Nanocomposite coatings containing core-shell nanofibers self-healing polymer with excellent corrosion resistance

A three-layered coating system with epoxy-silanized graphene oxide nanocomposites and electrospun core-shell nanofibers addresses the limitations of existing self-healing coatings by providing a robust, long-term corrosion-resistant barrier with enhanced self-healing properties and simplified fabrication.

WO2024231719A1PCT designated stage expired Publication Date: 2024-11-14MADANI SEYED MORTEZA +3
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
PCT/IB2023/058376
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-06
Filing Date
2023-08-23
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Current self-healing coatings for metal surfaces face challenges such as incomplete barrier formation, defects leading to corrosion, and complex fabrication processes, with existing vascular systems having limitations in uniformity and long-term effectiveness.

Method used

A three-layered coating system comprising an epoxy-silanized graphene oxide nanocomposite as both top and bottom layers, with a middle layer of electrospun core-shell nanofibers, where the nanofibers contain a PDMS core and PVA shell, providing enhanced corrosion resistance and self-healing properties through a simple and cost-effective method.

Benefits of technology

The coating system effectively prevents corrosive ion penetration and offers long-term self-healing capabilities, maintaining high corrosion resistance even after damage, with improved uniformity and ease of fabrication compared to previous methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2023058376_14112024_PF_FP_ABST
    Figure IB2023058376_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed herein is a self-healing anticorrosive coating for a metal surface. The self-healing anticorrosive coating includes a three-layered coating coated on the metal surface. The self-healing anticorrosive coating includes a layer of electrospun core-shell nanofibers as a middle layer between two layers of an epoxy-silanized graphene oxide nanocomposite. The self-healing anticorrosive coating includes a first layer of epoxy-silanized graphene oxide nanocomposite deposited on the metal surface, the layer of electrospun core-shell nanofibers directly formed on the first layer of epoxy-silanized graphene oxide nanocomposite, and a second layer of the epoxy-silanized graphene oxide nanocomposite coated on the layer of electrospun core-shell nanofibers. The epoxy-silanized graphene oxide nanocomposite includes graphene oxide nanosheets functionalized with 3-glycidyloxypropyltrimethoxysilane (GPTMS) dispersed in an epoxy matrix and each electrospun core-shell nanofiber of the electrospun core-shell nanofibers include a core including polydimethylsiloxane (PDMS) and a shell including polyvinyl alcohol (PVA) encapsulating the core.
Need to check novelty before this filing date? Find Prior Art

Description

352-8266 NANOCOMPOSITE COATINGS CONTAINING CORE-SHELL NANOFIBERS SELF-HEALING POLYMER WITH EXCELLENT CORROSION RESISTANCE TECHNICAL FIELD

[0001] The present disclosure generally relates to protection of metals against corrosion, and particularly, to a self-healing anti-corrosive coating for metallic surfaces and a method of fabrication thereof. BACKGROUND ART

[0002] Epoxy coatings are one of the most common organic coatings for protecting metal structures against corrosive environments, due to their unique properties such as good adhesion to metal surface and having a high density of cross-link. The main role of epoxy coatings in corrosion protection is that an epoxy coating creates a protective barrier against corrosive agents. However, epoxy coatings do not provide complete barrier and protective properties against the diffusion of corrosive environments. During a period of use and exploitation, defects are created in organic coatings, and through these defects, diffusion of corrosive solutions provides direct access to surface of a metal layer for corrosive ions, and finally, corrosion occurs.

[0003] Most of self-healing coatings are considered to be capable of restoring properties of coating after being exposed to small damage. An exemplary repairing process takes place at a place of a microcrack; allowing for prevention of growth of the crack and penetration of water, oxygen, and corrosive ions to surface of a metallic substrate, and in this way, an exemplary self-healing coating protects the metallic substrate against corrosion.

[0004] Self-healing in coating systems has been investigated for corrosion protection in pre- treatment and top coating layers using different properties and combination of inhibiting species by adding directly to coating or by storage done in reservoirs. Preparation of self- healing materials based on microcapsules is a method of encapsulating self-healing materials into microcapsules, which are used in various fields such as agriculture, medicine, food, fabric, coatings, flavorings, perfumes and adhesives because it is used for polymer composites and thin polymer coatings, and an amount of self-healing agent is controlled by adjusting a diameter of microcapsules. Jiyu Sun et al. published an article titled as “two preparation processes for anti-corrosion and self-healing epoxy coatings containing the poly352-8266 (calcium alginate) microcapsules loaded with tung oil” in the journal Colloids and Surfaces A: Physicochemical and Engineering Aspects, 641, 128600 (2022). In this paper, poly (calcium alginate) microcapsules loaded with tung oil were synthesized by emulsion gelation method. Self-healing microcapsules synthesized using emulsion gelation method, and an easily prepared, low-cost anti-corrosion coating was prepared by mixing it with epoxy resin. However, capsule-based self-healing methods / systems have several disadvantages such as low uniformity of dispersed capsules and complicated fabrication processes.

[0005] When environmental conditions change or matrix is damaged, monomers inside polymer capsules are released from capsule and polymerized inside damaged part, causing repair of matrix. However, in such systems, if an area is repaired after being damaged, that area loses its ability to repair again. Another method of encapsulating self-healing materials is coating systems based on vascular system where healing materials are inside hollow fibers or microtubes, and after fibers or microtubes are damaged, healing materials are released and matrix is repaired. X Ji, et al. published an article titled as “developing wide pH-responsive, self-healing, and anti-corrosion epoxy composite coatings based on encapsulating oleic acid / 2-mercaptobenzimidazole corrosion inhibitors in chitosan / poly(vinyl alcohol) core-shell nanofibers” in Journal of Progress in Organic Coatings, 161, 106454 (2021). In this research, oleic acid (OA) and 2-mercaptobenzimidazole (MBI) encapsulated in chitosan / poly(vinyl alcohol) (CS / PVA) core-shell nanofibers were synthesized and used for developing core- shell / epoxy composite coatings on Q235 steel substrate to enhance service-life of coating systems. The corrosion protection performance of the prepared composite coatings were evaluated by electrochemical impedance spectroscopy, revealing that the maximum inhibition efficiency of OA and MBI is 96.66% and 99.36% after 10 and 20 days immersion in alkaline and acidic electrolyte, respectively. However, there have been some difficulties in such coating systems. One of the advantages of these systems is that these vascular networks can be connected to a large source of repair material and cover large injuries. Depending on the type of materials used, these systems can be designed in one-dimensional, two-dimensional, and three-dimensional forms. It is evident that one of the most critical aspects that affect the development of a smart and efficient vascular self-repairing composite structure is the selection of a proper healing agent. Delivery mechanism, as well as physical and chemical properties (i.e. viscosity, curing time, etc.) of the healing agents, are fundamental to a repairing process.352-8266

[0006] Hence, there is a need in the art for a coating capable of being highly resistant against corrosion. There is further a need for a coating that may be long-term used on metal surfaces with high self-healing properties. Moreover, there is a need for a self-healing and anti- corrosive coating prepared via a simple and cost-effective method. SUMMARY OF THE DISCLOSURE

[0007] This summary is intended to provide an overview of the subject matter of this patent, and is not intended to identify essential elements or key elements of the subject matter, nor is it intended to be used to determine the scope of the claimed implementations. The proper scope of this patent may be ascertained from the claims set forth below in view of the detailed description below and the drawings.

[0008] In one general aspect, the present disclosure is directed to a self-healing anticorrosive coating for a metal surface. In an exemplary embodiment, the self-healing anticorrosive coating may include a first layer of epoxy-silanized graphene oxide nanocomposite deposited on the metal surface, a layer of electrospun core-shell nanofibers directly formed on the first layer of epoxy-silanized graphene oxide nanocomposite, and a second layer of the epoxy- silanized graphene oxide nanocomposite coated on the layer of electrospun core-shell nanofibers. In an exemplary embodiment, the epoxy-silanized graphene oxide nanocomposite may include graphene oxide nanosheets functionalized with 3- glycidyloxypropyltrimethoxysilane (GPTMS) dispersed in an epoxy matrix (GPTMS-GO- EP). In an exemplary embodiment, each electrospun core-shell nanofiber of the electrospun core-shell nanofibers may include a core including polydimethylsiloxane (PDMS) and a shell including polyvinyl alcohol (PVA) encapsulating the core.

[0009] In an exemplary embodiment, the graphene oxide nanosheets functionalized with GPTMS may be present in the GPTMS-GO-EP with an amount of 0.2 wt% based on a total weight of the GPTMS-GO-EP. In an exemplary embodiment, the epoxy matrix may include an epoxy resin. In an exemplary embodiment, the epoxy resin may include a bisphenol A (BPA)-based epoxy resin.

[0010] In an exemplary embodiment, the core-shell nanofibers may be formed from a PDMS solution containing an amount of PDMS in a range of 30 wt% to 50 wt% and a PVA solution containing an amount of PVA in a range of 5 wt% to 20 wt%. In an exemplary embodiment, each nanofiber of the electrospun core-shell nanofibers may have an average diameter in a352-8266 range of 100 nm to 500 nm and each core may have a thickness in a range of 80 nm to 200 nm.

[0011] In an exemplary embodiment, the first layer of the epoxy-silanized graphene oxide nanocomposite may have a thickness in a range of 30 µm to 40 µm. In an exemplary embodiment, the layer of electrospun core-shell nanofibers may have a thickness in a range of 15 µm to 20 µm. In an exemplary embodiment, the second layer of the epoxy-silanized graphene oxide nanocomposite may have a thickness more than a thickness of the first layer of the epoxy-silanized graphene oxide nanocomposite. In an exemplary embodiment, the thickness of the second layer of the epoxy-silanized graphene oxide nanocomposite may be in a range of 60 µm to 100 µm.

[0012] In another general aspect of the present disclosure, a method for producing a self- healing anticorrosive coating on a metal surface may be described. The method may include producing graphene oxide nanosheets functionalized with 3- glycidyloxypropyltrimethoxysilane (GPTMS) (GPTMS-GO) with a weight ratio of GPTMS to GPTMS-GO in a range of 0.1 wt% to 0.3 wt%, producing an epoxy-silanized graphene oxide nanocomposite by dispersing the formed GPTMS-GO in an epoxy matrix, preparing the metal surface of a metallic substrate, depositing a first layer of the epoxy-silanized graphene oxide nanocomposite on the prepared metal surface, electrospinning a layer of core- shell nanofibers on the first layer of the epoxy-silanized graphene oxide nanocomposite, depositing a second layer of the epoxy-silanized graphene oxide nanocomposite on the electrospun layer of core-shell nanofibers, and curing and drying a three-layered formed coating including the first layer of the epoxy-silanized graphene oxide nanocomposite, the electrospun layer of core-shell nanofibers, and the second layer of the epoxy-silanized graphene oxide nanocomposite formed on the metal surface. In an exemplary embodiment, the produced epoxy-silanized graphene oxide nanocomposite may include a nanocomposite of GPTMS-GO dispersed in the epoxy matrix (GPTMS-GO-EP).

[0013] In an exemplary embodiment, producing the graphene oxide nanosheets functionalized with GPTMS may include forming a mixture by adding graphene oxide nanosheets to a container containing ethanol, deionized water, and GPTMS, agitating the mixture by stirring the mixture for a time period in a range of 15 minutes to 1 hour, adjusting a pH value of the mixture within a range of 4 to 5 by adding a first base to the mixture while stirring the mixture, stirring the mixture for a time period in a range of 20 hours to 25 hours,352-8266 adjusting a pH value of the mixture within a range of 8.5 to 9.5 by adding a second base to the mixture while stirring the mixture, stirring the mixture at a constant temperature in a range of 65 ºC to 75 ºC for a time period in a range of 1 hour to 3 hours, removing unreacted ethanol, deionized water, and GPTMS from the mixture by dividing the mixture into a clear phase and a precipitation via centrifuging the mixture, removing an excess amount of unreacted GPTMS adsorbed on graphene oxide nanosheets by washing the precipitation using a mixture of ethanol-deionized water with a volume ratio of ethanol:deionized water equal to 3:1, and removing residual deionized water from the precipitation.

[0014] In an exemplary embodiment, centrifuging the mixture may include dividing the mixture into the clear phase and the precipitation and separating the precipitation from the clear phase. In an exemplary embodiment, the clear phase may include the unreacted ethanol, deionized water, and GPTMS. In an exemplary embodiment, the precipitation may include the graphene oxide nanosheets functionalized with GPTMS. In an exemplary embodiment, centrifuging the mixture may include centrifuging the mixture for a time period in a range of 3 minutes to 10 minutes at a centrifugation speed in a range of 3000 rpm to 5000 rpm. In an exemplary embodiment, removing residual deionized water from the precipitation may include washing the precipitation with diethyl ether and maintaining the precipitation in toluene.

[0015] In an exemplary embodiment, producing the epoxy-silanized graphene oxide nanocomposite may include forming a mixture of the GPTMS-GO in toluene and dispersing the GPTMS-GO in an epoxy resin matrix. In an exemplary embodiment, forming the mixture of the GPTMS-GO in toluene may include adding the GPTMS-GO to a container containing toluene and stirring the GPTMS-GO and the toluene for a time period in a range of 5 minute to 20 minutes at a temperature in a range of 0 ºC to 4 ºC using an ultrasonic probe. In an exemplary embodiment, dispersing the GPTMS-GO in the epoxy resin matrix may include adding an epoxy resin to the mixture of the GPTMS-GO in toluene, stirring the mixture of the GPTMS-GO in toluene with the epoxy resin at a stirring speed in a range of 500 rpm to 1500 rpm for a time period in a range of 20 hours and 30 hours using a mechanical stirrer, sonicating the mixture of the GPTMS-GO in toluene with the epoxy resin for a time period in a range of 5 minute to 20 minutes using an ultrasonic probe, adding a hardener with a weight ratio in a range of 1.3:1 (epoxy resin:hardener) to the mixture of the GPTMS-GO in toluene with the epoxy resin, and stirring the mixture of the GPTMS-GO in toluene with the epoxy352-8266 resin and the added hardener for a time period in a range of 5 minute to 20 minutes using a mechanical stirrer.

[0016] In an exemplary embodiment, preparing the metal surface of the metallic substrate may include grinding the metal surface using a silicon carbide (SiC) paper, washing and degreasing the ground metal surface with at least one of acetone, ethanol, distilled water, and combinations thereof, drying the washed metal surface, and preventing oxidation and / or rusting of the metal surface by maintaining the metallic substrate in a desiccator and vacuum environment before depositing the first layer of the epoxy-silanized graphene oxide nanocomposite thereon.

[0017] In an exemplary embodiment, depositing the first layer of the epoxy-silanized graphene oxide nanocomposite on the prepared metal surface may include forming a layer with a thickness in a range of 30 µm to 40 µm on the prepared metal surface by spraying the epoxy-silanized graphene oxide nanocomposite on the prepared metal surface.

[0018] In an exemplary embodiment, electrospinning the layer of core-shell nanofibers on the first layer of the epoxy-silanized graphene oxide nanocomposite may include coaxial electrospinning of two polymers on the first layer of the epoxy-silanized graphene oxide nanocomposite while the first layer of the epoxy-silanized graphene oxide nanocomposite being wet. In an exemplary embodiment, coaxial electrospinning of the two polymers may include electrospinning a first polymer through an inner nozzle of a coaxial pair of nozzles on the first layer of the epoxy-silanized graphene oxide nanocomposite and electrospinning a second polymer through an outer nozzle of a coaxial pair of nozzles on the first layer of the epoxy-silanized graphene oxide nanocomposite. In an exemplary embodiment, the first polymer may include a self-healing material. In an exemplary embodiment, the second polymer may include a hydrophilic polymer. In an exemplary embodiment, electrospinning the first polymer and the second polymer may be done simultaneously.

[0019] In an exemplary embodiment, electrospinning the first polymer may include electrospinning a solution of polydimethylsiloxane (PDMS) with a PDMS concentration in a range of 30 wt% to 50 wt% at a feeding rate in a range of 0.05 mL.h-1to 0.5 mL.h-1. In an exemplary embodiment, electrospinning the second polymer may include electrospinning a solution of polyvinyl alcohol (PVA) with a PVA concentration in a range of 5 wt% to 20 wt% at a feeding rate in a range of 0.5 mL.h-1to 2 mL.h-1. In an exemplary embodiment, electrospinning the layer of core-shell nanofibers on the first layer of the epoxy-silanized352-8266 graphene oxide nanocomposite may be done at a voltage in a range of 10 kV to 20 kV. In an exemplary embodiment, electrospinning the layer of core-shell nanofibers on the first layer of the epoxy-silanized graphene oxide nanocomposite may include forming a layer of electrospun core-shell nanofibers with a thickness in a range of 15 µm to 20 µm on the first layer of the epoxy-silanized graphene oxide nanocomposite.

[0020] In an exemplary embodiment, depositing the second layer of the epoxy-silanized graphene oxide nanocomposite on the electrospun layer of core-shell nanofibers may include forming a layer with a thickness in a range of 60 µm to 100 µm on the prepared metal surface by spraying the epoxy-silanized graphene oxide nanocomposite on the electrospun layer of core-shell nanofibers.

[0021] In an exemplary embodiment, curing and drying the three-layered formed coating may include maintaining the three-layered formed coating at ambient temperature in a range of 20 ºC to 30 ºC for a time period in a range of 20 hours to 60 hours and baking the three- layered formed coating at a temperature in a range of 55 ºC to 65 ºC for a time period in a range of 20 hours to 30 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawing figures depict one or more implementations in accord with the present teachings, by way of example only, not by way of limitation. In the figures, like reference numerals refer to the same or similar elements.

