Thermal recording medium
A laminated heat-sensitive recording material with a transparent base and specific crosslinking agents enhances transparency, addressing the issue of content visibility in food containers.
Patent Information
- Application Number
- JP2021560802
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-26
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-11-26
AI Technical Summary
Heat-sensitive recording materials used as labels or packaging films for containers containing various foods lack sufficient transparency, making it difficult for consumers to identify the contents.
A laminated heat-sensitive recording material structure comprising a transparent base material with a heat-sensitive recording layer containing a dispersant having a carboxyl group and a crosslinking agent, such as an epichlorohydrin-modified polyamide polyamine resin or an organic compound with an oxazoline group, and an intermediate layer with a core-shell structure to enhance transparency.
The structure improves the transparency of the heat-sensitive recording material, allowing consumers to easily identify the contents of containers.
Smart Images

Figure 0007563850000002 
Figure 0007563850000003 
Figure 0007563850000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosensitive recording medium, and more particularly to a thermosensitive recording medium having excellent transparency. [Background technology]
[0002] Thermal recording media develop color through a chemical reaction when heated by a thermal head or the like, resulting in a recorded image. They are used for a wide range of purposes, not only as recording media for facsimiles, automatic ticket vending machines, and scientific measuring instruments, but also as thermal recording labels for POS systems in retail stores, etc.
[0003] In addition, since the thermal recording medium is used outdoors in the above-mentioned automatic ticket vending machines, etc., those with excellent water resistance and storage stability have been proposed. More specifically, a thermal recording medium has been proposed in which the thermal recording layer contains a carboxyl group-containing resin such as carboxyl-modified polyvinyl alcohol, epichlorohydrin, and a polyamine / amide resin (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2008 / 139948 Summary of the Invention [Problem to be solved by the invention]
[0005] When the thermosensitive recording medium is used as a label or a packaging film for containers containing various foods, etc., the contents of the container are concealed by the label or film, making it difficult for consumers to check the contents. Therefore, it is desirable to make the labels or films made of the thermosensitive recording medium transparent so that the contents of the container can be checked.
[0006] However, the thermosensitive recording medium described in Patent Document 1 still has the problem that the transparency of the thermosensitive recording medium is insufficient.
[0007] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a thermosensitive recording medium having excellent transparency. [Means for solving the problem]
[0008] In order to achieve the above object, in a first aspect of the present invention, at least a thermal recording layer is provided on a transparent substrate. and the middle class but In this order The laminated thermosensitive recording medium is assumed to have a thermosensitive recording layer that contains a dispersant having a carboxyl group and a crosslinking agent mainly composed of an epichlorohydrin-modified polyamide polyamine resin or an organic compound containing an oxazoline group. The intermediate layer contains a resin having a core-shell structure. It is characterized by:
[0009] According to the above-mentioned construction, it is possible to provide a thermosensitive recording medium having excellent transparency.
[0010] In a second invention, the dispersant in the first invention is composed of a styrene acrylic ammonium salt or a styrene maleate salt.
[0011] In addition, in a third invention, in the first or second invention, the thermosensitive recording layer contains at least one of a particulate color former and a particulate color developer, and the particle diameter of the color former and the particle diameter of the color developer are set to 0.1 μm or more and 1.0 μm or less. Effect of the Invention
[0012] According to the present invention, a thermosensitive recording medium having excellent transparency can be provided. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a cross-sectional view illustrating a thermal recording medium according to the present embodiment. [Diagram 2]FIG. 2 is a diagram for explaining a crosslinking reaction between an azetidinium ring (AZR) in an epichlorohydrin-modified polyamide polyamine resin, which is a crosslinking agent, and a carboxyl group of a dispersant. [Diagram 3] FIG. 2 is a diagram for explaining a crosslinking reaction between an oxazoline group of an organic compound containing an oxazoline group, which is a crosslinking agent, and a carboxyl group of a dispersant. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following embodiment.
[0015] FIG. 1 is a cross-sectional view illustrating a thermal recording medium according to the present embodiment.
