Method for producing an aerogel composite and an aerogel composite

By impregnating fiber mats with catalyzed silica sol to form an airgel composite with controlled pore structures, the method addresses limitations in thermal insulation and sound absorption performance, achieving enhanced sound absorption and insulation properties.

JP7562217B2Active Publication Date: 2024-10-07LG CHEM LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023519132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-02
Filing Date
2022-03-23
Publication Date
2024-10-07
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

Existing sound-absorbing materials like glass fiber mats and polymer mats face limitations in improving thermal insulation and sound absorption performance, particularly in high frequency ranges, due to their pore structure.

Method used

A method involving impregnating a fiber mat with catalyzed silica sol at specific volume ratios, followed by gelling, aging, and drying to form an airgel composite with controlled pore sizes, reducing macropores and increasing mesopores, thereby enhancing sound absorption and thermal insulation.

Benefits of technology

The airgel composite achieves improved sound absorption coefficients across various frequencies, especially in high frequencies, and reduced thermal conductivity, making it an effective sound-absorbing and insulating material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562217000002
    Figure 0007562217000002
  • Figure 0007562217000001
    Figure 0007562217000001
Patent Text Reader

Abstract

The present invention relates to a method for producing an aerogel composite, which includes a step (S10) of impregnating a fiber mat with a catalyzed silica sol at a volume ratio of 0.1 to 1:1 (catalyzed silica sol:fiber mat) and gelling the impregnated fiber mat, and to an aerogel composite produced thereby.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0043328 filed on April 2, 2021, and all contents disclosed in the documents of said Korean patent application are incorporated by reference into this specification.

[0002] The present invention relates to a method for producing an aerogel composite having an improved sound absorption coefficient and usable as a sound absorbing material, and to an aerogel composite produced by the method. [Background technology]

[0003] Glass fiber mats or polymer mats, which are mainly used as sound absorbing materials, are widely used as insulating materials due to their excellent heat insulating and sound absorbing properties. However, since the glass fiber mats or polymer mats are mats containing fibers with diameters of several microns (μm) to several tens of microns (μm) and macropores in other spaces, there is a limit to improving the heat insulating and sound absorbing properties except by increasing the thickness of the mat.

[0004] Korean Patent Publication No. 10-1391098 discloses a sound-absorbing sheet made of glass fiber, cellulose fiber, and organic synthetic fiber in a nonwoven fabric in order to improve the sound-absorbing performance of a glass fiber mat. However, the sound-absorbing sheet has a large average pore size of 10 μm to 50 μm, so it is practically difficult to improve the heat insulation performance, and it is difficult to expect improvement in sound-absorbing performance in the high frequency range of 2,000 Hz or more, especially 2,500 Hz or more. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] KR10-1391098B1 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been devised to solve the problems of the conventional techniques described above, and aims to provide a method for producing an aerogel composite that has an improved sound absorption coefficient and can be used as a sound absorbing material while also ensuring thermal insulation performance, and an aerogel composite produced by the method. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides a method for producing an aerogel composite and an aerogel composite produced thereby.

[0008] (1) The present invention provides a method for producing an aerogel composite, comprising the step (S10) of impregnating a fiber mat with a catalyzed silica sol in a volume ratio of 0.1 to 1:1 (catalyzed silica sol:fiber mat) and gelling the fiber mat.

[0009] (2) The present invention provides the method for producing an aerogel composite according to (1), wherein the step (S10) is carried out by impregnating a fiber mat with a catalyzed silica sol in a volume ratio of 0.1 to 0.9:1 (catalyzed silica sol:fiber mat) and gelling the fiber mat.

[0010] (3) The present invention provides a method for producing an aerogel composite according to (1) or (2), in which the catalyzed silica sol is produced by the steps of: mixing a silica precursor, an organic solvent, and an aqueous solvent to produce a silica precursor composition (S1); mixing an organic solvent, a base catalyst, and a hydrophobizing agent to produce a catalyst composition (S2); and mixing the silica precursor composition and the catalyst composition to produce a catalyzed silica sol (S3).

[0011] (4) In the present invention, in the above (3), the silica concentration of the silica precursor composition produced in the step (S1) is 10 kg / m 3 ~100kg / m 3 The present invention provides a method for producing an aerogel composite.

[0012] (5) In the present invention, in the above (3) or (4), the silica concentration of the silica precursor composition produced in the step (S1) is 40 kg / m 3 ~70kg / m 3 The present invention provides a method for producing an aerogel composite.

[0013] (6) The present invention provides a method for producing an aerogel composite in any one of the above (1) to (5), comprising: a step (S20) of maturing the wet gel composite gelled in the step (S10); and a step (S30) of drying the wet gel composite maturated in the step (S20) to obtain an aerogel composite.

[0014] (7) The present invention provides the method for producing an aerogel composite according to the above (6), wherein the aerogel composite obtained in the step (S30) includes pores having a pore diameter of 2 nm to 50 nm.

[0015] (8) The present invention provides the method for producing an aerogel composite according to any one of the above items (1) to (7), wherein the fiber mat is a glass fiber mat.

