toner
The toner formulation with silica fine particles A addresses the challenge of high image quality and dot reproducibility by enhancing charge uniformity and transferability, ensuring stable image output in electrophotographic processes.
Patent Information
- Application Number
- JP2020179898
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Existing toners used in electrophotographic processes face challenges in achieving high image quality and dot reproducibility, particularly in the context of the print on demand (POD) market, despite improvements in transferability.
A toner formulation with silica fine particles A attached to the surface of toner particles, containing iron atoms at 20-2000 ppm, primary particles of 80-200 nm, and a coverage ratio of 31.0%-70.0%, which enhances charge uniformity and reduces non-electrostatic adhesion.
The toner achieves excellent transferability and good dot reproducibility by improving charge uniformity and maintaining charge retention over time, while minimizing uneven charge distribution and fogging.
Smart Images

Figure 0007562370000005 
Figure 0007562370000001 
Figure 0007562370000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing electrostatic images used in electrophotography, electrostatic recording and the like. [Background technology]
[0002] 2. Description of the Related Art In recent years, as full-color electrophotographic copying machines have come into widespread use, there has been a demand for even higher image quality as well as the ability to stably output high-quality images even during long-term use.
[0003] In order to achieve high image quality, it is essential to obtain high image reproducibility in processes such as development, transfer, and fixing. For example, in the transfer process, high image reproducibility can be obtained by efficiently transferring the toner developed on the electrostatic latent image carrier onto the intermediate transfer body or media.
[0004] To obtain high transferability, the force of the electric field that each toner particle receives from the transfer bias must be greater than the adhesive force between the toner and the electrostatic latent image carrier. Adhesion forces are broadly divided into non-electrostatic adhesive forces, such as van der Waals forces, and electrostatic adhesive forces, such as electrostatic image forces.
[0005] Patent Document 1 reports a method for reducing non-electrostatic adhesion by coating toner particles with silica fine particles having a large particle size in order to improve transferability. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-332253 Summary of the Invention [Problem to be solved by the invention]
[0007] The technology described in Patent Document 1 has improved transferability from the perspective of high image quality. However, there is still room for improvement in dot reproducibility in terms of achieving high image quality that meets the needs of the print-on-demand (POD) market.
[0008] It is therefore an object of the present invention to provide a toner that exhibits excellent transferability and good dot reproducibility. [Means for solving the problem]
[0009] The toner according to the present invention is A toner having toner particles and silica fine particles A, the toner particles containing a binder resin, the silica fine particles A being attached or fixed to the surfaces of the toner particles, The silica fine particles A contain iron atoms at a concentration of 20 ppm or more and 2000 ppm or less, The primary particles of the silica fine particles A have a number average particle size of 80 nm or more and 200 nm or less, The toner particles are covered with the fine silica particles A at a rate of 31.0% or more and 70.0% or less. Effect of the Invention
[0010] According to the present invention, it is possible to provide a toner that exhibits excellent transferability and good dot reproducibility. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram of a surface treatment device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In the present invention, the expressions "xx or more and xx or less" and "xx to xx" expressing a numerical range mean a numerical range including the lower and upper limit endpoints, unless otherwise specified.
[0013] The toner according to the present invention is a toner having toner particles and silica fine particles A, wherein the toner particles contain a binder resin, the silica fine particles A are present by adhering or fixing to the surfaces of the toner particles, the silica fine particles A contain iron atoms at a concentration of 20 ppm or more and 2000 ppm or less, primary particles of the silica fine particles A have a number-average particle diameter of 80 nm or more and 200 nm or less, and the coverage rate of the toner particles by the silica fine particles A is 31.0% or more and 70.0% or less.
[0014] By using the toner according to the present invention, it is possible to obtain the effect of improving dot reproducibility in addition to excellent transferability.
[0015] The reason why the toner according to the present invention exhibits an improved effect in dot reproducibility is believed to be as follows. In order to improve dot reproducibility, it is necessary to further improve the developability of the toner, and for this purpose, uniformity of charge on the surface layer of the toner particles is important. In toner obtained by externally adding silica fine particles to toner particles, the distribution of the silica fine particles on the surface layer of the toner particles may be uneven. In particular, when the amount of silica fine particles added is relatively large and the coverage rate of the toner particles with silica fine particles exceeds 30%, it is difficult to uniformize the distribution of the silica fine particles. When the distribution of the silica fine particles is uneven, there are sparse areas with high and low charge. Since silica fine particles have high electrical resistance, the uneven distribution of silica fine particles tends to cause the charge distribution to be uneven, and the toner image may be slightly disturbed relative to the latent image, which may affect dot reproducibility.
[0016] In the present invention, the silica fine particles A on the surface of the toner particles contain iron atoms at a concentration of 20 ppm or more and 2000 ppm or less. When the silica fine particles A contain iron atoms at a concentration within the above range, the effect of accelerating the movement of charges in the silica fine particles A can be obtained. Therefore, the effect of releasing and mitigating the charges at the highly charged sites of the silica fine particles A on the surface layer of the toner particles can be obtained. As a result, the charging uniformity on the surface layer of the toner particles is improved, and dot reproducibility is improved.
[0017] By containing iron atoms in a concentration of 20 ppm or more in the silica fine particles A, it becomes possible for the silica fine particles A to fully exhibit the effect of promoting the transfer of charges. Furthermore, by containing iron atoms in a concentration of 2000 ppm or less in the silica fine particles A, leakage of toner charge caused by excessively high electrical conductivity can be suppressed, and problems such as fogging can be prevented.
