Processing solution, substrate processing method, and semiconductor substrate manufacturing method

A processing liquid with a water-soluble organic solvent and metal ions addresses the challenge of removing resist patterns and embedded materials without corroding low-k dielectric materials, enhancing semiconductor substrate manufacturing efficiency.

JP7561261B1Active Publication Date: 2024-10-03TOKYO OHKA KOGYO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023211054
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-10-03
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

Existing semiconductor manufacturing processes face challenges in effectively removing resist patterns and other embedded materials while preventing corrosion of low-k dielectric materials, which are prone to damage during etching processes.

Method used

A processing liquid comprising a water-soluble organic solvent, water, and ions of typical metal elements, specifically Group 1, Group 2, and Group 13 metal ions, is used to enhance the removability of embedded materials and inhibit corrosion of low-k materials.

Benefits of technology

The solution provides excellent removability of embedded materials and effective corrosion inhibition of low-k materials, ensuring high-quality semiconductor substrate production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561261000001
    Figure 0007561261000001
  • Figure 0007561261000002
    Figure 0007561261000002
  • Figure 0007561261000003
    Figure 0007561261000003
Patent Text Reader

Abstract

The present invention provides a processing solution, a substrate processing method, and a semiconductor substrate manufacturing method, which are excellent in terms of removability of a filling material and corrosion inhibition of a low-k material. The present invention provides a processing solution for semiconductor devices, comprising (a) a water-soluble organic solvent, (b) water, and (c) ions of a main group metal element.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a processing liquid, a substrate processing method, and a semiconductor substrate manufacturing method. [Background technology]

[0002] A semiconductor device is formed by laminating a metal wiring layer, a low dielectric layer, an insulating layer, etc. on a substrate such as a silicon wafer, and such a semiconductor device is manufactured by processing each of the above-mentioned layers using a lithography method in which etching is performed using a resist pattern as a mask.

[0003] Resist patterns and filling materials (temporary laminated films, sacrificial layers, sacrificial films, spin-on-glass (SOG) materials, trench filling, etc.) used in the lithography method, as well as residues from the metal wiring layer and low-dielectric layer generated in the etching process, are removed using a cleaning solution so as not to impede the semiconductor device or to hinder the next process.

[0004] In recent years, with the increasing density and integration of semiconductor devices, a wiring formation method using the damascene process has been adopted. In such a wiring formation method, copper, which is prone to corrosion, is used as the metal wiring material constituting the metal wiring layer of the semiconductor device, and further, the dielectric constant of the low dielectric material (also called ILD material) constituting the low dielectric layer is becoming lower and lower, and ILD materials, which are prone to corrosion, are being used. Therefore, there is a demand for the development of a cleaning solution that does not cause corrosion of these easily corrodible materials when cleaning substrates.

[0005] Furthermore, in wiring formation methods using the damascene process, the materials used as temporary laminated films (sacrificial layers, sacrificial films, etc.) during etching processing and the ILD materials have very similar compositions, and there is a need to develop a cleaning solution that can leave one of these very similar materials (the ILD material) on the device without causing corrosion, while efficiently removing the other (the temporary laminated film).

[0006] As a technique relating to a cleaning solution for lithography used in such a semiconductor device manufacturing process, Patent Document 1 discloses a cleaning solution used in forming a dual damascene structure, in which a low dielectric layer laminated on a substrate having a metal layer is etched to form a first etching space, a sacrificial layer is filled in the first etching space, and then the low dielectric layer and the sacrificial layer are partially etched to form a second etching space communicating with the first etching space, and the sacrificial layer remaining in the first etching space is removed, the cleaning solution containing (a) 1 to 25 mass % of a quaternary ammonium hydroxide, (b) 30 to 70 mass % of a water-soluble organic solvent, and (c) 20 to 60 mass % of water. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2004-103771 A Summary of the Invention [Problem to be solved by the invention]

[0008] Incidentally, for example, when etching a low dielectric layer using a resist pattern as a mask, it is necessary to remove the remaining resist pattern and unnecessary layers and films to be removed after the etching process using a processing liquid. However, it is difficult to remove resists altered by etching and layers and films with high crosslinking density, while the low-k material constituting the low dielectric layer is easily corroded. For these reasons, it is required to effectively remove the filling material while suppressing the corrosion of the low-k material, but in reality, there is still room for improvement in this regard.

[0009] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a treatment liquid, a substrate treatment method, and a semiconductor substrate manufacturing method that are excellent in terms of removability of a filling material and corrosion inhibition of a low-k material. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors have conducted intensive research in order to achieve the above-mentioned object, and have discovered the necessity of creating a treatment liquid for semiconductor devices that contains (a) a water-soluble organic solvent, (b) water, and (c) ions of a typical group metal element, thereby completing the present invention.

