Resin composition, polyimide resin film, and method for producing same

A resin composition with a polyimide precursor and alkoxysilane compound addresses adhesion and peeling challenges in flexible substrates, ensuring strong adhesion and easy peeling with minimal discoloration and high transparency.

JP7564622B2Active Publication Date: 2024-10-09ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2020003861
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-04-17
Filing Date
2020-01-14
Publication Date
2024-10-09
Estimated Expiration
2036-04-13

AI Technical Summary

Technical Problem

Existing resin compositions for polyimide films used in flexible substrates lack sufficient adhesion to supports and are difficult to peel off, particularly in laser peeling processes, with insufficient transparency and potential discoloration during peeling.

Method used

A resin composition containing a polyimide precursor and an alkoxysilane compound with specific absorbance properties at 308 nm, allowing for both strong adhesion to supports and easy peeling, while maintaining transparency, is developed.

Benefits of technology

The composition achieves sufficient adhesion to glass substrates, enables easy peeling with low energy laser irradiation, and maintains transparency, reducing discoloration and improving the suitability for flexible transparent substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564622000001
    Figure 0007564622000001
  • Figure 0007564622000002
    Figure 0007564622000002
  • Figure 0007564622000003
    Figure 0007564622000003
Patent Text Reader

Abstract

To provide a resin composition containing a polyimide precursor which, in addition to having adequate transparency for use in a colorless, transparent flexible substrate, is capable of yielding a polyimide film that realizes both adequate adhesiveness with a support such as a glass substrate, and easy detachability in a separation step using laser peeling and the like.SOLUTION: Provided is a resin composition characterized by containing (a) a polyimide precursor that has a 308 nm absorbance of 0.1-0.8 when formed into a 0.1-μm-thick polyimide resin film by heating for one hour at 350°C, and (b) an alkoxysilane compound having a 308 nm absorbance of 0.1-1.0 at a solution thickness of 1 cm when made into a 0.001-mass% NMP solution.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a polyimide resin film, and a method for producing the same, which are used, for example, for substrates for flexible devices. [Background technology]

[0002] Generally, polyimide (PI) resin films are used for applications that require high heat resistance. General polyimide resins are highly heat-resistant resins that are produced by solution polymerization of aromatic tetracarboxylic dianhydride and aromatic diamine to produce a polyimide precursor, followed by ring-closing dehydration at high temperatures and thermal imidization or chemical imidization using a catalyst. Polyimide resin is an insoluble, infusible, and extremely heat-resistant resin with excellent properties such as thermal oxidation resistance, heat resistance, radiation resistance, low temperature resistance, and chemical resistance. For this reason, polyimide resin is used in a wide range of fields, including electronic materials such as insulating coating agents, insulating films, semiconductors, and electrode protective films for TFT-LCDs. Recently, it has also been considered for use in colorless, transparent, flexible substrates, taking advantage of its lightness and flexibility, as an alternative to glass substrates that have traditionally been used in the field of display materials such as liquid crystal alignment films.

[0003] When a polyimide resin is used as a flexible substrate, a widely used process is, for example, to apply a varnish containing a polyimide resin or a precursor thereof and other components onto a suitable support such as a glass substrate, dry the varnish to form a film, form elements, circuits, etc. on the film, and then peel the film from the glass substrate. Therefore, when a polyimide resin film is applied to a flexible substrate, it is required to have both the contradictory properties of adhesion to the substrate and releasability. To address this issue, a resin composition containing a compound having a specific chemical structure has been disclosed (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 073591 Summary of the Invention [Problem to be solved by the invention]

[0005] However, known resin compositions do not have sufficient properties for use as, for example, a semiconductor insulating film, a TFT-LCD insulating film, an electrode protective film, an ITO electrode substrate for a touch panel, or a heat-resistant colorless transparent substrate for a flexible display. Patent Document 1 describes that the resin composition described therein has an excellent balance between adhesion and releasability. However, the technology described in Patent Document 1 has insufficient adhesion and there is room for further improvement. In recent years, a process of peeling a film from a support by using a laser in the peeling step, so-called "laser peeling technology", has been used. The above Patent Document 1 does not consider the application of the laser peeling at all. When the present inventors confirmed the application of the technology of Patent Document 1 to the laser peeling technology, they found that there is room for improvement in this regard as well.

[0006] The present invention has been made in consideration of the above-described problems, The object of the present invention is to provide a resin composition containing a polyimide precursor, which can give a polyimide film having sufficient transparency for use in a colorless, transparent, flexible substrate, while simultaneously achieving sufficient adhesion to a support such as a glass substrate and easy peelability in a peeling step such as laser peeling. A further object of the present invention is to provide a polyimide resin film and a method for producing the same. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that, in a resin composition containing a polyimide precursor and an alkoxysilane, a polyimide resin film is obtained that has sufficient transparency and sufficient adhesion to a support, and can be easily peeled off in a peeling process such as laser peeling, when the polyimide precursor and the alkoxysilane are used in combination, each of which exhibits an absorbance in a specific range for light of a specific wavelength. Based on these findings, the present invention has been made. That is, the present invention is as follows.

[0008] [1] (a) a polyimide precursor having an absorbance at 308 nm of 0.1 to 0.8 when heated at 350°C for 1 hour to form a polyimide resin film having a thickness of 0.1 μm; (b) an alkoxysilane compound having an absorbance at 308 nm of 0.1 to 1.0 in a 0.001 mass % NMP solution in a 1 cm thickness of the solution; A resin composition comprising: [2] The (b) alkoxysilane compound, The following general formula (1): [ka] In the formula, R represents a single bond, an oxygen atom, a sulfur atom, a carbonyl group, or an alkylene group having 1 to 5 carbon atoms. } and a tetracarboxylic dianhydride represented by the formula An aminotrialkoxysilane compound; The resin composition according to [1], which is a reaction product of

[0009] [3] The (b) alkoxysilane compound is represented by the following general formulas (2) to (4), (9), and (10): [ka] The resin composition according to [1], wherein the compound is at least one selected from the group consisting of compounds represented by the following formula:

[0010] [4] The (a) polyimide precursor is represented by the following formulas (5) and (6): [ka] 4. The resin composition according to claim 1, comprising one or more structural units selected from the structural units represented by the formulae: {wherein X1 and X2 each independently represent a tetravalent organic group having 4 to 32 carbon atoms.}

[0011] [5] The (a) polyimide precursor is represented by the following formula (5-1): [ka] and a structural unit represented by the following formula (5-2): [ka] The resin composition according to [4], having a structural unit represented by the following formula: [6] The resin composition according to [5], wherein a molar ratio of the structural unit represented by the formula (5-1) to the structural unit represented by the formula (5-2) is 90 / 10 to 50 / 50.

[0012] [7] The (a) polyimide precursor is represented by the following formula (6-1): [ka] The resin composition according to [4], having a structural unit represented by the following formula:

[0013] [8] A polyimide resin film which is a cured product of the resin composition according to any one of [1] to [7]. [9] A resin film comprising the polyimide resin film according to [8].

[0014]

[10] A step of applying the resin composition according to any one of [1] to [7] onto a surface of a support; drying the applied resin composition to remove the solvent; a step of heating the support and the resin composition to form a polyimide resin film; peeling the polyimide resin film from the support; A method for producing a polyimide resin film, comprising the steps of:

[11] The method for producing a polyimide resin film according to

[10] , wherein the step of peeling the polyimide resin film from the support includes a step of irradiating a laser from the support side and then peeling.

[12] A laminate comprising a support and a polyimide resin film formed on a surface of the support, the polyimide resin film being a cured product of the resin composition according to any one of [1] to [7].