[0016] As shown in FIG. 1, the thermosensitive recording medium 1 of this embodiment has a structure in which a thermosensitive recording layer 3 that develops color when heated, an intermediate layer 4, and a topcoat layer 5 are laminated on a sheet-like transparent substrate 2.
[0017] A transparent synthetic resin film, such as a polypropylene film, a polyethylene terephthalate film, a polystyrene film, a polycarbonate film, etc., can be used as the substrate 2. The thickness of the substrate 2 is not particularly limited, but a thickness of about 10 μm to 100 μm is preferable because it has excellent coatability and transparency.
[0018] Materials for forming the thermosensitive recording layer 3 include a color former that changes color when heated, a color developer, a binder, a lubricant, and the like.
[0019] It is preferable to use materials having a fine particle size for improving the transparency of the thermosensitive recording layer 3. By using materials having a fine particle size in this way, diffuse reflection of the particles can be suppressed.
[0020] Specifically, examples of dyes that are color formers include 3-dibutylamino-6-methyl-7-anilinofluoran, and the particle size is preferably 0.1 to 1.0 μm, more preferably 0.1 to 0.6 μm or less, and particularly preferably 0.1 to 0.55 μm.
[0021] The developer may be, for example, 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone, and the particle size is preferably 0.1 to 1.0 μm, more preferably 0.1 to 0.6 μm, and particularly preferably 0.1 to 0.55 μm.
[0022] The particle size mentioned above refers to the 50% average particle size measured using a Microtrack laser analysis / scattering particle size analyzer.
[0023] An example of the binder is a styrene-butadiene copolymer.
[0024] Examples of the lubricant include polyethylene, zinc stearate, and paraffin, and the particle size thereof is preferably 0.5 μm or less.
[0025] In order to improve transparency, it is particularly effective to add paraffin, and it is preferable that the paraffin be a low-melting paraffin having a melting point lower than the color-developing temperature of the thermal recording layer 3, preferably lower than 80°C, and more preferably lower than 50°C.
[0026] The particle size of the low melting point paraffin is preferably 0.5 μm or less as described above. The content of the paraffin is, for example, 0.1 to 1.0 g / m in terms of dry weight. 2 It is preferable that:
[0027] By incorporating paraffin with such a low melting point, when the coating liquid for forming the thermosensitive recording layer is applied to the substrate 2 and dried, the paraffin melts and penetrates into the gaps between the uneven surfaces of the particles constituting the thermosensitive recording layer 3, thereby filling the gaps, thereby suppressing diffuse reflection from the particle surfaces and improving transparency.
[0028] The intermediate layer 4, which has a barrier property against water and oil, is mainly made of a resin. Examples of the resin for the intermediate layer 4 include an emulsion of an acrylic resin, a water-soluble resin such as a polyvinyl alcohol (PVA) resin, and an SBR resin.
[0029] In order to improve transparency, the resin is preferably a resin having a water-soluble portion, such as a polyvinyl alcohol (PVA) resin, which is a resin having a hydroxyl group as a hydrophilic structural unit, or a resin having a core-shell structure in which hydrophobic core particles are coated with a water-soluble shell polymer, such as a core-shell type acrylic resin.
[0030] Water-soluble polyvinyl alcohol (PVA) and core-shell type acrylic resins have good film-forming properties, and when a coating liquid for forming an intermediate layer is applied onto the thermosensitive recording layer 3 and dried, the resin having a water-soluble portion seeps into the thermosensitive recording layer 3 to form a smooth intermediate layer 4, thereby suppressing diffuse reflection in the thermosensitive recording layer 3 and improving transparency.
[0031] As the core-shell type resin, for example, a core-shell type acrylic resin commercially available under the name Barrierstar (manufactured by Mitsui Chemicals, Inc.) can be used.
[0032] The topcoat layer 5 improves the matching of the thermal recording medium 1 with the thermal head, thereby ensuring smooth color development of the thermal recording layer 3. For this topcoat layer 5, a binder containing added fillers, lubricants, crosslinking agents, etc. is used.
