How to cut composite materials

A method for dividing composite materials by forming processing grooves in the resin layer, using ultrashort pulse laser processing on the brittle material layer, and applying thermal stress from the opposite side to separate it, addresses the issue of cracks and resin deterioration, achieving clean separation with minimal thermal discoloration.

JP7561735B2Active Publication Date: 2024-10-04NITTO DENKO CORP

Patent Information

Application Number
JP2021532670
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-16
Filing Date
2020-02-19
Publication Date
2024-10-04
Estimated Expiration
2040-02-19

AI Technical Summary

Technical Problem

Existing methods for dividing composite materials with a brittle material layer and a resin layer, such as glass and polarizing film, result in cracks on the end faces of the brittle material layer and deteriorate the quality of the resin layer due to heat from ultrashort pulse laser processing.

Method used

A method involving the use of a first laser to form processing grooves in the resin layer, followed by ultrashort pulse laser processing on the brittle material layer to create machining marks, and then applying thermal stress from a second laser from the opposite side to separate the brittle material layer without causing cracks, while minimizing heat conduction to the resin layer.

Benefits of technology

The method effectively divides the composite material without cracks on the brittle material layer and maintains the quality of the resin layer, reducing thermal discoloration to less than 1000 μm from the end face.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561735000001
    Figure 0007561735000001
  • Figure 0007561735000002
    Figure 0007561735000002
  • Figure 0007561735000003
    Figure 0007561735000003
Patent Text Reader

Abstract

[Problem] To provide a method for dividing a composite material, said method causing no cracks in end surfaces of a brittle material layer and causing no deterioration in the quality of end parts of a resin layer. [Solution] The present invention is a method for dividing a composite material 10 wherein a brittle material layer 1 and a resin layer 2 are superposed upon each other, said method being characterized by comprising: a resin removal step wherein the resin layer is irradiated with laser light L1 oscillated from a first laser light source 20a along a planned dividing line DL of the composite material, thereby forming a processing groove 25 that extends along the planned dividing line; a brittle material removal step wherein the brittle material layer is irradiated with laser light L2 oscillated from an ultrashort pulse laser light source 30 along the planned dividing line after the resin removal step, thereby forming a processing mark 11 that extends along the planned dividing line; and a brittle material layer dividing step wherein a thermal stress is generated in the brittle material layer by irradiating a surface of the brittle material layer, said surface being on the reverse side from the resin layer, with laser light L3 oscillated from a second laser light source 20b after the brittle material layer removal step, thereby dividing the brittle material layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for dividing a composite material in which a brittle material layer and a resin layer are laminated, and in particular to a method capable of dividing a composite material without causing cracks on the end surface of the brittle material layer and without deteriorating the quality of the end portion of the resin layer. [Background technology]

[0002] In recent years, LCD panels have become thinner and more highly detailed, and in order to add variety to interfaces, LCD panels equipped with on-screen touch sensor functions are now being used in a wide range of fields, from mobile phones to information displays. A typical LCD panel equipped with a touch sensor function is one in which a film or glass having a sensor function is laminated on a polarizing film, and a reinforced glass called a front panel is placed on the top surface via a thick adhesive layer (OCA, Optical Clear Adhesive) to fill in the steps on the sensor surface. Recently, from the viewpoint of thinness and weight reduction, LCD panels with in-cell type liquid crystal cells in which a touch sensor is built into the glass substrate of the liquid crystal cell have appeared.

[0003] On the other hand, a front panel made of resin is used, and although efforts have been made to increase the hardness of this resin front panel, the current situation is that sufficient hardness has not been achieved. In addition, resin front panels have the problem of being poor in resistance to moisture.

[0004] Therefore, a film-like glass called thin glass is attracting attention as a front panel to be placed on the top surface of a liquid crystal panel. Thin glass can be wound into a roll, so it has the advantage of being adaptable to the so-called roll-to-roll manufacturing process, and a glass polarizing film integrated with a polarizing film has been proposed (for example, see Patent Document 1). Glass polarizing film can be used to produce an LCD panel equipped with a touch sensor function simply by bonding it to an in-cell type LCD cell, making the manufacturing process much simpler than that of conventional LCD panels that use tempered glass as a front panel.

[0005] Incidentally, as a method for cutting a composite material in which a brittle material layer made of glass or the like and a resin layer made of a polarizing film or the like are laminated as described above into a desired shape and size according to an application, there is a method in which the resin layer is laser processed and the brittle material layer is processed with a mechanical tool (for example, see Patent Document 2). However, according to the investigations conducted by the present inventors, it has been found that if the brittle material layer is processed with a mechanical tool after the resin layer is laser processed, cracks may occur on the end surface of the brittle material layer.

[0006] Here, a technology is known for precision machining of brittle materials such as glass by irradiating the brittle material with laser light (ultrashort pulse laser light) oscillated from an ultrashort pulse laser light source different from the laser light source used in the above-mentioned laser machining (see, for example, Patent Document 3). The machining technology using ultrashort pulse laser light as described in Patent Document 3 is excellent in productivity and also in quality as no cracks are generated on the end face after machining.

[0007] However, although processing techniques using ultrashort pulsed laser light are effective for a single brittle material such as glass, it is difficult to use the ultrashort pulsed laser light to cut a composite material in which a brittle material layer and a resin layer are laminated, because it causes a deterioration in the quality of the end surface after cutting. For example, even if ultrashort pulsed laser light is irradiated from the brittle material layer side of the composite material, the end of the resin layer will be thermally deteriorated by the ultrashort pulsed laser light that is transmitted without being consumed in removing the brittle material that forms the brittle material layer.

[0008] Non-Patent Document 1 describes that in a processing technique using an ultrashort pulsed laser beam, the filamentation phenomenon of the ultrashort pulsed laser beam is utilized, and a multi-focus optical system or a Bessel beam optical system is applied to an ultrashort pulsed laser light source. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2013-175767 [Patent Document 2] JP 2011-178636 A [Patent Document 3] Patent No. 6239461 [Non-patent literature]

[0010] [Non-Patent Document 1] John Lopez et al., “Glass Cutting Using Ultrashort Pulsed Bessel Beams,” [online], October 2015, International Congress on Applications of Lasers & Electro-Optics (ICALEO), [Retrieved July 8, 2019], Internet (URL: https: / / www.researchgate.net / publication / 284617626_GLASS_CUTTING_USING_ULTRASHORT_PULSED_BESSEL_BEAMS) Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made to solve the problems of the conventional technology as described above, and has an object to provide a method for dividing a composite material in which a brittle material layer and a resin layer are laminated, which method does not cause cracks to appear on the end face of the brittle material layer and does not deteriorate the quality of the end of the resin layer. [Means for solving the problem]

[0012] In order to solve the above problems, the present inventors have investigated a method of processing a brittle material layer using an ultrashort pulsed laser beam as described in the above Patent Document 3, instead of the method of processing a brittle material layer using a mechanical tool in the technology described in the above Patent Document 2. Then, they have investigated a method of subsequently applying a mechanical external force to the brittle material layer to divide it. However, it has been found that when a brittle material layer is divided by applying a mechanical external force to the brittle material layer, as in the method described in Patent Document 2, cracks may occur on the end surface of the brittle material layer.

