Silica-based hydrophobic powders with increased polarity
A silica-based powder with tailored properties addresses mechanical stability and compatibility issues, enhancing thermal insulation and antifouling in aqueous systems by maintaining low viscosity and uniform application.
Patent Information
- Application Number
- JP2022542369
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-14
- Filing Date
- 2021-01-06
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-01-06
AI Technical Summary
Existing silica-based thermal insulation materials face challenges with mechanical stability, high hydrophobicity, and compatibility with polar systems, leading to issues such as increased viscosity, material separation, and reduced thermal insulation properties when used in aqueous formulations.
A silica-based powder with specific pore volume, tap density, silanol group content, and surface treatment agent characteristics is developed, ensuring mechanical stability, high hydrophobicity, and compatibility with aqueous systems, allowing for high loading and uniform application without viscosity issues.
The solution provides thermal insulation compositions with improved mechanical stability, high hydrophobicity, and compatibility with aqueous formulations, preventing moisture ingress and enabling effective thermal insulation and antifouling properties.
Smart Images

Figure 0007561858000001 
Figure 0007561858000002 
Figure 0007561858000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrophobized silica-based granule, its preparation, its use for thermal and acoustic insulation and the corresponding insulating compositions. [Background technology]
[0002] Effective insulation of houses, industrial plants, pipelines, etc. is a major economic challenge. Most insulation materials based on organic substances, such as polyurethane foam, are flammable and can only be used at relatively low temperatures. These disadvantages do not occur with the hitherto less widespread insulation materials based on inorganic oxides (e.g. silicon dioxide, which is very porous).
[0003] Description of the Prior Art Patent Document 1 discloses a composition having a thermal conductivity of 50 mW / (mK) or less, comprising a silica aerogel component, a surfactant, either an inorganic compound or an inorganic binder-containing compound (e.g., cement, gypsum, lime, acrylate), and other components as necessary. Specifically, a highly viscous mixture of cement / grout / acrylate / hydrophobic aerogel material (weight ratio: 0.24 / 0.28 / 0.15 / 0.33) is hardened in a mold to obtain a compound having a thermal conductivity of 29.5 mW / (mK).
[0004] It is preferable to use hydrophobized silica particles as a filler for thermal insulation compositions based on aqueous formulations, rather than hydrophilic silica. In the case of hydrophilic silica, the pores of the silica material are easily filled with the hydrophilic formulation, and cannot impart additional thermal insulation properties to the final composition. In contrast, the porous structure of the hydrophobized material remains intact when mixed with the aqueous formulation.
[0005] One technical challenge with compositions containing insulating silica-based granules is related to fines. The presence of fines, which are particles of relatively small size, in a formulation usually leads to a rapid increase in viscosity as the amount of such particles added to the formulation increases. If the composition needs to be applied by spray techniques, such fines must be separated beforehand. This means a significant loss of material and additional efforts in handling solid particles. It is desirable to avoid the formation of such fines by minimizing the abrasion of the silica-based granules as they are incorporated into the insulating composition. This can be achieved by using more mechanically stable silica-based granules.
[0006] Patent document 2 discloses a granular insulation material comprising hydrophobic fumed silicon dioxide and an emulsifier, which is produced by mixing the hydrophobic silicon dioxide with an emulsifier, followed by densification to produce granules with a size of 0.25-2.5 mm. Importantly, it is impossible, or at least difficult, to densify hydrophobized silica powder to obtain relatively low density granules useful for insulation applications. Such granules containing such hydrophobized silica are usually not mechanically stable enough or have a relatively high tap density, usually 250-450 g / L, which adversely affects the insulation properties.
[0007] Patent Document 3 describes a granular material having a median particle size of 10 to 120 μm and a BET surface area of 40 to 400 m 2describes granules based on hydrophobic fumed silica with a pore volume of 0.5-2.5 mL / g, a cumulative pore volume over 2 nm of 0.5-2.5 mL / g, and a tap density of 220-700 g / L for use as catalyst supports. Granules of this kind are produced by spray drying an aqueous dispersion containing hydrophilic silica, followed by heat treatment and / or silanization, if required, at temperatures of 150-1,100 °C. Examples 3, 4 and 8 show hydrophobized granules that have been heat treated at 700 °C before being hydrophobized with silane. These granules have a pore volume of 1.51-1.68 mL / g and a tap density of 300-420 g / L. Although such granules are mechanically stable, they have a particular combination of physical properties (e.g., a relatively high tap density and a relatively low pore volume) that are disadvantageous when using them in thermal insulation applications.
[0008] US Pat. No. 5,399,633 describes the preparation of hydrophobized silica heat insulating moldings (e.g. silica granules) by preparing a wet mixture containing silica powder, at least one binder (e.g. silane) and an organic solvent containing at most traces of water, evaporating the solvent and granulating the wet mixture. During the preparation of this wet mixture and / or during the granulation process, the silica is hydrophobized. The granules thus prepared are completely hydrophobized and contain, for example, a relatively small amount of free silanol groups on the surface. Furthermore, such granules made of hydrophobized silica may have insufficient mechanical stability since no additional densification has been performed. This is likewise reflected in their relatively low skeletal density, measured by Hg porosimetry.
[0009] US Pat. No. 5,399,633 discloses granular insulation with improved mechanical stability, prepared by heat treatment at 200-1,200° C. of a dense mixture containing silica and at least one IR-opacifier, followed by hydrophobization with silane. A specific example in this patent application shows the preparation of hydrophobized silica-based granules, the hydrophobization step being carried out by treating hydrophilic granules with HMDS vapors. The granules thus prepared are mechanically stable. However, due to their relatively high hydrophobicity, it may be difficult to incorporate such granules into polar coating systems (e.g. water-based polymer compositions).
[0010] Hydrophobic silica powders can be prepared by treating the corresponding hydrophilic materials with silanes and, if necessary, water, as described, for example, in Patent Document 6 or Patent Document 7. Such hydrophobic silicas are usually characterized by high hydrophobicity (high methanol wettability) and, as a consequence, low compatibility with polar solvents. One possible way to improve the compatibility of such hydrophobized silica materials with polar systems is to reduce the amount of silane used for hydrophobization. Patent Document 8 describes hydrophobic silicas with a silanol group density of 0.9-1.7 SiOH / nm 2 They describe the preparation of partially hydrophobic silica particles that can be incorporated into aqueous resins. The preparation of such partially hydrophobic particles involves the addition of 0.015-0.15 mmol of silane to a silica gel having a BET surface area of 100 m. 2 / g of silica. The silica obtained has a carbon content of 0.3-1 wt. % and a relatively low methanol wettability (methanol number: 0-15). Such silica particles are therefore compatible with polar systems due to the absence of a large proportion of hydrophobic groups on the surface, but have a much lower hydrophobicity. Considering the teaching of US Pat. No. 5,999,336, it appears generally impossible to obtain silica particles that have both high hydrophobicity and good compatibility with polar systems.
[0011] US Pat. No. 5,399,633 relates to the production of silica-based granules for thermal insulation, suitable for incorporation into water-based formulations. This good compatibility with water-based systems is achieved in US Pat. No. 5,399,633 by applying a heat treatment step to at least partially pyrolyze the hydrophobic groups present on the surface of the hydrophobized silica granules. However, this method inevitably results in a concomitant decrease in hydrophobicity. Thus, the methanol wettability of such heat-treated granules is significantly lower (20-30%) than that of the corresponding untreated granules (40-45%). Making granules both highly hydrophilic and highly hydrophobic appears to be a challenge, starting from US Pat. No. 5,399,633.
[0012] Challenges and Solutions Thus, good compatibility of highly hydrophobic silica-based materials with typical aqueous coating formulations (such as aqueous acrylate formulations) often remains a challenge. Thus, silica particles hydrophobized with typical hydrophobic treatment reagents such as hexamethyldisilazane (HMDS) either remain separated from the aqueous acrylate binder system upon mixing or cause cracks in the final cured coating film. Therefore, new hydrophobized silica materials, especially mechanically stable granules, are needed, which are compatible with aqueous formulations and allow the preparation of compositions with high silica material loadings, good thermal insulation properties, high homogeneity before and after curing, and low cost. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] International Publication No. 2010 / 126792A2 [Patent Document 2] International Publication No. 2006 / 097668A1 [Patent Document 3] European Patent Publication No. 0725037A1 [Patent Document 4] International Publication No. 2017 / 036744A1 [Patent Document 5] International Publication No. 2018 / 134275A1 [Patent Document 6] European Patent Publication No. 0686676A1 [Patent Document 7] German Patent Publication No. 102006039273A1 [Patent Document 8] European Patent Publication No. 1433749A1 [Patent Document 9] European Patent Publication No. 3447038A1 Summary of the Invention [Problem to be solved by the invention]
[0014] The technical problem that the present invention aims to solve is to provide insulating silica-based hydrophobized granules with improved mechanical stability, high hydrophobicity and improved polarity, with a particle size distribution suitable for incorporation into polar systems, such as water-based insulating compositions. Such granules should provide good insulating and rheological properties to the insulating compositions in which they are incorporated. These granules should also be accessible in a simple and economically viable manner. Another technical problem is to provide such insulating compositions with significant hydrophobicity and water repellency, which effectively prevents the ingress of moisture through the coating layer and imparts water repellency, antifouling, protective and anticorrosive properties to the treated surfaces. [Means for solving the problem]
[0015] It has been found that all of the above technical problems can be effectively solved by the present invention.
