and then used as a carbon material filler for electromagnetic wave shielding.
[0032] The carbon material filler of the present invention has a sufficient electromagnetic wave shielding effect by itself, but can also impart a wider range of electromagnetic wave shielding performance by using it in combination with materials such as metal powder or magnetic powder.
[0033] In practical use, the carbon material filler for electromagnetic shielding of the present invention is used as a carbon material-containing molded body for electromagnetic shielding, solidified with a thermoplastic resin, a thermosetting resin, or a binder pitch, etc., as a binder for producing a molded body of any shape. In this case, for example, a molded body having electromagnetic shielding properties can be produced by cutting a large solid ingot of the graphitizable carbon material of the present invention, but this is not a desirable method because it increases the processing cost in practical use. In addition, since it is expected that the carbon material-containing molded body for electromagnetic shielding will be used in various shapes, a thermoplastic resin or a thermosetting resin that can be used with conventional equipment and does not change significantly in handling is more preferable as a binder. More preferably, the electromagnetic shielding carbon material filler of the present invention is blended and kneaded with a thermoplastic resin such as polypropylene or nylon, and then the mixture is injection or extrusion molded to obtain an electromagnetic shielding composite molding. The electromagnetic shielding molding thus obtained can be widely used in the fields of home appliances, industrial machinery, transportation, etc., and is particularly suitable for use in transportation equipment, etc., since it is lightweight due to the use of a carbon material filler. EXAMPLES
[0034] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the following examples, various measurements and evaluations were performed as follows.
[0035] [Electromagnetic shielding measurement] The electromagnetic shielding was measured using a KEC method evaluation device manufactured by Techno Science Japan, which conforms to the KEC method developed by the Kansai Electronics Industry Development Center (KEC), a general incorporated association, and the shielding performance of electromagnetic waves with a frequency of 1 MHz was evaluated. A value of 50 dB or more was rated as "○".
[0036] [Measurement of d002 by X-ray diffraction] The interplanar spacing (d) of the 002 plane of the sample measured with a BRUKER DISCOVOER-D8 was calculated from the diffraction angle θ of the maximum peak intensity at about 26° due to the 002 plane by the Bragg formula d=λ / {2×Sin(θ / 2)}. Note that λ was calculated using the wavelength of 0.15405 nm of Cu Kα1, the X-ray diffraction source used.
[0037] [Measurement of peak intensities and their ratios in X-ray diffraction] Using a BRUKER DISCOVOER-D8 machine, the X-ray diffraction pattern of the sample carbon material at diffraction angles of 10 to 90 degrees was measured, and the peak intensities of the X-ray diffraction peak at about 26° due to the 002 plane, the X-ray diffraction peak at about 43° due to the 100 plane, and the X-ray diffraction peak at about 54° due to the 004 plane were calculated, and the relative intensity ratio (A / B) of these peaks was calculated as the peak intensity of the "002 plane" (A) and the higher peak intensity selected from the "100 plane" and "004 plane" (B). In calculating the peak intensities, the line connecting the left and right inflection points of the diffraction peaks is used as the baseline, and a perpendicular line is drawn from the apex of each peak to the horizontal axis of the graph. The diffraction intensity (cps) of the length from the intersection of the baseline and the perpendicular line to the apex is used as the peak height (intensity).
[0038] [Method of measuring average particle size (D50)] Measurements were performed using an LA-920 (HORIBA) with a dispersion medium of water + surfactant (Lion Corporation, trade name Mama Lemon). The average particle size (D50) is the volume average particle size.
[0039] Examples 1 to 4, Comparative Examples 1 to 3 Coal-derived heavy oil was used as the raw material, and the delayed coking method was used to obtain raw coke by pyrolysis and polycondensation reaction at a temperature of about 500°C for about 24 hours using a delayed coker. The raw coke was then fired in a rotary kiln at a total of seven maximum temperatures within the range of 800°C to 1800°C in a low-oxygen atmosphere, producing seven types of graphitizable carbon materials with different crystal structures. These several types of graphitizable carbon materials were pulverized and classified in a jet mill so that the D50 was 25 μm or less, to obtain carbon material fillers for electromagnetic shielding. The crystal structure of each of the obtained carbon material fillers for electromagnetic shielding was measured by X-ray diffraction. Next, a commercially available polypropylene resin was used as a binder, and 60 parts by weight of the carbon material filler for electromagnetic shielding and 40 parts by weight of polypropylene resin were mixed, and the mixture was solidified using an injection molding machine to produce a flat plate of 150 mm x 150 mm x 3 mm thick. The electromagnetic shielding properties of this plate (molded product) were measured, and the results are shown in Table 1.
