Thermally conductive filler, thermally conductive composite material using same, and manufacturing method thereof

By coating aluminum nitride particles with boron nitride using an yttria aluminate phase, the composite material achieves superior thermal conductivity through reduced interfacial resistance, addressing the limitations of existing materials.

JP7562077B2Active Publication Date: 2024-10-07KK TOYOTA CHUO KENKYUSHO
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020104706
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-17
Publication Date
2024-10-07
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

Existing thermally conductive composite materials using boron nitride and aluminum nitride particles do not achieve sufficient thermal conductivity due to high interfacial thermal resistance and limited adhesion between particles.

Method used

A thermally conductive filler is created by coating at least a portion of the surface of aluminum nitride particles with boron nitride, utilizing an yttria aluminate phase to enhance adhesion and reduce interfacial thermal resistance, achieved by firing a mixture of aluminum nitride and yttrium oxide in an inert gas atmosphere, followed by coating with a boron nitride precursor.

Benefits of technology

The resulting composite material exhibits enhanced thermal conductivity due to increased contact area and reduced interfacial thermal resistance, leading to improved heat transfer properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562077000003
    Figure 0007562077000003
  • Figure 0007562077000004
    Figure 0007562077000004
  • Figure 0007562077000005
    Figure 0007562077000005
Patent Text Reader

Abstract

To provide a heat-conductive filler that can impart high heat conductivity to a matrix.SOLUTION: Provided is a heat-conductive filler that is characterized by containing a yttria aluminate phase-containing aluminum nitride particle, and a boron nitride that is covering at least a part of the surface of the aluminum nitride particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive filler and a thermally conductive composite material using the same, as well as methods for producing the same, and more particularly to a thermally conductive filler containing aluminum nitride and boron nitride, a thermally conductive composite material using the same, as well as methods for producing the same. [Background technology]

[0002] Boron nitride is known as a highly insulating material with high thermal conductivity, and various thermally conductive composite materials have been developed in which boron nitride particles are dispersed in a matrix as a thermally conductive filler. Thermally conductive composite materials have also been developed in which such boron nitride particles are combined with particles of other thermally conductive materials such as aluminum oxide, aluminum nitride, silicon oxide, silicon nitride, silicon carbide, zinc oxide, and graphite.

[0003] For example, JP 2019-43804 A (Patent Document 1) discloses that a thermally conductive filler containing boron nitride particles and aluminum nitride particles is obtained by compressing and sintering a mixture of boron nitride powder and aluminum nitride powder to produce a compressed and sintered body, and pulverizing the compressed and sintered body, the thermally conductive filler containing boron nitride particles and aluminum nitride particles, in which 50% or more of the outer surface of the aluminum nitride particles is contained inside the boron nitride particles and is formed in a state of contact with the boron nitride particles. In addition, Patent Document 1 discloses that by adding a sintering aid to a mixture of boron nitride powder and aluminum nitride powder and sintering it, the sintering aid is present at the bonding interface between the aluminum nitride particles and the boron nitride particles and sintering, so that the adhesion (bonding strength) is increased, and an yttrium compound such as yttrium oxide is described as the sintering aid. However, a composite material containing a thermally conductive filler obtained by compressing, sintering, and pulverizing a mixture of aluminum nitride particles and boron nitride particles has a limited improvement in thermal conductivity and does not necessarily achieve sufficient thermal conductivity. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-43804 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and aims to provide a thermally conductive filler capable of imparting high thermal conductivity to a matrix, a composite material having excellent thermal conductivity, and methods for producing the same. [Means for solving the problem]

[0006] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that by using aluminum nitride particles containing an yttria aluminate phase as the aluminum nitride particles when firing a mixture of aluminum nitride particles and a boron nitride precursor, a thermally conductive filler can be obtained in which at least a portion of the surface of the aluminum nitride particles containing the yttria aluminate phase is coated with boron nitride, and further that the use of this thermally conductive filler can impart high thermal conductivity to the matrix, thereby completing the present invention.

[0007] That is, the thermally conductive filler of the present invention is characterized by containing aluminum nitride particles containing an yttria aluminate phase, and boron nitride coating at least a portion of the surface of the aluminum nitride particles.

[0008] In the thermally conductive filler of the present invention, It is preferred that the boron nitride is a catalytic product of the yttria aluminate phase, and The yttria aluminate phase is at least one of a YAlO3 phase and a Y4Al2O9 phase. too Preferably, moreover The boron nitride is a thermal decomposition product of a melamine borate complex. too preferable.

[0009] The thermally conductive composite material of the present invention is characterized by containing a matrix and the thermally conductive filler of the present invention dispersed in the matrix.

[0010] The method for producing a thermally conductive filler of the present invention is characterized by comprising: a first step of firing a mixture of aluminum nitride powder and yttrium oxide powder in an inert gas atmosphere to obtain aluminum nitride particles containing an yttria aluminate phase; and a second step of firing a mixture of the aluminum nitride particles containing the yttria aluminate phase obtained in the first step and a boron nitride precursor in an inert gas atmosphere to obtain a thermally conductive filler in which at least a portion of the surface of the aluminum nitride particles containing the yttria aluminate phase is coated with boron nitride.

[0011] In the method for producing a thermally conductive filler of the present invention, the boron nitride precursor is preferably a melamine borate complex. In the second step, the mixture of the aluminum nitride particles containing the yttria aluminate phase and the boron nitride precursor is preferably compression molded and then fired.

[0012] The method for producing a thermally conductive composite material of the present invention is a method characterized by comprising the steps of producing a thermally conductive filler by the method for producing a thermally conductive filler of the present invention, and mixing the thermally conductive filler with a matrix to obtain a thermally conductive composite material in which the thermally conductive filler is dispersed in the matrix.