[0011] That is, the present invention is as follows. <1> The treatment liquid for semiconductor devices contains (a) a water-soluble organic solvent, (b) water, and (c) ions of a typical metal element. <2> The (c) ions of typical metal elements include at least one type of ion selected from the group consisting of (c-1) ions of Group 1 metal elements, (c-2) ions of Group 2 metal elements, and (c-3) ions of Group 13 metal elements. <1> It is a processing solution described in <3> The (c) ions of typical metal elements include (c-1) ions of a Group 1 metal element, (c-2) ions of a Group 2 metal element, and (c-3) ions of a Group 13 metal element. <1> or <2> It is a processing solution described in <4> The (c-1) Group 1 metal element ion is a potassium ion and / or a sodium ion. <2> or <3> It is a processing solution described in <5> The (c-2) Group 2 metal element ion is a magnesium ion and / or a calcium ion. <2> ~ <4> The present invention relates to a processing liquid according to any one of the above items. <6> The (c-3) ion of a Group 13 metal element is a boron ion and / or an aluminum ion. <2> ~ <5> The present invention relates to a processing liquid according to any one of the above items. <7> The (c-1) Group 1 metal element ion is added to the treatment solution at a concentration of 5×10 4 ppb quality quantity ~1×10 7 ppb quality quantityinclude, <2> ~ <6> The present invention relates to a processing liquid according to any one of the above items. <8> The (c-2) Group 2 metal element ion is added to the treatment solution at a concentration of 1×10 1 ppb quality quantity ~1×10 3 ppb quality quantity include, <2> ~ <7> The present invention relates to a processing liquid according to any one of the above items. <9> The (c-3) ions of the Group 13 metal element are added to the treatment solution at a concentration of 1×10 0 ppb quality quantity ~1×10 2 ppb quality quantity include, <2> ~ <8> The present invention relates to a processing liquid according to any one of the above items. <10> Further, (d) a base other than the component (a), the component (b), and the component (c) is contained. <1> ~ <9> The present invention relates to a processing liquid according to any one of the above items. <11> The (d) base is a quaternary ammonium hydroxide compound. <10> It is a processing solution described in <12> A preparation step of obtaining a laminated substrate including a substrate, a low dielectric layer laminated on the substrate, and a resist pattern laminated on the substrate; <1> ~ <11> and a treatment step of treating a substrate with the treatment liquid according to any one of claims 1 to 5. <13> The preparation step is a step of obtaining the laminated substrate by a damascene method. <12> 2. A method for treating a substrate according to claim 1. <14> A preparation step of obtaining a laminated substrate including a substrate, a low dielectric layer laminated on the substrate, and a resist pattern laminated on the substrate; <1> ~ <11> and a treatment step of treating the semiconductor substrate with the treatment liquid according to any one of claims 1 to 5. <15> and forming a metal wiring by filling a pattern space of the resist pattern with a metal after the treatment step. <14> 2 is a method for producing a semiconductor substrate according to the present invention. <16> The preparation step is a step of obtaining the laminated substrate by a damascene method. <14> or <15> 2 is a method for producing a semiconductor substrate according to the present invention. Effect of the Invention

[0012] According to the present invention, it is possible to provide a processing liquid, a substrate processing method, and a semiconductor substrate manufacturing method that are excellent in terms of removability of a filling material and corrosion inhibition of a low-k material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0014] <Processing solution>

[0015] The treatment liquid according to this embodiment is a treatment liquid for semiconductor devices, which contains (a) a water-soluble organic solvent, (b) water, and (c) ions of a typical metal element.

[0016] (a) Water-soluble organic solvent

[0017] The treatment liquid according to this embodiment contains (a) a water-soluble organic solvent. Examples of the component (a) include highly polar solvents having a dipole moment of 3.0 D or more, glycol ether solvents, polyhydric alcohols, and the like.

[0018] Specific examples of highly polar solvents include sulfoxides such as dimethyl sulfoxide (DMSO) (dipole moment: 4.6 D); sulfones such as dimethyl sulfone (dipole moment: 5.1 D), diethyl sulfone (dipole moment: 4.7 D), and tetramethylene sulfone (dipole moment: 5.0 D); N,N-dimethylformamide (DMF) (dipole moment: 4.5 D), N-methylformamide (DMF) (dipole moment: 4.5 D), and N-methylformamide (DMF) (dipole moment: 4.5 D). amides such as N-methyl-2-pyrrolidone (NMP) (dipole moment: 4.6 D), N,N-dimethylacetamide (DMAc) (dipole moment: 4.6 D), N-methylacetamide (dipole moment: 4.3 D), and N,N-diethylacetamide (dipole moment: 4.7 D); N-methyl-2-pyrrolidone (NMP) (dipole moment: 4.6 D), N-ethyl-2-pyrrolidone (dipole moment: 4.7 D), and N-hydroxy ...). lactams such as N-pyrrolidone (dipole moment: 3.1D), N-hydroxyethyl-2-pyrrolidone (dipole moment: 6.1D); β-propiolactone (dipole moment: 4.6D), γ-butyrolactone (GBL) (dipole moment: 5.1D), γ-valerolactone (dipole moment: 5.3D), δ-valerolactone (dipole moment: 5.4D), γ-caprolactone (dipole moment: 5 and lactones such as 1,3-dimethyl-2-imidazolidinone (DMI) (dipole moment: 4.5D), 1,3-diethyl-2-imidazolidinone (dipole moment: 4.5D), 1,3-diisopropyl-2-imidazolidinone (dipole moment: 4.3D).

