Manufacturing method of hard coat film

The die coating method with a designed die lip and controlled pressure stabilizes the coating process, addressing unevenness and defects to produce high-quality hard coat films.

JP7562119B2Active Publication Date: 2024-10-07NIPPON PAPER IND CO LTD

Patent Information

Application Number
JP2020009425
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-23
Publication Date
2024-10-07
Estimated Expiration
2040-01-23

AI Technical Summary

Technical Problem

Conventional die-coating methods and devices suffer from coating unevenness and defects, necessitating improvements in coating stability and uniformity for high-quality hard coat films used in optical members.

Method used

A die coating method with a specifically designed die lip shape and reduced pressure on the upstream side of the die lip, along with controlled viscosity, surface tension, and clearance, to stabilize the coating process and achieve uniform application.

Benefits of technology

The method reduces coating unevenness and defects, enabling the production of high-quality hard coat films with uniform properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562119000006
    Figure 0007562119000006
  • Figure 0007562119000007
    Figure 0007562119000007
  • Figure 0007562119000008
    Figure 0007562119000008
Patent Text Reader

Abstract

To provide a coating method of coating slip by a die coat method capable of obtaining stably uniform coatability by reducing generation of irregular coating or a defect.SOLUTION: Coating slip is coated on a substrate to be coated by using a die having a manifold and a slit land part for discharging uniformly in a width direction, in which a coating slip discharge port is a die lip. In this case, the die has such a shape that the ratio between a lip thickness of the die lip and a length of the land part satisfies following formula. Further, the upstream side of the die lip in a flow direction of the substrate to be coated is decompressed from atmospheric pressure: [formula] (lip thickness of die lip / length of land part)×100≤1.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for applying a coating liquid, and more particularly to a method for applying a coating liquid that is suitable for producing a hard coat film used for an optical member. [Background technology]

[0002] For example, the display surface of panel displays such as electroluminescence (EL) displays, liquid crystal displays (LCD), and plasma displays is required to be scratch-resistant so that the display surface is not scratched during handling and the visibility is not reduced. For this reason, a hard coat film having a hard coat layer provided on a substrate film is generally used to impart scratch resistance to the display surface of the display. In recent years, with the widespread use of touch panels that allow users to input data and instructions by touching the display screen with a finger or a pen while viewing the display, the functional requirements for hard coat films used in such optical components have further increased.

[0003] Conventionally, in order to apply a coating liquid for forming the hard coat layer onto a substrate film, known coating methods such as reverse coating, gravure coating, bar coating, die coating, spray coating, kiss coating, wire bar coating, and curtain coating have been used.

[0004] For example, the die coating method has the advantage that defects caused by contact of the bar with the substrate in the bar coating method can be reduced because coating is performed with the coating liquid discharge port of the die not in contact with the substrate. For example, the following Patent Documents 1 to 3 all disclose coating devices and coating methods for the die coating method. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 2917116 [Patent Document 2] Patent No. 4573550 [Patent Document 3] Patent No. 5085046 Summary of the Invention [Problem to be solved by the invention]

[0006] However, according to the investigations of the present inventors, the coating apparatus and coating method of the conventional die coating method as disclosed in the above Patent Documents 1 to 3 have shown improvements in terms of reducing coating defects, etc., but there is still room for further improvement in terms of coating stability, etc.

[0007] In order to solve the problems of the related art, the first object of the present invention is to provide a method for applying a coating liquid by a die coating method that reduces the occurrence of coating unevenness and defects and stably obtains uniform coating properties, and the second object of the present invention is to provide a method for producing a hard coat film that can obtain a high-quality hard coat film by applying the above-mentioned method for applying a coating liquid. [Means for solving the problem]

[0008] The inventors conducted extensive research to solve the above problems and found that in order to reduce the occurrence of coating unevenness and defects and to consistently obtain uniform coating properties in a die coating method, it is preferable to design the die lip of the die to be used to have a predetermined shape and, further, to reduce the pressure upstream of the die lip in the flow direction of the substrate to be coated below atmospheric pressure. The present invention was completed as a result of investigations based on various findings obtained. That is, the present invention has the following configuration.

[0009] (First invention) This is a method for applying a coating liquid to a substrate to be coated using a die having a manifold and a slit-shaped land portion for uniformly discharging the coating liquid in the width direction, and having a coating liquid discharge outlet in the form of a die lip, wherein the die has a shape such that the ratio of the lip thickness of the die lip to the length of the land portion satisfies the following formula, and the pressure upstream of the die lip in the flow direction of the substrate to be coated is reduced below atmospheric pressure. [formula] (Die lip thickness / land length) x 100≦1

[0010] (Second Invention) The method for applying a coating fluid according to the first aspect of the present invention is characterized in that the pressure on the upstream side of the die lip in the flow direction of the substrate to be coated is reduced by 0.05 kPa to 1.00 kPa below atmospheric pressure.