[0016] (9) The present invention provides the method for producing an aerogel composite according to any one of the above items (1) to (8), wherein the fiber mat contains pores having a pore diameter of 100 μm to 1,000 μm.

[0017] (10) The present invention provides an aerogel composite comprising a fiber mat and an aerogel formed inside and on the surface of the fiber mat, the aerogel composite having an overall average sound absorption coefficient of 0.41 or more, the average value being the average value of the sound absorption coefficients by frequency calculated by converting the sound absorption coefficients measured in the frequency range of 50 Hz to 6,400 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band.

[0018] (11) The present invention provides an aerogel composite according to the above (10), in which the aerogel composite has a high frequency average sound absorption coefficient of 0.35 or more, the high frequency average sound absorption coefficient being the average value of the sound absorption coefficients by frequency calculated by converting the sound absorption coefficients measured in a frequency range of 2,500 Hz to 6,400 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band.

[0019] (12) The present invention provides an aerogel composite according to the above (10) or (11), wherein the aerogel composite has a room-temperature thermal conductivity of 30.0 mW / mK or less. Effect of the Invention

[0020] The aerogel composite produced by the method for producing an aerogel composite of the present invention has the effect of reducing macropores and increasing mesopores in the fiber mat, thereby improving the sound absorption coefficient and heat insulation performance.

[0021] The aerogel composite of the present invention has excellent sound absorbing and heat insulating properties and is useful as a sound absorbing material.

[0022] Moreover, the aerogel composite of the present invention has particularly excellent sound absorbing properties in the high frequency range. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a graph showing the sound absorption coefficients for each frequency, which were calculated by converting the sound absorption coefficients measured in a frequency range of 50 Hz to 6,400 Hz using an Impedance Tube P-S40-20 in a third-one Octave band. The sound absorption coefficients were then calculated for each frequency, for the aerogel composites prepared in Examples 1 to 3 of the present invention and the glass fiber mat of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.

[0025] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0026] In the present invention, the terms "mesopore" and "macropore" refer to pores having a pore diameter classified according to the IUPAC recommendation, where mesopores refer to pores having a pore diameter of 2 nm to 50 nm, and macropores refer to pores having a pore diameter of more than 50 nm.

[0027] The present invention provides a method for producing an aerogel composite. The aerogel composite produced by the method has an improved sound absorption coefficient and is useful as a sound absorbing material.

[0028] According to one embodiment of the present invention, the method for producing the aerogel composite may include a step (S10) of impregnating a fiber mat with a catalyzed silica sol in a volume ratio of 0.1 to 1:1 (catalyzed silica sol:fiber mat) to form a gel.

[0029] According to one embodiment of the present invention, the step (S10) may be a step for forming an aerogel composite by impregnating a fiber mat with a catalyzed silica sol and gelling it to form an aerogel inside and on the surface of the fiber mat.

[0030] According to one embodiment of the present invention, the "impregnation" may be performed by introducing a fluid catalyzed silica sol into the fiber mat, and in this case, the catalyzed silica sol may penetrate into the pores inside the fiber mat.

[0031] According to one embodiment of the present invention, the "gelation" can be performed by gelling the catalyzed silica sol impregnated in the fiber mat, or by leaving the fiber mat impregnated with the catalyzed silica sol. The gelation can be performed simultaneously with the impregnation.

[0032] According to one embodiment of the present invention, the (S10) step can be carried out by putting the catalyzed silica sol and the fiber mat into a reaction vessel, or by putting the catalyzed silica sol onto a fiber mat moving on a conveyor belt in a roll-to-roll process.

[0033] According to one embodiment of the present invention, when the (S10) step is carried out by adding the catalyzed silica sol and the fiber mat to the reaction vessel, the order of adding the catalyzed silica sol and the fiber mat to the reaction vessel is not particularly limited. As a specific example, the impregnation in the (S10) step can be carried out by adding the catalyzed silica sol after adding the fiber mat to the reaction vessel, adding the catalyzed silica sol after adding the fiber mat to the reaction vessel, or adding the catalyzed silica sol and adding the fiber mat to the reaction vessel at the same time. Among them, the method of adding the catalyzed silica sol after adding the fiber mat is preferred in terms of inducing more uniform impregnation.

[0034] According to one embodiment of the present invention, the step (S10) can be carried out by impregnating the catalyzed silica sol into the fiber mat at a volume ratio of 0.1 to 1:1 (catalyzed silica sol:fiber mat) and gelling it, as described above. By adjusting the volume ratio of the catalyzed silica sol impregnated into the fiber mat in this manner, the macropores of the fiber mat can be reduced and the mesopores can be increased by the formation of aerogel in the fiber mat, thereby improving the sound absorption performance of the aerogel composite, and improving the heat insulation performance from the aerogel formed inside and on the surface of the fiber mat.