[0016] The present invention relates to - silica, at least one IR-opacifier selected from silicon carbide, titanium dioxide, zirconium dioxide, ilmenite, iron titanate, iron oxide, zirconium silicate, manganese oxide, graphite, carbon black, and mixtures thereof; Including, It is a silica-based powder that has been hydrophobized with a surface treatment agent that contains silicon atoms. a) Cumulative pore volume of pores larger than 4 nm is 2.5 cm3, measured by mercury intrusion porosimetry according to DIN ISO 15901-1 3 / g, b) the tap density is 140 g / L to 290 g / L; c) The number of silanol groups relative to the BET surface area, d, measured by reaction with lithium aluminum hydride SiOH is at least 0.5SiOH / nm 2 and d) Number of silicon atoms in the surface treatment agent relative to the BET surface area [Si] is at least 1.0 [Si atom] / nm 2 Powder and granular material This provides:
[0017] The hydrophobic silica powder and granules according to the present invention solve the above technical problems. The hydrophobized granules according to the invention are mechanically stable and do not undergo substantial mechanical abrasion during handling and incorporation into liquid compositions. Moreover, such granules are highly compatible with aqueous formulations, which allows, for example, high loadings of such granules in thermal insulation compositions, while at the same time providing good thermal insulation properties and high homogeneity before and after curing. Thermal insulation compositions comprising the hydrophobized granules according to the invention can contain surprisingly large amounts of fine particles of the hydrophobized granules and still have a relatively low viscosity. The low viscosity of such compositions does not prevent their easy application to the surfaces to be insulated, for example via spraying techniques. In addition, there is no need to separate the fine particles before incorporating them into the liquid composition. The composition containing the hydrophobized silica-based granules of the present invention has remarkable hydrophobicity and water repellency, which effectively prevents the intrusion of moisture through the coating layer and provides such compositions with water repellency, antifouling, protective and anticorrosive properties.
[0018] Powder material In the present invention, the terms "granular material", "granulate" and "granules" are used alternatively and are understood to mean particulate, easily pourable and flowable particulate solids. Granular materials according to the invention may be granular particles having a spherical or any other shape (e.g. pellets, rings) or irregularly shaped fragments of crushed granules, e.g. with a statistical particle size distribution. The term "granular material" in the context of the present invention includes powdered materials, i.e. materials having an average particle size d 50 It is preferable that the particle size does not include particles smaller than 10 μm.
[0019] The cumulative pore volume of pores larger than 4 nm can be measured by mercury intrusion porosimetry according to DIN ISO 15901-1. The principle of this method, first described by HL Ritter and LC Drake in Ind. Eng. Chem. Anal. Vol. 17 (1945) pp. 782-786 and 787-791, is based on measuring the volume of mercury intruded into the porous solid as a function of the applied pressure. At the maximum applied pressure (i.e. 417 MPa), only pores that can be penetrated by mercury (i.e. generally only pores with a pore diameter larger than 4 nm) are detected. Liquid mercury does not wet the surface of the probe porous solid and penetrates into the pores only under pressure. The pressure to be applied is inversely proportional to the opening width of the pore opening. For cylindrical pores, the pore radius r p The relationship between and pressure p can be calculated using the Washburn equation. r p =-(2×σ / p)×cosθ (In the formula, r p is the pore radius, p is the pressure, σ is the surface tension of mercury (0.48 N / m), and θ is the contact angle of mercury (140 degrees).
[0020] The cumulative pore volume of pores >4 nm corresponds to the cumulative pore volume of all pores measurable by mercury porosimetry according to DIN ISO 15901-1 up to the measurement limit at a maximum pressure of 417 MPa.
[0021] The cumulative pore volume of pores larger than 4 nm of the silica-based powder or granule of the present invention, measured by mercury intrusion porosimetry according to DIN ISO 15901-1, is preferably 2.6 cm 3 / g~10cm 3 / g, more preferably 2.6 cm 3 / g~9.5cm 3 / g, more preferably 2.6 cm 3 / g~9.0cm 3 / g, more preferably 2.6 cm 3 / g~8.5cm 3 / g, more preferably 2.6 cm 3 / g~8.0cm 3 / g, more preferably 3.0 cm 3 / g~7.5cm 3 / g, more preferably 3.5 cm 3 / g~7.0cm 3 / g, more preferably 3.5 cm 3 / g~6.5cm 3 / g, more preferably 4.0 cm 3 / g~6.0cm 3 / g.
[0022] The cumulative pore volume of pores <4 μm determined by mercury intrusion porosimetry in accordance with DIN ISO 15901-1 corresponds to the cumulative pore volume of all pores <4 μm determinable by this method. The cumulative pore volume of pores of less than 4 μm in the silica-based granules of the present invention, measured by mercury intrusion porosimetry in accordance with DIN ISO 15901-1, is preferably less than 1.0 cm 3 / g~7.0cm 3 / g, more preferably 1.2 cm 3 / g~6.5cm 3 / g, more preferably 1.4 cm 3 / g~6.0cm 3 / g, more preferably 1.6 cm 3 / g~5.5cm 3 / g, more preferably 1.8 cm 3 / g~5.0cm 3 / g, more preferably 2.0 cm 3 / g~5.0cm 3 / g, more preferably 2.2 cm 3 / g~4.5cm 3 / g, more preferably 2.4 cm 3 / g~4.2cm 3 / g, more preferably 2.5 cm 3 / g~4.0cm 3 / g, more preferably 2.6 cm 3 / g~3.8cm 3 / g.
[0023] The percentage ratio of the pore volume of pores less than 4 μm to the cumulative pore volume of pores greater than 4 nm of the powder or granule of the present invention (both pore volumes are measured by mercury intrusion porosimetry in accordance with DIN ISO 15901-1) is preferably greater than 35%, more preferably greater than 40%, more preferably greater than 45%, more preferably 45% to 75%, more preferably 45% to 70%, more preferably 50% to 65%, more preferably 50% to 60%. The percentage ratio of the pore volume of pores less than 4 μm to the cumulative pore volume of pores greater than 4 nm can be determined by dividing the pore volume of pores less than 4 μm by the pore volume of pores greater than 4 nm and multiplying it by 100%.
[0024] The skeletal density of a sample of material is the density without taking into account the porosity of the material, i.e. the ratio of the mass of the sample divided by the volume of the sample, without taking into account the volume of all its pores. The skeletal density of the granular material according to the invention can be calculated from the results of the analysis of the sample by mercury intrusion porosimetry according to DIN ISO 15901-1 after excluding the volume of all pores larger than 4 nm (maximum intrusion pressure: 417 MPa) from the estimated volume occupied by the material.
[0025] The skeletal density of the granules according to the invention, measured by mercury intrusion porosimetry according to DIN ISO 15901-1 at 417 MPa, is preferably at least 0.6 g / cm 3 , more preferably at least 0.7 g / cm 3 , more preferably 0.7 g / cm 3 ~4.0g / cm 3, more preferably 0.8 g / cm 3 ~3.0g / cm 3 , more preferably 0.9 g / cm 3 ~2.9g / cm 3 , more preferably 0.9 g / cm 3 ~2.80g / cm 3 , more preferably 1.0 g / cm 3 ~2.7g / cm 3 , more preferably 1.1 g / cm 3 ~2.6g / cm 3 , more preferably 1.2 g / cm 3 ~2.5g / cm 3 , more preferably 1.3 g / cm 3 ~2.4g / cm 3 It is.
[0026] The relatively high skeletal density of the granules according to the invention results in high mechanical stability which is beneficial for the application of such granules in, for example, thermal insulation compositions.
[0027] The number of silanol groups d relative to the BET surface area of the silica-based powder of the present invention SiOH is SiOH group / nm 2 and can be measured by the method described in detail in Patent Document 3, page 8, line 17 to page 9, line 12, by reaction of a silica-based material with lithium aluminum hydride. This method is also described in detail in Journal of Colloid and Interface Science, Vol. 125, No. 1 (1988), pp. 61-68. The silanol (SiOH) groups of silica-based materials react with lithium aluminum hydride (LiAlH4), and the amount of hydrogen gas formed during this reaction determines the amount of silanol groups in the sample, n OH (mmol SiOH / g) is measured. The corresponding BET surface area (m 2 / g) to calculate the silanol content (mmol OH / g) as the number of silanol groups relative to the BET surface area, d SiOH can be easily converted to . d OH [SiOH / nm 2 ]=(nOH [mmol SiOH / g]×N A / (BET[m 2 / g]×10 21 ) (In the formula, N A is Avogadro's constant (~6.022×10 23 )
[0028] The silica-based powder of the present invention preferably has a BET surface area d OH The number of hydroxyl groups per nm is at least 0.6SiOH / nm 2 , more preferably 0.6SiOH / nm 2 ~2.5SiOH / nm 2 , more preferably 0.7SiOH / nm 2 ~2.0SiOH / nm 2 , more preferably 0.7SiOH / nm 2 ~1.9 SiOH / nm 2 , more preferably 0.7SiOH / nm 2 ~1.8SiOH / nm 2 , more preferably 0.7SiOH / nm 2 ~1.7SiOH / nm 2 , more preferably 0.8SiOH / nm 2 ~1.6 SiOH / nm 2 , more preferably 0.9SiOH / nm 2 ~1.5SiOH / nm 2 It is.
[0029] The silica-based powder / granule according to the present invention preferably has a silanol group content of more than 0.03 mmol SiOH / g, more preferably 0.04 mmol SiOH / g to 0.50 mmol SiOH / g, more preferably 0.05 mmol SiOH / g to 0.45 mmol SiOH / g, more preferably 0.07 mmol SiOH / g to 0.40 mmol SiOH / g, more preferably 0.10 mmol SiOH / g to 0.40 mmol SiOH / g, and more preferably 0.15 mmol SiOH / g to 0.35 mmol SiOH / g.
[0030] The number of silicon atoms in the surface treatment agent relative to the BET surface area of the powder, d [Si] indicates the relative amount of the surface treatment group present in the powder or granule of the present invention relative to the surface area. SiOH and d [Si] Analysing the values of β-hydroxypropyltrimethylsilane (β) helps to characterise the degree of both hydrophilic and hydrophobic properties of the granules of the present invention and clearly demonstrates their uniqueness compared to materials known from the prior art.
[0031] The number of silicon atoms in the surface treatment agent relative to the BET surface area of the powder, d [Si] is at least 1.0 Si atom / nm 2 , preferably 1.2 Si atoms / nm 2 ~10Si atoms / nm 2 , more preferably 1.3 Si atoms / nm 2 ~9.0Si atoms / nm 2 , more preferably 1.4 Si atoms / nm 2 ~8.0Si atoms / nm 2 , more preferably 1.5 Si atoms / nm 2 ~7.0Si atoms / nm 2 , more preferably 1.8 Si atoms / nm 2 ~6.0Si atoms / nm 2 , more preferably 2.0 Si atoms / nm 2 ~5.0Si atoms / nm 2 It is.