[0033] Examples of the resin binder include acrylic resin, etc. Examples of the lubricant include polyethylene, zinc stearate, etc. Examples of the cross-linking agent include zirconium carbonate, etc.
[0034] Examples of the filler include colloidal silica, calcium carbonate, zirconium carbonate, polymethyl methacrylate (PMMA), polystyrene (PS), etc. The particle size of these fillers is preferably 1.0 μm or less. In order to improve transparency, colloidal silica with a small particle size is preferred as the filler.
[0035] Here, the thermosensitive recording material 1 of this embodiment is characterized in that the thermosensitive recording layer 3 contains a dispersant having a carboxyl group and a crosslinking agent whose main component is an epichlorohydrin-modified polyamide polyamine resin or an organic compound containing an oxazoline group.
[0036] Examples of dispersants having a carboxyl group include styrene acrylic ammonium salts such as styrene-acrylic polymers, and styrene maleate salts such as styrene maleic acid resins.
[0037] 2, in the thermosensitive recording layer 3, the azetidinium ring (AZR) in the epichlorohydrin-modified polyamide polyamine resin, which is the crosslinking agent, reacts with the carboxyl group of the dispersing agent to form a crosslinked structure, which is believed to improve the film-forming property of the thermosensitive recording layer 3 and fill the voids contained in the thermosensitive recording layer 3. As a result, the transparency of the thermosensitive recording layer 3 is improved, and a thermosensitive recording material 1 with excellent transparency can be obtained.
[0038] Similarly, in the thermosensitive recording layer 3, as shown in Fig. 3, the oxazoline group of the organic compound containing the oxazoline group, which is a crosslinking agent, reacts with the carboxyl group of the dispersant to form a crosslinked structure, which is thought to improve the film-forming property of the thermosensitive recording layer 3 and fill the voids contained in the thermosensitive recording layer 3. As a result, the transparency of the thermosensitive recording layer 3 is improved, and a thermosensitive recording material 1 with excellent transparency can be obtained.
[0039] The content of the dispersant in the entire thermosensitive recording layer 3 is preferably 5 to 20% by mass, and the content of the crosslinking agent in the entire thermosensitive recording layer 3 is preferably 0.5 to 10% by mass. EXAMPLES
[0040] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.
[0041] Example 1 (Preparation of thermal recording medium) <Thermal recording layer> The coating solution for forming the thermosensitive recording layer shown in Table 1 was prepared, and the coating solution was applied to a 40 μm-thick OPP (biaxially oriented polypropylene) film substrate in an amount of 4.0 to 6.0 g / m2 in terms of dry weight. 2 After coating, the mixture was dried to form a heat-sensitive recording layer having a thickness of 45 to 50 μm on the substrate. In Table 1, the values of each compounding ingredient indicate the weight ratio when dried.
[0042] As the compounding materials, styrene acrylic ammonium salt was used as the dispersant, and epichlorohydrin modified polyamide polyamine resin was used as the crosslinking agent. As the dye, 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.15 μm was used, as the color developer, 4-hydroxyphenyl (4'-n-propoxyphenyl) sulfone with a particle diameter of 0.15 μm was used, and as the binder, SBR with a glass transition temperature Tg of "-3°C" was used. As the lubricant, polyethylene (PE) with a melting point of 100°C and a particle diameter of 0.6 μm, and paraffin with a melting point of 46°C and a particle diameter of 0.2 μm were used. As the filler, kaolin with a particle diameter of 0.4 μm was used.
[0043] <Middle Class> A coating solution for forming an intermediate layer using a core-shell type acrylic resin was prepared, and the coating solution for forming the intermediate layer was applied to the above-mentioned thermal recording layer in a coating amount of 2.0 g / m2 on a dry basis. 2 After coating so as to obtain the above, the coating was dried to form an intermediate layer having a thickness of 2.0 μm on the thermal recording layer.
