Method for producing aerosol coating composition
By dispersing pigments with a dispersant and adding modified epoxy resin later, the method prevents agglomeration, ensuring efficient application of a coating film with superior rust prevention and water resistance on complex surfaces.
Patent Information
- Application Number
- JP2020153666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-14
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-09-14
AI Technical Summary
Existing aerosol paints containing pigments and modified epoxy resin tend to agglomerate upon contact with fillers, leading to inefficiencies in coating complex surfaces and inadequate rust prevention, water resistance, and strength.
A method involving dispersing pigments with a dispersant before adding a modified epoxy resin, using specific dispersants like cationic dispersants, and controlling particle size and solvent ratios to prevent agglomeration during aerosolization.
Produces a paint that maintains fluidity and applies a coating film with excellent rust prevention, water resistance, and strength without agglomeration, enhancing work efficiency on complex surfaces.
Smart Images

Figure 0007565069000006 
Figure 0007565069000007 
Figure 0007565069000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an aerosol coating composition. [Background technology]
[0002] When painting machine parts or building parts, a primer (undercoat) is applied to improve adhesion between the topcoat and the painted surface. Primers are required to have functionality such as rust prevention and water resistance in addition to adhesion, and pigments are blended to impart these functions. In addition, by blending modified epoxy resin as a binder, it is possible to create a one-component primer.
[0003] If the primer could be made into an aerosol, the work efficiency could be improved and it would be possible to paint on complex surface shapes. Patent Document 1 describes an aerosol paint in which modified epoxy resin, epoxy resin, pigment, solvent, etc. are mixed together. Other aerosol paints that do not contain pigments and paints that do not contain modified epoxy resins are known, but these aerosol paints cannot form a coating film that is excellent in rust prevention, water resistance, and strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-9121 A Summary of the Invention [Problem to be solved by the invention]
[0005] It is an object of the present invention to provide a method for producing a coating material that contains a pigment and a modified epoxy resin and that does not agglomerate when in contact with a filler for aerosolization. [Means for solving the problem]
[0006] The present inventors have discovered that by dispersing a pigment in advance with a dispersant and then adding a modified epoxy resin, it is possible to produce an aerosol coating composition that does not aggregate even when it comes into contact with a filler, and have completed the present invention.
[0007] That is, the present invention relates to a method for producing an aerosol coating composition, which comprises the steps of dispersing a pigment in a solvent containing a dispersant, and adding a modified epoxy resin.
[0008] In the dispersion step, it is preferable not to add a modified epoxy resin.
[0009] Preferably the dispersant is a cationic dispersant.
[0010] Preferably the pigment is talc, precipitated barium sulfate, or kaolin.
[0011] The present invention also relates to an aerosol coating composition obtained by the above-mentioned production method. Effect of the Invention
[0012] According to the manufacturing method of the present invention, it is possible to manufacture a paint that contains a pigment and a modified epoxy resin and does not aggregate even when it comes into contact with a filler for aerosolization. By aerosolizing this paint, it is possible to efficiently apply a coating film that has excellent rust prevention, water resistance, and strength. [Brief description of the drawings]
[0013] [Figure 1] 4 shows the flowability of Reference Example 8. [Diagram 2] 4 shows the flowability of Reference Example 9. [Figure 3A] 1 shows the state of aggregation in Example 1 and Comparative Example 1. [Figure 3B] FIG. 2 is an enlarged view of the state of aggregation in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention relates to a method for producing an aerosol coating composition, which comprises the steps of dispersing a pigment in a solvent containing a dispersant, and adding a modified epoxy resin.
[0015] <Pigments> The pigment is not particularly limited as long as it can be blended in the aerosol, and examples thereof include extender pigments, coloring pigments, rust-preventive pigments, and functional pigments. A major feature of the present invention is that the pigment is dispersed in advance with a dispersant, and then the modified epoxy resin is added.
[0016] Examples of color pigments include titanium oxide, carbon black, yellow iron oxide, red iron oxide, phthalocyanine blue, phthalocyanine green, permanent red, naphthol red, quinacridone red, benzimidazolone yellow, isoindoline yellow, etc. These color pigments can be appropriately selected depending on the color required for the paint.
[0017] Examples of the extender pigment include talc, precipitated barium sulfate, kaolin, silica, calcium carbonate, zinc stearate, etc. Among these, talc, precipitated barium sulfate, and kaolin are preferred.
[0018] The rust-preventive pigments include aluminum tripolyphosphate, zinc oxide, zinc phosphate, and the like.
[0019] Examples of functional pigments include heat shielding pigments, ultraviolet reflective pigments, conductive pigments, and photochromic pigments.