[0015]

[13] A step of applying the resin composition according to any one of [1] to [7] onto a surface of a support; drying the applied resin composition to remove the solvent; a step of heating the support and the resin composition to form a polyimide resin film; A method for producing a laminate, comprising:

[14] A step of applying the resin composition according to any one of [1] to [7] onto a support; drying the applied resin composition to remove the solvent; a step of heating the support and the resin composition to form a polyimide resin film; forming an element or a circuit on the polyimide resin film; a step of peeling off the polyimide resin film on which the element or circuit is formed from the support; A method for manufacturing a display substrate, comprising: Effect of the Invention

[0016] The resin composition containing the polyimide precursor according to the present invention has sufficient transparency for use as a colorless, transparent, flexible substrate, and can provide a polyimide film that simultaneously exhibits sufficient adhesion to a support such as a glass substrate and easy peelability in a peeling step by laser peeling or the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, exemplary embodiments of the present invention (hereinafter, abbreviated as "embodiments") will be described in detail. Note that the present invention is not limited to the following embodiments, and can be practiced with various modifications within the scope of the gist of the present invention. Note that the structural units in the formulas of the present disclosure do not intend a specific bonding style such as a block structure. In addition, unless otherwise specified, the characteristic values ​​described in the present disclosure are intended to be values ​​measured by the method described in the [Examples] section or a method that is understood to be equivalent to the method by a person skilled in the art.

[0018] <Resin composition> A resin composition provided by one embodiment of the present invention (hereinafter referred to as "the present embodiment") contains (a) a polyimide precursor and (b) an alkoxysilane compound. Hereinafter, each component contained in the resin composition of the present embodiment will be described in order.

[0019] [(a) Polyimide precursor] The polyimide precursor (a) in this embodiment is a polyimide precursor that has an absorbance of 0.1 to 0.8 at 308 nm when heated at 350° C. for 1 hour to form a polyimide resin film with a thickness of 0.1 μm. By setting the absorbance to 0.8 or less, the absorbance in the visible light region is sufficiently suppressed, making it possible to apply the polyimide resin film to flexible transparent substrates and the like, and also making it possible to suppress discoloration of the polyimide resin film after laser peeling. Although the mechanism of laser peeling is not yet clear, the present inventors speculate that the irradiated 308 nm laser light gasifies a part of the polyimide resin film near the support, which is derived from at least one of (a) polyimide precursor and (b) alkoxysilane compound, and the polyimide resin film peels off from the support. However, when the absorbance of the resin film exceeds 0.8, a large amount of gas is generated in a short time, and as a result, the resin film after peeling is discolored. From the viewpoint of more effectively suppressing the discoloration of the resin film after peeling, the above absorbance is preferably 0.7 or less, and particularly preferably 0.6 or less. On the other hand, by making the absorbance 0.1 or more, the resin film can be easily peeled off even by low energy irradiation. If the absorbance is less than 0.1, the resin film on the substrate cannot absorb the energy required for gasification, and therefore cannot be peeled off even when the alkoxysilane compound (b) described below is used. From this point of view, the absorbance is more preferably 0.2 or more, and particularly preferably 0.3 or more.

[0020] The (a) polyimide precursor in this embodiment is a polyamic acid obtained by reacting a tetracarboxylic dianhydride with a diamine. Specific examples of the tetracarboxylic dianhydride include 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (hereinafter, also referred to as 6FDA), 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2 dicarboxylic anhydride, pyromellitic dianhydride (hereinafter, also referred to as PMDA), 1,2,3,4-benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, and biphenyltetracarboxylic dianhydride (hereinafter, BPDA), methylene-4,4'-diphthalic dianhydride, 1,1-ethylidene-4,4'-diphthalic dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-biphenylbis(trimellitic acid monoester acid anhydride) (hereinafter also referred to as TAHQ), 4,4'-oxydiphthalic dianhydride (hereinafter also referred to as ODPA).), thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene dianhydride, 1,4-bis[2-(3,4 -dicarboxyphenyl)-2-propyl]benzene dianhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, bis(3,4-dicarboxy cyclo(phenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 1,2,7,8-phenanthrenetetracarboxylic dianhydride, ethylenetetracarboxylic dianhydride, 1,2,3,4-butanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride (hereinafter referred to as CHDA).), 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride, carbonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, methylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,2-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,1-ethylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 2,2-propylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, thio-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride Examples of the dianhydride include cyclohexane-1,2-dicarboxylic acid) dianhydride, sulfonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, rel-[1S,5R,6R]-3-oxabicyclo[3,2,1]octane-2,4-dione-6-spiro-3'-(tetrahydrofuran-2',5'-dione), 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, and ethylene glycol-bis-(3,4-dicarboxylic acid anhydride phenyl) ether. As the biphenyl tetracarboxylic acid dianhydride, 3,3',4,4'-biphenyl tetracarboxylic acid dianhydride is preferable.

[0021] Specific examples of the diamine include 4,4'-(diaminodiphenyl)sulfone (hereinafter also referred to as 4,4'-DAS), 3,4'-(diaminodiphenyl)sulfone and 3,3'-(diaminodiphenyl)sulfone, 2,2'-bis(trifluoromethyl)benzidine (hereinafter also referred to as TFMB), 2,2-dimethyl-4,4'-diaminobiphenyl, 1,4-diaminobenzene (hereinafter also referred to as p-PD), 1,3-diaminobenzene, 4-aminophenyl-4'-aminobenzoate, 4,4'-diaminobenzoate, 4,4'-(or 3,4' -3,3'-2,4'-)diaminodiphenyl ether, 4,4'-(or 3,3'-)diaminodiphenyl sulfone, 4,4'-(or 3,3'-)diaminodiphenyl sulfide, 4,4'-benzophenone diamine, 3,3'-benzophenone diamine, 4,4'-di(4-aminophenoxy)phenylsulfone, 4,4'-di(3-aminophenoxy)phenylsulfone, 4,4'-bis(4-aminophenoxy)biphenyl, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 2-bis{ 4-(4-aminophenoxy)phenyl}propane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane, 2,2',6,6'-tetramethyl-4,4'-diaminobiphenyl, 2,2',6,6'-tetratrifluoromethyl-4,4'-diaminobiphenyl, bis{(4-aminophenyl)-2-propyl}1,4-benzene, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis(4-aminophenoxyphenyl)fluorene, 3,3'-dimethylbenzidine, 3, 3'-Dimethoxybenzidine and 3,5-diaminobenzoic acid, 2,6-diaminopyridine, 2,4-diaminopyridine, bis(4-aminophenyl-2-propyl)-1,4-benzene, 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (3,3'-TFDB, 2,2'-bis[3(3-aminophenoxy)phenyl]hexafluoropropane (3-BDAF), 2,2'-bis[4(4-aminophenoxy)phenyl]hexafluoropropane (4-BDAF), 2,2'-bis(3-aminophenyl)hexafluoropropane (3,3'-6F), 2,2'-bis(4-aminophenyl)hexafluoropropane (4,4'-6F), etc.

[0022] The structure of the (a) polyimide precursor in the present embodiment is not limited as long as it satisfies the above requirements. However, from the viewpoint of suppressing YI, the polyimide precursor may be one having the structure represented by the following formulas (5) and (6): [ka] It is preferable that the compound has at least one structural unit selected from the structural units represented by the formulae: {wherein X1 and X2 each independently represent a tetravalent organic group having 4 to 32 carbon atoms.}. From the viewpoint of suppressing the coefficient of linear expansion (CTE) as low as possible when the resin composition of the present invention is formed into a cured film, it is preferable that the resin composition has a structural unit represented by the above general formula (5), From the viewpoint of reducing the YI and reducing the birefringence when the resin composition of the present invention is formed into a cured film, it is preferable that the resin composition has a structural unit represented by the above general formula (6). X1 in the formula (5) and X2 in the formula (6) are structural units derived from a tetracarboxylic dianhydride, and are tetravalent groups obtained by removing two acid anhydride groups from the tetracarboxylic dianhydride used.