[0018] In the toner according to the present invention, the primary particles of the silica fine particles A have a number-average particle size of 80 nm or more, so that even when the toner is used for a long period of time, the silica fine particles A are not embedded in the toner particles, and a high spacer effect and charge retention can be obtained for a long period of time. Furthermore, since the primary particles of the silica fine particles A have a number-average particle size of 200 nm or less, even when the toner is used for a long period of time, the silica fine particles A can be prevented from migrating from the toner particles to the carrier or components inside the developing device due to the mechanical load inside the developing device. Therefore, even when the toner is used for a long period of time, a high spacer effect and charge retention can be obtained for a long period of time.
[0019] In the toner according to the present invention, when the coverage of the toner particles with the fine silica particles A is 31.0% or more, the non-electrostatic adhesion of the toner can be sufficiently reduced, and high transferability can be obtained. In addition, by ensuring that the coverage rate of the toner particles with silica fine particles A is 70.0% or less, localized bias in the distribution of silica fine particles A on the surface of the toner particles is prevented from becoming too large, and areas of the toner particles that are locally highly charged are less likely to occur.
[0020] The toner according to the present invention has silica particles A having the above-mentioned characteristics on the surface of the toner particles, and therefore the charge leveling effect of the silica particles A can be sufficiently obtained. As a result, the charge uniformity on the surface layer of the toner particles is improved, and the dot reproducibility is improved.
[0021] Furthermore, the content of the silica fine particles A in the toner according to the present invention is preferably 2.1% by mass or more and 7.0% by mass or less based on the mass of the toner, from the viewpoint of improving the charging uniformity on the surface layer of the toner particles.
[0022] Furthermore, the adhesion rate of the silica fine particles A in the toner according to the present invention is preferably from 50% by mass to 90% by mass from the viewpoint of long-term stability of transferability and dot reproducibility.
[0023] Furthermore, in the toner according to the present invention, from the viewpoint of promoting charge transfer in the silica fine particles A, the silica fine particles A preferably contain aluminum atoms at a concentration of 200 ppm or more and 2000 ppm or less.
[0024] Next, preferred embodiments will be described. <Silica fine particles A> The silica fine particles A are particles mainly composed of silica (i.e., SiO2), and can be produced by known production methods such as a combustion method, a melting method, and hydrothermal synthesis. Among them, silica fine particles A produced by the combustion method or the melting method are preferred from the viewpoint of further enhancing the effect of reducing electrostatic charge in a high-temperature and high-humidity environment, and from the viewpoint of having high resistance and being less susceptible to the effects of humidity.
[0025] The combustion method is a method in which siloxane gas is produced by vaporizing siloxane compound, and introduced into a burner together with a carrier gas such as nitrogen, and the siloxane gas is diffused and mixed with a combustion-supporting gas such as oxygen, and then combusted to produce silica fine particles.Another combustion method is a method in which silicon tetrachloride is combusted at high temperature together with a mixed gas of oxygen, hydrogen, and a dilution gas such as nitrogen, to produce silica fine particles (fumed silica).
[0026] The melting method is a method in which a slurry of metal silicon particles is sprayed into a flame to cause an oxidation reaction and to form the particles into spheroids, thereby obtaining silica particles.
[0027] In the present invention, from the viewpoint of controlling the number average particle size of the primary particles of the silica microparticles A to a desired value and from the viewpoint of containing iron atoms, a combustion method in which siloxane gas is combusted to produce silica microparticles is cited as a preferred example.
[0028] Examples of the siloxane compound include hexamethylcyclotrisiloxane and octamethylcyclotetrasiloxane.
[0029] In the present invention, the silica fine particles A used in the present invention can be obtained by incorporating iron atoms, and preferably further aluminum atoms, into the silica fine particles A. As a method for incorporating these metal atoms into the silica fine particles A, the purity of a siloxane compound can be adjusted and incorporated.
[0030] Furthermore, the silica fine particles A are preferably surface-treated to be hydrophobic with a silane coupling agent, silicone oil, etc. As the silane coupling agent, hexamethyldisilazane (HMDS) is preferably used. As the silicone oil, dimethylsilicone oil is preferably used.
[0031] The method of surface treatment with a silane coupling agent is not particularly limited, and a known method can be used. For example, a method of spraying or vaporizing a vaporized silane coupling agent onto a cloud of silica fine particles A by stirring the silica fine particles A is generally and preferably used.
[0032] The silane coupling agent is preferably used for surface treatment in an amount ranging from 1 part by weight to 80 parts by weight per 100 parts by weight of the silica fine particles A.
[0033] The method of surface treatment with silicone oil is not particularly limited, and known methods can be used.For example, the method of directly mixing the silica fine particles A treated with organosilicon compound with silicone oil using a mixer such as FM mixer, or the method of spraying silicone oil onto silica fine particles A.Alternatively, the method of dissolving or dispersing silicone oil in a suitable solvent, adding silica fine particles A and mixing, and removing the solvent may be used.
[0034] The silicone oil is preferably used for surface treatment in an amount ranging from 1 part by mass to 40 parts by mass per 100 parts by weight of the silica fine particles A.
[0035] In the toner according to the present invention, the silica fine particles A may be used alone as an external additive, or the silica fine particles A may be used in combination with one or more types of other external additives.
[0036] <Other external additives> The toner according to the present invention may contain an external additive other than the silica fine particles A in order to improve the fluidity of the toner and adjust the amount of triboelectric charge.
[0037] Examples of external additives other than the silica fine particles A include resin fine particles and inorganic fine particles that act as charge assistants, conductivity imparting agents, fluidity imparting agents, caking prevention agents, release agents during heat roller fixing, lubricants, and abrasives. Examples of lubricants include polyfluoroethylene fine particles, zinc stearate fine particles, and polyvinylidene fluoride fine particles. Examples of abrasives include cerium oxide fine particles, silicon carbide fine particles, and strontium titanate fine particles. In the present invention, the external additive other than the silica fine particles A is preferably inorganic fine particles such as aluminum oxide (alumina), strontium titanate, titanium oxide (titania), and calcium carbonate.