[0013] Therefore, the inventors of the present invention have found, as a result of intensive research, that it is possible to divide (fracture) the brittle material layer without causing cracks on the end surface of the brittle material layer by processing the brittle material layer using an ultrashort pulse laser beam, and then applying heat to the brittle material layer to generate thermal stress in the brittle material layer. In addition, it has been found that, in this case, by applying heat to the brittle material layer from the brittle material layer side, rather than by heat conduction from the resin layer side, the quality of the end of the resin layer is not deteriorated (there is little discoloration due to thermal deterioration of the resin layer).

[0014] The present invention has been completed based on the above-mentioned findings of the present inventors. That is, in order to solve the above-mentioned problems, the present invention provides a method for dividing a composite material in which a brittle material layer and a resin layer are laminated, the method including: a resin removing step of irradiating the resin layer along a planned dividing line of the composite material with a laser beam oscillated from a first laser light source to remove the resin that forms the resin layer, thereby forming a processed groove along the planned dividing line; a brittle material removing step of irradiating the brittle material layer along the planned dividing line with a laser beam oscillated from an ultrashort pulse laser light source to remove the brittle material that forms the brittle material layer, thereby forming a processed mark along the planned dividing line; and a brittle material layer dividing step of applying heat to the brittle material layer from the opposite side to the resin layer along the planned dividing line to generate thermal stress in the brittle material layer, thereby dividing the brittle material layer, after the brittle material removing step. In the resin removing step, the resin forming the resin layer is removed so that a part of the resin is left as a residue at the bottom of the processed groove, and in the brittle material layer dividing step, after generating thermal stress in the brittle material layer, a mechanical external force is applied to the brittle material layer along the planned dividing line. The present invention provides a method for dividing a composite material, comprising the steps of:

[0015] According to the method of the present invention, in the resin removing step, the resin forming the resin layer is removed to form a processed groove along the planned dividing line, and then in the brittle material removing step, the brittle material forming the brittle material layer is removed to form a processed mark along the same planned dividing line. Then, in the brittle material layer dividing step, heat is applied to the brittle material layer from the opposite side to the resin layer (the brittle material layer side of the brittle material layer and the resin layer) along the same planned dividing line to generate thermal stress in the brittle material layer, which, as found by the inventors above, makes it possible to divide the brittle material layer without generating cracks on the end surface of the brittle material layer, and does not deteriorate the quality of the end of the resin layer. In addition, in the case where no resin residue remains at the bottom of the processed groove formed by removing the resin forming the resin layer in the resin removing step, and Brittle material removal process After performing the above, thermal stress is induced in the brittle material layer. The composite material can be broken simply by However, in the method according to the present invention, Resin residue remains at the bottom of the machined groove (In the resin removal process, the resin that forms the resin layer is removed so that a part of it remains as a residue at the bottom of the processed groove.) , resin removal process and Brittle material removal process After inducing thermal stress in the brittle material layer, To break up the resin residue , in the brittle material layer The composite material can be broken by applying external mechanical force. 。 Even if a mechanical external force is applied to the brittle material layer, at this point, Inducing thermal stress in a brittle material layer Since the brittle material layer has already been divided by the cutting, no cracks are generated at the end surface of the brittle material layer.

[0016] In the method according to the present invention, "irradiating the resin layer with a laser beam along the planned dividing line of the composite" means irradiating the resin layer with a laser beam along the planned dividing line as viewed from the thickness direction of the composite (lamination direction of the brittle material layer and the resin layer). In addition, in the method according to the present invention, "irradiating the brittle material layer with a laser beam along the planned dividing line" means irradiating the brittle material layer with a laser beam along the planned dividing line as viewed from the thickness direction of the composite (lamination direction of the brittle material layer and the resin layer). In the method according to the present invention, the type of the first laser light source used in the resin removal step is not particularly limited as long as the resin forming the resin layer can be removed by the oscillating laser light. However, it is preferable to use a CO2 laser light source or a CO laser light source that oscillates a laser light with a wavelength in the infrared range, since it is possible to increase the relative moving speed (processing speed) of the laser light with respect to the composite material.

[0017] In the method according to the present invention, the processing marks formed in the brittle material removing step can be, for example, perforated through holes along the planned dividing line. In this case, in the brittle material layer dividing step, due to thermal stress generated in the brittle material layer, cracks propagate along the planned dividing line so as to connect the perforated through holes, and the brittle material layer is divided (fractured). However, the processing marks formed in the brittle material removing process are not necessarily limited to perforated through holes. In the brittle material removing process, if the relative movement speed along the planned dividing line between the laser light emitted from the ultrashort pulse laser light source and the brittle material layer is set to be slow, or if the repetition frequency of the pulse oscillation of the ultrashort pulse laser light source is set to be high, a through hole (long hole) that is integrally connected along the planned dividing line is formed as the processing mark. Even in this case, the brittle material layer can be divided reliably by performing the brittle material layer dividing process.

[0018] Preferably, in the brittle material layer dividing step, a laser beam oscillated from a second laser light source is irradiated onto the brittle material layer from a side opposite to the resin layer, thereby generating thermal stress in the brittle material layer.

[0019] According to the above-mentioned preferred method, the temperature of the surface of the brittle material layer on the side irradiated with the laser light oscillated from the second laser light source becomes relatively high, and the temperature of the surface opposite to the side irradiated with the laser light becomes relatively low. As a result, compressive stress is generated on the surface irradiated with the laser light, and tensile stress is generated on the surface opposite to the side irradiated with the laser light. This stress difference causes cracks to grow starting from the processing marks, and the brittle material layer is divided (broken). In the above-mentioned preferred method, the type of the second laser light source used in the brittle material layer dividing step is not particularly limited as long as the brittle material layer can be divided by the thermal stress generated by the oscillated laser light. As the second laser light source, a CO2 laser light source or a CO laser light source that oscillates a laser light with a wavelength in the infrared region can be used, similar to the first laser light source.

[0020] The method of generating thermal stress in the brittle material layer in the brittle material layer dividing step is not limited to the method of irradiating the brittle material layer with the laser light oscillated from the second laser light source, but may also employ a method of heating the brittle material layer to a high temperature and then cooling it. Specifically, it is also possible to employ a method of heating the brittle material layer to several hundred degrees Celsius using hot air from a dryer or the like, and blowing water droplets or cold air onto the brittle material layer before the temperature drops, thereby generating thermal stress due to the temperature difference during cooling.

[0021] Preferably, in the brittle material layer dividing step, a spot diameter of the laser light oscillated from the second laser light source at a position irradiated on the brittle material layer is 2 mm or less.

[0022] According to the above-mentioned preferable method, the spot diameter of the laser light oscillated from the second laser light source is not excessively large, so that the effect of heat conduction on the resin layer can be reduced.

[0023] Preferably, in the brittle material layer dividing step, a spot diameter of the laser light oscillated from the second laser light source at a position irradiated on the brittle material layer is 400 μm or more.

[0024] According to the above preferred method, the spot diameter of the laser light emitted from the second laser light source is not excessively small, which has the advantage that the laser light emitted from the second laser light source can be easily irradiated along the intended dividing line.