[0040] [Table 1]
[0041] Examples 5 to 7, Comparative Examples 4 to 5 Using the same graphitizable carbon material as in Example 3, and in the same manner as in Example 3, except for changing the grinding conditions, several types of electromagnetic shielding carbon material fillers having a particle size of D50 were used, and then a binder was used to solidify the mixture, thereby producing flat plates (electromagnetic shielding carbon material-containing compacts). The electromagnetic shielding property was measured using this flat plate, and the moldability was also evaluated. The results are shown in Table 2. Note that, although Examples 5 to 7 all had good moldability (◯), Comparative Example 4 (D50: 0.5 μm) had poor moldability (△) due to increased viscosity, and Comparative Example 5 (D50: 5,500 μm) was brittle, making it impossible to produce a flat plate (×).
[0042] [Table 2]
[0043] As can be seen from the results of the Examples and Comparative Examples in Table 1, it has been confirmed that an electromagnetic wave shielding carbon material filler having high electromagnetic wave shielding properties can be obtained by appropriately selecting and controlling the structure of the main crystal plane constituting the carbon material of the graphitizable carbon material, which is an electromagnetic wave shielding carbon material filler, i.e., the relative intensity ratio (A / B) value between the peak intensity (A) of the "002 plane" detected when measured by X-ray diffraction measurement (XRD) and a higher peak intensity (B) selected from the "100 plane" and "004 plane." Furthermore, as can be seen from the results of the Examples and Comparative Examples in Table 2, even if the same graphitizable carbon material is used, ease of use in actual use differs depending on the particle size. Therefore, it was confirmed that within a specified particle size range, an electromagnetic shielding carbon material filler having high electromagnetic shielding properties and excellent moldability can be obtained.
Claims
1. A carbon material filler for electromagnetic wave shielding, which is made of an easily graphitizable carbon material and is blended into a molding material in order to absorb electromagnetic waves, and which satisfies the following (1) to (3): (1) The lattice spacing d 002 of the 002 plane of the graphitizable carbon material as measured by X-ray diffraction (XRD) is 0.338 nm or more. (2) When the graphitizable carbon material is subjected to X-ray diffraction measurement (XRD), the relative intensity ratio (A / B) value between the peak intensity (A) of the “002 plane” and a higher peak intensity (B) selected from the “100 plane” and the “004 plane” is 2.5 or more and less than 27. (3) It is in powder form and has an average particle diameter D50 of 1 μm or more and 5 mm or less.
2. 2. The carbon material filler for electromagnetic shielding according to claim 1, wherein the raw material of the easily graphitizable carbon material is coal and / or heavy oil derived from petroleum.
3. 3. The carbonaceous filler for electromagnetic shielding according to claim 1 or 2, having an average particle diameter D50 of 5 μm or more and 3 mm or less.
4. 4. An electromagnetic shielding material comprising the carbon material filler for electromagnetic shielding according to claim 1 blended with a molding material selected from a thermoplastic resin, a thermosetting resin, or a binder pitch.
5. 4. An electromagnetic wave shielding carbon material-containing molded body, comprising: the electromagnetic wave shielding carbon material filler according to claim 1; and a molding material selected from a thermoplastic resin, a thermosetting resin, or a binder pitch; and solidifying the mixture.
Citation Information
Patent Citations
Electromagnetic shielding resin composition
JP1994073248A
Conductive resin composition and electromagnetic wave shield material using the composition
JP1994251620A
Rubber-based radio-wave absorbing material
JP1996172292A
Conductive resin composition
JP2000095947A
Electromagnetic wave shielding material
JP2003258491A