[0038] <Binding resin> In the toner particles of the present invention, the following polymers can be used as the binder resin. Examples of suitable resins include homopolymers of styrene and its substituted derivatives, such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-based copolymers, such as styrene-p-chlorostyrene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-acrylic acid ester copolymer, and styrene-methacrylic acid ester copolymer; styrene-based copolymer resins, polyester resins, and hybrid resins in which polyester resins and vinyl resins are mixed or in which the two are partially reacted; polyvinyl chloride, phenolic resins, naturally modified phenolic resins, naturally modified maleic acid resins, acrylic resins, methacrylic resins, polyvinyl acetate, silicone resins, polyester resins, polyurethanes, polyamide resins, furan resins, epoxy resins, xylene resins, polyethylene resins, and polypropylene resins. Among these, it is preferable to use a polyester resin as the binder resin from the viewpoint of the low-temperature fixability and chargeability of the toner.
[0039] <Wax> The toner particles in the present invention may contain wax. Examples of the wax include the following. Hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or their block copolymers; waxes whose main component is fatty acid esters such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax. Among these, from the viewpoints of low-temperature fixing property and hot offset resistance of the toner, hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax, and fatty acid ester waxes such as carnauba wax are preferred.
[0040] The content of the wax in the toner particles is preferably 1.0 part by mass or more and 20.0 parts by mass or less with respect to 100 parts by mass of the binder resin in the toner particles.
[0041] <Coloring agent> The toner particles in the present invention may contain a colorant, such as a known yellow colorant, magenta colorant, cyan colorant, or black colorant. Examples of black colorants include carbon black, and colorants toned to black using a yellow colorant, a magenta colorant, and a cyan colorant. As the colorant, a pigment or a dye may be used alone, or a dye and a pigment may be used in combination. The content of the colorant in the toner particles is preferably 0.1 parts by mass or more and 30.0 parts by mass or less with respect to 100 parts by mass of the binder resin in the toner particles.
[0042] <Developer> The toner of the present invention can be used as a one-component developer, but in order to suppress localization of charge on the surface of the toner particles, the toner can also be mixed with a magnetic carrier and used as a two-component developer. Examples of magnetic carriers that can be used include the following: iron oxide; metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, and rare earth elements, alloy particles thereof, and oxide particles thereof; magnetic materials such as ferrite; and magnetic material-dispersed resin carriers (so-called resin carriers) that contain a magnetic material and a binder resin that holds the magnetic material in a dispersed state. When the toner is mixed with a magnetic carrier to be used as a two-component developer, the content of the magnetic carrier in the two-component developer is preferably 85% by mass or more and 98% by mass or less, and more preferably 87% by mass or more and 96% by mass or less, based on the total mass of the two-component developer.
[0043] <Toner manufacturing method> The method for producing the toner particles is not particularly limited, but a pulverization method is preferred from the viewpoint of dispersion of the toner materials such as pigments.
[0044] The procedure for producing the toner by the pulverization method will be described below. In the raw material mixing step, materials constituting the toner particles, such as a binder resin, a release agent, a colorant, and optionally other components such as a charge control agent, are weighed out in predetermined amounts, blended, and mixed.
[0045] Examples of the mixing device include a double cone mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, and a Mechano Hybrid (manufactured by Nippon Coke and Engineering Co., Ltd.).
[0046] Next, the mixed materials are melt-kneaded to disperse the pigment in the binder resin. In the melt-kneading process, a batch kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of continuous production. For example, a KTK twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Iron Works), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. Furthermore, the resin composition obtained by melt-kneading may be rolled with two rolls or the like and cooled with water or the like in a cooling process.
[0047] The cooled resin composition is then pulverized to a desired particle size in a pulverization step, for example, by coarse pulverization using a pulverizer such as a crusher, a hammer mill, or a feather mill, and then further pulverized in a fine pulverizer. Thereafter, the mixture is classified using a classifier or a sieve, if necessary.
[0048] The resin composition after pulverization or classification may be surface-treated, for example, using a surface treatment device shown in Fig. 1. The surface treatment using the surface treatment device shown in Fig. 1 will be described below.
[0049] The mixture supplied by the raw material constant-quantity supply means 1 is introduced into an introduction pipe 3, which is installed on the extension line of the raw material constant-quantity supply means 1, by compressed gas adjusted by a compressed gas flow rate adjustment means 2. The mixture passing through the introduction pipe 3 is uniformly dispersed by a conical protruding member 4 provided in the center of the introduction pipe 3, and is introduced into eight supply pipes 5 that radiate outward, and is introduced into a treatment chamber 6 where heat treatment is carried out.
[0050] At this time, the flow of the mixture supplied to the processing chamber 6 is regulated by a regulating means 9 for regulating the flow of the mixture provided in the processing chamber 6. Therefore, the mixture supplied to the processing chamber is heat-treated while swirling in the processing chamber 6, and then cooled.
[0051] Heat for heat-treating the supplied mixture is supplied from hot air supplying means 7, distributed by distribution member 12, and introduced into treatment chamber 6 by swirling member 13 for swirling the hot air in a spiral shape. In terms of configuration, swirling member 13 for swirling the hot air has multiple blades, and the swirling of the hot air can be controlled by the number and angle of the blades. Hot air is supplied from hot air supplying means outlet 11.
[0052] The heat-treated toner particles are cooled by cold air supplied from cold air supplying means 8 (cold air supplying means 8-1, cold air supplying means 8-2, and cold air supplying means 8-3).
