Transparent substrate with film

The film-coated transparent substrate with dielectric and metal tin layers addresses inefficiencies in display contrast enhancement by reducing transmittance and maintaining visibility, achieving stable and high-contrast displays for capacitive touch panels.

JP7563380B2Active Publication Date: 2024-10-08NIPPON ELECTRIC GLASS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021520789
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-21
Filing Date
2020-05-19
Publication Date
2024-10-08
Estimated Expiration
2040-05-19

AI Technical Summary

Technical Problem

Existing methods for improving display contrast by reducing visible light transmittance through light absorption layers are inefficient and do not maintain visibility and stability over time.

Method used

A film-coated transparent substrate with a transparent base material and an optical film comprising dielectric layers and light absorption layers made of metal tin, where the total physical thickness of the light absorption layers is 2 to 30 nm, and at least one layer is made of silicon oxide or aluminum oxide, with a protective layer of silicon oxide to prevent oxidation.

Benefits of technology

The solution effectively reduces visible light transmittance, maintains visibility, and enhances display contrast while ensuring high sheet resistance suitable for capacitive touch panel displays, with improved stability and reduced wavelength dependence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563380000007
    Figure 0007563380000007
  • Figure 0007563380000008
    Figure 0007563380000008
  • Figure 0007563380000009
    Figure 0007563380000009
Patent Text Reader

Abstract

A film-equipped transparent substrate 10 is provided with a transparent base material 11, and an optical film 12 provided on a first surface 11a of the transparent base material 11. The optical film 12 is provided with a plurality of dielectric layers 13, and one or more light absorption layers 14 sandwiched between the dielectric layers 13. The light absorption layers 14 include metallic tin. The total physical film thickness of the light absorption layers 14 is 2 to 30 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film-coated transparent substrate. [Background technology]

[0002] A known method for improving the contrast of a display is to reduce the visible light transmittance of a cover member attached to the display surface of the display. Patent Document 1 discloses a technology in which a light absorbing layer in which fine particles of a conductive material such as titanium nitride are dispersed is provided on an anti-reflection film provided on a substrate such as a camera lens, and the transmittance of visible light is reduced based on the light absorption properties of the light absorbing layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 09-073001 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention relates to a method for manufacturing a transparent substrate having a film for use on a display surface of a display, etc. Low The challenge is to bring it down. [Means for solving the problem]

[0005] According to one aspect of the present invention, a film-coated transparent substrate comprises a transparent base material and an optical film provided on a surface of the transparent base material, the optical film comprising a plurality of dielectric layers and one or more light absorbing layers sandwiched between the plurality of dielectric layers, the light absorbing layers containing metallic tin, and a total physical film thickness of the light absorbing layers being 2 to 30 nm.

[0006] In the above-mentioned film-attached transparent substrate, the physical thickness of a single layer of the light absorbing layer may be 20 nm or less. In the above-mentioned film-attached transparent substrate, at least one layer in contact with the light absorbing layer may be a layer made of silicon oxide or aluminum oxide.

[0007] In the above-mentioned film-coated transparent substrate, the plurality of dielectric layers may be a dielectric multilayer film in which high refractive index layers and low refractive index layers are alternately stacked, and the light absorption layer may be provided between layers of the dielectric multilayer film.

[0008] In the above-mentioned film-formed transparent substrate, the plurality of dielectric layers may contain one or more materials selected from an inorganic oxide, an inorganic nitride, and an inorganic oxynitride. In the above-mentioned film-attached transparent substrate, the average light transmittance in the wavelength range of 400 to 700 nm may be 44% or more and 90% or less.

[0009] In the above-mentioned film-attached transparent substrate, the difference between the maximum and minimum values ​​of light transmittance (%) in the wavelength range of 400 to 700 nm may be 30 or less. In the above-mentioned film-attached transparent substrate, the average light absorptance in the wavelength range of 400 to 700 nm may be 10% or more and 55% or less.

[0010] In the above-mentioned film-attached transparent substrate, the difference between the maximum and minimum values ​​of the light absorptance (%) in the wavelength range of 400 to 700 nm may be 30 or less. Effect of the Invention

[0011] According to the present invention, the visible light transmittance of the film-coated transparent substrate Low It can be lowered. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is an explanatory diagram of a transparent substrate with a film. [Diagram 2] Transmission, reflection and absorption spectra of Example 1. [Diagram 3] Transmission, reflection and absorption spectra of Example 2. [Figure 4] Transmission, reflection and absorption spectra of Example 3. [Diagram 5] Transmission, reflection and absorption spectra of Example 4. [Figure 6] Transmission, reflection and absorption spectra of Example 5. [Figure 7] Transmission, reflection and absorption spectra of Example 6. [Figure 8] Transmission, reflection and absorption spectra of Example 7. [Figure 9] Transmission, reflection and absorption spectra of Example 8. [Figure 10] Transmission, reflection, and absorption spectra of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described. As shown in FIG. 1, a film-coated transparent substrate 10 includes a plate-shaped transparent base material 11 and an optical film 12 provided on the surface of the transparent base material 11.

