Silicone acrylic graft copolymer resin, its manufacturing method and coating agent
The silicone-acrylic graft copolymer resin addresses the challenge of achieving transparency and sliding properties by graft copolymerizing acrylic or methacrylic ester monomers with organopolysiloxanes, resulting in a coating agent with enhanced transparency and slidability for diverse substrates.
Patent Information
- Application Number
- JP2023064969
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2038-12-03
AI Technical Summary
Existing silicone-based coating agents struggle to achieve both transparency and sliding properties, with issues such as whitening and reduced haze values, and silicone resins with phenyl groups lack the tactile properties required for sliding.
A silicone-acrylic graft copolymer resin is developed by graft copolymerizing acrylic or methacrylic ester monomers with specific organopolysiloxanes, comprising a ratio of polyorganosiloxane and monomers that enhance transparency and slidability.
The silicone-acrylic graft copolymer resin provides a coating agent with excellent transparency and slidability, forming a strong sea-island structure that imparts water resistance, weather resistance, and sliding properties to various substrates.
Smart Images

Figure 0007564910000001 
Figure 0007564910000002 
Figure 0007564910000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a graft copolymer resin obtained by graft copolymerizing a specific organopolysiloxane with a (meth)acrylic monomer or a mixed monomer component mainly composed of the same, and more specifically to a silicone acrylic graft copolymer resin which, as a coating agent, can impart sliding properties while maintaining transparency, a method for producing the same, and a coating agent containing the resin. [Background technology]
[0002] Silicone-based resins have been known as resins capable of imparting slidability to substrates. However, when silicone-based resins are used as coating agents, they have problems such as whitening of the coating film.
[0003] Therefore, silicone-based coating agents that can provide sliding properties without whitening have been developed. Specifically, silicone-based resins that form highly transparent films have been developed, and coating agents are obtained by mixing silicone-based resins with emulsions that have film-forming properties, such as urethane-based, acrylic-based, and vinyl chloride-based emulsions.
[0004] For example, JP 2013-67787 A (Patent Document 1) discloses that a coating agent made by mixing a urethane-, acrylic-, or vinyl chloride-based emulsion with a silicone-based resin can impart water repellency to a substrate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-67787 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the resin described in Patent Document 1 above was unable to achieve both sliding properties and transparency, and there was room for improvement in the point that the haze value of the coating film decreased (whitened) depending on the amount added. Also, although silicone resins into which phenyl groups have been introduced are effective in improving transparency, there was room for improvement in that the touch and sliding properties originally required of silicone were inferior compared to silicone resins containing only methyl groups, and satisfactory performance was not necessarily obtained.
[0007] Therefore, an object of the present invention is to provide a silicone acrylic graft copolymer resin capable of imparting transparency and sliding properties, a method for producing the same, and a coating agent containing the copolymer resin. [Means for solving the problem]
[0008] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, they discovered that a silicone acrylic graft copolymer resin obtained by graft copolymerizing an acrylic acid ester monomer and / or a methacrylic acid ester monomer onto a specific organopolysiloxane shown below has excellent transparency and sliding properties and is capable of solving the above-mentioned problems, thereby completing the present invention.
[0009] That is, the present invention provides the following silicone acrylic graft copolymer resin, its production method, and coating agent. A silicone acrylic graft copolymer resin obtained by polymerizing 50 to 99 parts by mass of (A) a polyorganosiloxane and 1 to 50 parts by mass of (B) an acrylic acid ester monomer and / or a methacrylic acid ester monomer (wherein the total of components A and B is 100 parts by mass), The (A) polyorganosiloxane is (a1) RSiO 1.0 (a2) RSiO 1.5 Units and / or SiO 2.0 RSiO 0.5 The silicone acrylic graft copolymer resin may contain 0 to 1 mol % of the unit based on the total moles of all siloxane units. (In the formula, R are each independently an alkoxy group having 1 to 20 carbon atoms, a hydroxyl group, or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, with the proviso that at least one R is an alkenyl group having 2 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms in which some of the hydrogen atoms bonded to the carbon atoms of the alkyl group have been substituted with mercapto groups, acryloxy groups, or methacryloxy groups). Effect of the Invention
[0010] The silicone acrylic graft copolymer resin of the present invention provides a coating agent having excellent transparency and sliding properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The silicone acrylic graft copolymer resin of the present invention is This is a silicone acrylic graft copolymer resin obtained by polymerizing 50 to 99 parts by mass of (A) polyorganosiloxane and 1 to 50 parts by mass of (B) acrylic acid ester monomer and / or methacrylic acid ester monomer (wherein the total of components A and B is 100 parts by mass). The polyorganosiloxane is represented by the following formula: (a1) R2SiO 1.0 (a2) RSiO 1.5 Units and / or SiO 2.0 RSiO 0.5 The unit may be contained in an amount of 0 to 1 mol % based on the total moles of all siloxane units.
[0012] In the above formula, R are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a hydroxyl group, provided that at least one R is an alkenyl group having 2 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms in which some of the hydrogen atoms bonded to the carbon atoms of the alkyl group are substituted with mercapto groups, acryloxy groups, or methacryloxy groups.