[0032] The number of silicon atoms in the surface treatment agent relative to the BET surface area of the powder or granule of the present invention, d [Si] [Unit: Si atom / nm 2 ] can be calculated from the carbon content of the granule related to the presence of a surface treatment (C*, wt%) and the chemical structure of the surface treatment, e.g., the number of carbon atoms per silicon atom of the surface treatment (N C / Si ) consider: d [Si] [Si atoms / nm 2 ]=(C*[weight%]×N A ) / (Mr C [g / mol]×N C / Si ×BET[m 2 / g]×10 20 ) (In the ceremony, Mr. C = 12,011 g / mol is the atomic weight of carbon, N A is Avogadro's number (~6.022*1023), N C / Si is the ratio of carbon atoms to silicon atoms in the surface treatment agent.)
[0033] Therefore, in the case of chlorotrimethylsilane [(CH3)3SiCl], N C / Si = 3. In the case of hexamethyldisilazane [HMDS, (CH3)3Si)2NH], N C / Si = 3. In the case of polymethyldisiloxane [PDMS], N C / Si =2.
[0034] In the case of a mixture of two different surface treatment agents containing silicon atoms, the molar average N C / Si The same calculation method as above can be used, except that the values are used. Thus, if a 1:1 (50:50 mol%) molar mixture of HMDS and PDMS is used as the surface treatment agent, N C / Si The value (2*0.5+3*0.5)=2.5 must be used in the calculation.
[0035] The carbon content (C*) of powders and grains related to the presence of surface treatments can be determined, for example, by solid-state NMR analysis using an internal standard ( 1 H or 13 The carbon content can be measured directly using 1C NMR analysis (or calculated from elemental analysis by extraction of the carbon content, if such can be determined), independent of the presence of a surface treatment. In the simplest and most common case, all of the carbon content of the granules of the present invention that is measurable by elemental analysis comes from the surface treatment.
[0036] The granules according to the invention have a carbon content of 0.2% to 15% by weight, preferably 0.3% to 12% by weight, more preferably 0.5% to 10% by weight, more preferably 1.0% to 8% by weight, even more preferably 1.2% to 5% by weight, even more preferably 1.5% to 3.5% by weight. The carbon content can be determined by elemental analysis according to EN ISO3262-20:2000 (chapter 8). The analysis sample is weighed into a ceramic crucible equipped with a burner and heated in an induction furnace under a flow of oxygen. The carbon present is oxidized to CO2. The amount of CO2 gas is quantified by an infrared detector. SiC does not burn and therefore does not affect the value of the carbon content. Thus, when silicon carbide is used, for example, as an IR opacifier, the stated carbon content of the granules according to the invention refers to the total carbon-containing components of the granule, excluding non-combustible compounds such as silicon carbide.
[0037] The silica-based powder and granules according to the present invention [si] / d SiOH The ratio is preferably 0.5 to 10, more preferably 0.8 to 7.0, more preferably 1.0 to 5.0, more preferably 1.2 to 4.5, more preferably 1.5 to 4.0, more preferably 1.7 to 3.5, more preferably 1.8 to 3.4, more preferably 1.9 to 3.3, more preferably 2.0 to 3.2, more preferably 2.1 to 3.1, and more preferably 2.2 to 3.1.
[0038] More than 10 d [si] / d SiOH A high ratio of d corresponds to highly hydrophobic particles with a relatively low content of free silanol groups and therefore a low affinity of the material for polar systems. In contrast, a d ratio smaller than 1 corresponds to highly hydrophobic particles with a relatively low content of free silanol groups and therefore a low affinity of the material for polar systems. [si] / d SiOH A low ratio of is characteristic of highly polar materials with a relatively high content of free silanol groups, good compatibility with polar systems, but low hydrophobicity. The granules of the present invention preferably have [si] / d SiOH has a molecular weight of 1-10, making it sufficiently polar to be incorporated into polar systems such as water-based coating formulations, yet sufficiently hydrophobic to be used as an effective thermal insulating material.
[0039] The powder of the present invention is silica-based, i.e., the powder contains silica as a main component. Preferably, the powder contains at least 30% by weight, more preferably at least 40% by weight, more preferably at least 50% by weight, more preferably 60% to 99% by weight, more preferably 70% to 98% by weight, more preferably 75% to 95% by weight of silica.
[0040] The particle size distribution of granules can have a substantial effect on maximum material loading, viscosity, thermal conductivity, and other parameters important for the successful application of such granules in thermal insulation compositions. The optimal particle size distribution can also depend on the particular binder used in such thermal insulation compositions, and the thickness of the thermal insulation coating required.
[0041] The granular material according to the present invention preferably has a numerical median particle size d 50 is up to 6000 μm, more preferably 10 μm to 5000 μm, more preferably 20 μm to 3000 μm, more preferably 30 μm to 2500 μm, more preferably 40 μm to 2000 μm, more preferably 50 μm to 1500 μm, more preferably 80 μm to 1000 μm, more preferably 100 μm to 900 μm, more preferably 120 μm to 800 μm, even more preferably 150 μm to 700 μm, and most preferably 200 μm to 500 μm. The numerical median particle size of the granules can be measured by laser diffraction particle size analysis in accordance with ISO13320:2009. The measured particle size distribution can be used to determine the median d 50 This indicates the particle size that does not exceed 50% of all particles as the numerical median particle size.
[0042] The powder according to the present invention preferably has 10 The value is preferably 5 μm to 800 μm, more preferably 10 μm to 500 μm, more preferably 20 μm to 400 μm, more preferably 30 μm to 300 μm, more preferably 40 μm to 200 μm, and more preferably 50 μm to 150 μm. 90The value is 200 μm to 3000 μm, more preferably 300 μm to 2000 μm, more preferably 350 μm to 1500 μm, more preferably 400 μm to 1000 μm, more preferably 450 μm to 900 μm, and more preferably 500 μm to 800 μm. 10 value and d 50 The value can be measured by laser diffraction particle size analysis in accordance with ISO13320:2009. The measured particle size distribution can be used to determine the d 10 value and d 90 values are defined, which indicate the particle size that does not exceed 10% or 90%, respectively, of all particles.
[0043] The granular material according to the present invention preferably has a particle size of 10000 μm or less, preferably 7000 μm or less, more preferably 5000 μm or less, more preferably 4000 μm or less, more preferably 3000 μm or less, more preferably 2000 μm or less, more preferably 1500 μm or less, more preferably 1200 μm or less. To ensure that no particles have a particle size outside a certain range, the granules can be sieved, for example, through a suitable sieve.
[0044] Preferably, at least 5% by weight, more preferably at least 10% by weight, more preferably at least 15% by weight of the granules of the present invention have a particle size of less than 200 μm. In this case, it is surprising that so-called fines, i.e. particles with a particle size of less than 200 μm, do not interfere with the use of the granules as additives in liquid formulations. Such granules containing fines do not cause a substantial increase in the viscosity of the formulation, as is often the case with similar silica-based granules. Thus, the fines do not need to be separated from the granules before incorporating such granules into liquid formulations. Moreover, the presence of such fines in granules unexpectedly imparts high surface hydrophobicity and significant water repellency to insulating compositions containing such granules, the degree of water repellency being determined by measuring the water contact angle.
[0045] The tamped density of various powdery or coarse granules can be measured according to DIN ISO787-11:1995 "General test methods for pigments and extenders - Part 11: Determination of tamped volume and apparent density after tamping". This includes measuring the apparent density of the bed after stirring and tamping. The granules of the present invention have a tamped density of 140g / L to 290g / L, more preferably 140g / L to 270g / L, more preferably 150g / L to 250g / L, more preferably 150g / L to 240g / L, more preferably 150g / L to 230g / L, more preferably 160g / L to 220g / L.
[0046] The powder of the present invention has a BET surface area of 20 m 2 / g, preferably 30m 2 / g~500m 2 / g, more preferably 50m 2 / g~400m 2 / g, more preferably 70m 2 / g~300m 2 / g, most preferably 80m 2 / g~200m 2 The specific surface area, also simply called the BET surface area, can be determined by nitrogen adsorption according to the Brunauer-Emmett-Teller method in accordance with DIN 9277:2014.
[0047] The loss on drying (LOD) of the granular material according to the present invention is preferably less than 5.0% by weight, more preferably less than 3.0% by weight, more preferably less than 2.0% by weight, more preferably less than 1.0% by weight, more preferably less than 0.8% by weight, more preferably less than 0.5% by weight. Loss on drying can be measured according to ASTM D280-01 (Method A).
[0048] The thermal conductivity of the hydrophobized powder or granule of the present invention is preferably less than 70 mW / (mK), more preferably less than 50 mW / (mK), more preferably 10 mW / (mK) to 45 mW / (mK), particularly preferably 15 mW / (mK) to 40 mW / (mK), and most preferably 20 mW / (mK) to 35 mW / (mK), as measured at an average measurement temperature of 10°C, a contact pressure of 250 Pa, in an air atmosphere, and at standard pressure (1 atm) in accordance with EN12667:2001 using a bed type hot plate and a heat flow meter.
[0049] silica The silica may be a separate compound (silicon dioxide), a silica-based mixed oxide, a silica-based doped oxide, or a mixture thereof.
[0050] The silica may be selected from fumed silica, precipitated silica, silica aerogel, silica xerogel, perlite, silicate minerals or clay minerals, and mixtures thereof.
[0051] Silicate minerals are ionic solids whose anions are primarily the silicate anion SiO3 2- Each silicon atom is the center of a tetrahedron, and at the corners of the tetrahedron are four oxygen atoms covalently bonded to silicon. Two adjacent tetrahedra may share a vertex. Apart from Si and O atoms, silicate minerals may contain alkali metal, alkaline earth and other metal cations. One group of silicate minerals are the clays, also known as clay minerals, which are hydrous aluminum phyllosilicates (layered silicates) that may contain varying amounts of iron, magnesium, alkali metal, alkaline earth, and other cations found on or near the surfaces of some planets. Examples of clay minerals are halloysite, kaolinite, illite, montmorillonite, verniculite, talc, sepiolite, palygorskite and pyrophyllite.