[0035] According to one embodiment of the present invention, in order to improve the insulation performance of the fiber mat to a predetermined level or more and to further improve the sound absorption performance, especially the sound absorption performance in the high frequency range (meaning 2,500 Hz or more), the catalyzed silica sol may be impregnated into the fiber mat at a volume ratio of 0.1 or more, 0.2 or more, or 0.3 or more, and may be impregnated at a volume ratio of 1.0 or less, 0.9 or less, 0.8 or less, or 0.7 or less. As a specific example, the (S10) step may be performed by impregnating the fiber mat with the catalyzed silica sol at a volume ratio (catalyzed silica sol:fiber mat) of 0.1 to 0.9:1, 0.2 to 0.8, or 0.3 to 0.7, and gelling the mixture, in which case the insulation performance of the fiber mat can be secured to a predetermined level or more and the sound absorption performance at high frequencies can be further improved.

[0036] According to one embodiment of the present invention, the catalyzed silica sol may be prepared by the steps of: (S1) preparing a silica precursor composition by mixing a silica precursor, an organic solvent, and an aqueous solvent; (S2) preparing a catalyst composition by mixing an organic solvent, a base catalyst, and a hydrophobizing agent; and (S3) preparing a catalyzed silica sol by mixing the silica precursor composition and the catalyst composition.

[0037] According to one embodiment of the present invention, the silica precursor composition prepared in the step (S1) may be a silica precursor composition for finally preparing a silica aerogel through a gelation reaction of the catalyzed silica sol prepared in the step (S3) by mixing with the catalyst composition prepared in the step (S2).

[0038] According to an embodiment of the present invention, the silica precursor in the step (S1) is for making the aerogel produced by gelation in the step (S10) contain silica, and examples of the silica precursor include tetra methyl orthosilicate (TMOS), tetra ethyl orthosilicate (TEOS), methyl triethyl orthosilicate, dimethyl diethyl orthosilicate, tetra propyl orthosilicate, tetra isopropyl orthosilicate, tetra butyl orthosilicate, tetra secondary butyl orthosilicate, tetra tertiary butyl orthosilicate, tetra hexyl orthosilicate, tetra ethyl ... The silica precursor may be one or more selected from the group consisting of tetracyclohexyl orthosilicate, tetracyclohexyl orthosilicate, and tetradodecyl orthosilicate, or a pre-hydrolysate of the above compounds. When the pre-hydrolysate is used, the addition of an acid is not required, the hydrolysis step of the silica precursor can be shortened or omitted, and the surface modification effect can be promoted.As a specific example, the silica precursor may be prehydrolyzed polyethylsilicate (HTEOS), which is a prehydrolyzed ethylpolysilicate oligomer having a wide molecular weight distribution. When the prehydrolyzed polyethylsilicate (HTEOS) is synthesized into an oligomer form from tetraethylorthosilicate (TEOS) by varying the degree of prehydrolysis (hydration degree), physical properties such as gelation time can be adjusted, and therefore the HTEOS can be easily applied according to the reaction conditions of the user.

[0039] According to one embodiment of the present invention, the organic solvent in step (S1) may be an alcohol. The alcohol may be a monohydric alcohol such as methanol, ethanol, isopropanol, or butanol; or a polyhydric alcohol such as glycerol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, or sorbitol, and any one or a mixture of two or more of these may be used. Among them, taking into consideration the miscibility with the aqueous solvent and the aerogel, the organic solvent may be a monohydric alcohol having 1 to 6 carbon atoms such as methanol, ethanol, isopropanol, or butanol, and a specific example may be ethanol.

[0040] According to one embodiment of the present invention, the aqueous solvent in step (S1) may be water, and a specific example thereof may be distilled water.

[0041] According to one embodiment of the present invention, the silica concentration of the silica precursor composition prepared in step (S1) is 10 kg / m 3 ~100kg / m 3 The silica concentration is the concentration of silica contained in the silica precursor relative to the silica precursor composition, and can be adjusted based on the composition of the silica precursor, the organic solvent, and the aqueous solvent. As a specific example, the silica concentration of the silica precursor composition prepared in the step (S1) can be 20 kg / m 3 ~80kg / m 3 , 30kg / m 3~70kg / m 3 , 30kg / m 3 ~60kg / m 3 , or 35 kg / m 3 ~45kg / m 3 Within this range, the aerogel formed in the fiber mat reduces the macropores of the fiber mat while increasing the mesopores, thereby improving the sound absorption performance of the aerogel composite, and improving the heat insulation performance from the aerogel formed inside and on the surface of the fiber mat.

[0042] According to one embodiment of the present invention, the step (S1) may be performed by mixing the silica precursor, the organic solvent, and the aqueous solvent in a weight ratio of 1:0.1-1.5:0.1-0.5, 1:0.5-1.5:0.1-0.4, or 1:0.5-1.2:0.1-0.3 to satisfy the silica concentration of the silica composition precursor prepared by the step (S1).

[0043] According to one embodiment of the present invention, the catalyst composition prepared in the step (S2) may be a catalyst composition for finally producing a silica aerogel by inducing a gelation reaction of the catalyzed silica sol prepared in the step (S3) through mixing with the silica precursor composition prepared in the step (S1).