[0013] The silicone acrylic graft copolymer resin of the present invention is a copolymer obtained by graft polymerization of the polyorganosiloxane (A) and an acrylic acid ester monomer and / or a methacrylic acid ester monomer (B). The mass ratio of the components (A) and (B) is 50 to 99 parts by mass of the component (A) to 1 to 50 parts by mass of the component (B), and more preferably 70 to 95 parts by mass of the component (A) to 5 to 30 parts by mass of the component (B) (the total of the components (A) and (B) is 100 parts by mass).
[0014] (A) Polyorganosiloxane is (a1) RSiO 1.0 Units and (a2) RSiO 1.5 Units and / or SiO 2.0 Also includes units, and optionally RSiO 1 / 2Here, R are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, preferably an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group, and preferably a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms. Examples of the alkyl groups include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl groups, cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups, alkenyl groups such as vinyl and allyl groups, aryl groups such as phenyl, tolyl, and naphthyl groups, alkenylaryl groups such as vinylphenyl groups, aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups, and alkenylaralkyl groups such as vinylbenzyl and vinylphenylpropyl groups, and those in which some or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, bromine, and chlorine, acryloxy groups, methacryloxy groups, mercapto groups, carboxyl groups, alkoxy groups, alkenyloxy groups, amino groups, or amino groups substituted with alkyl groups, alkoxy groups, or (meth)acryloxy groups. R is preferably a methyl group. However, at least one of R's is an alkyl group having 1 to 6 carbon atoms in which some of the hydrogen atoms bonded to carbon atoms of the alkyl group are substituted with mercapto groups, acryloxy groups or methacryloxy groups, or an alkenyl group having 2 to 6 carbon atoms, preferably a vinyl group.
[0015] (A) Of all the siloxane units in the polyorganosiloxane, (a1) RSiO 1.0 It is 80 to 99 mol %, more preferably 85 to 99 mol %. If it is less than the lower limit, the lubricity will be significantly reduced, and if it exceeds the upper limit, there will be a problem that the transparency is not effectively improved.
[0016] (A) Of all the siloxane units in the polyorganosiloxane, (a2) RSiO 1.5 and / or SiO 2.0It is 1 to 20 mol %, more preferably 1 to 15 mol %. If it is less than the lower limit, there is no effect of improving transparency during mixing, and if it exceeds the upper limit, there is a problem that emulsification is difficult.
[0017] The component (A) is preferably an organopolysiloxane represented by the following average composition formula (1). [ka] In the formula, R 1 and R 3 are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, R 2 are each independently an alkenyl group having 2 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms in which a portion of the hydrogen atoms bonded to the carbon atoms is substituted with a mercapto group, an acryloxy group or a methacryloxy group; each X is each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a hydroxyl group; each Y is independently a group defined by X, or -[O-Si(X)2] d A group represented by -X, in which at least two of the groups represented by X and Y are hydroxyl groups, and each Z is independently an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group.
[0018] a is a number of 0 or more, b is a positive number that is 79.9 to 98.9% of the total number of a to f, and c is a positive number that is 0.01 to 1% of the total number of a to f, with the proviso that the total ratio of a+b+c to the total number of a to f is 80 to 99%, more preferably 85 to 99%. d and e are each independently a number of 1 or more, and the ratio of d+e to the total number of a to f is 1 to 20%, more preferably 1 to 15%. f is a number that is 0 to 1% of the total number of a to f, preferably 0 to 0.5%. When the M unit is contained, the lower limit of f is 0.05% or more, preferably 0.1% or more. The viscosity and weight average molecular weight of the organopolysiloxane may be such that the number (molar number) of the siloxane units represented by a to f satisfies the above range. For example, the organopolysiloxane has a weight average molecular weight of 10,000 to 500,000, preferably 15,000 to 300,000, and more preferably 50,000 to 100,000. The weight average molecular weight is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0019] In the above formula (1), R 1 and R 3are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. Examples of the alkyl groups include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl groups; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups; alkenyl groups such as vinyl and allyl groups; aryl groups such as phenyl, tolyl, and naphthyl groups; alkenylaryl groups such as vinylphenyl groups; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups; and alkenylaralkyl groups such as vinylbenzyl and vinylphenylpropyl groups. These groups may have some or all of their hydrogen atoms substituted with halogen atoms such as fluorine, bromine, and chlorine, acryloxy, methacryloxy, mercapto, carboxyl, alkoxy, alkenyloxy, amino, or an amino group substituted with an alkyl group, an alkoxy group, or a (meth)acryloxy group. 1 and R 3 is preferably a methyl group.
[0020] In the above formula (1), R 2 is an alkyl group having 1 to 6 carbon atoms, or an alkenyl group having 2 to 6 carbon atoms, in which some of the hydrogen atoms bonded to the carbon atoms are substituted with a mercapto group, an acryloxy group, or a methacryloxy group. For example, a mercaptopropyl group, an acryloxypropyl group, a methacryloxypropyl group, a vinyl group, etc. are preferred.
[0021] In the above formula (1), X's are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a hydroxyl group. Examples of the unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms include R 1Examples of the alkoxy group having 1 to 20 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a hexyloxy group, a heptyloxy group, an octyloxy group, a decyloxy group, and a tetradecyloxy group. X is preferably a hydroxyl group, a methyl group, a butyl group, or a phenyl group.
[0022] In the above formula (1), Y is, independently of each other, a group defined by X or -[O-Si(X)2] d -X, provided that at least two of the groups represented by X and Y are hydroxyl groups.
[0023] In the above formula (1), Z is an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group, and is preferably a hydroxyl group or a methyl group.