[0020] The average particle size of the pigment is preferably 5 to 50 μm, more preferably 20 to 30 μm. If the dispersed particle size exceeds 50 μm, the coating composition is likely to aggregate. If the dispersed particle size is less than 5 μm, re-aggregation may occur in the solvent, resulting in large particles.
[0021] The amount of pigment is not particularly limited, but is preferably 50 to 85% by weight, more preferably 60 to 80% by weight, based on the solid content of the aerosol coating composition. If it is less than 50% by weight, sagging of the coating film tends to occur easily, and if it exceeds 85% by weight, the physical properties of the coating film tend to deteriorate.
[0022] <Dispersant> The dispersant is not particularly limited as long as it can disperse the pigment in the solvent. Examples of the dispersant include cationic dispersants, anionic dispersants, amphoteric dispersants, nonionic dispersants, and polymeric dispersants.
[0023] Cationic dispersants include alkylamine salts and quaternary ammonium salts such as lauryltrimethylammonium chloride, hexadecyltrimethylammonium bromide, etc. Commercially available products include DISPERBYK-2164, DISPERBYK-164, and DISPERBYK-2155.
[0024] Examples of anionic dispersants include sodium alkyl sulfate having an alkyl group, polyoxyethylene alkyl ether sulfate, alkylbenzene sulfonate, and polyester phosphate. Commercially available products include DISPERBYK-110 and BYK-P105.
[0025] Examples of the amphoteric dispersant include alkyl betaines and alkyl amine oxides.
[0026] Non-ionic dispersants include polyoxyethylene alkyl ethers, block copolymers composed of ethylene oxide and propylene oxide, alkylphenol polyethylene glycol ethers, and sorbitan fatty acid esters. Commercially available products include DISPERBYK-2152.
[0027] Polymeric dispersants include polyvinylpyrrolidone, polyvinyl alcohol, hydroxycellulose, hydroxyalkylcellulose, carboxymethylcellulose, and carboxypropylcellulose. Commercially available products include DISPERBYK-145 and DISPERBYK-106.
[0028] Among the above-mentioned dispersants, cationic dispersants are preferred from the viewpoint of dispersion stability after the addition of the modified epoxy resin. Also, dispersants that are compatible with the solvent described below are preferred.
[0029] The amount of dispersant added is preferably 1.5 to 4.0 parts by weight, more preferably 2.0 to 3.0 parts by weight, in terms of solid content, per 100 parts by weight of pigment. If it is less than 1.5 parts by weight, the pigment tends to aggregate and cause clogging when the aerosol is filled, and if it exceeds 4.0 parts by weight, the coating performance tends to decrease.
[0030] <Solvent> Examples of the solvent include glycol ether solvents (cellosolves) such as propylene glycol monomethyl ether, ethylene glycol monobutyl ether, and diethylene glycol monobutyl ether, ketone solvents such as isophorone, cyclohexanone, methyl ethyl ketone, methyl isobutyl ketone, and acetone, ester solvents such as normal butyl acetate, ethyl acetate, and butyl acetate, aromatic hydrocarbon solvents such as toluene, xylene, and ethylbenzene, and alcohol solvents such as methyl alcohol, ethyl alcohol, isopropyl alcohol, normal propyl alcohol, and normal butyl alcohol. These may be used alone or in combination of two or more.
[0031] Among the above solvents, examples of the solvents that can be used alone include glycol ether solvents, cyclohexanone, and isophorone.
[0032] The mixed solvent may be a solvent in which an aromatic hydrocarbon solvent and an alcohol solvent are mixed in a ratio of aromatic hydrocarbon solvent:alcohol solvent = 60:40 to 80:20. Here, examples of the aromatic hydrocarbon solvent include toluene, xylene, ethylbenzene, and naphtha, and examples of the alcohol solvent include ethyl alcohol, isopropyl alcohol, and normal butyl alcohol.
[0033] The solvent may be added in the pigment dispersion step, or in the modified epoxy resin addition step or thereafter. The ratio of the amount added in the pigment dispersion step to the amount added in the modified epoxy resin addition step or thereafter is preferably 30:70 to 50:50 by weight. When the solvent is added in the modified epoxy resin addition step, it is preferable to mix and stir the pigment dispersion liquid and the modified epoxy resin, and then add the solvent.
[0034] If a solvent is added alone between the pigment dispersion step and the modified epoxy resin addition step, aggregation may occur due to mixing of the coating composition and the filler, so it is preferable not to add a solvent alone between the pigment dispersion step and the modified epoxy resin addition step.