[0025] Preferably, in the brittle material layer dividing step, the energy density of the laser light oscillated from the second laser light source at a position on the brittle material layer is 78 W / mm2 The following is the result.

[0026] According to the above preferred method, the energy density of the laser light oscillated from the second laser light source (=laser light output / laser light spot area) is not excessively large, so that the effect of heat conduction on the resin layer can be reduced.

[0027] The laser light emitted from the first laser light source is used to form a groove along the planned cutting line in the resin removal step, so the spot diameter needs to be made small to some extent so that the width of the groove does not become excessively large. On the other hand, the laser light emitted from the second laser light source is used to apply heat to the brittle material layer to generate thermal stress in the brittle material layer cutting step, so the spot diameter does not need to be made as small as when forming a groove. In other words, since the applications of the laser lights are different, it is preferable that the spot diameter of the laser light emitted from the first laser light source is smaller than the spot diameter of the laser light emitted from the second laser light source. Specifically, in the resin removing step, it is preferable that the spot diameter of the laser light oscillated from the first laser light source at the irradiation position on the resin layer is 300 μm or less.

[0028] The thickness of the brittle material layer to which the method according to the present invention is applied can be, for example, 30 to 150 μm, and the thickness of the resin layer can be, for example, 50 to 300 μm.

[0029] good Preferably, in the brittle material layer dividing step, after thermal stress is generated in the brittle material layer, air is blown onto the brittle material layer from the machined groove side along the intended dividing line.

[0030] According to the above preferred method, in addition to inducing thermal stress in the brittle material layer, 、 Since air is blown onto the brittle material layer, the brittle material layer can be reliably divided.

[0031] The method according to the present invention is preferably used in the case where, for example, the brittle material layer includes glass and the resin layer includes a polarizing film.

[0032] According to the method of the present invention, the discolored region caused by thermal deterioration of the resin layer after the brittle material layer dividing step can be limited to a region less than 1000 μm from the end face of the divided brittle material layer. Effect of the Invention

[0033] According to the present invention, a composite material in which a brittle material layer and a resin layer are laminated can be divided without causing cracks on the end surface of the brittle material layer and without deteriorating the quality of the end of the resin layer. [Brief description of the drawings]

[0034] [Figure 1] 1A to 1C are explanatory diagrams for explaining a schematic procedure of a composite material dividing method according to one embodiment of the present invention. [Diagram 2] 1A to 1C are explanatory diagrams for explaining a schematic procedure of a composite material dividing method according to one embodiment of the present invention. [Diagram 3] 1A to 1C are explanatory diagrams for explaining a schematic procedure of a composite material dividing method according to one embodiment of the present invention. [Figure 4] The test conditions and evaluation results for Examples 1 to 11 and a reference example are shown below. [Diagram 5] FIG. 2 is an explanatory diagram illustrating a thermal discoloration width. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, a method for dividing a composite material according to one embodiment of the present invention will be described with reference to the accompanying drawings as appropriate. 1 to 3 are explanatory diagrams that diagrammatically explain the procedure of a composite material dividing method according to one embodiment of the present invention. FIG. 1(a) is a cross-sectional view showing a resin removing step in the cutting method according to the present embodiment, and FIG. 1(b) is a cross-sectional view showing a brittle material removing step in the cutting method according to the present embodiment. 2(a) and (b) are cross-sectional views showing the brittle material dividing step of the dividing method according to this embodiment. FIG. 3(a) is a plan view (viewed from the brittle material layer side) showing the brittle material removal step of the cutting method according to this embodiment, and FIG. 3(b) is a perspective view showing the brittle material removal step of the cutting method according to this embodiment. In FIG. 3, the ultrashort pulse laser light source 30 is omitted. The cutting method according to this embodiment is a method for cutting a composite material 10 in which a brittle material layer 1 and a resin layer 2 are laminated, in the thickness direction (the lamination direction of the brittle material layer 1 and the resin layer 2, the vertical direction in Figure 1, the Z direction).

[0036] The brittle material layer 1 and the resin layer 2 are laminated by any appropriate method. For example, the brittle material layer 1 and the resin layer 2 can be laminated by a so-called roll-to-roll method. That is, the brittle material layer 1 and the resin layer 2 can be laminated by conveying the long brittle material layer 1 and the main body of the long resin layer 2 (in this embodiment, the polarizing film 21, the adhesive 22, and the release liner 23 constituting the resin layer 2) in the longitudinal direction, aligning the longitudinal directions of the layers, and bonding them to each other via the adhesive 24. Alternatively, the brittle material layer 1 and the main body of the resin layer 2 may be cut into a predetermined shape and then laminated.

[0037] Examples of the brittle material that forms the brittle material layer 1 include glass and single crystal or polycrystalline silicon. Preferably, glass is used. Glass can be classified according to composition, such as soda-lime glass, borate glass, aluminosilicate glass, quartz glass, and sapphire glass. Glass can be classified according to alkali content, such as non-alkali glass and low-alkali glass. The content of alkali metal components (e.g., Na2O, K2O, Li2O) in glass is preferably 15% by weight or less, and more preferably 10% by weight or less.

[0038] The thickness of the brittle material layer 1 is preferably 150 μm or less, more preferably 120 μm or less, and further preferably 100 μm or less. On the other hand, the thickness of the brittle material layer 1 is preferably 30 μm or more, and more preferably 80 μm or more. If the thickness of the brittle material layer 1 is in this range, lamination with the resin layer 2 by roll-to-roll is possible.

[0039] When the brittle material forming the brittle material layer 1 is glass, the light transmittance of the brittle material layer 1 at a wavelength of 550 nm is preferably 85% or more. When the brittle material forming the brittle material layer 1 is glass, the refractive index of the brittle material layer 1 at a wavelength of 550 nm is preferably 1.4 to 1.65. When the brittle material forming the brittle material layer 1 is glass, the density of the brittle material layer 1 is preferably 2.3 g / cm 3 ~3.0g / cm 3 and more preferably 2.3 g / cm 3 ~2.7g / cm 3 It is.

[0040] When the brittle material forming the brittle material layer 1 is glass, a commercially available glass plate may be used as it is, or may be polished to a desired thickness and used as the brittle material layer 1. Examples of commercially available glass plates include "7059", "1737" or "EAGLE2000" manufactured by Corning Incorporated, "AN100" manufactured by Asahi Glass Co., Ltd., "NA-35" manufactured by NH Techno Glass Co., Ltd., "OA-10G" manufactured by Nippon Electric Glass Co., Ltd., and "D263" or "AF45" manufactured by Schott.

[0041] Examples of the main body of the resin layer 2 include a single layer film formed of a plastic material such as polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), acrylic resin such as polymethyl methacrylate (PMMA), cyclic olefin polymer (COP), cyclic olefin copolymer (COC), polycarbonate (PC), urethane resin, polyvinyl alcohol (PVA), polyimide (PI), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), polystyrene (PS), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), ethylene-vinyl acetate (EVA), polyamide (PA), silicone resin, epoxy resin, liquid crystal polymer, and various resin foams, or a laminate film consisting of multiple layers.