[0044] According to one embodiment of the present invention, the organic solvent in step (S2) may be an alcohol. The alcohol may be a monohydric alcohol such as methanol, ethanol, isopropanol, or butanol; or a polyhydric alcohol such as glycerol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, or sorbitol, and any one or a mixture of two or more of these may be used. Among them, taking into consideration the miscibility with the aqueous solvent and the aerogel, the organic solvent may be a monohydric alcohol having 1 to 6 carbon atoms such as methanol, ethanol, isopropanol, or butanol, and a specific example may be ethanol.

[0045] According to one embodiment of the present invention, the base catalyst in the (S2) step can be a base catalyst that can create a pH condition for gelation of the catalyzed silica sol, and examples thereof include inorganic bases such as sodium hydroxide, potassium hydroxide, etc.; or organic bases such as ammonium hydroxide.

[0046] According to one embodiment of the present invention, the organic base is ammonium hydroxide (NH 4 OH), tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide (TPAH), tetrabutylammonium hydroxide (TBAH), methylamine, ethylamine, isopropylamine, monoisopropylamine, diethylamine, diisopropylamine, dibutylamine, trimethylamine, triethylamine, triisopropylamine, tributylamine, choline, monoethanolamine, diethanolamine, 2-aminoethanol, 2-(ethylamino)ethanol, 2-(methylamino)ethanol, N-methyldiethanolamine, dimethylaminoethanol, diethylaminoethanol, nitrile ethanol, 2-(2-aminoethoxy)ethanol, 1-amino-2-propanol, triethanolamine, monopropanolamine, and dibutanolamine. Specific examples of the ammonium hydroxide (aqueous ammonia; NH 4 OH).

[0047] According to an embodiment of the present invention, the hydrophobizing agent in step (S2) may be an alkylsilane compound, and a specific example of the hydrophobizing agent may be an alkylsilane compound containing an alkyl group that induces hydrophobization and a silane functional group that can react with the "-Si-O-" functional group of the wet gel. As a more specific example, the hydrophobizing agent may be one or more selected from the group consisting of trimethylethoxysilane (TMES), trimethylsilanol (TMS), trimethylchlorosilane (TMCS), methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), dimethyldiethoxysilane (DMDEOS), ethyltriethoxysilane, and phenyltriethoxysilane. The alkylsilane compound may participate in the gelation reaction of the silica precursor as a co-precursor, thereby hydrophobizing the wet gel composite formed by gelation. That is, the alkylsilane compound can be gelled together with the silica precursor during the gelling step (S10), and the alkylsilane compound that is not gelled and is trapped in the gel can form an alkyl-Si-O-Si network during aging to hydrophobize the wet gel composite.

[0048] According to one embodiment of the present invention, the (S2) step may be performed by mixing the organic solvent, the base catalyst, and the hydrophobizing agent in a weight ratio of 1:0.01-0.1:0.1-0.5, 1:0.02-0.08:0.1-0.3, or 1:0.04-0.06:0.1-0.2.

[0049] According to one embodiment of the present invention, the (S3) step is a step for preparing a catalyzed silica sol to be impregnated and gelled into a fiber mat in the (S10) step, and may be performed by mixing the silica precursor composition prepared in the (S1) step and the catalyst composition prepared in the (S2) step.

[0050] According to one embodiment of the present invention, the step (S3) may be performed by mixing the silica precursor composition and the catalyst composition in a volume ratio of 1:0.1-10.0, 1:0.5-5.0, 1:0.7-2.0, or 1:0.8-1.2.

[0051] According to one embodiment of the present invention, the aerogel composite manufactured by the impregnation and gelation in the (S10) step may be obtained in the form of a gelled wet gel composite containing a solvent. Thus, the method for manufacturing the aerogel composite may include a step (S20) of aging the wet gel composite gelled in the (S10) step to obtain a dried aerogel composite, and a step (S30) of drying the wet gel composite aged in the (S20) step to obtain an aerogel composite.

[0052] According to one embodiment of the present invention, the step (S20) is an aging step in which the gelled wet-gel composite is left at an appropriate temperature to complete chemical changes, and the network structure formed by the gelation can be made stronger, thereby improving the mechanical stability of the aerogel composite.

[0053] According to one embodiment of the present invention, the (S20) step may be performed by leaving the gelled wet gel composite at an appropriate temperature by itself. As another example, the (S20) step may be performed by leaving the gelled wet gel composite at an appropriate temperature by itself in the presence of the wet gel blanket composite. 4The method may be carried out by adding a solution of a base catalyst such as dimethyl ether (DMSO), triethylamine, or pyridine diluted in an organic solvent at a concentration of 1 to 10%. In this case, the Si-O-Si bonding is maximally induced in the aerogel, making the network structure of the silica gel stronger and making it easier to maintain the pore structure in the subsequent drying process. In this case, the organic solvent may be the above-mentioned alcohol, and specifically, may include ethanol.