[0023] FIG. 1A shows a schematic side view of an exemplary self-healing anticorrosive coating, consistent with one or more exemplary embodiments of the present disclosure.

[0024] FIG. 1B shows a perspective schematic view of an exemplary self-healing anticorrosive coating, consistent with one or more exemplary embodiments of the present disclosure.

[0025] FIG. 1C shows a schematic view of an exemplary nanofiber of layer of an exemplary electrospun core-shell nanofibers, consistent with one or more exemplary embodiments of the present disclosure.

[0026] FIG. 1D shows a schematic image of an exemplary self-healing and repairing mechanism of an exemplary self-healing anticorrosive coating coated on an exemplary metal surface after scratching by an exemplary scratch, consistent with one or more exemplary embodiments of the present disclosure.352-8266

[0027] FIG. 2 shows a flowchart of an exemplary method for producing a self-healing anticorrosive coating on a metal surface, consistent with one or more exemplary embodiments of the present disclosure.

[0028] FIG. 3 shows Fourier transform infrared (FTIR) spectra of an exemplary polyvinyl alcohol (PVA) polymer solution, an exemplary polydimethylsiloxane (PDMS) polymer solution, and exemplary core-shell fibers (PDMS-PVA), consistent with one or more exemplary embodiments of the present disclosure.

[0029] FIG. 4 shows a transmission electron microscopy (TEM) image of exemplary PDMS- PVA core-shell nanofibers, consistent with one or more exemplary embodiments of the present disclosure.

[0030] FIG. 5 shows a field emission scanning electron microscopy (FESEM) image of cross-sectional surface of an exemplary produced self-healing anticorrosive coating including an exemplary epoxy-silanized graphene oxide coating containing core-shell fibers, a cross- sectional image of an exemplary portion of middle layer of an exemplary produced self- healing anticorrosive coating, linear elemental EDAX analysis in direction of white arrow along with thickness of an exemplary produced self-healing anticorrosive coating, and magnification of an exemplary portion of PDMS-PVA core-shell nanofibers of an exemplary portion of middle layer of an exemplary produced self-healing anticorrosive coating, consistent with one or more exemplary embodiments of the present disclosure.

[0031] FIG. 6 shows FTIR spectra of pure epoxy, epoxy-graphene oxide, and an exemplary epoxy-silanized graphene oxide nanocomposite, consistent with one or more exemplary embodiments of the present disclosure.

[0032] FIG. 7 shows a thermal analysis of epoxy-graphene oxide coating in two cases without and with an exemplary graphene oxide functionalized with silane precursor, consistent with one or more exemplary embodiments of the present disclosure.

[0033] FIG. 8 shows FESEM images of an epoxy-graphene oxide coating at 0.2 wt% (, an epoxy-functionalized graphene oxide with silane coating at 0.2 wt%, and EDAX elemental analysis related to an exemplary FESEM image of an exemplary epoxy-functionalized graphene oxide with silane coating at 0.2 wt%, consistent with one or more exemplary embodiments of the present disclosure.

[0034] FIG. 9 shows FESEM and fluorescent microscope images of morphology of exemplary coaxial electrospun core-shell fibers at 13 kV voltage, core feeding rate 0.2 mL.h-352-82661, distance 18 cm from tip of syringe to collector, PDMS 40 wt% core solution, and concentration of PVA shell material of 15 wt%, 10 wt%, and 7 wt%, consistent with one or more exemplary embodiments of the present disclosure.

[0035] FIG. 10 shows FESEM and fluorescent microscope images of morphology of exemplary coaxial electrospun core-shell fibers at 13 kV voltage, distance 18 cm from tip of syringe to collector, PDMS 40 wt% core solution, concentration of PVA shell material of 10 wt%, at core feeding rates of 0.3 mL.h-1, 0.2 mL.h-1, and 0.1 mL.h-1, consistent with one or more exemplary embodiments of the present disclosure.

[0036] FIG. 11 shows FESEM and fluorescent microscope images of morphology of exemplary coaxial electrospun core-shell fibers at core feeding rate of 0.2 mL.h-1, distance 18 cm from tip of syringe to collector, PDMS 40 wt% core solution, concentration of PVA shell material of 10 wt%, at applied voltages of 16 kV, 13 kV, and 11 kV, consistent with one or more exemplary embodiments of the present disclosure.

[0037] FIG. 12 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with 7 wt% PVA shell solution (named as EPGSi-7%) at different immersion times in 3.5 wt% sodium chloride medium up to 1 day, for 5, 12, 18, 29 and 46 days, at 63, 78, 99, 120 and 132 days, and after 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0038] FIG. 13 shows equivalent electrical circuit of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers in 3.5 wt% sodium chloride solution during long immersion times at early times and at long times of immersion, consistent with one or more exemplary embodiments of the present disclosure.

[0039] FIG. 14 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with 10 wt% PVA shell solution (named as EPGSi-10%) at different immersion times in 3.5 wt% sodium chloride medium of 1, 5, 12 and 18 days, at 29, 46, 63 and 78 days, and after 99, 120, 132 and 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0040] FIG. 15 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with 15 wt% PVA shell solution (named as EPGSi-15%) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days and at 120, 132 and 148 days, consistent with one or more exemplary embodiments of the present disclosure.352-8266

[0041] FIG. 16 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers at voltage of 11 kV (named as EPGSi-11kV) at different immersion times in 3.5 wt% sodium chloride medium up to 78 days, at 12 and 99 days, after 18, 29, 120, and 132 days, and up to 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0042] FIG. 17 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers at voltage of 13 kV (named as EPGSi-13kV) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days and after 120, 132, and 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0043] FIG. 18 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers at voltage of 16 kV (named as EPGSi-16kV) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days, at 29, 46, 63, 78, and 99 days, and after 120, 132, and 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0044] FIG. 19 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with a core feeding rate of 0.1 mL.h-1(named as EPGSi-0.1) at different immersion times in 3.5 wt% sodium chloride medium up to 1 day, at 5, 12 and 18 days, after 29 and 46 days, after 63, 78, 99 and 120 days, and after 132 and 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0045] FIG. 20 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with a core feeding rate of 0.2 mL.h-1(named as EPGSi-0.2) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days and after 120, 132, and 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0046] FIG. 21 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with a core feeding rate of 0.3 mL.h-1(named as EPGSi-0.3) at different immersion times in 3.5 wt% sodium chloride medium after 1, 5, 45 and 78 days, at 12, 18, and 29 days, after 63, 99, 120, 132, and 148 days, and at 148 days, consistent with one or more exemplary embodiments of the present disclosure.

[0047] FIG. 22 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a PVA solution having a PVA352-8266 concentration of 7 wt% (named as EPGSi-7%-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, after 8 and 12 days, and up to 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0048] FIG. 23 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a PVA solution having a PVA concentration of 10 wt% (named as EPGSi-10%-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, after 8 and 12 days, and up to 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0049] FIG. 24 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a PVA solution having a PVA concentration of 15 wt% (named as EPGSi-15%-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, and after 8, 12 and 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0050] FIG. 25 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with an applied voltage of 11 kV (named as EPGSi-11kV-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, after 8 and 12 days, and up to 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0051] FIG. 26 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with an applied voltage of 13 kV (named as EPGSi-13kV-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, and after 8, 12, and 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0052] FIG. 27 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with an applied voltage of 16 kV (named as EPGSi-16kV-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 and 36 hours, up to 8 days, up to 12 days, and up to 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0053] FIG. 28 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a core feeding rate of 0.1 mL.h-1(named as EPGSi-0.1-scratched) at different immersion times in 3.5 wt% sodium chloride352-8266 medium up to 24 hours, up to 36 hours, and up to 8, 12, and 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0054] FIG. 29 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a core feeding rate of 0.2 mL.h-1(named as EPGSi-0.2-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, and up to 8, 12, and 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0055] FIG. 30 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a core feeding rate of 0.3 mL.h-1(named as EPGSi-0.3-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours, up to 36 hours, and up to 8, 12, and at 16 days, consistent with one or more exemplary embodiments of the present disclosure.

[0056] FIG. 31 shows digital camera images related to a salt spray test on an exemplary surface of an exemplary coating containing core-shell fibers at different applied voltages of 11, 13, and 16 kV of electrospinning exposed to 5± 1 wt% sodium chloride after 480 hours, consistent with one or more exemplary embodiments of the present disclosure.

[0057] FIG. 32 shows digital camera images related to an exemplary salt spray test on an exemplary surface of an exemplary coating containing core-shell fibers electrospun at core feeding rates of 0.1, 0.2 and 0.3 mL.h-1after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure.

[0058] FIG. 33 shows digital camera images related to an exemplary salt spray test from an exemplary surface of an exemplary coating containing core-shell fibers electrospun in concentrations of 7, 10, and 15 wt% of PVA in shell solution and after 480 hours exposed to 5 ± 1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure.

[0059] FIG. 34 shows FESEM images and EDAX analysis taken from surface morphology of an exemplary scratch area of exemplary produced coatings containing electrospun core- shell fibers in concentrations of 7, 10, and 15 wt% after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure.

[0060] FIG. 35 shows FESEM images and EDAX analysis taken from surface morphology of an exemplary scratch area of exemplary produced coatings containing core-shell fibers352-8266 electrospun at core feeding rates of 0.1 mL.h-1, 0.2 mL.h-1, and 0.3 mL.h-1after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure.

[0061] FIG. 36 shows FESEM images and EDAX analysis taken from surface morphology of an exemplary scratch area of exemplary produced coatings containing core-shell fibers electrospun at applied voltages of 11 kV, 13 kV, and 16 kV after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure. DESCRIPTION OF EMBODIMENTS

[0062] In the following detailed description, numerous specific details are set forth by way of examples in order to provide a thorough understanding of the relevant teachings. However, it should be apparent that the present teachings may be practiced without such details. In other instances, well known methods, procedures, components, and / or circuitry have been described at a relatively high-level, without detail, in order to avoid unnecessarily obscuring aspects of the present teachings.

[0063] Herein, a coating for metal surfaces with improved self-healing properties as well as high resistance against corrosive environments is described. An exemplary coating may include a three-layered coating coated on a metallic surface. A first layer of an exemplary coating may include a layer of an epoxy-silanized graphene oxide nanocomposite coated on an exemplary metallic surface. A second layer of an exemplary coating may include a layer of electrospun core-shell nanofibers directly formed on the first layer of an exemplary coating through an electrospinning process. A third layer of an exemplary coating may include another layer of an exemplary epoxy-silanized graphene oxide nanocomposite coated on the second layer of an exemplary coating. In an exemplary embodiment, an exemplary epoxy- silanized graphene oxide nanocomposite may include graphene oxide nanosheets functionalized with 3-glycidyloxypropyltrimethoxysilane (GPTMS) dispersed in an epoxy matrix (GPTMS-GO-EP). In an exemplary embodiment, each electrospun core-shell nanofiber of electrospun core-shell nanofibers may include a core including polydimethylsiloxane (PDMS) and a shell including polyvinyl alcohol (PVA).

[0064] Epoxy resins may be utilized for coating metallic surfaces due to their high adhesion, excellent electrical insulation properties, low shrinkage during curing, and high chemical352-8266 stability. However, exemplary epoxy resins may provide a path for diffusing corrosive ions into a coating containing exemplary epoxy resins due to brittleness and defects such as pores and cracks created during a synthesis process, which leads to destruction of an exemplary coating and reduction of corrosion resistance over time. An exemplary epoxy-silanized graphene oxide nanocomposite may include graphene oxide nanosheets functionalized with GPTMS dispersed in epoxy matrix (GPTMS-GO-EP). An exemplary silane group of an exemplary silane-containing compound (i.e., GPTMS) may be attached to graphene oxide nanosheets; thereby, resulting in high and uniform dispersion of graphene oxide nanosheets in an exemplary epoxy matrix and an increase in inter-space interactions. Exemplary graphene oxide nanosheets may be added to an epoxy matrix to improve anti-corrosion performance of exemplary epoxy resins due to high specific surface area of graphene oxide nanosheets related to their sheet-shaped structure. Well-dispersed graphene oxide nanoparticles may reduce pores in an exemplary epoxy matrix, electrolyte penetration towards an exemplary metallic surface, and water penetration coefficient which may be considered as major drawbacks of currently used epoxy resins as coatings for metallic surfaces.

[0065] An exemplary disclosed here, may have self-healing properties as well as anri- corrosive capability for using on metallic surfaces. An exemplary coating has a three-layered structure coated layer-by-layer on an exemplary metallic surface, which make it difficult for a corrosive substance to reach an exemplary metallic surface. An exemplary coating has a sandwich-like structure in which a layer of a plurality of core-shell nanofibers is compacted between two layers of epoxy-silanized graphene oxide nanocomposite. An exemplary layer of an exemplary plurality of core-shell nanofibers may include a self-healing agent preserved as a core material inside a hydrophilic shell material. An exemplary epoxy-silanized graphene oxide nanocomposite may provide two anti-corrosive layers at top and down of an exemplary layer of an exemplary plurality of core-shell nanofibers. However, even if a corrosive substance penetrates through an exemplary top layer of epoxy-silanized graphene oxide nanocomposite, an exemplary self-healing agent may be released and activated due to dissolution of an exemplary shell material into an exemplary corrosive substance.

[0066] FIG. 1A shows a schematic side view of a self-healing anticorrosive coating 100, consistent with one or more exemplary embodiments of the present disclosure. In an exemplary embodiment, self-healing anticorrosive coating 100 may include a three-layer352-8266 sandwich structure, including a layer of electrospun core-shell nanofibers 103 placed and compacted between two layers of an epoxy-silanized graphene oxide nanocomposite 102 and 104. In an exemplary embodiment, self-healing anticorrosive coating 100 may be coated on a metal surface 101 of a metallic substrate 105.

[0067] Regarding FIG. 1A, self-healing anticorrosive coating 100 may include a first layer of epoxy-silanized graphene oxide nanocomposite 102 deposited on metal surface 101, layer of electrospun core-shell nanofibers 103 coated on first layer of epoxy-silanized graphene oxide nanocomposite 102, and a second layer of epoxy-silanized graphene oxide nanocomposite 104 deposited on layer of electrospun core-shell nanofibers 103. In an exemplary embodiment, layer of electrospun core-shell nanofibers 103 may act as a source of healable materials. In an exemplary embodiment, layer of electrospun core-shell nanofibers 103 may be formed directly on first layer of epoxy-silanized graphene oxide nanocomposite 102. In an exemplary embodiment, layer of electrospun core-shell nanofibers 103 may be electrospun on first layer of epoxy-silanized graphene oxide nanocomposite 102. In an exemplary embodiment, each layer of first layer of epoxy-silanized graphene oxide nanocomposite 102 and / or second layer of epoxy-silanized graphene oxide nanocomposite 104 may include a layer of a nanocomposite including graphene oxide nanosheets functionalized with a silane- containing compound, which may be dispersed in an epoxy matrix. In an exemplary embodiment, a silane group of an exemplary silane-containing compound may be attached to graphene oxide nanosheets; thereby, resulting in high and uniform dispersion of graphene oxide nanosheets in an exemplary epoxy matrix.

[0068] In an exemplary embodiment, first layer of epoxy-silanized graphene oxide nanocomposite 102 may have a thickness 106 in a range of 30 µm to 40 µm. In an exemplary embodiment, second layer of epoxy-silanized graphene oxide nanocomposite 104 may have a thickness 107 in a range of 60 µm to 100 µm. In an exemplary embodiment, first layer of epoxy-silanized graphene oxide nanocomposite 102 and second layer of epoxy-silanized graphene oxide nanocomposite 104 may have the same structure and composition. In an exemplary embodiment, first layer of epoxy-silanized graphene oxide nanocomposite 102 and second layer of epoxy-silanized graphene oxide nanocomposite 104 may have different thicknesses. In an exemplary embodiment, thickness 107 of second layer of epoxy-silanized graphene oxide nanocomposite 104 may be greater than thickness 106 of first layer of epoxy- silanized graphene oxide nanocomposite 102. In an exemplary embodiment, layer of352-8266 electrospun core-shell nanofibers 103 may have a thickness 108 in a range of 15 µm to 20 µm.

[0069] FIG. 1B shows a perspective schematic view of self-healing anticorrosive coating 100, consistent with one or more exemplary embodiments of the present disclosure. In an exemplary embodiment, each layer of epoxy-silanized graphene oxide nanocomposite 102 or 104 may include an epoxy-silanized graphene oxide nanocomposite. In an exemplary embodiment, each layer of epoxy-silanized graphene oxide nanocomposite 102 or 104 may include GPTMS-GO 111 dispersed in an epoxy matrix 114. In an exemplary embodiment, GPTMS-GO 111 may include graphene oxide nanosheets 110 functionalized with 3- glycidyloxypropyltrimethoxysilane (GPTMS) 112. In an exemplary embodiment, each layer of epoxy-silanized graphene oxide nanocomposite 102 or 104 may include graphene oxide nanosheets 110 functionalized with GPTMS 112 dispersed in epoxy matrix 114 (GPTMS- GO-EP). In an exemplary embodiment, GPTMS 112 may include two functional groups Si- O-Si 112a and Glycidoxy 112b linked to graphene oxide nanosheets 110. In an exemplary embodiment, GPTMS-GO 111 may be present in GPTMS-GO-EP in each layer of epoxy- silanized graphene oxide nanocomposite 102 or 104 with an amount in a range of about 0.1 wt% to about 0.3 wt% based on a total weight of GPTMS-GO-EP. In an exemplary embodiment, GPTMS-GO 111 may be present in GPTMS-GO-EP in each layer of epoxy- silanized graphene oxide nanocomposite 102 or 104 with an amount of about 0.2 wt% based on an exemplary total weight of GPTMS-GO-EP.