[0024] The polyorganosiloxane represented by the above average composition formula (1) is represented, for example, by the following general formula (I). [ka] In the formula, R 1 , R 3 , R 2 , X, Y, and Z are as defined above, a is a number from 0 to 1,000, b is a positive number from 100 to 10,000, c is a positive number from 1 to 100, and d and e are each independently a positive number from 1 to 1,000.
[0025] a is a number from 0 to 1,000, preferably a number from 0 to 200. If a is greater than 1,000, the strength of the resulting coating film is insufficient. b is a positive number from 100 to 10,000, preferably a positive number from 1,000 to 5,000. If b is less than 100, the coating film will have poor flexibility. c is a positive number from 1 to 100, and if it exceeds 100, there is a problem that the abrasion resistance is not improved when coated. d and e are each independently a positive number from 1 to 1,000, preferably a positive number from 1 to 200. In addition, from the viewpoint of crosslinking, it is preferable to use one having at least two, preferably 2 to 4, hydroxyl groups in one molecule, formed at both ends.
[0026] The method for producing such (A) polyorganosiloxane is not particularly limited, but it is preferably in the form of emulsion, and commercially available products may be used. The production method may be a known emulsion polymerization method, and for example, in a water-soluble solvent in the presence of a surfactant, the organosilicon compounds as raw materials are mixed, emulsified, and polymerized, so that it can be easily produced as an organosilicone emulsion composition. More specifically, (a1) R2SiO 1.0 (a2) RSiO 1.5 Units and / or SiO 2.0 The compound can be easily synthesized by emulsifying and dispersing an alkoxysilane or the like serving as a unit source and a silane coupling agent represented by the following general formula (2) in water using an anionic surfactant, and then adding a polymerization catalyst such as an acid as necessary to carry out a polymerization reaction. R 3 (4-e-f) R 4 f Si(OR 5 ) e (2) (In the formula, R 3R represents a monovalent organic group having a polymerizable double bond, particularly an alkyl group having 1 to 6 carbon atoms substituted with an acryloxy group or a methacryloxy group. 4 is an alkyl group having 1 to 4 carbon atoms, R 5 is an alkyl group having 1 to 4 carbon atoms, e is an integer of 2 to 3, f is an integer of 0 to 1, and e+f=2 to 3. The organosilicon compounds that serve as raw materials for each unit will be described in more detail below.
[0027] Above (a1) RSiO 1.0 The units can be obtained by ring-opening polymerization of cyclic organosiloxanes. The cyclic organosiloxanes used as raw materials include hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecamethylcyclohexasiloxane (D6), 1,1-diethylhexamethylcyclotetrasiloxane, phenylheptamethylcyclotetrasiloxane, 1,1-diphenylhexamethylcyclotetrasiloxane, 1,3,5,7-tetravinyltetramethylcyclotetrasiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5,7-tetracyclohexyltetramethylcyclotetrasiloxane, tris(3,3,3-trifluoropropyl)trimethylcyclotrisiloxane, 1,3,5,7-tetra(3-methacryloxypropyl)tetramethy Examples of the tetramethylcyclotetrasiloxane include 1,3,5,7-tetra(3-acryloxypropyl)tetramethylcyclotetrasiloxane, 1,3,5,7-tetra(3-carboxypropyl)tetramethylcyclotetrasiloxane, 1,3,5,7-tetra(3-vinyloxypropyl)tetramethylcyclotetrasiloxane, 1,3,5,7-tetra(p-vinylphenyl)tetramethylcyclotetrasiloxane, 1,3,5,7-tetra[3-(p-vinylphenyl)propyl]tetramethylcyclotetrasiloxane, 1,3,5,7-tetra(N-acryloyl-N-methyl-3-aminopropyl)tetramethylcyclotetrasiloxane, and 1,3,5,7-tetra(N,N-bis(lauroyl)-3-aminopropyl)tetramethylcyclotetrasiloxane.
[0028] The above (a2) RSiO 1.5 Units (T units) and / or SiO 2.0 The unit (Q unit) is obtained from alkoxysilane, etc. RSiO 1.5 Examples of monomers that form the (T unit) include alkyltrialkoxysilanes such as methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, and ethyltriethoxysilane. SiO 2.0 Examples of monomers that form the units (Q units) include tetraalkoxysilanes such as tetramethoxysilane and tetraethoxysilane.
[0029] Furthermore, it is preferable to copolymerize a silane coupling agent represented by the following general formula (2): The copolymerization of the silane coupling agent has the effect of assisting the bonding of the polyorganosiloxane (A) with the component (B) and the component (C) described below. R 3 (4-e-f) R 4 f Si(OR 5 ) e (2) (In the formula, R 3 R represents a monovalent organic group having a polymerizable double bond, particularly an alkyl group having 1 to 6 carbon atoms substituted with an acryloxy group or a methacryloxy group. 4 is an alkyl group having 1 to 4 carbon atoms, R 5 is an alkyl group having 1 to 4 carbon atoms, e is an integer of 2 to 3, f is an integer of 0 to 1, and e+f=2 to 3.
[0030] Examples of the silane coupling agent represented by the general formula (2) include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane, etc. These silane coupling agents are preferably blended in an amount of 0.01 to 20 parts by mass, more preferably 0.01 to 5 parts by mass, per 100 parts by mass of the cyclic organosiloxane.