[0054] According to one embodiment of the present invention, the (S20) step may be performed at a temperature of 30°C to 70°C, 40°C to 70°C, or 50°C to 70°C for 1 hour to 30 hours, 10 hours to 30 hours, or 20 hours to 25 hours in order to strengthen the pore structure. Within this range, a decrease in productivity can be prevented, and a loss of the solvent due to evaporation can be prevented, thereby preventing an increase in production costs.

[0055] According to one embodiment of the present invention, the (S20) step may be carried out in a separate reaction vessel after recovering the gelled wet-gel composite, or may be carried out within the reaction vessel in which the (S10) step was carried out.

[0056] According to an embodiment of the present invention, the step (S30) is a step of drying the wet gel composite aged in the step (S20) to obtain a dried aerogel composite, and the drying may be performed by supercritical drying or atmospheric drying to remove the solvent while maintaining the pore structure of the aged gel.

[0057] According to one embodiment of the present invention, the supercritical drying may be performed using supercritical carbon dioxide. 2Carbon dioxide is in a gaseous state at room temperature and pressure, but when it exceeds a certain temperature and pressure limit called the supercritical point, it enters a critical state where the evaporation process does not occur and it cannot be distinguished between gas and liquid, and carbon dioxide in this critical state is called supercritical carbon dioxide. Supercritical carbon dioxide has a molecular density close to that of a liquid, but has low viscosity and properties close to that of a gas, and it diffuses quickly, has high thermal conductivity, has high drying efficiency, and can shorten the drying process time. The supercritical drying involves a solvent replacement process in which the matured wet gel composite is placed in a supercritical drying reactor, filled with liquid carbon dioxide, and the alcohol solvent inside the wet gel is replaced with carbon dioxide. After this, the temperature is raised to 40°C to 80°C, 50°C to 80°C, or 60°C to 80°C at a heating rate of 0.1°C / min to 1°C / min, and then carbon dioxide (CO) is added to the reactor at a pressure of at least the pressure at which carbon dioxide enters a supercritical state, specifically, a pressure of 100 bar to 150 bar, to thereby obtain a solvent. 2 ) for a desired time, specifically 20 minutes to 1 hour. Generally, carbon dioxide becomes supercritical at a temperature of 31°C and a pressure of 73.8 bar. After maintaining the temperature and pressure at which carbon dioxide becomes supercritical for 2 hours to 12 hours, more specifically 2 hours to 6 hours, the pressure is gradually removed to complete the supercritical drying process, and an aerogel composite can be obtained. Here, the solvent, such as the organic solvent, removed from the wet gel composite by supercritical drying can be separately recovered through a separator connected to the supercritical drying reactor.

[0058] According to one embodiment of the present invention, the atmospheric drying can be carried out by a conventional method such as hot air drying, infrared drying (IR drying) at a temperature of 70° C. to 200° C. and atmospheric pressure (1±0.3 atm).

[0059] According to one embodiment of the present invention, the aerogel composite obtained in step (S30) may include pores having a pore diameter of 2 nm to 50 nm. For example, the volume ratio of the pores having a pore diameter of 2 nm to 50 nm may be greater than the volume ratio of the pores having a pore diameter of 100 μm to 1,000 μm. As a result, the formation of aerogel in the fiber mat reduces macropores and increases mesopores in the fiber mat, thereby improving the sound absorption performance of the aerogel composite and improving the heat insulation performance from the aerogel formed inside and on the surface of the fiber mat.

[0060] According to one embodiment of the present invention, the fiber mat may be a glass fiber mat that can be used as a sound absorbing material, and as a specific example, the fiber mat may be formed of fibers or glass fibers having a diameter of more than 1 μm, for example, a diameter of 1 μm to 100 μm, and the fiber mat may include pores, i.e., macropores, having pores with a pore diameter of more than 50 nm, for example, a pore diameter of 100 μm to 1,000 μm, between the fibers or glass fibers.

[0061] According to the method for producing an aerogel composite of the present invention, as described above, by forming an aerogel composite on a fiber mat, specifically a glass fiber mat, which can be used as a sound absorbing material by itself, it is possible to simultaneously improve sound absorbing performance and heat insulating performance by decreasing the macropores of the fiber mat and increasing the mesopores.

[0062] The present invention provides an aerogel composite. The aerogel composite may be manufactured by the manufacturing method of the aerogel composite, and may have an improved sound absorption coefficient and be useful as a sound absorbing material.

[0063] According to an embodiment of the present invention, the aerogel composite includes a fiber mat and an aerogel formed inside and on a surface of the fiber mat, and has an overall average sound absorption coefficient of 0.41 or more, which is an average value of sound absorption coefficients by frequency calculated by converting sound absorption coefficients measured in a frequency range of 50 Hz to 6,400 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band.

[0064] According to one embodiment of the present invention, the fiber mat may be the same as the fiber mat described in the method for producing an aerogel composite, and the aerogel may be an aerogel formed by the method for producing an aerogel composite.