[0035] The final solid content of the aerosol coating composition is preferably 30 to 50% by weight, more preferably 35 to 45% by weight. If it is less than 30% by weight, the pigment tends to settle in the aerosol, and the pigment content required for the coating film to exhibit its performance tends not to be discharged. If it exceeds 50% by weight, the viscosity of the coating increases, and nozzle clogging tends to occur during aerosol spraying.
[0036] <Dispersion process> In the dispersion step, the pigment is dispersed in a solvent containing a dispersant. The machine used for dispersion is not particularly limited, but examples thereof include a bead mill, a basket mill, a roll mill, a sand mill, and a high-pressure homogenizer. When dispersion is performed using a bead mill, the bead diameter is preferably 1.00 to 2.00 mm, and more preferably 1.00 to 1.40 mm. If the bead diameter is less than 1.00 mm, the pigment may be pulverized to a primary particle size or smaller and re-aggregated.
[0037] When the pigment is dispersed in the presence of modified epoxy resin, the modified epoxy resin preferentially adheres to the pigment and tends to aggregate when the aerosol coating composition is mixed with the filler, so it is preferred not to add modified epoxy resin during the dispersion step.
[0038] <Modified epoxy resin addition process> In the production method of the present invention, a modified epoxy resin is added to a pigment dispersion.
[0039] The mass average molecular weight of the modified epoxy resin used in the present invention is preferably 10,000 or more, more preferably 12,000 or more, and even more preferably 14,000 or more. If the mass average molecular weight is less than 10,000, the hardness of the coating film formed using the aerosol coating composition tends to be insufficient. The upper limit of the mass average molecular weight is not particularly limited, but is generally 50,000 or less. The modified epoxy resin is preferably a resin obtained by polymerizing a bisphenol A type epoxy resin using a modifier.
[0040] Examples of modified epoxy resins include urethane-modified epoxy resins, amine-modified epoxy resins, isocyanate-modified epoxy resins, acrylic-modified epoxy resins, phenol-modified epoxy resins, polyester-modified epoxy resins, and acid-modified epoxy resins.
[0041] Specific examples of modified epoxy resins include Arakawa Chemical Industries Co., Ltd.'s Araquid 9201N, Araquid 9203N, Araquid 9205, Araquid 9208, Araquid 9212, KA-1439A, KA-1492, KA-1550, and Modepics 401. Examples of modified epoxy resins include Mitsui Chemicals' Epokey 871T, Epokey 810STS, Epokey 811, Epokey 813, Epokey 814, Epokey 818, Epokey 861, Epokey 863, Epokey 864, Epokey 872, Epokey 877, Epokey 891, Epokey 878, and Epokey 879. Examples of modified epoxy resins include DIC's H-301-35PX, H-303-45M, H-304-40, and H-601-55.
[0042] The glass transition temperature of the modified epoxy resin is preferably from 25°C to 130°C, and more preferably from 40°C to 90°C.
[0043] The amount of modified epoxy resin is not particularly limited, but is preferably 10 to 35% by weight, more preferably 25 to 30% by weight, based on the solid content of the aerosol coating composition. If it exceeds 35% by weight, sagging of the coating film tends to occur easily, and if it is less than 10% by weight, the physical properties of the coating film tend to deteriorate.
[0044] <Additives> The aerosol coating composition may contain additives such as unmodified epoxy resin, modifier, curing agent, curing accelerator, defoamer, surface conditioner, etc. in addition to the solvent, dispersant, suspending agent, pigment, and modified epoxy resin.
[0045] As the unmodified epoxy resin, mainly bisphenol A type epoxy resin can be used. The mass average molecular weight of the unmodified epoxy resin is preferably less than 10,000, more preferably 8,000 or less, and even more preferably 6,000 or less. Although the unmodified epoxy resin is not essential, when the unmodified epoxy resin is added, the solid weight ratio of the above-mentioned modified epoxy resin to the unmodified epoxy resin is preferably 99.9:0.1 to 30:70, and more preferably 95:5 to 40:60. The timing of adding the unmodified epoxy resin is not particularly limited, but it is preferable to add it in the process of dispersing the pigment.
[0046] The modifier is not particularly limited as long as it is a material compatible with the modified epoxy resin, and examples thereof include acrylic resin, polyester resin, alkyd resin, epoxy ester resin, silane coupling agent, etc. Modified epoxy resins having a larger mass average molecular weight than the modified epoxy resin described above can also be used. Compatibility can be confirmed by the presence or absence of cloudiness when mixed with the modified epoxy resin.
[0047] When a curing agent is used, examples of the curing agent include amine compounds and blocked isocyanates.
