Dihexylbenzene dicarboxylate plasticizer composition and resin composition containing the same

A dihexylbenzenedicarboxylate plasticizer derived from hexyl alcohol isomers enhances PVC resin compositions by improving plasticization efficiency and migration resistance, addressing environmental concerns and cost issues.

JP7562213B2Active Publication Date: 2024-10-07LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023518012
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-24
Filing Date
2021-11-23
Publication Date
2024-10-07
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing plasticizers, such as di(2-ethylhexyl) terephthalate (DEHTP), suffer from low plasticization efficiency, poor migration resistance, and environmental concerns, leading to unpredictable physical property changes and high costs when used in PVC resin compositions.

Method used

A plasticizer composition containing dihexylbenzenedicarboxylate derived from a mixture of hexyl alcohol isomers, including 1-hexanol, 2-methylpentanol, and other branched alcohols, is developed to enhance plasticization efficiency while maintaining balance between tensile strength, elongation, and migration resistance.

Benefits of technology

The composition significantly improves plasticization efficiency, mechanical properties, and migration resistance, addressing environmental issues and reducing product costs, while maintaining excellent physical property balance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562213000001
    Figure 0007562213000001
  • Figure 0007562213000002
    Figure 0007562213000002
  • Figure 0007562213000003
    Figure 0007562213000003
Patent Text Reader

Abstract

The present invention is characterized in that dihexylbenzene dicarboxylate has an alkyl group derived from a mixture of hexyl alcohol isomers, and when this is applied to a resin, stress resistance and mechanical properties can be maintained at equivalent or higher levels, and plasticization efficiency can be significantly improved while maintaining a balance between tensile strength, elongation, and migration resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0158964, filed on November 24, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a plasticizer composition containing dihexylbenzene dicarboxylate derived from a mixed alcohol of isomers of hexyl alcohol, and a resin composition containing the same. [Background technology]

[0003] Plasticizers are usually made by reacting alcohol with polycarboxylic acids such as phthalic acid and adipic acid to form the corresponding esters. In addition, in consideration of domestic and international regulations on phthalate-based plasticizers, which are harmful to the human body, research is ongoing into plasticizer compositions that can be used to replace phthalate-based plasticizers, such as terephthalate-based, adipate-based, and other polymer-based plasticizers.

[0004] Meanwhile, the need for such environmentally friendly products is increasing in the plastisol industry, such as flooring, wallpaper, soft and hard sheets, the calendaring industry, and the extrusion / injection compounding industry. In order to enhance the quality characteristics, processability, and productivity of each finished product, it is necessary to use appropriate plasticizers taking into consideration discoloration, migration, mechanical properties, etc.

[0005] In these various areas of use, PVC resin is blended with secondary materials such as plasticizers, fillers, stabilizers, viscosity reducers, dispersants, defoamers, and foaming agents depending on the characteristics required by each industry, such as tensile strength, elongation, light resistance, migration, gelling properties, and absorption speed.

[0006] For example, when di(2-ethylhexyl) terephthalate (DEHTP), which is relatively inexpensive and most widely used among plasticizer compositions applicable to PVC, is applied, the hardness or sol viscosity is high, the absorption rate of the plasticizer is relatively slow, and the migration and stress migration properties are also poor.

[0007] One possible solution to this problem is to use the product of a transesterification reaction with butanol as a plasticizer in a composition containing DEHTP. However, although this improves the plasticization efficiency, it also leads to a deterioration in the loss on heating and thermal stability, and some decrease in mechanical properties, so improvements in physical properties are required. Therefore, there is currently no solution other than to supplement this by mixing it with another secondary plasticizer.

[0008] However, when using secondary plasticizers, it is difficult to predict the change in physical properties, which may lead to increased product costs, and there are drawbacks such as the occurrence of unpredictable problems, such as the improvement of physical properties being unclear except in specific cases and causing compatibility problems with resins.

[0009] In addition, when a trimellitate-based product such as tri(2-ethylhexyl) trimellitate or triisononyl trimellitate is used to improve the poor migration, weight loss and light resistance of the DEHTP product, the migration and weight loss properties are improved, but the plasticization efficiency is deteriorated and a considerable amount must be added to give the resin an appropriate plasticization effect. Therefore, the product is relatively expensive and cannot be commercially used.

[0010] In addition, when a substance such as dibutyl terephthalate is mixed into a terephthalate-based product, there is a problem that the use of the substance beyond a certain amount is restricted, since it causes environmental problems such as air pollution during processing due to deterioration in weight loss caused by heating, and thus the plasticization efficiency cannot be improved.

[0011] Therefore, there is a demand for development of products that solve the environmental problems of existing phthalate-based products or products that improve the poor physical properties of environmentally friendly products to improve the environmental problems of phthalate-based products. Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention aims to provide a plasticizer composition characterized by having, as dihexylbenzene dicarboxylate, an alkyl group derived from a mixture of hexyl alcohol isomers, and thereby to provide a plasticizer composition which, when applied to a resin, can significantly improve plasticization efficiency while maintaining a balance between tensile strength, elongation, and migration resistance. [Means for solving the problem]

[0013] In order to solve the above problems, the present invention provides a plasticizer composition.