[0053] Next, the cooled toner particles are collected by the collecting means 10 at the bottom end of the processing chamber. A blower (not shown) is provided ahead of the collecting means, so that the toner particles are sucked and transported by the blower.
[0054] The powder particle supply port 14 is provided so that the swirling direction of the supplied mixture and the swirling direction of the hot air are the same, and the recovery means 10 of the thermal sphering treatment device is provided on the outer periphery of the treatment chamber so as to maintain the swirling direction of the swirled powder particles. Furthermore, the cold air supplied from the cold air supply means 8 is configured to be supplied horizontally and tangentially from the outer periphery of the device to the circumferential surface inside the treatment chamber.
[0055] Next, the resin composition is divided into a fine powder portion and a coarse powder portion. For example, the resin composition is divided into two portions using an inertial classification system, Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.). A desired amount of an external additive is added to the surface of each of the two heat-treated toner particles. As a method for adding an external additive, a method of stirring and mixing using the following mixer as an external adder can be mentioned. Mixing equipment: Double Cone Mixer, V-type Mixer, Drum Type Mixer, Super Mixer, Henschel Mixer, Nauta Mixer, Mechano Hybrid (manufactured by Nippon Coke & Co., Ltd.), Nobilta (manufactured by Hosokawa Micron Corporation), etc. In this case, if necessary, an external additive such as a fluidizing agent may be added to the mixture.
[0056] In the present invention, it is preferable that the silica fine particles A are added to the outside before the above-mentioned surface treatment by heating (heat treatment), and then embedded in the surface of the toner particles by heat treatment, which improves the adhesion rate of the silica fine particles A in the toner, and makes it easy to adjust the adhesion rate to a preferred range of 50% by mass to 90% by mass.
[0057] It is also preferable to carry out a surface treatment after externally adding silica fine particles A, and then to further externally add silica fine particles A. This improves the uniformity of the surface charge density when the toner is charged, and further improves the transferability and dot reproducibility.
[0058] Various measurement methods will be described below. <Water washing method> Silica fine particles A are extracted from the toner by a water washing process. Specifically, a sucrose aqueous solution prepared by dissolving 31.1 g of sucrose (Kishida Chemical Co., Ltd.) in 10.3 g of ion-exchanged water is added to 6 mL of Contaminon N in a 30 mL glass vial and thoroughly mixed to prepare a dispersion. Contaminon N: A neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder; manufactured by Wako Pure Chemical Industries, Ltd. Glass vial: Nichiden Rika Glass Co., Ltd., VCV-30, outer diameter 35 mm, height 70 mm 1.0 g of toner is added to this glass vial, and the toner is left to stand until it settles naturally to prepare a pre-treatment dispersion. This dispersion is shaken for 5 minutes at a shaking speed of 200 rpm in a shaker (YS-8D type: manufactured by Yayoi Co., Ltd.) to separate the silica fine particles A from the surface of the toner particles. A centrifuge is used to separate the toner particles from the silica fine particles A that have been detached from the surface of the toner particles. The centrifugation process is carried out at 3700 rpm for 30 minutes. The silica fine particles A that have been detached from the surface of the toner particles and the toner are each collected by suction filtration, and dried to obtain the silica fine particles A and the toner after washing with water.
[0059] <Method for measuring the content of metal elements in silica fine particles A> The silica fine particles A obtained by repeatedly performing the above water washing treatment are subjected to fluorescent X-ray measurement, and the contents of iron atoms and aluminum atoms are calculated. The X-ray fluorescence measurement of each element conforms to JIS K 0119-1969, and specifically, is as follows. As a measuring device, for example, a wavelength dispersive X-ray fluorescence analyzer "Axios" (manufactured by PANalytical) is used. 2 g of sample is weighed into a cup for powder measurement recommended by PANalytical with a dedicated PP (polypropylene) film attached to the bottom, a layer of uniform thickness is formed on the bottom, and the lid is placed. Next, elements from Na to U in the silica particles are measured using the FP method under atmospheric pressure He atmosphere. At this time, it is assumed that all detected elements are oxides, and their total mass is set to 100%, and the content (mass%) of Fe2O3 and Al2O3 relative to the total mass is calculated as oxide equivalent values using the software SpectraEvaluation (version 5.0L).
[0060] <Method for measuring the number average particle size of primary particles of silica fine particles A> The number average particle diameter of the primary particles of silica fine particles A can be calculated from an image of the surface of the toner particles of silica fine particles A taken with a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation). The image taking conditions for the S-4800 are as follows.
[0061] (1) Sample preparation Apply a thin layer of conductive paste to a sample stage (aluminum sample stage 15 mm x 6 mm) and spray toner onto it. Then use air to remove excess toner from the sample stage and dry thoroughly. Set the sample stage in the sample holder and adjust the sample stage height to 36 mm using the sample height gauge.
[0062] (2) S-4800 observation condition setting The number average particle size is calculated using images obtained by backscattered electron image observation with the S-4800. Backscattered electron images have less charge-up of particles than secondary electron images, so particle size can be measured with high accuracy.
[0063] Pour liquid nitrogen into the anti-contamination trap attached to the S-4800 body until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2, and execute it. Check that the emission current due to flushing is 20-40 μA. Insert the specimen holder into the specimen chamber of the S-4800 body. Press [Origin] on the control panel to move the specimen holder to the observation position.
[0064] Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [1.1kV] and the emission current to [20μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Upper (U)] and [+BSE], and select [LA100] in the selection box to the right of [+BSE] to set the mode to observation with backscattered electron images. In the same [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [4.5mm]. Press the [ON] button in the accelerating voltage display of the control panel to apply the accelerating voltage.