[0052] The granules according to the invention preferably comprise amorphous silica. Amorphous or non-crystalline silica lacks the long-range order characteristic of crystalline silica, such as that present in quartz.
[0053] The amorphous silica present in the granules according to the invention can be chosen from fumed silica, precipitated silica, silica aerogels, silica xerogels, and mixtures thereof.
[0054] The powder or granule of the present invention preferably contains 30% to 95% by weight of silica selected from fumed silica, precipitated silica, silica aerogel, silica xerogel, and mixtures thereof.
[0055] Silicon dioxide produced by precipitation (precipitated silica) is produced, for example, during the reaction of waterglass solution (water-soluble sodium silicate) with mineral acids.
[0056] Aerogels can be produced by supercritical drying of SiO2 gels produced by the so-called sol-gel process. The starting materials for the synthesis of SiO2 sols are often silicon alcoholates. The hydrolysis of such precursors and the condensation between the resulting reactive species are the main basic reactions of the sol-gel process. Tetraalkyl orthosilicates such as tetramethyl orthosilicate or tetraethyl orthosilicate are particularly suitable as silicon sources. The alcohols produced during the hydrolysis of tetraalkyl orthosilicates are removed under supercritical conditions (temperatures above 239.4 °C and pressures above 80.9 bar for methanol) to produce highly porous SiO2 aerogels.
[0057] Drying under subcritical conditions can produce materials with nearly the same properties as supercritically dried aerogels, commonly called xerogels. The preparation of such xerogels is described, for example, in U.S. Patent Publication No. 5,565,142 A1.
[0058] Particularly preferred for the present invention are pyrogenic (fumed) silicas and silica-based pyrogenic mixed oxides. Fumed silicas are prepared by flame hydrolysis or flame oxidation. This involves the oxidation or hydrolysis of hydrolyzable or oxidizable starting materials, generally in a hydrogen / oxygen flame. The starting materials used in the pyrogenic process include organic and inorganic substances. Silicon tetrachloride is particularly suitable. The hydrophilic silicas thus obtained are amorphous. Fumed silicas are generally in an aggregated form. "Agglomeration" is understood to mean that what are called primary particles formed at the beginning of the development are firmly bonded to each other in a subsequent reaction to form a three-dimensional network. The primary particles are substantially free of pores and have free hydroxyl groups on their surface. Such hydrophilic silicas can be hydrophobized if necessary, for example by treatment with reactive silanes.
[0059] It is also known to produce exothermic mixed oxides by simultaneously reacting at least two different metal sources in the form of volatile metal compounds (e.g. chlorides) in a H2 / O2 flame. An example of such an oxide is the SiO2 / Al2O3 mixed oxide produced by Evonik under the name Aerosil® MOX170. For the production of Aerosil® MOX170, a mixture of SiCl4 and AlCl3 is hydrolyzed directly in the flame. As described in DE-A 952 891, DE-A 25 33 925 and DE-A 27 02 896, the corresponding silanes, e.g. methyltrichlorosilane, trichlorosilane, etc., may also be used as raw materials instead of or in addition to the chlorides.
[0060] All components of the mixed oxide thus prepared (e.g., silica and alumina in the aforementioned cases) are generally uniformly distributed throughout the mixed oxide material, in contrast to other types of materials such as mechanical mixtures of multiple metal oxides, doped metal oxides, etc. In the latter case, e.g., in the case of a mixture of multiple metal oxides, there may be separate regions of corresponding pure oxides, which determine the properties of such mixtures.
[0061] IR Opacifier The granule of the present invention contains at least one IR opacifier. Such an IR opacifier reduces the infrared transmittance of the insulation material, thereby minimizing the heat transfer by radiation. The IR opacifier is selected from the group consisting of silicon carbide, titanium dioxide, zirconium dioxide, ilmenite, iron titanate, iron oxide, zirconium silicate, manganese oxide, graphite, carbon black, and mixtures thereof. The average particle size of the IR opacifier is preferably 0.1 to 25 μm.
[0062] The powder or granule of the present invention may contain 1% by weight to 70% by weight, more preferably 3% by weight to 65% by weight, more preferably 5% by weight to 60% by weight, more preferably 10% by weight to 50% by weight, and more preferably 12% by weight to 30% by weight of an IR opacifier.
[0063] Surface Treatment Agents In the present invention, the term "hydrophobized with a surface treatment agent containing silicon atoms" refers to a chemical reaction between a material containing silica and a corresponding surface treatment agent containing silicon atoms, which imparts hydrophobicity to the material containing silica by completely or partially modifying the silica surface with hydrophobic groups containing silicon atoms.
[0064] The term "hydrophobized" or "hydrophobic" in the context of the present invention relates to surface-treated particles that have a low affinity for polar media such as water. In contrast, hydrophilic particles have a high affinity for polar media such as water. The hydrophobicity of hydrophobic materials is usually obtained by applying suitable non-polar groups to the silica surface. The degree of hydrophobicity of a hydrophobic oxide (e.g. silica) can be measured by parameters such as its methanol wettability, as described in detail for example in WO 2011 / 076518 A1, pages 5-6. In pure water, the hydrophobic silica completely separates from the water and floats on its surface without being wetted by the solvent. In contrast, in pure methanol, the hydrophobic silica is distributed throughout the solvent and is completely wetted. In the measurement of methanol wettability, the maximum methanol content at which the silica is not yet wetted is measured in a methanol / water test mixture. This means that 100% of the silica used remains separated from the test mixture in an unwetted state after contact with the test mixture. This methanol content (volume %) in the methanol / water mixture is called the methanol wettability. The higher the level of such methanol wettability, the more hydrophobic the silica. The lower the methanol wettability, the less hydrophobic and more hydrophilic the material.
[0065] The powder or granule of the present invention preferably has a methanol content, which is methanol wettable in a methanol / water mixture, of more than 10 volume %, more preferably 20 volume % to 90 volume %, more preferably 30 volume % to 85 volume %, particularly preferably 35 volume % to 80 volume %, and most preferably 40 volume % to 75 volume %.
[0066] The surface treatment agent containing silicon atoms is preferably selected from the group consisting of organosilanes, silazanes, acyclic polysiloxanes, cyclic polysiloxanes, and mixtures thereof.
[0067] One type of preferred organosilane has the general formula: R' x (RO) y Si(C n H 2n+1) (Ia), and R' x (RO) y Si(C n H 2n-1 ) (Ib) (wherein R=alkyl, e.g., methyl-, ethyl-, n-propyl-, i-propyl-, butyl-, etc.) R'=alkyl or cycloalkyl, e.g., methyl, ethyl, n-propyl, i-propyl, butyl, cyclohexyl, octyl, hexadecyl, etc.; n=1 to 20, x+y=3, x=0~2, and y=1~3.) It is an alkylorganosilane.
[0068] Among the alkylorganosilanes of formulae (Ia) and (Ib), particularly preferred are octyltrimethoxysilane, octyltriethoxysilane, hexadecyltrimethoxysilane, and hexadecyltriethoxysilane.
[0069] The organosilanes used for the surface treatment may contain halogens such as Cl or Br. The following types of halogenated organosilanes are particularly preferred: - organosilanes of the general formula: X3Si(C n H 2n+1 ) (IIa), and X3Si(C n H 2n-1 ) (IIb) (In the formula, X=Cl, Br; n=1 to 20.) - organosilanes of the general formula: X2(R')Si(C n H 2n+1 ) (IIIa) and X2(R')Si(C n H 2n-1 ) (IIIb) (In the formula, X=Cl, Br; R'=alkyl, for example, cycloalkyl such as methyl, ethyl, n-propyl, i-propyl, butyl, cyclohexyl, etc.; n=1 to 20.) - organosilanes of the general formula: X(R')2Si(C n H 2n+1 ) (IVa) and X(R')2Si(C n H 2n-1 ) (IVb) (In the formula, X=Cl, Br; R'=alkyl, for example, cycloalkyl such as methyl, ethyl, n-propyl, i-propyl, butyl, cyclohexyl, etc.; n=1 to 20.)
[0070] Among the halogenated organosilanes of the formulae (II) to (IV), dimethyldichlorosilane and chlorotrimethylsilane are particularly preferred.
[0071] The organosilanes used can contain, in addition to alkyl or halogen substituents, for example fluorine substituents or multiple functional groups. It is preferred to use functionalized organosilanes of the general formula: (R' ') x (RO) y Si(CH2) m R' (V) (Wherein R' '=alkyl such as methyl, ethyl, propyl, etc., or halogen such as Cl or Br; R = alkyl, such as methyl, ethyl, or propyl; x+y=3 x=0~2, y=1~3, m=1~20, R' = methyl-, aryl (e.g., phenyl or substituted phenyl residues), heteroaryl-CF, OCF-CHF-CF, -CF 13, -O-CF2-CHF2, -NH2, -N3, -SCN, -CH=CH2, -NH-CH2-CH2-NH2, -N-(CH2-CH2-NH2)2, -OOC(CH3)C=CH2 , -OCH2-CH(O)CH2, -NH-CO-N-CO-(CH2)5, -NH-COO-CH3, -NH-COO-CH2-CH3, -NH-(CH2)3Si(OR)3, -S x -(CH2)3Si(OR)3, -SH, -NR 1 R 2 R 3 (In the formula, R 1 = alkyl, aryl; R 2 =H, alkyl, aryl; R 3 =H, alkyl, aryl, benzyl, C2H4NR 4 R 5 (In the formula, R 4 =H, alkyl; R 5 =H, alkyl).
[0072] Of the functionalized organosilanes of formula (V), 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, glycidyloxypropyltrimethoxysilane, glycidyloxypropyltriethoxysilane, aminopropyltriethoxysilane are particularly preferred.
[0073] Silazanes of the general formula R'R2SiNH-SiR2R'(VI), where R=alkyl, such as methyl, ethyl, propyl, etc.; R'=alkyl, vinyl, are also suitable as surface treatment agents. The most preferred silazane of formula (VI) is hexamethyldisilazane (HMDS).