[0044] <Topcoat layer> A coating solution for forming a topcoat layer shown in Table 1 was prepared, and the coating solution for forming a topcoat layer was applied to the intermediate layer described above in an amount of 1.5 g / m2 in terms of dry weight. 2 After coating so as to obtain a coating composition having a thickness of 1.5 μm, the coating composition was dried to form a top coat layer having a thickness of 1.5 μm on the intermediate layer.
[0045] The binder used was acrylic resin, the lubricants were polyethylene (PE) and zinc stearate (St-Zn), the fillers were colloidal silica with particle diameters of several nm and colloidal silica with particle diameters of several tens of nm, and the cross-linking agent was zirconium carbonate.
[0046] The thermal recording medium of this example was prepared by the above method.
[0047] <Haze value measurement> The haze value of the obtained thermal recording medium was measured in accordance with JIS-K7136:2000 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: NDH7000). The results are shown in Table 1.
[0048] Example 2 A thermal recording medium was prepared in the same manner as in Example 1 above, except that the crosslinking agent in the thermal recording layer was changed to an epichlorohydrin-modified polyamide polyamine resin, which has a 10% lower reaction point than the above-mentioned crosslinking agent, a lower degree of cationization, and a smaller molecular weight.
[0049] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0050] Example 3 A thermosensitive recording medium was prepared in the same manner as in Example 1 above, except that in the thermosensitive recording layer, the crosslinking agent was changed to an organic compound containing an oxazoline group.
[0051] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0052] Example 4 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone having a particle diameter of 0.25 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran having a particle diameter of 0.25 μm.
[0053] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0054] Example 5 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the crosslinking agent was changed to an organic compound containing an oxazoline group, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.25 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.25 μm.
[0055] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0056] Example 6 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone having a particle diameter of 0.46 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran having a particle diameter of 0.46 μm.
[0057] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0058] Example 7 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the crosslinking agent was changed to an organic compound containing an oxazoline group, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.46 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.46 μm.
[0059] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0060] Example 8 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone having a particle diameter of 0.55 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran having a particle diameter of 0.55 μm.
[0061] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0062] Example 9 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the dispersant was changed to styrene maleate, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.55 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.55 μm.
[0063] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0064] Comparative Example 1 A thermosensitive recording medium was prepared in the same manner as in Example 1 above, except that no crosslinking agent was added.
[0065] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0066] Comparative Example 2 A thermal recording medium was prepared in the same manner as in Example 1 above, except that no crosslinking agent was added to the thermal recording layer, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.25 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.25 μm.
[0067] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0068] Comparative Example 3 A thermal recording medium was prepared in the same manner as in Example 1 above, except that no crosslinking agent was added to the thermal recording layer, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.46 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.46 μm.
[0069] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0070] Comparative Example 4 A thermal recording medium was prepared in the same manner as in Example 1 above, except that no crosslinking agent was added to the thermal recording layer, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone having a particle diameter of 0.55 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran having a particle diameter of 0.55 μm.
[0071] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0072] Comparative Example 5 A thermal recording medium was prepared in the same manner as in Example 1 above, except that no crosslinking agent was added to the thermal recording layer, the dispersant was changed to styrene maleate, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.55 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.55 μm.
[0073] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0074] Comparative Example 6 A thermal recording medium was prepared in the same manner as in Example 1 above, except that in the thermal recording layer, the dispersant was changed to polyvinyl alcohol with a degree of polymerization of 500 and a degree of saponification of 86.5 to 89.0, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.55 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.55 μm.
[0075] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0076] Comparative Example 7 A thermal recording medium was prepared in the same manner as in Example 1 above, except that no crosslinking agent was added to the thermal recording layer, the dispersant was changed to polyvinyl alcohol with a degree of polymerization of 500 and a degree of saponification of 86.5 to 89.0, the developer was changed to 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone with a particle diameter of 0.55 μm, and the dye was changed to 3-dibutylamino-6-methyl-7-anilinofluoran with a particle diameter of 0.55 μm.