[0048] <Filling agent> The aerosol coating composition is filled into an aerosol container together with a filler. The filler is not particularly limited as long as it is used in aerosols, and examples of the filler include liquefied petroleum gas (LPG), dimethyl ether, and fluorohydrocarbons. Among these, a solvent with a medium degree of hydrogen bonding compatibility with epoxy resin is recommended, and therefore dimethyl ether with a hydrogen bonding parameter of 1.0 is preferred.
[0049] The filler is preferably used in an amount such that the aerosol coating composition and the filler have a volume ratio of 55:45 to 40:60, and more preferably 50:50 to 45:55.
[0050] In the present invention, a coating material that does not aggregate even when it comes into contact with a filler for aerosolization can be produced by dispersing the pigment and then adding a modified epoxy resin. Here, the aggregation property of the coating material composition can be evaluated after filling an aerosol container when dimethyl ether is used as the filler, but it can also be evaluated after mixing with diethyl ether under atmospheric pressure. Like dimethyl ether, diethyl ether has a medium level of intermolecular hydrogen bonding and has a similar SP value (the SP value of dimethyl ether is 7.3 cal / cm 3 , and the SP value of diethyl ether is 7.4 cal / cm 3 However, since diethyl ether is a liquid at room temperature, it is possible to evaluate the cohesion of the aerosol coating composition produced by the method of the present invention without filling it under high pressure.
[0051] <Coating film formation on substrate> The aerosol coating composition produced by the method of the present invention has excellent adhesion to the substrate, and is also excellent in rust prevention and water resistance. The substrate can be wood or metal. Examples of metals include steel, galvanized steel, stainless steel, magnesium alloy, aluminum alloy, brass, etc., and among them, non-ferrous metals such as aluminum alloy and stainless steel are preferred.
[0052] A coating film can be formed by spraying the aerosol onto a substrate and drying. Drying can be performed, for example, by leaving the composition to stand at room temperature (23°C) for 20 to 40 minutes. When the aerosol coating composition contains a curing agent, it can be cured under conditions according to the type of curing agent. For example, when a melamine resin is used as the curing agent, drying can be performed at 120 to 140°C, and when a blocked isocyanate is used, drying can be performed at 110 to 150°C. EXAMPLES
[0053] (1) Materials used (1-1) Pigments TITANIX JR-701 (Teika) Mistron Paper (Imeris) Precipitated Barium Sulfate HF (Tomatec)
[0054] (1-2) Dispersant DISPERBYK-2164(BYK) DISPERBYK-2155(BYK) (1-3) Suspension inhibitor ASA DS-313 (Ito Oil)
[0055] (1-4) Epoxy resin Epicron H-601-55 (DIC, solid content 55%) Arakid 9205 (Arakawa Chemical, solid content 40%) KA-1550 (Arakawa Chemical, solid content 40%) Modepics 401 (Arakawa Chemical, solid content 40%) Epoxy 871T (Mitsubishi Chemical, solid content 45%) Epicron 7050-60M (DIC, solids content 60%) Epicron 1050-70X (DIC, solid content 70%) Epicron 850 (DIC, 100% solids)
[0056] (1-5) Solvent Mixed thinner (cyclohexanone: 77.6%, propylene glycol monomethyl ether: 10.1%, n-butyl acetate: 3.4%, methyl ethyl ketone: 9.0%) Cyclohexanone
[0057] (2) Mixing Pigments, Additives, and Epoxy Resins All at Once (Comparative Examples 1 to 5, Reference Examples 1 to 3) The pigment, additives, epoxy resin, and solvent listed in Table 1 were mixed and dispersed for 30 minutes using beads with a particle size of 1.0 to 1.4 mm to prepare a paint. The modified epoxy resin and diethyl ether (DEE), which has a similar SP value to dimethyl ether used as a propellant, were mixed at a paint / DEE ratio of 1 / 1, and the dilutability of the mixture at room temperature was visually observed.
[0058] [Table 1]
[0059] In all of Comparative Examples 1 to 5, solid aggregates were found at the bottom and around the test tube immediately after mixing (marked with x in Table 1). No aggregates were found in Reference Examples 1 to 3. Since various functional groups are added to the modified epoxy resin, it is considered that the modified epoxy resin easily adheres to the pigment due to the same action as a dispersant. When a solvent that is poorly compatible with the modified epoxy resin is added while the modified epoxy resin is in a state where the modified epoxy resin is attached to the pigment, the modified epoxy resin that escapes from the solvent interface moves with the pigment, and it is considered that the pigments aggregate together.