[0074] Cyclic polysiloxanes such as octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecamethylcyclohexasiloxane (D6), hexamethylcyclotrisiloxane (D6), etc. are also suitable as surface treatment agents. Among the cyclic polysiloxanes, it is most preferable to use D4.
[0075] Another useful type of surface treatment agent has the general formula (VII):
[0076] [ka]
[0077] (In the formula, Y=H, CH3, C n H 2n+1 (in the formula, n=1~20), Si(CH3) a X b (In the formula, a=2 to 3, b=0 or 1, and a+b=3), X=H, OH, OCH3, C m H 2m+1 (In the formula, m=1~20), R, R' = alkyl such as CoH2o+1 (where o = 1 to 20), aryl such as phenyl and substituted phenyl residues, heteroaryl, (CH2) k -NH2 (in the formula, k=1~10), H, u=2 to 1000, preferably u=3 to 100.) The polysiloxane or silicone oil is
[0078] Among the polysiloxanes and silicone oils of formula (VII), polydimethylsiloxanes are most preferably used as surface treatment agents. Such polydimethylsiloxanes usually have a molar mass of 162 g / mol to 7500 g / mol, a density of 0.76 g / mL to 1.07 g / mL, and a viscosity of 0.6 mPa·s to 1,000,000 mPa·s.
[0079] Powder manufacturing method The present invention further provides a method for producing silica-based powder or granules according to any one of claims 1 to 11, comprising the following steps: a) hydrophilic silica; at least one IR-opacifier selected from the group consisting of silicon carbide, titanium dioxide, zirconium dioxide, ilmenite, iron titanate, iron oxide, zirconium silicate, manganese oxide, graphite, carbon black, and mixtures thereof; drying and densifying the powder to produce a hydrophilic granule having a tamped density of at least 80 g / L; b) heat-treating the hydrophilic powder produced in step a) at a temperature of 300°C to 1,400°C; c) A step of hydrophobizing the hydrophilic powder or granules that have been heat-treated in step b) in the presence of a surface treatment agent containing silicon atoms and water. The molar ratio of water to silicon atoms in the surface treatment agent containing silicon atoms is 0.1-100, preferably 0.2-50, more preferably 0.4-20, more preferably 0.5-10, and more preferably 1-5.
[0080] The term "drying to densify" in the context of the present invention refers to any process aimed at increasing the density (e.g. tamping density) of a granular material, in which little or no liquid, such as water, is used. Preferably, in step a) of the present invention, not more than 15% by weight, more preferably not more than 12% by weight, more preferably not more than 10% by weight, more preferably not more than 8% by weight, more preferably not more than 5% by weight of liquid (e.g. water), based on the mass of the powder comprising hydrophilic silica, is used. Thus, densification of silica powder by spray drying of an aqueous dispersion of silica powder, as disclosed in US Pat. No. 5,399,363, does not fall within the term "drying to densify" according to the present invention.
[0081] In step a) of the method according to the invention, the powder comprising hydrophilic silica is densified, for example by degassing or compaction, to produce a hydrophilic granule having a tamped density of at least 80 g / L, preferably from 80 g / L to 400 g / L, more preferably from 80 g / L to 350 g / L, more preferably from 80 g / L to 300 g / L, more preferably from 80 g / L to 250 g / L, more preferably from 85 g / L to 220 g / L, more preferably from 90 g / L to 200 g / L. The main objective of step a) of the method according to the invention is to produce hydrophilic granules with the required particle size and tamping density, which are important for the mechanical and insulating properties of the final hydrophobized granules prepared by the method according to the invention. The process of the invention may further comprise a further step a-1) of preparing a powder mixture comprising hydrophilic silica and at least one IR opacifier, which is carried out before step a) of the process according to the invention. In step a1), the silica, the IR opacifier and any other additives may be mixed together. This mixing of hydrophilic silica with at least one IR opacifier and, if necessary, any other additives according to step a1) of the method of the present invention can be carried out in any suitable mixing device known to those skilled in the art. Any mixer or mill that allows good homogenization, such as blade mixers, plowshare mixers, fluidized bed mixers, centrifugal mixers or air-swept mixers, is suitable for carrying out step a1) of the method. Particularly suitable mixers are those that can further compact the materials to be mixed, such as plowbar mixers, pan mills or ball mills. Thus, steps a1) and a) of the method of the present invention can be carried out as separate independent stages or combined in one process.
[0082] In step b) of the method according to the present invention, the hydrophilic powder-granule produced in step a) is heat-treated at a temperature of 300° C. to 1400° C., preferably 400° C. to 1350° C., more preferably 450° C. to 1300° C., more preferably 550° C. to 1280° C., more preferably 600° C. to 1250° C., more preferably 700° C. to 1200° C., more preferably 750° C. to 1200° C., more preferably 800° C. to 1190° C., more preferably 850° C. to 1180° C., more preferably 900° C. to 1150° C. The duration of step b) depends on the applied temperature and is generally 1 minute to 20 hours, preferably 5 minutes to 10 hours.
[0083] The heat treatment of step b) of the method according to the invention reduces the number of free silanol groups, increases the skeletal density of the silica-based powder and granules and significantly increases the mechanical strength of the hydrophilic powder and granules.
[0084] The hydrophilic granules produced in step b) of the process according to the invention preferably have a number of silanol groups d relative to the BET surface area, measured by reaction with lithium aluminum hydride. SiOH But 2.0SiOH / nm 2 less than 0.3 to 1.9SiOH / nm 2 , more preferably 0.4 to 1.8SiOH / nm 2 , more preferably 0.5 to 1.7SiOH / nm 2 , more preferably 0.5 to 1.6SiOH / nm 2 , more preferably 0.5 to 1.5SiOH / nm 2 , more preferably 0.6 to 1.4SiOH / nm 2 , more preferably 0.7 to 1.3SiOH / nm 2 It is.
[0085] In the method according to the invention, after step a) and / or step b) and / or step c), the different size fractions of the granular material are separated from each other in such a way that only one or more fractions having a specific particle size are separated and further used. Such a separation can be achieved by sieving through suitable sieves.
[0086] Separation of particles larger than 4000 μm, more preferably larger than 3000 μm, more preferably larger than 2000 μm, more preferably larger than 1500 μm is preferably carried out before carrying out step c) of the method according to the invention. The smaller particles thus obtained can be further used in step c) of the method, while the separated larger particles can be recycled and further used in the previous steps of the method, for example in step a).
[0087] In step c) of the method according to the present invention, the hydrophilic powder or granule that has been subjected to the heat treatment in step b) is hydrophobized in the presence of a silicon atom-containing surface treatment agent and water. The molar ratio of water to silicon atoms in the silicon atom-containing surface treatment agent is 0.01 to 100, preferably 0.05 to 50, more preferably 0.1 to 40, more preferably 0.1 to 30, more preferably 0.2 to 20, more preferably 0.5 to 15, more preferably 0.8 to 10, more preferably 0.9 to 8, and more preferably 1 to 6.
[0088] The use of both the silicon-containing surface treatment agent and water in the above-mentioned ratios in step c) of the process according to the invention is essential for achieving the unique properties of the granular material according to the invention, namely its relatively high hydrophobicity and relatively high polarity.
[0089] The silicon-containing surface treatment agent and / or water are preferably used in liquid form in the method according to the present invention.
[0090] Step c) of the method according to the invention can be carried out at a temperature between 10°C and 250°C for 1 min to 24 h. The duration of step c) can be selected according to the specific requirements of the method and / or the targeted granule properties. Thus, usually, the lower the treatment temperature, the longer the hydrophobization time. In a preferred embodiment of the invention, the hydrophobization of the hydrophilic granules is carried out at 10-80°C for 3-24 h, preferably 5-24 h. In another preferred embodiment of the invention, step c) of the method is carried out at 90-200°C, preferably 100-180°C, most preferably 120-160°C, for 0.5-10 h, preferably 1-8 h. Step c) of the method according to the invention can be carried out under a pressure of 0.1-10 bar, preferably 0.5-8 bar, more preferably 1-7 bar, most preferably 1.1-5 bar. Most preferably, step c) is carried out in a closed system at the reaction temperature and under the natural vapor pressure of the surface treatment agent used.
[0091] In step c) of the method according to the invention, the hydrophilic granules subjected to the heat treatment in step b) are preferably sprayed at ambient temperature (about 25° C.) with liquid water and then with a liquid surface treatment agent, or with a liquid surface treatment agent and then with liquid water, or with a liquid mixture of water and liquid surface treatment agent, after which the mixture is heat treated at a temperature between 50° C. and 400° C. for 1 hour to 6 hours.
[0092] An alternative method of surface treatment in step c) can be carried out by treating the hydrophilic granules heat-treated in step b) first with water and then with the surface treatment agent, or first with the surface treatment agent and then with water, or with a mixture of water and the surface treatment agent (the water and / or the surface treatment agent are in vapor form), followed by heat treatment of the mixture at a temperature of 50°C to 800°C for 0.5 to 6 hours.
[0093] The heat treatment after hydrophobization in step c) can be carried out under a protective gas, for example nitrogen. The surface treatment can be carried out continuously or batchwise in a heatable mixer and dryer equipped with a spraying device. Suitable devices can be, for example, a plowshare mixer, a free-fall mixer or plate, a cyclone, or a fluidized bed dryer.
[0094] The amount of surface treatment agent used may depend on the type of particles and surface treatment agent applied, but typically 1% to 15% by weight, preferably 2% to 10% by weight, of the surface treatment agent is used relative to the amount of hydrophilic powder or granule.
[0095] The amount of surface treatment agent used may depend on the type of particles and surface treatment agent applied, but typically 1% to 25% by weight, preferably 2% to 20% by weight, more preferably 5% to 18% by weight of the surface treatment agent is used relative to the amount of hydrophilic powder or granules subjected to heat treatment in step b).
[0096] The amount of water used may also depend on the type of particles and surface treatment agent applied, but typically 0.5% to 15% by weight, preferably 1% to 12% by weight, more preferably 2% to 10% by weight of water is used relative to the amount of hydrophilic granules heat-treated in step b).