[0070] In an exemplary embodiment, an exemplary epoxy-silanized graphene oxide nanocomposite of each layer of epoxy-silanized graphene oxide nanocomposite 102 or 104 may further include a hardener that may be added to epoxy matrix 114; allowing for performing curing process of epoxy matrix 114 during fabrication of an exemplary epoxy- silanized graphene oxide nanocomposite. In an exemplary embodiment, an exemplary hardener may be present in an exemplary epoxy-silanized graphene oxide nanocomposite with a weight ratio of 1.3:1 (epoxy resin:hardener). In an exemplary embodiment, epoxy matrix 114 may include a bisphenol A (BPA)-based epoxy resin.

[0071] In an exemplary embodiment, first layer of epoxy-silanized graphene oxide nanocomposite 102 may be used to improve adhesion of self-healing anticorrosive coating 100 to metal surface 101 and prevent a possible disbanding. In an exemplary embodiment, layer of electrospun core-shell nanofibers 103 may be responsible for storing healable352-8266 materials therein and provide self-healing properties. In an exemplary embodiment, second layer of epoxy-silanized graphene oxide nanocomposite 104 with a greater thickness than first layer of epoxy-silanized graphene oxide nanocomposite 102 may act as a barrier against penetration of corrosive solutions into metallic substrate 105. In an exemplary embodiment, electrospun nanofibers 116 may be used for loading a reactive agent (i.e., PDMS) in self- healing anticorrosive coating 100. In an exemplary embodiment, when a mechanical damage occurs in self-healing anticorrosive coating 100 and causes plurality of nanofibers 116 to break, self-healing materials located in core 118 of plurality of nanofibers 116 may be released and repair a damaged area.

[0072] Regarding FIG. 1B, layer of electrospun core-shell nanofibers 103 may include a plurality of nanofibers 116. FIG. 1C shows a schematic view of an exemplary nanofiber 116 of layer of electrospun core-shell nanofibers 103, consistent with one or more exemplary embodiments of the present disclosure. In an exemplary embodiment, nanofiber 116 may include a core 118 and a shell 120 encapsulating core 118. In an exemplary embodiment, core 118 may include an organic polymer. In an exemplary embodiment, core 118 may include a healable material loaded inside shell 120. In an exemplary embodiment, an exemplary healable material of core 118 may be released when a corrosive material contacts with layer of electrospun core-shell nanofibers 103. In an exemplary embodiment, core 118 may include polydimethylsiloxane (PDMS) surrounded by shell 120. In an exemplary embodiment, shell 120 may include polyvinyl alcohol (PVA). In an exemplary embodiment, nanofiber 116 may have an average diameter 122 in a range of 100 nm to 500 nm. In an exemplary embodiment, core 118 may have an average diameter 124 in a range of 80 nm to 200 nm.

[0073] FIG. 1D shows a schematic image of an exemplary self-healing and repairing mechanism of self-healing anticorrosive coating 100 coated on metal surface 101 after scratching by an exemplary scratch 126, consistent with one or more exemplary embodiments of the present disclosure. In an exemplary embodiment, when local corrosion occurs, regeneration and oxidation reactions take place and cause pH distribution in cathodic and anodic areas. In case of local corrosion in organic coatings, a damaged area of an exemplary organic coating may be an anode, and an undamaged area may act as a local cathode. Regeneration of oxygen in cathodic areas may leads to alkalization, which raises pH value to above 5. In an exemplary embodiment, due to pH changes in damaged areas, self-healing materials inside plurality of nanofibers 116 may be released through polymer nanochannels352-8266 of plurality of nanofibers 116. In addition, silane compounds may be important materials that may act as repairing agents; allowing for forming protective films. Exemplary reactions of an exemplary zone 128 containing exemplary GPTMS-GO 111 may be summarized as shown in box 130. Silane precursor (i.e., GPTMS) has organic groups along with silicon, which may tend to hydrolyze in an aqueous environment. Hydrolysis reaction may lead to cross-linking, which ultimately leads to formation of a solid coating film. Such a feature shows a potential of this material as a repairing agent in organic coatings. In an exemplary embodiment, a diffusion of a corrosive solution inside self-healing anticorrosive coating 100 leading to a contact with plurality of nanofibers 116 may allow for releasing PDMS polymer core as a result of dissolution of hydrophilic PVA polymer shell and forming a passive protective layer on metal surface 101. Such passive protective layer may prevent further penetration of corrosive ions through self-healing anticorrosive coating 100. In an exemplary embodiment, after diffusion of aqueous solution into self-healing anticorrosive coating 100, Si-OR groups may be hydrolyzed and form Si-OH bonds. Moreover, some condensation reactions may further occur and other Si-O-Si and Si-O-C bonds may be formed inside self-healing anticorrosive coating 100. By formation of these silane bonds in an exemplary epoxy polymer matrix, a density of cross-link may increase, and diffusion paths of electrolyte through self- healing anticorrosive coating 100 may be reduced.

[0074] In an exemplary embodiment, each part of self-healing anticorrosive coating 100 may have at least one of a self-healing role, an anti-corrosive role, and combinations thereof while self-healing anticorrosive coating 100 being coated on metal surface 101. In an exemplary embodiment, core 118 including an organic polymer may be designed to protect metal surface 101 against corrosion. In an exemplary embodiment, core 118 may be an effective physical barrier for preventing corrosive agents to reach an interface of metallic substrate 105. In an exemplary embodiment, epoxy resins of epoxy matrix 114 may be utilized in layers of epoxy-silanized graphene oxide nanocomposite 102 or 104 for coating metal surface 101 and producing a composite material due to their high adhesion, excellent electrical insulation properties, low shrinkage during curing, and high chemical stability. However, exemplary epoxy resins may provide a path for diffusing corrosive ions into a coating containing exemplary epoxy resins due to brittleness and defects such as pores and cracks created during a synthesis process, which leads to destruction of an exemplary coating and reduction of corrosion resistance over time. Herein, graphene oxide nanosheets 110 may be352-8266 added to epoxy matrix 114 to improve anti-corrosion performance of exemplary epoxy resins, which may be ascribed to high specific surface area of graphene oxide nanosheets 110 due to its sheet-shaped structure. Well-dispersed graphene oxide nanoparticles may reduce pores in epoxy matrix 114, electrolyte penetration towards metallic substrate 105, and water penetration coefficient. Generally, graphene oxide may contain many reactive functional groups such as carboxylic acid at the edge, and epoxy and hydroxyl groups in a base sheet of graphene oxide, which may cause an inconsistency with organic solvents and polymers based on these solvents. In an exemplary embodiment, functionalizing graphene oxide with organic and / or inorganic compounds may be utilized for making a graphene oxide containing composition, which may be easily dispersed in polymers and increases inter-space interactions. Herein, graphene oxide nanosheets 110 functionalized with 3- glycidyloxypropyltrimethoxysilane (GPTMS) 112 may be used as a nanofiller to improve corrosion resistance and self-healing properties of an exemplary nanocomposite coating of layers of epoxy-silanized graphene oxide nanocomposite 102 or 104.

[0075] FIG. 2 shows a flowchart of a method 200 for producing a self-healing anticorrosive coating on a metal surface, consistent with one or more exemplary embodiments of the present disclosure. In an exemplary embodiment, method 200 may include producing graphene oxide nanosheets functionalized with 3-glycidyloxypropyltrimethoxysilane (GPTMS) (GPTMS-GO) (step 202), producing an epoxy-silanized graphene oxide nanocomposite by dispersing an exemplary formed GPTMS-GO in an epoxy matrix (step 204), preparing an exemplary metal surface of a metallic substrate for coating an exemplary self-healing anticorrosive coating thereon (step 206), depositing a first layer of an exemplary epoxy-silanized graphene oxide nanocomposite on an exemplary prepared metal surface (step 208), electrospinning a layer of core-shell nanofibers on an exemplary first layer of the epoxy-silanized graphene oxide nanocomposite (step 210), depositing a second layer of an exemplary epoxy-silanized graphene oxide nanocomposite on an exemplary electrospun layer of core-shell nanofibers (step 212), and curing and drying a three-layered formed coating comprising the first layer of the epoxy-silanized graphene oxide nanocomposite, the electrospun layer of core-shell nanofibers, and the second layer of the epoxy-silanized graphene oxide nanocomposite formed on the metal surface (step 214). In an exemplary embodiment, method 200 may be utilized for forming self-healing anticorrosive coating 100352-8266 on metal surface 101, so steps of method 200 may be described herein below in connection with FIGs.1A-1D.

[0076] In further detail with respect to step 202, step 202 may include producing graphene oxide nanosheets functionalized with 3-glycidyloxypropyltrimethoxysilane (GPTMS) (GPTMS-GO). In an exemplary embodiment, step 202 may include producing graphene oxide nanosheets 110 functionalized with GPTMS 112 (GPTMS-GO 111). In an exemplary embodiment, producing graphene oxide nanosheets 110 functionalized with GPTMS 112 may include forming a mixture by adding a plurality of graphene oxide nanosheets to a container containing ethanol, deionized water, and GPTMS, agitating an exemplary mixture by stirring an exemplary mixture for a time period in a range of about 15 minutes to about 1 hour, adjusting a pH value of an exemplary mixture within a range of 4 to 5 by adding a first base to an exemplary mixture while stirring an exemplary mixture, stirring an exemplary mixture for a time period in a range of 20 hours to 25 hours, adjusting a pH value of an exemplary mixture within a range of 8.5 to 9.5 by adding a second base to an exemplary mixture while stirring an exemplary mixture, and stirring an exemplary mixture at a constant temperature in a range of 65 ºC to 75 ºC for a time period in a range of 1 hour to 3 hours. In an exemplary embodiment, each of an exemplary first base and second base may include sodium hydroxide (NaOH).

[0077] In an exemplary embodiment, an exemplary mixture may be in form of a suspension. In an exemplary embodiment, step 202 may further include removing unreacted ethanol, deionized water, and GPTMS from an exemplary mixture. In an exemplary embodiment, removing unreacted ethanol, deionized water, and GPTMS from an exemplary mixture may include centrifuging an exemplary mixture for a time period in a range of 3 minutes to 10 minutes at a centrifugation speed in a range of 3000 rpm to 5000 rpm. In an exemplary embodiment, centrifuging an exemplary mixture may include dividing an exemplary suspension into a clear phase and a precipitation. In an exemplary embodiment, an exemplary clear phase may include unreacted ethanol, deionized water, and GPTMS. In an exemplary embodiment, an exemplary precipitation may include GPTMS-GO 111.

[0078] In an exemplary embodiment, step 202 may further include removing an excess amount of unreacted GPTMS adsorbed on graphene oxide nanosheets from an exemplary precipitation by washing an exemplary precipitation using a mixture of ethanol-deionized water with a volume ratio of ethanol:deionized water equal to 3:1.352-8266

[0079] In an exemplary embodiment, step 202 may further include removing excess residual deionized water from an exemplary precipitation by washing an exemplary precipitation with diethyl ether and maintaining an exemplary precipitation in toluene. In an exemplary embodiment, an exemplary precipitation after removing unreacted ethanol, deionized water, and GPTMS may include GPTMS-GO 111 including graphene oxide nanosheets 110 functionalized with GPTMS 112 with a weight ratio of GPTMS to GPTMS-GO 111 in a range of about 0.1 wt% to about 0.3 wt%. In an exemplary embodiment, a weight ratio of GPTMS to GPTMS-GO 111 in exemplary formed GPTMS-GO 111 may be about 0.2 wt%.

[0080] In further detail with respect to step 204, step 204 may include producing an epoxy- silanized graphene oxide nanocomposite by dispersing exemplary formed GPTMS-GO in an epoxy matrix. In an exemplary embodiment, an exemplary produced epoxy-silanized graphene oxide nanocomposite in step 204 may include a nanocomposite of GPTMS-GO 111 dispersed in exemplary epoxy matrix 114 (GPTMS-GO-EP). In an exemplary embodiment, step 204 may include producing an exemplary nanocomposite of graphene oxide nanosheets 110 functionalized with GPTMS 112 dispersed in epoxy matrix 114.

[0081] In an exemplary embodiment, producing an exemplary nanocomposite of graphene oxide nanosheets 110 functionalized with GPTMS 112 dispersed in epoxy matrix 114 may include forming a mixture of GPTMS-GO 111 in an organic solvent and dispersing GPTMS- GO 114 in epoxy matrix 114. In an exemplary embodiment, forming an exemplary mixture of GPTMS-GO 111 may include adding GPTMS-GO 111 to a container containing an exemplary organic solvent and stirring GPTMS-GO 111 and an exemplary organic solvent for a time period in a range of 5 minute to 20 minutes at a temperature in a range of 0 ºC to 4 ºC. In an exemplary embodiment, a mixture of GPTMS-GO 111 and an exemplary organic solvent may be stirred using an ultrasonic probe. In an exemplary embodiment, an exemplary organic solvent may include at least one of toluene, methylbenzene, phenylmethane, and combinations thereof. In an exemplary embodiment, an exemplary may be placed in an ice bath, where stirring GPTMS-GO 111 and an exemplary organic solvent may be carried out at an exemplary temperature range of 0 ºC to 4 ºC. In an exemplary embodiment, a mixture of GPTMS-GO 111 and an exemplary organic solvent may be stirred for about 10 minutes.

[0082] In an exemplary embodiment, dispersing GPTMS-GO 114 in epoxy matrix 114 may include adding an epoxy resin to an exemplary mixture of GPTMS-GO 111 in an exemplary organic solvent; stirring an exemplary mixture of GPTMS-GO 111 in an exemplary organic352-8266 solvent with an exemplary epoxy resin at a stirring speed in a range of 500 rpm to 1500 rpm for a time period in a range of 20 hours and 30 hours using a mechanical stirrer, sonicating an exemplary mixture of GPTMS-GO 111 in an exemplary organic solvent with an exemplary epoxy resin for a time period in a range of 5 minute to 20 minutes using an ultrasonic probe, adding a hardener with a weight ratio in a range of 1.3:1 (epoxy resin:hardener) to an exemplary mixture of GPTMS-GO 111 in an exemplary organic solvent with an exemplary epoxy resin, and stirring an exemplary mixture of GPTMS-GO 111 in an exemplary organic solvent with an exemplary epoxy resin and an exemplary added hardener for a time period in a range of 5 minute to 20 minutes using a mechanical stirrer. In an exemplary embodiment, an exemplary mixture of GPTMS-GO 111 in an exemplary organic solvent with an exemplary mixture of an exemplary epoxy resin and an exemplary hardener may be stirred mechanically, using a propeller or a blade. In an exemplary embodiment, an exemplary epoxy resin may include a bisphenol A (BPA)-based epoxy resin. In an exemplary embodiment, an exemplary hardener may include an amide hardener.

[0083] In further detail with respect to step 206, step 206 may include preparing an exemplary metal surface of a metallic substrate for coating an exemplary self-healing anticorrosive coating thereon. In an exemplary embodiment, step 206 may include preparing metal surface 101 of metallic substrate 105 for coating self-healing anticorrosive coating 100 thereon. In an exemplary embodiment, step 206 of preparing metal surface 101 may include grinding metal surface 101 using a silicon carbide (SiC) paper, washing and degreasing an exemplary ground metal surface 101 with at least one of acetone, ethanol, distilled water, and combinations thereof, drying an exemplary washed metal surface 101, and preventing oxidation and / or rusting of metal surface 101 by maintaining metallic substrate 105 in a desiccator and vacuum environment before depositing an exemplary epoxy-silanized graphene oxide nanocomposite thereon. In an exemplary embodiment, maintaining metallic substrate 105 in a desiccator and vacuum environment may prevent moisture absorption onto metallic substrate 105; allowing for preventing oxidation and / or rusting of metal surface 101.

[0084] In further detail with respect to step 208, step 208 may include depositing a first layer of an exemplary epoxy-silanized graphene oxide nanocomposite on an exemplary prepared metal surface. In an exemplary embodiment, step 208 may include depositing first layer of epoxy-silanized graphene oxide nanocomposite 102 on exemplary prepared metal surface 101. In an exemplary embodiment, depositing first layer of epoxy-silanized graphene oxide352-8266 nanocomposite 102 on exemplary prepared metal surface 101 may include forming a layer with a thickness in a range of 30 µm to 40 µm on prepared metal surface 101 by spraying an exemplary epoxy-silanized graphene oxide nanocomposite on the prepared metal surface 101.

[0085] In further detail with respect to step 210, step 210 may include electrospinning a layer of core-shell nanofibers on an exemplary first layer of the epoxy-silanized graphene oxide nanocomposite. In an exemplary embodiment, step 210 may include forming layer of electrospun core-shell nanofibers 103 on first layer of epoxy-silanized graphene oxide nanocomposite 102. In an exemplary embodiment, step 210 may include forming layer of electrospun core-shell nanofibers 103 by coaxial electrospinning of two polymers on first layer of epoxy-silanized graphene oxide nanocomposite 102. In an exemplary embodiment, forming layer of electrospun core-shell nanofibers 103 on first layer of epoxy-silanized graphene oxide nanocomposite 102 may include coaxial electrospinning of two exemplary polymers on first layer of epoxy-silanized graphene oxide nanocomposite 102 while first layer of epoxy-silanized graphene oxide nanocomposite 102 being wet or before first layer of epoxy-silanized graphene oxide nanocomposite 102 become dried. In an exemplary embodiment, layer of electrospun core-shell nanofibers 103 may be formed on first layer of epoxy-silanized graphene oxide nanocomposite 102 within a time period of 10 min to 40 min after depositing first layer of epoxy-silanized graphene oxide nanocomposite 102 on exemplary prepared metal surface 101. In an exemplary embodiment, an exemplary coaxial electrospinning process may allow for producing core-shell spiral morphology for loading a self-healing agent (i.e., PDMS) in a polymeric matrix.