[0014] The transparent substrate 11 is a substrate having a first surface 11a and a second surface 11b located on the opposite side of the first surface 11a. The thickness of the transparent substrate 11 is not particularly limited and can be appropriately set in consideration of mechanical properties and the like. The thickness of the transparent substrate 11 is, for example, in the range of 0.05 mm or more and 10 mm or less. The transparency of the transparent substrate 11 means, for example, that it transmits 80% or more of visible light (wavelength range of 400 to 700 nm) on average.

[0015] Examples of the material of the transparent substrate 11 include glass and resin. Examples of the glass that can be used include known glasses such as non-alkali glass, aluminosilicate glass, soda-lime glass, and quartz glass. Also, reinforced glass such as chemically reinforced glass and crystallized glass such as LAS-based crystallized glass can be used. The glass is preferably aluminosilicate glass, and the aluminosilicate glass more preferably contains, in mass %, SiO2: 50 to 80%, Al2O3: 5 to 25%, B2O3: 0 to 15%, Na2O: 1 to 20%, and K2O: 0 to 10%. Examples of the resin include acrylic resins such as polymethyl methacrylate, polycarbonate resins, and epoxy resins. The transparent substrate 11 is preferably made of glass in that the transmittance of visible light is unlikely to change over time.

[0016] As shown in Fig. 1, the optical film 12 includes a plurality of dielectric layers 13 and one or more light absorbing layers 14 sandwiched between the dielectric layers 13. Fig. 1 illustrates an example in which the optical film 12 includes one light absorbing layer 14. Hereinafter, the side of the optical film 12 closer to the transparent substrate 11 in the thickness direction is referred to as the inside, and the side farther from the transparent substrate 11 is referred to as the outside.

[0017] The plurality of dielectric layers 13 are formed of one or more selected from inorganic oxides, inorganic nitrides, inorganic oxynitrides, and inorganic fluorides. The dielectric layers 13 are, for example, a dielectric multilayer film in which high-refractive index layers and low-refractive index layers are alternately laminated. Examples of materials constituting the high-refractive index layers include titanium oxide, niobium oxide, lanthanum oxide, tantalum oxide, zirconium oxide, hafnium oxide, and silicon nitride. Examples of materials constituting the low-refractive index layers include silicon oxide, aluminum oxide, and magnesium fluoride. The physical film thickness and material of each dielectric layer 13 and the number of layers of the dielectric layers 13 may be designed according to the type (optical characteristics) of the dielectric multilayer film. For example, the number of layers of each dielectric layer 13 may be 1, 2, 3, 4, 5, or more, independently of each other. The thickness of each dielectric layer 13 may be, for example, 40 nm or more and 300 nm or less, independently of each other. The thickness of each layer in the dielectric layer 13 may be, for example, 5 nm or more and 130 nm or less, independently of each other. Examples of types of dielectric multilayer films include anti-reflection films, half mirrors, and band-pass filters.

[0018] At least one layer of the dielectric layer 13 in contact with the light absorbing layer 14 is preferably made of silicon oxide or aluminum oxide. In this case, it becomes easy to reduce the wavelength dependency of the transmittance of the light absorbing layer 14 in the visible light wavelength range.

[0019] The light absorbing layer 14 is a layer that absorbs visible light to reduce the transmittance of visible light, contains metal tin, and is provided between the dielectric layers 13. The position of the light absorbing layer 14 between the dielectric layers 13 is not particularly limited, and it is sufficient that one or more dielectric layers 13 are located on both the inside and outside of the light absorbing layer 14. When two or more light absorbing layers 14 are provided, one or more dielectric layers 13 are further provided between the light absorbing layers 14.

[0020] The light absorbing layer 14 containing metallic tin has the property of decreasing the visible light transmittance to a greater extent as the total physical thickness of the light absorbing layer 14 increases. The total physical thickness of the light absorbing layer 14 is 2 to 30 nm. When the total physical thickness of the light absorbing layer 14 is 2 nm or more, the visible light transmittance can be reliably decreased. When the total physical thickness of the light absorbing layer 14 is 30 nm or less, a visible light transmittance of 20% or more can be obtained.