[0065] (3) Focus adjustment Rotate the focus knob [COARSE] on the operation panel, and adjust the aperture alignment once the image is in focus to a certain extent. Click [Align] on the control panel to display the alignment dialog and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles. Next, select [Aperture] and rotate the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or to minimize its movement. Close the aperture dialog and adjust the focus using autofocus. After that, set the magnification to 80,000 (80k)x, adjust the focus using the focus knob and STIGMA / ALIGNMENT knob as above, and then adjust the focus using autofocus again. Repeat this operation to adjust the focus. Here, if the inclination angle of the observation surface is large, the measurement accuracy of the coverage rate is likely to be low, so when adjusting the focus, select an observation surface with as little surface inclination as possible for analysis by selecting one that can simultaneously bring the entire observation surface into focus.
[0066] (4) Image storage Adjust the brightness in ABC mode, take a photo with a size of 640 x 480 pixels, and save it. Use this image file to perform the following analysis. Take one photo for each toner particle, and obtain images of at least 25 toner particles.
[0067] (5) Image analysis The particle diameters of at least 300 silica fine particles A on the surface of the toner particle are measured to determine the number average particle diameter. In the present invention, the number average particle diameter can be calculated by binarizing the image obtained by the above-mentioned method using image analysis software Image-Pro Plus ver.5.0.
[0068] <Coverage of silica particles A> Twenty toner surface images taken with a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation) were randomly sampled. The image information is binarized using the image analysis software Image-Pro Plus ver.5.0 (Nippon Roper Co., Ltd.) by utilizing the difference in brightness between the toner particle surface and the silica fine particle A part. This binarization separates the area of the silica fine particle A part, SSiO2, from the area of the toner particle part (including the area of the silica fine particle A part), SToner. The coverage (%) of the toner particles with the fine silica particles A, σSiO2, is calculated by the following formula. σSiO2(%)=SSiO2 / SToner×100
[0069] <Method for measuring the content of silica fine particles A in toner> The toner is subjected to fluorescent X-ray measurement, and the content of silica fine particles A is calculated. The measurement of fluorescent X-rays for each element conforms to JIS K 0119-1969, and specifically, is as follows. For the measurements, a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data are used. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. A proportional counter (PC) is also used for the measurements. The measurement sample is prepared by placing about 4 g of toner in a dedicated aluminum ring for pressing, flattening it, and pressing it at 20 MPa for 60 seconds using a tablet press to form pellets with a thickness of about 2 mm and a diameter of about 39 mm. The tablet press used is the tablet press "BRE-32" (manufactured by Maekawa Test Machine Co., Ltd.). Measurement is carried out under the above conditions, the silicon element is identified based on the peak position of the obtained X-rays, and the content of silica fine particles A is calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time.
[0070] <Method for measuring adhesion rate of silica fine particles A in toner> The toner before and after the above water washing treatment is subjected to fluorescent X-ray measurement, and the adhesion rate of the silica fine particles A in the toner is calculated. First, the amount of silica particles A contained in the toner before the above-mentioned washing process is quantified. In the quantification of silica particles A, the silicon element strength in the toner is measured using a wavelength dispersive X-ray fluorescence analyzer Axios advanced (manufactured by PANalytical). Next, the silicon element strength of the toner after the above-mentioned washing process is measured in the same manner. The adhesion rate is calculated by (silicon element strength of toner after washing / silicon element strength in toner)×100(%).
[0071] <Method of measuring weight average particle size (D4) of toner particles> The weight average particle diameter (D4) of the toner particles can be calculated by measuring with an effective measurement channel count of 25,000 channels using the following device and software, and analyzing the measurement data. - "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.) is a precision particle size distribution measuring device using the narrow hole electrical resistance method with a 50 μm aperture tube. - Dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (Beckman Coulter, Inc.) included with the above device for setting measurement conditions and analyzing measurement data The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0072] Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 1 μm or more and 30 μm or less.
[0073] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the "Multisizer 3," set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube.
[0074] (2) About 30 mL of the electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant.
[0075] (3) Prepare an ultrasonic disperser "Ultrasonic Dispension System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase difference of 180 degrees and an electrical output of 120 W. Place a specified amount of ion-exchanged water in a water tank equipped with this ultrasonic disperser, and add about 2 mL of the above-mentioned Contaminon N to this water tank.
[0076] (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized.
[0077] (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower.
[0078] (6) Using a pipette, add the electrolyte solution (5) containing the toner dispersed therein to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000.
[0079] (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4). EXAMPLES
[0080] The present invention will be specifically described below based on Production Examples, Examples, and Comparative Examples. However, the present invention is not limited to these Examples. In addition, all parts are by weight unless otherwise specified.
[0081] <Production Example of Silica Fine Particle A1> Silica fine particles A1 were produced by a diffusion combustion method as follows. In producing silica microparticles A1, a double-tube hydrocarbon-oxygen mixed burner in which an inner flame and an outer flame are formed was used as the combustion furnace. This burner is configured so that a two-fluid nozzle for injecting slurry is grounded in the center of the burner, and the raw silicon compound is introduced. In addition, a flammable hydrocarbon-oxygen gas is injected from the periphery of the two-fluid nozzle, forming an inner flame and an outer flame, which are reducing atmospheres. The atmosphere, temperature, and flame length can be adjusted by controlling the amount and flow rate of the flammable gas and oxygen. In the flame, silica fine particles are generated from the raw silicon compound, and the silica fine particles can be fused until they reach a desired particle size. After that, they are cooled and the generated silica fine particles are collected by a bag filter or the like to obtain silica fine particles A having a desired particle size. As the raw silicon compound, a hexamethylcyclotrisiloxane compound containing 150 ppm of iron atoms and 500 ppm of aluminum atoms was used to produce silica fine particles A1. Next, 100 parts by mass of the obtained silica fine particles A were subjected to a surface treatment with 4% by mass of hexamethyldisilazane to obtain silica fine particles A1. The number average particle size of the primary particles of the obtained silica fine particles A1 is shown in Table 1. The iron content and aluminum content contained in the silica fine particles A1 are also shown in Table 1.