[0042] When the main body of the resin layer 2 is a laminated film composed of a plurality of layers, various adhesives such as acrylic adhesives, urethane adhesives, silicone adhesives, or adhesives may be interposed between the layers. Furthermore, on the main surface of the resin layer 2, a conductive inorganic film such as indium tin oxide (ITO), Ag, Au, Cu, or the like may be formed. The cutting method according to this embodiment is particularly suitable for use in cases where the main body of the resin layer 2 is various optical films such as polarizing films and retardation films used in displays. The thickness of the main body of the resin layer 2 is preferably 20 to 500 μm, and more preferably 50 to 300 μm.

[0043] 1 illustrates an example in which the main body of the resin layer 2 is a laminated film in which a polarizing film 21 and a release liner 23 are laminated via an adhesive 22. The main body of the resin layer 2 is laminated to the brittle material layer 1 via an adhesive 24. In this embodiment, the combination of the main body of the resin layer 2 (polarizing film 21, adhesive 22, and release liner 23) and the adhesive 24 is referred to as the resin layer 2.

[0044] The polarizing film 21 has a polarizer and a protective film disposed on at least one side of the polarizer. The thickness of the polarizer is not particularly limited, and an appropriate thickness can be adopted depending on the purpose. The thickness of the polarizer is typically about 1 to 80 μm. In one embodiment, the thickness of the polarizer is preferably 30 μm or less. The polarizer is an iodine-based polarizer. More specifically, the polarizer can be composed of a polyvinyl alcohol-based resin film containing iodine.

[0045] Examples of methods for producing the polarizer constituting the polarizing film 21 include the following methods 1 and 2. (1) Method 1: A method of stretching and dyeing a polyvinyl alcohol resin film alone. (2) Method 2: A method in which a laminate (i) having a resin substrate and a polyvinyl alcohol-based resin layer is stretched and dyed. Method 1 is a method well known and commonly used in the art, and therefore a detailed description thereof will be omitted. Method 2 preferably includes a step of stretching and dyeing a laminate (i) having a resin substrate and a polyvinyl alcohol-based resin layer formed on one side of the resin substrate to produce a polarizer on the resin substrate. The laminate (i) can be formed by applying a coating liquid containing a polyvinyl alcohol-based resin onto a resin substrate and drying it. Alternatively, the laminate (i) may be formed by transferring a polyvinyl alcohol-based resin film onto the resin substrate. Details of Method 2 are described in, for example, JP 2012-73580 A, which is incorporated herein by reference.

[0046] The protective film constituting the polarizing film 21 is disposed on one or both sides of the polarizer. As the protective film, a triacetyl cellulose film, an acrylic film, a cycloolefin film, a polyethylene terephthalate film, or the like can also be used. The polarizing film 21 may further include a retardation film as appropriate. The retardation film may have any appropriate optical properties and / or mechanical properties depending on the purpose.

[0047] For example, a polyester adhesive, a polyurethane adhesive, a polyvinyl alcohol adhesive, or an epoxy adhesive can be used as the adhesive 24. In particular, it is preferable to use an epoxy adhesive since good adhesion can be obtained. If the adhesive 24 is a thermosetting adhesive, it can be heated to cure (solidify) and thereby exhibit peel resistance. If the adhesive 24 is a light-curing adhesive such as an ultraviolet-curing adhesive, it can be cured by irradiating it with ultraviolet light or other light and thereby exhibit peel resistance. Furthermore, if the adhesive 24 is a moisture-curing adhesive, it can be cured by reacting with moisture in the atmosphere and therefore can be cured by being left alone and exhibit peel resistance. As the adhesive 24, for example, a commercially available adhesive may be used, or various curable resins may be dissolved or dispersed in a solvent to prepare an adhesive solution (or dispersion). The thickness of the adhesive 24 is preferably 10 μm or less, more preferably 1 to 10 μm, further preferably 1 to 8 μm, and particularly preferably 1 to 6 μm.

[0048] The cutting method according to the present embodiment includes a resin removing step, a brittle material removing step, and a brittle material layer cutting step. Each step will be described below in order.

[0049] <Resin removal process> 1(a), in the resin removal step, a laser beam L1 emitted from a first laser light source 20a is irradiated onto the resin layer 2 along the planned dividing line of the composite material 10 to remove the resin forming the resin layer 2. As a result, a processed groove 25 is formed along the planned dividing line. 1 to 3, for convenience, a straight line DL extending in the Y direction of the two orthogonal directions (X direction and Y direction) in the plane of the composite material 10 (within an XY two-dimensional plane) is illustrated as the planned division line, but the present invention is not limited to this, and various planned division lines can be set, for example, a planned division line in which a plurality of straight lines DL extending in the X direction and a plurality of straight lines DL extending in the Y direction are set in a lattice pattern. Hereinafter, this straight line DL will be referred to as the "planned division line DL". The planned dividing line DL can be actually drawn on the composite material 10 as a visually recognizable mark, or its coordinates can be input in advance to a control device (not shown) that controls the relative positional relationship between the laser light L1 and the composite material 10 on an XY two-dimensional plane. The planned dividing line DL shown in Figs. 1 to 3 is a virtual line whose coordinates are input in advance to the control device and which is not actually drawn on the composite material 10. The planned dividing line DL is not limited to a straight line and may be a curved line. By determining the planned dividing line DL according to the application of the composite material 10, the composite material 10 can be divided into any shape and size according to the application.

[0050] In this embodiment, a CO2 laser light source that oscillates laser light L1 with a wavelength of 9 to 11 μm in the infrared range is used as the first laser light source 20a. However, the present invention is not limited to this, and it is also possible to use a CO laser light source that oscillates laser light L1 with a wavelength of 5 μm as the first laser light source 20a. Also, a visible light and ultraviolet (UV) pulsed laser light source can be used as the first laser light source 20a. Examples of visible light and UV pulsed laser light sources include those that emit laser light L1 with a wavelength of 532 nm, 355 nm, 349 nm, or 266 nm (high-order harmonics of a solid-state laser light source using Nd:YAG, Nd:YLF, or YVO4 as a medium), excimer laser light sources that emit laser light L1 with a wavelength of 351 nm, 248 nm, 222 nm, 193 nm, or 157 nm, and F2 laser light sources that emit laser light L1 with a wavelength of 157 nm. Also, as the first laser light source 20a, it is possible to use a pulsed laser light source that emits laser light L1 having a wavelength outside the ultraviolet region and a pulse width on the order of femtoseconds or picoseconds. If the laser light L1 emitted from this pulsed laser light source is used, it is possible to induce ablation processing based on a multiphoton absorption process. Furthermore, as the first laser light source 20a, it is also possible to use a semiconductor laser light source or a fiber laser light source that oscillates laser light L1 with a wavelength in the infrared region.