[0014] (1) The present invention provides a plasticizer composition comprising one or more dihexylbenzene dicarboxylates, the dihexylbenzene dicarboxylate being one or more selected from dihexyl isophthalate and dihexyl terephthalate, the hexyl group of the dihexylbenzene dicarboxylate being derived from an isomeric mixture of hexyl alcohol, and the isomeric mixture of hexyl alcohol comprising two or more selected from the group consisting of 1-hexanol, 1-methylpentanol, 2-methylpentanol, 3-methylpentanol, 4-methylpentanol, 1,1-dimethylbutanol, 1,2-dimethylbutanol, 1,3-dimethylbutanol, 2,2-dimethylbutanol, 2,3-dimethylbutanol, 3,3-dimethylbutanol, 1-ethylbutanol, 2-ethylbutanol, 3-ethylbutanol, and cyclopentylmethanol.

[0015] (2) The present invention provides a plasticizer composition according to the above (1), wherein the mixture of hexyl alcohol isomers contains 1-hexanol and 2-methylpentanol.

[0016] (3) The present invention provides the plasticizer composition according to (1) or (2) above, wherein the isomer mixture of hexyl alcohol contains 30 parts by weight or more of a branched alcohol per 100 parts by weight of the isomer mixture.

[0017] (4) The present invention provides a plasticizer composition according to any one of the above items (1) to (3), wherein the isomer mixture of hexyl alcohol contains 40 to 95 parts by weight of a branched alcohol per 100 parts by weight of the isomer mixture.

[0018] (5) The present invention provides a plasticizer composition according to any one of the above items (1) to (4), wherein the isomer mixture of hexyl alcohol contains 40 parts by weight or less of 1-hexanol per 100 parts by weight of the isomer mixture.

[0019] (6) The present invention provides the plasticizer composition according to any one of the above (1) to (5), wherein the dihexylbenzene dicarboxylate is dihexyl isophthalate.

[0020] (7) The present invention provides the plasticizer composition according to any one of the above (1) to (6), wherein the dihexylbenzene dicarboxylate is dihexyl terephthalate.

[0021] (8) The present invention provides the plasticizer composition according to any one of the above (1) to (7), wherein the dihexylbenzene dicarboxylate is a mixture of dihexyl isophthalate and dihexyl terephthalate.

[0022] (9) The present invention provides a plasticizer composition according to any one of the above items (1) to (8), wherein the mixture of hexyl alcohol isomers contains 1-hexanol, 2-methylpentanol, and 3-methylpentanol.

[0023] (10) The present invention provides a resin composition comprising 100 parts by weight of a resin and 5 to 150 parts by weight of the plasticizer composition according to any one of (1) to (9) above.

[0024] (11) The present invention provides a resin composition according to (10) above, wherein the resin is at least one selected from the group consisting of straight vinyl chloride polymer, paste vinyl chloride polymer, ethylene-vinyl acetate copolymer, ethylene polymer, propylene polymer, polyketone, polystyrene, polyurethane, polylactic acid, natural rubber, and synthetic rubber. Effect of the Invention

[0025] When used in a resin composition, the plasticizer composition according to one embodiment of the present invention can significantly improve the plasticization efficiency while maintaining a balance between tensile strength, elongation, and migration resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0027] Definition of Terms The term "composition" as used herein includes mixtures of materials which comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0028] The term "straight vinyl chloride polymer" as used herein means one type of vinyl chloride polymer, which may be polymerized by suspension polymerization, bulk polymerization, or the like, and which has the form of porous particles with a large number of pores having sizes of tens to hundreds of micrometers distributed therein, is non-aggregating, and has excellent fluidity.

[0029] The term "paste vinyl chloride polymer" as used herein refers to a type of vinyl chloride polymer, which may be polymerized by fine suspension polymerization, fine seed polymerization, emulsion polymerization, or the like, and is a polymer in the form of fine, dense, void-free particles having a size of tens to thousands of nanometers, which has agglomeration properties, and which has poor fluidity.

[0030] The terms "comprise", "have" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether specifically disclosed or not. To avoid any uncertainty, all compositions claimed by use of the term "comprise" may include any additional additives, adjuvants, or compounds, whether polymeric or otherwise, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any consecutive description any other component, step or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step or procedure not specifically described or listed.

[0031] Measurement method In this specification, the content of components in a composition is analyzed by gas chromatography measurement using a gas chromatography device manufactured by Agilent (product name: Agilent 7890 GC, column: HP-5, carrier gas: helium (flow rate 2.4 mL / min), detector: FID, injection volume: 1 μL, initial value: 70° C. / 4.2 min, final value: 280° C. / 7.8 min, program rate: 15° C. / min).

[0032] In this specification, "hardness" refers to Shore hardness (Shore "A" and / or Shore "D") at 25°C in accordance with ASTM D2240, measured under conditions of 3T 10s, and can be an index for evaluating plasticization efficiency, with a lower hardness indicating a more excellent plasticization efficiency.

[0033] In this specification, the "tensile strength" is calculated according to the ASTM D638 method by measuring the point where a test piece breaks after pulling it at a cross head speed of 200 mm / min (1T) using a UTM (manufacturer: Instron, model name: 4466) which is a test device, and calculating it according to the following mathematical formula 1.

[0034] [Mathematical formula 1] Tensile strength (kgf / cm 2 ) = Load value (kgf) / (Thickness (cm) x Width (cm))

[0035] In the present specification, the "elongation rate" is calculated by the following Equation 2 after measuring the point where the test piece breaks after pulling the test piece at a cross head speed of 200 mm / min (1T) using the UTM in accordance with the ASTM D638 method.