[0011] (Third Invention) The method for applying a coating fluid according to the first or second aspect of the present invention is characterized in that the viscosity of the coating fluid is 100 mPa·s or less. (Fourth Invention) The method for applying a coating fluid according to any one of the first to third aspects of the present invention is characterized in that the surface tension of the coating fluid is 50 mN / m or less.

[0012] (Fifth Invention) The method for applying a coating fluid according to any one of the first to fourth aspects of the present invention is characterized in that the die lip has a lip thickness of 0.5 mm or less.

[0013] (Sixth Invention) The method for applying a coating fluid according to any one of the first to fifth aspects of the present invention is characterized in that a clearance between the substrate to be coated and the die lip is 50 μm to 500 μm.

[0014] (Seventh Invention) The method for producing a hard coat film is characterized in that the coating liquid is a paint for forming a hard coat layer, and a coating method for the coating liquid described in any one of the first to sixth inventions is applied to coat the coating liquid on the substrate to form a hard coat layer. (8th invention) A seventh aspect of the present invention provides a method for producing a hard coat film, wherein the substrate to be coated is a film substrate. Effect of the Invention

[0015] According to the present invention, it is possible to provide a method for applying a coating liquid by a die coating method, which reduces the occurrence of coating unevenness and defects and stably obtains uniform coating properties. Furthermore, according to the present invention, it is possible to provide a method for producing a hard coat film, which is capable of obtaining a high quality hard coat film by applying the above-mentioned coating liquid. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic diagram showing a method for applying a coating liquid according to the present invention. [Diagram 2] FIG. 2 is a longitudinal sectional view showing the structure of a die used in the present invention. [Diagram 3] FIG. 2 is an enlarged view of the die lip of the die. [Figure 4] FIG. 2 is a schematic diagram for explaining a coating method of a coating liquid according to the present invention. [Diagram 5] 1A is a schematic diagram showing a state when the vacuum pressure is at a lower limit, and FIG. 1B is a schematic diagram showing a state when the vacuum pressure is at an upper limit. [Figure 6] FIG. 2 is a schematic cross-sectional view of a hard coat film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail. In the present invention, unless otherwise specified, the expression "XX to △△" means "not less than XX and not more than △△."

[0018] The method for applying the coating liquid according to the present invention will be described below. The coating method of the present invention is a die coating method in which a die equipped with a slit-shaped coating liquid flow path is used to form a so-called coating bead on the surface of the substrate to be coated, and the coating liquid is uniformly applied to the surface of the substrate to be coated.

[0019] FIG. 1 is a schematic diagram showing a method for applying a coating fluid according to the present invention. A coating fluid 60 stored in the fluid tank 10 is supplied to the die 30 while being metered at a predetermined amount by, for example, a precision metering pump 20. Then, the coating fluid 60 discharged from a coating fluid discharge port at the tip of the die 30 is applied, with a coating bead formed, to the surface of a substrate 70 to be coated that is being conveyed on a back roll 40, for example, from the direction of arrow A to the direction of arrow B in the figure.

[0020] When such a coating method of the coating liquid is applied to the production of a hard coat film having a hard coat layer on a film substrate, the coating liquid 60 is a paint containing a binder resin for forming a hard coat layer, and the substrate 70 to be coated is a film substrate. The details of the production of the hard coat film will be described later.

[0021] Fig. 2 is a vertical cross-sectional view showing the structure of a die used in the present invention, and Fig. 3 is an enlarged view of a die lip of the die shown in Fig. 2. Also, Fig. 4 is a schematic diagram for explaining a method for applying a coating fluid according to the present invention.

[0022] As shown in FIG. 2, the die 30 is integrally configured with at least an upstream die body 34a located on the upstream side in the flow direction of the substrate 70 to be coated and a downstream die body 34b located on the downstream side. The die 30 also has a manifold 31 and a slit-shaped land portion 32 for uniformly discharging the coating liquid in the width direction of the coating surface. The manifold 31 is a groove for uniformly spreading and conveying the coating liquid in the width direction. The cross-sectional shape is approximately trapezoidal in the embodiment shown in FIG. 2, but is not limited thereto and may be formed, for example, in a semicircular shape. The land portion 32 is a slit-shaped flow path for the purpose of rectifying the flow of the coating liquid from the manifold 31 to the coating liquid discharge port, and is formed with a predetermined width in the width direction of the die 3.