[0013] The reason why the thermally conductive filler of the present invention can produce a thermally conductive filler in which at least a part of the surface of the aluminum nitride particles is coated with boron nitride is not necessarily clear, but the present inventors speculate as follows. That is, in the thermally conductive filler production method of the present invention, first, a mixture of aluminum nitride powder and yttrium oxide powder is fired to form aluminum nitride particles containing an yttria aluminate phase. At this time, yttrium oxide reacts with aluminum nitride to form an yttria aluminate phase, and it is speculated that the yttria aluminate phase is formed on the surface of the aluminum nitride particles because the yttrium oxide particles react with the surface of the aluminum nitride particles. Then, in the thermally conductive filler production method of the present invention, a mixture of aluminum nitride particles with such an yttria aluminate phase formed on the surface and a boron nitride precursor is fired. At this time, a boron nitride intermediate is generated by thermal decomposition of the boron nitride precursor, and this boron nitride intermediate is converted to boron nitride. The conversion of this boron nitride intermediate to boron nitride is promoted by the yttria aluminate phase on the surface of the aluminum nitride particles as a catalyst, so that the boron nitride intermediate spontaneously migrates to the yttria aluminate phase and is then converted to boron nitride. As a result, it is presumed that a thermally conductive filler in which the surfaces of the aluminum nitride particles are coated with boron nitride is obtained.

[0014] On the other hand, when the mixture of aluminum nitride particles without yttria aluminate phase and boron nitride precursor is calcined, the catalytic action of the yttria aluminate phase as described above is not obtained, so it is presumed that the boron nitride intermediate produced by thermal decomposition of the boron nitride precursor is converted to boron nitride without spatially relating to the aluminum nitride particles. As a result, it is presumed that plate-shaped boron nitride particles independent from the aluminum nitride particles are produced, and a mixture of aluminum nitride particles and plate-shaped boron nitride particles is obtained.

[0015] In addition, the reason why a composite material with excellent thermal conductivity can be obtained by using such a thermally conductive filler of the present invention is not necessarily clear, but the present inventors speculate as follows. That is, in a composite material in which a thermally conductive filler is dispersed in a matrix, heat is transferred through the contact site of the filler particles. The thermally conductive filler of the present invention is a composite particle in which at least a part of the surface of an aluminum nitride particle containing an yttria aluminate phase is coated with boron nitride, and such a composite particle with a surface coated with boron nitride has a large contact area between particles, and the interparticle thermal resistance (interface thermal resistance) is small. For this reason, it is speculated that a composite material in which a thermally conductive filler of the present invention is dispersed in a matrix exhibits excellent thermal conductivity.

[0016] On the other hand, since aluminum nitride particles are hard particles, they do not deform when they come into contact with each other, forming point contacts with a small contact area, which results in a large interparticle thermal resistance (interface thermal resistance). In contrast, boron nitride particles are softer than aluminum nitride particles, and have a larger contact area than point contacts, resulting in a small interparticle thermal resistance (interface thermal resistance). However, in a composite material in which a thermally conductive filler consisting of a mixture of aluminum nitride particles and plate-shaped boron nitride particles is dispersed in a matrix, there is contact between aluminum nitride particles with large interparticle thermal resistance (interface thermal resistance) and contact between aluminum nitride particles and boron nitride particles with large interfacial thermal resistance, so the thermal conductivity is not necessarily sufficiently high. Effect of the Invention

[0017] According to the present invention, it is possible to obtain a thermally conductive filler capable of imparting high thermal conductivity to a matrix, and a composite material having excellent thermal conductivity. [Brief description of the drawings]

[0018] [Figure 1] 1 is a graph showing an X-ray diffraction pattern of the yttria-containing AlN particles used in Example 3. [Diagram 2]2 is a graph showing an X-ray diffraction pattern of the AlN particles used in Comparative Example 1. [Diagram 3] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Example 1. [Figure 4] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Example 2. [Diagram 5] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Example 3. [Figure 6] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Comparative Example 1. [Figure 7] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Example 4. [Figure 8] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Example 5. [Figure 9] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Example 6. [Figure 10] 1 is a scanning electron microscope photograph showing the thermally conductive filler obtained in Comparative Example 2. [Figure 11] FIG. 2 is a schematic diagram showing cylindrical composite materials prepared in the examples and comparative examples and samples for measuring thermal conductivity cut out from the composite materials. [Figure 12] Graph showing the above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described in detail below based on preferred embodiments thereof.

[0020] [Thermal conductive filler] First, the thermally conductive filler of the present invention will be described. The thermally conductive filler of the present invention contains aluminum nitride particles containing an yttria aluminate phase, and boron nitride coating at least a portion of the surface of the aluminum nitride particles.

[0021] Compared with hard, highly thermally conductive particles such as diamond particles or alumina particles, the aluminum nitride particles in the thermally conductive filler of the present invention are capable of forming a tightly contacting interface with boron nitride through sintering. Therefore, by coating the particle surfaces with boron nitride, composite particles can be formed that have low interfacial thermal resistance between the aluminum nitride particle surfaces and boron nitride.

[0022] The aluminum nitride particles in the thermally conductive filler of the present invention contain an yttria aluminate phase. Examples of the yttria aluminate phase include the YAlO3 phase and the Y4Al2O9 phase, and either one of these phases may be included, or both may be included. This yttria aluminate phase acts as a catalyst when the boron nitride intermediate produced by the thermal decomposition of the boron nitride precursor is converted to boron nitride, so that the conversion from the boron nitride intermediate to boron nitride occurs preferentially on the surface of the aluminum nitride particles, making it possible to coat the surface of the aluminum nitride particles with boron nitride. On the other hand, aluminum nitride particles that do not contain an yttria aluminate phase cannot obtain such a catalytic action, so that the conversion from the boron nitride intermediate to boron nitride occurs independently of the aluminum nitride particles (i.e., spatially unrelated), resulting in the generation of plate-shaped boron nitride particles, and the surface of the aluminum nitride particles cannot be coated with boron nitride. In addition, in the aluminum nitride particles in the thermally conductive filler of the present invention, from the viewpoint of promoting the conversion of a boron nitride intermediate to boron nitride on the surface of the aluminum nitride particles and coating the surface of the aluminum nitride particles with boron nitride, it is preferable that the yttria aluminate phase is present on the surface of the aluminum nitride particles.