[0036] [Mathematical formula 2] Elongation rate (%) = length after elongation / initial length x 100

[0037] In this specification, the term "migration loss" refers to a test piece having a thickness of 2 mm or more, which is obtained according to KSM-3156, and after attaching glass plates to both sides of the test piece, the test piece is subjected to a pressure of 1 kgf / cm 2 A load of 10 ...

[0038] [Mathematical formula 3] Migration loss (%) = {[(initial weight of test piece) - (weight of test piece after leaving in oven)] / (initial weight of test piece)} x 100

[0039] In this specification, the "volatile loss" is calculated by measuring the weight of a test piece after treating the test piece at 80°C for 72 hours.

[0040] [Mathematical formula 4] Heat loss (%) = {[(initial weight of test piece) - (weight of test piece after treatment)] / (initial weight of test piece)} x 100

[0041] In the case of the various measurement conditions, the detailed conditions such as temperature, rotation speed, time, etc. may vary slightly depending on the case, and if they do vary, the measurement method and conditions will be separately specified.

[0042] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.

[0043] According to one embodiment of the present invention, the plasticizer composition includes one or more dihexylbenzene dicarboxylates, the dihexylbenzene dicarboxylates being one or more selected from dihexyl isophthalate and dihexyl terephthalate, and the hexyl group of the dihexylbenzene dicarboxylate is derived from an isomer mixture of hexyl alcohol.

[0044] According to one embodiment of the present invention, the isomeric mixture of hexyl alcohols of the plasticizer composition comprises two or more selected from the group consisting of 1-hexanol, 1-methylpentanol, 2-methylpentanol, 3-methylpentanol, 4-methylpentanol, 1,1-dimethylbutanol, 1,2-dimethylbutanol, 1,3-dimethylbutanol, 2,2-dimethylbutanol, 2,3-dimethylbutanol, 3,3-dimethylbutanol, 1-ethylbutanol, 2-ethylbutanol, 3-ethylbutanol, and cyclopentylmethanol.

[0045] The alkyl groups of the dihexylbenzene dicarboxylate can be determined by the alcohols contained in the hexyl alcohol isomers, and the final composition can include various compositions in which the two alkyl groups are bonded to the isomeric alkyl groups of hexyl alcohol, or one alkyl group is bonded to each of the two alkyl groups, or none is bonded to each of the two alkyl groups, and the ratio of the components in the final composition can be determined by the ratio of the reacting alcohol components.

[0046] Thus, when benzenedicarboxylate is applied, if an alcohol having 6 carbon atoms is used, an appropriate level of absorption speed can be ensured, compared to when the carbon number is less than 6, thereby improving processability, and tensile strength, elongation, and heat loss can be significantly improved. In addition, compared to when the carbon number is more than 6, excellent plasticization efficiency can be achieved, and great migration resistance and stress resistance can be expected.

[0047] The branching degree of the hexyl alcohol isomer mixture of the plasticizer composition according to one embodiment of the present invention may be 2.0 or less, preferably 1.5 or less. Specifically, the branching degree may be 1.5 or less, 1.3 or less, and more preferably 1.1 or less. Also, it may be 0.1 or more, 0.2 or more, 0.3 or more, and most preferably 0.7 or more. The branching degree of the hexyl alcohol isomer mixture may be maintained even when it is converted to dihexylbenzene dicarboxylate by esterification reaction. If the branching degree exceeds 2.0, the balance between physical properties may be lost, and a problem may occur in which the product does not meet one or more evaluation criteria. However, if the branching degree is 1.5 or less as a preferred range, the improvement of not only mechanical properties but also migration loss and heat loss may be more optimized, and the balance between physical properties may be excellent.

[0048] Here, the degree of branching may mean how many branched carbons the alkyl group bonded to a substance contained in the composition has, and the degree of branching may be determined according to the weight ratio of the substance. For example, assuming that an alcohol mixture contains 60% by weight of n-hexyl alcohol, 30% by weight of methylpentyl alcohol, and 10% by weight of ethylbutyl alcohol, the branched carbon numbers of each alcohol are 0, 1, and 2, respectively, so the branching degree can be calculated as [(60×0)+(30×1)+(10×2)] / 100, which is 0.5. Here, in the case of cyclopentylmethanol, the branched carbon number is considered to be 0.

[0049] The plasticizer composition according to one embodiment of the present invention may contain 1-hexanol and 2-methylpentanol in the hexyl alcohol isomer mixture. In this case, excellent effects can be obtained in terms of migration resistance and heat loss.

[0050] The branched hexyl alcohol including 2-methylpentanol may be included in an amount of 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, and preferably 60 parts by weight or more, 70 parts by weight or more, based on 100 parts by weight of the isomer mixture. The maximum amount may be entirely branched, and may be 99 parts by weight or less, 98 parts by weight or less, and preferably 95 parts by weight or less, or 90 parts by weight or less. When the branched hexyl alcohol is included in this range, improvement in mechanical properties can be expected.

[0051] In addition, the linear alcohol of 1-hexanol may be included in an amount of 50 parts by weight or less, 40 parts by weight or less, and preferably 30 parts by weight or less, based on 100 parts by weight of the isomer mixture. The 1-hexanol may not be present in the component, but may be included in an amount of at least 2 parts by weight, in which case, it is possible to obtain an advantage in that mechanical properties are improved while maintaining a balance between physical properties.

[0052] The plasticizer composition according to one embodiment of the present invention may contain 1-hexanol, 2-methylpentanol, and 3-methylpentanol in the isomer mixture of hexyl alcohol. By further containing 3-methylpentanol, the heat loss can be further improved while maintaining a balance between physical properties. In this case, 3-methylpentanol may be included as a component of the branched hexyl alcohol and may be present so as to satisfy the content of the branched hexyl alcohol described above.