[0019] Among these, preferred are highly polar solvents having a dipole moment of 3.5 to 7.0 D, and more preferred are highly polar solvents having a dipole moment of 4.0 to 6.0 D. In particular, from the viewpoint of stability in alkaline chemical solutions, preferred are one or more selected from the group consisting of sulfoxides, amides, lactams, and lactones, and more preferred are one or more selected from the group consisting of dimethyl sulfoxide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, and γ-butyrolactone.

[0020] Examples of glycol ether solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, diethylene glycol monomethyl ether (MDG), diethylene glycol monoethyl ether (EDG), diethylene glycol monopropyl ether, and diethylene glycol monobutyl ether (BDG).

[0021] Among these, from the viewpoints of water solubility, resist pattern removal performance, flammability, and the like, at least one selected from the group consisting of diethylene glycol monomethyl ether (MDG), diethylene glycol monoethyl ether (EDG), diethylene glycol monopropyl ether, and diethylene glycol monobutyl ether (BDG) is preferred, and at least one selected from the group consisting of diethylene glycol monomethyl ether (MDG), diethylene glycol monoethyl ether (EDG), and diethylene glycol monobutyl ether (BDG) is more preferred.

[0022] Examples of polyhydric alcohols include ethylene glycol, propylene glycol, butylene glycol, glycerin, etc. Among these, from the viewpoints of safety, viscosity, etc., it is preferable to use at least one selected from the group consisting of ethylene glycol, propylene glycol, and glycerin.

[0023] (a) The water-soluble organic solvent may be one of the above, or two or more of them may be used in combination. As an example of a preferred combination, it is preferable to use two or more selected from the group consisting of a highly polar solvent having a dipole moment of 3.0D or more, a glycol ether-based solvent, and an alcohol; it is more preferable to use a highly polar solvent having a dipole moment of 3.0D or more, a glycol ether-based solvent, and a polyhydric alcohol; it is more preferable to use one or more selected from the group consisting of sulfoxides, amides, lactams, and lactones as the highly polar solvent, at least one selected from the group consisting of diethylene glycol monomethyl ether (MDG), diethylene glycol monoethyl ether (EDG), and diethylene glycol monobutyl ether (BDG) as the glycol ether-based solvent, and ethylene glycol monoethyl ether (EDG) as the polyhydric alcohol. and at least one selected from the group consisting of ethylene glycol, propylene glycol, and glycerin; and still more preferably at least one selected from the group consisting of dimethyl sulfoxide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, and γ-butyrolactone as a highly polar solvent, at least one selected from the group consisting of diethylene glycol monomethyl ether (MDG), diethylene glycol monoethyl ether (EDG), and diethylene glycol monobutyl ether (BDG) as a glycol ether solvent, and at least one selected from the group consisting of ethylene glycol, propylene glycol, and glycerin as a polyhydric alcohol.

[0024] The content of the (a) water-soluble organic solvent is preferably 15 to 80% by mass based on the total amount of the treatment liquid. The lower limit is more preferably 20% by mass or more, and even more preferably 25% by mass or more. The upper limit is more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0025] When a highly polar solvent is contained, the content of the highly polar solvent is preferably 5 to 60 mass% based on the total amount of the treatment liquid. The lower limit is more preferably 10 mass% or more, and more preferably 20 mass% or more. The upper limit is more preferably 50 mass% or less, and more preferably 30 mass% or less. By setting the content of the highly polar solvent within the above range, the removability of the filling material and the effect of inhibiting corrosion of the low-k material can be further improved.

[0026] When a glycol ether solvent is contained, the content of the glycol ether solvent is preferably 5 to 55 mass% based on the total amount of the treatment liquid. The lower limit is more preferably 10 mass% or more, and even more preferably 15 mass% or more. The upper limit is more preferably 30 mass% or less, and even more preferably 20 mass% or less. By setting the content of the glycol ether solvent within the above range, it is possible to further improve the removability of the filling material and the effect of inhibiting corrosion of the low-k material.

[0027] When a polyhydric alcohol is contained, the content of the polyhydric alcohol is preferably 5 to 30 mass % based on the total amount of the treatment liquid. The lower limit is more preferably 10 mass % or more, and even more preferably 15 mass % or more. The upper limit is more preferably 25 mass % or less. By setting the content of the polyhydric alcohol within the above range, it is possible to further improve the removability of the filling material and the effect of inhibiting corrosion of the low-k material.

[0028] ((b) water)

[0029] The treatment liquid according to the present embodiment contains (b) water. The content of (b) water may be contained as the balance of components other than water. The content of (b) water is preferably 15% by mass to 85% by mass with respect to the total amount of the treatment liquid. The lower limit may be 20% by mass or more, 25% by mass or more, or may be a value greater than 40% by mass. The upper limit may be less than 80% by mass, less than 75% by mass, less than 65% by mass, or less than 60% by mass. By setting the content of water within the above range, the removability of the filling material and the effect of inhibiting corrosion of the low-k material can be further improved.