[0023] In the aluminum nitride particles containing such an yttria aluminate phase, the content of yttria is preferably 0.1 to 20 mass%, more preferably 0.1 to 10 mass%, particularly preferably 0.2 to 5 mass%, and most preferably 0.3 to 1 mass%, based on the mass of the aluminum nitride particles. If the content of yttria is less than the lower limit, the amount of boron nitride coating on the surface of the aluminum nitride particles is reduced, and the contact area between the thermally conductive filler particles is not sufficiently increased, so that the thermal resistance (interface thermal resistance) between the thermally conductive filler particles is not sufficiently reduced, and the thermal conductivity of the obtained composite material tends to be not sufficiently improved. On the other hand, if the content of yttria exceeds the upper limit, the amount of boron nitride coating on the surface of the aluminum nitride particles is saturated, and the contact area between the thermally conductive filler particles is also saturated, so that the thermal resistance (interface thermal resistance) between the thermally conductive filler particles is not further reduced, and the effect of improving the thermal conductivity by adding yttria in the obtained composite material tends to be saturated.

[0024] The average particle size of the aluminum nitride particles is not particularly limited, but is preferably 0.2 to 100 μm, more preferably 0.3 to 95 μm, even more preferably 0.5 to 90 μm, particularly preferably 0.5 to 50 μm, and most preferably 1 to 20 μm. If the average particle size of the aluminum nitride particles is less than the lower limit, the number of grain boundaries between the thermally conductive filler particles in the resulting composite material increases, so that the thermal resistance of the entire composite material tends to increase, whereas if it exceeds the upper limit, the dispersion uniformity and filling rate of the thermally conductive filler in the resulting composite material decreases, so that the thermal conductivity tends not to be sufficiently improved.

[0025] In this specification, the term "average particle size" refers to the average particle size of 300 or more particles randomly selected by observation with a scanning electron microscope (SEM) or the like, excluding catalog values ​​related to raw material powders, etc. In addition, when the particles are not spherical (have a circular cross section), the circumscribing circle of the particle (cross section) is assumed, and the diameter of the circumscribing circle is taken as the particle size.

[0026] The boron nitride in the thermally conductive filler of the present invention covers at least a part of the surface of the aluminum nitride particles. Since boron nitride is softer than aluminum nitride, by covering the surface of the aluminum nitride particles with boron nitride, the contact area between the thermally conductive filler particles can be increased, and the interparticle thermal resistance (interface thermal resistance) can be reduced, thereby improving the thermal conductivity of the resulting composite material.

[0027] The boron nitride in the thermally conductive filler of the present invention is preferably a pyrolysis product of a borate melamine complex. By pyrolyzing a borate melamine complex to generate boron nitride on the surface of the aluminum nitride particles, boron nitride can be adhered to the surface of the aluminum nitride particles, the interface thermal resistance between the surface of the aluminum nitride particles and boron nitride is reduced, and the thermal conductivity of the resulting composite material can be improved. On the other hand, when boron nitride particles are attached to the surface of the aluminum nitride particles, the adhesion between the surface of the aluminum nitride particles and the boron nitride particles is not sufficient, the interface thermal resistance between the surface of the aluminum nitride particles and boron nitride is not sufficiently reduced, and the thermal conductivity of the resulting composite material tends not to be sufficiently improved.

[0028] In the thermally conductive filler of the present invention, as long as at least a part of the surface of the aluminum nitride particles is coated with boron nitride, the entire surface of the aluminum nitride particles does not necessarily have to be coated, but it is preferable that 40% or more of the surface of the aluminum nitride particles is coated, more preferably 60% or more, particularly preferably 80% or more, and most preferably the entire surface is coated. If the coverage rate with boron nitride is less than the lower limit, the contact area between the thermally conductive filler particles does not increase sufficiently, so that the thermal resistance (interface thermal resistance) between the thermally conductive filler particles is not sufficiently reduced, and the thermal conductivity of the obtained composite material tends not to be sufficiently improved.

[0029] In the thermally conductive filler of the present invention, the volume ratio of the aluminum nitride particles to boron nitride (aluminum nitride particles: boron nitride) is not particularly limited, but is preferably 30:70 to 98:2, more preferably 40:60 to 90:10, and particularly preferably 50:50 to 85:15. If the volume ratio of the aluminum nitride particles to boron nitride is less than the lower limit, the effect of improving thermal conductivity by the aluminum nitride particles is not sufficiently obtained, and the thermal conductivity of the resulting composite material tends not to be sufficiently improved, while if it exceeds the upper limit, the contact interface with high thermal resistance involving the aluminum nitride particles increases relatively in the resulting composite material, and the thermal conductivity tends not to be sufficiently improved.

[0030] The average particle size of the thermally conductive filler of the present invention is not particularly limited, but is preferably 0.3 to 200 μm, more preferably 0.3 to 95 μm, and particularly preferably 0.5 to 90 μm. If the average particle size of the thermally conductive filler is less than the lower limit, the number of grain boundaries between the thermally conductive filler particles in the obtained composite material increases, so that the thermal resistance of the entire composite material tends to increase, while if it exceeds the upper limit, the dispersion uniformity and filling rate of the thermally conductive filler in the obtained composite material decreases, so that the thermal conductivity tends not to be sufficiently improved.

[0031] In addition, the thermally conductive filler of the present invention is preferably surface-alkylated, which makes it possible to suppress aggregation of the thermally conductive filler when the thermally conductive filler is added to a matrix described below, and improves the fluidity of the composite material, thereby making it possible to obtain a composite material with further reduced thermal resistance and further improved thermal conductivity.