[0053] More preferably, the mixture of hexyl alcohol isomers may further contain cyclopentylmethanol, which is expected to have the effect of complementing migration resistance and stress migration.

[0054] In this case, the cyclopentylmethanol may be present independently in an amount of 20 parts by weight or less, preferably 15 parts by weight or less, and more preferably 10 parts by weight or less, per 100 parts by weight of the isomer mixture, and may be absent or the minimum amount for obtaining the effect thereof may be 2 parts by weight.

[0055] In this case, the 3-methylpentanol and cyclopentylmethanol may each independently be present in an amount of 20 parts by weight or less, preferably 15 parts by weight or less, and more preferably 10 parts by weight or less, based on 100 parts by weight of the isomer mixture, and may be absent or the minimum amount for obtaining the effect thereof may be 2 parts by weight.

[0056] Specifically, depending on the ratio of branched alkyl groups to the total alkyl radicals in the final composition, and further, the ratio of a specific branched alkyl radical to the branched alkyl groups, the physical properties of plasticization efficiency and migration / weight loss characteristics can be balanced, and mechanical properties such as tensile strength and elongation and stress resistance can be maintained at the same or higher levels. Good carbonization properties can be achieved by the interaction between various types of benzene dicarboxylates contained in the composition, which can be achieved by the components of the above-mentioned hexyl alcohol isomers and their component ratios.

[0057] This makes it possible to eliminate the environmental problems associated with existing phthalate-based products and realize products with improved weight loss properties; it also makes it possible to significantly improve the migration and weight loss properties of existing terephthalate-based products, thereby enabling the realization of products with significantly improved mechanical properties and migration resistance compared to existing commercial products.

[0058] According to an embodiment of the present invention, the dihexylbenzene dicarboxylate is at least one selected from dihexyl isophthalate and dihexyl terephthalate. When the dihexylbenzene dicarboxylate is dihexyl phthalate, it is not a substance regulated due to environmental concerns, but it has potential environmental concerns and many restrictions on use. In addition, it has very poor mechanical properties such as tensile strength and elongation compared to isophthalate and terephthalate, and its plasticization efficiency is also low, so it is not suitable.

[0059] In addition, in the case of isophthalate and terephthalate, they are widely used as a substitute for phthalate-based plasticizers, but the alkyl group used is mostly C8 2-ethylhexyl, and it is common to use a composition in which this C8 isophthalate or terephthalate is mixed with a secondary plasticizer as a plasticizer, or to use a ternary composition in which the molecular weight of this substance is controlled by a transesterification reaction with an alcohol having a low carbon number, for example, a C3-C5 alcohol, as a plasticizer. As for the use of isomers, there are no substances other than C5 terephthalate and C9 terephthalate that have been used.

[0060] However, in the present invention, hexyl alcohol having 6 carbon atoms is used to maintain an optimal balance between physical properties without any one of the physical properties being significantly inferior, and in this case, it is not used alone but is used as a mixture of isomers, thereby providing the effect of improving the plasticization efficiency to the maximum.

[0061] Specifically, the dihexylbenzene dicarboxylate may be dihexyl isophthalate, dihexyl terephthalate, or a mixture of isophthalate and terephthalate. The isophthalate and terephthalate may be appropriately selected and applied depending on the intended use, and when a mixture of these two components is used, it is advantageous in that it is easier to balance the physical properties.

[0062] The method for producing the plasticizer composition according to one embodiment of the present invention is a method well known in the art and can be applied without any particular limitation as long as it can produce the above-mentioned plasticizer composition.

[0063] For example, the composition can be prepared by directly esterifying a benzenedicarboxylic acid (isophthalic acid and / or terephthalic acid) or anhydride with an isomeric mixture of hexyl alcohol, or by transesterifying an isomeric mixture of dihexylbenzenedicarboxylate with hexyl alcohol.

[0064] The plasticizer composition according to one embodiment of the present invention is a material prepared by appropriately carrying out the esterification reaction, and as long as it satisfies the above-mentioned conditions, in particular, the ratio of branched alcohol in the isomer mixed alcohol is controlled and specific components are included, there is no particular limitation on the preparation method.

[0065] For example, the direct esterification reaction may be carried out by adding benzenedicarboxylic acid or a derivative thereof and two or more mixed alcohols, adding a catalyst, and reacting under a nitrogen atmosphere, removing unreacted raw materials, neutralizing (or inactivating) the unreacted raw materials and the catalyst, and removing impurities (e.g., distillation under reduced pressure, etc.), and filtering.

[0066] The components and weight ratios of the isomer mixture of hexyl alcohol are as described above. The isomer mixture of alcohol can be used in a range of 200-900 mol%, 200-700 mol%, 200-600 mol%, 250-500 mol%, or 270-400 mol% relative to 100 mol% of the acid, and the component ratio in the final composition can be controlled by controlling the content of this alcohol.

[0067] The catalyst may be one or more selected from acid catalysts such as sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, paratoluenesulfonic acid, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, alkylsulfuric acid, etc., metal salts such as aluminum lactate, lithium fluoride, potassium chloride, cesium chloride, calcium chloride, iron chloride, aluminum phosphate, etc., metal oxides such as heteropolyacids, natural / synthetic zeolites, cation and anion exchange resins, and organic metals such as tetraalkyl titanate and its polymers. As a specific example, the catalyst may be tetraalkyl titanate. Preferably, paratoluenesulfonic acid, methanesulfonic acid, etc. are suitable as acid catalysts with low activation temperatures.