[0023] X1 in the formula (5) is preferably a tetravalent group derived from one or more tetracarboxylic acid anhydrides selected from PMDA, BPDA, ODPA, 6FDA, and TAHQ. It is preferable that the polymer contains both a tetravalent group derived from PMDA and a tetravalent group derived from BPDA, from the viewpoints of reducing residual stress, improving Tg, and improving mechanical elongation. It is preferable that the copolymer contains both a tetravalent group derived from PMDA and a tetravalent group derived from ODPA or 6FDA from the viewpoint of decreasing the YI and improving the mechanical elongation, and It is preferable for the copolymer to contain both a tetravalent group derived from PMDA and a tetravalent group derived from TAHQ, from the viewpoints of decreasing YI, improving Tg, and improving mechanical elongation.

[0024] The (a) polyimide precursor having a structural unit represented by the above general formula (5) includes a polyimide precursor having the following formula (5-1): [ka] and a structural unit represented by the following formula (5-2): [ka] A polyimide precursor having a structural unit represented by the following formula is preferred.

[0025] Here, the ratio (molar ratio) of the structural units (5-1) and (5-2) of the copolymer is preferably (5):(6)=90:10 to 50:50 from the viewpoint of the CTE and yellowness index (YI) of the resulting polyimide resin film. The ratio of the above formulas (5) and (6) is, for example, 1 It can be determined from the results of H-NMR spectrum. The copolymer may be a block copolymer or a random copolymer. Such a polyimide precursor (copolymer) can be obtained by polymerizing PMDA, 6FDA, and TFMB. That is, PMDA and TMFB are polymerized to form a structural unit (5-1), and 6FDA and TFMB are polymerized to form a structural unit (5-2). The ratio of the structural units (5-1) and (5-2) can be adjusted by changing the ratio of PMDA and 6FDA used.

[0026] The polyimide precursor (a) in the present embodiment may contain structural units other than the structural unit represented by the above formula (5) as necessary, within the scope that does not impair the performance expected by the present invention. In the (a) polyimide precursor (copolymer) according to the present embodiment, the mass of the structural unit (5) is preferably 30 mass% or more based on the total mass of the copolymer from the viewpoint of low CTE, and preferably 70 mass% or more from the viewpoint of low YI, and most preferably 100 mass%.

[0027] X2 in the formula (6) is preferably a tetravalent group derived from one or more tetracarboxylic acid anhydrides selected from PMDA, BPDA, ODPA, 6FDA, and TAHQ. It is preferable that the polymer contains a tetravalent group derived from PMDA or BPDA from the viewpoints of reducing residual stress, improving Tg, and improving mechanical elongation. It is preferable that the copolymer contains a tetravalent group derived from ODPA or 6FDA from the viewpoint of decreasing YI and improving mechanical elongation. It is preferable for the copolymer to contain a tetravalent group derived from TAHQ from the viewpoints of decreasing YI, improving Tg, and improving mechanical elongation.

[0028] X2 in the formula (6) preferably contains a tetravalent group derived from BPDA. In this case, the polyimide precursor is represented by the following formula (6-1): [ka] The biphenyl unit on the left side of the above formula (6-1) is preferably bonded at the 3,3' or 3,4' positions. Such a polyimide precursor can be obtained by polymerization of BPDA and 4,4'-DAS. In this case, other tetracarboxylic dianhydrides may be used together with BPDA, or other diamines may be used together with 4,4'-DAS.

[0029] The polyimide precursor (a) in the present embodiment may contain structural units other than the structural unit represented by the above formula (5) as necessary, to the extent that the desired performance of the present invention is not impaired. In the (a) polyimide precursor (copolymer) according to the present embodiment, the mass of the structural unit (6) is preferably 30% by mass or more based on the total mass of the copolymer from the viewpoint of low birefringence, preferably 70% by mass or more from the viewpoint of low YI, and most preferably 100% by mass.

[0030] The most preferred polyimide precursor (a) in the present embodiment is a polyimide precursor having only the structural unit represented by the above formula (5) or a polyimide precursor having only the structural unit represented by the above formula (6).

[0031] The molecular weight of the (a) polyimide precursor (polyamic acid) of the present invention is preferably 10,000 to 500,000, more preferably 10,000 to 300,000, and particularly preferably 20,000 to 200,000, as weight average molecular weight. If the weight average molecular weight is 10,000 or more, cracks do not occur in the resin film during the process of heating the applied resin composition, and good mechanical properties can be obtained. On the other hand, if the weight average molecular weight is 500,000 or less, the weight average molecular weight can be controlled during the synthesis of the polyamic acid, or a resin composition with an appropriate viscosity can be obtained.

[0032] The number average molecular weight of the (a) polyimide precursor according to the present embodiment is preferably 3,000 to 500,000, more preferably 5,000 to 500,000, even more preferably 7,000 to 300,000, and particularly preferably 10,000 to 250,000. The molecular weight is preferably 3,000 or more from the viewpoint of obtaining good heat resistance and strength (e.g., strength and elongation), and is preferably 500,000 or less from the viewpoint of the solubility of the (a) polyimide precursor in a solvent and from the viewpoint of being able to apply the film at a desired film thickness without bleeding during application. From the viewpoint of obtaining high mechanical elongation, the number average molecular weight is preferably 50,000 or more. In the present disclosure, the weight average molecular weight and the number average molecular weight are values ​​determined by gel permeation chromatography in terms of standard polystyrene.

[0033] In a preferred embodiment, the polyimide precursor (a) may have a part of its structure imidized, as will be described in detail below.

[0034] The polyimide precursor (polyamic acid) (a) in this embodiment can be synthesized by a conventionally known synthesis method, for example, by dissolving a predetermined type and amount of diamine in a solvent to prepare a solution, adding a predetermined type and amount of tetracarboxylic dianhydride to the solution, and stirring the mixture. When dissolving each monomer component, heating may be performed as necessary. The reaction temperature is preferably -30 to 200°C, more preferably 20 to 180°C, and particularly preferably 30 to 100°C. The reaction is preferably performed for 3 to 100 hours, and the polymerization is completed within this range of time. Specifically, after maintaining the above-mentioned preferred reaction temperature for the above-mentioned preferred reaction time, stirring is continued at room temperature (20 to 25°C) or at an appropriate temperature, and the reaction can be terminated when it is confirmed by GPC measurement that the desired molecular weight has been achieved.

[0035] The polyamic acid obtained as described above may be added with N,N-dimethylformamide dimethyl acetal or N,N-dimethylformamide diethyl acetal and heated to esterify a part or all of the carboxylic acids contained in the polyamic acid. This treatment can improve the viscosity stability of the solution containing (a) the polyimide precursor and a solvent during storage at room temperature.

[0036] The above-mentioned ester-modified polyamic acid can be synthesized by pre-esterification in addition to the above-mentioned post-esterification. That is, the above-mentioned tetracarboxylic dianhydride is reacted in advance with one equivalent of monohydric alcohol relative to the acid anhydride group, and then with a suitable dehydration condensing agent such as thionyl chloride or dicyclohexylcarbodiimide, followed by condensation reaction with a diamine to obtain an ester-modified polyamic acid.

[0037] The solvent for the polymerization reaction is not particularly limited as long as it can dissolve the diamine, the tetracarboxylic dianhydride, and the resulting polyamic acid. Specific examples of such solvents include aprotic solvents, phenolic solvents, and ether and glycolic solvents.