[0032] [Method of producing thermally conductive filler] Next, a method for producing the thermally conductive filler of the present invention will be described. The method for producing the thermally conductive filler of the present invention includes a first step of sintering a mixture of aluminum nitride powder and yttrium oxide powder under an inert gas atmosphere to obtain aluminum nitride particles containing an yttria aluminate phase; A second step of firing the mixture of the aluminum nitride particles containing the yttria aluminate phase obtained in the first step and a boron nitride precursor under an inert gas atmosphere to obtain a thermally conductive filler in which at least a portion of the surface of the aluminum nitride particles containing the yttria aluminate phase is coated with boron nitride. The method includes:

[0033] (First step) In the first step, a mixture of aluminum nitride powder and yttrium oxide powder is prepared. The aluminum nitride powder used here is a raw material powder that becomes aluminum nitride particles in the thermally conductive filler of the present invention, and its average particle size is not particularly limited, but for example, it is preferably 0.2 to 100 μm, more preferably 0.3 to 95 μm, even more preferably 0.5 to 90 μm, particularly preferably 0.5 to 50 μm, and most preferably 1 to 20 μm. The yttrium oxide powder used here is a raw material powder that becomes the yttria aluminate phase in the thermally conductive filler of the present invention, and its average particle size is not particularly limited, but for example, it is preferably 10 nm to 1 μm, more preferably 10 nm to 0.2 μm, even more preferably 10 nm to 0.1 μm, particularly preferably 20 nm to 0.1 μm, and most preferably 20 nm to 50 nm.

[0034] The mixing method for preparing the mixture is not particularly limited, and for example, a wet ball mill grinding and mixing method, a dry ball mill grinding and mixing method, a mechanical mixing method, a stirring and mixing method, a mixing method using a mortar, etc. can be used, and if necessary, treatments such as filtration, washing, drying, and size classification can be performed. There are no particular limitations on such treatments such as filtration, washing, drying, and size classification, and known methods can be appropriately used.

[0035] The mixing ratio of the aluminum nitride powder and the yttrium oxide powder is not particularly limited, but a mixing ratio that allows the content of yttria in the resulting aluminum nitride particles containing an yttria aluminate phase to fall within the above range is preferred.

[0036] Next, the mixture thus obtained is fired under an inert gas atmosphere, whereby the surfaces of the aluminum nitride particles react with the yttrium oxide particles to generate yttria aluminate, thereby obtaining aluminum nitride particles containing an yttria aluminate phase (e.g., YAlO3 phase, Y4Al2O9 phase) (preferably, aluminum nitride particles having the yttria aluminate phase on the surface).

[0037] The inert gas includes nitrogen, rare gas (e.g., argon, helium, neon), etc. The firing temperature is not particularly limited as long as the mixture is sufficiently sintered, but is preferably 1800 to 2200° C., and more preferably 1800 to 2000° C. The firing time is not particularly limited as long as the mixture is sufficiently sintered, but is preferably 0.5 to 6 hours, and more preferably 1 to 4 hours.

[0038] (Second step) In the second step, a mixture of the aluminum nitride particles containing the yttria aluminate phase obtained in the first step and a boron nitride precursor is prepared. The boron nitride precursor used here is a raw material compound that becomes boron nitride in the thermally conductive filler of the present invention. By using the boron nitride precursor, boron nitride can be adhered to the surface of the aluminum nitride particles, and the interface thermal resistance between the surface of the aluminum nitride particles and boron nitride is reduced, so that the thermal conductivity of the resulting composite material can be improved. On the other hand, when boron nitride particles are attached to the surface of the aluminum nitride particles, the adhesion between the surface of the aluminum nitride particles and the boron nitride particles is not sufficient, so the interface thermal resistance between the surface of the aluminum nitride particles and boron nitride is not sufficiently reduced, and the thermal conductivity of the resulting composite material tends not to be sufficiently improved.

[0039] The boron nitride precursor is not particularly limited as long as it produces boron nitride by thermal decomposition, but from the viewpoint of increasing adhesion between the produced boron nitride and the surface of the aluminum nitride particles, a boric acid complex is preferred, and as the boric acid complex, a melamine borate complex or a urea borate complex is preferred, with a melamine borate complex being more preferred.

[0040] The mixing method for preparing the mixture is not particularly limited, and for example, a wet ball mill grinding and mixing method, a dry ball mill grinding and mixing method, a mechanical mixing method, a stirring and mixing method, a mixing method using a mortar, etc. can be used, and if necessary, treatments such as filtration, washing, drying, and size classification can be performed. There are no particular limitations on such treatments such as filtration, washing, drying, and size classification, and known methods can be appropriately used.

[0041] The mixing ratio of the aluminum nitride particles and the boron nitride precursor is not particularly limited, but a mixing ratio in which the volume ratio of the aluminum nitride particles to the boron nitride precursor in the obtained thermally conductive filler falls within the above range is preferable.

[0042] Next, the mixture thus obtained is fired under an inert gas atmosphere. At this time, a boron nitride intermediate is generated by thermal decomposition of the boron nitride precursor, and the boron nitride intermediate is converted to boron nitride. As described above, the yttria aluminate phase contained in the aluminum nitride particles acts as a catalyst when the boron nitride intermediate is converted to boron nitride, and the conversion from the boron nitride intermediate to boron nitride occurs preferentially on the surface of the aluminum nitride particles, so that the thermally conductive filler of the present invention is obtained in which at least a part of the surface of the aluminum nitride particles containing the yttria aluminate phase is coated with boron nitride.

[0043] The inert gas includes nitrogen, rare gas (e.g., argon, helium, neon), etc. The firing temperature is not particularly limited as long as the mixture is sufficiently sintered, but is preferably 1800 to 2200° C., and more preferably 1800 to 2000° C. The firing time is not particularly limited as long as the mixture is sufficiently sintered, but is preferably 0.5 to 6 hours, and more preferably 1 to 4 hours.

[0044] In the second step, it is preferable to compress and mold the mixture of the aluminum nitride particles containing the yttria aluminate phase and the boron nitride precursor, and then sinter the mixture, which allows the boron nitride to be further adhered to the surface of the aluminum nitride particles, and further reduces the interface thermal resistance between the surface of the aluminum nitride particles and the boron nitride, thereby further improving the thermal conductivity of the resulting composite material.