[0021] The physical thickness of the single layer of the light absorbing layer 14 is 30 nm or less, preferably 20 nm or less, and more preferably 15 nm or less. By making the physical thickness of the single layer of the light absorbing layer 14 30 nm or less, a decrease in the sheet resistance of the optical film 12 is suppressed, and a high sheet resistance (for example, 1 GΩ / □ or more) can be ensured. This makes it possible to apply the film-coated transparent substrate 10 to a capacitive touch panel display.

[0022] The physical thickness of the single layer of the light absorbing layer 14 is preferably 1 nm or more, and more preferably 5 nm or more. When the optical film 12 has a single light absorbing layer 14, the physical thickness of the single layer of the light absorbing layer 14 is 2 nm or more. When the optical film 12 has two or more light absorbing layers 14, the physical thicknesses of the light absorbing layers 14 may be the same or different.

[0023] The physical thickness and number of layers of the single layer of the light absorbing layer 14 can be appropriately set according to the visible light transmittance required for the film-coated transparent substrate 10. For example, in the case of a film-coated transparent substrate 10 applied to a capacitive touch panel display, when the visible light transmittance required for the film-coated transparent substrate 10 is low (for example, the average transmittance is 50% or less), it is preferable to lower the transmittance by providing two or more light absorbing layers 14 with a physical thickness of 20 nm or less. On the other hand, when the average visible light transmittance required for the film-coated transparent substrate 10 is 70% or more and 90% or less, it is preferable to provide only one light absorbing layer 14 with a physical thickness of 20 nm or less.

[0024] The light absorbing layer 14 may have a tin oxide layer formed by oxidizing metal tin on a part of its surface. In this case, however, the physical film thickness of the non-oxidized part of the light absorbing layer 14 is configured to be within the above-mentioned numerical range.

[0025] Optionally, the optical film 12 may include a protective layer 15 provided on the outer surface of the light absorbing layer 14. The protective layer 15 includes a first layer 15a made of silicon oxide. The physical thickness of the first layer 15a is, for example, 1 to 20 nm, and preferably 2 to 10 nm. The protective layer 15 may further include a second layer 15b made of metallic silicon, and the second layer 15b is preferably in contact with the outer side of the light absorbing layer 14. The physical thickness of the second layer 15b is, for example, 0.2 to 1.0 nm.

[0026] The protective layer 15 is a layer for suppressing deterioration of the light absorbing layer 14 due to oxidation when the dielectric layer 13 is formed on the outside of the light absorbing layer 14 in the manufacturing process of the optical film 12. If the dielectric layer 13 is formed directly on the outer surface of the light absorbing layer 14 in the manufacturing process of the optical film 12, a part of the light absorbing layer 14 may be oxidized and the light absorbing layer 14 may be deteriorated.

[0027] Therefore, it is preferable to form a metal silicon layer on the outer surface of the light absorbing layer 14, and then form the first dielectric layer 13 on the metal silicon layer. In this case, the metal silicon layer is oxidized before the light absorbing layer 14 is oxidized, thereby consuming oxygen atoms, and thus it is possible to suppress deterioration of the light absorbing layer 14 due to oxidation.

[0028] The first layer 15a of the protective layer 15 is a layer formed by oxidizing the metal silicon layer on the outer surface of the light absorbing layer 14 to silicon oxide when forming the first dielectric layer 13. If the metal silicon layer is entirely oxidized when forming the dielectric layer 13, the protective layer will include only the first layer 15a made of silicon oxide, and the first layer 15a will be in contact with the outside of the light absorbing layer 14.

[0029] When forming the dielectric layer 13, if a portion of the metal silicon layer remains without being oxidized, the protective layer 15 will have a first layer 15a made of silicon oxide and a second layer 15b made of metal silicon, with the second layer 15b being in contact with the outside of the light absorbing layer 14.

[0030] The film-coated transparent substrate 10 is used, for example, as a cover member to be attached to the display surface of a display. The sheet resistance of the optical film 12 is preferably 1 GΩ / □ or more, more preferably 5 GΩ / □ or more, and even more preferably 10 GΩ / □ or more.

[0031] According to the above configuration, a film-coated transparent substrate that can be applied to a capacitive touch panel display can be obtained. The average transmittance of the film-coated transparent substrate 10 in the visible light wavelength range (400 to 700 nm) is preferably 20% or more, more preferably 40% or more, and even more preferably 60% or more. The average transmittance can be, for example, 35% or more, 44% or more, 48% or more, 57% or more, 66% or more, 71% or more, or 77% or more.

[0032] According to the above-mentioned configuration, the visibility of a display in which the film-coated transparent substrate 10 is used as a cover member can be maintained. The average transmittance of the film-coated transparent substrate 10 in the visible light wavelength range (400 to 700 nm) is preferably 90% or less, more preferably 85% or less, for example, 86% or less, 84% or less, or 78% or less.