[0060] (3) Adhesion test between pigment and modified epoxy resin (Reference Examples 4 to 11) The epoxy resins used in Comparative Examples 1 to 5 and Reference Examples 1 to 3 were mixed with the pigment at a weight ratio of 4% in terms of solid content. Specifically, the pigment was added to a solvent in which the resin had been dissolved while stirring with a disperser, and it was observed whether the fluidity could be maintained.
[0061] [Table 2]
[0062] In Reference Examples 4 to 8, the fluidity was maintained, and the pigment could be added to the end (◯ in Table 2). In Reference Examples 9 to 11, the fluidity was lost, and the pigment could not be added halfway through (× in Table 2). From these results, it is presumed that the modified epoxy resin has high adhesion to the pigment, which caused the aggregation in Comparative Examples 1 to 5.
[0063] Photographs of the aerosol coating compositions of Reference Examples 8 and 9 during stirring are shown in Figures 1 and 2. Reference Example 8 maintained fluidity due to its low viscosity, but Reference Example 9 had an extreme increase in viscosity, causing the stirring blades to spin freely, and the pigment remained in powder form without being stirred.
[0064] (4) Addition of epoxy resin in the finishing process (Examples 1 to 5) The pigment, additives, and solvent shown in Table 3 were dispersed for 30 minutes using beads with a particle size of 1.0 to 1.4 mm (dispersion step). The modified epoxy resin and solvent shown in Table 3 were added to the dispersed mixture (finishing step) to produce a paint. As in Comparative Examples 1 to 5, the paint was mixed at a paint / DEE ratio of 1 / 1, and the mixture was visually observed for dilution at room temperature.
[0065] [Table 3]
[0066] In all of Examples 1 to 5, no aggregates were observed when observed several minutes after mixing, and no aggregates were observed even after 24 hours (marked with ◯ in Table 3). As shown in Reference Examples 4 to 8, these modified epoxy resins have high adhesion to pigments, so it is presumed that by adding them in the finishing process, the pigments are no longer affected by the resin.
[0067] The aerosol coating compositions of Example 1 and Comparative Example 1 were each placed in equal amounts together with DEE into a test tube, and the state after thorough shaking is shown in Figure 3A. An enlarged view of the composition is shown in Figure 3B. No aggregates were observed in Example 1, while aggregated pigment was confirmed on the inner wall of the test tube in Comparative Example 1.
[0068] (5) Production of aerosol (Example 6) The pigment, additives, epoxy resin, and solvent shown in Table 4 were mixed (dispersion step). The modified epoxy resin and solvent shown in Table 4 were added to the dispersed mixture in this order (finishing steps (1) and (2)) to produce the paint. In the finishing steps (1) and (2), the components were added and then stirred for several minutes using a disperser. After that, the dilution property was confirmed with a paint / DEE ratio of 1:1, and the paint was filled with dimethyl ether using a filling machine.
[0069] [Table 4]
[0070] When the paint was observed a few minutes after mixing with DEE, no agglomerates were observed, and no agglomerates were observed even after 24 hours. In addition, when the paint was aerosolized, it sprayed smoothly and no clogging occurred.
[0071] (6) Addition of epoxy resin in the finishing process (Examples 7 to 8) The pigment, dispersant, suspending agent, epoxy resin, and solvent shown in Table 5 were mixed (dispersion step). Modified epoxy resin and solvent were added to the mixture after dispersion (finishing step) to produce a paint. The paint / DEE was mixed at 1 / 1, and the mixture was visually observed at room temperature.
[0072] [Table 5]
[0073] In all of Examples 7 to 8, no aggregates were observed when observed several minutes after mixing, and no aggregates were observed even after 24 hours (see circle in Table 5). In addition, the dispersants used in Examples 7 to 8 had good solubility in DEE.
[0074] In addition, when 10% by weight of the dispersant was added to diethyl ether (DEE) to check the compatibility of the dispersant itself with diethyl ether, it was confirmed that all of the dispersants of Examples 7 to 8 did not become cloudy after mixing with diethyl ether, and were compatible ("10% dispersant / DEE" in Table 5).
Claims
1. A method for producing a pigment comprising the steps of: dispersing a pigment in a solvent containing a cationic dispersant; and adding a modified epoxy resin; No modified epoxy resin is added in the dispersion process. A method for producing an aerosol coating composition.
2. 2. The process of claim 1, wherein the pigment is talc, precipitated barium sulfate, or kaolin.
Citation Information
Patent Citations
Propellant pressing composition and its production
JP1986197661A
Aerosol coating composition
JP1991285962A
Stock solution composition for aerosol paint
JP1995316490A
Aerosol coating composition and its production
JP1998140074A
Coating composition for aerosol
JP2018009121A