[0038] Specifically, examples of the aprotic solvent include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), N-methylcaprolactam, 1,3-dimethylimidazolidinone, tetramethylurea, and the compounds represented by the following general formula (8): [ka] {wherein R1 is a methyl group or an n-butyl group.}; lactone solvents such as γ-butyrolactone and γ-valerolactone; phosphorus-containing amide solvents such as hexamethylphosphoric amide and hexamethylphosphine triamide; sulfur-containing solvents such as dimethylsulfone, dimethylsulfoxide and sulfolane; ketone solvents such as cyclohexanone and methylcyclohexanone; tertiary amine solvents such as picoline and pyridine; and ester solvents such as acetic acid (2-methoxy-1-methylethyl). The compound represented by the above formula (3) is available as a commercially available product. For example, Equamide M100 (R1=methyl group) and Equamide B100 (R1=n-butyl group) manufactured by Idemitsu Kosan Co., Ltd.

[0039] Examples of phenol-based solvents include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol. Examples of ether and glycol solvents include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, and 1,4-dioxane.

[0040] Among these, solvents having a boiling point at normal pressure of 60 to 300° C. are preferred, solvents having a boiling point of 140 to 280° C. are more preferred, and solvents having a boiling point of 170 to 270° C. are particularly preferred. If the boiling point of the solvent is 300° C. or lower, the time of the drying step in film formation can be shortened. By setting the boiling point of the solvent to 60° C. or higher, a uniform resin film without surface roughness or bubbles can be obtained in the drying step. For the same reason, the vapor pressure of the organic solvent at 20° C. is preferably 250 Pa or less.

[0041] From the viewpoints of solubility and edge repellency during coating, it is preferable that the organic solvent has a boiling point of 170 to 270° C. and a vapor pressure of 250 Pa or less at 20° C. More specifically, examples of preferable solvents include N-methyl-2-pyrrolidone, γ-butyrolactone, Equamide M100, and Equamide B100. These solvents may be used alone or in combination of two or more.

[0042] The (a) polyimide precursor (polyamic acid) in the present invention is obtained as a solution in the above-exemplified organic solvent (hereinafter, also referred to as polyamic acid solution). From the viewpoint of film-forming properties, the ratio of the polyamic acid component to the total amount of the obtained polyamic acid solution is preferably 5 to 60 mass%, more preferably 10 to 50 mass%, and particularly preferably 10 to 40 mass%.

[0043] The solution viscosity of the polyamic acid solution at 25°C is preferably 500 to 200,000 mPa·s, more preferably 2,000 to 100,000 mPa·s, and particularly preferably 3,000 to 30,000 mPa·s. The solution viscosity can be measured using an E-type viscometer (VISCONICEHD manufactured by Toki Sangyo Co., Ltd.). If the solution viscosity is 300 mPa·s or more, the solution can be easily applied during film formation. On the other hand, if the solution viscosity is 200,000 mPa·s or less, stirring during synthesis of (a) the polyimide precursor becomes easy. However, even if the solution becomes highly viscous during synthesis of the polyamic acid, it is possible to obtain a polyamic acid solution with a viscosity that is easy to handle by adding a solvent after completion of the reaction and stirring.

[0044] The polyimide precursor (a) of the present embodiment can form a polyimide film having a YI of 15 or less at a thickness of 10 μm, and therefore has an advantage of being easily applicable to a display manufacturing process having a TFT element device on a colorless and transparent polyimide substrate. In a preferred aspect of the present embodiment, the polyimide precursor (a) is dissolved in a solvent (e.g., N-methyl-2-pyrrolidone), the resulting solution is applied to the surface of a support, and the resulting solution is heated (e.g., for 1 hour) at 300 to 550° C. (e.g., 380° C.) in a nitrogen atmosphere to obtain a resin film having a thickness of 10 μm, and the yellowness index YI is 15 or less. When the thickness is not 10 μm, the value at a thickness of 10 μm can be found by a thickness conversion method known to those skilled in the art.

[0045] [Alkoxysilane compounds] Next, the (b) alkoxysilane compound according to this embodiment will be described. The alkoxysilane compound according to the present embodiment has an absorbance at 308 nm when made into a 0.001 wt % NMP solution, and the absorbance is 0.1 to 1.0 in a solution thickness of 1 cm. As long as this requirement is satisfied, the structure is not particularly limited. By having the absorbance within this range, the obtained resin film can be easily peeled off by laser while maintaining high transparency. From the viewpoint of facilitating laser peeling, the absorbance is preferably 0.12 or more, and more preferably 0.15 or more, and from the viewpoint of transparency, the absorbance is preferably 0.4 or less, and more preferably 0.3 or less. The absorption of light having a wavelength of 308 nm by the (b) alkoxysilane compound according to the present embodiment is attributed to functional groups in the compound, such as benzophenone groups, biphenyl groups, diphenyl ether groups, nitrophenol groups, and carbazole groups. The absorbance of light having a wavelength of 308 nm by the alkoxysilane compounds contained in conventionally known resin film precursor compositions was less than 0.1. However, the present invention uses the (b) alkoxysilane compound having a functional group having absorption at a wavelength of 308 nm. This makes it possible to peel off the film by low-energy laser irradiation while suppressing the absorption of visible light by the resulting polyimide resin film.

[0046] The alkoxysilane compound is, for example, Reaction of a tetracarboxylic dianhydride with an aminotrialkoxysilane compound, Reaction of a dicarboxylic acid anhydride with an aminotrialkoxysilane compound; Reaction of an amino compound with an isocyanatotrialkoxysilane compound; Reaction of an amino compound with a trialkoxysilane compound having an acid anhydride group The above tetracarboxylic dianhydrides, dicarboxylic anhydrides, and amino compounds each preferably have an aromatic ring (particularly a benzene ring).

[0047] The alkoxysilane compound according to the present embodiment is represented by the following general formula (1): [ka] {wherein R represents a carbonyl group, a single bond, an oxygen atom, a sulfur atom, or an alkylene group having 1 to 5 carbon atoms.} and a reaction product of an aminotrialkoxysilane compound; The following equations (9) and (10): [ka] and the like.

[0048] The reaction of the tetracarboxylic dianhydride with aminotrialkoxysilane in this embodiment can be carried out, for example, by adding 1 mole of tetracarboxylic dianhydride to a solution obtained by dissolving 2 moles of aminotrialkoxysilane in a suitable solvent, at a reaction temperature of preferably 0° C. to 50° C., and for a reaction time of preferably 0.5 to 8 hours. The solvent is not limited as long as it dissolves the raw material compounds and the product. From the viewpoint of compatibility with the polyimide precursor (a) above, preferred solvents include, for example, N-methyl-2-pyrrolidone, γ-butyrolactone, Equamide M100 (trade name, manufactured by Idemitsu Retail Sales Co., Ltd.), and Equamide B100 (trade name, manufactured by Idemitsu Retail Sales Co., Ltd.).

[0049] From the viewpoints of transparency, adhesion, and releasability, the alkoxysilane compound according to the present embodiment is represented by the above formulas (9) and (10) and the following general formulas (2) to (4): [ka] It is preferable that the compound is at least one selected from the group consisting of the compounds represented by the following formula: The content of the (b) alkoxysilane compound in the resin composition according to the present embodiment can be appropriately designed within a range in which sufficient adhesion and peelability are exhibited. A preferable range is, for example, 0.01 to 20 mass% of the (b) alkoxysilane compound relative to 100 mass% of the (a) polyimide precursor.

[0050] By making the content of the (b) alkoxysilane compound 0.01% by mass or more relative to 100% by mass of the (a) polyimide precursor, it is possible to obtain good adhesion to the support in the obtained resin film. From the viewpoint of storage stability of the resin composition, it is preferable that the content of the (b) alkoxysilane compound is 20% by mass or less. The content of the (b) alkoxysilane compound is more preferably 0.02 to 15% by mass, further preferably 0.05 to 10% by mass, and particularly preferably 0.1 to 8% by mass relative to the (a) polyimide precursor.

[0051] <Resin composition> Another aspect of the present invention provides a resin composition comprising the above-mentioned (a) polyimide precursor and (b) an alkoxysilane compound, and preferably further comprising (c) an organic solvent. The resin composition is typically a varnish.