[0031] The polymerization catalyst used in the production of the polyorganosiloxane (A) may be a known polymerization catalyst. Among them, strong acids are preferred, and examples thereof include hydrochloric acid, sulfuric acid, dodecylbenzenesulfonic acid, citric acid, lactic acid, and ascorbic acid. Dodecylbenzenesulfonic acid having emulsifying ability is preferred. The amount of the acid catalyst is preferably 0.01 to 10 parts by mass, more preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the cyclic organosiloxane. The polymerization temperature is preferably 50 to 75°C, and the polymerization time is preferably 10 hours or more, and even more preferably 15 hours or more. Furthermore, it is particularly preferred to age the product after polymerization at 5 to 30°C for 10 hours or more.
[0032] The surfactant used in the polymerization reaction is preferably an anionic surfactant. Examples include sodium lauryl sulfate, sodium laureth sulfate, N-acylamino acid salt, N-acyltaurate salt, aliphatic soap, and alkyl phosphate, among which those that are easily soluble in water and do not have a polyethylene oxide chain are preferred. More preferred are N-acylamino acid salt, N-acyltaurate salt, aliphatic soap, and alkyl phosphate, and particularly preferred are sodium lauroyl methyl taurate, sodium myristoyl methyl taurate, and sodium lauryl sulfate. The amount of the anionic surfactant is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, relative to 100 parts by mass of the cyclic organosiloxane.
[0033] The silicone acrylic graft copolymer resin of the present invention is a copolymer obtained by radical polymerization of the polymerizable group of (A) the polyorganosiloxane and the (meth)acrylic group of (B) an acrylic acid ester monomer and / or a methacrylic acid ester monomer (hereinafter collectively referred to as "(meth)acrylic acid ester monomer"). The component (A) can be obtained as an emulsion composition containing the organopolysiloxane (A) and a surfactant by the above-mentioned production method. The graft copolymer resin of the present invention can be obtained by mixing the emulsion composition with the (meth)acrylic acid ester monomer (B) and emulsion-polymerizing it to obtain a graft copolymer resin obtained by polymerization of the above-mentioned (A) and (B) components.
[0034] The component (B) is an acrylic acid ester monomer and / or a methacrylic acid ester monomer, and is an acrylic acid ester monomer or a methacrylic acid ester monomer that does not have a functional group such as a hydroxy group, an amide group, or a carboxyl group. An acrylic acid alkyl ester or a methacrylic acid alkyl ester having an alkyl group with 1 to 10 carbon atoms is preferred, and a monomer that makes the glass transition temperature (hereinafter sometimes referred to as Tg) of the acrylic component polymer 40°C or higher, preferably 60°C or higher, is more preferred. Examples of such a monomer include methyl (meth)acrylate, isopropyl (meth)acrylate, ethyl (meth)acrylate, and cyclohexyl (meth)acrylate. The upper limit of Tg is preferably 200°C or lower, more preferably 150°C or lower. The glass transition temperature can be measured based on JIS K7121.
[0035] In the silicone acrylic graft copolymer resin of the present invention, the mass ratio of the polyorganosiloxane (A) to the (meth)acrylic acid ester monomer (the mass ratio of the polyorganosiloxane of formula (1) to the (meth)acrylic unit) is 50:50 to 99:1, and preferably 60:40 to 99:1. If the ratio of the silicone component is less than 30, there is a risk of a problem in that the abrasion resistance is not improved when coated, which is not preferable.
[0036] A radical initiator is preferably used for the polymerization reaction between the above-mentioned components (A) and (B). Examples of the radical initiator include persulfates such as potassium persulfate and ammonium persulfate, hydrogen persulfate water, t-butyl hydroperoxide, and hydrogen peroxide. If necessary, a redox system using a reducing agent such as sodium sulfite, Rongalite, L-ascorbic acid, tartaric acid, sugars, and amines in combination may be used. The amount of these to be added may be appropriately selected according to a conventionally known method.
[0037] When the component (A) is used in the polymerization reaction as the above-mentioned emulsion composition, the surfactant already contained in the emulsion composition can sufficiently carry out graft polymerization, but it is preferable to further add an anionic surfactant to improve stability. As the anionic surfactant, sodium lauryl sulfate, sodium laureth sulfate, N-acyl amino acid salt, N-acyltaurine salt, aliphatic soap, alkyl phosphate, etc. can be added. In addition, nonionic emulsifiers such as polyoxyethylene lauryl ether and polyoxyethylene tridecyl ether can also be added.
[0038] In the polymerization reaction between the (A) component and the (B) component, a (C) functional group-containing monomer copolymerizable with the (B) component can be further copolymerized. The (C) component is a monomer having an unsaturated bond including a carboxyl group, an amide group, a hydroxyl group, a vinyl group, an allyl group, etc. Examples of the (C) component include methacrylic acid, acrylic acid, acrylamide, allyl methacrylate, vinyl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. By copolymerizing these, the compatibility of the resulting copolymer resin with hydrophilic monomers can be improved. Methacrylic acid, acrylic acid, and 2-hydroxyethyl methacrylate are particularly preferred. The amount of the (C) component may be appropriately selected within a range that does not impair the effects of the present invention. For example, the amount is 0.5 to 20 parts by mass, preferably 2 to 10 parts by mass, based on 100 parts by mass of the total of the (A) component and the (B) component.