[0030] ((c) Ions of main group metal elements)

[0031] The treatment liquid according to the present embodiment contains (c) ions of a typical metal element. The component (c) preferably contains at least one metal ion selected from the group consisting of (c-1) ions of a Group 1 metal element, (c-2) ions of a Group 2 metal element, and (c-3) ions of a Group 13 metal element.

[0032] (c-1) Examples of ions of Group 1 metal elements include lithium (Li) ions, sodium (Na) ions, potassium (K) ions, rubidium (Rb) ions, and cesium (Cs) ions. Among these, potassium ions and sodium ions are preferred. It is more preferred that the treatment liquid according to this embodiment contains potassium ions and / or sodium ions.

[0033] (c-2) Examples of ions of Group 2 metal elements include beryllium (Be) ions, magnesium (Mg) ions, calcium (Ca) ions, strontium (Sr) ions, barium (Ba) ions, etc. Among these, magnesium ions and calcium ions are preferred. It is more preferred that the treatment liquid according to this embodiment contains magnesium ions and / or calcium ions.

[0034] (c-3) Examples of ions of Group 13 metal elements include boron (B) ions, aluminum (Al) ions, gallium (Ga) ions, and indium (In) ions. Among these, boron ions and aluminum ions are preferred. The treatment liquid according to the present embodiment further preferably contains boron ions and / or aluminum ions.

[0035] In the case where the component (c) contains ions of a Group 1 metal element (c-1), the content of the ions of the Group 1 metal element (c-1) is 5×10 4 ppb quality quantity ~1×10 7 ppb quality quantity The lower limit is preferably 1×10 5 ppb quality quantity It is preferable that the value is 3×10 or more. 5 ppb quality quantity More preferably, it is 4×10 or more. 5 ppb quality quantity More preferably, the upper limit is 1×10 6 ppb quality quantity It is more preferable that it is 9×10 or less. 5 ppb quality quantity More preferably, it is 8×10 or less. 5 ppb quality quantity It is even more preferable that the total amount of the component (c-1) is within the above range. When two or more types of ions are contained as the component (c-1), it is preferable that the total amount of the component (c-1) is within the above range.

[0036] When the (c-2) ion of a Group 2 metal element is contained as the (c) component, the content of the (c-2) ion of the Group 2 metal element is 1×10 1 ppb quality quantity ~1×10 3 ppb quality quantity The lower limit is preferably 5×10 1 ppb quality quantity More preferably, it is 1×10 2 ppb quality quantity More preferably, it is 1.5×10 or more.2 ppb quality quantity More preferably, the upper limit is 7×10 2 ppb quality quantity More preferably, it is 6×10 2 ppb quality quantity More preferably, it is 5×10 or less. 2 ppb quality quantity It is even more preferable that the total amount of the component (c-2) is within the above range. When two or more types of ions are contained as the component (c-2), the total amount of the component (c-2) is preferably within the above range.

[0037] In the case where the component (c) contains ions of a Group 13 metal element (c-3), the content of the ions of the Group 13 metal element (c-3) is 1×10 0 ppb quality quantity ~1×10 2 ppb quality quantity The lower limit is preferably 5×10 0 ppb quality quantity More preferably, it is 1×10 1 More preferably, it is 1.5×10 1 It is even more preferable that the concentration is ppb by weight or more. The upper limit is 9×10 1 ppb quality quantity More preferably, it is 7×10 or less. 1 ppb quality quantity More preferably, it is 6×10 1 ppb quality quantity More preferably, it is 5×10 or less. 1 ppb quality quantity It is even more preferable that the total amount of the component (c-3) is within the above range. When two or more types of ions are contained as the component (c-3), the total amount of the component (c-3) is preferably within the above range.

[0038] ((d) Base)

[0039] The treatment liquid according to the present embodiment preferably further contains (d) a base. The (d) base is a base other than the (a), (b), and (c) components. Examples of the (d) base include quaternary ammonium hydroxide compounds such as tetramethylammonium hydroxide (TMAH) and tetraethylammonium hydroxide (TEAH). Among these, quaternary ammonium hydroxide compounds are preferred, and tetramethylammonium hydroxide (TMAH) and tetraethylammonium hydroxide (TEAH) are more preferred.

[0040] When the (d) base is contained, the content of the (d) base is preferably 0.5% by mass to 20% by mass based on the total amount of the treatment liquid. The lower limit is more preferably 2% by mass or more, and even more preferably 4% by mass or more. The upper limit is more preferably 18% by mass or less, and even more preferably 15% by mass or less. By setting the content of the (d) base within the above range, the removability of the filling material and the effect of inhibiting corrosion of the low-k material can be further improved. Note that, when two or more types of bases are contained as the (d) component, the total amount of the (d) component is preferably within the above range.