[0052] [(c) Organic solvent] The (c) organic solvent is not particularly limited as long as it can dissolve the (a) polyimide precursor (polyamic acid) and (b) alkoxysilane compound in the present invention. As such (c) organic solvent, the above-mentioned solvents that can be used in the synthesis of the (a) polyimide precursor can be used. The (c) organic solvent may be the same as or different from the solvent used in the synthesis of the (a) polyamic acid. The amount of (c) organic solvent used is preferably an amount that allows the solid content of the resin composition to be 3 to 50 mass %. The viscosity of the resin composition (25° C.) is preferably 500 mPa·s to 100,000 mPa·s.

[0053] [Other ingredients] The resin composition of the present invention may contain a surfactant, a leveling agent, or the like in addition to the above components (a) to (c).

[0054] (Surfactant or leveling agent) By adding a surfactant or a leveling agent to the resin composition, the coatability of the resin composition can be improved. Specifically, the occurrence of streaks in the coating film after coating can be prevented. Such surfactants or leveling agents include, for example, silicone surfactants, fluorine surfactants, and other nonionic surfactants. Specific examples of these are as follows:

[0055] Silicone surfactants: organosiloxane polymers KF-640, 642, 643, KP341, X-70-092, X-70-093, KBM303, KBM403, KBM803 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.); SH-28PA, SH-190, SH-193, SZ-6032, SF-8428, DC-57, DC-190 (all trade names, manufactured by Toray Dow Corning Silicones Co., Ltd.); SILWET L-77, L-7001, FZ-2105, FZ-2120, FZ-2154, FZ-2164, FZ-2166, L-7604 (all trade names, manufactured by Nippon Unicar Co., Ltd.); DBE-814, DBE-224, DBE-621, CMS-626, CMS-222, KF-352A, KF-354L, KF-355A, KF-6020, DBE-821, DBE-712 (Gelest), BYK-307, BYK-310, BYK-378, BYK-333 (all trade names, manufactured by BYK Japan); Granol (trade name, manufactured by Kyoeisha Chemical Co., Ltd.), etc. Fluorosurfactants: Megafac F171, F173, R-08 (trade names, manufactured by Dainippon Ink and Chemicals, Inc.); Fluorad FC4430, FC4432 (trade names, manufactured by Sumitomo 3M Limited), etc.

[0056] Other nonionic surfactants: polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenol ether, etc. Among these surfactants, from the viewpoint of the coatability of the resin composition (suppression of streaks in the coating film), silicone-based surfactants or fluorine-based surfactants are preferred, and from the viewpoint of reducing the oxygen concentration dependency during curing of the YI value and the total light transmittance, silicone-based surfactants are more preferred.

[0057] When a surfactant or leveling agent is used, the amount thereof is preferably 0.001 to 5 parts by mass, and more preferably 0.01 to 3 parts by mass, per 100 parts by mass of the polyimide precursor (a) in the resin composition.

[0058] After preparing the resin composition containing each of the above-mentioned components, the resulting solution may be heated at 130 to 200°C for 5 minutes to 2 hours to partially imidize the (a) polyimide precursor to an extent that the precursor does not precipitate. The imidization rate can be controlled by appropriately adjusting the temperature and time. By partially imidizing the (a) polyimide precursor, the viscosity stability of the resin composition during storage at room temperature can be improved. In this case, the imidization rate is preferably in the range of 5% to 70%, from the viewpoint of balancing both the solubility of the (a) resin precursor and the storage stability of the resin composition.

[0059] The method for producing the resin composition of the present invention is not particularly limited. For example, when the solvent used in synthesizing the (a) polyimide precursor and the (c) organic solvent are the same, the (b) alkoxysilane compound and other components can be added to the synthesized (a) polyimide precursor solution to prepare a resin composition. After adding the (c) organic solvent and other additives, the mixture may be stirred and mixed at room temperature as necessary. This stirring and mixing can be performed using an appropriate device such as a Three-One Motor (manufactured by Shinto Chemical Co., Ltd.) equipped with stirring blades, a planetary centrifugal mixer, etc. When the viscosity of the varnish is high, heat of 26 to 100°C may be applied in order to reduce the viscosity.

[0060] On the other hand, when the solvent used in synthesizing (a) the polyimide precursor is different from the organic solvent (c), the solvent in the synthesized polyimide precursor solution may be removed by a suitable method such as reprecipitation or solvent distillation to obtain (a) the polyimide precursor, and then (c) the organic solvent and, if necessary, other components may be added and mixed by stirring at a temperature range of room temperature to 80°C.

[0061] The water content of the resin composition according to the present invention is preferably 3,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 500 ppm or less, from the viewpoint of viscosity stability during storage of the resin composition. When the water content of the resin composition is within the above range, the reason why the storage stability is good is unclear. However, it is thought that the water is involved in the decomposition and recombination of the polyimide precursor.

[0062] In a preferred embodiment of the present invention, the resin composition of the present embodiment is applied to the surface of a support, and the resulting coating is heated in a nitrogen atmosphere at 300° C. to 550° C. to obtain a resin film having a thickness of 10 μm, which has a yellowness index of 15 or less. When the film thickness is not 10 μm, the value at a film thickness of 10 μm can be determined by a film thickness conversion method known to those skilled in the art. The resin composition according to the present embodiment has excellent room temperature storage stability, and the rate of change in viscosity when stored at room temperature for two weeks is 10% or less compared to the initial viscosity. Since the resin composition according to the present embodiment has excellent room temperature storage stability, it does not require freezing and is easy to handle.

[0063] The resin composition of the present invention can be used to form a transparent substrate for a display device such as a liquid crystal display, an organic electroluminescence display, a field emission display, electronic paper, etc. Specifically, it can be used to form a substrate for a thin film transistor (TFT), a substrate for a color filter, a substrate for a transparent conductive film (ITO, Indium Thin Oxide), etc.

[0064] <Resin film> Another aspect of the present invention provides a polyimide resin film obtained by heating the above-mentioned resin composition. A step of applying the resin composition onto a surface of a support (application step); A step of drying the applied resin composition and removing the solvent (drying step); a step of heating the support and the resin composition to imidize a resin precursor contained in the resin composition to form a polyimide resin film (heating step); a step of peeling the polyimide resin film from the support (peeling step); The present invention provides a method for producing a resin film, comprising the steps of:

[0065] In the method for producing a resin film according to the present embodiment, the support is not particularly limited as long as it has heat resistance at the drying temperature in the subsequent process and has good peelability. For example, a substrate made of glass (e.g., alkali-free glass), silicon wafer, PET (polyethylene terephthalate), OPP (oriented polypropylene), stainless steel, alumina, copper, nickel, polyethylene glycol terephthalate, polyethylene glycol naphthalate, polycarbonate, polyimide, polyamideimide, polyetherimide, polyetheretherketone, polyethersulfone, polyphenylenesulfone, polyphenylenesulfide, etc. may be used.

[0066] More specifically, the resin composition of the present embodiment is applied onto an adhesive layer formed on the main surface of the substrate, dried, and heated and cured at a temperature of 300 to 500° C. in an inert atmosphere, to form a desired polyimide resin film. Finally, the resulting polyimide resin film is peeled off from the support.

[0067] Examples of the coating method include coating methods using a doctor blade knife coater, an air knife coater, a roll coater, a rotary coater, a flow coater, a die coater, a bar coater, etc., and coating methods such as spin coating, spray coating, and dip coating; Printing techniques such as screen printing and gravure printing; etc. can be applied. The coating thickness of the resin composition in the present invention is appropriately adjusted depending on the thickness of the desired polyimide resin film and the solid content ratio in the resin composition. It is preferably about 1 to 1,000 μm. The coating process may be carried out at room temperature, or the resin composition may be heated in the range of 40 to 80° C. If the latter temperature is adopted, the viscosity of the resin composition decreases, and the workability of the coating process can be improved.