[0033] According to the above-mentioned configuration, it is possible to improve the contrast of a display in which the film-coated transparent substrate 10 is used as a cover member. The average visible light transmittance of the film-coated transparent substrate 10 can be, for example, 40 to 80% or 44 to 90%.

[0034] The difference between the maximum and minimum transmittance (%) of the film-coated transparent substrate 10 in the visible light wavelength range (400 to 700 nm) can be, for example, 30 or less, 29 or less, 28 or less, 27 or less, 26 or less, 25 or less, 24 or less, 23 or less, 22 or less, 21 or less, 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, 8 or less, or 7 or less.

[0035] The average absorptance of the film-coated transparent substrate 10 in the visible light wavelength range (400 to 700 nm) is preferably 75% or less, more preferably 60% or less, and even more preferably 40% or less. The average absorptance can be, for example, 55% or less, 51% or less, 42% or less, 33% or less, 28% or less, or 22% or less.

[0036] According to the above-mentioned configuration, the visibility of a display in which the film-coated transparent substrate 10 is used as a cover member can be maintained. The average absorptance of the film-coated transparent substrate 10 in the visible light wavelength range (400 to 700 nm) is preferably 10% or more, and more preferably 15% or more. The average absorptance can be, for example, 12% or more.

[0037] According to the above-mentioned configuration, it is possible to improve the contrast of a display in which the film-coated transparent substrate 10 is used as a cover member. The average visible light absorptance of the film-coated transparent substrate 10 can be, for example, 10 to 55%.

[0038] The difference between the maximum and minimum absorptance (%) of the film-coated transparent substrate 10 in the visible light wavelength range (400 to 700 nm) can be, for example, 30 or less, 29 or less, 28 or less, 27 or less, 26 or less, 25 or less, 24 or less, 23 or less, 22 or less, 21 or less, 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, 8 or less, 7 or less, or 6 or less.

[0039] Specific examples of the film configuration of the optical film 12 are shown in Tables 1 to 4. The values ​​in the tables indicate the physical film thickness of each layer. Configuration example 1 is a configuration example of a light-absorbing antireflection film in which the layer in contact with the inner side of the light-absorbing layer 14 is a dielectric layer 13 made of silicon oxide, and the layer in contact with the outer side of the light-absorbing layer 14 is a first layer 15a of a protective layer 15 also made of silicon oxide.

[0040] Configuration example 2 is a configuration example of a light absorbing antireflection film in which the layer in contact with the inner side of the light absorbing layer 14 is a dielectric layer 13 made of niobium oxide, and the layer in contact with the outer side of the light absorbing layer 14 is a first layer 15a of a protective layer 15 made of silicon oxide.

[0041] Configuration example 3 is a configuration example of a light absorptive antireflection film in which the layers in contact with the inside and outside of light absorbing layer 14 are both dielectric layers 13 made of silicon oxide, and no protective layer 15 is provided. Configuration examples 4 to 8 are configuration examples of a light absorptive antireflection film in which the layer in contact with the inside of the light absorbing layer 14 is a dielectric layer 13 made of silicon oxide, and the layer in contact with the outside of the light absorbing layer 14 is a first layer 15a of a protective layer 15 made of silicon oxide, and in particular, the physical film thickness of the light absorbing layer 14 is varied in stages.

[0042] Configuration example 9 is a configuration example of a light absorptive antireflection film in which the layer in contact with the inside of the light absorbing layer 14 is a dielectric layer 13 made of silicon oxide, the layer in contact with the outside of the light absorbing layer 14 is a second layer 15b of the protective layer 15 made of silicon metal, and the protective layer 15 further includes a first layer 15a made of silicon oxide on the outside of the second layer 15b.

[0043] Configuration example 10 is a configuration example of a light absorbing antireflection film having two light absorbing layers 14 .

[0044] [Table 1]

[0045] [Table 2]

[0046] [Table 3]

[0047] [Table 4] Next, a method for producing the film-coated transparent substrate 10 will be described.

[0048] An example of a method for manufacturing the film-coated transparent substrate 10 includes a first dielectric layer forming step, a light absorbing layer forming step, a metal silicon layer forming step, and a second dielectric layer forming step, which are described below, in this order. (First dielectric layer forming process) The first dielectric layer forming step is a step of forming the dielectric layer 13 located inside the light absorbing layer 14. The dielectric layer 13 is preferably formed by a sputtering method, since it can be formed accurately and stably. Among sputtering methods, a reactive sputtering method such as a radical assisted sputtering (RAS) method is particularly preferred, since it has a high film formation speed for the dielectric layer 13 and is excellent in productivity.