[0041] (e) Corrosion inhibitors

[0042] The treatment liquid according to the present embodiment may further contain (e) an anticorrosive agent. The treatment liquid according to the present embodiment is expected to simultaneously achieve the anticorrosive effect of (e) the anticorrosive agent. The (e) anticorrosive agent is preferably at least one selected from the group consisting of benzotriazole-based compounds and mercapto group-containing compounds.

[0043] The benzotriazole-based compound includes, for example, a compound represented by the following general formula (1).

[0044] [ka]

[0045] In the above general formula (1), R 1 , R 2each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, a carboxyl group, an amino group, a hydroxyl group, a cyano group, a formyl group, a sulfonylalkyl group, or a sulfo group, and P represents a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 14 carbon atoms which may have a substituent (provided that the hydrocarbon group may be interrupted by an amide bond or an ester bond), or a group represented by the following general formula (2):

[0046] [ka]

[0047] In the above general formula (2), R 3 represents an alkylene group having 1 to 6 carbon atoms; R 4 , R 5 each independently represents a hydrogen atom, a hydroxyl group, or a hydroxyalkyl group or alkoxyalkyl group having 1 to 6 carbon atoms.

[0048] In the above general formula (1), R 1 , R 2 In the definitions of P, the hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, may have an unsaturated bond, and may be any of linear, branched, and cyclic. Examples of aromatic hydrocarbon groups include phenyl and p-tolyl groups. Examples of linear aliphatic hydrocarbon groups include methyl, n-propyl, and vinyl groups. Examples of branched aliphatic hydrocarbon groups include isobutyl and tert-butyl groups. Examples of cyclic aliphatic hydrocarbon groups include cyclopentyl and cyclohexyl groups. Examples of substituted hydrocarbon groups include hydroxyalkyl and alkoxyalkyl groups.

[0049] In addition, in the above general formula (1), P is preferably a group represented by the above general formula (2). In particular, among the groups represented by the above general formula (2), R 4 , R 5are preferably selected as groups each independently being a hydroxyalkyl group or an alkoxyalkyl group having 1 to 6 carbon atoms.

[0050] Furthermore, P is preferably selected so that the compound represented by the above general formula (1) exhibits water solubility. Specifically, P is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms (i.e., a methyl group, an ethyl group, a propyl group, an isopropyl group), a hydroxyalkyl group having 1 to 3 carbon atoms, a hydroxyl group, etc.

[0051] Examples of benzotriazole compounds include benzotriazole, 5,6-dimethylbenzotriazole, 1-hydroxybenzotriazole, 1-methylbenzotriazole, 1-aminobenzotriazole, 1-phenylbenzotriazole, 1-hydroxymethylbenzotriazole, 1-methylbenzotriazole, 5-benzotriazolecarboxylic acid, 1-methoxy-benzotriazole, 1-(2,2-dihydroxyethyl)-benzotriazole, 1-(2,3-dihydroxypropyl)benzotriazole, 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, 2,2'-{[(5-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethane, and 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bispropane. Among these, 1-(2,3-dihydroxypropyl)-benzotriazole, 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, 2,2'-{[(5-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, etc. are preferably used. These may be used alone or in combination of two or more.

[0052] The mercapto group-containing compound is preferably a compound having a hydroxyl group and / or a carboxyl group at at least one of the α-position and β-position of the carbon atom bonded to the mercapto group. Examples of such compounds include 1-thioglycerol, 3-(2-aminophenylthio)-2-hydroxypropyl mercaptan, 3-(2-hydroxyethylthio)-2-hydroxypropyl mercaptan, 2-mercaptopropionic acid, and 3-mercaptopropionic acid. Among these, 1-thioglycerol is preferred. These may be used alone or in combination of two or more.

[0053] (Surfactant)

[0054] The treatment liquid according to the present embodiment may contain a surfactant as necessary. As such a surfactant, an acetylene alcohol-based surfactant or the like can be preferably used. The content of the surfactant is preferably less than 0.5% by mass with respect to the total amount of the treatment liquid.

[0055] <Processing methods, semiconductor substrate manufacturing methods, wiring formation methods, etc.>

[0056] The treatment liquid according to the present embodiment is a treatment liquid for lithography, but can be suitably used for treating a laminated substrate that has been etched. For example, there can be mentioned a method for treating a substrate, which includes a preparation step for obtaining a laminated substrate including a substrate, a low dielectric layer laminated on the substrate, and a resist pattern laminated on the substrate, and a treatment step for treating the laminated substrate with the treatment liquid described above.

[0057] The preparation process for obtaining the laminated substrate described above may include a process (pre-process) of preparing a laminated substrate including a substrate, a low dielectric layer formed on a surface of the substrate, and a resist pattern formed on the surface of the substrate, and a process (etching process) of forming an etching space in the resist pattern of the laminated substrate by etching treatment.

[0058] The preparation step for obtaining the multilayer substrate is preferably performed using a damascene method, that is, the preparation step described above is preferably a step for obtaining the multilayer substrate using a damascene method.