[0068] The coating step is followed by a drying step. The drying step is carried out for the purpose of removing the organic solvent. This drying step can be carried out using an appropriate device such as a hot plate, a box-type dryer, a conveyor-type dryer, etc. The drying temperature is preferably 80 to 200°C, more preferably 100 to 150°C.

[0069] This is followed by a heating step, which is a step for removing the organic solvent remaining in the resin film in the drying step and for promoting the imidization reaction of the polyimide precursor in the resin composition to obtain a polyimide resin film. The heating step can be carried out using an appropriate device such as an inert gas oven, a hot plate, a box-type dryer, a conveyor-type dryer, etc. This heating step may be carried out simultaneously with the drying step, or may be carried out successively following the drying step.

[0070] The heating step may be performed in an air atmosphere or an inert gas atmosphere. From the viewpoints of safety and the transparency and YI value of the resulting polyimide resin film, it is recommended to perform the heating step in an inert gas atmosphere. Examples of the inert gas include nitrogen and argon. The heating temperature in the heating step is preferably 250°C to 550°C, more preferably 300°C to 350°C, depending on the type of (c) organic solvent. If the heating temperature is 250°C or higher, sufficient imidization can be achieved, and if the heating temperature is 550°C or lower, a polyimide resin film having a low YI value and high heat resistance can be obtained. The heating time is preferably about 0.5 to 3 hours.

[0071] In the present invention, the oxygen concentration in the heating step is preferably 2,000 ppm or less, more preferably 100 ppm or less, and even more preferably 10 ppm or less, from the viewpoint of the transparency and YI value of the resulting polyimide resin film. By setting the oxygen concentration at 2,000 ppm or less, the YI value of the resulting polyimide resin film can be set to 15 or less, calculated as a 10 μm film thickness.

[0072] Depending on the application and purpose of the polyimide resin film, a peeling step of peeling the obtained polyimide resin film from the support may be required after the heating step. This peeling step is carried out after cooling the polyimide resin film formed on the substrate to room temperature to about 50°C. The peeling step can be carried out by the following method. (1) A method of obtaining a laminate containing a polyimide resin film / support by the above-mentioned method, irradiating a laser from the support side of the laminate to ablate the interface between the polyimide resin film and the support, thereby peeling off the polyimide resin film. Examples of the type of laser used here include solid (YAG) lasers and gas (UV excimer) lasers. The wavelength of the laser is preferably a spectrum of 308 nm or the like (see JP-T-2007-512568A and JP-T-2012-511173A, etc.). (2) A method in which a polyimide resin film is formed on a release layer previously formed on a support, a laminate including a polyimide resin film / release layer / support is obtained, and then the polyimide resin film is peeled off. Examples of the release layer used here include a method using Parylene (registered trademark, manufactured by Japan Parylene LLC), tungsten oxide, etc.; a method using a vegetable oil-based, silicone-based, fluorine-based, alkyd-based, or other release agent; etc. (3) A method in which a laminate including a polyimide resin film / metal support is obtained by using an etchable metal as a support, and then etching the metal with an etchant to obtain a polyimide resin film. Examples of the metal used here include copper (specific examples include electrolytic copper foil "DFF" manufactured by Mitsui Mining & Smelting Co., Ltd.) and aluminum; Examples of etchants include copper: ferric chloride, aluminum: dilute hydrochloric acid, and the like. (4) A method in which, after obtaining a laminate including a polyimide resin film / support by the above-mentioned method, an adhesive film is attached to the surface of the polyimide resin film, the adhesive film / polyimide resin film is separated from the support, and then the polyimide resin film is separated from the adhesive film.

[0073] Among these peeling methods, From the viewpoints of the refractive index difference between the front and rear surfaces of the resulting polyimide resin film, the YI value, and the elongation, method (1) or method (2) is appropriate; From the viewpoint of the refractive index difference between the front and back of the resulting polyimide resin film, the method (1) is more appropriate. A mode in which the method (1) and the method (2) are used in combination is also suitable (see JP-A-2010-67957, JP-A-2013-179306, etc.). When copper was used as the support in method (3), the YI value of the resulting polyimide resin film was large and the elongation was small. This is thought to be due to some involvement of copper ions.

[0074] The thickness of the polyimide resin film (cured product) according to this embodiment is not particularly limited, but is preferably in the range of 1 to 200 μm, and more preferably 5 to 100 μm. The resin film according to the present embodiment preferably has a yellowness index at a film thickness of 10 μm or less of 15. Such characteristics are satisfactorily achieved, for example, by imidizing the resin precursor of the present disclosure in a nitrogen atmosphere, more preferably at an oxygen concentration of 2,000 ppm or less, at 300° C. to 550° C., more particularly at 350° C.

[0075] <Laminate> Another aspect of the present invention provides a laminate comprising a support and a polyimide resin film formed on a surface of the support, the polyimide resin film being obtained by heating the above-mentioned resin composition. Yet another aspect of the present invention is a method for producing a film-forming material comprising the steps of: applying the above-mentioned resin composition onto a surface of a support; a step (heating step) of heating the support and the resin composition to imidize the polyimide precursor (a) contained in the resin composition to form a polyimide resin film, thereby obtaining a laminate including the support and the polyimide resin film; The present invention provides a method for producing a laminate, comprising: Such a laminate can be produced, for example, by forming a polyimide resin film in the same manner as in the above-mentioned method for producing a resin film, without peeling it off from the support.

[0076] This laminate is used, for example, in the manufacture of a flexible device. More specifically, an element or a circuit is formed on a polyimide resin film formed on a support, and then the support is peeled off to obtain a flexible device having a flexible transparent substrate made of a polyimide resin film. Therefore, another aspect of the present invention provides a flexible device material comprising a polyimide resin film obtained by heating the above-mentioned resin composition.

[0077] As described above, by using the polyimide precursor (a) according to the present embodiment, a resin composition having excellent storage stability and excellent coatability can be produced. The yellowness index (YI value) of the polyimide resin film obtained from this resin composition is less dependent on the oxygen concentration during curing. Therefore, the resin composition is suitable for use in transparent substrates for flexible displays.

[0078] Moreover, the polyimide resin film according to the present embodiment preferably has a yellowness index of 15 or less based on a film thickness of 10 μm. Generally, the less the oxygen concentration dependency in the oven used for producing a polyimide resin film, the more advantageous it is for stably obtaining a resin film with a low YI value. However, the resin composition according to the present embodiment can stably produce a polyimide resin film having a low YI value at an oxygen concentration of 2,000 ppm or less. The polyimide resin film according to the present embodiment preferably has excellent breaking strength from the viewpoint of improving the yield when handling the flexible substrate. Quantitatively, the polyimide resin film preferably has a tensile elongation of 30% or more.

[0079] Another aspect of the present invention provides a polyimide resin film for use in manufacturing a display substrate. A step of applying the resin composition according to the present embodiment onto a surface of a support (application step); a step of heating the support and the resin composition to (a) imidize the polyimide precursor and form the polyimide resin film described above (heating step); a step of forming an element or a circuit on the polyimide resin film (mounting step); a step of peeling off the polyimide resin film on which the element or circuit is formed (peeling step); The present invention provides a method for manufacturing a display substrate, comprising: In the above method, the coating step, the heating step, and the peeling step can be carried out in the same manner as in the above-mentioned method for producing the polyimide resin film and the laminate, respectively.

[0080] The resin film according to the present embodiment, which satisfies the above physical properties, is suitable for applications in which the use of existing polyimide resin films is limited due to their yellow color, particularly as colorless transparent substrates for flexible displays, protective films for color filters, etc. Furthermore, it is suitable for applications such as protective films, light-diffusing sheets and coating films in TFT-LCDs, etc. (e.g., interlayers, gate insulating films, and liquid crystal alignment films for TFT-LCDs); Fields that require colorless transparency and low birefringence, such as ITO substrates for touch panels and resin substrates to replace cover glass for smartphones; When the polyimide according to the present embodiment is applied as a liquid crystal alignment film, it contributes to an increase in the aperture ratio, making it possible to manufacture a TFT-LCD with a high contrast ratio.