[0051] As an example of the manner in which the laser light L1 is irradiated along the planned dividing line of the composite material 10 (the manner in which the laser light L1 is scanned), for example, the sheet-like composite material 10 is placed on an XY two-axis stage (not shown) and fixed (for example, fixed by suction), and the XY two-axis stage is driven by a control signal from the control device to change the relative position of the composite material 10 on the XY two-dimensional plane with respect to the laser light L1. It is also possible to change the position of the laser light L1 irradiated to the composite material 10 on the XY two-dimensional plane by fixing the position of the composite material 10 and deflecting the laser light L1 oscillated from the first laser light source 20a using a galvanometer mirror or a polygon mirror driven by a control signal from the control device. Furthermore, it is also possible to use both the scanning of the composite material 10 using the above-mentioned XY two-axis stage and the scanning of the laser light L1 using a galvanometer mirror or the like in combination.

[0052] The oscillation form of the first laser light source 20a may be pulse oscillation or continuous oscillation. The spatial intensity distribution of the laser light L1 may be a Gaussian distribution, or may be shaped into a flat-top distribution using a diffractive optical element (not shown) or the like in order to suppress thermal damage to the brittle material layer 1 that is not a target for removal by the laser light L1. There is no restriction on the polarization state of the laser light L1, and it may be any of linear polarization, circular polarization, and random polarization.

[0053] By irradiating the resin layer 2 with the laser light L1 along the planned dividing line DL of the composite material 10, a local temperature rise occurs due to infrared light absorption of the resin irradiated with the laser light L1 among the resins forming the resin layer 2, and the resin is scattered, and the resin is removed from the composite material 10, and a processed groove 25 is formed in the composite material 10. In order to prevent the scattered resin removed from the composite material 10 from re-adhering to the composite material 10, it is preferable to provide a dust collection mechanism near the planned dividing line DL. In order to prevent the groove width of the processed groove 25 from becoming too large, it is preferable to focus the laser light L1 so that the spot diameter Da (see FIG. 1(a)) at the irradiation position on the resin layer 2 is 300 μm or less, and it is more preferable to focus the laser light L1 so that the spot diameter Da is 200 μm or less.

[0054] According to the findings of the present inventors, in the case of a resin removal method based on the principle of local temperature rise accompanying infrared light absorption by resin irradiated with laser light L1, it is possible to roughly estimate the input energy required to form the processed groove 25 from the thickness of the resin layer 2, regardless of the type of resin or the layer structure of the resin layer 2. Specifically, the input energy required to form the processed groove 25, expressed by the following formula (1), can be estimated based on the thickness of the resin layer 2 by the following formula (2). Input energy [mJ / mm] = average power of laser light L1 [mW] / processing speed [mm / sec] (1) Input energy [mJ / mm] = 0.5 × thickness of resin layer 2 [μm] (2) The input energy to be actually set is preferably set to 20 to 180% of the input energy estimated by the above formula (2), and more preferably set to 50 to 150%. The reason for providing a margin for the estimated input energy in this way is that it is considered that the input energy required to form the groove 25 varies depending on the light absorptance (light absorptance at the wavelength of the laser light L1) of the resin forming the resin layer 2 and the thermal properties such as the melting point and decomposition point of the resin. Specifically, for example, a sample of the composite material 10 to which the cutting method according to the present embodiment is applied is prepared, and a preliminary test is performed to form the groove 25 in the resin layer 2 of this sample with a plurality of input energies within the above preferred range, and an appropriate input energy can be determined.

[0055] In the resin removal process of this embodiment, the laser light L1 emitted from the first laser light source 20a is not irradiated multiple times in the area where the planned cutting lines DL intersect. Specifically, as described above, the coordinates of the planned cutting lines DL are input in advance to the control device, so the control device can recognize the coordinates of the area where the planned cutting lines DL intersect. Therefore, when the laser light L1 is about to be scanned for the second time in the intersecting area of ​​the planned cutting lines DL, the control device can control the output of the laser light L1 irradiating the intersecting area to 0%. The same applies when the laser light L1 is about to be scanned three or more times in the intersecting area. As a result, the laser light L1 oscillated from the first laser light source 20a is not irradiated multiple times in the area where the planned cutting lines DL intersect. In this manner, the laser light L1 is not irradiated multiple times in the region where the planned division lines DL intersect, thereby reducing thermal damage to the brittle material layer 1. This provides an advantage that cracks are less likely to occur on the end face of the brittle material layer 1 (the end face in the vicinity of the intersection region of the planned division lines DL) when processing marks are formed in the brittle material removal process described below. As a method for controlling the output of the laser light L1, for example, a method of pulse-controlling the excitation source of the first laser light source 20a or a method of turning it on and off with a mechanical shutter can be used.

[0056] In this embodiment, in the resin removing process, the laser light L1 emitted from the first laser light source 20a is not irradiated multiple times in the region where the planned cutting lines DL intersect, but the present invention is not limited to this, and it is also possible to adopt a mode in which the amount of irradiation of the laser light L1 is reduced in the region where the planned cutting lines DL intersect, compared to the region other than the region where the planned cutting lines DL intersect. Specifically, for example, when the laser light L1 is scanned in the intersecting region of the planned cutting lines DL for the second or subsequent times, it is also possible to control the output of the laser light L1 to be reduced from the output when the intersecting region was scanned for the first time (not reduced in the region other than the region where the planned cutting lines DL intersect).

[0057] The resin removal step of this embodiment is characterized in that the resin forming the resin layer 2 is removed so that a part of it remains as a residue at the bottom of the processed groove 25. The thickness of the residue is preferably 1 to 30 μm. Fig. 1(a) shows an example in which only the adhesive 24 remains as a residue, but it may also be an embodiment in which in addition to the adhesive 24, a part of the polarizing film 21 also remains as a residue. In this way, by removing the resin so that a residue remains at the bottom of the processing groove 25, the thermal damage to the brittle material layer 1 is further reduced by the amount of the residue remaining, compared to the case where the resin forming the resin layer 2 along the planned division line DL is completely removed, and the advantage is that cracks are less likely to occur at the end surface of the brittle material layer 1.

[0058] <Brittle material removal process> As shown in Figures 1(b) and 3, in the brittle material removal process, after the resin removal process, laser light (ultrashort pulse laser light) L2 oscillated (pulsed) from an ultrashort pulse laser light source 30 is irradiated onto the brittle material layer 1 along the planned cutting line DL to remove the brittle material that forms the brittle material layer 1, thereby forming a processing mark 11 along the planned cutting line DL. The manner in which the laser light L2 is irradiated along the planned division line DL (the manner in which the laser light L2 is scanned relatively) can be the same as the manner in which the laser light L1 described above is irradiated along the planned division line DL, so detailed explanation will be omitted here.

[0059] The brittle material forming the brittle material layer 1 is removed by utilizing the filamentation phenomenon of the laser light L2 emitted from the ultrashort pulse laser light source 30, or by applying a multi-focus optical system (not shown) or a Bessel beam optical system (not shown) to the ultrashort pulse laser light source 30. The use of the filamentation phenomenon of ultrashort pulsed laser light and the application of a multi-focus optical system or a Bessel beam optical system to an ultrashort pulsed laser light source are described in the above-mentioned Non-Patent Document 1. Trumpf, Germany, also sells products related to glass processing in which a multi-focus optical system is applied to an ultrashort pulsed laser light source. As described above, the use of the filamentation phenomenon of ultrashort pulsed laser light and the application of a multi-focus optical system or a Bessel beam optical system to an ultrashort pulsed laser light source are publicly known, and therefore detailed description thereof will be omitted here.