[0068] The amount of catalyst used may vary depending on the type. For example, in the case of a homogeneous catalyst, the amount may be within the range of 0.01 to 5 wt%, 0.01 to 3 wt%, 1 to 5 wt%, or 2 to 4 wt%, relative to 100 wt% of the total amount of reactants. In the case of a heterogeneous catalyst, the amount may be within the range of 5 to 200 wt%, 5 to 100 wt%, 20 to 200 wt%, or 20 to 150 wt%, relative to the total amount of reactants.

[0069] At this time, the reaction temperature can be within the range of 100°C to 280°C, 100°C to 250°C, or 120°C to 230°C.

[0070] As another example, the transesterification reaction may involve the reaction of isophthalate or terephthalate with an alcohol having an alkyl group different from the alkyl groups of the two benzenedicarboxylates, where the alkyl groups of the benzenedicarboxylate and the alcohol may be cross-linked.

[0071] The term "transesterification reaction" as used herein means a reaction in which an alcohol reacts with an ester to exchange the alkyl groups of the ester and the alkyl groups of the alcohol, as shown in Reaction Scheme 1 below.

[0072] [Reaction Scheme 1] [ka]

[0073] The mixture produced by the transesterification reaction can control the composition ratio of the mixture according to the amount of alcohol added. The amount of alcohol added can be 0.1 to 200 parts by weight, specifically 1 to 150 parts by weight, and more specifically 5 to 100 parts by weight, based on 100 parts by weight of dihexylbenzene dicarboxylate. For reference, the component ratio in the final composition can be determined by the amount of alcohol added, as in the direct esterification reaction.

[0074] According to one embodiment of the present invention, the transesterification reaction is carried out at a reaction temperature of 120°C to 190°C, preferably 135°C to 180°C, more preferably 141°C to 179°C, for 10 minutes to 10 hours, preferably 30 minutes to 8 hours, more preferably 1 to 6 hours. Within the above temperature and time ranges, the component ratio of the final plasticizer composition can be efficiently controlled. In this case, the reaction time can be calculated from the time when the reactants reach the reaction temperature after heating.

[0075] The transesterification reaction can be carried out in the presence of an acid catalyst or a metal catalyst, which has the effect of shortening the reaction time.

[0076] The acid catalyst may be, for example, sulfuric acid, methanesulfonic acid, or p-toluenesulfonic acid, and the metal catalyst may be, for example, an organometallic catalyst, a metal oxide catalyst, a metal salt catalyst, or a metal itself.

[0077] The metal component may be, for example, any one selected from the group consisting of tin, titanium, and zirconium, or a mixture of two or more of these.

[0078] According to another embodiment of the present invention, there is provided a resin composition comprising the above-described plasticizer composition and a resin.

[0079] The resin may be any resin known in the art, including, but not limited to, a mixture of one or more selected from the group consisting of straight vinyl chloride polymer, paste vinyl chloride polymer, ethylene-vinyl acetate copolymer, ethylene polymer, propylene polymer, polyketone, polystyrene, polyurethane, polylactic acid, natural rubber, synthetic rubber, and thermoplastic elastomer.

[0080] The plasticizer composition can be contained in an amount of 5 to 150 parts by weight, preferably 5 to 130 parts by weight, or 10 to 120 parts by weight, based on 100 parts by weight of the resin.

[0081] Generally, the resin in which the plasticizer composition is used can be manufactured as a resin product by melt processing or plastisol processing, and melt-processed resins and plastisol-processed resins can be produced differently depending on the polymerization method.

[0082] For example, when vinyl chloride polymer is used in melt processing, it is produced by suspension polymerization or the like and is in the form of solid resin particles with a large average particle size, and this type of vinyl chloride polymer is called straight vinyl chloride polymer, whereas when it is used in plastisol processing, it is produced by emulsion polymerization or the like and is in the form of fine resin particles in a sol state, and this type of vinyl chloride polymer is called paste vinyl chloride resin.

[0083] In this case, in the case of the straight vinyl chloride polymer, the plasticizer is preferably contained in a range of 5 to 80 parts by weight per 100 parts by weight of the polymer, and in the case of a paste vinyl chloride polymer, the plasticizer is preferably contained in a range of 40 to 120 parts by weight per 100 parts by weight of the polymer.

[0084] The resin composition may further contain a filler, the amount of the filler being 0 to 300 parts by weight, preferably 50 to 200 parts by weight, and more preferably 100 to 200 parts by weight, relative to 100 parts by weight of the resin.

[0085] The filler can be any filler known in the art, and is not particularly limited.For example, the filler can be one or more mixtures selected from silica, magnesium carbonate, calcium carbonate, hard carbon, talc, magnesium hydroxide, titanium dioxide, magnesium oxide, potassium hydroxide, aluminum hydroxide, aluminum silicate, magnesium silicate and barium sulfate.

[0086] Furthermore, the resin composition may further contain other additives such as a stabilizer, if necessary. The amount of each of the other additives such as the stabilizer may be, for example, 0 to 20 parts by weight, preferably 1 to 15 parts by weight, per 100 parts by weight of the resin.

[0087] The stabilizer may be, for example, a calcium-zinc (Ca-Zn) stabilizer such as a calcium-zinc complex stearate or a barium-zinc (Ba-Zn) stabilizer, but is not particularly limited thereto.