[0097] The required amounts of water and surface treatment agent may depend on the BET surface area of the hydrophilic granules used. Thus, the BET specific surface area of the hydrophilic granules heat-treated in step b) is 2 Per unit weight, 0.1 μmol to 100 μmol, more preferably 1 μmol to 50 μmol, and more preferably 3.0 μmol to 20 μmol of silicon atoms in the surface treatment agent and 0.1 μmol to 500 μmol, more preferably 1 μmol to 100 μmol, and more preferably 10 μmol to 50 μmol of water are used.
[0098] Thermal Insulation Composition Another subject of the invention is a thermal insulation composition comprising the hydrophobized granules of the invention. The thermal insulation composition according to the invention can comprise at least one binder, i.e. a binder capable of binding the individual parts of the cured composition to one another and, if necessary, to one or more fillers and / or other additives, thereby improving the mechanical properties of the cured composition. Such binders can comprise organic or inorganic substances. The binders optionally comprise reactive organic substances. Organic binders can be selected, for example, from the group consisting of (meth)acrylates, alkyd resins, epoxy resins, gum arabic, casein, vegetable oils, polyurethanes, silicone resins, waxes, cellulose adhesives, and mixtures thereof. Such organic substances can harden the thermal insulation composition used, for example, by evaporation of the solvent, polymerization, crosslinking reactions, or another type of physical or chemical transformation. Such hardening can be carried out, for example, by heat or under the action of UV radiation or other radiation. Both single (one) component (1-C) and multi-component systems, in particular two-component systems (2-C), can be applied as binders. Particularly preferred for the present invention are water-based or (preferably as a two-component system) water-(meth)acrylate-based binders and miscibility with epoxy resins.
[0099] Most organic binder materials, such as (meth)acrylates and epoxy resins, have certain thermal limitations and cannot be used at temperatures above 150° C. In contrast, siloxane-based materials (silicone resins) are generally thermally stable and can be applied at temperatures up to about 600° C. without thermal degradation. Such organosiloxane binders (silicone resins), or hybrid systems that include silicone systems and other organic components, are particularly preferred for use in the compositions of the present invention.
[0100] In addition to or as an alternative to organic binders, the insulating composition of the present invention may contain inorganic hardening substances. Such inorganic binders, also called mineral binders, play essentially the same role as organic binders, that is, to bind the additive materials together. In addition, inorganic binders are divided into non-hydraulic and hydraulic binders. Non-hydraulic binders are water-soluble binders such as calcium lime, dolomitic lime, gypsum, and anhydrite that harden only in air. Hydraulic binders are binders that harden in air and in the presence of water and become water-insoluble after hardening. They include hydraulic lime, cement, and masonry cement. Mixtures of various inorganic binders may also be used in the insulating composition of the present invention.
[0101] The insulating composition of the invention may contain 10-90% by weight of hydrophobized powder and 10-90% by weight of binder and optionally present solvent (preferably water). The weight ratio of hydrophobized powder and binder / solvent in such an insulating composition may vary significantly depending on the amount of water and / or other solvents present in the insulating composition. Thus, in an insulating composition ready for application ("wet", "liquid"), the proportion of binder, which may contain water or other solvents, is usually higher. In this case, the insulating composition of the invention may contain 10% to 60% by weight, more preferably 15% to 50% by weight, of hydrophobized powder according to the invention, and 40% to 90% by weight, more preferably 50% to 85% by weight, of solvent and inorganic and / or organic binder. After application of such a "wet" insulating composition to the surface to be separated, the solvent is usually at least partially removed, leaving a "dry" and usually solid insulating composition. The heat insulating composition contains 20% to 90% by weight, more preferably 30% to 70% by weight, of the hydrophobized powder or granule of the present invention, and 10% to 80% by weight, more preferably 20% to 60% by weight, of an inorganic and / or organic binder.
[0102] The curing of the heat insulating composition can be achieved by at least partial polymerization and / or removal of the solvent. Depending on the system used, this step can be carried out at temperatures preferably between 0 and 500 ° C, particularly preferably between 5 and 400 ° C, very particularly preferably between 10 and 300 ° C. Curing can be carried out in the presence of air or with the exclusion of oxygen, for example under a protective gas atmosphere of nitrogen or carbon dioxide. The above steps can be carried out under standard pressure or under reduced pressure, for example under vacuum.
[0103] Apart from the hydrophobized granules and the binder, the heat insulating composition according to the invention may further comprise at least one solvent and / or filler and / or other additives.
[0104] The solvent used in the composition of the present invention can be selected from the group consisting of water, alcohols, aliphatic and aromatic hydrocarbons, ethers, esters, aldehydes, ketones, and mixtures thereof. For example, the solvent used can be water, methanol, ethanol, propanol, butanol, pentane, hexane, benzene, toluene, xylene, diethyl ether, methyl tert-butyl ether, ethyl acetate, and acetone. Particularly preferably, the solvent used in the heat insulating composition has a boiling point of less than 300°C, particularly preferably less than 200°C. Such relatively volatile solvents can be easily evaporated or vaporized during the curing of the heat insulating composition according to the present invention. Most preferably, the heat insulating composition of the present invention comprises water as the only solvent.
[0105] In one embodiment of the present invention, a mixture of the hydrophobized powder of the present invention, preferably based on fumed silica, and hydrophobized silica aerogel powder is used in the thermal insulation composition, in such a case the ratio of the hydrophobized powder of the present invention to the aerogel material is preferably between 10:1 and 1:1 by weight.
[0106] The thermal conductivity of the insulating composition, measured in accordance with EN12667:2001 using a method using a guarded hot plate and a heat flow meter device at an average measurement temperature of 10°C and a contact pressure of 250 Pa under an air atmosphere at standard pressure (1 atm), is preferably less than 70 mW / (mK), more preferably less than 50 mW / (mK), more preferably 10 mW / (mK) to 45 mW / (mK), particularly preferably 15 mW / (mK) to 40 mW / (mK), and most preferably 20 mW / (mK) to 35 mW / (mK).
[0107] Use of powder and heat insulating composition The hydrophobized powders and / or heat insulating compositions based thereon according to the invention can be used generally for thermal insulation and / or sound insulation, in particular for sound and / or thermal insulation of walls, roofs, houses, as well as for thermal insulation of industrial plants, parts of industrial equipment, tanks, process pipes, ducts, pipelines, etc.
[0108] The insulating composition comprising the granules of the present invention can be applied to the surfaces to be isolated by any suitable method, such as brushing, spraying, troweling, dip coating, and the like. EXAMPLES
[0109] Analysis methods, measurement / calculation of parameters The cumulative pore volume of pores larger than 4 nm (Hg-pore volume larger than 4 nm) [unit: cm ] was determined by mercury intrusion porosimetry in accordance with DIN ISO 15901-1 using an AutoPore V 9600 instrument (Micomeritics). 3 / g] was measured. Only the pore volume of pores that could be penetrated by mercury at the maximum applied pressure (417 MPa) (i.e., pores with a pore diameter of more than 4 nm) was detected.
[0110] Cumulative pore volume of pores less than 4 μm (Hg-pore volume less than 4 μm, unit: cm 3 / g) was determined by the same mercury intrusion method in accordance with DIN ISO 15901-1 and corresponds to the cumulative pore volume of all pores smaller than 4 μm that can be distinguished in this way.
[0111] After excluding the volume of all pores larger than 4 nm (at maximum intrusion pressure: 417 MPa) from the volume assumed to be occupied by the material, the skeletal density [unit: g / cm 3 ] was measured.
[0112] Loss on drying (LOD, unit: wt%) was measured according to ASTM D280-01 (Method A).
[0113] The BET specific surface area [units: m2] was determined according to DIN 9277:2014 by nitrogen adsorption using the Brunauer-Emmett-Teller method. 2 / g] was measured.
[0114] The tamping density [unit: g / L] was measured according to DIN ISO787-11:1995.
[0115] Methanol wettability [volume % of methanol in methanol / water mixture] was measured according to the method detailed on pages 5-6 of WO 2011 / 076518 A1.
[0116] The carbon content (in weight %) was determined by elemental analysis using a carbon measuring system C632 (manufacturer: LECO) in accordance with EN ISO3262-20:2000 (chapter 8). The analyzed samples were weighed into ceramic crucibles equipped with a burner and heated in an induction furnace under a flow of oxygen. The carbon present is oxidized to CO2. The amount of CO2 gas is quantified by an infrared detector (IR). SiC does not burn and therefore does not affect the value of the carbon content.
[0117] As described in detail in Patent Document 3, page 8, line 17 to page 9, line 12, the number of silanol groups relative to the BET surface area d is increased by reacting a pre-dried sample of granules with a lithium aluminum hydride solution. SiOH [Unit: SiOH / nm 2 ] was measured.
[0118] The number of silicon atoms in the surface treatment agent relative to the BET surface area of the powder or granule of the present invention, d [Si] [Unit: Si atom / nm 2 ] is calculated from the carbon content associated with the presence of the surface treatment (=carbon content measured by elemental analysis of all test samples) and the chemical structure of the surface treatment, e.g., the number of carbon atoms per silicon atom of the surface treatment (N C / Si ) taking into account: d [Si] [Si atoms / nm 2 ]=(C*[weight%]×N A ) / (Mr C [g / mol]×N C / Si ×BET[m 2 / g]×10 20 ) (3) (In the ceremony, Mr. C = 12,011 g / mol is the atomic weight of carbon, N A is Avogadro's constant (~6.022*10 23 ) and NC / Si is the ratio of carbon atoms to silicon atoms in the surface treatment agent. (In the case of hexamethyldisilazane, N C / Si =3)
[0119] The number of silicon atoms in the surface treatment agent relative to the BET surface area (d [Si] ) is the number of silanol groups relative to the BET surface area (d SiOH ) by dividing by d [Si] / d SiOH The ratio was calculated.
[0120] Thermal conductivity [mW / (m*K)] was measured using a guarded hot plate and heat flow meter in accordance with EN12667:2001. The average measurement temperature was 10°C and the contact pressure was 1000 Pa. The measurements were performed in air at standard pressure.
[0121] Preparation of silica-based materials Comparative Example 1 (Silica powder hydrophobized with HMDS) Silica powder hydrophobized with HMDS AEROSIL® R812 (BET=172 m 2 / g, manufacturer: EVONIK Resource Efficiency GmbH) was used as a reference material. The physicochemical properties of this silica powder are shown in Table 2.