[0086] In an exemplary embodiment, step 210 of coaxial electrospinning of two exemplary polymers may include electrospinning a first polymer through an inner nozzle of a coaxial pair of nozzles on first layer of epoxy-silanized graphene oxide nanocomposite 102 and electrospinning a second polymer through an outer nozzle of an exemplary coaxial pair of nozzles on first layer of epoxy-silanized graphene oxide nanocomposite 102. In an exemplary embodiment, an exemplary first polymer may include a self-healing material. In an exemplary embodiment, an exemplary first polymer may include PDMS and an exemplary second polymer may include PVA. In an exemplary embodiment, forming layer of electrospun core-shell nanofibers 103 may include coaxial electrospinning of PDMS as core 118 of and PVA as shell 120 of each nanofiber 116 of layer of electrospun core-shell nanofibers 103 on first layer of epoxy-silanized graphene oxide nanocomposite 102.352-8266

[0087] In an exemplary embodiment, coaxial electrospinning of two exemplary polymers may be done at a PDMS concentration range of 20 wt% to 50 wt% in a PDMS solution electrospun using an exemplary inner nozzle. In an exemplary embodiment, coaxial electrospinning of two exemplary polymers may be done at a PVA concentration range of 5 wt% to 20 wt% in a PVA solution electrospun using an exemplary outer nozzle. In an exemplary embodiment, coaxial electrospinning of two exemplary polymers may be done at a voltage in a range of 10 kV to 20 kV. In an exemplary embodiment, coaxial electrospinning of two exemplary polymers may be done at a shell feeding rate (PVA feeding rate) in a range of 0.5 mL.h-1to 2 mL.h-1. In an exemplary embodiment, coaxial electrospinning of two exemplary polymers may be done at a core feeding rate (PDMS feeding rate) in a range of 0.05 mL.h-1to 0.5 mL.h-1.

[0088] In further detail with respect to step 212, step 212 may include depositing a second layer of an exemplary epoxy-silanized graphene oxide nanocomposite on an exemplary electrospun layer of core-shell nanofibers. In an exemplary embodiment, step 212 may include depositing second layer of an exemplary epoxy-silanized graphene oxide nanocomposite 104 on electrospun layer of core-shell nanofibers 103. In an exemplary embodiment, depositing second layer of an exemplary epoxy-silanized graphene oxide nanocomposite 104 on electrospun layer of core-shell nanofibers 103 may include forming a layer with a thickness in a range of 60 µm to 100 µm on electrospun layer of core-shell nanofibers 103 by spraying an exemplary epoxy-silanized graphene oxide nanocomposite on electrospun layer of core-shell nanofibers 103.

[0089] In an exemplary embodiment, a sandwich-like self-healing anticorrosive coating 100 may be coated on metal surface 101. In an exemplary embodiment, sandwich-like self- healing anticorrosive coating 100 may include a three-layer coating including electrospun layer of core-shell nanofibers 103 placed between first layer of epoxy-silanized graphene oxide nanocomposite 102 and second layer of an exemplary epoxy-silanized graphene oxide nanocomposite 104, which may be coated on metal surface 101. In further detail with respect to step 214, step 214 may include curing and drying an exemplary three-layered coating formed on metal surface 101. In an exemplary embodiment, step 214 may include curing and drying self-healing anticorrosive coating 100. In an exemplary embodiment, step 214 may include curing and drying self-healing anticorrosive coating 100 by maintaining an exemplary three-layered formed coating at ambient temperature in a range of 20 ºC to 30 ºC352-8266 for a time period in a range of 20 hours to 60 hours and baking an exemplary three-layered formed coating at a temperature in a range of 55 ºC to 65 ºC for a time period in a range of 20 hours to 30 hours. In an exemplary embodiment, a thickness of self-healing anticorrosive coating 100 after drying and curing may be in a range of about 100 µm to about 150 µm.

[0090] EXAMPLE 1: Producing a self-healing anticorrosive coating

[0091] In this example, a self-healing anticorrosive coating similar to self-healing anticorrosive coating 100 was produced utilizing a method similar to method 200. Graphene oxide (GO) prepared using a modified Hummers' method was used as a corrosion resistant improver for producing an epoxy-graphene (EPG) nanocomposite. GPTMS with 98% purity was used for functionalizing the graphene oxide. An epoxy resin (Epiran-01X75), which was a solvent base may was used for creating a polymer matrix in an exemplary nanocomposite coating. In detail, precursor compound GPTMS (C9H20O4Si) with a molecular weight of 236. 34 g / mol (98%), ethanol (C2H5OH) 98%, sodium hydroxide (NaOH), deionized water were used utilizing a sol-gel method for dispersion and consistency of graphene oxide and to create a strong chemical bond in an epoxy polymer matrix.

[0092] First, 54.04 mL of the graphene oxide mixture (3.7 g / L) containing 0.2 g of graphene oxide was added to a container containing 80 mL of ethanol, 15 mL of deionized water, and 5 mL of GPTMS and stirred for 30 min using a magnetic stirrer to form a mixture. pH of the mixture was adjusted to 4.5 by adding 5 wt % sodium hydroxide. After that, the mixture was stirred on a magnetic stirrer for 22 hours. pH of a resultant mixture wase raised to 9 by using sodium hydroxide 5 wt %. The mixture was stirred on a heater at a constant temperature of 70 °C for 2 hours. Adsorbed silanes on graphene oxide surface were allowed to perform condensation reaction better and intensify formation of silicon oxide particles. A formed GO- SiO2suspension was centrifuged for 5 min at 4000 rpm for five times, and an unreacted mixture of water, alcohol, and silane was removed. Furthermore, unreacted excess silanes adsorbed on surface of graphene oxide were removed by washing the resultant mixture by using a mixture of ethanol-deionized water (V / V, 3:1) five times. Finally, the resultant mixture was washed with diethyl ether five times and kept in toluene to remove residual water. GO-SiO2 mixture with 0.2 wt% was added to a beaker containing toluene and stirred using an ultrasonic probe for 10 min in an ice bath. Then, the resultant mixture was added to an epoxy resin, and an amide hardener was added to the epoxy-GO-SiO2 mixture with a weight ratio of 1.3:1 (resin to hardener) and mechanically stirred. Crayamid115 amide352-8266 hardener was used as the hardener and toluene was used as a solvent for dissolving and diluting the epoxy resin and amide hardener. The mixture was stirred for 24 hours at a speed of 1000 rpm for dispersing the graphene oxide using a propeller mechanical stirrer. The epoxy-GO-SiO2 mixture was sonicated using an ultrasonic probe for 10 minutes. Then, the epoxy-GO-SiO2 nanocomposite mixture was coated on surface of steel substrates through the spray method. ST-12 steel was used as a metallic substrate which is widely used in industry. ST-12 steel samples with a dimension of 2.5 cm × 6 cm × 0.1 cm were ground with silicon carbide (SiC) paper with grit sizes of 200-600, and washed and degreased with ethanol, acetone, and distilled water, and then dried. To prevent oxidation or rusting of steel sheet surfaces due to moisture absorption, they were placed in a desiccator and vacuum environment before coating. At about 30 minutes after coating a first layer of epoxy-GO- SiO2 nanocomposite mixture on the steel substrates and while surface of first layer of epoxy- GO-SiO2 nanocomposite mixture was not completely dried, the coated steel substrates were placed in an electrospinning system as a collector, and coaxial electrospinning of PDMS- PVA (core-shell) fibers at a voltage of about 13 kV was done. The electrospinning process of PDMS-PVA (core-shell) fibers was carried out using a PDMS solution with 40 %wt of PDMS as the core material, a PVA solution with 7, 10, and 15 wt% of PVA as the shell material, a shell feeding rate of 1 mL.h-1, and a core feeding rate of 0.2 mL.h-1. A coaxial needle with an inner needle number G24 (with outer diameter of 0.55 mm and inner diameter of 0.30 mm) and an outer needle numbered G18 (with an outer diameter of 1.26 mm and an inner diameter of 0.9 mm)) was used. Electrospinning distance between a coaxial nozzle and steel substrates was about 18 cm. After the electrospinning process, the samples were kept at room temperature for 24 hours and finally annealed at 60°C for 24 hours.

[0093] FIG. 3 shows Fourier transform infrared (FTIR) spectra 300 of polyvinyl alcohol (PVA) polymer solution (FTIR spectrum 302), polydimethylsiloxane (PDMS) polymer solution (FTIR spectrum 304), and core-shell fibers (PDMS-PVA) (FTIR spectrum 306), consistent with one or more exemplary embodiments of the present disclosure. It is apparent from the FTIR spectrum 302 of polyvinyl alcohol that the absorption band in the region of 3448 cm-1is related to OH groups that are free or bound to the molecule. The absorption band at 2954 cm-1corresponds to the symmetric stretching vibration of the alkyl group (-CH2) in polyvinyl alcohol. The absorption band at 1635 cm-1region corresponds to the stretching carbonyl group (C=O), the absorption band at 1422 cm-1region corresponds to CH2 groups352-8266 (C–H bending vibrations), at 1100 cm-1corresponds to C– O of acetyl group and at 1750 cm- 1 corresponds to the stretching group C-C, all of these chemical species represent PVA. Si- CH3stretching bond at 1262 cm-1, Si-O-Si stretching bond at 1090-1022 cm-1, Si-CH3bending bond at 800 cm-1, and C-H bond is observed at 2963 cm-1, which represents the peaks observed in PDMS solution. Lipophilic and hydrophobic behavior is attributed to the presence of methyl groups around the Si-O-Si polymer. The dissociation energy of the Si-O bond is equal to 1110 kcal.mol-1, which is larger than the energy of C-O (5.85 kcal.mol-1), C- C (6.182 kcal.mol-1) and Si-C (76 kcal.mol-1) is the reason for the high thermal stability of polyorganosiloxanes. It has also been observed from the FTIR spectrum 306 of core-shell fibers of PDMS-PVA that the bonds presented in the spectra 302 and 304 related to PVA and PDMS are present in core-shell spectrum 306 and no new bond that indicates the reaction of these two polymers in core-shell fibers has been observed, therefore, PDMS is well loaded to the core of nanofiber.

[0094] FIG. 4 shows a transmission electron microscopy (TEM) image of PDMS-PVA core- shell nanofibers, consistent with one or more exemplary embodiments of the present disclosure. TEM analysis was done to ensure the formation of core-shell structure in PDMS- PVA nanofibers. As it is clear from FIG. 4, the structure of the core-shell fibers has been created with completely separate boundaries without nodes or defects. The continuous presence of core material within the core-shell fibers is also evident. The size of the core and core-shell fiber diameter was measured by Image J software.

[0095] After forming electrospun layer of core-shell fibers on the first layer of epoxy-GO- SiO2nanocomposite mixture on the steel substrates, a second layer of epoxy-GO-SiO2nanocomposite mixture was sprayed on the electrospun layer of core-shell fibers. Finally, to curing and drying the final three-layer sandwich structure, the samples were kept at ambient temperature for 24 hours and finally baked at 60°C for 24 hours. A thickness of the entire three-layer sandwich coating after drying was measured to be about 120 ± 10 µm.

[0096] FIG. 5 shows a FESEM image of cross-sectional surface of a produced self-healing anticorrosive coating including an epoxy-silanized graphene oxide coating containing core- shell fibers (image 502), a cross-sectional image of a portion of middle layer 501 of the produced self-healing anticorrosive coating (image 504), linear elemental EDAX analysis in direction of white arrow 503 along with thickness of the produced self-healing anticorrosive coating (diagram 506), and magnification of a portion of PDMS-PVA core-shell nanofibers352-8266 505 of portion of middle layer 501 of the produced self-healing anticorrosive coating (image 508), consistent with one or more exemplary embodiments of the present disclosure. As may be observed form image 502, a total thickness of the produced self-healing anticorrosive coating is about 120 µm. A first layer of GPTMS-GO-EP nanocomposite has a thickness of about 39 µm, a middle layer of PDMS-PVA core-shell nanofibers has a thickness of about 17 µm, and a second layer of GPTMS-GO-EP nanocomposite has a thickness of about 71 µm. As may be seen from EDAX analysis diagram 506, carbon, oxygen, and silicon elements are evident in the produced self-healing anticorrosive coating. An intensity of silicon element has increased in the middle layer, which indicates a presence of the PDMS core in these fibers, while it has the same intensity in the first and the second layers of GPTMS-GO-EP nanocomposite. The presence of core-shell PDMS-PVA fibers in the produced self-healing anticorrosive coating is clearly identified in FESEM image 508.

[0097] EXAMPLE 2: The effect of functionalizing graphene oxide with silane precursor in the epoxy-silanized graphene oxide nanocomposite

[0098] In this example, an effect of functionalizing graphene oxide with silane precursor (GPTMS) in epoxy-silanized graphene oxide nanocomposite layers of an exemplary produced self-healing anticorrosive coating in EXAMPLE 1 was analyzed.

[0099] FIG. 6 shows Fourier transform infrared (FTIR) spectra of pure epoxy (spectrum 602), epoxy-graphene oxide (spectrum 604), and epoxy-silanized graphene oxide nanocomposite (spectrum 606), consistent with one or more exemplary embodiments of the present disclosure. The range around 3400 cm-1is related to the stretch vibration of the hydroxyl (OH) groups. The peaks at 2870 and 2930 cm-1are ascribed to the C-H stretch vibration of the CH2 and CH3 bonds. The approximate peaks at 1724, 1248, and 1037 cm-1are assigned to the stretch vibration of carbonyl (C=O), carboxyl (C-OH), and epoxide (C-O) groups, respectively. The peaks belonging to the epoxy groups were observed at 829 and 913 cm-1. Comparing the FTIR spectra of epoxy and the above-mentioned nanocomposites indicated that the position of the OH stretch vibration peak in the epoxy / silica nanocomposite shifted to a higher frequency indicating the participation of the hydroxyl functional group in the bonding between the substrate and the graphene oxide nanosheets in the nanocomposite. The FTIR spectra of epoxy-functionalized graphene oxide shows the Si-O-Si bands include an asymmetric vibration peak at 460 cm-1, which proves a presence of silanes and silicon oxide nanoparticles on graphene oxide sheets in the nanocomposite structure.352-8266

[0100] An effect of functionalizing graphene oxide on thermal stability of epoxy coating was evaluated using thermogravimetric analysis (TGA) test. FIG. 7 shows a thermal analysis of epoxy-graphene oxide coating in two cases without (curve 702) and with (curve 704) graphene oxide functionalized with silane precursor, consistent with one or more exemplary embodiments of the present disclosure. Weight loss occurs in four temperature ranges including 90-250 °C, 250-354 °C, 354-465 °C, and 465-700 °C. The weight loss in the range of 90-250 °C and 250-354 °C related to water removal and decomposition of oxygenated groups such as hydroxyl. A significant weight loss is observed at about 354-465 °C, which may be attributed to the decomposition of organic compounds in the epoxy coating structure. Finally, the weight loss related to the temperature range of 465-700 °C is due to the decomposition of the C-C bonds of the carbon structure of the coating. The weight loss in the first range in the epoxy-functionalized graphene oxide was lower compared with that of the epoxy-graphene oxide coatings. The greater thermal stability is related to the reaction of functional groups on graphene oxide sheets such as hydroxyl with silicon oxide nanoparticles and functional groups of the silanized-functionalized compound.

[0101] Further thermal stability of epoxy-functionalized graphene oxide composite coating is related to a better distribution of modified nanosheets in an exemplary epoxy matrix compared to non-functionalized GO sheets, formation of more silica nanoparticles, and interactions between GO surface and epoxy matrix. FIG. 8 shows FESEM images of an epoxy-graphene oxide coating at 0.2 wt% (image 802), an epoxy-functionalized graphene oxide with silane coating at 0.2 wt% (image 804), and EDAX elemental analysis 806 related to image 804 of the epoxy-functionalized graphene oxide with silane coating at 0.2 wt%, consistent with one or more exemplary embodiments of the present disclosure.

[0102] As observed in image 804, spreading and delamination of graphene oxide sheets in matrix of epoxy coating are significantly improved after being functionalized with silane compared to distribution of non-functionalized graphene oxide sheets of image 802. Silane- functionalized GO nanosheet is distributed in the epoxy polymer matrix homogeneously and uniformly. The absorption of silicon oxide nanoparticles and the binding of silane molecules on the graphene oxide sheets increase their distance and, as a result, decrease the hydrophilicity and increase the affinity of the particles to the polymer, which prevents an accumulation of GO sheets and causes a better distribution of GO nanosheets. It can also be seen that the silanized GO sheets are placed inside the polymer matrix and do not protrude352-8266 from the polymer matrix, which is due to an strong bond between the silane graphene oxide particles and the polymer through terminal functional groups in the silane structure. EDAX elemental analysis 806 shows an spectrum of EDAX analysis taken from the epoxy-silanized graphene oxide composite coating surface, and a presence of silicon and oxygen peaks indicates a presence of silicon oxide on the coating surface. In silanized graphene oxide with the GPTMS precursor, the C-O-C epoxy functional group acts as an active site for reaction with the polymer matrix during resin curing. Functional groups of epoxy on silanized graphene oxide sheets are similar to epoxy groups in epoxy resin. In addition, silane molecules reduce hydrophilicity of the graphene oxide surface and increase its compatibility with the polymer matrix.