[0065] According to one embodiment of the present invention, the aerogel composite may include a fiber mat component having pores with a pore diameter of 100 μm to 1,000 μm formed from fibers or glass fibers having a diameter of more than 1 μm derived from the fiber mat, and macropores in the fiber mat, specifically pores with a pore diameter of 100 μm to 1,000 μm, which are mesopores formed by aerogel formation in the pores having a pore diameter of 2 nm to 50 nm. In this way, by forming aerogel in the fiber mat to reduce macropores and increase mesopores, the average diameter of the overall pores in the fiber mat can be reduced, improving sound absorption performance, and the aerogel formed in the fiber mat can also improve heat insulation performance.

[0066] According to one embodiment of the present invention, the aerogel composite may include some pores having a pore diameter of more than 50 nm, specifically pores having a pore diameter of 100 μm to 1,000 μm, i.e., macropores, derived from the fiber mat. However, even in this case, the aerogel composite may have pores having a pore diameter of 2 nm to 50 nm, i.e., mesopores, whose volume ratio is larger than pores having a pore diameter of more than 50 nm, i.e., macropores, and thus, the formation of aerogel in the fiber mat reduces the macropores of the fiber mat while increasing the mesopores, thereby improving the sound absorption performance of the aerogel composite and improving the heat insulation performance from the aerogel formed inside and on the surface of the fiber mat.

[0067] According to one embodiment of the present invention, the aerogel composite has an overall average sound absorption coefficient, which is an average value of sound absorption coefficients by frequency calculated by converting sound absorption coefficients measured in a frequency range of 50 Hz to 6,400 Hz using an Impedance Tube P-S40-20 into data in 1 / 3 octave bands, of 0.41 or more, 0.41 to 0.60, or 0.43 to 0.54. It is considered that the aerogel composite has excellent sound absorption performance within this range.

[0068] According to one embodiment of the present invention, the aerogel composite may have a sound absorption coefficient calculated by converting the sound absorption coefficient measured at a frequency of 2,500 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band of 0.50 or more, 0.51 or more, or 0.59 or more, and may be 1.00 or less, 0.95 or less, or 0.91 or less. In addition, in order to ensure sound absorption performance in the high frequency range, the aerogel composite may have a sound absorption coefficient at a frequency of 2,500 Hz of 0.60 or more, 0.65 or more, 0.70 or more, 0.71 or more, or 0.82 or more.

[0069] According to one embodiment of the present invention, the aerogel composite may have a sound absorption coefficient calculated by converting the sound absorption coefficient measured at a frequency of 3,150 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band of 0.35 or more, 0.39 or more, or 0.41 or more, and may be 1.00 or less, 0.95 or less, 0.90 or less, or 0.89 or less. In addition, in order to ensure sound absorption performance in the high frequency range, the aerogel composite may have a sound absorption coefficient at a frequency of 3,150 Hz of 0.47 or more, 0.52 or more, 0.60 or more, 0.70 or more, or 0.77 or more.

[0070] According to one embodiment of the present invention, the aerogel composite may have a sound absorption coefficient calculated by converting the sound absorption coefficient measured at a frequency of 4,000 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band of 0.28 or more, 0.31 or more, or 0.36 or more, and may be 1.00 or less, 0.95 or less, 0.90 or less, or 0.87 or less. In addition, in order to ensure sound absorption performance in the high frequency range, the aerogel composite may have a sound absorption coefficient at a frequency of 4,000 Hz of 0.37 or more, 0.40 or more, 0.50 or more, 0.60 or more, or 0.61 or more.

[0071] According to one embodiment of the present invention, the aerogel composite may have a sound absorption coefficient calculated by converting the sound absorption coefficient measured at a frequency of 5,000 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band of 0.25 or more, 0.27 or more, or 0.35 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.79 or less. In addition, in order to ensure sound absorption performance in the high frequency range, the aerogel composite may have a sound absorption coefficient at a frequency of 5,000 Hz of 0.52 or more, 0.53 or more, 0.60 or more, 0.67 or more, or 0.69 or more.

[0072] According to one embodiment of the present invention, the aerogel composite may have a sound absorption coefficient calculated by converting the sound absorption coefficient measured at a frequency of 6,300 Hz using an Impedance Tube P-S40-20 into data in a 1 / 3 octave band of 0.25 or more, 0.35 or more, or 0.36 or more, or may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.74 or less. In addition, in order to ensure sound absorption performance in the high frequency range, the aerogel composite may have a sound absorption coefficient at a frequency of 6,300 Hz of 0.43 or more, 0.50 or more, 0.60 or more, 0.62 or more, or 0.68 or more.

[0073] According to one embodiment of the present invention, the aerogel composite has a high frequency average sound absorption coefficient, which is an average value of the sound absorption coefficients by frequency calculated by converting the sound absorption coefficient measured in the frequency range of 2,500 Hz to 6,400 Hz using Impedance Tube P-S40-20 into data in 1 / 3 octave bands, of 0.35 or more, 0.44 or more, or 0.48 or more, and may be 1.00 or less, 0.95 or less, 0.90 or less, 0.85 or less, or 0.82 or less. In addition, in order to ensure sound absorption performance in the high frequency range, the aerogel composite may have the high frequency average sound absorption coefficient of 0.53 or more, 0.60 or more, 0.65 or more, or 0.69 or more.