[0060] The processing marks 11 formed in the brittle material removing step of this embodiment are perforated through holes along the planned dividing line DL. The pitch P of the through holes is determined by the repetition frequency of the pulse oscillation and the relative moving speed (processing speed) of the laser light L2 with respect to the composite material 10. In order to simply and stably perform the brittle material layer dividing step described later, the pitch P of the through holes is preferably set to 10 μm or less, and more preferably set to 5 μm or less. In many cases, the diameter of the through holes is 5 μm or less.

[0061] The wavelength of the laser light L2 emitted from the ultrashort pulse laser light source 30 is preferably 500 nm to 2500 nm, which exhibits high light transmittance when the brittle material forming the brittle material layer 1 is glass. In order to effectively induce a nonlinear optical phenomenon (multiphoton absorption), the pulse width of the laser light L2 is preferably 100 picoseconds or less, and more preferably 50 picoseconds or less. The oscillation form of the laser light L2 may be single pulse oscillation or burst mode multi-pulse oscillation.

[0062] In the brittle material removal process of this embodiment, the laser light L2 oscillated from the ultrashort pulse laser light source 30 is irradiated onto the brittle material layer 1 from the side opposite to the processed groove 25 formed in the resin removal process. In the example shown in FIGS. 1(a) and 1(b), the first laser light source 20a is disposed on the lower side in the Z direction with respect to the composite material 10 so as to face the resin layer 2, and the ultrashort pulse laser light source 30 is disposed on the upper side in the Z direction with respect to the composite material 10 so as to face the brittle material layer 1. Then, after the processed groove 25 is formed by the laser light L1 oscillated from the first laser light source 20a in the resin removal process, the oscillation of the laser light L1 is stopped, and the processed mark 11 is formed by the laser light L2 oscillated from the ultrashort pulse laser light source 30 in the brittle material removal process. However, the present invention is not limited to this, and it is also possible to adopt a method in which the first laser light source 20a and the ultrashort pulse laser light source 30 are both placed on the same side of the composite material 10 (upper or lower in the Z direction), and the composite material 10 is inverted upside down using a known inversion mechanism so that the resin layer 2 faces the first laser light source 20a in the resin removal process, and the brittle material layer 1 faces the ultrashort pulse laser light source 30 in the brittle material removal process. By irradiating the laser light L2 emitted from the ultrashort pulse laser light source 30 from the side opposite the machining groove 25, even if resin residue remains at the bottom of the machining groove 25, it is possible to form an appropriate machining mark 11 in the brittle material layer 1 without being affected by the residue.

[0063] However, the present invention is not limited thereto, and may further include a cleaning step of removing the resin residue forming the resin layer 2 by applying various wet or dry cleaning methods to the processed groove 25 formed in the resin removal step before the brittle material removal step. In the brittle material removal step, it is also possible to form the processing mark 11 by irradiating the brittle material layer 1 with the laser light L2 oscillated from the ultrashort pulse laser light source 30 from the processed groove 25 side. If the resin residue forming the resin layer 2 is removed in the cleaning step, even if the brittle material layer 1 is irradiated with the laser light L2 oscillated from the ultrashort pulse laser light source 30 from the processed groove 25 side in the brittle material removal step, the laser light L2 is not affected by the resin residue, and it is possible to form an appropriate processing mark 11 in the brittle material layer 1.

[0064] <Brittle material layer separation process> 2(a), in the brittle material layer dividing step, after the brittle material removing step, heat is applied to the brittle material layer 1 from the side opposite to the resin layer 2 along the planned dividing line DL to cause thermal stress in the brittle material layer 1, thereby dividing the brittle material layer 1. Specifically, laser light L3 oscillated from the second laser light source 20b is irradiated onto the brittle material layer 1 from the side opposite to the resin layer 2, thereby causing thermal stress in the brittle material layer 1, and thus dividing the brittle material layer 1. The manner in which the laser light L3 is irradiated along the planned division line DL (the manner in which the laser light L3 is scanned relatively) can be the same as the manner in which the laser light L1 and the laser light L2 described above are irradiated along the planned division line DL, so a detailed explanation will be omitted here. Furthermore, in the brittle material layer dividing step, as necessary, after thermal stress is generated in the brittle material layer 1, a mechanical external force may be applied to the brittle material layer 1 along the planned dividing line DL as shown in FIG. 2(b) to reliably divide the brittle material layer 1 and the composite material 10. When dividing the composite material 10 by mechanical breaking (mountain folding), it is preferable to apply an external force with the brittle material layer 1 on the mountain side (with the resin layer 2 on the valley side) so that tensile stress acts on the brittle material layer 1. In addition, after thermal stress is generated in the brittle material layer 1, air may be blown onto the brittle material layer 1 from the machined groove 25 side along the planned dividing line DL to reliably divide the brittle material layer 1 and the composite material 10. The air may be air at room temperature or hot air. In this manner, the brittle material layer 1 and therefore the composite material 10 are divided. In the example shown in Fig. 2(b), the composite material 10 is divided into composite pieces 10a and 10b.

[0065] In this embodiment, a CO2 laser light source that oscillates laser light L3 with a wavelength of 9 to 11 μm in the infrared range is used as the second laser light source 20b. However, the present invention is not limited to this. As with the first laser light source 20a, it is also possible to use other laser light sources as the second laser light source 20b, such as a CO laser light source that oscillates laser light L3 with a wavelength of 5 μm. The oscillation mode of the second laser light source 20b and the spatial intensity distribution of the oscillated laser light L3 can also be similar to those of the first laser light source 20a. However, by changing or adjusting the focusing optical system used in the second laser light source 20b, the spot diameter Db (see FIG. 2(a)) at the irradiation position of the laser light L3 emitted from the second laser light source 20b on the brittle material layer 1 is set to be larger than the spot diameter Da at the irradiation position of the laser light L1 emitted from the first laser light source 20a on the resin layer 2. Specifically, the laser light L3 is focused so that the spot diameter Db is 2 mm or less. This can reduce the influence of heat conduction on the resin layer 2. From the viewpoint of the influence of heat conduction on the resin layer 2, the spot diameter Db is preferably 1.2 mm or less, more preferably 1 mm or less, and even more preferably 0.9 mm or less. In addition, the laser light L3 is focused so that the spot diameter Db is 400 μm or more. This has the advantage that the laser light L3 can be easily irradiated along the planned division line DL. From the viewpoint of easy irradiation of the laser light L3 along the planned division line DL, the spot diameter Db is preferably 0.6 mm or more. Furthermore, the energy density at the irradiation position of the laser light L3 on the brittle material layer 1 is 78 W / mm 2 The values ​​are set as follows: This makes it possible to reduce the effect of heat conduction on the resin layer 2.