[0122] Comparative Example 2 (HMDS-Hydrophobicized Silica / SiC Granules) mixture 20% by weight of 1000F silicon carbide (Carsimet, manufacturer: Keyvest) and AEROSIL® R812 hydrophobic silica (hydrophobized with HMDS, BET = 172 m 2 % (by weight) of 100g / g, manufacturer: EVONIK Resource Efficiency GmbH) was mixed using a Minox PSM300HN / 1MK ploughshare mixer.
[0123] High density The mixture of AEROSIL® R812 and silicon carbide produced as described above was densified with Grenzebach densification rolls (Vacupress VP160 / 220). The tamping density of the resulting granulate was adjusted to 166 g / L by the applied contact pressure, roll speed and vacuum. The applied vacuum was less than 300 mbar (absolute). The roll speed was 5 rpm and the pressure was 2000 N.
[0124] Sieving / Sorting To obtain the desired fraction, the powder was first fed into a vibrating sieve mill (manufacturer: FREWITT) with a mesh size of 3150 μm, and in order to establish an upper limit for the particles, particles larger than this upper limit were removed. The particle fraction was then separated to obtain a particle fraction with a particle size between 200 and 1190 μm. This was done using a vibrating sieve model LS18S manufactured by Sweco. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0125] Comparative Example 3 (without heat treatment) mixture 20% by weight of 1000F silicon carbide (Carsimet, manufacturer: Keyvest) and AEROSIL® 300 hydrophilic silica (BET = 300 m 2 % (by weight) of 100g / g, manufacturer: EVONIK Resource Efficiency GmbH) was mixed using a Minox PSM300HN / 1MK ploughshare mixer.
[0126] High density The above produced mixture of AEROSIL® 300 and silicon carbide was densified with Grenzebach densification rolls (Vacupress VP160 / 220). The tamping density of the resulting granulate was adjusted to 120±5 g / L by the applied contact pressure, roll speed and vacuum. The applied vacuum was less than 300 mbar (absolute). The roll speed was 5 rpm and the pressure was 2000 N.
[0127] Sieving / Sorting To obtain the desired fraction, the granules were fed into a vibrating sieve mill (manufacturer: FREWITT) with a mesh size of 1000 μm, and in order to establish an upper particle limit, particles larger than this limit were removed.
[0128] Hydrophobization The hydrophilic granules (100 g) after the densification process were placed in a grounded metal bucket and mixed with a propeller mixer at 200 rpm, and water (8 g) was sprayed onto its surface with continuous stirring at 25 °C, followed by 12 g of hexamethyldisilazane (HMDS). Mixing was continued for 5 min. The bucket was then sealed with a lid with several holes of 0.5-1 mm diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The granules were then placed in a drying pan and dried in an oven at 120 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances.
[0129] The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0130] Comparative Example 4 (heat treatment, no hydrophobic treatment) mixture 20% by weight of 1000F silicon carbide (Carsimet, manufacturer: Keyvest) and AEROSIL® 300 hydrophilic silica (BET = 300 m 2 % (80% by weight) of 1000g / g (manufacturer: EVONIK Resource Efficiency GmbH) was mixed with a Minox PSM300HN / 1MK ploughshare mixer. High density The above produced mixture of AEROSIL® 300 and silicon carbide was densified with Grenzebach densification rolls (Vacupress VP160 / 220). The tamping density of the resulting granulate was adjusted to 120±5 g / L by the applied contact pressure, roll speed and vacuum. The applied vacuum was less than 300 mbar (absolute). The roll speed was 5 rpm and the pressure was 2000 N. Sintering / hardening Subsequent heat hardening was carried out in a XR310 chamber kiln from Schroder Industrieofen GmbH. For this purpose, a temperature program was applied in multiple layers with a bed height of up to 5 cm. The temperature gradient was 300 K / h up to the target temperature of 1025° C. The holding time was 3 h. The samples were then cooled (without active cooling) until removal. The tamped density of the resulting sintered granules was 180±10 g / L. Sieving / Sorting To obtain the desired fraction, the thermoset granules were fed into a vibrating sieve mill (manufacturer: FREWITT) with a mesh size of 1000 μm, and in order to establish an upper particle limit, particles larger than this limit were removed. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0131] Comparative Example 5 (Heat treatment, hydrophobization without water) mixture 20% by weight of 1000F silicon carbide (Carsimet, manufacturer: Keyvest) and AEROSIL® 300 hydrophilic silica (BET = 300 m 2 % (80% by weight) of 1000g / g (manufacturer: EVONIK Resource Efficiency GmbH) was mixed with a Minox PSM300HN / 1MK ploughshare mixer. High density The above produced mixture of AEROSIL® 300 and silicon carbide was densified with Grenzebach densification rolls (Vacupress VP160 / 220). The tamping density of the resulting granulate was adjusted to 120±5 g / L by the applied contact pressure, roll speed and vacuum. The applied vacuum was less than 300 mbar (absolute). The roll speed was 5 rpm and the pressure was 2000 N. Sieving / Sorting To obtain the desired fraction, the thermoset granules were fed into a vibrating sieve mill (manufacturer: FREWITT) with a mesh size of 1000 μm, and in order to establish an upper particle limit, particles larger than this limit were removed. Sintering / hardening Subsequent heat hardening was carried out in a XR310 chamber kiln from Schroder Industrieofen GmbH. For this purpose, a temperature program was applied in multiple layers with a bed height of up to 5 cm. The temperature gradient was 300 K / h up to the target temperature of 1025° C. The holding time was 3 h. The samples were then cooled (without active cooling) until removal. The tamped density of the resulting sintered granules was 180±10 g / L. Hydrophobization The hydrophilic granules (500 g) after the densification process were placed in a grounded metal bucket, mixed with a propeller mixer at 300-500 rpm, and hexamethyldisilazane (HMDS) (60 g) was sprayed onto its surface with continuous stirring at 25 °C. Mixing was continued for 10 min. The bucket was then sealed with a lid with several holes of 0.5-1 mm diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The granules were then placed in a drying pan and dried in an oven at 145 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances. Separation of particle fractions, when necessary, was performed using a Sweco vibrating screen model LS18S. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0132] Comparative Example 6 (Heat treatment, hydrophobization in the form of steam) The preparation of hydrophobized silica granules containing an IR opacifier was carried out as described in International Application No. PCT / EP2018 / 051142. mixture 20% by weight of 1000F silicon carbide (Carsimet, manufacturer: Keyvest) and AEROSIL® 300 hydrophilic silica (BET = 300 m 2 % (80% by weight) of 1000g / g (manufacturer: EVONIK Resource Efficiency GmbH) was mixed with a Minox PSM300HN / 1MK ploughshare mixer. High density The above produced mixture of AEROSIL® 300 and silicon carbide was densified with Grenzebach densification rolls (Vacupress VP160 / 220). The tamping density of the resulting granulate was adjusted to 121 g / L by the applied contact pressure, roll speed and vacuum. The applied vacuum was less than 300 mbar (absolute). The roll speed was 5 rpm and the pressure was 2000 N. Sintering / hardening Subsequent heat hardening was carried out in a XR310 chamber kiln from Schroder Industrieofen GmbH. For this purpose, a temperature program was applied in multiple layers with a bed height of up to 5 cm. The temperature gradient was 300 K / h up to the target temperature of 900 °C. The holding time was 3 h. The samples were then cooled (without active cooling) until removal. The tamped density of the resulting sintered granules was 180 g / L. Hydrophobization Final hydrophobization of the thermoset granules was carried out at high temperature in the gas phase. For this purpose, hexamethyldisilazane (HMDS, 8.6% by weight based on the weight of the hydrophilic plate) as hydrophobizing agent was evaporated and a decompression method was carried out according to the method of Example 1 of WO 2013 / 013714 A1. The test specimens were heated in a desiccator to above 100° C. and then evacuated. Gaseous HMDS was then introduced into the desiccator until the pressure rose to 300 mbar. The samples were purged with air and then removed from the desiccator. Sieving / Sorting To obtain the desired fraction, the thermoset granules were fed into a vibrating sieve mill (manufacturer: FREWITT) with a mesh size of 1000 μm, and in order to establish an upper particle limit, particles larger than this limit were removed. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0133] Example 1 The powder according to the present invention was prepared in the same manner as in Comparative Example 5, but the hydrophobic portion was made as follows: The hydrophilic granules (500 g) after the sintering process were placed in a grounded metal bucket and mixed by a propeller mixer at 300-500 rpm, and water (40 g) was sprayed on its surface with continuous stirring at 25 °C, followed by hexamethyldisilazane (HMDS) (60 g). Mixing was continued for 10 min. After that, the bucket was sealed with a lid with several holes of 0.5-1 mm diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The powder granules were then placed in a drying pan and dried in an oven at 145 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0134] Example 2 The powder according to the present invention was prepared in the same manner as in Comparative Example 5, but the hydrophobic portion was made as follows: The hydrophilic granules (500 g) after the sintering process were placed in a grounded metal bucket and mixed by a propeller mixer at 300-500 rpm, and water (40 g) was sprayed on its surface with continuous stirring at 25 °C, followed by hexamethyldisilazane (HMDS) (37.5 g). Mixing was continued for 10 min. After that, the bucket was sealed with a lid with several holes of 0.5-1 mm diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The powder granules were then placed in a drying pan and dried in an oven at 145 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0135] Example 3 The powder according to the present invention was prepared in the same manner as in Comparative Example 5, but the hydrophobic portion was made as follows: The hydrophilic granules (500 g) after the sintering process were placed in a grounded metal bucket and mixed by a propeller mixer at 300-500 rpm, and water (20 g) was sprayed on its surface with continuous stirring at 25 °C, followed by hexamethyldisilazane (HMDS) (40 g). Mixing was continued for 10 min. After that, the bucket was sealed with a lid with several holes of 0.5-1 mm in diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The powder granules were then placed in a drying pan and dried in an oven at 145 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0136] Example 4 The powder according to the present invention was prepared in the same manner as in Comparative Example 5, but the hydrophobic portion was made as follows: The hydrophilic granules (500 g) after the sintering process were placed in a grounded metal bucket and mixed at 300-500 rpm by a propeller mixer. Water (40 g) was sprayed onto its surface with continuous stirring at 25 °C, followed by a mixture of 60 g of hexamethyldisilazane (HMDS) and 10 g of 3-(trimethoxysilyl)propyl methacrylate (MEMO). Mixing was continued for 10 min. After that, the bucket was sealed with a lid with several holes of 0.5-1 mm in diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The powder granules were then placed in a drying pan and dried in an oven at 145 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances. Separation of particle fractions, when required (see Table 3), was performed using a Sweco vibrating screen model LS18S. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0137] Example 5 The powder according to the present invention was prepared in the same manner as in Comparative Example 5, but the hydrophobic portion was made as follows: The hydrophilic granules (500 g) after the sintering process were placed in a grounded metal bucket and mixed at 300-500 rpm by a propeller mixer. Water (40 g) was sprayed onto its surface with continuous stirring at 25 °C, followed by a mixture of 60 g of hexamethyldisilazane (HMDS) and 10 g of 3-(glycidoxypropyl)trimethoxysilane (GLYMO). Mixing was continued for 10 min. After that, the bucket was sealed with a lid with several holes of 0.5-1 mm in diameter for pressure compensation and kept in an oven at 145 °C for 6 h. The powder granules were then placed in a drying pan and dried in an oven at 145 °C under nitrogen atmosphere for 3 h to evaporate the volatile substances. Separation of particle fractions, when required (see Table 3), was performed using a Sweco vibrating screen model LS18S. The physicochemical properties of the silica-based powder thus prepared are shown in Table 2.