[0103] EXAMPLE 3: The effect of electrospinning parameters on core-shell nanofibers

[0104] In this example, electrospinning parameters in forming core-shell PDMS-PVA nanofibers as layer of electrospun core-shell nanofibers 103 of self-healing anticorrosive coating 100 were investigated. To investigate polymer shell concentration in coaxial electrospinning process for production of core-shell nanofibers as an intermediated layer of an exemplary three-layer sandwich coating on protection performance of an exemplary coating against corrosive environment and self-healing rate, shell concentrations of 7, 10, and 15 wt% PVA were tested. Furthermore, to investigate an effect of core feeding rate in an exemplary coaxial electrospinning process for production of core-shell nanofibers as an exemplary intermediated layer on protection performance of an exemplary coating against corrosive environment and self-healing rate, feeding rates of 0.1, 0.2 and 0.3 mL.h-1was varied. Moreover, to investigate effect of applied voltage in an exemplary coaxial electrospinning process for production of core-shell nanofibers as an intermediated layer of an exemplary three-layer sandwich coating on protection performance against corrosive environment and self-healing rate, voltages of 11, 13, and 16 kV were used. In all tests, core material solution was a PDMS solution with a PDMS concentration of 40 %wt, electrospinning distance from tip of syringe to collector was about 18 cm, and shell feeding rate was 1 mL.h-1.

[0105] FIG. 9 shows field emission scanning electron Microscopy (FESEM) and fluorescent microscope images of morphology of coaxial electrospun core-shell fibers at 13 kV voltage, core feeding rate 0.2 mL.h-1, distance 18 cm from tip of syringe to collector,352-8266 PDMS 40 wt% core solution, and concentration of PVA shell material of 15 wt% (FESEM image 902 and fluorescent image 908), 10 wt% (FESEM image 904 and fluorescent image 910), and 7 wt% (FESEM image 906 and fluorescent image 912), consistent with one or more exemplary embodiments of the present disclosure. As FESEM images of core-shell fibers can be seen in FIG. 9, with increasing concentration of PVA from 7 and 10 to 15 wt% which is used as the shell material, a diameter of core-shell fibers, also increased. Furthermore, distribution of fibers in a case where a concentration of shell polymer solution was 15 wt% (FESEM image 902), is more uniform and more precipitation than cases where concentration of PVA solution was 7 wt% (FESEM image 906) and 10 wt% (FESEM image 904). An increase in concentration causes an increase in polymer chain conflicts, which is necessary to achieve continuity of accelerated flow of solution during electrospinning. An increase in polymeric solution concentration may cause fiber diameter to increase, which may be probably due to that increasing the concentration of the polymer solution causes an increase in conflicts of an exemplary polymer chain, which is necessary to achieve the continuity of the accelerated flow of the solution during electrospinning. In an exemplary embodiment, diameter and width of fibers may increase with an increase in polymer solution concentration probably due to a greater resistance of the polymer solution to being pulled by the charges on the accelerated flow of the solution. Another reason for increasing an exemplary diameter of fibers with an increase in concentration of shell polymer solution is that an area of deposition of fibers on collecting plate is smaller at higher concentrations. An increase in concentration means that a viscosity of solution is strong enough to prevent bending instability of accelerated flow of solution relative to exit point of an exemplary used needle, and in fact, this causes fibers to accumulate in the smaller area. Therefore, a path of accelerated flow of the solution is shortened and a tendency of the solution to fog around is reduced. In addition, this reduction of the jet path means that the solution is subjected to less tension, which increases the diameter of the fibers. Also, at higher concentrations, an amount of solvent in the solution jet is less and the solvent evaporates faster. Therefore, with the evaporation of the solvent, it becomes more difficult to pull the jet, and fibers with a larger diameter are formed on the collector.

[0106] Moreover, images related to core-shell fibers obtained by using a fluorescent microscope, in different concentrations of the shell material, as can be seen in FIG. 9, the core material is continuously placed inside the core-shell fibers, and with the increase in352-8266 concentration of the shell polymer solution from 7 wt% (fluorescent image 912) to 15 wt% (fluorescent image 908), the core material is loaded with a larger amount, without any defect in the path of the core material in the shell.

[0107] FIG. 10 shows FESEM and fluorescent microscope images of morphology of coaxial electrospun core-shell fibers at 13 kV voltage, distance 18 cm from tip of syringe to collector, PDMS 40 wt% core solution, concentration of PVA shell material of 10 wt%, at core feeding rates of 0.3 mL.h-1(FESEM image 1002 and fluorescent image 1008), 0.2 mL.h-1(FESEM image 1004 and fluorescent image 1010), and 0.1 mL.h-1(FESEM image 1006 and fluorescent image 1012), consistent with one or more exemplary embodiments of the present disclosure. The FESEM microscope images and fluorescent microscope images shows the core-shell fibers produced in the mentioned electrospinning conditions at the feeding rates of 0.1 mL.h-1and 0.2 mL.h-1has a suitable morphology. They have no defects, such as nodes and fractures. By increasing the feeding rate of core material from 0.2 mL.h-1to 0.3 mL.h-1(FESEM image 1002 and fluorescent image 1008), diameter of core-shell fibers has increased and swollen areas may be seen along the length of the fibers, which indicates a non-uniform distribution of the core material inside the shell of the core-shell fibers. It can be seen in the fluorescent microscope images that continuity of the core material inside the core-shell fibers is less at the core feeding rate of 0.3 mL.h-1(fluorescent image 1008) compared to 0.2 mL.h-1(fluorescent image 1010). When the core feeding rate increases, there is a reciprocal increase in the fiber diameter that may be due to a larger volume of solution drawn out of the tip of the needle. However, there is a limit to increasing fiber diameter using higher feed rates. This means that if the feeding rate is a constant value at which an accelerated flow of the electrospinning solution exits, the electric charges are also constant. But, when the feed rate increases, the electrical loads must also increase. Therefore, an increase in electrical charges causes a reciprocal increase in tension of the solution, which opposes the increase in diameter and, as a result, the increase in volume. At the feeding rate of 0.3 mL.h-1, the fiber diameter increased, but the precipitation rate was lower than the rate of 0.2 mL.h-1. Some sprinkling is also seen in the fluorescent image, and in this case, the feeding rate of 0.2 mL.h-1is better for loading more repair material in core-shell fibers. In the feeding rate of 0.3 mL.h-1, although more material reached the needle and more fibers may be expected to be produced, since the electric charge is constant, the deposition rate, especially in the case of circular fibers, is lower than in the case of is 0.2 mL.h-1.352-8266

[0108] FIG. 11 shows FESEM and fluorescent microscope images of morphology of coaxial electrospun core-shell fibers at core feeding rate of 0.2 mL.h-1, distance 18 cm from tip of syringe to collector, PDMS 40 wt% core solution, concentration of PVA shell material of 10 wt%, at applied voltages of 16 kV (FESEM image 1102 and fluorescent image 1108), 13 kV (FESEM image 1104 and fluorescent image 1110), and 11 kV (FESEM image 1106 and fluorescent image 1112), consistent with one or more exemplary embodiments of the present disclosure. With an increase in the applied voltage, both the strength of the electric field and the number of electric charges on the surface of the polymer molecules increase and cause more tension resulting from the repulsion of the coulombic forces, which has led to a decrease in the diameter of the electrospun fibers. With the increase of the applied voltage from 11 to 13 and 16 kV, the diameter of the core-shell fibers decreased. At the voltage of 13 kV compared to 11 and 16 kV, the distribution of fibers is more uniform. At the voltage of 11 kV, although the diameter of the fibers is larger than 13 and 16 kV, due to the lower strength of the electric field, the deposition rate of the core-shell fibers is less, and uniform distribution of the core material in the fibers is not observed. As shown by fluorescent microscope images of core-shell fibers that have PDMS core mixed with methyl orange dye, the core material is continuously inside the shell. Although at the voltage of 13 kV, the continuity of the core material is more uniform.

[0109] EXAMPLE 4: The effect of electrospinning parameters on the protection performance of the self-healing anticorrosive coating

[0110] In this example, protection performance of exemplary self-healing anticorrosive coatings fabricated at different electrospinning conditions according to EXAMPLE 3 herein above, were tested and investigated. As a first analysis, electrochemical impedance spectroscopy tests were performed using a potentiostat / galvanostat apparatus and a frequency response analyzer in a frequency range of 100 kHz to 10 mHz and 50 steps per decade. Oscillation amplitude of 10 mV was used in a three-electrode cell to obtain Nyquist curves, bode, and bode phase in 3.5 wt% sodium chloride solution as an exemplary corrosive solution. The reference electrode was Ag / AgCl / Sat KCl, the auxiliary electrode was a platinum foil, and an exemplary coated metallic substrate with an exemplary self-healing anticorrosive coating was considered as the working electrode with a surface area of 1 cm2each. To confirm the reproducibility of the data, each measurement was performed for three samples prepared under the same conditions and representative values were reported. To352-8266 avoid complexity, only Nyquist curves are presented in the DRAWINGS and electrochemical impedance spectroscopy curves are not illustrated. However, electrochemical parameters related to fitting of impedance curves of an exemplary coating with equivalent electrical circuits during 148 days immersion in sodium chloride solution are summarized in following Tables. The results related to investigating an effect of PVA amount in an exemplary PVA shell solution are presented in FIGs.12, 14, and 15 and Tables 1-3 herein below.

[0111] FIG. 12 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with 7 wt% PVA shell solution (named as EPGSi-7%) at different immersion times in 3.5 wt% sodium chloride medium up to 1 day (diagram 1202), for 5, 12, 18, 29 and 46 days (diagram 1204), at 63, 78, 99, 120 and 132 days (diagram 1206), and 148 days (diagram 1208), consistent with one or more exemplary embodiments of the present disclosure. As can be seen at the initial immersion times, the diameter of the semicircle of the capacitive loop decreased by increasing the immersion times. The results indicate a decrease in the resistance of the coating against the corrosive environment, which corresponds to decreasing the impedance value at a low frequency over time. In this case, where the PVA polymer solution with a concentration of 7 wt% is used as the shell of the core-shell fibers, the diameter of the core-shell fibers is the lowest compared to the cases where concentrations of 10 and 15 wt% are used. In this case, less healable material is loaded as the core in produced fibers, which is consistent with the results of examining the morphology of these fibers.

[0112] FIG. 13 shows equivalent electrical circuit of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers in 3.5 wt% sodium chloride solution during long immersion times at early times (circuit 1302) and at long times (circuit 1302) of immersion, consistent with one or more exemplary embodiments of the present disclosure. Electrical circuits 1302 and 1304 contain Rs, Rc, Rct, CPEc, CPEdl, and n, which are listed in Table. 1. It may be seen that after 63 days, the second time constant, which indicates the beginning of corrosion reactions at an interface between an exemplary metallic substrate and an exemplary self-healing anticorrosive coating, appeared. In this self-healing anticorrosive coating, the resistance of the coating and the roughness parameter of the coating surface showed an increasing trend at 46, 78, and 132 days. At days 46 and 78, due to a self- healing function caused by the presence of core-shell fibers and the creation of a passive barrier layer due to the release of the PDMS core, and at day 132 of immersion, due to the352-8266 creation of a weak and loose layer of corrosion products, it led to an improvement in the protective performance of the coating.

[0113] Table 1. Electrochemical parameters related to fitting of impedance curves of an exemplary epoxy-silanized graphene oxide nanocomposite coating containing electrospun core-shell fibers with 7 wt% PVA shell solution with equivalent electrical circuits 1302 and 1304 during 148 days immersion in 3.5 wt% sodium chloride solution

[0114] FIG. 14 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with 10 wt% PVA shell solution (named as EPGSi-10%) at different immersion times in 3.5 wt% sodium chloride medium of 1, 5, 12 and 18 days (diagram 1402), 29, 46, 63 and 78 days (diagram 1404), and 99, 120, 132 and 148 days (diagram 1406), consistent with one or more exemplary embodiments of the present disclosure. A diameter of the semicircular capacitive loop in the Nyquist curve is smaller with increasing immersion time. In fact, an exemplary epoxy-silanized graphene oxide coating has a lower protection function with more penetration of corrosive solution and destruction of an exemplary epoxy-silanized graphene oxide coating. Compared to the 7 wt% cases, with the increase in the concentration of the polymer solution, due to more resistance of the solution to being stretched by the electric charges, the diameter of the shell fibers352-8266 increases, and the possibility of loading more healable material, PDMS, has been provided. In this case, at times 46, 78, and 132 days, the trend of increasing the impedance of the coating has been observed at low frequency, which is in good agreement with the behavior of the impedance spectra curves in this case. The self-healing process at 46 and 78 days has led to an increase in protective performance of the coating and prevented the continuation of the decreasing process. Creation of corrosion products at the interface between an exemplary metallic substrate and the coating is the reason for the relative and partial improvement of the impedance value in 132 days. The values related to fitting the impedance curves in Table 2 are in good agreement with the behavior of the impedance spectra curves. With an increase of immersion time, the resistances of the coating and the roughness parameter have decreased and the capacitor capacitance of the coating has increased. The increasing trend of Rc and n occurred at 46, 78, and 132 days and the decreasing trend of the CPEc occurred at this time. In an exemplary embodiment, at times 46 and d 78 days, it is due to the self-healing function of the core-shell fibers and at the time 132 days, due to the function caused by the formation of corrosion products.

[0115] Table 2. Electrochemical parameters related to fitting of impedance curves of an exemplary epoxy-silanized graphene oxide nanocomposite coating containing electrospun core-shell fibers with 10 wt% PVA shell solution with equivalent electrical circuits 1302 and 1304 during 148 days immersion in 3.5 wt% sodium chloride solution352-8266

[0116] FIG. 15 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with 15 wt% PVA shell solution (named as EPGSi-15%) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days (diagram 1502) and at 120, 132 and 148 days (diagram 1504), consistent with one or more exemplary embodiments of the present disclosure. According to FIG. 15, the immersion of the capacitive loop of the Nyquist semicircle is not complete until 99 days, which also indicates the low rate of corrosion in an exemplary coating. By increasing the immersion time from 29 to 46 days, the impedance value has increased from 8.50×109 Ω.cm2to 1.23×1011Ω.cm2and has increased by two times, which is due to the self-healing performance of the core-shell fibers in the coating is related to the early times of immersion. In this case, considering that the core-shell fibers are electrospun with PVA solution with a concentration of 15 wt% and considering the morphology of these fibers, the amount of healable material is loaded in the interconnected three-dimensional network of the core-shell fibers, which provides the possibility of more healing. The electrochemical parameters, measured by fitting impedance curves of the EPGSi-15% coating are summarized in Table 3. The resistance of the coating after one day of immersion is equal to 8.5×1010Ω.cm2and the capacitance of the coating at this time is 1.08×10-10Sn.Ω-1.cm-2, which shows high protection performance of352-8266 the coating in the early times of immersion. By further increasing the immersion time to 46 days, the resistance of the coating increased by more than one order, and the capacitance of the coating also decreased by about one order, which indicates the increase in the resistance of the coating.

[0117] Table 3. Electrochemical parameters related to fitting of impedance curves of an exemplary epoxy-silanized graphene oxide nanocomposite coating containing electrospun core-shell fibers with 15 wt% PVA shell solution with equivalent electrical circuits 1302 and 1304 during 148 days immersion in 3.5 wt% sodium chloride solution

[0118] In fact, as a result of the contact a corrosive aqueous solution with the core-shell fibers and the release of the PDMS polymer as a result of the dissolution of the PVA polymer shell, a passive protective layer has been created that prevents further penetration of corrosive ions into an exemplary produced coating. After the penetration of the aqueous solution into the coating, the Si-OR groups are hydrolyzed and form Si-OH bonds, and then the condensation reaction occurs, and other Si-O-Si and Si-O-C bonds are formed inside the coating. With the formation of these silane bonds in the epoxy polymer matrix, the density of the cross-link increases and the penetration paths of the electrolyte in the coating are reduced. In an exemplary embodiment, by increasing the immersion time to 63 days, the resistance of the coating decreases and the capacitance of the coating increases to a small amount. In an352-8266 exemplary embodiment, it may be observed that by increasing the immersion time to 78 days, the resistance of the coating increases and the capacitance of the coating decreases due to the self-healing function of the core-shell fibers loaded in the coating. In an exemplary embodiment, it should be noted that after 78 days of immersion in the corrosive solution, the resistance of the coating is in the range of 1010Ω.cm2and it shows the preservation of the resistance of the coating against the penetration of corrosive ions inside the coating due to the self-repairing function of the core-shell fibers.

[0119] Similarly, anti-corrosive protection performance of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers was tested by varying an exemplary applied voltage at three voltages of 11, 13, and 16 kV during an exemplary step of electrospinning of core-shell PDMS-PVA nanofibers as presented in FIGs. 16-18 herein below.