[0023] The coating liquid discharge port at the tip of the die 30 is a die lip 33 having an upstream lip 33a and a downstream lip 33b, and the gap between the upstream lip 33a and the downstream lip 33b forms the land portion 32. The gap between the upstream lip 33a and the downstream lip 33b, i.e., the slit width (S) of the land portion 32 (see FIG. 3), is a constant predetermined width regulated by the thickness of a shim plate 35 interposed between the upstream die body 34a and the downstream die body 34b.

[0024] As shown in FIG. 4, the tip of the die 30 is positioned at a certain distance (hereinafter referred to as "clearance (H)") from (non-contact with) the surface of the substrate 70 to be coated, and the coating fluid 60 ejected from the die lip 33, which is the coating fluid ejection outlet at the tip of the die 30, is applied to the surface of the substrate 70 to be coated, which is transported in the direction of arrow B in the figure, with a coating bead formed, at a film thickness t (wet film thickness).

[0025] The coating theory of the coating method according to the present invention will now be described with reference to FIG. In the coating method according to the present invention, coating is possible when the "capillary coefficient" expressed by μU / σ is smaller than the critical capillary number expressed by the following formula.

[0026]

number

[0027] Here, μ is the viscosity of the coating liquid, σ is the surface tension of the coating liquid, and U is the coating speed. As mentioned above, t is the coating thickness, and H is the clearance.

[0028] That is, the conditions under which coating can be performed by the coating method of the present invention are those under which the following formula is satisfied.

[0029]

number

[0030] From the above formula for coatable conditions, we can see that coating is easier when the left side of the formula, i.e. the capillary coefficient, is small, or the right side of the formula, i.e. the critical capillary number, is large. Therefore, in theory, coating is easy when, for example, the viscosity of the coating fluid is small, the surface tension of the coating fluid is large, the coating speed is small (slow), and the clearance is small (narrow).

[0031] As explained above, according to the study by the present inventors, although improvements were made in the coating apparatus and coating method using the conventional die coating method with respect to reducing coating defects, etc., there was room for further improvement in terms of coating stability, etc. As a result of intensive study to solve the above-mentioned conventional problems, the present inventors have found that in order to reduce the occurrence of coating unevenness and defects and to stably obtain uniform coating properties in a coating method using the die coating method, it is preferable to design the die lip of the die to have a predetermined shape and further reduce the pressure on the upstream side of the die lip in the flow direction of the substrate to be coated below atmospheric pressure.

[0032] That is, this is a method for applying a coating liquid to a substrate to be coated using a die 30 having a manifold 31 and a slit-shaped land portion 32 for uniformly discharging the above-mentioned coating liquid in the width direction, and a coating liquid discharge outlet of which is a die lip 33, and it is important that the die 30 has a shape such that the ratio of the lip thickness of the die lip 33 to the length of the land portion 32 satisfies the following formula: [formula] (Die lip thickness / land length) x 100≦1

[0033] Here, the lip thickness of the die lip refers to the vertical length L of the tip end surface of the upstream lip 33a (or the downstream lip 33b) as shown in Figs. Moreover, the length of the land portion refers to the length R from the tip (liquid discharge port) of the land portion 32 to the manifold 31, as shown in FIG.

[0034] The die 30 used in the coating method of the present invention has a shape in which the ratio of the lip thickness L of the die lip 33 to the length R of the land portion 32 satisfies the above formula, thereby reducing the occurrence of coating unevenness, particularly horizontal step-like unevenness at a constant pitch, and defects (scratches, etc.), resulting in a good coating appearance. Moreover, coating can be performed with a uniform film thickness in the width direction of the substrate to be coated, and uniform coating properties can be stably obtained.

[0035] On the other hand, if the ratio of the lip thickness L of the die lip 33 to the length R of the land portion 32 does not satisfy the above formula, that is, if (lip thickness of the die lip / length of the land portion) × 100 > 1, coating unevenness such as horizontal step unevenness is likely to occur, and a coating appearance with a good quality cannot be obtained.

[0036] In the present invention, it is necessary that the ratio of the lip thickness L of the die lip 33 to the length R of the land portion 32 satisfies the above formula, and in this case, the lip thickness L is not particularly limited, but is preferably 0.5 mm or less. If the lip thickness L is thicker than 0.5 mm, the above coating unevenness is likely to occur.

[0037] The length R of the land portion 32 is not particularly limited, but if the length R of the land portion 32 is too long, the flow of the coating liquid in the land portion becomes laminar, which tends to cause coating unevenness. On the other hand, if the length R of the land portion 32 is too short, the internal pressure in the die 30 is not uniform in the width direction, which affects the uniformity of the film thickness in the width direction. Therefore, the length R of the land portion 32 is preferably 50 mm or less, and more preferably 30 mm or more.