[0039] The graft polymerization temperature of the component (B) and optional component (C) is preferably 25 to 55° C., more preferably 25 to 40° C. The polymerization time is preferably 2 to 8 hours, more preferably 3 to 6 hours.
[0040] Furthermore, a chain transfer agent can be added to adjust the molecular weight and graft ratio of the graft polymer. Examples of the chain transfer agent include normal octyl mercaptan. The amount of the agent to be added may be appropriately selected according to a conventionally known method.
[0041] The silicone acrylic graft copolymer resin of the present invention is a polymer in which the (B) component and optional (C) component are randomly grafted to the (A) organopolysiloxane. The silicone acrylic graft copolymer resin can be produced as an emulsion composition by the above-mentioned method. In this case, the solid content of the silicone acrylic graft copolymer resin in the emulsion composition is preferably 35 to 50 mass %. The viscosity (25°C) is preferably 500 mPa·s or less, more preferably 50 to 500 mPa·s. The viscosity can be measured by a rotational viscometer. The average particle size of the emulsion is preferably 0.1 μm (100 nm) to 0.5 μm (500 nm), more preferably 0.15 μm (150 nm) to 0.3 μm (300 nm).
[0042] The silicone acrylic graft copolymer resin of the present invention may be granulated and powdered by the following methods. That is, spray drying, air flow drying, etc. may be mentioned, but a spray dryer is preferred in terms of productivity. Powdering is preferably performed by hot drying, and preferably at 80 to 150°C. The smaller the average particle size of the obtained powder particles, the better, and it is preferably 50 μm or less, and more preferably 1 to 40 μm. In the present invention, the particle size of the above emulsion and powder is measured using a cumulative mass average value D 50 It can be measured as:
[0043] The silicone acrylic graft copolymer resin of the present invention can be used as a coating agent. The solid content in the coating agent is preferably 1 to 60 mass%, more preferably 5 to 30 mass%, and even more preferably 5 to 20 mass%. If the silicone acrylic graft copolymer resin is less than 1 mass%, there is a problem that no improvement in abrasion resistance is observed, and if it exceeds 60 mass%, there is a problem that whitening occurs and the abrasion resistance also decreases. In addition, the emulsion composition of the silicone acrylic graft copolymer resin obtained by the above-mentioned method may be used as a coating agent as it is. In addition, the coating agent may not contain a solvent. The method of use as a coating agent may be appropriately selected according to conventionally known coating agents.
[0044] When the silicone acrylic graft copolymer resin of the present invention is used as a coating agent, it may be mixed with a resin emulsion other than the silicone acrylic graft copolymer resin. The resin emulsion should have a film-forming ability, and examples thereof include acrylic resin emulsions using (meth)acrylic monomers such as (meth)acrylic acid and (meth)acrylic acid esters, urethane resin emulsions, vinyl chloride resin emulsions using vinyl chloride, vinyl chloride / vinyl acetate, or vinyl chloride / (meth)acrylic acid or its esters, etc. By mixing these in a water system using a known mixing and preparation method such as a propeller stirrer or homogenizer, a coating agent composition can be obtained. When mixed with a resin emulsion having film-forming ability, the blending amounts are preferably 1 to 40 mass% silicone acrylic graft copolymer resin in terms of solid content, and 60 to 99 mass% of at least one resin emulsion selected from a urethane resin emulsion, an acrylic resin emulsion, and a vinyl chloride resin emulsion (however, the total is 100 parts by mass), and preferably 5 to 35 mass% and more preferably 10 to 30 mass% silicone acrylic graft copolymer resin in terms of solid content, and 65 to 95 mass% and more preferably 70 to 90 mass% of the resin emulsion (however, the total is 100 parts by mass).
[0045] In addition, antioxidants, colorants, ultraviolet absorbers, light stabilizers, antistatic agents, plasticizers, flame retardants, thickeners, surfactants, organic solvents such as film-forming assistants, other resins, and the like may be added within a range that does not affect the performance of the present invention.
[0046] When the coating composition of the present invention is applied or immersed on one or both sides of various substrates such as plastics (PET, PI, synthetic leather, etc.), glass (general-purpose glass, SiO2, etc.), metals (Si, Cu, Fe, Ni, Co, Au, Ag, Ti, Al, Zn, Sn, Zr, alloys thereof, etc.), wood, fibers (cloth, thread, etc.), paper, ceramics (fired oxides, carbides, nitrides, etc.), etc.), and dried (room temperature to 150°C), it is possible to impart the advantages of the silicone copolymer resin, such as water repellency, weather resistance, heat resistance, cold resistance, gas permeability, and sliding properties, for a long period of time while maintaining the advantages of the resin emulsion. This is believed to be because the resin emulsion having film-forming ability and the silicone copolymer resin of the present invention form a strong sea-island structure.
[0047] Here, examples of the plastic substrate include poly(meth)acrylic acid esters such as polymethyl methacrylate, polycarbonate, polystyrene, polyethylene terephthalate, polyvinyl chloride, polyester, cellulose, diethylene glycol bisallyl carbonate polymer, acrylonitrile-butadiene-styrene polymer, polyurethane, and epoxy resin. Examples of plastic processed products include automobile interior materials, organic glass, electrical materials, building materials, exterior materials for buildings, optical films used in liquid crystal displays, light diffusion films, mobile phones, and home appliances. Drying methods include leaving the substrate at room temperature for 1 to 10 days, but from the viewpoint of rapidly progressing curing, a method of heating the substrate at a temperature of 20 to 150°C for 1 second to 10 hours is preferred. In addition, when the plastic substrate is made of a material that is easily deformed or discolored by heating, drying is preferably performed at a relatively low temperature of 20 to 100°C.