[0120] FIG. 16 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers at voltage of 11 kV (named as EPGSi-11kV) at different immersion times in 3.5 wt% sodium chloride medium up to 78 days (diagram 1602), 12 and 99 days (diagram 1604), 18, 29, 120, and 132 days (diagram 1606), and up to 148 days (diagram 1608), consistent with one or more exemplary embodiments of the present disclosure. As it is clear from the Nyquist curves, in the initial times of immersion, it has a large and incomplete capacitive loop, which indicates the high resistance of the coating against corrosion. In an exemplary embodiment, by increasing the immersion time up to 29 days, the diameter of the capacitive loops of the Nyquist curve is smaller and the semicircle tends to be complete. In fact, with the increase of immersion times up to 29 days due to the greater penetration of the corrosive electrolyte and the lower self-healing performance of the core-shell fibers, the resistance of the coating against the corrosive environment has decreased by about four times. By further increasing the immersion time to 46 days, the capacitive loop of the Nyquist curve has become larger. All of these cases confirm the increase in impedance value and the improvement of the protective performance of the coating as a result of the self-healing process of the core-shell fiber. An increase of the impedance value at low frequency may be observed at 78 days compared to 63 days. In 46 and 78 days, compared to the previous times, resistance of the coating and the surface roughness parameter of the coating may be increased and the capacitance of the coating decreased, which indicates the self-healing performance of the coating in these times.352-8266

[0121] FIG. 17 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers at voltage of 13 kV (named as EPGSi-13kV) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days (diagram 1702) and after 120, 132, and 148 days (diagram 1704), consistent with one or more exemplary embodiments of the present disclosure. As may be seen, the immersion of the capacitive loops of the Nyquist semicircle is not complete until 99 days, which also indicates the low rate of corrosion in this coating. By increasing the immersion time from 29 to 46 days, the impedance value has increased from 8.5×1010Ω.cm2to 1.23×1011Ω.cm2, which is related to the self-healing performance of the existing core-shell fibers. It is related to the coating in the early times of immersion. By increasing the immersion time from 46 to 63 days, the impedance value at the frequency of 10 mHz has decreased by one order, and the phase angle has decreased. By increasing the immersion time to 78 days, the impedance value may be increased again and the breakdown frequency was appeared in a lower frequency range compared to 63 days, which indicates the improvement of the protective performance of the coating during this time. This increase in resistance against the corrosive environment is due to the self-healing function of the core-shell fibers which are in the form of an interconnected network in the coating. The increase in the resistance of the coating against the corrosive media is due to the self-healing function of the core-shell fibers that are located in the coating in the form of an interconnected network. In this case, considering that the core-shell fibers are electrospun with a voltage of 13 kV and considering the morphology of these fibers, more amount of self-healing material is loaded in the interconnected three- dimensional network of the core-shell fibers, which provides more repair possibilities.

[0122] In fact, as a result of due to contact corrosive aqueous solution with the core-shell fibers and the release of the PDMS polymer as a result of the dissolution of the PVA polymer shell, a passive protective layer has been created that prevents further penetration of corrosive ions into the coating. After the penetration of the aqueous solution into the coating, the Si-OR groups may be hydrolyzed and form Si-OH bonds, and then condensation reaction occurs and other Si-O-Si and Si-O-C bonds may be formed inside the coating. With the formation of these silane bonds in the epoxy polymer matrix, the density of the cross-link increases and the penetration paths of the electrolyte in the coating may be reduced. With the increase of immersion times up to 120 days, a decrease in the resistance of the coating and an increase in the capacitor capacitance of the coating was observed, which indicates a decrease in the352-8266 protective performance of the coating. Although the amount of this reduction is not significant.

[0123] FIG. 18 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers at voltage of 16 kV (named as EPGSi-16kV) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days (diagram 1802), 29, 46, 63, 78, and 99 days (diagram 1804), and after 120, 132, and 148 days (diagram 1806), consistent with one or more exemplary embodiments of the present disclosure. As it has been obtained from the Nyquist curves of this sample, in the initial immersion times (1, 5, and 12 days), the diameter of the semicircular capacitive loop is 108Ω.cm2. The impedance value at low frequency in this sample is about two orders of magnitude lower than the sample in which the core-shell fibers are electrospun with an applied voltage of 13 kV. At the voltage of 16 kV compared to 13 kV, the core-shell fibers have a smaller diameter and have a lower possibility of loading healable materials. Therefore, the self-healing and barrier performance is lower than the 13 kV voltages. With the increase of immersion time, the trend of decreasing impedance at low frequencies was observed, and at 46 and 78 days, an increase in the value of impedance at low frequencies was observed due to the presence of self-healing materials and the creation of barrier due to the formation of the passive layer.

[0124] Moreover, anti-corrosive protection performance of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers was tested by varying an exemplary core feeding rate at three values of 0.1, 0.2, and 0.3 mL.h-1during an exemplary step of electrospinning of core-shell PDMS-PVA nanofibers as presented in FIGs. 19-21 herein below.

[0125] FIG. 19 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with a core feeding rate of 0.1 mL.h-1(named as EPGSi-0.1) at different immersion times in 3.5 wt% sodium chloride medium up to 1 day (diagram 1902), 5, 12 and 18 days (diagram 1904), 29 and 46 days (diagram 1906), 63, 78, 99 and 120 days (diagram 1908), and after 132 and 148 days (diagram 1910), consistent with one or more exemplary embodiments of the present disclosure. According to the Nyquist curves of the EPGSi-0.1 specimen in FIG. 19, it shows that the impedance at the frequency of 10 mHz after one day of immersion is 8.45×109Ω.cm2and its Nyquist curve is an incomplete semicircle which indicates the corrosion is low. With the increase of the immersion time up to 63 days, the impedance value has reached 4.89×106Ω.cm2, the352-8266 diameter of the semicircle of the Nyquist is smaller and the semicircle moves towards completion, which indicates the decrease corrosion resistance of the coating up to 3 times. By increasing the immersion time, the corrosive solution has penetrated through the defects in the coating and has reduced the resistance of the coating. With the increase of immersion time from 63 to 78 days, a relative and small increase in the impedance value at the frequency of 10 mHz has occurred from 4.89×106to 7.91×106Ω.cm2. This relative increase is due to the release of the self-healing PDMS polymer, due to the dissolution of the hydrophilic PVA polymer shell from the core-shell fibers, due to the contact of the aqueous solution with the hydrophilic shell. The reason for the low increasing is due to the lower loading of the healable material due to the low feeding rate in the electrospinning process. At 132 days of immersion, it was observed that the decreasing trend of resistance stopped and a slight increase in the resistance of the coating and charge transfer due to the formation of corrosion products and the creation of a barrier layer against the penetration of corrosive ions. With the increase of the immersion time up to 148 days, there is again a decreasing trend in the resistance of the coating and charge transfer, which indicates the poor performance of the corrosion products.

[0126] FIG. 20 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with a core feeding rate of 0.2 mL.h-1(named as EPGSi-0.2) at different immersion times in 3.5 wt% sodium chloride medium up to 99 days (diagram 2002) and after 120, 132, and 148 days (diagram 2004), consistent with one or more exemplary embodiments of the present disclosure. The impedance at the frequency of 10 mHz with increasing the feeding rate to 0.2 mL.h-1after one day of immersion was 8.50×1010Ω.cm2, which has increased compared to the feeding rate of 0.1 mL.h-1. By increasing the immersion time from 29 to 46 days, the impedance value increased from 8.50×109to 1.23×1011Ω.cm2, which is related to the self-healing performance of the existing core-shell fibers. It is related to the coating in the early times of immersion. By increasing the immersion time to 78 days, the impedance value increased again and the breakdown frequency compared to 63 days was appeared in a lower frequency range, which indicates the improvement of the protective performance of the coating at this time. This increase in resistance to the corrosive environment is due to the self-healing function of the core-shell fibers that are in the form of an interconnected network in the coating. In this case, since the fibers of the core-shell are electrospun with a feeding rate of 0.2 mL.h-1, and according to the352-8266 morphology of these fibers, a greater amount of self-healing material is loaded in the interconnected three-dimensional network of the core-shell fibers, which is possible to provide more loading healable material.

[0127] FIG. 21 shows Nyquist curves of an exemplary epoxy-silanized graphene oxide coating containing electrospun core-shell fibers with a core feeding rate of 0.3 mL.h-1(named as EPGSi-0.3) at different immersion times in 3.5 wt% sodium chloride medium after 1, 5, 45 and 78 days (diagram 2102), 12, 18, and 29 days (diagram 2104), 63, 99, 120, 132, and 148 days (diagram 2106), and 148 days (diagram 2108), consistent with one or more exemplary embodiments of the present disclosure. The impedance value at the frequency of 10 mHz after one day of immersion was 8.16×1010Ω.cm2. The large and incomplete capacitive loop of the Nyquist curve at this time indicates the better corrosion resistance performance of this coating in the initial times of immersion. In an exemplary embodiment, by increasing the immersion time up to 29 days, the diameter of the capacitive loop of the Nyquist curves may became smaller and more complete, which is consistent with the decrease in impedance at the frequency of 10 mHz continuously and partially, which indicates a partial decrease in resistance against the corrosive environment. There was an increase in impedance at the frequency of 10 mHz for immersion times of 46 and 78 days. In addition, increase the diameter of the incomplete capacitive loop of the Nyquist curve, and a transition of the breakdown frequency to a lower frequency range compared to the previous immersion times was illustrated, which indicates the protective performance of the coating is improved. In fact, for the EPGSi-0.3, the core-shell fibers are electrospun with a higher feeding rate than EPGSi-0.2. So, we expect to have more materials in the core of these fibers, but due to the lack of proper drying time during electrospinning and instability jet, the solvent did not have enough time to evaporate. Therefore, the amount of self-healing material was loaded in the core, and it is obvious that it shows a lower self-healing performance than the EPGSi-0.2.

[0128] EXAMPLE 5: The self-healing performance of the produced self-healing anticorrosive coatings at different electrospinning conditions via electrochemical impedance spectroscopy

[0129] In this example, the protective and self-healing effect of exemplary produced coatings according to EXAMPLE 3 described herein above, a deep cut was made on surface of exemplary metallic substrate with a sharp surgical blade, 4 cm long and 2 mm wide, to an extent that it was deep to top of the metallic substrate. Then, the effect of immersion times on352-8266 the corrosion resistance of coating was performed by electrochemical impedance spectroscopy similar to exemplary procedure explained in EXAMPLE 4 herein above.

[0130] In a first set of tests, performance of self-healing property of an exemplary nanocomposite coating containing core-shell nanofibers electrospun at concentrations of 7, 10 and 15 wt% of PVA was investigated via electrochemical impedance spectroscopy curves (for the simplicity, only Nyquist curves are illustrated in FIGs.22-24).

[0131] FIG. 22 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a PVA solution having a PVA concentration of 7 wt% (named as EPGSi-7%-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 2202), up to 36 hours (diagram 2204), after 8 and 12 days (diagram 2206), and up to 16 days (diagram 2208), consistent with one or more exemplary embodiments of the present disclosure. As it shows, after creating a scratch and after 24 hours of immersion, the Nyquist curve consists of two loops. At low frequencies, which is related to performing electrochemical reactions at the interface between the metallic substrate and the coating, and the second ring at higher frequencies, is related to the formation of a passive barrier layer due to the release of the self-healing material from the core-shell fibers. In fact, after creating a scratch, the self-healing process occurred in the first initial 24 hours of immersion, but with increasing immersion times, the impedance value at low frequencies has reduced significantly. In an exemplary embodiment, for the EPGSi-7% sample due to using a PVA polymer solution with a low concentration of 7 wt%, the diameter of the core-shell fibers may be decreased and the amount of loaded material is less than the self-healing material, and a weaker self-healing process has been observed in this case compared to 10 and 15 wt% (which confirmed morphological investigations explained in EXAMPLE 3 herein above). The fitting results of electrochemical impedance spectroscopy curves also show the increase of electrochemical corrosion reactions at the metal-coating interface with the decrease of Rcand Rctand the increase of CPEcand CPEdl(Table 4).

[0132] Table 4. Electrochemical parameters related to fitting of impedance curves of an exemplary scratched epoxy-silanized graphene oxide nanocomposite coating containing electrospun core-shell fibers with 7 wt% PVA shell solution with equivalent electrical circuits 1302 and 1304 during 16 days immersion in 3.5 wt% sodium chloride solution Sample Time RsCPEcn RcCPEdln Rct22352-8266 EPGSi-7%- 24 h 6972 3.055×10- 90.92 2.197×1072.291×10- 70.66scratched 1 5.017×10 36 h 4.704 8.909×10- 60.78 1.453×1052.752×10- 50.57 1.371×104oxide coating containing core-shell fibers electrospun with a PVA solution having a PVA concentration of 10 wt% (named as EPGSi-10%-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 2302), up to 36 hours (diagram 2304), after 8 and 12 days (diagram 2306), and up to 16 days (diagram 2308), consistent with one or more exemplary embodiments of the present disclosure. The Nyquist curves of the EPGSi-10% sample have increased in diameter at 36 hours compared to the initial 24 hours, and the impedance value has increased at low frequencies, which indicates the self-healing process at 36 hours of immersion. As the immersion time increases, the impedance value has decreased and the capacitance range and phase angles have decreased. At time 12 days, two capacitive loops is seen in the Nyquist curve, one at low frequency, which is related to the corrosion reactions at the interface between the metallic substrate and the coating, and the other at a higher frequency, which is related to the destruction of the coating. According to Table 5, Rcand Rctand parameter n increased at 36 hours of immersion compared to 24 hours of immersion, and CPEcand CPEctdecreased, which indicates the formation of a passive barrier film in the path of diffusion of the corrosive solution and prevention of corrosion reactions. In this case, the resistance values of the coating, the charge transfer resistance, and its decreasing trend with the passage of time are improved as compared to EPGSi-7% samples. In fact, by increasing the shell polymer solution concentration from 7 to 10 wt%, the diameter of the core-shell fibers increased, the amount of self-healing material loading increased, and finally, a greater self-healing process was carried out than EPGSi-7%.

[0134] Table 5. Electrochemical parameters related to fitting of impedance curves of an exemplary scratched epoxy-silanized graphene oxide nanocomposite coating containing electrospun core-shell fibers with 10 wt% PVA shell solution with equivalent electrical circuits 1302 and 1304 during 16 days immersion in 3.5 wt% sodium chloride solution Sample Time RsCPEcn RcCPEdln Rct22352-8266 8 d 29710 7.427×10- 70.72 1.531×1061.743×10- 60.89 7.931×10512 d 11276 7.169×10- 60.69 1.296×1052.482×10- 60.86 3.158×10516 d 7962 9.751×10- 60.63 4.261×1041.159×10- 50.62 3.957×104oxide coating containing core-shell fibers electrospun with a PVA solution having a PVA concentration of 15 wt% (named as EPGSi-15%-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 2402), up to 36 hours (diagram 2404), and after 8, 12 and 16 days (diagram 2406), consistent with one or more exemplary embodiments of the present disclosure. After 36 hours, the diameter of the semicircle of the capacitive loop in the Nyquist curve has become larger and the capacitive behavior has appeared in a larger range compared to 24 hours, which indicates the ability of active repair for self-healing coatings after the initial damage. Self-healing materials have prevented the diffusion of the corrosive environment into the coating and have led to the improvement of the protective performance of the coating. With the further increase of the immersion time, the impedance value in low frequencies continuously decreased. This behavior is in good agreement with the reduction of the diameter of the Nyquist semicircle and the reduction of the phase angle. However, in the EPGSi-15% sample compared to the EPGSi-7% and EPGSi-10%, the magnitude of the impedance is higher at all immersion times and the rate of impedance reduction is low. In such a way, after 16 days of immersion, the impedance at the low frequency of the scratched sample in the EPGSi-15% sample is equal to 1.39×108Ω.cm2, compared to the EPGSi-10% sample (4.26×104Ω .cm2) at the same time it is three times larger. In fact, in the EPGSi-15% sample, due to the higher feeding rate and deposition of core-shell fibers with a more uniform distribution, it is possible to load more and better self- healing material, which leads to better self-healing and increase the barrier properties as a result of the formation of the passive layer. Data in Table 6 shows a good agreement between the values obtained by fitting the impedance curves at different immersion times. The values of Rc and Rct after 36 hours in comparative to 24 hours increased. Increasing Rc and Rct indicates the formation of a passive film at the interface of the metal and coating layer, which can affect the adhesion of the epoxy coating to improve the surface of the metal and prevent the cathodic delamination of the coating, and limits the diffusion of corrosion products under the coating. There is no significant difference in the increase of the capacitor capacitance of the coating and the double layer capacitor capacitance, which shows the diffusion of water in352-8266 the coating, is the lowest and the passive film has limited the access of the corrosive electrolyte to the active sites on the surface of the steel substrate. Cathodic and anodic reactions have occurred in the presence of the passive film at the lower level and have resulted in lower corrosion products under the coating.

[0136] Table 6. Electrochemical parameters related to fitting of impedance curves of an exemplary scratched epoxy-silanized graphene oxide nanocomposite coating containing electrospun core-shell fibers with 15 wt% PVA shell solution with equivalent electrical circuits 1302 and 1304 during 16 days immersion in 3.5 wt% sodium chloride solution Sample Time RsCPEcn RcCPEdln Rct(d) (Ω.cm2) (Y0(Sn.Ω-1.cm-2)) (Ω.cm2) (Y0(Sn.Ω-1.cm-2)) (Ω.cm2)nanocomposite coating containing core-shell nanofibers electrospun at applied voltages of 11, 13 and 16 kV was investigated via electrochemical impedance spectroscopy curves (for the simplicity, only Nyquist curves are illustrated in FIGs. 25-27).

[0138] FIG. 25 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with an applied voltage of 11 kV (named as EPGSi-11kV-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 and 36 hours (diagram 2502), after 8 days (diagram 2504), after 12 days (diagram 2506), and up to 16 days (diagram 2508), consistent with one or more exemplary embodiments of the present disclosure. After 24 hours of immersion, two capacitive loops were created in the Nyquist curve, the larger loop at high frequencies is related to the formation of a passive barrier layer due to the release of the self-healing core, and the second loop at low frequencies is related to the electrochemical reactions of corrosion at the metal- coating interface. With further increase of immersion time, impedance value at low frequency had a decreasing trend. In fact, with the increase of the immersion time, more penetration of the corrosive solution into the coating and electrochemical corrosion reactions occurred at the interface between the metal and the coating. The decrease in the diameter of the rings352-8266 appearing in the Nyquist curve indicates a decrease in the resistance of the coating and charge transfer resistance, and as a result, the self-healing performance of the coating is lower. In this case, since the voltage of 11 kV was used in the electrospinning of core-shell fibers, the fiber with a larger diameter may be formed.