[0066] In the brittle material cutting process of this embodiment, as described above, the laser light L3 oscillated from the second laser light source 20b is irradiated onto the brittle material layer 1 from the side opposite to the resin layer 2. In the example shown in FIG. 2(a), similarly to the ultrashort pulse laser light source 30, the second laser light source 20b is disposed on the upper side in the Z direction with respect to the composite material 10 so as to face the brittle material layer 1. Then, after the processing mark 11 is formed by the laser light L2 oscillated from the ultrashort pulse laser light source 30 in the brittle material removing process, the oscillation of the laser light L2 is stopped, and the brittle material layer 1 is cut by the laser light L3 oscillated from the second laser light source 20b in the brittle material cutting process. However, the present invention is not limited to this, and it is also possible to adopt a method in which the second laser light source 20b is positioned below the composite material 10 in the Z direction, and in the brittle material layer dividing process, a known inversion mechanism is used to invert the composite material 10 (see Figure 1 (b)) upside down after the processing mark 11 is formed in the brittle material removal process.

[0067] According to the above-described dividing method according to the present embodiment, in the resin removing step, the resin forming the resin layer 2 is removed to form a processed groove 25 along the planned dividing line DL, and then in the brittle material removing step, the brittle material forming the brittle material layer 1 is removed to form a processed mark 11 along the same planned dividing line DL. Then, in the brittle material layer dividing step, heat is applied to the brittle material layer 1 by the laser light L3 oscillated from the second laser light source 20b from the opposite side to the resin layer 2 along the same planned dividing line DL, thereby generating thermal stress in the brittle material layer 1. This makes it possible to divide the brittle material layer 1 without generating cracks on the end face (end face along the planned dividing line DL) of the brittle material layer 1, and does not deteriorate the quality of the end of the resin layer (end along the planned dividing line DL).

[0068] Hereinafter, an example of the results of a test performed to cut the composite material 10 using the cutting method according to this embodiment (Examples 1 to 11) and the cutting method according to a reference example will be described. FIG. 4 shows the test conditions and evaluation results for Examples 1 to 11 and the Reference Example.

[0069] <Example 1> In Example 1, a polyvinyl alcohol film was first dyed with a dichroic substance such as iodine or a dichroic dye and uniaxially stretched to obtain a polarizer. The polarizer had a thickness of 28 μm. Next, an acrylic protective film (thickness: 40 μm) was attached to one surface of the polarizer, and a triacetyl cellulose protective film (thickness: 30 μm) was attached to the other surface to obtain a polarizing film 21. Then, a polyethylene terephthalate release film (thickness: 38 μm) serving as a release liner 23 was attached to the polarizing film 21 via an acrylic adhesive (thickness: 30 μm) serving as an adhesive 22, to obtain the main body of the resin layer 2.

[0070] On the other hand, as the brittle material layer 1, a glass film (manufactured by Nippon Electric Glass Co., Ltd., product name "OA-10G", thickness: 100 μm) was prepared. In addition, as adhesive 24, an epoxy-based adhesive was prepared by mixing 70 parts by weight of Celloxide 2021P (manufactured by Daicel Chemical Industries, Ltd.), 5 parts by weight of EHPE3150, 19 parts by weight of Aron Oxetane OXT-221 (manufactured by Toa Gosei Co., Ltd.), 4 parts by weight of KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.), and 2 parts by weight of CPI101A (manufactured by San-Afro Co., Ltd.).

[0071] Next, the brittle material layer 1 and the main body of the resin layer 2 were bonded together via the adhesive 24. At this time, the main body of the resin layer 2 was arranged so that the acrylic protective film was on the brittle material layer 1 side. Next, the adhesive 24 was irradiated with ultraviolet light (500 mJ / cm2) from a high-pressure mercury lamp. 2 ) and the adhesive 24 was cured to obtain a composite material 10. The thickness of the adhesive 24 after curing was 5 μm.

[0072] After the composite material 10 obtained as described above was separated into sheets, a resin removal process was carried out. Specifically, a TLSU series (oscillation wavelength 9.4 μm, power of laser light L1 250 W) manufactured by Takei Electric Co., Ltd. was used as a laser processing device equipped with an optical system and a control device for controlling the scanning of the first laser light source 20a and the laser light L1, and the output of the laser light L1 oscillated from the first laser light source 20a was set to 20 W, and the laser light L1 was focused to a spot diameter of 100 μm using a focusing lens, and the resin layer 2 was irradiated along the planned division lines DL (plural planned division lines set in a lattice pattern) of the composite material 10. The relative moving speed (processing speed) of the laser light L1 with respect to the composite material 10 was set to 500 mm / sec. In this way, the resin forming the resin layer 2 was removed, and a processed groove 25 along the planned division lines DL was formed. At this time, the resin was removed so that a part of the resin forming the resin layer 2 remained as a residue (thickness: 10 to 20 μm) at the bottom of the processed groove 25. In addition, in the region IS where the planned cutting lines DL intersect, when the laser light L1 is about to be scanned for the second time, the output of the laser light L1 is controlled to 0% so that the laser light L1 is not irradiated multiple times to the region IS where the planned cutting lines DL intersect.

[0073] After the above-mentioned resin removal process, the brittle material removal process was carried out. Specifically, an ultrashort pulse laser light source 30 was used, which had an oscillation wavelength of 1064 nm, a pulse width of 10 picoseconds for the laser light L2, a repetition frequency of pulse oscillation of 50 kHz, and an average power of 10 W. The laser light L2 emitted from the ultrashort pulse laser light source 30 was irradiated onto the brittle material layer 1 of the composite material 10 from the opposite side to the resin layer 2 (the brittle material layer 1 side) via a multi-focus optical system. The relative moving speed (processing speed) of the laser light L2 with respect to the composite material 10 was set to 100 mm / sec, and the laser light L2 was scanned along the planned division line DL, resulting in the formation of perforations (diameter of about 1 to 2 μm) with a pitch of 2 μm as the processing marks 11.

[0074] After the brittle material removal process, the brittle material cutting process was carried out. Specifically, a Keyence MLG-9300 (oscillation wavelength 10.6 μm, laser light L3 power 30 W) was used as a laser processing device equipped with an optical system and a control device for controlling the scanning of the second laser light source 20b and the laser light L3, and the output of the laser light L3 oscillated from the second laser light source 20b was set to 80% (i.e., output 24 W) and focused to a spot diameter of 0.7 mm using a focusing lens (energy density at this time was 62 W / m 2 ), the brittle material layer 1 was irradiated from the opposite side to the resin layer 2 along the planned dividing line DL of the composite material 10. At this time, the relative moving speed of the laser beam L3 with respect to the composite material 10 was set to 500 mm / sec. Finally, a mechanical external force was applied to the composite material 10 to break up the resin residue remaining at the bottom of the processed groove 25 after the resin removal step, and the composite material 10 was broken up.

[0075] <Examples 2 to 11> In Examples 2 to 11, as shown in FIG. 4, at least one parameter among the output of the second laser light source 20b, the spot diameter Db of the laser light L3, and the relative moving speed of the laser light L3 was made different from that in Example 1, and the other parameters were the same as those in Example 1, and the composite material 10 was divided.

[0076] <Reference example> In the reference example, the composite material 10 was divided under the same conditions as in Example 1, except that the brittle material layer 1 was irradiated with the laser light L3 oscillated from the second laser light source 20b from the resin layer 2 side.