[0038] As described above, the slit width (S) of the land portion 32 (see Figs. 3 and 4) can be adjusted by the thickness of the shim plate 35 interposed between the upstream die body 34a and the downstream die body 34b, but if the slit width S of the land portion 32 is particularly wide, it may affect the uniformity of the film thickness in the width direction and the coating appearance. Therefore, in the present invention, the slit width S of the land portion 32 is preferably in the range of, for example, 50 µm to 130 µm.

[0039] In the present invention, in order to stably obtain uniform coating properties, the viscosity of the coating fluid used is preferably, for example, 100 mPa s or less. If the viscosity of the coating fluid used is higher than 100 mPa s, the internal pressure in the die 30 becomes too high, making it impossible to obtain a uniform discharge amount in the width direction.

[0040] In the present invention, the viscosity is particularly preferably 30 mPa·s or less. If the viscosity of the coating liquid is too low, coating unevenness becomes noticeable, and therefore in the present invention, the viscosity of the coating liquid used is preferably, for example, 3 mPa·s or more.

[0041] The viscosity of the coating liquid can be adjusted, for example, by adjusting the solid content concentration, the molecular weight of the resin, etc. In the present invention, the viscosity of the coating liquid refers to a value measured by a B-type viscometer (rotational viscometer).

[0042] In the present invention, the surface tension of the coating liquid is not particularly limited, but from the viewpoint of obtaining stable and uniform coating properties, it is preferably, for example, 50 mN / m or less, and more preferably in the range of 20 mN / m to 25 mN / m.

[0043] The surface tension of the coating liquid can be adjusted, for example, by adding a leveling agent, a solvent, etc. In the present invention, the surface tension of the coating liquid refers to a value measured by the plate method (Wilhelmy method).

[0044] In the present invention, the concentration (solid content concentration) of the coating liquid is not particularly limited, but may be, for example, in the range of about 30% by weight to 70% by weight. For example, in terms of coating stability (clearance expansion), the range is preferably 40% by weight to 50% by weight, and particularly preferably 40% by weight to 45% by weight. If the concentration of the coating liquid is higher than 50% by weight, it is difficult to expand the clearance because the wet film thickness (the above-mentioned film thickness t) is reduced in order to match the film thickness after drying to a predetermined film thickness. If the concentration of the coating liquid is lower than 40% by weight, the wet film thickness increases, making it easier to expand the clearance, but the viscosity of the coating liquid decreases, resulting in noticeable coating unevenness.

[0045] In the present invention, the coating speed is not particularly limited, but as the coating speed decreases, the capillary coefficient decreases, and the above-mentioned clearance can be increased. However, in consideration of productivity, the appropriate coating speed is about 5 to 50 m / min.

[0046] Furthermore, in the coating method of the present invention, the coating fluid 60 discharged from the die lip 33 of the die 30 is applied to the surface of the substrate 70 to be coated with a bead formed between the tip of the die lip 33 and the substrate coating surface, and therefore, in order to obtain uniform coating properties, it is desirable to stabilise this bead.

[0047] In the present invention, in order to stabilize this bead, it is a preferred embodiment to reduce the pressure on the upstream side of the die lip in the flow direction of the substrate to be coated.

[0048] 1, a vacuum chamber 50 is provided to reduce the pressure on the upstream side of the die lip 33 in the flow direction of the substrate 70 to be coated. This reduces the pressure below the bead formed between the tip of the die lip 33 and the coating surface of the substrate.

[0049] In the present invention, from the viewpoint of stabilizing the bead, it is preferable to reduce the pressure on the upstream side of the die lip 33 in the flow direction of the substrate 70 to, for example, a pressure in the range of 0.05 kPa to 1.00 kPa lower than atmospheric pressure. Note that if the reduced pressure (vacuum pressure) is insufficient or if the reduced pressure (vacuum pressure) is excessive, problems such as those described below may occur.

[0050] FIG. 5A is a schematic diagram showing a state when the vacuum pressure is at the lower limit, and FIG. 5B is a schematic diagram showing a state when the vacuum pressure is at the upper limit.

[0051] As shown in Fig. 5(A), when the vacuum pressure Pvac is at the lower limit, the vacuum pressure Pvac is insufficient, causing problems such as bead breakage and air bubbles 36 forming inside the bead. On the other hand, when the vacuum pressure Pvac is excessive and at the upper limit, as shown in Fig. 5(B), the coating liquid forming the bead leaks to the vacuum side, resulting in a problem of insufficient coating amount.

[0052] ΔP expressed by the following formula B is the lower limit of the vacuum pressure Pvac.

[0053]

number

[0054] In addition, ΔP expressed by the following formula Lis the upper limit of the vacuum pressure Pvac.