[0048] As the glass substrate, soda-lime glass, quartz glass, lead glass, borosilicate glass, alkali-free glass, etc. are used. As the glass processed products, there are architectural plate glass, glass for vehicles such as automobiles, glass for lenses, glass for mirrors, glass for display panels, glass for solar cell modules, etc. As a method for drying, a method of leaving it at room temperature for about 1 to 10 days or heating it at a temperature of 20 to 150°C, particularly 60 to 150°C, for 1 second to 10 hours is preferable.
[0049] As the wood substrate, wood from the family Maple, Betulaceae, Lauraceae, Chestnut, Scrophulariaceae, Araucaria, Ulmaceae, Bignoniaceae, Rosaceae, Cupressaceae, Dipterocarpaceae, Myrtaceae, Fagaceae, Pinaceae, Fabaceae, Oleaceae, etc. is used. The wood processed product may be selected from processed and molded products made from wood itself, plywood and laminated lumber, processed and molded products thereof, and combinations thereof, and includes, for example, building materials including materials for the exterior and interior of buildings, furniture such as desks, wooden toys, musical instruments, etc. A method of hot air drying at 20 to 150°C, particularly 50 to 150°C, for 0.5 to 5 hours is preferred. In addition, discoloration of the coating film can be avoided by keeping the drying temperature at 120°C or less.
[0050] Examples of the fiber substrate include natural fibers such as cotton, hemp, linen, wool, silk, cashmere, and asbestos, and chemical fibers such as polyamide, polyester, viscose, cellulose, glass, and carbon. Examples of the processed fiber products include all kinds of woven fabrics, knitted fabrics, nonwoven fabrics, films, and papers. As a drying method, a method of leaving it at room temperature for 10 minutes to several tens of hours or drying at a temperature of 20 to 150°C for 0.5 minutes to 5 hours is preferable.
[0051] The method for applying the coating composition of the present invention is not particularly limited, and examples thereof include application methods using various coaters such as a gravure coater, a bar coater, a blade coater, a roll coater, an air knife coater, a screen coater, a curtain coater, and brush coating, spray coating, immersion, etc. The amount of application is not particularly limited, but is usually preferably 1 to 300 g / m2 in terms of solid content from the viewpoints of antifouling properties, application workability, etc. 2 , more preferably 5 to 100 g / m 2 The film may be formed by drying naturally or by heating at 100 to 200° C. EXAMPLES
[0052] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, parts and % respectively indicate parts by mass and % by mass.
[0053] [Example 1] i) Preparation of an emulsion composition containing organopolysiloxane 555g of octamethylcyclotetrasiloxane (D4), 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 44g of KBE-13 (methyltriethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 430g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying the silicone emulsion composition at 105° C. for 3 hours, the non-volatile content was 44.5%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 225g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.9%.
[0054] [Example 2] i) Preparation of an emulsion composition containing organopolysiloxane 578g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 22g of KBE-13 (methyltriethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 450g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying the silicone emulsion composition at 105° C. for 3 hours, the non-volatile content was 44.7%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 225g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.8%.
[0055] [ Reference example 3] i) Preparation of an emulsion composition containing organopolysiloxane 542g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 58g of KBE-04 (tetraethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 400g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying this silicone emulsion composition at 105°C for 3 hours, the non-volatile content was 44.6%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 215g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.8%.
[0056] [Example 4] i) Preparation of an emulsion composition containing organopolysiloxane 566g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 34g of KBM-13 (methyltrimethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 450g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying the silicone emulsion composition at 105° C. for 3 hours, the non-volatile content was 44.5%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 225g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 45.2%.
[0057] [Example 5] i) Preparation of an emulsion composition containing organopolysiloxane 583g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 17g of KBM-13 (methyltrimethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 460g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying this silicone emulsion composition at 105°C for 3 hours, the non-volatile content was 45.4%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 230g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 45.5%.
[0058] [Example 6] i) Preparation of an emulsion composition containing organopolysiloxane 559g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 22g of KBE-13 (methyltriethoxysilane), 19g of KBE-04 (tetraethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. After that, 410g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours, after which it was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying this silicone emulsion composition at 105°C for 3 hours, the non-volatile content was 44.8%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 215g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 45.3%.
[0059] [Example 7] i) Preparation of an emulsion composition containing organopolysiloxane 555g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 44g of KBE-13 (methyltriethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 430g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying the silicone emulsion composition at 105° C. for 3 hours, the non-volatile content was 44.5%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 60g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, yielding an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.8%.
[0060] [Example 8] i) Preparation of an emulsion composition containing organopolysiloxane 450g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 150g of KBE-13 (methyltriethoxysilane), 18g of sodium lauryl sulfate dissolved in 100g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 280g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying the silicone emulsion composition at 105° C. for 3 hours, the non-volatile content was 44.5%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 205g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.8%.
[0061] [Comparative Example 1] i) Preparation of an emulsion composition containing organopolysiloxane 600g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 460g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying this silicone emulsion composition at 105°C for 3 hours, the non-volatile content was 45.3%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 230g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.7%.