[0059] The layer structure of the laminated substrate to be processed may include a substrate, a low dielectric layer, and a resist pattern layer, and may be a multilayer structure including other layers. For example, various layers described later may be provided between the substrate and the low dielectric layer, or between the low dielectric layer and the resist pattern layer, or an additional layer may be provided on the resist pattern layer.

[0060] The treatment liquid and the treatment method according to the present embodiment can be suitably used in a method for manufacturing a semiconductor substrate. For example, the treatment liquid and the treatment method can be suitably used in a method for manufacturing a semiconductor substrate when treating a laminated substrate that has been etched. A suitable example of a method for manufacturing a semiconductor substrate includes a preparation step of obtaining a laminated substrate including a substrate, a low dielectric layer laminated on the substrate, and a resist pattern laminated on the substrate, and a treatment step of treating the laminated substrate with the treatment liquid described above.

[0061] Furthermore, the method for producing a semiconductor substrate preferably includes, after the treatment step, a step of forming metal wiring by filling the pattern spaces of the resist pattern with metal. By carrying out such a step, fine metal wiring can be formed in spaces such as via holes and trenches, and a semiconductor substrate having a damascene structure, which will be described later, can be obtained.

[0062] The preparation step for obtaining the multilayer substrate is preferably performed using a damascene method, that is, the preparation step described above is preferably a step for obtaining the multilayer substrate using a damascene method.

[0063] As described above, the treatment liquid according to this embodiment is a treatment liquid for lithography, but can be suitably used in a wiring formation method using a damascene method in particular. More specifically, it can be used in a wiring formation method using a damascene method in which a metal wiring layer is formed by filling a pattern space (etching space, etc.) formed in a low dielectric layer using a resist pattern with a metal. The treatment liquid according to this embodiment can be suitably used in both a single damascene process and a dual damascene process. Several aspects will be described below as examples.

[0064] An example of a wiring formation method using the damascene method is to form a resist pattern (e.g., a trench resist pattern) as a mask on a low dielectric layer formed on a substrate, and then etch the low dielectric layer to form an etching space (trench pattern, groove), and fill the etching space with metal to form a metal wiring. A bottom anti-reflective coating (BARC) or the like may be formed under the resist pattern. A sacrificial film may also be temporarily filled in the etching space.

[0065] As a more specific example, a semiconductor substrate with a dual damascene structure of Cu metal wiring will be described. In the case of Cu metal wiring, the etching resistance of Cu is low, so a method of forming Cu multilayer wiring using a damascene method can be suitably used. Various methods have been proposed as the dual damascene method, and one example is to provide a Cu layer on a substrate, stack a low dielectric layer, and then form a photoresist pattern on the top layer by lithography technology. Using this photoresist pattern as a mask, the low dielectric layer is etched to form a via hole that communicates with the Cu layer. Then, the photoresist pattern is peeled off. Then, a sacrificial layer such as an alkoxysilane material is filled in the via hole. Next, a new photoresist pattern is formed on the top layer of the remaining multilayer stack, and using this as a mask, the low dielectric layer and the sacrificial layer are etched to form a wiring groove (trench) that communicates with the via hole, and then the sacrificial layer remaining in the via hole is washed and removed. Then, after peeling off the photoresist pattern, the via hole and the trench are filled with Cu by plating or the like, thereby forming a multilayer Cu wiring.

[0066] The treatment liquid according to the present embodiment can effectively remove the resist pattern after etching, and the residues derived from the low dielectric layer and the metal wiring layer generated in the etching process. In addition, the treatment liquid according to the present embodiment is excellent in stripping the filling material and inhibiting the corrosion of the low-k material, so that it is possible to effectively remove the resist pattern, the lower anti-reflective film, and the like while suppressing the corrosion of the ILD material. Therefore, it can be suitably used when removing at least the resist pattern and the lower anti-reflective film after forming an etching space in the low dielectric layer using the resist pattern and the lower anti-reflective film.

[0067] The method for removing the resist pattern and the residue using the treatment liquid according to this embodiment is not particularly limited as long as it is a commonly used removal method. Specifically, for example, the treatment is performed by contacting the treatment liquid according to this embodiment with the substrate using a dipping method, a paddle method, a shower method, etc. The dipping time is not particularly limited, but is, for example, 5 seconds to 60 minutes, and the dipping temperature is not particularly limited, but is, for example, 20 to 80°C.

[0068] Here, as the material for forming the resist pattern, a resist material commonly used for (KrF, ArF, F2, EUV) excimer laser or electron beam can be used in a conventional manner. As the material for forming the lower anti-reflection film, a commonly used inorganic or organic lower anti-reflection film material can be used in a conventional manner.

[0069] Using such resist material and underlayer anti-reflective coating material, a resist pattern and underlayer anti-reflective coating are formed on the interlayer insulating layer or the barrier layer thereon, and after pattern exposure through a mask, a resist pattern is formed by developing. Next, the resist pattern residue after etching using this resist pattern as a mask is removed by the treatment liquid according to this embodiment together with other residues derived from the underlayer anti-reflective coating, the sacrificial film, and the metal wiring layer and the low dielectric layer generated in the etching process.