[0139] However, due to the lower power of the electric field, the deposition rate of the fibers was lower and the fibers had a more uneven distribution compared to the voltages of 13 and 16 kV. Therefore, the amount of self-healing material was loaded less and less self- healing occurred, and this is consistent with the decreasing rate of coating resistance and charge transfer resistance, which occurred more strongly than in other cases. The decrease in charge transfer resistance indicates the increase in the penetration of the corrosive solution and the performance of anodic and cathodic reactions in the active places on the surface of the metallic substrate and the decrease in the corrosion resistance of the coating.

[0140] FIG. 26 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with an applied voltage of 13 kV (named as EPGSi-13kV-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 2602), up to 36 hours (diagram 2604), and after 8, 12, and 16 days (diagram 2606), consistent with one or more exemplary embodiments of the present disclosure. After 24 hours of immersion, the impedance value at low frequency in this sample had a five-times decrease compared to the sample without scratches. But with the passage of 36 hours, the diameter of the semicircle of the capacitive loop in the Nyquist curve became larger and the capacitive behavior appeared in a larger range compared to the time of 24 hours.

[0141] All these cases indicate the ability of active repair for self-healing coatings after the initial damage. Self-healing materials prevented the penetration of the corrosive media into the coating and led to the improvement of the protective performance of the coating. With the further increase of the immersion time, the process of decreasing the impedance value was done at low frequencies. This behavior is in good agreement with the decreasing of the diameter of the Nyquist semicircle and the decreasing of the phase angle. However, in the EPGSi-13 kV sample, compared to the EPGSi-11 kV and EPGSi-16 kV, the magnitude of the impedance is greater in all immersion times and the rate of impedance decrease with time is less. In fact, in the EPGSi-13 kV sample, due to the higher deposition rate of core-shell fibers with more uniform distribution, it is possible to load more and better self-healing material352-8266 which has led to better self-healing and increased barrier properties as a result of the formation of a passive layer at the metal-coating interface. This film can improve the adhesion of the epoxy coating to the metallic substrate, prevent the cathodic delamination of the coating, and limit the penetration of corrosion products under the coating. There is no significant difference in the increase of the capacitor capacitance of the coating and the double layer capacitor capacitance over time. This indicates that the penetration of water in the coating is the lowest and the passive film has limited the access of the corrosive electrolyte to the active sites on the surface of the steel substrate.

[0142] FIG. 27 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with an applied voltage of 16 kV (named as EPGSi-16kV-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 and 36 hours (diagram 2702), up to 8 days (diagram 2704), up to 12 days (diagram 2706), and up to 16 days (diagram 2708), consistent with one or more exemplary embodiments of the present disclosure. With the increase of immersion time and after 36 hours, two capacitive loops appeared in low and high frequencies. The resistance of the coating, which is shown by the capacitor loop at high frequencies, increased compared to the 24 hours, which is caused by the formation of a passive barrier layer. In addition, the capacitive loop at low frequencies indicates an increase in charge transfer resistance, slowing down the anodic and cathodic electrochemical reactions at the interface. By increasing the immersion time, the diameter of the semicircle of the capacitance loops related to the coating and the charge transfer resistance decreased. The magnitude of the impedance at low frequency in all immersion times decreased by about two orders compared to the EPGSi-13 kV sample. In fact, as the voltage increases, the diameter of the fibers decreased. According to the morphology of the core-shell fibers, it has a non-uniform distribution and a lower deposition rate compared to the 13 kV voltage, which leads to decrease the amount of loading of self-healing material and the efficiency of self-healing are lower at different immersion times. In general, the EPGSi-13 kV sample has a better protective performance and corrosion resistance compared to 11 and 16 kV, which is in good agreement with the digital images of the surface of the scratched area after the impedance tests, and in the EPGSi-13 kV sample, rust and blisters and corrosion products have not been seen.

[0143] In a third set of tests, performance of self-healing property of an exemplary nanocomposite coating containing core-shell nanofibers electrospun at different core feeding352-8266 rates of 0.1, 0.2, and 0.3 mL.h-1was investigated via electrochemical impedance spectroscopy curves (for the simplicity, only Nyquist curves are illustrated in FIGs.28-30).

[0144] FIG. 28 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a core feeding rate of 0.1 mL.h-1(named as EPGSi-0.1-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 2802), up to 36 hours (diagram 2804), and up to 8, 12, and 16 days (diagram 2806), consistent with one or more exemplary embodiments of the present disclosure. In the EPGSi-0.1 sample, which is electrospun core-shell fibers with a feeding rate of 0.1 mL.h-1, according to the Nyquist curves, a sharp drop in impedance was observed at low frequencies compared to the same coating in the state without scratches. The impedance value at low frequency showed a decrease of about 5 times. After 36 hours of immersion, the impedance value at low frequency increased 2 times and the second Nyquist loop that appeared in 24 hours disappeared in 36 hours. These cases indicate the formation of a protective film in the scratch area as a result of the release of the PDMS polymer and the increase in the density of the cross-link of the coating, which makes the coating resistant to the penetration of the electrolyte into the coating. At 8 days of immersion, two capacitive loops appeared in the Nyquist curve, which indicates the penetration and reaching of the corrosive solution to the metal-coating interface. With the further increase of the immersion time, the decreasing trend of the impedance value at low frequency has continued. With the formation of scratches, the resistance of the coating and the charge transfer resistance decreased significantly, and the capacitor capacitance of the coating and the double layer capacitor capacitance increased significantly compared to the sample without scratches. In the EPGSi-0.1 sample, due to the lower feeding rate during the electrospinning of core-shell fibers and lower loading of self-healing materials, the protection performance of the coating was lower than the feeding rate of 0.2 and 0.3 mL.h-1.

[0145] FIG. 29 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a core feeding rate of 0.2 mL.h-1(named as EPGSi-0.2-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 2902), up to 36 hours (diagram 2904), and up to 8, 12, and 16 days (diagram 2906), consistent with one or more exemplary embodiments of the present disclosure. After 24 hours of immersion, the impedance value at low frequency in this sample had a five-times decrease compared to the sample without scratches. But, with the passage of352-8266 36 hours, the diameter of the semicircle of the capacitive loop in the Nyquist curve increased and the capacitive behavior has appeared in a larger range compared to the time of 24 hours. These data cases indicate the ability of active repair for self-healing coatings after initial damage. Self-healing materials prevented the penetration of the corrosive environment into the coating and have led to the improvement of the protective performance of the coating. In the EPGSi-0.2, compared to the EPGSi-0.1 and EPGSi-0.3, the magnitude of the impedance is higher at all immersion times and the rate of impedance decrease with time is lower. So that after 16 days of immersion, the impedance at low frequency of the scratched sample in the EPGSi-0.2 sample is equal to 1.39×108Ω.cm2, which is compared to the impedance value in the EPGSi-0.1 sample (2.45×105Ω.cm2) is three times greater. In fact, in the EPGSi-0.2 sample, due to the higher feeding rate and deposition of core-shell fibers with more uniform distribution, it is possible to load more and better self-healing material, which has led to better self-healing and increased barrier properties as a result of the formation of a passive layer at the metal-coating interface.

[0146] FIG. 30 shows Nyquist curves of an exemplary scratched epoxy-silanized graphene oxide coating containing core-shell fibers electrospun with a core feeding rate of 0.3 mL.h-1(named as EPGSi-0.3-scratched) at different immersion times in 3.5 wt% sodium chloride medium up to 24 hours (diagram 3002), up to 36 hours (diagram 3004), and up to 8, 12, and 16 days (diagram 3006), consistent with one or more exemplary embodiments of the present disclosure. In this case, by creating a scratch, the impedance value at low frequency decreased five times in magnitude. The diameter of Nyquist's semicircle and the range of capacitive behavior and phase angle reduced. After 36 hours of immersion, the diameter of the Nyquist semicircle increased, the range of capacitive behavior appeared in a larger frequency range, the phase angle increased, and the breakdown frequency moved to smaller frequencies.

[0147] In an exemplary embodiment, when the feeding rate increases, more material reaches the needle tip, and obviously, a larger volume of the solution may be pulled out from the needle tip which will lead to an increase in the diameter of the fibers. Nevertheless, when the feeding rate increases, the electric charges increase and cause a mutual increase in tension, which opposes the increase in diameter and volume. Therefore, at the feeding rate of 0.3 compared to 0.2 mL.h-1, more material has reached the coaxial needle and more fibers with a larger diameter are expected. But, since the electric charge has been constant, the352-8266 deposition rate is lower than the feeding rate of 0.2 mL.h-1, and the amount of self-healing material loading is lower than the feeding rate of 0.2 mL.h-1, and this causes the performance of self-healing is reduced.

[0148] EXAMPLE 6: The self-healing performance of the produced self-healing anticorrosive coatings at different electrospinning conditions via salt spray test

[0149] In this example similar to EXAMPLE 5, the protective and self-healing effect of exemplary produced coatings according to EXAMPLE 3 described herein above, a deep cut was made on surface of exemplary metallic substrate by a sharp surgical razor, 4 cm long and 2 mm wide, to an extent that it was deep to top of the metallic substrate. Then, salt spray test in accordance with ASTM B 117 standard was carried out on scratched coatings. In each salt spray test, a solution containing 5 wt% of Sodium chloride was sprayed using compressed air in a chamber where the samples were placed therein. The temperature and pressure of the salt spray was kept at 35 ± 2ºC and 0.83–1.24 bar. The samples were placed at an angle of 15–30 degrees to the vertical.

[0150] FIG. 31 shows digital camera images related to a salt spray test on an exemplary surface of an exemplary coating containing core-shell fibers at different applied voltages of 11, 13, and 16 kV of electrospinning exposed to 5± 1 wt% sodium chloride after 480 hours, consistent with one or more exemplary embodiments of the present disclosure. In the 11 kV sample after 48 hours, a small amount of rust signs is seen on the scratched area, but there are no traces of rust and corrosion products in the scratched area in the 13 and 16 kV samples. After 144 hours of salt spray test, the intensity of rust may be increased in samples 11 and 16 kV, and the first blisters may be appeared in these samples, but in sample 13 kV, there is no trace of the rusted area, blisters, and corrosion products. In the 16 kV sample, the penetration of the corrosive solution from the lower surface of the sample appeared inside. With the passage of 216 hours from the salt spray test, corrosion products and blisters, and rust areas in the scratch area have increased in samples 11 and 16 kV, while still in the 13 kV sample, no traces of corrosion and rust products and blisters was seen.

[0151] Furthermore, at 240 and 264 hours of salt spray test, there was no significant change in the surface of the scratched area compared to the previous times in terms of corrosion products. After 384 hours of the salt spray test, the amount of blistering and rusting increased for the 11 kV sample, and for the 16 kV, the extent of rusting in the scratched area increased. Up to 480 hours, there is minor changes in the surface of the scratched area, and other352-8266 surfaces of these samples may not be damaged, and in the 13 kV sample, no corrosion products.

[0152] FIG. 32 shows digital camera images related to an exemplary salt spray test on an exemplary surface of an exemplary coating containing core-shell fibers electrospun at core feeding rates of 0.1, 0.2 and 0.3 mL.h-1after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure. As it is shown, in the case where the feeding rate of 0.1 mL.h-1was used, after 48 hours of the salt spray test, the first signs of rust appeared in the sample, while in the samples with feeding rate of 0.2 and 0.3 mL.h-1, no symptoms were seen. Thereafter, after 72 hours of the salt spray test, no signs of corrosion such as laminating, rusting, and blistering were observed in samples with a feeding rate of 0.2 and 0.3 mL.h-1.But, in the sample with a feeding rate of 0.1 mL.h-1, the intensity of rusting in the scratched increased and diffusion of the corrosive solution started from the lower surface of the sample. The size of the rusted area in the scratched area of the sample with a feeding rate of 0.1 mL.h-1, increased by increasing the time of the salt spray test to 168 hours. But there was no change in the lower blistered area of the sample. The poor performance of the sample with a feeding rate of 0.1 mL.h-1is due to the lower amount of core material loaded in the core-shell fibers in the coating. By increasing the feeding rate to 0.2 mL.h-1, more material from the core was loaded into the core-shell fibers, and it is obvious that more repair and improvement in corrosion resistance may be expected. This is in accordance with the results of electrochemical studies of impedance spectra in scratched and non-scratched samples, as explained in EXAMPLEs 4 and 5, and scanning electron microscope studies of the morphology of the scratched area, as explained in EXAMPLE 3.

[0153] FIG. 33 shows digital camera images related to an exemplary salt spray test from an exemplary surface of an exemplary coating containing core-shell fibers electrospun in concentrations of 7, 10, and 15 wt% of PVA in shell solution and after 480 hours exposed to 5 ± 1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure. The first signs of rust appeared after 48 hours, while there were no signs for samples with 15 wt%. The first signs of blistering in the scratched area appeared for the sample with a concentration of 7 wt% of PVA after 144 hours of the salt fog test, and the intensity of rusting is greater than in the sample with a concentration of 10 wt%. After 168 hours, the initial blisters started to grow for the sample with a concentration of 7 wt%, while352-8266 for the sample with a concentration of 10 wt%, a few blisters were formed on the surface of the scratched area. The time of the salt spray test passages, blisters grow in the scratched area, and at 264 hours, blisters appeared in other areas of the sample with a concentration of 7 wt%, while in the sample with a concentration of 15 wt%, there were no blisters and corrosion products. No samples were seen in the scratched area and other areas. In addition, the intensity of corrosion products and rusted areas in the scratch area and its surroundings in the sample with 7 wt% concentration grew at a higher rate than the sample with 10 wt% concentration and reached its highest level after 384 hours. There was no significant difference after 408 to 480 hours. Investigation of the images of the core-shell fiber morphology showed that by increasing the shell polymer solution concentration, the diameter of the fibers and the loading rate of the self-healing core material increased. Therefore, there is a possibility of higher loading of repair material and the self-healing process, and this may be the reason for the fewer corrosion products on the surface of the scratched area of the 15% samples.

[0154] EXAMPLE 7: Investigation of morphology of the scratched area of the produced self-healing anticorrosive coatings at different electrospinning conditions via salt spray test

[0155] In this example, morphology of a scratch area of exemplary coating samples containing electrospun core-shell fibers produced at different conditions according to EXAMPLE 3 described herein above is investigated.

[0156] FIG. 34 shows FESEM images and EDAX analysis taken from surface morphology of an exemplary scratch area of exemplary produced coatings containing electrospun core- shell fibers in concentrations of 7 (FESEM image 3402 and EDAX analysis 3404), 10 (FESEM image 3406 and EDAX analysis 3408), and 15 wt% (FESEM image 3410 and EDAX analysis 3412) after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure. As it is observed, on the surface of the coating containing core-shell fibers with a concentration of 7 wt% shell, the scratched area may be healed to a small extent, and some corrosion products can be seen in the areas around the scratch (FESEM image 3402). By increasing the concentration of the polymer shell to 10 wt%, the scratch area was partially healed, and the edges of the scratch area on the left side do not show any traces of corrosion products and roughness (FESEM image 3406). In the sample containing core-shell fibers with a concentration of 15 wt% shell,352-8266 no traces of corrosion and corrosion products were observed on both sides of the edges of the scratched area, and the scratched area was completely healed (FESEM image 3410). Qualitative EDAX analysis taken from the surface of the scratched area of these samples shows the presence of more silicon element released from the PDMS core material in the scratched area with 15 wt% concentration.

[0157] According to FIG. 34, the number of elements in the scratched area of the coating samples containing core-shell fibers in the concentration of 7, 10, and 15% was summarized in EDAX analysis 3404, 3408, and 3412. It may be seen that with the increase in the concentration of the PVA polymer shell from 7 to 10 and 15 wt%, respectively, the weight percentage of oxygen and chlorine elements as active elements of the corrosive environment decreased, and the weight percentage of silicon and iron elements increased. It is the reason for improving the corrosion performance and self-healing of the coating.

[0158] As it has been obtained from investigation of the morphology of coaxial electrospun core-shell fibers in different shell concentrations, with the increase of shell concentration, the diameter of core-shell fibers is gotten bigger than before, and the possibility of loading self- healing core materials and repairing the scratched area increased with the time. It provides the release of PDMS material due to the dissolution of the PVA polymer material of the shell in contact with the aqueous solution. These results confirmed the electrochemical investigations of impedance spectroscopy and morphology of the scratch area after the salt spray test explained herein above in EXAMPLEs 5 and 6.

[0159] FIG. 35 shows FESEM images and EDAX analysis taken from surface morphology of an exemplary scratch area of exemplary produced coatings containing core-shell fibers electrospun at core feeding rates of 0.1 mL.h-1(FESEM image 3502 and EDAX analysis 3504), 0.2 mL.h-1(FESEM image 3506 and EDAX analysis 3508), and 0.3 mL.h-1(FESEM image 3510 and EDAX analysis 3512) after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure. At the feeding rate of 0.1 mL.h-1(FESEM image 3502), there is a little amount of corrosion products on the surface of the sample, and a few repairing has occurred inside the scratched area. By increasing the core feeding rate from 0.1 to 0.2 mL.h-1, the scratched area is free of any corrosion products and the scratched area is well repaired (FESEM image 3506).