[0045] The pressure during compression molding is preferably 20 MPa or more, more preferably 60 MPa or more, and particularly preferably 80 MPa or more. If the pressure during compression molding is less than the lower limit, the aluminum nitride particles and boron nitride are not sufficiently bonded to each other, so that the interfacial thermal resistance between the surfaces of the aluminum nitride particles and the boron nitride is not sufficiently reduced, and the thermal conductivity of the obtained composite material tends not to be sufficiently improved.

[0046] The method of compression molding the mixture is not particularly limited, but compression molding under hydrostatic pressure is preferred. This allows pressure to be applied uniformly to the mixture, and a compression molded body in an effective tightly adhered state can be obtained. In addition, compression molding under hydrostatic pressure can suppress the thermal conductivity anisotropy of the thermal conductive filler due to the orientation of boron nitride. Such thermal conductivity anisotropy of the thermal conductive filler causes thermal conductivity anisotropy due to molding history, which is not preferred in some cases.

[0047] In this way, when the mixture is compressed and molded and then sintered, the obtained compressed sintered body is pulverized. At this time, the boron nitride of the compressed sintered body is selectively broken, so that a thermally conductive filler in which at least a part of the surface of the aluminum nitride particles is coated with boron nitride is obtained. There is no particular limitation on the method for pulverizing the compressed sintered body, and for example, a pulverization method using various pulverizers (mills) or mortars, a pulverization method using a wet ball mill or a dry ball mill, etc. can be adopted.

[0048] Furthermore, in the method for producing a thermally conductive filler of the present invention, it is preferable to react the thermally conductive filler with a silazane coupling agent or a titanate coupling agent, whereby the BN particles in the thermally conductive filler react with the silazane coupling agent or the titanate coupling agent to alkylate the surface of the thermally conductive filler, and when the thermally conductive filler is added to a matrix described below, the aggregation of the thermally conductive filler can be suppressed, and the flowability of the composite material is improved, making it possible to obtain a composite material with further reduced thermal resistance and further excellent thermal conductivity.

[0049] Of the silazane-based coupling agents and the titanate-based coupling agents, the silazane-based coupling agents are preferred from the viewpoints that they can sufficiently suppress aggregation of the thermally conductive filler, improve the fluidity of the composite material, and do not cause an increase in the contact thermal resistance between the thermally conductive fillers due to the presence of a gel, thereby further reducing the thermal resistance of the obtained composite material and increasing its thermal conductivity.

[0050] Examples of a method for reacting the thermally conductive filler with a silazane-based coupling agent or a titanate-based coupling agent include a method in which the thermally conductive filler is dispersed in an organic solvent such as toluene, a silazane-based coupling agent or a titanate-based coupling agent is added to the obtained dispersion, and then the mixture is heated.

[0051] The mixing ratio of the thermally conductive filler and the silazane-based coupling agent or the titanate-based coupling agent is preferably 1 to 20 parts by mass, and more preferably 5 to 10 parts by mass, of the silazane-based coupling agent or the titanate-based coupling agent per 100 parts by mass of the thermally conductive filler.

[0052] The reaction temperature is preferably from room temperature to 100° C., more preferably from 40 to 60° C. The reaction time is preferably from 0.5 to 20 hours, more preferably from 1 to 5 hours.

[0053] [Thermal Conductive Composite Materials] Next, the thermally conductive composite material of the present invention will be described. The thermally conductive composite material of the present invention contains a matrix and the thermally conductive filler of the present invention dispersed in the matrix.

[0054] In the thermally conductive composite material of the present invention, the matrix is ​​preferably an insulating resin or an insulating oil. For example, the resin may be a thermosetting resin such as an epoxy resin, a phenolic resin, or a silicone resin, or a thermoplastic resin such as polystyrene, polymethyl methacrylate, polycarbonate, polyolefin (e.g., polyethylene, polypropylene), polyolefin elastomer, polyethylene terephthalate, nylon, ABS resin, polyamide, polyimide, polyamideimide, ethylene-propylene-diene rubber (EPDM), butyl rubber, natural rubber, polyisoprene, or polyetherimide. In addition, the oil may be a silicone oil, a modified silicone oil, a fluoroether oil, a mineral oil, an animal or vegetable natural oil, paraffin, or a synthetic oil, and preferably a silicone oil, a modified silicone oil, a paraffin, or a synthetic oil having a boiling point of 200° C. or higher. These resins or oils may be used alone or in combination of two or more.

[0055] In the thermally conductive composite material of the present invention, the surface of the thermally conductive filler is preferably alkylated, which can suppress aggregation of the thermally conductive filler in the matrix and improve the flowability of the composite material, thereby further reducing the thermal resistance of the composite material and further improving the thermal conductivity.

[0056] In the thermally conductive composite material of the present invention, the content of the thermally conductive filler is not particularly limited, but is preferably 10 to 90 vol%, more preferably 15 to 70 vol%, and particularly preferably 20 to 60 vol% based on the total amount of the thermally conductive composite material. If the content of the thermally conductive filler is less than the lower limit, the network structure of the thermally conductive path in which heat is diffused through the contact parts between the thermally conductive fillers in the composite material is not sufficiently formed, and the thermal conductivity of the obtained composite material tends not to be sufficiently improved, while if the content of the thermally conductive filler exceeds the upper limit, the obtained composite material tends to become brittle, making it difficult to obtain a self-supporting composite material.

[0057] [Method of producing thermally conductive composite material] Next, a method for producing a thermally conductive composite material of the present invention will be described. The method for producing a thermally conductive composite material of the present invention includes a step of producing a thermally conductive filler by the method for producing a thermally conductive filler of the present invention, and a step of mixing the thermally conductive filler with the matrix to obtain a thermally conductive composite material in which the thermally conductive filler is dispersed in the matrix.

[0058] When the thermally conductive filler and the matrix are mixed, the mixing ratio of the thermally conductive filler and the matrix is ​​determined so that the content of the thermally conductive filler in the resulting composite material is a desired content. The method for mixing the thermally conductive filler and the matrix is ​​not particularly limited, and a known mixing method is appropriately used.