[0055]

number

[0056] In the above formulas, P 0 is atmospheric pressure. The other symbols μ, σ, U, t, H, and L are all the same as above.

[0057] As mentioned above, the difference between the upper and lower limits of the vacuum pressure Pvac is 6μUL / H. 2 The larger this value is, the greater the vacuum pressure that can be applied. Therefore, it is easier to apply vacuum pressure when, for example, the viscosity of the coating fluid is high, the coating speed is high (fast), the lip thickness of the die lip is thick, and the clearance is small (narrow).

[0058] From the above, for example, the narrower the clearance H, the greater the vacuum pressure Pvac that can be applied, and there is a correlation (negative correlation) between the clearance H and the vacuum pressure Pvac.

[0059] In the present invention, as described above, from the viewpoint of stabilizing the bead, it is preferable to adjust the vacuum pressure, for example, in the range of 0.05 kPa to 1.00 kPa, and particularly preferably in the range of 0.05 kPa to 0.6 kPa. In the present invention, when the pressure on the upstream side of the die lip 33 is reduced by, for example, 0.05 kPa to 1.00 kPa below atmospheric pressure, the clearance H (see FIG. 4) between the substrate 70 to be coated and the die lip 33 is preferably in the range of, for example, 50 μm to 500 μm. By reducing the pressure in this manner, there is also an effect of increasing the clearance (improving coating stability).

[0060] As described above, according to the method for applying a coating fluid of the present invention, the occurrence of coating unevenness and defects can be reduced, and uniform coatability can be stably obtained.

[0061] [Method of manufacturing hard coat film] Next, a method for producing the hard coat film will be described. The method for producing a hard coat film of the present invention uses a coating material for forming a hard coat layer as the coating liquid, and applies the coating liquid on a substrate to be coated by the above-mentioned coating method of the present invention to form a hard coat layer, thereby producing a hard coat film.

[0062] As the substrate to be coated with this hard coat film, a film substrate is usually used.

[0063] According to the method for producing a hard coat film of the present invention, a high quality hard coat film can be obtained by applying the above-mentioned coating liquid according to the present invention.

[0064] Fig. 6 is a schematic cross-sectional view of a hard coat film, which shows a typical example of the hard coat film, and has a hard coat layer 2 on at least one surface of a film substrate 1.

[0065] (Film substrate) First, the film substrate 1 will be described. The film substrate 1 used in the present invention is not particularly limited, and examples thereof include triacetyl cellulose, polyethylene terephthalate, cycloolefin polymer, polycarbonate, polyethylene naphthalate, polyethylene, polytrimethylene terephthalate, polypropylene, polybutylene terephthalate, polybutylene naphthalate, polystyrene, polymethyl methacrylate, polystyrene glycidyl methacrylate, aromatic polyimide, alicyclic polyimide, polyamideimide, and mixtures thereof, but from the viewpoints of heat resistance, availability, and economy, it is preferable to use a thermoplastic resin film made of polyethylene terephthalate, polyethylene naphthalate, or triacetyl cellulose as a constituent material. In particular, a polyethylene terephthalate film is preferable because it is highly transparent, inexpensive, and easily available.

[0066] (Hard coat layer) Next, the hard coat layer 2 will be described. The resin contained in the hard coat layer 2 can be any resin capable of forming a coating, without any particular limitation. In particular, it is preferable to use an ionizing radiation curable resin, since it can impart surface hardness (pencil hardness, scratch resistance) to the hard coat layer, and it is possible to adjust the degree of crosslinking by the amount of exposure to ultraviolet light, thereby enabling adjustment of the surface hardness of the hard coat layer.

[0067] The ionizing radiation curable resin used in the present invention is not particularly limited as long as it is a transparent resin that is cured by irradiation with ultraviolet light (hereinafter abbreviated as "UV") or an electron beam (hereinafter abbreviated as "EB"), but in order to provide coating hardness and form a three-dimensional crosslinked structure in the hard coat layer, it is preferable to use a polyfunctional acrylate that is curable by UV or EB and has three or more (meth)acryloyloxy groups in one molecule. Specific examples of UV- or EB-curable polyfunctional acrylates having three or more (meth)acryloyloxy groups in the molecule include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane ethoxy triacrylate, glycerin propoxy triacrylate, ditrimethylolpropane tetraacrylate, etc. The polyfunctional acrylates may be used alone or in combination of two or more.

[0068] Furthermore, the ionizing radiation curable resin used in the present invention is preferably a polymer having a weight average molecular weight in the range of, for example, 700 to 3600, more preferably 700 to 3000, and even more preferably 700 to 2400. If the weight average molecular weight is less than 700, the curing shrinkage when cured by UV or EB irradiation is large, and the phenomenon (curl) in which the hard coat film warps toward the hard coat layer side becomes large, causing problems in the subsequent processing steps and poor processing suitability. Also, if the weight average molecular weight exceeds 3600, the flexibility of the hard coat layer increases, but the hardness is insufficient, making it unsuitable.