[0062] [Comparative Example 2] i) Preparation of an emulsion composition containing organopolysiloxane 597.6g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 2.4g of KBE-13 (methyltriethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 460g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying this silicone emulsion composition at 105°C for 3 hours, the non-volatile content was 45.1%, and the organopolysiloxane in the emulsion was in the form of a non-fluid soft gel. ii) Preparation of silicone acrylic graft copolymer resin While dropping 230g of methyl methacrylate (MMA) into the silicone emulsion composition obtained above over a period of 3 to 5 hours, a peroxide and a reducing agent were added at 30°C to carry out an oxidation-reduction reaction to effect acrylic graft copolymerization, thereby obtaining an emulsion composition containing a silicone acrylic graft copolymer resin. The non-volatile content of the emulsion composition was 44.7%.
[0063] [Comparative Example 3] A solution of 300 g of octamethylcyclotetrasiloxane, 0.6 g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 300 g of KBE-13 (methyltriethoxysilane), 6 g of sodium lauryl sulfate dissolved in 54 g of ion-exchanged water, and 6 g of dodecylbenzenesulfonic acid dissolved in 54 g of pure water were charged into a 2 L polyethylene beaker, but it was not possible to emulsify the mixture using a homomixer.
[0064] [Comparative Example 4] 555g of octamethylcyclotetrasiloxane, 0.6g of KBM-502 (γ-methacryloxypropylmethyldimethoxysilane), 44g of KBE-13 (methyltriethoxysilane), 6g of sodium lauryl sulfate dissolved in 54g of ion-exchanged water, and 6g of dodecylbenzenesulfonic acid dissolved in 54g of pure water were charged into a 2L polyethylene beaker and emulsified uniformly using a homomixer. Then, 430g of ion-exchanged water was gradually added to dilute the mixture, and the mixture was stirred at a pressure of 300kgf / cm. 2 The mixture was passed through a high-pressure homogenizer twice at 100°C to obtain a uniform white emulsion. This emulsion was transferred to a 2 L glass flask equipped with a stirrer, thermometer, and reflux condenser, and subjected to a polymerization reaction at 50-70°C for 24 hours. After that, the mixture was neutralized with 12 g of a 10% aqueous sodium carbonate solution to a pH of 6-8 to obtain a silicone emulsion composition. After drying this silicone emulsion composition at 105°C for 3 hours, the non-volatile content was 44.5%, and the organopolysiloxane in the emulsion was in the form of a non-flowable soft gel.
[0065] For the emulsion compositions containing organopolysiloxane prepared in the above Examples and Comparative Examples, the constituent ratio of siloxane units, the parts by mass of each component, and the average particle size, solid content, and pH of the emulsion measured by the methods described below are shown in Table 1.
[0066] The emulsion compositions containing the silicone acrylic graft copolymer resins obtained in the above Examples and Comparative Examples were subjected to the following evaluation tests. The results are shown in Table 2. <Measurement of evaporation residue (solid concentration)> Weigh approximately 1 g of the emulsion composition containing the silicone acrylate graft copolymer resin into a dish made of aluminum foil, place it in a dryer maintained at 105 - 110 °C, heat it for 1 hour, take it out of the dryer, and let it cool in a desiccator. Then weigh the weight of the silicone acrylate graft copolymer resin after drying, and calculate the evaporation residue by the following formula.
Equation
[0067] <Measurement of average particle size> Weigh 0.01 g of the emulsion composition containing the silicone acrylate graft copolymer resin, and use a laser diffraction particle size distribution analyzer (manufactured by Horiba, Ltd., product name: LA-950V2) to measure the average particle size of the emulsion (the value of the particle size corresponding to 50% of the particle size cumulative distribution) under the following conditions. [Measurement conditions] Measurement temperature: 25 ± 1 °C Solvent: Ion-exchanged water Also, the average particle size of the emulsion in the emulsion composition containing (A) organopolysiloxane was measured by the same method as above. The results are shown in Table 1.
[0068] <pH measurement> Using a pH meter HM-25R manufactured by Toa DKK Corporation, measure the pH of the emulsion composition containing the silicone acrylate graft copolymer resin at 25 °C based on JIS Z8802:2011.
[0069] <Film-forming method> Apply the emulsion composition containing the silicone acrylate graft copolymer resin to a slide glass with a bar coater, dry it at 105 °C for 3 minutes, and form a coating film to be approximately 23 μm thick when dry.
[0070] <Haze value measurement> The haze value of the coating film was measured using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) The preferred range of haze value on a slide glass (haze value 0.70%) is 0.70 to 1.50.
[0071] <Static and dynamic friction coefficient measurement> A 200 g metal indenter was placed in contact with the coating film perpendicularly using a HEIDON TYPE-38 (manufactured by Shinto Scientific Co., Ltd.), and the frictional force was measured when the indenter was moved at 3 cm / min, from which the friction coefficient was calculated. The preferred ranges for the static and kinetic friction coefficients on a slide glass are 0.01 to 0.15 for the static friction coefficient and 0.01 to 0.10 for the kinetic friction coefficient.