[0088] As described above, the resin composition may be applied to both melt processing and plastisol processing. For example, the melt processing may be a calendaring process, an extrusion process, or an injection process, and the plastisol processing may be a coating process.

[0089] Working Example Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0090] Example 1-1 Into a four-necked 3-liter reactor equipped with a cooler, condenser, decanter, reflux pump, temperature controller, stirrer, etc., 516.5 g of isophthalic acid, 1,170 g of hexanol (n-hexanol and 2-methylpentanol mixed at a weight ratio of 1:9), and 1.55 g of tetraisopropyl titanate as a catalyst were added, the reaction temperature was set to 230°C, and nitrogen gas was continuously added to carry out a direct esterification reaction for about 6 hours, and the reaction was completed when the acid value reached 0.1.

[0091] After the reaction was completed, distillation extraction was carried out under reduced pressure to remove unreacted raw materials. After distillation extraction, a neutralization process, a dehydration process, and a filtration process were performed to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nH2MPIP), and di(2-methylpentyl)isophthalate (D2MPIP).

[0092] Example 1-2 The same procedure was carried out as in Example 1-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 3:7 was used as hexanol, to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nHMPIP), and di(2-methylpentyl)isophthalate (DMPIP).

[0093] Examples 1-3 The same procedure was carried out as in Example 1-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 5:5 was used as hexanol, to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nHMPIP), and di(2-methylpentyl)isophthalate (DMPIP).

[0094] Examples 1-4 The same procedure was carried out as in Example 1-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 7:3 was used as hexanol, to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nHMPIP), and di(2-methylpentyl)isophthalate (DMPIP).

[0095] Examples 1-5 The same procedure was carried out as in Example 1-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 9:1 was used as hexanol, to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nHMPIP), and di(2-methylpentyl)isophthalate (DMPIP).

[0096] Examples 1-6 A plasticizer composition was obtained in the same manner as in Example 1-1, except that a mixture of n-hexanol, 2-methylpentanol, and 3-methylpentanol in a weight ratio of 2:3:5 was used as hexanol.

[0097] Examples 1-7 A plasticizer composition was obtained in the same manner as in Example 1-1, except that a mixture of n-hexanol, 2-methylpentanol, 3-methylpentanol, and cyclopentylmethanol in a weight ratio of 7:37:44:12 was used as hexanol.

[0098] When the total amount of the hexyl alcohol isomer mixture used in Examples 1-1 to 1-7 was 100 parts by weight, the relative weight parts of each alcohol contained in the mixture were summarized in Table 1 below.

[0099] [Table 1]

[0100] Example 2-1 Into a four-necked 3-liter reactor equipped with a cooler, condenser, decanter, reflux pump, temperature controller, stirrer, etc., 516.5 g of terephthalic acid, 1,170 g of hexanol (n-hexanol and 2-methylpentanol mixed at a weight ratio of 1:9), and 1.55 g of tetraisopropyl titanate as a catalyst were added, the reaction temperature was set to 230°C, and nitrogen gas was continuously added to carry out a direct esterification reaction for about 6 hours, and the reaction was completed when the acid value reached 0.1.

[0101] After the reaction was completed, distillation extraction was carried out under reduced pressure to remove unreacted raw materials. After distillation extraction, a neutralization process, a dehydration process, and a filtration process were performed to obtain a composition containing di(n-hexyl) terephthalate (DnHTP), (n-hexyl)(2-methylpentyl) terephthalate (nH2MPTP), and di(2-methylpentyl) terephthalate (D2MPTP).

[0102] Example 2-2 The same procedure was carried out as in Example 2-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 3:7 was used as hexanol, to obtain a composition containing di(n-hexyl)terephthalate (DnHTP), (n-hexyl)(2-methylpentyl)terephthalate (nH2MPTP), and di(2-methylpentyl)terephthalate (D2MPTP).

[0103] Example 2-3 The same procedure was carried out as in Example 2-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 7:3 was used as hexanol, to obtain a composition containing di(n-hexyl)terephthalate (DnHTP), (n-hexyl)(2-methylpentyl)terephthalate (nHMPTP), and di(2-methylpentyl)terephthalate (DMPTP).

[0104] Examples 2-4 The same procedure was carried out as in Example 2-1, except that a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 9:1 was used as hexanol, to obtain a composition containing di(n-hexyl)terephthalate (DnHTP), (n-hexyl)(2-methylpentyl)terephthalate (nHMPTP), and di(2-methylpentyl)terephthalate (DMPTP).

[0105] Examples 2-5 A plasticizer composition was obtained in the same manner as in Example 2-1, except that a mixture of n-hexanol, 2-methylpentanol, and 3-methylpentanol in a weight ratio of 2:3:5 was used as hexanol.

[0106] Examples 2-6 A plasticizer composition was obtained in the same manner as in Example 2-1, except that a mixture of n-hexanol, 2-methylpentanol, 3-methylpentanol, and cyclopentylmethanol in a weight ratio of 7:37:44:12 was used as hexanol.

[0107] In Examples 2-1 to 2-6, when the total amount of the hexyl alcohol isomer mixture was 100 parts by weight, the relative parts by weight of each alcohol contained in the mixture were summarized in Table 2 below.

[0108] [Table 2]

[0109] Comparative Example 1 Dioctyl phthalate (DOP), manufactured by LG Chem, was used as the plasticizer composition.

[0110] Comparative Example 2 Diisononyl phthalate (DINP) manufactured by LG Chem was used as the plasticizer composition.