[0082] <Production Examples of Silica Particles A2 to A11> In the manufacturing example of silica fine particles A1, the number average particle diameter, iron atom concentration, and aluminum atom concentration of the primary particles were changed to obtain silica fine particles A2 to A11. The number average particle diameter, iron atom concentration, and aluminum atom concentration of the primary particles of each silica fine particle are shown in Table 1.
[0083] [Table 1]
[0084] <Production example of binder resin 1> The following materials were prepared: Polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 80.0 mol% based on the total number of moles of polyhydric alcohol Polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 20.0 mol% based on the total number of moles of polyhydric alcohol Terephthalic acid: 80.0 mol% based on the total number of moles of polycarboxylic acids Trimellitic anhydride: 20.0 mol% based on the total number of moles of polycarboxylic acids Titanium tetrabutoxide (esterification catalyst): 0.51 parts by mass These were put into a reaction vessel (flask) equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Then, 1.5 parts of tin 2-ethylhexanoate (esterification catalyst) was added as a catalyst to 100 parts of the total amount of monomers. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised while stirring, and the reaction was carried out for 2.5 hours while stirring at a temperature of 200°C. The pressure in the flask was then reduced to 8.3 kPa and maintained for 1 hour, after which the flask was cooled to 180°C and reacted as is. After confirming that the softening point, measured in accordance with ASTM D36-86, reached 110°C, the temperature was reduced to stop the reaction.
[0085] <Toner 1 Manufacturing Example> The following materials were prepared: Binding resin 1 100 parts Fischer-Tropsch wax (melting point: 90°C) 6 parts CI Pigment Blue 15:3 4 parts These were premixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.), and then melt-kneaded at 160° C. using a twin-screw kneading extruder (PCM-30, manufactured by Ikegai Co., Ltd.). The obtained kneaded product was cooled, coarsely pulverized to 1 mm or less using a hammer mill, and then finely pulverized using a mechanical pulverizer (T-250, manufactured by Turbo Kogyo Co., Ltd.). The resulting finely pulverized material was classified using a Faculty (F-300, manufactured by Hosokawa Micron Corp.) The operating conditions were a classifying rotor rotation speed of 11,000 rpm and a dispersing rotor rotation speed of 7,200 rpm. As a result, negatively triboelectrically charged toner particles 1 having a weight average particle size (D4) of 6.0 μm were obtained.
[0086] Next, 100 parts of toner particles 1 and 2.5 parts of silica fine particles A1 were mixed using a Henschel mixer (FM-10C type, manufactured by Nippon Coke Co., Ltd.) at a rotation speed of 2000 rpm for a rotation time of 2 min. Then, heat treatment was performed using the surface treatment device shown in FIG. 1 to obtain heat-treated toner base particles 1. The operating conditions of the surface treatment device were feed rate = 5 kg / hr, hot air temperature C = 160°C, and hot air flow rate = 6 m. 3 / min., cold air temperature E=-5℃, cold air flow rate=4m 3 / min., Blower air volume = 20m 3 / min., Injection air flow rate = 1m 3 / min. The obtained heat-treated toner base particles 1 were classified using an inertial classification system Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.) to obtain heat-treated toner base particles 1M. The obtained heat-treated toner base particles 1M had a weight average particle size (D4) of 5.5 μm.
[0087] Next, 100 parts of the heat-treated toner base particles 1M and 0.5 parts of strontium titanate particles (primary particles having a number-average diameter (D1) of 15 nm) were mixed using a Henschel mixer (FM-10C, manufactured by Nippon Coke Co., Ltd.). The mixing conditions were a rotation speed of 67 s -1 (4000 rpm) for 2 minutes. The mixture was then passed through an ultrasonic vibration sieve with 54 μm mesh to obtain Toner 1. The weight average particle size (D4) of Toner 1 was 5.5 μm. The coverage of Toner 1 with Silica Fine Particles A and the adhesion rate of Silica Fine Particles A in Toner 1 are shown in Table 2.
[0088] [Table 2]
[0089] <Production Example of Toners 2 to 4> Toners 2 to 4 were obtained in the same manner as in the production method of Toner 1, except that the type of silica fine particles A used was changed as shown in Table 2. The weight average particle size (D4) of Toners 2 to 4 was all 5.5 μm.
[0090] <Production Examples of Toners 5 and 6> Toners 5 and 6 were obtained in the same manner as in the manufacturing method of toner 4, except that the heat treatment temperature was changed as shown in Table 2. The weight average particle size (D4) of toner 5 was 5.2 μm, and the weight average particle size (D4) of toner 6 was 5.8 μm.
[0091] <Production Example of Toner 7> 100 parts of toner particles 1 and 2.5 parts of silica fine particles A4 were mixed using a Henschel mixer (FM-10C type, manufactured by Nippon Coke Co., Ltd.) at a rotation speed of 67 s-1 (4000 rpm) for a rotation time of 2 min. The mixture was then sieved through a mesh with an opening of 150 μm to obtain toner 7. The weight average particle size (D4) of toner 7 was 5.0 μm.