[0059] When the resin is used as such a matrix, the thermally conductive filler and the resin are mixed to form a homogeneous mixture, and the mixture is molded to obtain the thermally conductive composite material. When the thermally conductive filler and the resin are mixed to form a homogeneous mixture, a dispersion medium may be further added to form a homogeneous slurry. In this case, it is preferable to remove the dispersion medium by a known method such as vacuum drying before molding. Such a dispersion medium is not particularly limited, and examples thereof include N-methyl-2-pyrrolidone, chloroform, dichloromethane, carbon tetrachloride, acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, pentyl acetate, isopentyl acetate, amyl acetate, tetrahydrofuran, dimethylformaldehyde, dimethylacetamide, dimethylsulfoxide, acetonitrile, methanol, ethanol, propanol, isopropanol, butanol, hexanol, octanol, hexafluoropropane, hexafluoropropane, hexafluoroisopropyl ether ... Examples of organic solvents include isopropanol, ethylene glycol, propylene glycol, tetramethylene glycol, tetraethylene glycol, hexamethylene glycol, diethylene glycol, benzene, toluene, xylene, chlorobenzene, dichlorobenzene, trichlorobenzene, chlorophenol, phenol, tetrahydrofuran, sulfolane, 1,3-dimethyl-2-imidazolidinone, γ-butyrolactone, N-dimethylpyrrolidone, pentane, hexane, neopentane, cyclohexane, heptane, octane, isooctane, nonane, decane, and diethyl ether.

[0060] When the mixture is molded, it is preferable to compress it by applying pressure. The compression method is not particularly limited, and may be uniaxial compression or biaxial compression. It may also be isotropically compressed by hydrostatic pressure. The compression pressure is also not particularly limited, but is preferably 5 to 20 MPa. If the compression pressure is less than the lower limit, voids tend to remain in the obtained composite material, while if it exceeds the upper limit, the destruction and deformation of the filler in the obtained composite material becomes significant, and residual strain tends to occur.

[0061] The method for solidifying the resin when molding the mixture is not particularly limited, and any known method can be used, for example, a cooling method such as standing to cool when a thermoplastic resin is used as the resin, or an appropriate hardening method when various (heat, light, water) curable resins are used. In addition, such solidification may be performed either during or after molding.

[0062] When the oil is used as the matrix, the thermally conductive composite material (i.e., the grease composition) can be obtained by mixing the thermally conductive filler with the oil to form a uniform slurry. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The synthesis method of the melamine borate complex used in the examples and comparative examples is shown below.

[0064] (Synthesis Example 1) 24g of boric acid was added to 800ml of water heated to 95℃, and dissolved by stirring. Then, 16g of melamine was added and dissolved by stirring. Heating and stirring were continued for 10 minutes to react boric acid and melamine, and the resulting reaction liquid was cooled with water and left at room temperature for 12 hours. The precipitated crystals were then collected by filtration and vacuum dried at 40℃ to obtain 31.5g of boric acid melamine complex.

[0065] Example 1 <Preparation of yttria-containing AlN particles> First, 40 g of aluminum nitride (AlN) powder (Tokuyama Corporation, "High Purity Aluminum Nitride Powder / Granules E Grade", average particle size 1 μm) and 0.2 g of yttrium oxide (Y2O3) nanoparticles (Aldrich, average particle size 50 nm) were added to a polyethylene pot, and 500 g of zirconia balls (3 mm diameter) and 165 g of acetone were added and mixed for 1 hour at 400 rpm using a ball mill. The zirconia balls were then removed by filtration, and the acetone was completely removed by evaporation and vacuum drying. The resulting mixture was sintered at 1800 °C for 1 hour in a nitrogen atmosphere. The resulting sintered body was cooled to room temperature, milled for 60 seconds, and passed through a sieve with 150 μm openings to obtain yttria-containing AlN particles (yttria content: 0.5 mass%).

[0066] <Preparation of thermally conductive filler> Next, 11.4 g of the yttria-containing AlN particles (yttria content: 0.5 mass%) and 9.9 g of the borate melamine complex obtained in Synthesis Example 1 were put into a polyethylene pot so that the composition ratio of the resulting compressed sintered body was aluminum nitride (AlN) / boron nitride (BN) = 80 vol% / 20 vol%, and further, 500 g of zirconia balls (3 mm diameter) and 165 g of acetone were put and mixed for 12 hours under the condition of 400 rpm by a ball mill. Thereafter, the zirconia balls were removed by filtration, and further, the acetone was completely removed by evaporation and vacuum drying. The obtained mixture was compressed under a hydrostatic pressure of 294 MPa, heated at 900 ° C for 1 hour in a nitrogen atmosphere, and further sintered at 1800 ° C for 1 hour to obtain a compressed sintered body. This compressed sintered body was cooled to room temperature, then milled for 60 seconds and passed through a sieve with 53 μm openings to obtain a thermally conductive filler in which the surfaces of the yttria-containing AlN particles were coated with boron nitride.

[0067] <Preparation of composite material> Next, the thermally conductive filler and one-liquid thermosetting epoxy resin ("EP160" manufactured by Cemedine Co., Ltd.) were mixed so that the volume fraction of the filler was 60%, and dichloromethane was added to prepare a slurry. The obtained slurry was stirred in the air to evaporate dichloromethane, and further, the dichloromethane was completely removed by vacuum drying for 15 minutes. The epoxy resin composition thus obtained was quickly filled into a cylindrical container (inner diameter 14 mm) preheated at 110°C for 30 minutes so that the thickness after molding was within the range of 30 to 40 mm, and then compressed in the longitudinal direction of the cylindrical container with a plunger at a pressure within the range of 5 to 10 MPa, and the epoxy resin was cured by heating at 110°C for 30 minutes while maintaining this compressed state with a clamp, to obtain a cylindrical composite material in which the thermally conductive filler was dispersed in the epoxy resin cured product.