[0111] Comparative Example 3 Di(2-ethylhexyl) terephthalate (DEHTP, LGflex GL300) manufactured by LG Chemical was used as the plasticizer composition.

[0112] Comparative Example 4 A mixture of di(2-ethylhexyl) terephthalate (DEHTP), butyl(2-ethylhexyl) terephthalate (BEHTP) and dibutyl terephthalate (DBTP) (LGflex GL500) manufactured by LG Chem was used as the plasticizer composition.

[0113] Comparative Example 5 A plasticizer composition was obtained in the same manner as in Example 1-1, except that a single compound, 2-methylpentanol, was used as hexanol instead of a mixture.

[0114] Comparative Example 6 A plasticizer composition was obtained in the same manner as in Example 2-1, except that a single compound, 2-methylpentanol, was used as hexanol instead of a mixture.

[0115] Comparative Example 7 A plasticizer composition was obtained in the same manner as in Example 1-1, except that n-heptanol was used instead of hexanol.

[0116] Comparative Example 8 The same procedure was carried out as in Example 1-3, except that phthalic acid was used instead of isophthalic acid, to obtain a composition containing di(n-hexyl)phthalate (DnHPh), (n-hexyl)(2-methylpentyl)phthalate (nH2MPPh), and di(2-methylpentyl)tetraacetate (D2MPPh).

[0117] Experimental example 1: Evaluation of seat performance Using the plasticizers of the Examples and Comparative Examples, test pieces were prepared according to the following recipe and preparation conditions in accordance with ASTM D638.

[0118] (1) Formulation: 100 parts by weight of straight vinyl chloride polymer (LS100), 50 parts by weight of plasticizer, and 3 parts by weight of stabilizer (BZ-153T)

[0119] (2) Mixing: Mix at 98℃ and 700 rpm

[0120] (3) Preparation of test pieces: 1T, 2T and 3T sheets were prepared by treating in a roll mill at 160°C for 4 minutes, and in a press at 180°C for 2.5 minutes (low pressure) and 2 minutes (high pressure).

[0121] (4) Evaluation items 1)Hardness In accordance with ASTM D2240, Shore hardness (Shore "A" and "D") at 25°C was measured for 10 seconds using a 3T test piece. The smaller the value, the better the plasticization efficiency.

[0122] 2) Tensile strength According to ASTM D638, the test equipment UTM (manufacturer: Instron, model name: 4466) was used to measure the point at which the 1T test piece broke after pulling at a cross head speed of 200 mm / min. The tensile strength was calculated as follows: Tensile strength (kgf / cm 2 ) = Load value (kgf) / thickness (cm) x width (cm)

[0123] 3) Measurement of elongation rate According to the ASTM D638 method, the UTM was used to measure the point at which the 1T test piece broke after pulling at a cross head speed of 200 mm / min, and the elongation was calculated as follows: The elongation rate (%) was calculated as follows: length after elongation / initial length×100.

[0124] 4) Measurement of migration loss According to KSM-3156, a test piece with a thickness of 2 mm or more is obtained, and a glass plate is attached to both sides of the 1T test piece, and then the specimen is subjected to a pressure of 1 kgf / cm 2 A load of 10 ... Migration loss (%) = [{(initial weight of test piece at room temperature) - (weight of test piece after leaving in oven)} / (initial weight of test piece at room temperature)] × 100

[0125] 5) Measurement of stress transfer A 2 mm thick test piece is bent and left at 23°C for 168 hours, after which the degree of migration (extent of separation) is observed and the results are recorded as a number; the closer to 0, the better the characteristics.

[0126] 6) Evaluation of carbonization characteristics : A test piece with a thickness of 0.25 mm was prepared in a size of 40 cm x 40 cm, and a carbonization test was performed in a Mathis Oven at 230℃ at a speed of 5 mm / 10 sec. The time at which the material started to turn black was compared and evaluated. Excellent carbonization characteristics means that the material started to turn black relatively slowly, and poor carbonization characteristics means that the material started to turn black relatively quickly. Of the values ​​from 1 to 5, 1 means the poorest and 5 means the best.

[0127] (5) Evaluation results The evaluation results for the above items are shown in Table 3 below.

[0128] [Table 3]

[0129] Referring to the results of Table 3, it can be seen that the plasticizer composition of the present invention maintains the same level of tensile strength and elongation as existing plasticizers, and achieves improved effects in terms of plasticization efficiency and migration resistance. In addition, it can be seen that the stress migration and carbonization properties are not inferior in any one aspect, and achieves a well-balanced effect. Comparative Examples 1 and 2 were the most commonly used plasticizer products in the past, but are currently prohibited from use due to environmental regulations. The plasticizers according to the embodiments of the present invention showed better plasticization efficiency and mechanical properties than the plasticizers of Comparative Examples 1 and 2, and also showed improved effects in terms of carbonization properties. This shows that the plasticizer of the present invention can be used in place of existing plasticizer products that are not environmentally friendly, and can provide better effects. In addition, Comparative Examples 3 and 4 are environmentally friendly plasticizers used instead of Comparative Examples 1 and 2, but Comparative Examples 3 and 4, like Comparative Examples 1 and 2, showed inferior plasticization efficiency compared to the plasticizers according to the Examples of the present invention, and showed some excellent effects in terms of mechanical properties, but showed significantly inferior results in terms of migration loss and stress migration. Migration loss and stress migration are indicators of the stability of a plasticizer product when applied, and the above results mean that the plasticizer compositions of the Examples of the present invention can achieve more stable performance, and even if some of the mechanical properties of Comparative Examples 3 and 4 are excellent, it is expected that it will be difficult to fully demonstrate excellent mechanical properties when applied to actual products due to their inferior plasticization efficiency and migration resistance.