[0077] Next, the haze value was measured in the same manner as in Example 1. The results are shown in Table 1.
[0078] [Table 1]
[0079] As shown in Table 1, the thermal recording papers of Examples 1 to 3, in which the thermal recording layer contains a dispersant having a carboxyl group and a crosslinking agent (dye and developer particle diameter of 0.15 μm), have smaller haze values than Comparative Example 1, which does not contain a crosslinking agent (dye and developer particle diameter of 0.15 μm), demonstrating improved transparency of the thermal recording medium.
[0080] Furthermore, as shown in Table 1, the thermal recording papers of Examples 4 and 5, in which the thermal recording layer contains a dispersant having a carboxyl group and a crosslinking agent (dye and developer particle diameter of 0.25 μm), have smaller haze values than Comparative Example 2, which does not contain a crosslinking agent (dye and developer particle diameter of 0.25 μm), demonstrating improved transparency of the thermal recording medium.
[0081] Furthermore, as shown in Table 1, the thermal recording papers of Examples 6 to 7, in which the thermal recording layer contains a dispersant having a carboxyl group and a crosslinking agent (dye and developer particle diameter of 0.46 μm), have a smaller haze value than Comparative Example 3, which does not contain a crosslinking agent (dye and developer particle diameter of 0.46 μm), demonstrating improved transparency of the thermal recording medium.
[0082] Furthermore, as shown in Table 1, the thermal recording paper of Example 8, in which the thermal recording layer contains a dispersant having a carboxyl group and a crosslinking agent (dye and developer particle diameter: 0.55 μm), has a smaller haze value than Comparative Example 4, which does not contain a crosslinking agent (dye and developer particle diameter: 0.55 μm), indicating that the transparency of the thermal recording material is improved.
[0083] Furthermore, as shown in Table 1, the thermal recording paper of Example 9, in which the thermal recording layer contains a dispersant having a carboxyl group and a crosslinking agent (the dispersant is styrene maleate, and the particle diameter of the dye and developer is 0.55 μm), has a smaller haze value than Comparative Example 5, which does not contain a crosslinking agent (the dispersant is styrene maleate, and the particle diameter of the dye and developer is 0.55 μm), indicating that the transparency of the thermal recording material is improved.
[0084] In addition, in Comparative Examples 6 to 7 (dye and developer particle diameter 0.55 μm) in which a dispersant without a carboxyl group (polyvinyl alcohol) was used, the transparency of the thermal recording medium was found to be reduced compared to Examples 8 to 9 (dye and developer particle diameter 0.55 μm) in which a dispersant with a carboxyl group (styrene acrylic ammonium salt, or styrene maleate) was used, regardless of the presence or absence of a crosslinking agent. [Industrial Applicability]
[0085] As described above, the present invention is particularly useful for thermosensitive recording media used as labels for containers in which various foods and the like are stored, and as packaging films. [Explanation of symbols]
[0086] 1 Thermal recording medium 2 Base material 3. Thermal recording layer 4. Middle Tier 5 Topcoat layer
Claims
1. A thermal recording medium in which at least a thermal recording layer and an intermediate layer are laminated in this order on a transparent substrate, the heat-sensitive recording layer contains a dispersant having a carboxyl group and a crosslinking agent mainly composed of an epichlorohydrin-modified polyamide polyamine resin or an organic compound containing an oxazoline group, The intermediate layer contains a resin having a core-shell structure, A thermal recording medium, wherein the dispersant is a styreneacrylammonium salt.
2. the thermal recording layer contains at least one of a particulate color former and a particulate color developer, 2. The thermal recording medium according to claim 1, wherein the particle diameter of said color former and the particle diameter of said developer are from 0.1 to 1.0 [mu]m.
Citation Information
Patent Citations
Thermal recording material
JP1996011436A
Thermal recording body
JP2002113947A
Heat sensitive recording body
JP2002316482A
Thermosensitive recording medium
JP2004188706A
Thermal recording material
JP2008194843A