[0138] All the powders prepared in Examples 1 to 5 have high porosity, mechanical stability, relatively high bone skeletal density, and relatively high hydrophobicity (high d [Si] , methanol wettability value), and relatively high polarity (d [SiOH] These physicochemical properties make such granules suitable for various applications related to thermal or acoustic insulation, in particular for the preparation of thermal insulation coatings prepared on the basis of aqueous binder systems.
[0139] The granules of Comparative Example 2 were prepared by densifying the hydrophobized silica powder Aerosil R812 (Comparative Example 1) with SiC. The interparticle space in the granules is reduced compared to the powder, so the porosity values (Hg pores > 4 nm) are significantly reduced (5.22 cm for the granules). 3 / g, 13.13 cm for powder 3 The tamping density and skeletal density increased with densification, but the hydrophobicity and polarity remained unchanged (Tables 1-2).
[0140] The granules of Comparative Example 3 were prepared similarly to those of Example 1, with the only difference being that no heat treatment step was applied. The tamping density, skeletal density, and overall mechanical stability of this sample were significantly lower than those of the granules prepared in Example 1 (Tables 1-2).
[0141] The granules of Comparative Example 5 and Comparative Example 6, which were prepared without using water in the hydrophobization step, had significantly lower d SiOH Therefore, these materials are less suitable for incorporation into polar systems such as water-based thermal barrier coatings.
[0142] Preparation of Liquid Insulating Compositions: General Procedure The mixing vessel was charged with the required amount of acrylic binder dispersion (styrene acrylic dispersion Acronal S790, manufacturer: BASF, 50 wt% of total formulation). Water (17 wt% of total formulation) is added followed by stepwise addition of granular material (32 wt% of total formulation) under slow impeller stirring. The mixer speed was increased to maintain a vortex. Ceramic fibers (Lapinus Rockwool) with an average fiber length of 900 μm (approximately 1 wt% of total formulation) were added. All granules were completely dispersed within the dispersion / water medium. Modifiers such as plasticizers, rheology control agents, coalescents, etc. can be added during the mixing process for optimization.
[0143] [Table 1]
[0144] [Table 2]
[0145] Similar to the general procedure using the styrene acrylic dispersion Acronal S790, the granules of the present invention can be incorporated into the following binder types, resulting in corresponding insulating compositions with high granule loadings (up to 25-30% by weight of the total formulation): - Vinnapas 224HD (Wacker, styrene acrylic dispersion copolymerized with vinylsilane); - CE330 Epoxy Binder (two-component, 100% solids epoxy resin, manufactured by Cornerstone Construction Materials, LLC); - 100% solids polyurethane binder; - Water-based stucco mixes in which sand is replaced by granular powder.
[0146] Preparation of solid (dry) insulating compositions Samples of the insulating composition were applied onto a polycarbonate substrate measuring 20 cm x 20 cm x 1 cm, compacted with a spatula to produce a wet film approximately 3-5 cm thick, and air-dried on a laboratory bench for 24-36 hours at 20°C and 50% relative humidity. All insulating compositions thus prepared contained 84.5% by volume of granules in the dry film. This volume ratio was calculated as follows: 100 g of dried insulating composition (MG) 100 (in grams) and the known tamped density of the granules, d G (g / L), the volume V of the granules in 100 g of this composition G100 was calculated. V G100 =M G100 / d G
[0147] The measured volume V of 100 g of dry insulation composition C100 From this, the volume fraction of granules in the dry insulation composition was calculated as follows: r G (Volume%)=V G100 *100% / V C100 After drying, thermal conductivity measurements were performed on all samples. The results of the preparation of liquid and dry insulating compositions are summarized in Table 3.
[0148] Due to the relatively high dynamic viscosity of the composition containing the granules of Comparative Example 5, this composition could not be applied by spraying. Conversely, the thermal insulation composites containing the granules of Examples 1, 3, 4 and 5 could be applied by brushing as well as spraying techniques. In all these cases, dry films with thicknesses of 1 to 2.5 mm could be produced.
[0149] [Table 3]
Claims
1. Silica and at least one IR-opacifier selected from silicon carbide, titanium dioxide, zirconium dioxide, ilmenite, iron titanate, iron oxide, zirconium silicate, manganese oxide, graphite, carbon black, and mixtures thereof; Including, It is a silica-based powder that has been hydrophobized with a surface treatment agent that contains silicon atoms. a) A cumulative pore volume of pores larger than 4 nm, measured by mercury intrusion porosimetry in accordance with DIN ISO 15901-1, of 2.5 cm 3 / g, b) a tamped density of 140 g / L to 290 g / L; c) The number of silanol groups relative to the BET surface area, d, as determined by reaction with lithium aluminum hydride. SiOH is at least 0.5 SiOH / nm 2 and d) the number of silicon atoms in the surface treatment agent relative to the BET surface area, [Si] is at least 1.0 [Si atom] / nm 2 That is, Powder material.
2. 2. The granular material of claim 1, comprising from 30% to 95% by weight of silica selected from fumed silica, precipitated silica, silica aerogel, silica xerogel, and mixtures thereof.
3. 3. The granular material according to claim 1, comprising 1% to 70% by weight of at least one IR-opacifying agent selected from the group consisting of silicon carbide, titanium dioxide, zirconium dioxide, ilmenite, iron titanate, iron oxide, zirconium silicate, manganese oxide, graphite, carbon black, and mixtures thereof.
4. The powder or granule according to any one of claims 1 to 3, wherein the surface treatment agent containing silicon atoms is selected from the group consisting of organosilanes, silazanes, acyclic polysiloxanes, cyclic polysiloxanes, and mixtures thereof.
5. Median particle size d 50 The powder or granule according to any one of claims 1 to 4, wherein the particle size is 10 µm to 5,000 µm.
6. The powder according to any one of claims 1 to 5, wherein at least 5% by weight of the powder has a particle size of less than 200 µm.
7. The powder or granule according to any one of claims 1 to 6, having a carbon content of 0.5% by weight to 10% by weight.
8. The pore volume of pores smaller than 4 μm is 2 cm3, as measured by mercury intrusion porosimetry in accordance with DIN ISO 15901-1. 3 / g to 5 cm 3 The powder or granule according to any one of claims 1 to 7, wherein the powder or granule has a molecular weight of 1 / g.
9. the percentage ratio of the pore volume of pores less than 4 μm to the cumulative pore volume of pores greater than 4 nm is greater than 35%; The powder or granule according to any one of claims 1 to 8, wherein both pore volumes are measured by mercury intrusion porosimetry in accordance with DIN ISO 15901-1.
10. The powder according to any one of claims 1 to 9, having a skeletal density of at least 0.6 g / mL, measured by mercury intrusion porosimetry according to DIN ISO 15901-1 at 417 MPa.
11. ratio d [si] / d SiOH The powder or granule according to any one of claims 1 to 10, wherein is 1 to 10.
12. a) hydrophilic silica; an IR-opacifying agent selected from the group consisting of silicon carbide, titanium dioxide, zirconium dioxide, ilmenite, iron titanate, iron oxide, zirconium silicate, manganese oxide, graphite, carbon black, and mixtures thereof; drying and densifying the powder to produce a hydrophilic granule having a tamped density of at least 80 g / L; b) heat-treating the hydrophilic powder produced in step a) at a temperature of 300° C. to 1,400° C.; c) hydrophobizing the hydrophilic powder or granule that has been heat-treated in step b) in the presence of a surface treatment agent containing silicon atoms and water; The method for producing silica-based powder or granular material according to any one of claims 1 to 11, wherein a molar ratio of the water to the silicon atoms in the surface treatment agent containing silicon atoms is 0.1 to 100.
13. A heat insulating composition comprising the powder or granule according to any one of claims 1 to 11.
14. 14. The insulating composition of claim 13, further comprising a binder selected from the group consisting of (meth)acrylates, alkyd resins, epoxy resins, gum arabic, casein, vegetable oils, polyurethanes, silicone resins, hybrid systems containing silicone-based components and other organic components, waxes, cellulose adhesives, and mixtures thereof.
15. Use of the granules according to any one of claims 1 to 11 for thermal and / or acoustic insulation.
Citation Information
Patent Citations
fumed silica for use as an excipient in pharmaceutical and cosmetic compositions
DE102006039273A1
Process for silylating inorganic oxides
EP0686676A1
Granules on the basis of pyrogenic silica, process for their preparation and use thereof
EP0725037A1
Wettable silylated metal oxides
EP1433749A1
Thermal insulation granulate with reduced hydrophobicity and manufacturing method for same
EP3447038A1