[0081] The resin film and laminate produced by using the resin precursor according to the present embodiment can be suitably used, for example, as a substrate in the production of a semiconductor insulating film, a TFT-LCD insulating film, an electrode protection film, and a flexible device. Examples of the flexible device include a flexible display, a flexible solar cell, a flexible touch panel electrode substrate, a flexible lighting device, and a flexible battery. EXAMPLES

[0082] The present invention will now be described in more detail with reference to examples, which are provided for illustrative purposes and are not intended to limit the scope of the present invention. Various evaluations in the examples and comparative examples were carried out as follows.

[0083] (Preparation of polyimide resin film and laminate) The polyamic acid was applied onto alkali-free glass (Corning, 10 cm x 10 cm x 0.7 mm) using a spin coater (MIKASA) so that the film thickness after curing would be 10 μm, and prebaked on a hot plate at 100° C. for 30 minutes. Thereafter, the film was heated and cured in a curing furnace (Koyo Lindberg) under a nitrogen atmosphere at 350° C. for 1 hour to obtain a laminate having the glass substrate and the polyimide film formed above.

[0084] (Adhesion evaluation) The laminate having the polyimide film (thickness: 10 μm) formed on the glass substrate obtained above was cut into a piece having a width of 2.5 cm, and the polyimide film was slightly peeled off from the glass substrate. The peel strength was then measured using an autograph at a peel angle of 180° and a peel speed of 50 mm / min in an atmosphere of 23°C and 50% RH. (Laser peel strength measurement) A laminate having a 10 μm-thick polyimide film on an alkali-free glass substrate, obtained by the coating method and curing method described above, was irradiated with an excimer laser (wavelength 308 nm, repetition rate 300 Hz) to determine the minimum energy required to peel off the entire surface of a 10 cm × 10 cm polyimide film.

[0085] (Measurement of weight average molecular weight and number average molecular weight) The weight average molecular weight (Mw) and the number average molecular weight (Mn) were measured by gel permeation chromatography (GPC) under the following conditions. Solvent: N,N-dimethylformamide (Wako Pure Chemical Industries, Ltd., for high-performance liquid chromatography) to which 24.8 mmol / L lithium bromide monohydrate (Wako Pure Chemical Industries, Ltd., purity 99.5%) and 63.2 mmol / L phosphoric acid (Wako Pure Chemical Industries, Ltd., for high-performance liquid chromatography) were added prior to measurement. Calibration curve for calculating weight average molecular weight: Created using standard polystyrene (manufactured by Tosoh Corporation) Column: Shodex KD-806M (Showa Denko) Flow rate: 1.0mL / min Column temperature: 40℃ Pump: PU-2080Plus (JASCO) Detector: RI-2031Plus (RI: differential refractometer, manufactured by JASCO) UV-2075Plus (UV-VIS: Ultraviolet-visible absorption spectrometer, manufactured by JASCO)

[0086] (Evaluation of Yellowness (YI value)) The resin compositions prepared in each of the above Examples and Comparative Examples were coated on a 6-inch silicon wafer substrate having an aluminum vapor deposition layer on its surface so that the film thickness after curing would be 10 μm, forming a coating film on the substrate. The substrate with the coating film was prebaked at 80° C. for 60 minutes, and then subjected to a heat curing treatment at 350° C. for 1 hour using a vertical curing furnace (manufactured by Koyo Lindberg Co., Ltd., model name VF-2000B) to produce a wafer on which a polyimide film was formed. The wafer was immersed in a dilute hydrochloric acid aqueous solution to peel off the polyimide film, thereby obtaining a polyimide film. The YI (calculated as a film thickness of 10 μm) of the obtained polyimide film was measured using a Nippon Denshoku Industries Co., Ltd. spectrophotometer (SE600) under a D65 light source.

[0087] <Synthesis of alkoxysilane compounds> [Synthesis Example 1] In a nitrogen-substituted 50 ml separable flask, 19.5 g of N-methyl-2-pyrrolidone (NMP) was placed, and 2.42 g (7.5 mmol) of BTDA (benzophenonetetracarboxylic dianhydride) as raw material compound 1 and 3.321 g (15 mmol) of 3-aminopropyltriethoxysilane (product name: LS-3150, manufactured by Shin-Etsu Chemical Co., Ltd.) as raw material compound 2 were further placed, and the mixture was allowed to react at room temperature for 5 hours to obtain an NMP solution of alkoxysilane compound 1.

[0088] [Synthesis Examples 2-4] In the above Synthesis Example 1, the amount of N-methyl-2-pyrrolidone (NMP) used, and the types and amounts of raw material compounds 1 and 2 used were as shown in Table 1, respectively. The same procedure as in Synthesis Example 1 was repeated to obtain NMP solutions of alkoxysilane compounds 2 to 4.

[0089] [Table 1]

[0090] The abbreviations of the compound names in Table 1 have the following meanings: [Raw material compound 1] BTDA: Benzophenonetetracarboxylic dianhydride BPDA: Biphenyltetracarboxylic dianhydride ANPH: 2-amino-4-nitrophenol DACA: 3,6-diaminocarbazole [Raw material compound 2] LS-3150: Product name, manufactured by Shin-Etsu Chemical Co., Ltd., 3-aminopropyltriethoxysilane LS-3415: Product name, manufactured by Shin-Etsu Chemical Co., Ltd., 3-isocyanate propyl triethoxy Silane

[0091] [Absorbance measurement of alkoxysilane compounds at 308 nm] The above alkoxysilane compounds 1 to 4 were each dissolved in 0.001% by mass in NMP, and the resulting solution was filled in a quartz cell having a measurement thickness of 1 cm, and the absorbance at a wavelength of 308 nm was measured using a UV-1600 (manufactured by Shimadzu Corporation). The results are shown in Table 2. Table 2 also shows the absorbance of (3-triethoxysilylpropyl)-t-butylcarbamate (manufactured by GELEST) (alkoxysilane compound 5) measured by the same method.

[0092] [Table 2]

[0093] <Synthesis of polyimide precursor> [Synthesis Example 5] A 500 ml separable flask was replaced with nitrogen, and N-methyl-2-pyrrolidone (NMP) was added as a solvent to the separable flask in an amount such that the solid content after polymerization was 15% by mass. Furthermore, 15.69 g (49.0 mmol) of 2,2'-bis(trifluoromethyl)benzidine (TFMB) was added as a diamine, and the mixture was stirred to dissolve TFMB. Then, 9.82 g (45.0 mmol) of pyromellitic dianhydride (PMDA) and 2.22 g (5.0 mmol) of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) were added as tetracarboxylic dianhydrides. The mixture was then stirred at 80°C for 4 hours under a nitrogen flow to carry out polymerization. After cooling to room temperature, NMP was added to adjust the solution viscosity to 51,000 mPa·s to obtain NMP solution of polyamic acid P-1. The weight average molecular weight (Mw) of the obtained polyamic acid was 180,000.

[0094] [Synthesis Examples 6-11] Polyamic acid NMP solutions P-2 to P-7 were obtained in the same manner as in Synthesis Example 5, except that in Synthesis Example 5, the types and amounts of diamines and tetracarboxylic dianhydrides shown in Table 3 were used. The weight average molecular weights (Mw) of the obtained polyamic acids are also shown in Table 3.

[0095] [Measurement of absorbance of polyimide resin film at 308 nm] Each of the above solutions P-1 to P-7 was spin-coated on a quartz glass substrate and heated at 350°C for 1 hour in a nitrogen atmosphere to obtain a polyimide resin film with a thickness of 0.1 μm. The absorbance of each of these polyimide films was measured at 308 nm using a UV-1600 (manufactured by Shimadzu Corporation). The results are shown in Table 3.