[0092] <Production Examples of Toners 8 to 17 and Comparative Toners 1 to 5> In the manufacturing method of toner 7, the type of silica fine particles A used and the amount of silica fine particles A added to toner particles 1 were changed as shown in Table 2. Otherwise, toners 8 to 17 and comparative toners 1 to 5 were obtained in the same manner as in the manufacturing method of toner 7. The weight average particle size (D4) of toners 8 to 17 and comparative toners 1 to 5 was all 5.0 μm.
[0093] Table 2 shows the coverage with the silica fine particles A and the adhesion rate of the silica fine particles A for the toners 2 to 17 and the comparative toners 1 to 5 produced as described above.
[0094] <Production Example of Magnetic Core Particle 1> The ferrite raw materials were weighed out so as to have the following composition ratio. ·Fe2O362.7 parts ·MnCO329.5 parts ·Mg(OH)26.8 parts ·SrCO31.0 parts The mixture was then ground and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch. The ground material was then made into pellets of approximately 1 mm square in a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder. Then, after passing through a vibrating sieve with 0.5 mm openings to remove fine powder, the pellets were fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the calcined ferrite obtained was as follows: (MnO) a (MgO) b (SrO) c (Fe2O3) d In the above formula, a = 0.257, b = 0.117, c = 0.007, d = 0.393
[0095] The calcined ferrite was crushed to about 0.3 mm using a crusher, and then 30 parts of water was added to 100 parts of the calcined ferrite using zirconia beads with a diameter of 1 / 8 inch, and the mixture was crushed in a wet ball mill for 1 hour. The resulting slurry was then crushed in a wet ball mill with alumina beads with a diameter of 1 / 16 inch for 4 hours to obtain a ferrite slurry (finely crushed calcined ferrite). To the ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 2.0 parts of polyvinyl alcohol as a binder were added per 100 parts of the calcined ferrite, and the mixture was granulated into spherical particles using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.) The particle size of the resulting particles was adjusted, and then the particles were heated at 650°C for 2 hours using a rotary kiln to remove the organic components of the dispersant and binder.
[0096] In order to control the firing atmosphere, the material was heated from room temperature to 1300° C. in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at a temperature of 1150° C. for 4 hours. The material was then cooled to 60° C. over a period of 4 hours, returned from the nitrogen atmosphere to the air, and removed at a temperature of 40° C. or less. After crushing the agglomerated particles, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic core particles 1 having a volume distribution standard 50% particle size (D50) of 37.0 μm.
[0097] <Preparation of resin solution 1> The following materials were prepared: Cyclohexyl methacrylate monomer 26.8% by mass Methyl methacrylate monomer 0.2% by mass Methyl methacrylate macromonomer 8.4% by mass (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene 31.3% by mass Methyl ethyl ketone 31.3% by mass Azobisisobutyronitrile 2.0% by mass Among the above materials, cyclohexyl methacrylate monomer, methyl methacrylate monomer, methyl methacrylate macromonomer, toluene, and methyl ethyl ketone were placed in the following device. The device was a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer. Nitrogen gas was then introduced to create a sufficient nitrogen atmosphere, and the mixture was heated to 80°C, azobisisobutyronitrile was added, and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction mixture to precipitate the copolymer. The resulting precipitate was filtered off and then dried in vacuum to obtain a resin. Next, 30 parts of the resin was dissolved in a mixed solvent of 40 parts of toluene and 30 parts of methyl ethyl ketone to obtain a resin solution 1 (solid content concentration: 30% by mass).
[0098] <Preparation of coating resin solution 1> The following materials were prepared: ·Resin solution 1 (resin solid content concentration 30%) 33.3% by mass Toluene 66.4% by mass Carbon black (Regal 330; Cabot Corporation) 0.3% by mass (Number average particle size of primary particles: 25 nm, Nitrogen adsorption specific surface area: 94 m 2 / g, DBP oil absorption: 75mL / 100g) These were placed in a paint shaker and dispersed for 1 hour using zirconia beads with a diameter of 0.5 mm. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.
[0099] <Magnetic Carrier 1 Manufacturing Example> Coating resin solution 1 and magnetic core particles 1 were added to a vacuum degassing kneader maintained at room temperature (the amount of coating resin solution 1 added was 2.5 parts as a resin component per 100 parts of magnetic core particles 1). After the addition, the mixture was stirred at a rotation speed of 30 rpm for 15 minutes. After a certain amount of the solvent (80% by mass) had evaporated, the mixture was heated to 80° C. while mixing under reduced pressure, and the toluene was distilled off over 2 hours, after which the mixture was cooled. The obtained magnetic carrier was subjected to magnetic separation to separate out low magnetic particles, which were passed through a sieve with 70 μm openings and then classified with an air classifier to obtain magnetic carrier 1 having a volume distribution standard 50% particle size (D50) of 38.2 μm.
[0100] <Production Examples of Developers 1 to 17 and Comparative Developers 1 to 5> Toners 1 to 17 and magnetic carrier 1 were mixed so that the amounts of toners 1 to 17 were 10 parts each for 90 parts of magnetic carrier 1. The mixing was carried out using a V-type mixer (V-10 type: Tokuju Seisakusho Co., Ltd.) at 0.5 s -1 The mixture was mixed under the conditions of 100 ml / min, 100 ml of water, and 5 min of rotation time. As a result, developers 1 to 17 and comparative developers 1 to 5 were obtained. Table 4 shows the correspondence between the toner used and the obtained developers.