[0068] Example 2 Yttria-containing AlN particles (yttria content: 1 mass%) and a thermally conductive filler in which the surfaces of the yttria-containing AlN particles are coated with boron nitride were prepared in the same manner as in Example 1, except that the amount of Y2O3 nanoparticles was changed to 0.4 g. Furthermore, a cylindrical composite material in which this thermally conductive filler was dispersed in a cured epoxy resin was produced.

[0069] Example 3 Yttria-containing AlN particles (yttria content: 3 mass%) and a thermally conductive filler in which the surfaces of the yttria-containing AlN particles are coated with boron nitride were prepared in the same manner as in Example 1, except that the amount of Y2O3 nanoparticles was changed to 1.2 g. Furthermore, a cylindrical composite material in which this thermally conductive filler was dispersed in a cured epoxy resin was produced.

[0070] Example 4 Yttria-containing AlN particles (yttria content: 0.5 mass%) and a thermally conductive filler in which the surfaces of the yttria-containing AlN particles are coated with boron nitride were prepared, and further a cylindrical composite material in which this thermally conductive filler is dispersed in a cured epoxy resin was produced. Example 1 was repeated, except that 40 g of AlN powder (Thrutek's AlN05AF) having an average particle size of 5 μm was used instead of the AlN powder (Tokuyama Corporation's High Purity Aluminum Nitride Powder / Granules Grade E).

[0071] Example 5 Yttria-containing AlN particles (yttria content: 1 mass%) and a thermally conductive filler in which the surfaces of the yttria-containing AlN particles are coated with boron nitride were prepared in the same manner as in Example 4, except that the amount of Y2O3 nanoparticles was changed to 0.4 g. Furthermore, a cylindrical composite material in which this thermally conductive filler was dispersed in a cured epoxy resin was produced.

[0072] Example 6 Yttria-containing AlN particles (yttria content: 3 mass%) and a thermally conductive filler in which the surfaces of the yttria-containing AlN particles are coated with boron nitride were prepared in the same manner as in Example 4, except that the amount of Y2O3 nanoparticles was changed to 1.2 g. Furthermore, a cylindrical composite material in which this thermally conductive filler was dispersed in a cured epoxy resin was produced.

[0073] Comparative Example 1 The same procedure as in Example 1 was repeated, except that 11.4 g of AlN particles (Tokuyama Corporation's "High Purity Aluminum Nitride Powder / Granules E Grade", average particle size 1 μm) was used instead of the yttria-containing AlN particles. Thermally conductive filler Furthermore, a cylindrical composite material was fabricated in which this thermally conductive filler was dispersed in a cured epoxy resin.

[0074] Comparative Example 2 The same procedure as in Example 4 was repeated, except that 11.4 g of AlN particles ("AlN05AF" manufactured by Thrutek, average particle size: 5 μm) was used instead of the yttria-containing AlN particles. Thermally conductive filler Furthermore, a cylindrical composite material was fabricated in which this thermally conductive filler was dispersed in a cured epoxy resin.

[0075] Comparative Example 3 <Preparation of thermally conductive filler> First, 9.9 g of the borate melamine complex obtained in Synthesis Example 1, 11.4 g of aluminum nitride (AlN) powder (Tokuyama Corp. "High Purity Aluminum Nitride Powder / Granules E Grade", average particle size 1 μm), and 0.23 g (2 mass % based on the AlN powder) of yttrium oxide (Y2O3) nanoparticles (Aldrich Corp., average particle size 50 nm) as a sintering aid were added to a polyethylene pot, and 500 g of zirconia balls (3 mm diameter) and 165 g of acetone were added and mixed for 12 hours at 400 rpm using a ball mill. Thereafter, the zirconia balls were removed by filtration, and the acetone was completely removed by evaporation and vacuum drying. The resulting mixture was compressed under a hydrostatic pressure of 294 MPa, and then sintered at 1800 °C for 1 hour in a nitrogen atmosphere to obtain a compressed sintered body. The compressed sintered body was cooled to room temperature, milled for 60 seconds, and sieved through a sieve with a mesh size of 53 μm. Thermally conductive filler obtained.

[0076] <Preparation of composite material> Next, a cylindrical composite material in which the thermally conductive filler was dispersed in a cured epoxy resin was produced in the same manner as in Example 1, except that the thermally conductive filler was used.

[0077] [X-ray diffraction measurement] The X-ray diffraction patterns of the yttria-containing AlN particles used in the examples and the AlN particles used in the comparative examples were measured to confirm the crystalline phases present in the yttria-containing AlN particles and the AlN particles. The results are shown in Table 1. As an example of the X-ray diffraction pattern, FIG. 1 shows the X-ray diffraction pattern of the yttria-containing AlN particles used in Example 3, and FIG. 2 shows the X-ray diffraction pattern of the AlN particles used in Comparative Example 1. As shown in Table 1 and FIG. 1, it was found that the yttria-containing AlN particles used in Examples 1 to 6 contain an yttria aluminate phase (YAlO3 phase, Y4Al2O9 crystal phase) in addition to the AlN crystal phase. It is considered that this yttria aluminate phase was formed by the reaction between Y2O3 and the AlN particle surface. On the other hand, as shown in Table 1 and FIG. 2, it was confirmed that the crystal phase present in the AlN particles used in Comparative Examples 1 and 2 was only the AlN crystal phase.