[0049] An example of a method for forming the dielectric layer 13 by reactive sputtering will be described. The transparent substrate 11 is set in a sputtering device. As a target for the sputtering device, for example, a metal target such as silicon, aluminum, tantalum, lanthanum, niobium, titanium, hafnium, zirconium, etc. can be used.

[0050] A mixed gas of an inert gas and an active gas is introduced into a sputtering device, and a predetermined target is sputtered to form a layer made of the predetermined target components on the transparent substrate 11. The formed layer reacts with the active gas activated by plasma or the like to form a dielectric layer 13. In this manner, a first film is obtained in which the dielectric layer 13 is formed on the transparent substrate 11. As the inert gas, argon gas can be used. As the active gas, oxygen gas, nitrogen gas, hydrogen gas, or a mixture of these gases can be used. It is desirable to introduce the mixed gas of the inert gas and the active gas after exhausting the inside of the sputtering device with a vacuum pump or the like. The mixture ratio of the inert gas and the active gas (inert gas:active gas) is not particularly limited, and can be within the range of, for example, 2:1 to 8:1.

[0051] (Light absorbing layer forming process) The light absorbing layer forming step is a step of forming a light absorbing layer 14 on the dielectric layer 13 of the first film formed body. The light absorbing layer 14 can be formed by, for example, a sputtering method, a physical vapor deposition method such as a vacuum deposition method, or a plating method. In order to form the light absorbing layer 14 having a thickness of 1 to 30 nm while controlling the thickness with high precision, a sputtering method is preferred.

[0052] An example of a method for forming the light absorbing layer 14 by the sputtering method will be described. The first film body is set in a sputtering device. Metallic tin is prepared as a target for the sputtering device. Next, an inert gas is introduced into the sputtering device to sputter the metallic tin, thereby obtaining a second film body in which the light absorbing layer 14 made of metallic tin is formed on the dielectric layer 13 of the first film body. Argon gas can be used as the inert gas. It is preferable to introduce the inert gas after evacuating the inside of the sputtering device using a vacuum pump or the like.

[0053] (Metal silicon layer formation process) The metal silicon layer forming step is a step of forming a metal silicon layer, which will later become the protective layer 15, on the light absorbing layer 14 of the second film formation body. The metal silicon layer can be formed by, for example, a sputtering method, a physical vapor deposition method such as a vacuum deposition method, or a plating method. In order to form the metal silicon layer while controlling the film thickness with high precision, the sputtering method is preferred.

[0054] An example of a method for forming the protective layer 15 by the sputtering method will be described. The second film-formed body is set in a sputtering device. Metallic silicon is prepared as a target for the sputtering device. Next, an inert gas is introduced into the sputtering device to sputter the metallic silicon, thereby obtaining a third film-formed body in which a metallic silicon layer is formed on the dielectric layer 13 of the second film-formed body. Here, the metallic silicon layer is formed so that its thickness is the total thickness of the first layer 15a and the second layer 15b of the protective layer 15. Argon gas can be used as the inert gas. It is preferable to introduce the inert gas after evacuating the inside of the sputtering device using a vacuum pump or the like.

[0055] (Second dielectric layer forming process) The second dielectric layer forming step is a step of forming the dielectric layer 13 located on the outer side of the light absorbing layer 14. In the second dielectric layer forming step, it is preferable to form the dielectric layer 13 by a sputtering method, similarly to the first dielectric layer forming step.

[0056] An example of a method for forming the dielectric layer 13 by reactive sputtering will be described. The third film-forming body is set in a sputtering device. As a target for the sputtering device, for example, a metal target such as silicon, aluminum, tantalum, lanthanum, niobium, titanium, hafnium, zirconium, etc. can be used.

[0057] A mixed gas of an inert gas and an active gas is introduced into the sputtering device, and a predetermined target is sputtered to form a layer made of the predetermined target components on the third film-forming body. The formed layer reacts with the active gas activated by plasma or the like to form the dielectric layer 13. In this manner, a film-coated transparent substrate 10 on which an optical film 12 is formed is obtained.

[0058] In the second dielectric layer forming step, when a predetermined target component that will become dielectric layer 13 reacts with an active gas activated by plasma or the like, the metal silicon layer formed on the third film-forming body also reacts with the active gas activated by plasma or the like to become silicon oxide, and a first layer 15a of protective layer 15 made of silicon oxide is formed. At this time, if the inner part of the metal silicon layer is not oxidized and is left as metal silicon, a second layer 15b of protective layer 15 is formed.