[0069] Furthermore, when the ionizing radiation curable resin used in the present invention has a weight average molecular weight of less than 1500, the number of functional groups in one molecule is desirably 3 or more and less than 10. When the weight average molecular weight of the ionizing radiation curable resin is 1500 or more, the number of functional groups in one molecule is desirably 3 or more and less than 20. Within the above ranges, curling can be suppressed while suppressing the occurrence of cracks under heat-resistant conditions (storage at 100°C for 5 minutes), and appropriate processability can be maintained.

[0070] In addition to the above-mentioned ionizing radiation curable resin, the resin contained in the hard coat layer 2 may include thermoplastic resins such as polyethylene, polypropylene, polystyrene, polycarbonate, polyester, acrylic, styrene-acrylic, and cellulose, and thermosetting resins such as phenol resin, urea resin, unsaturated polyester, epoxy, and silicone resin, within a range that does not impair the hardness and scratch resistance of the hard coat layer.

[0071] It is also possible to further improve the surface hardness (scratch resistance) by incorporating inorganic oxide fine particles in the hard coat layer 2. In this case, the average particle diameter of the inorganic oxide fine particles is preferably in the range of 5 to 50 nm, more preferably in the range of 10 to 20 nm. If the average particle diameter is less than 5 nm, it is difficult to obtain sufficient surface hardness. On the other hand, if the average particle diameter exceeds 50 nm, the gloss and transparency of the hard coat layer are likely to decrease, and the flexibility may also decrease.

[0072] In the present invention, examples of the inorganic oxide fine particles include alumina, silica, etc. Among these, alumina, which is mainly composed of aluminum, is particularly suitable because it has high hardness and can be effective with a smaller amount than silica.

[0073] A known photopolymerization initiator may be contained in the hard coat coating material for forming the hard coat layer 2. As such a photopolymerization initiator, acetophenones and benzophenones may be used.

[0074] A leveling agent can be used for the hard coat layer 2 to improve the coating property, and known leveling agents such as fluorine-based, acrylic, siloxane-based, and their adducts or mixtures can be used. In addition, in touch panel applications, etc., when adhesion using an optically transparent adhesive OCR is required for the purpose of adhesion to the cover glass (CG), transparent conductive member (TSP), liquid crystal module (LCM), etc. of a touch panel terminal, it is preferable to use an acrylic leveling agent or a fluorine-based leveling agent with high surface free energy (approximately 40 mN / m or more).

[0075] Other additives that may be added to the hard coat layer 2, such as an ultraviolet absorber, an antifoaming agent, a surface tension adjusting agent, an antifouling agent, an antioxidant, an antistatic agent, and a light stabilizer, may be blended as required.

[0076] The hard coat layer 2 can be formed by coating the film substrate 1 with a coating material prepared by dissolving and dispersing the above-mentioned ionizing radiation curable resin, as well as a photopolymerization initiator and other additives in a suitable solvent, and then irradiating the coating material with ionizing radiation such as UV or EB to cause photopolymerization, thereby obtaining a hard coat layer 2 having excellent hardness.

[0077] The solvent can be appropriately selected depending on the solubility of the resin to be blended, and may be any solvent capable of uniformly dissolving or dispersing at least the solid contents (resin, photopolymerization initiator, other additives, etc.). Examples of such solvents include known organic solvents such as aromatic solvents such as toluene, xylene, and n-heptane, aliphatic solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane, ester solvents such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, and methyl lactate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, and alcohol solvents such as methanol, ethanol, isopropyl alcohol, and n-propyl alcohol, which may be used alone or in combination.

[0078] The amount of ionizing radiation (UV, EB, etc.) irradiated after application of the coating material for forming the hard coat layer may be any amount necessary to impart sufficient hardness to the hard coat layer 2, and can be appropriately set depending on the type of ionizing radiation curable resin, etc.

[0079] The above-mentioned method for applying the coating liquid according to the present invention can be preferably applied as a method for applying the hard coat paint to form the hard coat layer 2. By applying the method for applying the coating liquid according to the present invention, the occurrence of coating unevenness and defects can be reduced, and uniform coating properties can be stably obtained.

[0080] The coating thickness of the hard coat layer 2 is not particularly limited, but is preferably in the range of 1.0 μm to 5.0 μm, and more preferably in the range of 1.5 μm to 3.5 μm. If the coating thickness is less than 1.0 μm, the necessary scratch resistance and pencil hardness are reduced, which is not preferable. If the coating thickness exceeds 5.0 μm, curling is likely to occur, which is not preferable, as the handling properties during the manufacturing process are reduced.