[0077] <Evaluation content and results> The end faces of the brittle material layer 1 of the composite material 10 (composite material pieces) cut by the cutting methods according to Examples 1 to 11 and the Reference Example were visually observed to evaluate the presence or absence of cracks. The "A" and "B" in the "Brittle material layer splitting status" column in Figure 4 respectively indicate the following results. A: The brittle material layer 1 was separated (fractured) without any problems, and no cracks were generated. B: The brittle material layer 1 was separated (fractured) without any problems, and slight cracks occurred that did not pose any problems to the product.

[0078] In addition, the ends of the resin layer 2 of the composite materials (composite material pieces) cut by the cutting methods of Examples 1 to 11 and the reference example were observed with a microscope (VHX-2000 manufactured by Keyence Corporation), and the extent of the discolored area (also called the yellow band) due to thermal degradation of the resin layer 2 (polarizing film 21) was evaluated. The letters "A," "B," and "C" in the "Thermal Discoloration Width" column in Fig. 4 respectively indicate the following results. Note that the "thermal discoloration width" refers to the distance YB from the end face of the divided brittle material layer 1 to the innermost point of the region where discoloration (yellowish discoloration) has occurred in the resin layer 2 (the hatched region in Fig. 5) in the cross section of the composite material 10, as shown in Fig. 5. A: Discoloration width YB is less than 200 μm (very good) B: Discoloration width YB is less than 500 μm (good) C: Discoloration width YB is less than 1000 μm (acceptable) D: Discoloration width YB is 1000μm or more (not acceptable)

[0079] As shown in FIG. 4, in the cutting methods according to Examples 1 to 11 and the Reference Example, the "cutting state of the brittle material layer" was either "A" or "B," and no problems occurred in cutting the brittle material layer 1. In addition, the reason why the "Brittle material layer division state" was "B" in the division methods according to Examples 5 and 6 is considered to be due to the small spot diameter Db and / or the small energy density of the laser light L3. When the spot diameter Db becomes small, the energy of the spot part is high, and the energy drops suddenly when it is out of the spot part, so that it becomes difficult to divide when the energy irradiation position is out of the planned division line DL. The reason why the "division state of the brittle material layer" was "B" in the dividing methods according to Examples 7 and 11 is considered to be because the energy density of the laser light L3 was small.

[0080] In addition, in the cutting methods according to Examples 1 to 11, the "thermal discoloration width" was "A," "B," or "C," and no problem occurred in the quality of the end of the resin layer 2. The reason that the "thermal discoloration width" was "C" in the cutting method according to Example 11 was that the energy density of the laser light L3 was low (0.95 W / mm 2 ), however, the relative moving speed of the laser beam L3 with respect to the composite material 10 was also small (25 mm / sec), which is thought to have caused the influence of heat conduction from the brittle material layer 1 side to the resin layer 2 side. On the other hand, in the cutting method according to the reference example, the "thermal discoloration width" was "D", and a problem arose in the quality of the end portion of the resin layer 2. In the cutting method according to the reference example, the laser light L3 oscillated from the second laser light source 20b is directly irradiated onto the resin layer 2, which is considered to have caused the discolored area to become wider due to thermal degradation.

[0081] 1...brittle material layer 2. Resin layer 10...Composite material 11... Machining marks 20a...First laser light source 20b Second laser light source 21. Polarizing film 24...Adhesive 25... Machining groove 30 Ultrashort pulse laser light source DL... Planned division line L1, L2, L3...Laser light YB: Discoloration width

Claims

1. A method for dividing a composite material in which a brittle material layer and a resin layer are laminated, comprising the steps of: a resin removing step of irradiating the resin layer with a laser beam emitted from a first laser light source along a planned dividing line of the composite material to remove a resin forming the resin layer, thereby forming a processed groove along the planned dividing line; After the resin removal step, a brittle material removal step is performed in which a laser beam oscillated from an ultrashort pulse laser source is irradiated onto the brittle material layer along the planned dividing line to remove the brittle material that forms the brittle material layer, thereby forming a processing mark along the planned dividing line; a brittle material layer dividing step of dividing the brittle material layer by applying heat to the brittle material layer from the side opposite to the resin layer along the planned dividing line to generate thermal stress in the brittle material layer, after the brittle material removing step; Including, In the resin removing step, the resin forming the resin layer is removed so that a part of the resin remains as a residue at the bottom of the processed groove; In the brittle material layer dividing step, after generating thermal stress in the brittle material layer, a mechanical external force is applied to the brittle material layer along the planned dividing line. A method for dividing a composite material, comprising:

2. In the brittle material layer dividing step, a laser beam oscillated from a second laser light source is irradiated onto the brittle material layer from a side opposite to the resin layer, thereby generating thermal stress in the brittle material layer. The method for cutting a composite material according to claim 1 .

3. The second laser light source used in the brittle material layer dividing step is a CO 2 A laser light source. The method for cutting a composite material according to claim 2 .

4. In the brittle material layer dividing step, a spot diameter of the laser light oscillated from the second laser light source at a position on the brittle material layer is 2 mm or less.

4. The method for dividing a composite material according to claim 2 or 3.

5. In the brittle material layer dividing step, a spot diameter of the laser light oscillated from the second laser light source at a position irradiated on the brittle material layer is 400 μm or more.

5. The method for dividing a composite material according to claim 2, wherein the cutting step comprises cutting the composite material by cutting the composite material.

6. In the brittle material layer dividing step, the energy density at the irradiation position of the brittle material layer with the laser light oscillated from the second laser light source is 78 W / mm 2 Below is the 6. The method for dividing a composite material according to claim 2, wherein the dividing step comprises the steps of:

7. In the resin removing step, a spot diameter of the laser light oscillated from the first laser light source at a position on the resin layer is 300 μm or less.

7. The method for dividing a composite material according to claim 1, wherein the cutting is performed by cutting the composite material.

8. The thickness of the brittle material layer is 30 to 150 μm, and the thickness of the resin layer is 50 to 300 μm.

8. The method for dividing a composite material according to claim 1, wherein the cutting step comprises cutting the composite material by cutting the composite material.

9. In the brittle material layer dividing step, after generating thermal stress in the brittle material layer, air is blown onto the brittle material layer from the machined groove side along the intended dividing line.

9. The method for dividing a composite material according to claim 1, wherein the cutting step comprises cutting the composite material by cutting the composite material.

10. The brittle material layer includes glass, and the resin layer includes a polarizing film.

10. The method for dividing a composite material according to claim 1 ,

11. The discolored region due to thermal deterioration of the resin layer after the brittle material layer dividing step is a region less than 1000 μm from an end surface of the divided brittle material layer.

11. The method for dividing a composite material according to claim 1 .

Citation Information

Patent Citations

  • Band for package made of polypropylene and manufacture thereof

    JP1987039461A

  • How to break a glass sheet

    JP1998506087A

  • Method for dividing brittle material substrate, and brittle material member

    JP2011178636A

  • Production method of flexible film

    JP2017145188A

  • Cutting method and cutting device of resin layer-equipped brittle material substrate

    JP2018170474A

Cited By

  • Method for manufacturing secondary battery electrode, secondary battery electrode, and electrode manufacturing system used in said method