[0059] When forming an optical film 12 having a plurality of light absorbing layers 14, the light absorbing layer forming step, the metal silicon layer forming step, and the second dielectric layer forming step are repeated according to the number of light absorbing layers 14. When manufacturing a film-coated transparent substrate 10 that does not include a protective layer 15, the metal silicon layer forming step is omitted.

[0060] Next, the operation and effects of the above embodiment will be described. (1) The film-coated transparent substrate 10 includes a transparent base material 11 and an optical film 12 provided on a first surface 11a of the transparent base material 11. The optical film 12 includes a plurality of dielectric layers 13 and one or more light absorbing layers 14 sandwiched between the plurality of dielectric layers 13. The light absorbing layers 14 contain metallic tin. The total physical film thickness of the light absorbing layers 14 is 2 to 30 nm.

[0061] According to the above-mentioned configuration, the light absorbing layer 14 containing metallic tin absorbs visible light, thereby decreasing the transmittance of visible light. In addition, the decrease in the transmittance of visible light improves the contrast of a display when the film-coated transparent substrate 10 is attached to the display for use.

[0062] By providing the dielectric layer 13 on the inner side of the light absorbing layer 14 in the optical film 12, the adhesion of the optical film 12 to the transparent substrate 11 is improved compared to a case in which the dielectric layer 13 is not provided. By providing the dielectric layer 13 on the outer side of the light absorbing layer 14 in the optical film 12, deterioration of the light absorbing layer 14 caused by the outside air, etc. is suppressed, and the stability of the transmittance over time is improved.

[0063] By setting the total physical film thickness of the light absorbing layer 14 to 2 to 30 nm, the transmittance of the transparent substrate 10 can be reduced, the contrast of the display can be improved, and a high sheet resistance of the optical film (for example, 1 GΩ / □ or more) can be ensured.

[0064] (2) The physical thickness of the single layer of the light absorbing layer 14 is 20 nm or less. According to the above-mentioned configuration, the decrease in sheet resistance caused by providing the light absorbing layer 14, which is a metal tin layer, is suppressed, and a high sheet resistance (for example, 1 GΩ / □ or more) can be ensured. This makes it possible to provide the film-coated transparent substrate 10 applicable to a capacitive touch panel display.

[0065] (3) At least one layer in contact with the light absorbing layer 14 is a layer made of silicon oxide or aluminum oxide. A layer made of silicon oxide or aluminum oxide has a property that oxygen atoms constituting the oxide are less likely to be transmitted to an adjacent layer compared to layers made of other oxides. Therefore, according to the above-mentioned configuration, it is possible to suppress a part of the metal tin constituting the light absorbing layer 14 from being oxidized due to oxygen atoms contained in a layer in contact with the light absorbing layer 14. As a result, it is possible to reduce the wavelength dependency of the transmittance of the light absorbing layer 14 in the visible light wavelength range. The layer made of silicon oxide or aluminum oxide also includes the first layer 15a of the protective layer 15.

[0066] (4) The plurality of dielectric layers 13 constitute a dielectric multilayer film in which high refractive index layers and low refractive index layers are alternately laminated, and the light absorbing layer 14 is provided between the layers of the dielectric multilayer film. According to the above-mentioned configuration, the dielectric multilayer film can be provided with light absorbing properties with a simple configuration.

[0067] (5) The optical film 12 is in contact with the outer side of the light absorbing layer 14 and includes a protective layer 15 containing silicon oxide. According to the above-mentioned configuration, deterioration of the light absorbing layer 14 due to oxidation during the manufacturing process can be suppressed.

[0068] (6) The protective layer 15 includes a first layer 15a made of silicon oxide and a second layer 15b made of metallic silicon, and the second layer 15b is in contact with the outside of the light absorbing layer . According to the above configuration, oxygen atoms are consumed in the oxidation of the metallic silicon of the second layer 15b before being transferred to the light absorbing layer 14, so that the oxygen atoms are less likely to be transferred to the light absorbing layer 14. This makes it possible to further reduce the wavelength dependency of the transmittance in the visible light wavelength range. In addition, the stability of the transmittance over time is improved.

[0069] This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that there is no technical contradiction. The multiple dielectric layers 13 do not have to constitute a dielectric multilayer film.

[0070] The film-coated transparent substrate 10 may further include a functional layer such as an antiglare layer or an antifouling layer. For example, an antiglare layer formed by a process of applying a coating agent may be provided on the first surface 11a of the transparent base material 11, and the optical film 12 may be provided on the antiglare layer. In addition, an antifouling layer may further be provided on the optical film 12. EXAMPLES

[0071] The above embodiment will be described in more detail below with reference to examples and comparative examples, although the present invention is not limited thereto. Example 1 As Example 1, a transparent substrate with a film was produced that had the light absorbing antireflection film of Configuration Example 1 shown in Table 1. As the first dielectric layer formation step, a Nb2O5 film, a SiO2 film, a Nb2O5 film, and a SiO2 film were formed in this order by sputtering on a transparent substrate (chemically strengthened glass substrate: T2X-1 manufactured by Nippon Electric Glass Co., Ltd.) having a thickness of 1.3 mm to obtain a first film body. A load-lock type reactive sputtering device was used to form each film by sputtering.