[0081] As described above in detail, the present invention can provide a method for applying a coating liquid by a die coating method that reduces the occurrence of coating unevenness and defects and can stably obtain uniform coatability. Furthermore, according to the present invention, a high-quality hard coat film can be obtained by applying the coating material for forming a hard coat layer onto the film substrate 1 by applying the coating method of the coating liquid according to the present invention described above to form a hard coat layer 2. EXAMPLES

[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples, the production of a hard coat film by applying the coating method of the present invention to the coating liquid will be described, but the coating method of the present invention is not limited to the production of a hard coat film.

[0083] Example 1 [Preparation of paint for forming hard coat layer] Toluene / ethyl cellosolve = 70 / 30 parts by weight, 100 parts by weight of an electron beam curable resin (trade name: EBECRYL1290, manufactured by Daicel-Allnex Co., Ltd., weight average molecular weight 2000) mainly composed of urethane acrylate having six (meth)acryloyl groups, 2 parts by weight of a photopolymerization initiator (trade name: Omunirad-184, manufactured by BASF Japan Co., Ltd.), and 0.3 parts by weight of a leveling agent (trade name: Futergent 650A, manufactured by Neos Co., Ltd.) were mixed to prepare a paint for forming a hard coat layer with a solid concentration of 40% by weight (hereinafter referred to as "hard coat paint"). The viscosity and surface tension of this hard coat paint were measured by the above-mentioned measuring method, and the values ​​are shown in Table 1 below.

[0084] [Preparation of hard coat film] Using the above-mentioned coating method of the coating liquid of the present invention, the above-mentioned hard coat paint was applied to one side of a polyethylene terephthalate (PET) film (product name: Cosmoshine A4300, manufactured by Toyobo Co., Ltd.) having a thickness of 125 μm and a width of 1500 mm, so that the film thickness after drying would be 10 μm. The coating speed was 25 m / min. During coating, a vacuum pressure of 0.3 kPa was applied to the upstream side of the die lip to reduce the pressure.

[0085] The die (material: SUS) used in this example has a lip thickness of 0.1 mm, a land length (hereinafter referred to as "land length") of 30 mm, and a shape that satisfies the condition (lip thickness of die lip / land length) × 100 ≦ 1. In addition, the slit width S of this die was adjusted to 130 μm using a SUS shim plate. In this example, the clearance between the coating substrate (the above PET film) and the die lip and the coating amount are as shown in Table 1 below.

[0086] Next, the coating layer was dried at 80°C for 1 minute to evaporate the solvent, and then the integrated light dose was 250 mJ / cm 2 The coating was cured by ultraviolet irradiation treatment to obtain a hard coat film having a hard coat layer.

[0087] Example 2 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Example 1, except that a vacuum pressure of 0.05 kPa was applied to the upstream side of the die lip during application of the hard coat coating material.

[0088] Example 3 The hard coat paint was applied in the same manner as in Example 1, except that a die having a die lip thickness of 0.4 mm and a land length of 50 mm was used, to produce a hard coat film.

[0089] Example 4 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Example 1, except that the solid content concentration of the hard coat coating material in Example 1 was adjusted to 70% by weight and the coating viscosity was adjusted to 98 mPa s.

[0090] Example 5 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Example 1, except that the solid content concentration of the hard coat coating material in Example 1 was adjusted to 50% by weight and the coating viscosity was adjusted to 12.4 mPa s.

[0091] Example 6 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Example 1, except that the solid content concentration of the hard coat coating material in Example 1 was adjusted to 50% by weight, the coating viscosity was adjusted to 12.4 mPa s, and a vacuum pressure of 0.6 kPa was applied to the upstream side of the die lip to reduce the pressure when the hard coat coating material was applied.

[0092] Example 7 A hard coat paint with a solids concentration of 40% by weight was prepared by stirring and mixing 32.0 parts by weight of radiation curable resin dipentaerythritol hexaacrylate (trade name: NK Ester A-9550, manufactured by Shin-Nakamura Chemical Co., Ltd.), 28.0 parts by weight of crosslinked acrylic monodisperse particles (trade name: MX-500, manufactured by Soken Chemical & Engineering Co., Ltd., particle size 5 μm), 1.5 parts by weight of photopolymerization agent 1-hydroxy-cyclohexyl-phenyl-ketone (trade name: Irgacure 184, manufactured by BASF), 0.5 parts by weight of leveling fluorine-based compound (trade name: Megafac RS-75, manufactured by DIC Corporation), 23 parts by weight of ketone-based solvent methyl ethyl ketone, and 15 parts by weight of propylene glycol monomethyl ether. The above hard coat coating material was used, and a hard coat film was produced by coating the hard coat coating material in the same manner as in Example 1, except that a vacuum pressure of 0.2 kPa was applied to the upstream side of the die lip during coating.