[0074] According to one embodiment of the present invention, the aerogel composite has excellent sound absorbing properties as well as excellent heat insulating properties, and the room temperature thermal conductivity may be 30.0 mW / mK or less, 1.0 mW / mK to 30.0 mW / mK, 10.0 mW / mK to 29.0 mW / mK, or 18.3 mW / mK to 28.8 mW / mK. It is considered that the heat insulating performance is sufficiently ensured within this range.

[0075] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0076] Working Example Example 1 A silica precursor composition was prepared by adding prehydrolyzed TEOS (silica content: 20 wt%, HTEOS), ethanol and distilled water in a weight ratio of 1:0.9:0.22 to a reactor and mixing them. Here, the silica concentration in the silica precursor composition was 40 kg / m 3 At the same time, ethanol, ammonia water (concentration: 30 wt%) and trimethylethoxysilane (TMES) were added to another reactor in a weight ratio of 1:0.054:0.154 and mixed to prepare a catalyst composition. The prepared silica precursor composition and catalyst composition were mixed in a volume ratio of 1:1 to prepare a catalyzed silica sol.

[0077] Next, a glass fiber mat (manufactured by Hyundai Fiber) containing pores with a pore size of 100 μm to 1,000 μm was placed in the reaction vessel, and the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 0.3:1 (catalyzed silica sol:glass fiber mat) relative to the volume of the glass fiber mat. After 10 minutes, the mixture was gelled to produce a wet gel composite. The gelled wet gel composite was then left to mature in a chamber at 70°C for 24 hours. The wet gel composite that had completed the aging process was placed in a 7.2 L supercritical extractor and carbon dioxide (CO 2 ) was injected into the separator. Next, the temperature inside the extractor was raised to 75°C, and when it reached 75°C and 150 bar, carbon dioxide was injected and discharged at a rate of 0.5 L / min for 20 minutes, and the process of stopping the injection of carbon dioxide for 20 minutes was repeated four times. During the injection and discharge of carbon dioxide, ethanol was collected through the bottom end of the separator. Next, carbon dioxide was vented for 2 hours. After the supercritical drying was completed, a completely dried aerogel composite was obtained.

[0078] Example 2 The same procedure as in Example 1 was repeated, except that the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 0.7:1 (catalyzed silica sol:glass fiber mat) and gelled after 10 minutes to prepare a wet gel composite.

[0079] Example 3 The same procedure as in Example 1 was repeated, except that the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 1:1 (catalyzed silica sol:glass fiber mat) and gelled after 10 minutes to prepare a wet gel composite.

[0080] Example 4 In the above Example 1, when the silica precursor composition was prepared, the silica concentration in the silica precursor composition was 50 kg / m 3 The same procedure as in Example 1 was carried out, except that the weight ratio of prehydrolyzed TEOS (silica content: 20 wt %, HTEOS), ethanol, and distilled water in the reactor was adjusted to prepare a silica precursor composition.

[0081] Example 5 The same procedure as in Example 4 was repeated, except that the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 0.7:1 (catalyzed silica sol:glass fiber mat) and gelled after 10 minutes to prepare a wet gel composite.

[0082] Example 6 The same procedure as in Example 4 was repeated, except that the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 1:1 (catalyzed silica sol:glass fiber mat) and gelled after 10 minutes to prepare a wet gel composite.

[0083] Example 7 In Example 1, when the silica precursor composition was prepared, the silica concentration in the silica precursor composition was 70 kg / m 3The same procedure as in Example 1 was carried out, except that the weight ratio of prehydrolyzed TEOS (silica content: 20 wt %, HTEOS), ethanol, and distilled water in the reactor was adjusted to prepare a silica precursor composition.

[0084] Example 8 The same procedure as in Example 7 was carried out, except that the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 0.7:1 (catalyzed silica sol:glass fiber mat) and gelled after 10 minutes to prepare a wet gel composite.

[0085] Example 9 The same procedure as in Example 7 was carried out, except that the catalyzed silica sol was impregnated into the glass fiber mat at a volume ratio of 1:1 (catalyzed silica sol:glass fiber mat) and gelled after 10 minutes to prepare a wet gel composite.

[0086] Comparative Example 1 A glass fiber mat (manufactured by Hyundai Fiber Co., Ltd.) containing pores with pore diameters of 100 μm to 1,000 μm was used as is.

[0087] Experimental Example The sound absorption coefficients at different frequencies, the average sound absorption coefficients, and the room temperature thermal conductivities of the aerogel composites or glass fiber mats prepared in Examples 1 to 9 and Comparative Example 1 were measured and are shown in Table 1 below.

[0088] *Sound absorption coefficient and average sound absorption coefficient by frequency: The aerogel composite was cut into 30cm x 30cm pieces to prepare test pieces, and the sound absorption coefficient measured in the frequency range of 50Hz to 6,400Hz was converted into data in 1 / 3 octave bands using an Impedance Tube P-S40-20 manufactured by Bruel & Kjaer to calculate the sound absorption coefficient by frequency. From this, the overall average sound absorption coefficient for the overall average value and the high frequency average sound absorption coefficient for the average value in the high frequency range (2,500Hz to 6,300Hz) were calculated.