[0096] [Table 3]

[0097] The abbreviations of the compound names in Table 3 have the following meanings: (Diamine) TFMB: 2,2'-bis(trifluoromethyl)benzidine 4,4'-DAS: 4, 4'-(diaminodiphenyl)sulfone p-PD: 1,4-diaminobenzene (Tetracarboxylic acid dianhydride) PMDA: Pyromellitic dianhydride 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic anhydride ODPA: 4,4'-oxydiphthalic dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride CHDA: Cyclohexane-1,2,4,5-tetracarboxylic dianhydride

[0098] [Examples 1 to 8 and Comparative Examples 1 to 4] The types and amounts of polyamic acid solutions and alkoxysilane compounds shown in Table 4 were charged into a vessel and thoroughly stirred to prepare resin compositions containing polyamic acids, which are polyimide precursors. The adhesion, laser peelability, and YI measured for each of the resin compositions by the methods described above are shown in Table 4. In Comparative Examples 2 and 3, the laser intensity in the measurement of the laser peel strength was 300 mJ / cm 2 The YI value in Comparative Example 4 exceeded 30.

[0099] [Table 4]

[0100] From the above results, it was confirmed that the polyimide film obtained from the resin composition according to the present invention is a resin film that has a low yellowness index, a high adhesive strength to a glass substrate, and requires low energy for laser peeling. The present invention is not limited to the above-described embodiment, but can be implemented with various modifications. [Industrial Applicability]

[0101] The present invention can be suitably applied, for example, to a semiconductor insulating film, a TFT-LCD insulating film, an electrode protection film, a flexible display substrate, and a substrate for an ITO electrode of a touch panel, and is particularly suitable as a substrate.

Claims

1. (a) a polyimide precursor having an absorbance at 308 nm of 0.1 to 0.8 when heated at 350° C. for 1 hour to form a polyimide resin film having a thickness of 0.1 μm; (b) an alkoxysilane compound having an absorbance at 308 nm of 0.1 to 1.0 in a 0.001% by mass NMP solution in a 1 cm thickness of the solution; (c) a solvent selected from aprotic solvents, phenolic solvents, and ether and glycol solvents; Contains The (a) polyimide precursor is represented by the following formulas (5) and (6): 【Chemistry 1】 {In the formula, X 1 and X 2 are each independently a tetravalent group having 4 to 32 carbon atoms obtained by removing two acid anhydride groups from a tetracarboxylic dianhydride.}, and the (b) alkoxysilane compound is a reaction product of a tetracarboxylic dianhydride having an aromatic ring with an aminotrialkoxysilane compound, and is a compound having a benzophenone group, a biphenyl group, a diphenyl ether group, a nitrophenol group, or a carbazole group; However, the (b) alkoxysilane compound is represented by the following formula: 【Chemistry 2】 The resin composition, except for the compound represented by the formula:

2. (a) a polyimide precursor having an absorbance at 308 nm of 0.1 to 0.8 when heated at 350° C. for 1 hour to form a polyimide resin film having a thickness of 0.1 μm; (b) an alkoxysilane compound having an absorbance at 308 nm of 0.1 to 1.0 in a 0.001% by mass NMP solution in a 1 cm thickness of the solution; (c) a solvent selected from aprotic solvents, phenolic solvents, and ether and glycol solvents; Contains The (a) polyimide precursor is represented by the following formulas (5) and (6): 【Chemistry 3】 {In the formula, X 1 and X 2 are each independently a tetravalent group having 4 to 32 carbon atoms obtained by removing two acid anhydride groups from a tetracarboxylic dianhydride.}, and The resin composition, characterized in that the (b) alkoxysilane compound is a reaction product of a dicarboxylic acid anhydride having an aromatic ring and an aminotrialkoxysilane compound, and is a compound having a benzophenone group, a biphenyl group, a diphenyl ether group, a nitrophenol group, or a carbazole group.

3. (a) a polyimide precursor having an absorbance at 308 nm of 0.1 to 0.8 when heated at 350° C. for 1 hour to form a polyimide resin film having a thickness of 0.1 μm; (b) an alkoxysilane compound having an absorbance at 308 nm of 0.1 to 1.0 in a 0.001% by mass NMP solution in a 1 cm thickness of the solution; (c) a solvent selected from aprotic solvents, phenolic solvents, and ether and glycol solvents; Contains The (a) polyimide precursor is represented by the following formulas (5) and (6): 【Chemistry 4】 {In the formula, X 1 and X 2 are each independently a tetravalent group having 4 to 32 carbon atoms obtained by removing two acid anhydride groups from a tetracarboxylic dianhydride.}, and The resin composition, characterized in that the (b) alkoxysilane compound is a reaction product of an amino compound having an aromatic ring and an isocyanate trialkoxysilane compound, and is a compound having a benzophenone group, a biphenyl group, a diphenyl ether group, a nitrophenol group, or a carbazole group.

4. (a) a polyimide precursor having an absorbance at 308 nm of 0.1 to 0.8 when heated at 350° C. for 1 hour to form a polyimide resin film having a thickness of 0.1 μm; (b) an alkoxysilane compound having an absorbance at 308 nm of 0.1 to 1.0 in a 0.001% by mass NMP solution in a 1 cm thickness of the solution; (c) a solvent selected from aprotic solvents, phenolic solvents, and ether and glycol solvents; Contains The (a) polyimide precursor is represented by the following formulas (5) and (6): 【Chemistry 5】 {In the formula, X 1 and X 2 are each independently a tetravalent group having 4 to 32 carbon atoms obtained by removing two acid anhydride groups from a tetracarboxylic dianhydride.}, and The resin composition, characterized in that the (b) alkoxysilane compound is a reaction product of an amino compound having an aromatic ring and a trialkoxysilane compound having an acid anhydride group, and is a compound having a benzophenone group, a biphenyl group, a diphenyl ether group, a nitrophenol group, or a carbazole group.

5. The (a) polyimide precursor is represented by the following formula (5-1): 【Chemistry 6】 and a structural unit represented by the following formula (5-2): 【Chemistry 7】 The resin composition according to any one of claims 1 to 4, having a structural unit represented by the following formula:

6. The resin composition according to claim 5, wherein the molar ratio of the structural unit represented by the formula (5-1) to the structural unit represented by the formula (5-2) is 90 / 10 to 50 / 50.

7. The (a) polyimide precursor is represented by the following formula (6-1): 【Chemistry 8】 The resin composition according to any one of claims 1 to 4, having a structural unit represented by the following formula:

8. A step of applying the resin composition according to any one of claims 1 to 7 onto a surface of a support; drying the applied resin composition to remove the solvent; a step of heating the support and the resin composition to form a polyimide resin film; peeling the polyimide resin film from the support; A method for producing a polyimide resin film, comprising the steps of:

9. The method for producing a polyimide resin film according to claim 8 , wherein the step of peeling the polyimide resin film from the support includes a step of irradiating the polyimide resin film with a laser from the support side and then peeling the polyimide resin film.

10. A step of applying the resin composition according to any one of claims 1 to 7 onto a surface of a support; drying the applied resin composition to remove the solvent; and heating the support and the resin composition to form a polyimide resin film.

11. A step of applying the resin composition according to any one of claims 1 to 7 to a support; drying the applied resin composition to remove the solvent; a step of heating the support and the resin composition to form a polyimide resin film; forming an element or a circuit on the polyimide resin film; a step of peeling off the polyimide resin film on which the element or circuit is formed from the support; A method for manufacturing a display substrate, comprising:

Citation Information

Patent Citations

  • JP2017

  • Substrate for flexible device, flexible device and method for producing same, laminate and method for producing same, and resin composition