[0093] Example 8 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Example 7, except that a vacuum pressure of 0.05 kPa was applied to the upstream side of the die lip to reduce the pressure when applying the hard coat coating material.

[0094] Example 9 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Example 7, except that a vacuum pressure of 1.0 kPa was applied to the upstream side of the die lip to reduce the pressure when applying the hard coat coating material.

[0095] Comparative Example 1 A hard coat coating material was applied to produce a hard coat film in the same manner as in Example 1, except that a die having a lip thickness of 1 mm and a land length of 50 mm, and a die shape not satisfying the condition (die lip lip thickness / land length)×100≦1, was used. However, in this comparative example, pressure reduction was not performed (vacuum pressure was zero), and coating was performed under atmospheric pressure.

[0096] Comparative Example 2 The hard coat coating material was applied to prepare a hard coat film in the same manner as in Comparative Example 1, except that a vacuum pressure of 0.6 kPa was applied to the upstream side of the die lip to reduce the pressure when applying the hard coat coating material.

[0097] <Evaluation> The hard coat films of the Examples and Comparative Examples prepared as described above were evaluated for the following items, and the results are summarized in Table 1. The die shape, coating conditions, etc. in each Example and Comparative Example are also summarized in Table 1.

[0098] <Coating layer thickness uniformity> The total thickness of the PET substrate and coating layer was measured at 9 points within a 420 mm width of the coating surface using a linear gauge, and the average value and standard deviation of the 9 points were calculated. The uniformity of the coating layer thickness was evaluated based on the standard deviation value.

[0099] <Coating appearance> The coated surface was visually observed for the presence or absence of horizontal step-like unevenness, and the coating appearance was evaluated according to the following criteria. ◯: No horizontal unevenness is observed at all. Δ: A small amount of horizontal step unevenness is observed, but it is at a level that does not cause any practical problems. ×: Horizontal step-like unevenness with a pitch of 5 to 10 mm is clearly observed.

[0100] [Table 1]

[0101] From the results in Table 1, it can be seen that the examples based on the coating conditions of the coating fluid of the present invention reduce the occurrence of coating unevenness and the like, and provide a stable coating with good coating appearance and uniform coating properties. In addition, reducing the pressure upstream of the die lip during coating provides a better coating appearance and also has the effect of expanding the clearance. Therefore, the present invention is suitable for producing hard coat films for optical applications, for which high quality has been particularly demanded in recent years. On the other hand, in the case of the comparative examples which do not satisfy the coating conditions of the coating liquid of the present invention, coating unevenness occurs and good coating appearance cannot be obtained. [Explanation of symbols]

[0102] 1 Film substrate 2 Hard coat layer 10 Liquid tank 20 Precision metering pump 30 Die 31 Manifold 32 Land Department 33 Die Lip 33a Upstream lip 33b Downstream lip 34a Upstream die body 34b downstream die body 35 Shim plate 40 Back Roll 50 Vacuum Chamber 60 Coating Fluid 70 Substrate to be coated

Claims

1. A method for producing a hard coat film, comprising the steps of: applying a coating liquid onto a substrate to be coated using a die having a manifold and slit-shaped land portions for uniformly discharging a coating liquid in a width direction, the die having a coating liquid discharge port being a die lip; and applying the coating liquid to the substrate to be coated, the method comprising the steps of: The coating liquid is a coating material for forming a hard coat layer, which contains a polyfunctional acrylate, The surface tension of the coating liquid is 50 mN / m or less, The substrate to be coated is a film substrate, The die has a lip thickness of 0.5 mm or less, and the land portion has a length of 30 mm or more and 50 mm or less, and reducing the pressure on the upstream side of the die lip in the flow direction of the substrate to be coated by 0.05 kPa to 1.00 kPa below atmospheric pressure.

2. 2. The method for producing a hard coat film according to claim 1, wherein the viscosity of the coating liquid is 100 mPa·s or less.

3. 3. The method for producing a hard coat film according to claim 1, wherein the clearance between the substrate to be coated and the die lip is 50 μm to 500 μm.

Citation Information

Patent Citations

  • JP1975085046A

  • Coating method

    JP2003236451A

  • Method for forming thin film and thin film

    JP2014226620A

  • Hard coat film and method for producing the same

    JP2019127010A

  • Coating method of coating liquid and production method of hard coat film

    JP2021109152A

Cited By

  • Coating apparatus, coating method, and printing system

    JP2026166222A