[0070] The low dielectric layer such as the above-mentioned low-k film is specifically a layer formed of, for example, a carbon-doped oxide (SiOC)-based, methylsilsesquioxane (MSQ)-based, or hydroxysilsesquioxane (HSQ)-based material. In order not to affect the electrical properties of the metal wiring layer, the low dielectric layer preferably has a dielectric constant (k) of 3.0 or less.

[0071] Moreover, examples of the barrier layer include SiC, SiN, SiCN, Ta, TaN, etc. Such a barrier layer may be formed between low dielectric layers.

[0072] In addition, the metal material for forming the metal wiring layer used in the Damascene method is mainly Cu, but conductive materials other than Cu, such as Al, Ti, and W, are also laminated on the same substrate. According to the treatment liquid of this embodiment, even if the cleaning liquid comes into contact with these metal materials, corrosion can be effectively suppressed.

[0073] The treatment solution according to this embodiment is useful in the Damascene method, particularly in the wiring formation method in which a sacrificial film is temporarily provided in the formed etching space, and specifically, as a material (filling material) for forming such a sacrificial film, a spin-on-glass (SOG) material obtained by a condensation reaction is suitable. The spin-on-glass material can also be used to reduce the step of an interlayer insulating film, fill the groove between wiring, etc.

[0074] As the spin-on glass material for forming the sacrificial film, for example, those described in JP-A-2001-092122 can be used. As a specific example of the spin-on glass material, a compound obtained by hydrolyzing at least one compound selected from the compounds represented by the following general formulas (3) to (5) under the action of an acid in the presence of water is preferable. From this viewpoint, as the spin-on glass material, a compound obtained by hydrolyzing a combination of a compound represented by the following general formula (3) and a compound represented by the following general formula (4) under the action of an acid in the presence of water is more preferable.

[0075] [ka]

[0076] In the above general formulas (3) to (5), R 6 ~R 9 , R 11 ~R 13 , R 16 , and R 17 each independently represents an alkyl group having 1 to 4 carbon atoms or a phenyl group; R 10 , R 14 , and R 15each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0077] Among the compounds represented by the above general formula (3), tetramethoxysilane or tetraethoxysilane, or their oligomers are preferred. Among the compounds represented by the above general formula (4), trimethoxysilane or triethoxysilane, or their oligomers are preferred. Furthermore, among the compounds represented by the above general formula (5), dimethoxysilane, diethoxysilane, methyldimethoxysilane, or their oligomers are preferred. These spin-on glass materials can be used alone or in combination of two or more.

[0078] Furthermore, a highly absorbent substance may be appropriately blended with the compounds represented by the general formulas (3) to (5). Such highly absorbent substances are not particularly limited as long as they have a substituent in their structure that can be condensed with the spin-on-glass material, have high absorption ability for light in the photosensitive wavelength range of the photosensitive component in the resist material, and prevent standing waves caused by reflected light from the substrate and diffuse reflection due to steps on the substrate surface. For example, sulfone-based compounds, benzophenone-based compounds, anthracene-based compounds, and naphthalene-based compounds substituted with hydroxyl and / or carboxyl groups are included. In particular, bisphenylsulfone-based compounds and benzophenone-based compounds having at least two hydroxyl groups, anthracene-based compounds having at least one hydroxyl and / or hydroxyalkyl group, anthracene-based compounds having a carboxyl and / or hydroxyl group, and naphthalene-based compounds substituted with at least one carboxyl and / or hydroxyl group are preferred.

[0079] The content of the high-absorbent substance in the spin-on-glass material is preferably 10 to 50 mass %, and more preferably 15 to 40 mass %, in terms of SiO2 solid content concentration. EXAMPLES

[0080] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples. Unless otherwise specified, the experiments were carried out at 25° C. under atmospheric pressure.

[0081] (Preparation of Lithography Processing Solution)

[0082] Lithography cleaning solutions were prepared based on the compositions and amounts of ingredients shown in Tables 1 to 4. Unless otherwise specified, commercially available reagents were used for each reagent. The values ​​in the tables are expressed in units of mass %.

[0083] The abbreviations in the table are as follows. TMAH: Tetramethylammonium hydroxide TEAH: Tetraethylammonium hydroxide DMSO: Dimethyl sulfoxide NMP: N-methyl-2-pyrrolidone DMF: N,N-dimethylformamide GBL: gamma-butyrolactone EDG: Diethylene glycol monoethyl ether MDG: Diethylene glycol monomethyl ether BDG: Diethylene glycol monobutyl ether PG: Propylene glycol EG: Ethylene glycol

[0084] For example, the cleaning solution for lithography in Example 1 contains (a) 5% by mass of dimethyl sulfoxide (DMSO), 35% by mass of diethylene glycol monoethyl ether (EDG), and 20% by mass of propylene glycol (PG) as water-soluble organic solvents, and (c-1) 2×10 Na ions as Group 1 metal element ions. 2 ppb quality quantity , and K ions 5 x 10 5 ppb quality quantity (c-2) As an ion of a Group 2 metal element, Mg ion 2×10 2ppb quality quantity , and Ca ions 5 x 10 -1 ppb quality quantity (c-3) As the ion of the Group 13 metal element, B ion 2×10 1 ppb quality quantity , and Al ions 4 x 10 -1 ppb quality quantity and (d) 10 mass % of tetramethylammonium hydroxide (TMAH) as a base, and the remainder being (b) water.