[0072] Next, as the light absorbing layer forming process, a load-lock reactive sputtering device was used to form a light absorbing layer made of metal tin on the dielectric layer of the first film formed body, thereby obtaining a second film formed body. At this time, the flow rate of argon gas was set to 500sccm. The film forming pressure of the light absorbing layer was set to 0.3Pa.

[0073] Next, in the metal silicon layer forming step, the metal silicon target was sputtered while keeping the argon gas at the same flow rate to form a metal silicon layer on the light absorbing layer, thereby obtaining a third film formed body. At this time, the film forming pressure of the metal silicon layer was set to 0.3 Pa.

[0074] Next, as a second dielectric layer forming process, a mixed gas of argon gas and oxygen gas was introduced into the sputtering device, and then a metal silicon target was sputtered to form a SiO2 film on the metal silicon layer. At this time, the flow rate of the argon gas was set to 500 sccm, and the flow rate of the oxygen gas was set to 220 sccm. The deposition pressure of the SiO2 film was set to 0.3 Pa. In this SiO2 film forming process, the metal silicon layer was oxidized to form a first layer of the protective layer made of silicon oxide.

[0075] Next, while keeping the mixed gas of argon gas and oxygen gas at the same flow rate, a niobium target was sputtered to form an Nb2O5 film on the SiO2 film, and then a metal silicon target was sputtered to form an SiO2 film on the Nb2O5 film, thereby obtaining a film-coated transparent substrate of Example 1. At this time, the film-coating pressure for the Nb2O5 film was 0.3 Pa, and the film-coating pressure for the SiO2 film was 0.3 Pa. The physical film thickness of each layer of the film-coated transparent substrate of Example 1 is as shown in Configuration Example 1 in Table 1.

[0076] Example 2 As Example 2, a film-coated transparent substrate was produced that had the light-absorbing antireflection film of Configuration Example 2 shown in Table 1. As a first dielectric layer formation step, a Nb2O5 film, a SiO2 film, and a Nb2O5 film were formed in this order by sputtering on a transparent substrate (chemically strengthened glass substrate: T2X-1 manufactured by Nippon Electric Glass Co., Ltd.) having a thickness of 1.3 mm to obtain a first film-formed body.

[0077] Next, a light absorbing layer forming step, a metal silicon layer forming step, and a second dielectric layer forming step were performed in the same manner as in Example 1 to obtain a film-coated transparent substrate of Example 2. The physical film thickness of each layer of the film-coated transparent substrate of Example 2 is as shown in Configuration Example 2 in Table 1.

[0078] Example 3 As Example 3, a film-attached transparent substrate was produced that had the light-absorbing antireflection film of Configuration Example 3 shown in Table 1. A first dielectric layer forming step and a light-absorbing layer forming step were performed in the same manner as in Example 1 to obtain a second film-attached body. Next, a second dielectric layer forming step was performed in the same manner as in Example 1 (except that only one SiO2 film was formed), to obtain a film-attached transparent substrate of Example 3.

[0079] (Examples 4 to 8) As Examples 4 to 8, film-coated transparent substrates were prepared that had the light absorptive antireflection films of Configuration Examples 4 to 8 shown in Table 2. The transparent substrates used and the method for forming each layer were the same as in Example 1.

[0080] Comparative Example 1 As Comparative Example 1, a film-attached transparent substrate was produced that had an anti-reflection film in which the light absorbing layer and the protective layer were omitted from Configuration Example 1 shown in Table 1. A first dielectric layer forming step was performed in the same manner as in Example 1 to obtain a first film-formed body. Next, a second dielectric layer forming step was performed in the same manner as in Example 1 to obtain a film-attached transparent substrate of Comparative Example 1.

[0081] (Evaluation of transmittance, reflectance, and absorptance) For each of the film-attached transparent substrates of the Examples and Comparative Examples, the transmittance and reflectance in the visible light wavelength range (400 to 700 nm) were measured using a spectrophotometer (U-4000 manufactured by Hitachi High-Tech Corporation). The absorptance was calculated using the following formula (1).