[0101] [Table 4]
[0102] <Example 1> 13、15~ 17 , Reference example 1, and Comparative Examples 1 to 5> The above obtained developers 1 to 17 and comparative developers 1 to 5 were used to carry out the following evaluations. In the evaluation, a color copier imagePRESS C850 manufactured by Canon Inc. or a modified version thereof was used as the image forming apparatus. Each developer was put into the developing device of the cyan color station of the image forming apparatus, and the formed images were evaluated for fog, and the transferability and dot reproducibility were also evaluated before and after a paper feed durability test. To evaluate transferability and dot reproducibility, a paper-feed durability test was performed in a printing environment of 23°C temperature / 5% relative humidity (hereinafter referred to as "N / L" environment), in which 10,000 images were formed using a test chart with an image ratio of 5%.
[0103] Conditions for paper feed durability test to evaluate transferability and dot reproducibility: Paper: High white paper GF-C081 (81.4g / m 2 )(Canon Marketing Japan Inc.) Image forming speed: A4 size, full color 85 sheets / min Development conditions: The development contrast can now be adjusted to any value, and the automatic correction by the camera body has been prevented from operating.
[0104] In the evaluation of fogging, images were formed in a printing environment of 30° C. temperature / 80% relative humidity (hereinafter, “H / H” environment). Image formation conditions for fog evaluation: Paper: Bleached paper CS-068 (68.0g / m 2 )(Canon Marketing Japan Inc.) Image forming speed: A4 size, full color 85 sheets / min Development conditions: The development contrast can now be adjusted to any value, and the automatic correction by the camera body has been prevented from operating.
[0105] The evaluation method for each evaluation item is shown below. <Dot reproducibility> Before and after the paper feed durability test, the dot reproducibility was evaluated as follows. A halftone (30h) image was formed and evaluated based on the following criteria. It should be noted that a 30h image is a halftone image in which 256 gradations are expressed in hexadecimal, with 00h representing solid white (non-image) and FFh representing a solid image (full image). The images were taken using a digital microscope VHX-500 (lens wide range zoom lens VH-Z100 manufactured by Keyence Corporation), and the area of 1,000 dots was measured.
[0106] The number average (S) of the dot area and the standard deviation (σ) of the dot area were calculated, and the dot reproducibility index was calculated according to the following formula. Dot reproducibility index (I) = σ / S × 100
[0107] Dot reproducibility was evaluated by the dot reproducibility index (I) of the halftone image. The smaller the dot reproducibility index (I) value, the better the dot reproducibility. (Evaluation Criteria) A:I is less than 1.0 B: I is 1.0 or more and less than 2.0 C:I is 2.0 or more and less than 4.0 D:I is 4.0 or more and less than 6.0 E:I is 6.0 or more and less than 8.0 F:I is 8.0 or higher The results are shown in Table 5.
[0108] <Transferability> Before and after the paper feed durability test, the transferability was evaluated as follows. A solid (FFh) image was formed, and the transferability was evaluated based on the following criteria. The toner remaining on the photoconductor after the primary transfer and the toner before the primary transfer were taped and peeled off with transparent polyester adhesive tape. The peeled adhesive tape was applied to a piece of paper, and the density was measured with a spectrodensitometer 500 series (X-Rite Corporation).
[0109] The rate of change between the density before the primary transfer and the density of the transfer residue obtained above was taken as the transfer efficiency, and was evaluated based on the following evaluation criteria: C or higher was determined to be the effect of the present invention. (Evaluation Criteria) A: Transfer efficiency: 90% or more B: Transfer efficiency: 85% or more but less than 90% C: Transfer efficiency: 80% or more but less than 85% D: Transfer efficiency: less than 80% The results are shown in Table 5.
[0110] <Face covering> A solid white (00h) image was formed, and the fogging was evaluated based on the following criteria. The measurement was performed using a reflectometer (product name: TC-6DS, manufactured by Tokyo Denshoku Co., Ltd.). The reflection density was measured at nine points on the white background after image formation, and the lowest value among the obtained values was taken as Ds. In addition, the reflection density was measured at nine points on the recording medium before image formation, and the average value of the obtained values was taken as Dr.
[0111] The fog amount was evaluated using Dr-Ds. The smaller the value, the less fog there was. (Evaluation Criteria) A: Fog amount is less than 1.00 B: Fog amount is 1.00 or more and less than 3.00 C: Fog amount is 3.00 or more
[0112] The results are shown in Table 5. [Table 5] [Explanation of symbols]
[0113] 1.Means for quantitative supply of raw materials 2. Compressed gas flow rate adjustment means 3.Introduction tube 4. Protruding parts 5. Supply pipe 6. Processing Room 7.Hot air supply means 8. Cold air supply means 9. Regulatory measures 10. Recovery Methods 11.Hot air supply means outlet 12.Distribution member 13. Swivel member 14. Powder particle supply port
Claims
1. A toner having toner particles and silica fine particles A, the toner particles containing a binder resin, the silica fine particles A being attached or fixed to the surfaces of the toner particles, The silica fine particles A contain iron atoms at a concentration of 150 ppm or more and 2000 ppm or less, The primary particles of the silica fine particles A have a number average particle size of 80 nm or more and 200 nm or less, The toner, wherein a coverage rate of the toner particles with the fine silica particles A is 31.0% or more and 70.0% or less.
2. 2. The toner according to claim 1, wherein the content of the silica fine particles A in the toner is from 2.1% by mass to 7.0% by mass based on the mass of the toner.
3. 3. The toner according to claim 1, wherein the adhesion rate of the silica fine particles A in the toner is 50% by mass or more and 90% by mass or less.
4. 4. The toner according to claim 1, wherein the silica fine particles A contain aluminum atoms at a concentration of 200 ppm or more and 2000 ppm or less.
Citation Information
Patent Citations
Production of electrophotographic toner
JP1994332253A
silica
JP2005536611A
Toner
JP2009134073A
silanized fumed silica
JP2009520667A
Hydrophobic fumed silica and silicone rubber materials containing the fumed silica
JP2010527882A