[0078] <Electron microscope observation of thermally conductive filler> The thermally conductive fillers obtained in the examples and comparative examples were observed using a scanning electron microscope ("NB-5000" manufactured by Hitachi High-Technologies Corporation). FIGS. 3 to 5 show scanning electron microscope photographs of the thermally conductive fillers obtained in Examples 1 to 3, respectively. FIG. 6 shows a scanning electron microscope photograph of the thermally conductive filler obtained in Comparative Example 1. FIGS. 7 to 9 show scanning electron microscope photographs of the thermally conductive fillers obtained in Examples 4 to 6, respectively. FIG. 10 shows a scanning electron microscope photograph of the thermally conductive filler obtained in Comparative Example 2. The bright areas in FIGS. 3 to 10 are AlN, and the bright gray areas are BN. As shown in FIGS. 3 to 5 and 7 to 9, it was found that the thermally conductive fillers obtained in Examples 1 to 6 were AN / BN composite particles in which at least a part of the surface of the yttria-containing AlN particles was coated with BN. From this result, it was found that when yttria is contained in the AlN particles, by mixing with a BN precursor and firing, BN accumulates on the surface of the yttria AlN particles, forming composite particles with a core-shell structure. On the other hand, as shown in Figures 6 and 10, it was found that the thermally conductive fillers obtained in Comparative Examples 1 and 2 are mixed particles of AlN particles and plate-like BN particles. From this result, it was found that when the AlN particles do not contain yttria, by mixing with a BN precursor and firing, plate-like BN crystals are formed in places other than the AlN particle surfaces.

[0079] <Thermal conductivity of composite materials> As shown in Fig. 11, a sample 2 for measuring thermal conductivity (z-axis direction thickness: 3 mm, diameter: 14 mmφ) was cut out from the cylindrical composite material 1 obtained in the examples and comparative examples, and the surface of the obtained sample was blackened with black spray. The thickness direction (z-axis direction) of this sample was set as the heat flow direction, and the thermal diffusivity in the direction parallel to the compression direction (z-axis direction) was measured using a xenon flash analyzer (NETZSCH "LFA 447 NanoFlash").

[0080] The specific heat of the sample was measured by the DSC method using a thermal oscillation type differential scanning calorimeter (manufactured by TA Instruments). Furthermore, the density of the sample was determined by the water substitution method (Archimedes method). From these results, the following formula was calculated: Thermal conductivity (W / (m K)) = specific heat (J / (kg K)) × density (kg / m 3 ) × thermal diffusivity (m 2 / sec) The thermal conductivity in the direction parallel to the compression direction (z-axis direction) was calculated by the above method. The results are shown in Tables 1 and 2 and in FIG.

[0081] [Table 1]

[0082] As shown in Figure 12, it was found that the thermal conductivity of a composite material containing a thermally conductive filler including AlN particles and BN increases as the yttria content in the AlN particles increases, and that the thermal conductivity saturates when the yttria content in the AlN particles becomes approximately 1 mass%.

[0083] [Table 2]

[0084] From the results of Examples 2 and 3 shown in Table 2, it is considered that the thermal conductivity of a composite material in which a thermally conductive filler in which yttria-containing AlN particles with an yttria content of 2 mass% and the surfaces of which are coated with boron nitride are dispersed in a cured epoxy resin is in the range of 5.6 to 5.9 W / mK. On the other hand, when 2 mass% yttria was added to the AlN particles as a sintering aid when sintering a mixture of the AlN particles and boron nitride (Comparative Example 3), Obtained thermally conductive filler The thermal conductivity of the composite material in which yttria was dispersed in the cured epoxy resin was 4.45 W / mk. These results show that in a composite material containing a thermally conductive filler in which the surfaces of AlN particles are coated with boron nitride, sintering AlN particles containing yttria with boron nitride improves thermal conductivity compared to when yttria is added to a mixture of AlN particles and boron nitride and then sintered. [Industrial Applicability]

[0085] As described above, according to the present invention, it is possible to obtain a thermally conductive filler capable of imparting high thermal conductivity to a matrix, and a composite material containing the same. Therefore, the composite material of the present invention has excellent thermal conductivity and is useful, for example, as a heat dissipation material or heater material for automobiles, electronic elements, and various electric products, a grease composition, etc. [Explanation of symbols]

[0086] 1: Composite material 2: Sample for thermal conductivity measurement

Claims

1. A thermally conductive filler comprising aluminum nitride particles containing an yttria aluminate phase and boron nitride coating at least a portion of the surface of the aluminum nitride particles.

2. The thermally conductive filler as described in claim 1, characterized in that the boron nitride is a product of catalytic action of the yttria aluminate phase.

3. The yttria aluminate phase is YAlO 3 Phase and Y 4 A 2 O 9 3. The thermally conductive filler according to claim 1, which is at least one of the phases.

4. 4. The thermally conductive filler according to claim 1, wherein the boron nitride is a thermal decomposition product of a boric acid melamine complex.

5. A thermally conductive composite material comprising a matrix and the thermally conductive filler according to any one of claims 1 to 4 dispersed in the matrix.

6. a first step of firing a mixture of aluminum nitride powder and yttrium oxide powder under an inert gas atmosphere to obtain aluminum nitride particles containing an yttria aluminate phase; and a second step of firing a mixture of the aluminum nitride particles containing the yttria aluminate phase obtained in the first step and a boron nitride precursor under an inert gas atmosphere to obtain a thermally conductive filler in which at least a portion of the surface of the aluminum nitride particles containing the yttria aluminate phase is coated with boron nitride. A method for producing a thermally conductive filler, comprising:

7. 7. The method for producing a thermally conductive filler according to claim 6, wherein the boron nitride precursor is a melamine borate complex.

8. The method for producing a thermally conductive filler according to claim 6 or 7, characterized in that in the second step, a mixture of aluminum nitride particles containing the yttria aluminate phase and a boron nitride precursor is compression molded and then sintered.

9. A step of producing a thermally conductive filler by the method according to any one of claims 6 to 8; mixing the thermally conductive filler with a matrix to obtain a thermally conductive composite material in which the thermally conductive filler is dispersed in the matrix; A method for producing a thermally conductive composite material, comprising:

Citation Information

Patent Citations

  • Production of boron nitride

    JP1986191505A

  • BN-aln-based compound sintered compact and its production

    JP1992292467A

  • Method for producing ain / BN composite powder and method for producing ain / BN composite sintered material

    JP2005029421A

  • Aluminum nitride-based powder and method for producing the same

    JP2019019045A

  • Heat-conductive filler, heat-conductive composite material, and method for producing the heat-conductive filler

    JP2019043804A