[0082] Absorption rate (%) = 100 - transmittance (%) - reflectance (%) (1) The transmission, reflection, and absorption spectra of the film-attached transparent substrates of each Example and Comparative Example are shown in Figures 2 to 10. In addition, the average values ​​of the transmittance, reflectance, and absorptance in the visible light wavelength range, as well as the difference between the maximum and minimum values ​​of the transmittance and absorptance, were calculated. The results are shown in Tables 5 and 6.

[0083] (Evaluation of sheet resistance) For the film-attached transparent substrates of Examples 1 to 6, the sheet resistance of the optical film was measured. A pair of electrodes made of solder were formed on the optical film of the film-attached transparent substrate, extending from the surface of the optical film to the dielectric layer in contact with the transparent substrate. The pair of electrodes were linear and spaced apart so as to be parallel to each other, and the distance and length of the pair of electrodes was 80 mm. A tester (Loresta MP manufactured by Mitsubishi Chemical Corporation) was connected to the pair of electrodes, and the electrical resistance of the optical film was measured to calculate the sheet resistance. The results are shown in Tables 5 and 6.

[0084] [Table 5]

[0085] [Table 6] As shown in Tables 5 and 6, the transmittance of each Example is lower than that of Comparative Example 1, which does not have a light absorbing layer. The film-coated transparent substrates of Examples 1 to 6, whose sheet resistances were measured, all had sheet resistances of 1 GΩ / □ or more, and therefore can be used as cover members for capacitive touch panel displays.

[0086] With reference to the transmittance and absorptance of Examples 1 to 3, which have the same thickness of the light absorbing layer, Example 1, in which the dielectric layer in contact with the inside of the light absorbing layer is silicon oxide, has a smaller difference between the maximum and minimum transmittance values, and therefore has a smaller wavelength dependency of the transmittance, compared to Example 2, in which the dielectric layer in contact with the inside of the light absorbing layer is niobium oxide. Example 1, which has a protective layer, has a smaller difference between the maximum and minimum transmittance values, and therefore has a smaller wavelength dependency of the transmittance, compared to Example 3, which does not have a protective layer.

[0087] Referring to the transmittance and absorptance of Examples 4 to 8 in which the thickness of the light absorbing layer is varied stepwise, it can be seen that as the thickness of the light absorbing layer increases, the transmittance decreases and the absorptance increases. [Explanation of symbols]

[0088] Reference Signs List 10: transparent substrate with film, 11: transparent base material, 12: optical film, 13: dielectric layer, 14: light absorbing layer, 15: protective layer, 15a: first layer, 15b: second layer.

Claims

1. A film-attached transparent substrate to be applied to a display surface of a display, comprising: A transparent substrate and an optical film provided on a surface of the transparent substrate, When the side closer to the transparent substrate in the thickness direction of the optical film is defined as the inside and the side farther from the transparent substrate is defined as the outside, The optical film is A light absorbing layer; a first dielectric layer located inside the light absorbing layer and including alternating high refractive index layers and low refractive index layers; a second dielectric layer located outside the light absorbing layer and including alternating high refractive index layers and low refractive index layers; the light absorbing layer comprises metallic tin; the total physical film thickness of the light absorbing layer is 2 to 30 nm; The light absorbing layer located between the first dielectric layer and the second dielectric layer is a single layer.

2. 2. The film-attached transparent substrate according to claim 1, wherein the physical thickness of the single layer of the light absorbing layer is 20 nm or less.

3. 3. The film-attached transparent substrate according to claim 1, wherein at least one layer in contact with the light absorbing layer is a layer made of silicon oxide or aluminum oxide.

4. The film-attached transparent substrate according to any one of claims 1 to 3, wherein the first dielectric layer and the second dielectric layer contain at least one material selected from an inorganic oxide, an inorganic nitride, and an inorganic oxynitride.

5. 5. The film-attached transparent substrate according to claim 1, wherein the average light transmittance in the wavelength region of 400 to 700 nm is 44% or more and 90% or less.

6. 6. The film-attached transparent substrate according to claim 1, wherein the difference between the maximum and minimum light transmittance (%) in the wavelength region of 400 to 700 nm is 30 or less.

7. 7. The film-attached transparent substrate according to claim 1, wherein an average light absorptance in the wavelength region of 400 to 700 nm is 10% or more and 55% or less.

8. 8. The film-attached transparent substrate according to claim 1, wherein the difference between the maximum and minimum light absorptance (%) in the wavelength region of 400 to 700 nm is 30 or less.

Citation Information

Patent Citations

  • Filter for image sensor, image sensor and image information processor

    JP1995170366A

  • Antireflection film

    JP1997073001A

  • Optical product and cathode-ray tube using it

    JP2000162405A

  • Liquid crystal display device

    JP2007155943A

  • Optical filter and light receiving device

    JP2010152256A