[0130] On the other hand, in Comparative Examples 5 and 6, when isophthalic acid or terephthalic acid is applied, a single branched hexyl alcohol is used as the alcohol, instead of an isomer mixture of hexyl alcohol, and it can be seen that the mechanical properties such as tensile strength and elongation are inferior to those of the Examples, and the migration loss and stress migration properties are also inferior to those of the Examples. This means that the excellent mechanical properties and migration resistance achieved in the present invention are generated by the appropriate balance between the various alkyl groups derived from the isomer mixture of hexyl alcohol, and that the excellent properties of the plasticizer composition are not achieved by simply applying an alcohol having 6 carbon atoms.

[0131] In addition, Comparative Example 7, in which an alcohol having 7 carbon atoms, not 6 carbon atoms, was used for isophthalic acid, showed inferior plasticization efficiency, mechanical properties, and migration resistance compared to the Examples. This means that when the number of carbon atoms in the alkyl group bonded to benzenedicarboxylate is greater than 6, it is not possible to achieve properties comparable to those of the plasticizer compositions of the Examples of the present invention, and the excellent effects shown by the plasticizer compositions of the Examples of the present invention are achieved only when the alkyl group bonded to benzenedicarboxylate has 6 carbon atoms.

[0132] Finally, Comparative Example 8 relates to the case where phthalic acid is used as the acid, instead of isophthalic acid or terephthalic acid. In terms of plasticization efficiency, the plasticizer composition shows a similar level to the plasticizer compositions of the Examples of the present invention. However, in terms of mechanical properties, migration resistance, and carbonization properties, the plasticizer composition of Comparative Example 8 shows inferior effects compared to the Examples. Since the plasticizer composition of Comparative Example 8 contains a component derived from phthalic acid, it still has the problem of being unenvironmental, as in Comparative Examples 1 and 2 described above.

Claims

1. A plasticizer composition comprising one or more dihexylbenzene dicarboxylates, The dihexylbenzene dicarboxylate is at least one selected from dihexyl isophthalate and dihexyl terephthalate, The hexyl group of the dihexylbenzene dicarboxylate is derived from an isomeric mixture of hexyl alcohol, the isomeric mixture of hexyl alcohols comprises 1-hexanol and 2-methylpentanol; The isomer mixture of hexyl alcohol contains 10 to 95 parts by weight of a branched alcohol per 100 parts by weight of the isomer mixture. Plasticizer composition.

2. The isomer mixture of hexyl alcohol is one or more selected from the group consisting of 1-methylpentanol, 3-methylpentanol, 4-methylpentanol, 1,1-dimethylbutanol, 1,2-dimethylbutanol, 1,3-dimethylbutanol, 2,2-dimethylbutanol, 2,3-dimethylbutanol, 3,3-dimethylbutanol, 1-ethylbutanol, 2-ethylbutanol, 3-ethylbutanol, and cyclopentylmethanol. The plasticizer composition of claim 1 , comprising:

3. 2. The plasticizer composition according to claim 1, wherein the isomer mixture of hexyl alcohol contains 30 to 95 parts by weight of a branched alcohol per 100 parts by weight of the isomer mixture.

4. 2. The plasticizer composition according to claim 1, wherein the isomer mixture of hexyl alcohol contains 40 to 95 parts by weight of a branched alcohol per 100 parts by weight of the isomer mixture.

5. 2. The plasticizer composition according to claim 1, wherein the isomer mixture of hexyl alcohol contains 40 parts by weight or less of 1-hexanol per 100 parts by weight of the isomer mixture.

6. 2. The plasticizer composition of claim 1, wherein the dihexylbenzene dicarboxylate is dihexyl isophthalate.

7. 2. The plasticizer composition of claim 1, wherein the dihexylbenzene dicarboxylate is dihexyl terephthalate.

8. 2. The plasticizer composition of claim 1, wherein the dihexylbenzene dicarboxylate is a mixture of dihexyl isophthalate and dihexyl terephthalate.

9. 2. The plasticizer composition of claim 1, wherein the isomeric mixture of hexyl alcohols comprises 1-hexanol, 2-methylpentanol, and 3-methylpentanol.

10. A resin composition comprising 100 parts by weight of a resin and 5 to 150 parts by weight of the plasticizer composition according to claim 1 relative to 100 parts by weight of the resin.

11. The resin composition according to claim 10, wherein the resin is at least one selected from the group consisting of straight vinyl chloride polymer, paste vinyl chloride polymer, ethylene-vinyl acetate copolymer, ethylene polymer, propylene polymer, polyketone, polystyrene, polyurethane, polylactic acid, natural rubber, and synthetic rubber.

Citation Information

Patent Citations

  • Preparation of diterephthalate based on degradative esterexchange of scrapped or unused terephthalic polyester

    JP1991056446A

  • Production of ester mixture

    JP2016150940A

  • Ester-based compound, plasticizer composition containing the same, method for producing the same, and resin composition containing the same

    JP2017506216A

  • Ester-based compound, plasticizer composition containing the same, method for producing the same, and resin composition containing the same

    JP2017509592A

  • Cyclohexane triester based plasticizer composition and resin composition comprising the same

    KR1020200127890A