[0072] [Table 1]
[0073] [Table 2]
[0074] As shown in Table 2 above, the graft copolymer resin obtained using an organopolysiloxane having a low ratio of (a2) units to (a1) units or not containing (a2) units gave a coating film with a high haze value and insufficient transparency (Comparative Examples 1 and 2). The organopolysiloxane of Comparative Example 3 did not emulsify because it contained too much methyltriethoxysilane. The coating film obtained from the organopolysiloxane emulsion composition of Comparative Example 4, in which methyl methacrylate (MMA) was not polymerized, was poor in both transparency and sliding properties. In contrast, as shown in Table 2, the graft copolymer resin of the present invention, when applied to a slide glass (haze value 0.70%), gave a coating film with excellent transparency, a haze value of 1.0 to 1.3%, and small static and dynamic friction coefficients, resulting in excellent sliding properties.
[0075] [ reference Examples 9 to 18 and referenceComparative Examples 5 to 9 Polycarbonate-based polyurethane resin emulsion (Permarine UA-368, water-based paint resin, manufactured by Sanyo Chemical Industries, Ltd.) and each of the silicone acrylic graft copolymer resin emulsion compositions 1 to 10 and 12 listed in Table 2 were mixed in the ratios shown in Table 3 in terms of solid content, stirred and mixed at room temperature for 10 minutes, and then filtered through an 80 mesh. The mixture was applied to a slide glass with a bar coater and dried at 105°C for 3 minutes to form a coating film with a dry thickness of approximately 23 μm. <Haze value measurement> The haze value of the coating film was measured using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) The preferred range of the haze value on a glass slide (haze value 0.70%) is 0.7 to 6.0%. <Static and dynamic friction coefficient measurement> A 200 g metal indenter was placed in contact with the coating film perpendicularly using a HEIDON TYPE-38 (manufactured by Shinto Scientific Co., Ltd.), and the frictional force was measured when the indenter was moved at 3 cm / min, and the friction coefficient was calculated from the frictional force. The preferred ranges for the static and kinetic friction coefficients on a slide glass are 0.01 to 0.20 for the static friction coefficient and 0.01 to 0.10 for the kinetic friction coefficient.
[0076] [Table 3]
[0077] As shown in Table 3, reference Even when emulsion compositions 9, 10, and 12 of the silicone acrylic graft copolymer resin obtained in Comparative Examples 1, 2, and 4 were mixed with a polyurethane resin emulsion, the sliding properties were improved, but the haze value was high and the transparency was poor. In contrast, by mixing the silicone acrylic graft copolymer resin of the present invention with a polyurethane resin emulsion, it is possible to form a film with improved sliding properties and good transparency. However, reference As shown in Comparative Example 9, if the blending ratio of the silicone acrylic graft copolymer resin of the present invention is too high when mixed with the resin emulsion, the haze value becomes high, which is not preferable. [Industrial Applicability]
[0078] The silicone acrylic graft copolymer resin of the present invention has excellent transparency and sliding properties and is useful as a coating agent to be applied to the surfaces of various substrates.
Claims
1. An emulsion composition comprising a silicone acrylic graft copolymer resin obtained by polymerizing 50 to 99 parts by mass of (A) a polyorganosiloxane and 1 to 50 parts by mass of an acrylic acid ester monomer and / or a methacrylic acid ester monomer (B) (wherein the total of components A and B is 100 parts by mass), in an amount of 1 to 60% by mass in terms of solid content relative to the total mass of the composition, The polyorganosiloxane (A) is 2 SiO 1.0 (a2) RSiO 1.5 Units and / or SiO 2.0 % based on the total moles of all siloxane units, and optionally R 3 SiO 0.5 units in an amount of 0 to 1 mol % based on the total moles of all siloxane units (wherein, R are each independently an alkoxy group having 1 to 20 carbon atoms, a hydroxyl group, or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, provided that at least one R is an alkenyl group having 2 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms in which a portion of the hydrogen atoms bonded to the carbon atoms of the alkyl group are substituted with a mercapto group, an acryloxy group, or a methacryloxy group), and The (A) polyorganosiloxane is composed of siloxane units represented by the following average formula (1): [Case 1] (In the formula, R 1 and R 3 are each independently an unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; R 2are each independently an alkenyl group having 2 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms in which a portion of the hydrogen atoms bonded to the carbon atoms is substituted with a mercapto group, an acryloxy group, or a methacryloxy group; each X is each independently an unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a hydroxyl group; each Y is each independently a group defined by X; each Z is each independently an alkyl group having 1 to 4 carbon atoms, an acryloxy group having 1 to 4 carbon atoms, a is a alkoxy group or a hydroxyl group, a is a number equal to or greater than 0, b is a positive number which is 79.9 to 98.9% of the total number of a to f, c is a positive number which is 0.01 to 1% of the total number of a to f, provided that the total proportion of a+b+c to the total number of a to f is 80 to 99%, e is a number equal to or greater than 1, d and e are each independently a number which is 1 to 20% of the total number of a to f, and f is a number which is 0 to 1% of the total number of a to f. The emulsion composition (However, the emulsion composition does not contain a pH buffer consisting of a phosphate compound).
2. 2. The emulsion composition according to claim 1, wherein the polyorganosiloxane (A) has at least two hydroxyl groups represented by X and Y in one molecule.
3. 2. The emulsion composition according to claim 1, wherein the silicone acrylic graft copolymer resin is contained in an amount of 35 to 50% by mass in terms of solid content based on the mass of the entire composition.
Citation Information
Patent Citations
Coating composition and laminate
JP2013067787A
Poly-organosiloxane particle-containing graft copolymer and thermoplastic resin composition thereof
JP2017114994A
Polyorganosiloxane-containing graft copolymer, resin composition, molded article, sliding-properties improvement agent, and sliding member