[0089] In addition, the calculated sound absorption coefficients for each frequency for the aerogel composites prepared in Examples 1 to 3 and the glass fiber mat of Comparative Example 1 were graphed and shown in FIG.

[0090] *Thermal conductivity (mW / mK) at room temperature (23±5°C): The aerogel composite or glass fiber mat was cut into 30cm x 30cm pieces to prepare test pieces, and the thermal conductivity at room temperature (23±5°C) was measured using a NETZSCH HFM 436 Lambda instrument.

[0091] [Table 1]

[0092] As shown in Table 1 and FIG. 1, the aerogel composites of Examples 1 to 9 prepared according to the present invention have higher overall average sound absorption coefficients and improved sound absorption performance, and have lower room temperature thermal conductivity and excellent heat insulation performance, compared to the glass fiber mat of Comparative Example 1.

[0093] In particular, in the case of Examples 1, 2, 4, 5, 7, and 8, which were produced by impregnating a fiber mat with catalyzed silica sol at a volume ratio of 0.3:1 and 0.7:1 (catalyzed silica sol:fiber mat) and gelling during the production of the aerogel composite, it was confirmed that sufficient insulation performance was ensured compared to Comparative Example 1, and that the sound absorption coefficients for each frequency in the high frequency range and the average sound absorption coefficient at high frequencies were all improved compared to Examples 3, 6, and 9, which had the same silica concentration as each Example and were produced by impregnating a fiber mat with catalyzed silica sol at a volume ratio of 1:1 (catalyzed silica sol:fiber mat) and gelling.

[0094] From these results, it was confirmed that when an aerogel composite is produced by the production method of the aerogel composite of the present invention, the macropores of the fiber mat are reduced and the mesopores are increased, thereby improving the sound absorption coefficient and heat insulation performance. As a result, it was confirmed that the aerogel composite of the present invention has excellent sound absorption performance and heat insulation performance and is useful as a sound absorbing material.

Claims

1. A method for producing an aerogel composite, comprising: impregnating a fiber mat with a catalyzed silica sol in a volume ratio (catalyzed silica sol:fiber mat) of 0.1 to 0.8:1, and gelling the fiber mat (S10).

2. The catalyzed silica sol is A step (S1) of preparing a silica precursor composition by mixing a silica precursor, an organic solvent and an aqueous solvent; (S2) mixing an organic solvent, a base catalyst and a hydrophobizing agent to prepare a catalyst composition; and (S3) mixing the silica precursor composition and the catalyst composition to produce a catalyzed silica sol.

3. The silica concentration of the silica precursor composition produced in the step (S1) is 10 kg / m 3 ~100kg / m 3 The method for producing an aerogel composite according to claim 2,

4. The silica concentration of the silica precursor composition produced in the step (S1) is 40 kg / m 3 ~70kg / m 3 The method for producing an aerogel composite according to claim 2 or 3,

5. The method for producing the aerogel composite includes: A step (S20) of aging the wet-gel composite gelled in the step (S10); The method for producing an aerogel composite according to any one of claims 1 to 4, further comprising: (S30) drying the wet gel composite aged in the (S20) step to obtain an aerogel composite.

6. The method for producing an aerogel composite according to claim 5, wherein the aerogel composite obtained in the step (S30) includes pores having a pore diameter of 2 nm to 50 nm.

7. The method for producing an aerogel composite according to any one of claims 1 to 6, wherein the fiber mat is a glass fiber mat.

8. The method for producing an aerogel composite according to any one of claims 1 to 7, wherein the fiber mat contains pores having a pore diameter of 100 μm to 1,000 μm.

9. A fiber mat and a silica aerogel formed inside and on a surface of the fiber mat, The overall average sound absorption coefficient, which is the average value of the sound absorption coefficients by frequency calculated by converting the sound absorption coefficients measured in the frequency range of 50 Hz to 6,400 Hz into data in 1 / 3 octave bands, is 0.41 or more; An aerogel composite having a high frequency average sound absorption coefficient of 0.44 or more, which is the average value of the sound absorption coefficients by frequency calculated by converting the sound absorption coefficients measured in the frequency range of 2,500 Hz to 6,400 Hz into data in 1 / 3 octave bands. (However, this does not include cases where the aerogel composite has a laminated structure of three or more layers in which three layers made of two components, fiber and nano-sized porous body, are bonded together.)

10. The aerogel composite according to claim 9, wherein the aerogel composite has a room temperature thermal conductivity of 30.0 mW / mK or less.

Citation Information

Patent Citations

  • Composite material and method of producing the same

    JP2018140554A

  • Sound absorption sheet wiht excellent acoustic absorption

    KR101391098B1

  • Method for preparing high-insulation aerogel-impregnated fiber

    KR1020110082379A

  • Method of manufacturing aerogel blanket and aerogel and produced aerogel blanket

    KR1020190063799A

  • Aerogel blanket

    KR1020210028082A