[0085] [Table 1]

[0086] [Table 2]

[0087] [Table 3]

[0088] [Table 4]

[0089] (Peelability of embedding material)

[0090] First, a sample substrate was prepared by depositing a filler made of a spin-on-glass material on a laminate substrate having a Cu layer on a Si substrate. The spin-on-glass material used was in accordance with the description in JP 2001-092122 A. Then, the sample substrate was immersed in the cleaning solution for lithography of each example and each comparative example at 50° C. for 1 minute, and then rinsed with pure water. The peeling state of the filler at this time was evaluated by measuring the film thickness of the Cu layer. The results are shown in Table 5.

[0091] (Corrosion inhibition of low-k materials)

[0092] First, a sample substrate was prepared by forming a low dielectric layer (dielectric constant 2.7 to 2.8) by CVD deposition on a laminate substrate having a Cu layer on a Si substrate. Then, a trench resist pattern was formed as a mask on the low dielectric layer of the sample substrate by lithography. The low dielectric layer was formed by firing the same type of material as the spin-on glass material disclosed in JP-A-2001-092122 at a temperature lower than the crystallization temperature. Then, the low dielectric layer was dry etched to form a trench pattern, thereby obtaining a patterned substrate.

[0093] The patterned substrate was immersed in the cleaning solution for lithography of each Example and Comparative Example at 50°C for 10 minutes, and then rinsed with pure water. The corrosion state of the low-k material at this time was evaluated by observation with an SEM (scanning electron microscope, Hitachi "S-5200"). The results are shown in Table 5.

[0094] In the evaluation results in Table 5, "A" and "B" indicate that good strippability or corrosion inhibition was observed, with "A" indicating that particularly good strippability or corrosion inhibition was observed, while "C" indicates that strippability or corrosion inhibition was insufficient.

[0095] [Table 5]

[0096] From the above, it was confirmed that the treatment liquid of this example is at least excellent in removing the filling material and inhibiting corrosion of the low-k material.

Claims

1. (a) as a water-soluble organic solvent, at least one selected from the group consisting of dimethyl sulfoxide, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol, and glycerin; (b) water; (c) ions of typical metal elements: (c-1) potassium ions and sodium ions as ions of Group 1 metal elements, (c-2) magnesium ions and calcium ions as ions of Group 2 metal elements, and (c-3) boron ions and aluminum ions as ions of Group 13 metal elements; (d) tetramethylammonium hydroxide as a base other than the component (a), the component (b), and the component (c); A processing solution for semiconductor devices comprising: The treatment liquid contains the component (a) in an amount of 20% by mass to 80% by mass based on the total mass of the treatment liquid, (c-1) The treatment solution contains ions of a Group 1 metal element in an amount of 4×10 5 ppb to 8×10 5 ppb by mass relative to the total mass of the treatment solution; The (c-2) Group 2 metal element ion is added to the treatment solution at a concentration of 1×10 1 ppb mass ~ 5×10 2ppb mass included, (c-3) the treatment solution contains ions of a Group 13 metal element in an amount of 5×10 0 ppb to 5×10 1 ppb by mass relative to the total mass of the treatment solution; The (d) component is contained in an amount of 4% by mass to 15% by mass. Processing fluid for semiconductor devices.

2. A preparation step of obtaining a laminated substrate, the laminated substrate including a substrate, a low dielectric layer laminated on the substrate, and a resist pattern laminated on the substrate; A treatment step of treating the laminated substrate with the treatment liquid according to claim 1; A method for processing a substrate, comprising:

3. The preparation step is a step of obtaining the laminated substrate by a damascene method. The method for processing a substrate according to claim 2 .

4. A preparation step of obtaining a laminated substrate, the laminated substrate including a substrate, a low dielectric layer laminated on the substrate, and a resist pattern laminated on the substrate; A treatment step of treating the laminated substrate with the treatment liquid according to claim 1; A method for manufacturing a semiconductor substrate, comprising:

5. and forming a metal wiring by filling a pattern space of the resist pattern with a metal after the treatment step. The method for manufacturing a semiconductor substrate according to claim 4 .

6. The preparation step is a step of obtaining the laminated substrate by a damascene method. The method for manufacturing a semiconductor substrate according to claim 4 .

Citation Information

Patent Citations

  • Washing liquid used for dual damascene structure formation process, and processing method of substrate

    JP2004103771A

  • Treatment liquid for manufacturing semiconductor and pattern forming method

    JP2020122983A

  • Treatment liquid and treatment method

    WO2019151141A1