[0160] Moreover, at the feeding rate of 0.3 mL.h-1, the amount of repair in the scratched area is lower than at the feeding rate of 0.2 mL.h-1, and some corrosion products may be seen352-8266 on the right side of the edge scratched area (FESEM image 3510). Qualitative elemental analysis of EDAX taken from the surface of the scratched area has shown that with increasing the feeding rate from 0.1 (EDAX analysis 3504) to 0.2 mL.h-1(EDAX analysis 3508), the amount of silicon and iron elements are more and the amount of oxygen and chlorine elements decreased. The weight percentage of silicon element at the feeding rate of 0.2 mL.h-1is the highest and the weight percentage of chlorine element is the lowest. This measurement indicates the release of the silicon element in the core of the core-shell fibers, loading in the composite coating, and preventing the corrosion process due to the penetration of corrosive solutions along the coating-metal interface. By increasing the feeding rate to 0.3 mL.h-1, the weight percentage of the chlorine element increased slightly compared to the feeding rate of 0.2 mL.h-1and the weight percentage of the iron element is lower, which indicates the formation of corrosion products.

[0161] FIG. 36 shows FESEM images and EDAX analysis taken from surface morphology of an exemplary scratch area of exemplary produced coatings containing core-shell fibers electrospun at applied voltages of 11 kV (FESEM image 3602 and EDAX analysis 3604), 13 kV (FESEM image 3606 and EDAX analysis 3608), and 16 kV (FESEM image 3610 and EDAX analysis 3612) after 480 hours exposed to 5±1 wt% sodium chloride, consistent with one or more exemplary embodiments of the present disclosure. In the case where core-shell fibers were electrospun at 11 kV voltage (FESEM image 3602), the scratched area was partially repaired and no significant corrosion products was seen at the edges of the scratched area. While in the sample with a voltage of 13 kV (FESEM image 3606), the scratched area was completely repaired and no corrosion or unevenness was seen on the sides of the edges of the scratched area.

[0162] Furthermore, by increasing the applied voltage to 16 kV, some corrosion products was seen on the left side of the scratched area and the scratched area was partially repaired (FESEM image 3610). Any change in the width of this narrow channel, caused by the swelling of the walls of the coating in the scratched area due to the absorption of water or the accumulation of corrosion products, may create a barrier against the passage of corrosive agents and change the corrosion resistance in a cross-sectional manner. Qualitative elemental analysis with EDAX of three nanocomposite coatings at the voltage of 13 kV (EDAX analysis 3608) as compared to 11 kV (EDAX analysis 3604) showed that the weight percent of silicon and iron elements is the highest and the weight percentage of oxygen and chlorine352-8266 elements is the lowest, which indicates the corrosion resistance and self-healing of these samples. In the sample with a voltage of 16 kV (EDAX analysis 3612), the weight percent of iron and silicon decreased in comparison to the voltage of 13 kV, which is consistent with the presence of more corrosion products and partial repairing of the scratched area in this case. As mentioned in EXAMPLEs 5 and 6 herein above, with increasing voltage, the diameter of the core-shell fibers decreased. The deposition rate of fibers and loading of the core material at 13 kV voltage is higher than 16 kV voltage, and the continuity of fibers and the distribution of fibers are more uniform and this is the reason for loading more core repair material and better self-healing performance of samples containing fibers synthesized at this voltage. Industrial Applicability

[0163] Herein, a coating with both anti-corrosive and self-healing properties is disclosed for using on metallic surfaces. An exemplary coating has a three-layered structure coated layer-by-layer on an exemplary metallic surface, which make it difficult for a corrosive substance to reach an exemplary metallic surface. An exemplary coating has a sandwich-like structure in which a layer of a plurality of core-shell nanofibers is compacted between two layers of epoxy-silanized graphene oxide nanocomposite. An exemplary layer of an exemplary plurality of core-shell nanofibers may include a self-healing agent preserved as a core material inside a hydrophilic shell material. An exemplary epoxy-silanized graphene oxide nanocomposite may provide two anti-corrosive layers at top and down of an exemplary layer of an exemplary plurality of core-shell nanofibers. However, even if a corrosive substance penetrates through an exemplary top layer of epoxy-silanized graphene oxide nanocomposite, an exemplary self-healing agent may be released and activated due to dissolution of an exemplary shell material into an exemplary corrosive substance. An exemplary epoxy-silanized graphene oxide nanocomposite may include graphene oxide nanosheets functionalized with GPTMS dispersed in epoxy matrix (GPTMS-GO-EP). An exemplary silane group of an exemplary silane-containing compound (i.e., GPTMS) may be attached to graphene oxide nanosheets; thereby, resulting in high and uniform dispersion of graphene oxide nanosheets in an exemplary epoxy matrix and an increase in inter-space interactions. Exemplary graphene oxide nanosheets may be added to an epoxy matrix to improve anti-corrosion performance of exemplary epoxy resins due to high specific surface area of graphene oxide nanosheets related to their sheet-shaped structure. Well-dispersed graphene oxide nanoparticles may reduce pores in an exemplary epoxy matrix, electrolyte352-8266 penetration towards an exemplary metallic surface, and water penetration coefficient which may be considered as major drawbacks of currently used epoxy resins as coatings for metallic surfaces. Furthermore, an exemplary coating may be fabricated through an exemplary cost- effective and non-complicated method using industrially available raw materials which may make it capable of easily and widely used in industry and other places.

[0164] While the foregoing has described what are considered to be the best mode and / or other examples, it is understood that various modifications may be made therein and that the subject matter disclosed herein may be implemented in various forms and examples, and that the teachings may be applied in numerous applications, only some of which have been described herein. It is intended by the following claims to claim any and all applications, modifications and variations that fall within the true scope of the present teachings.

[0165] Unless otherwise stated, all measurements, values, ratings, positions, magnitudes, sizes, and other specifications that are set forth in this specification, including in the claims that follow, are approximate, not exact. They are intended to have a reasonable range that is consistent with the functions to which they relate and with what is customary in the art to which they pertain.

[0166] The scope of protection is limited solely by the claims that now follow. That scope is intended and should be interpreted to be as broad as is consistent with the ordinary meaning of the language that is used in the claims when interpreted in light of this specification and the prosecution history that follows and to encompass all structural and functional equivalents. Notwithstanding, none of the claims are intended to embrace subject matter that fails to satisfy the requirement of Sections 101, 102, or 103 of the Patent Act, nor should they be interpreted in such a way. Any unintended embracement of such subject matter is hereby disclaimed.

[0167] Except as stated immediately above, nothing that has been stated or illustrated is intended or should be interpreted to cause a dedication of any component, step, feature, object, benefit, advantage, or equivalent to the public, regardless of whether it is or is not recited in the claims.

[0168] It will be understood that the terms and expressions used herein have the ordinary meaning as is accorded to such terms and expressions with respect to their corresponding respective areas of inquiry and study except where specific meanings have352-8266 otherwise been set forth herein. Relational terms such as first and second and the like may be used solely to distinguish one entity or action from another without necessarily requiring or implying any actual such relationship or order between such entities or actions. The terms “comprises,” “comprising,” or any other variation thereof, are intended to cover a non- exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements does not include only those elements but may include other elements not expressly listed or inherent to such process, method, article, or apparatus. An element proceeded by “a” or “an” does not, without further constraints, preclude the existence of additional identical elements in the process, method, article, or apparatus that comprises the element.

[0169] The Abstract of the Disclosure is provided to allow the reader to quickly ascertain the nature of the technical disclosure. It is submitted with the understanding that it will not be used to interpret or limit the scope or meaning of the claims. In addition, in the foregoing Detailed Description, it can be seen that various features are grouped together in various implementations. This is for purposes of streamlining the disclosure, and is not to be interpreted as reflecting an intention that the claimed implementations require more features than are expressly recited in each claim. Rather, as the following claims reflect, inventive subject matter lies in less than all features of a single disclosed implementation. Thus, the following claims are hereby incorporated into the Detailed Description, with each claim standing on its own as a separately claimed subject matter.

[0170] While various implementations have been described, the description is intended to be exemplary, rather than limiting and it will be apparent to those of ordinary skill in the art that many more implementations and implementations are possible that are within the scope of the implementations. Although many possible combinations of features are shown in the accompanying figures and discussed in this detailed description, many other combinations of the disclosed features are possible. Any feature of any implementation may be used in combination with or substituted for any other feature or element in any other implementation unless specifically restricted. Therefore, it will be understood that any of the features shown and / or discussed in the present disclosure may be implemented together in any suitable combination. Accordingly, the implementations are not to be restricted except in light of the attached claims and their equivalents. Also, various modifications and changes may be made within the scope of the attached claims.

Claims

352-8266 What is claimed is:

1. A self-healing anticorrosive coating for a metal surface, comprising: a first layer of epoxy-silanized graphene oxide nanocomposite, the epoxy- silanized graphene oxide nanocomposite comprising graphene oxide nanosheets functionalized with 3-glycidyloxypropyltrimethoxysilane (GPTMS) dispersed in an epoxy matrix (GPTMS-GO-EP), the first layer of epoxy-silanized graphene oxide nanocomposite configured to be deposited on the metal surface; a layer of electrospun core-shell nanofibers directly formed on the first layer of GPTMS-GO-EP, each respective electrospun core-shell nanofiber comprising: a core, comprising polydimethylsiloxane (PDMS); and a shell encapsulating the core, the shell comprising polyvinyl alcohol (PVA); and a second layer of the epoxy-silanized graphene oxide nanocomposite coated on the layer of electrospun core-shell nanofibers.

2. The self-healing anticorrosive coating of claim 1, wherein the graphene oxide nanosheets functionalized with GPTMS is present in the GPTMS-GO-EP with an amount of 0.2 wt% based on a total weight of the GPTMS-GO-EP.

3. The self-healing anticorrosive coating of claim 1, wherein the core-shell nanofibers are formed from a PDMS solution containing an amount of PDMS in a range of 30 wt% to 50 wt% and a PVA solution containing an amount of PVA in a range of 5 wt% to 20 wt%.

4. The self-healing anticorrosive coating of claim 1, wherein the epoxy matrix comprises an epoxy resin, the epoxy resin comprising a bisphenol A (BPA)-based epoxy resin.352-8266 5. The self-healing anticorrosive coating of claim 1, wherein the first layer of the epoxy- silanized graphene oxide nanocomposite has a thickness in a range of 30 µm to 40 µm.

6. The self-healing anticorrosive coating of claim 1, wherein the layer of electrospun core-shell nanofibers has a thickness in a range of 15 µm to 20 µm.

7. The self-healing anticorrosive coating of claim 1, wherein each nanofiber of the electrospun core-shell nanofibers has an average diameter in a range of 100 nm to 500 nm and each respective core has a thickness in a range of 80 nm to 200 nm.

8. The self-healing anticorrosive coating of claim 1, wherein the second layer of the epoxy-silanized graphene oxide nanocomposite has a thickness more than a thickness of the first layer of the epoxy-silanized graphene oxide nanocomposite, the thickness of the second layer of the epoxy-silanized graphene oxide nanocomposite being in a range of 60 µm to 100 µm.

9. A method for producing a self-healing anticorrosive coating on a metal surface, the method comprising: producing graphene oxide nanosheets functionalized with 3- glycidyloxypropyltrimethoxysilane (GPTMS) (GPTMS-GO) with a weight ratio of GPTMS to GPTMS-GO in a range of 0.1 wt% to 0.3 wt%; producing an epoxy-silanized graphene oxide nanocomposite by dispersing the formed GPTMS-GO in an epoxy matrix, the produced epoxy-silanized graphene oxide nanocomposite comprising a nanocomposite of GPTMS-GO dispersed in the epoxy matrix (GPTMS-GO-EP);352-8266 preparing the metal surface of a metallic substrate; depositing a first layer of the epoxy-silanized graphene oxide nanocomposite on the prepared metal surface; electrospinning a layer of core-shell nanofibers on the first layer of the epoxy- silanized graphene oxide nanocomposite; depositing a second layer of the epoxy-silanized graphene oxide nanocomposite on the electrospun layer of core-shell nanofibers; and curing and drying a three-layered formed coating comprising the first layer of the epoxy-silanized graphene oxide nanocomposite, the electrospun layer of core-shell nanofibers, and the second layer of the epoxy-silanized graphene oxide nanocomposite formed on the metal surface.

10. The method of claim 9, wherein producing the graphene oxide nanosheets functionalized with GPTMS comprises: forming a mixture by adding graphene oxide nanosheets to a container containing ethanol, deionized water, and GPTMS; agitating the mixture by stirring the mixture for a time period in a range of 15 minutes to 1 hour; adjusting a pH value of the mixture within a range of 4 to 5 by adding a first base to the mixture while stirring the mixture; stirring the mixture for a time period in a range of 20 hours to 25 hours; adjusting a pH value of the mixture within a range of 8.5 to 9.5 by adding a second base to the mixture while stirring the mixture; stirring the mixture at a constant temperature in a range of 65 ºC to 75 ºC for a time period in a range of 1 hour to 3 hours;352-8266 removing unreacted ethanol, deionized water, and GPTMS from the mixture by centrifuging the mixture for a time period in a range of 3 minutes to 10 minutes at a centrifugation speed in a range of 3000 rpm to 5000 rpm, centrifuging the mixture comprising: dividing the mixture into a clear phase comprising the unreacted ethanol, deionized water, and GPTMS and a precipitation comprising the graphene oxide nanosheets functionalized with GPTMS; and separating the precipitation from the clear phase; removing an excess amount of unreacted GPTMS adsorbed on graphene oxide nanosheets by washing the precipitation using a mixture of ethanol-deionized water with a volume ratio of ethanol:deionized water equal to 3:1; and removing residual deionized water from the precipitation, comprising: washing the precipitation with diethyl ether; and maintaining the precipitation in toluene.

11. The method of claim 9, wherein producing the epoxy-silanized graphene oxide nanocomposite comprises: forming a mixture of the GPTMS-GO in toluene, comprising: adding the GPTMS-GO to a container containing toluene; and stirring the GPTMS-GO and the toluene for a time period in a range of 5 minute to 20 minutes at a temperature in a range of 0 ºC to 4 ºC using an ultrasonic probe; and dispersing the GPTMS-GO in an epoxy resin matrix, comprising: adding an epoxy resin to the mixture of the GPTMS-GO in toluene;352-8266 stirring the mixture of the GPTMS-GO in toluene with the epoxy resin at a stirring speed in a range of 500 rpm to 1500 rpm for a time period in a range of 20 hours and 30 hours using a mechanical stirrer; sonicating the mixture of the GPTMS-GO in toluene with the epoxy resin for a time period in a range of 5 minute to 20 minutes using an ultrasonic probe; adding a hardener with a weight ratio in a range of 1.3:1 (epoxy resin:hardener) to the mixture of the GPTMS-GO in toluene with the epoxy resin; and stirring the mixture of the GPTMS-GO in toluene with the epoxy resin and the added hardener for a time period in a range of 5 minute to 20 minutes using a mechanical stirrer.

12. The method of claim 9, wherein preparing the metal surface of the metallic substrate comprises: grinding the metal surface using a silicon carbide (SiC) paper; washing and degreasing the ground metal surface with at least one of acetone, ethanol, distilled water, and combinations thereof; drying the washed metal surface; and preventing oxidation and / or rusting of the metal surface by maintaining the metallic substrate in a desiccator and vacuum environment before depositing the first layer of the epoxy-silanized graphene oxide nanocomposite thereon.

13. The method of claim 9, wherein depositing the first layer of the epoxy-silanized graphene oxide nanocomposite on the prepared metal surface comprises forming a layer with352-8266 a thickness in a range of 30 µm to 40 µm on the prepared metal surface by spraying the epoxy-silanized graphene oxide nanocomposite on the prepared metal surface.

14. The method of claim 9, wherein electrospinning the layer of core-shell nanofibers on the first layer of the epoxy-silanized graphene oxide nanocomposite comprises coaxial electrospinning of two polymers on the first layer of the epoxy-silanized graphene oxide nanocomposite while the first layer of the epoxy-silanized graphene oxide nanocomposite being wet, the coaxial electrospinning of two polymers comprising: electrospinning a first polymer through an inner nozzle of a coaxial pair of nozzles on the first layer of the epoxy-silanized graphene oxide nanocomposite, the first polymer comprising a self-healing material; and electrospinning a second polymer through an outer nozzle of a coaxial pair of nozzles on the first layer of the epoxy-silanized graphene oxide nanocomposite, the second polymer comprising a hydrophilic polymer, wherein electrospinning the first polymer and the second polymer are done simultaneously.

15. The method of claim 14, wherein electrospinning the first polymer comprises electrospinning a solution of polydimethylsiloxane (PDMS) with a PDMS concentration in a range of 30 wt% to 50 wt% at a feeding rate in a range of 0.05 mL.h-1to 0.5 mL.h-1.

16. The method of claim 14, wherein electrospinning the second polymer comprises electrospinning a solution of polyvinyl alcohol (PVA) with a PVA concentration in a range of 5 wt% to 20 wt% at a feeding rate in a range of 0.5 mL.h-1to 2 mL.h-1.352-8266 17. The method of claim 14, wherein electrospinning the layer of core-shell nanofibers on the first layer of the epoxy-silanized graphene oxide nanocomposite is done at a voltage in a range of 10 kV to 20 kV.

18. The method of claim 14, wherein electrospinning the layer of core-shell nanofibers on the first layer of the epoxy-silanized graphene oxide nanocomposite comprises forming a layer of electrospun core-shell nanofibers with a thickness in a range of 15 µm to 20 µm on the first layer of the epoxy-silanized graphene oxide nanocomposite.

19. The method of claim 9, wherein depositing the second layer of the epoxy-silanized graphene oxide nanocomposite on the electrospun layer of core-shell nanofibers comprises forming a layer with a thickness in a range of 60 µm to 100 µm on the prepared metal surface by spraying the epoxy-silanized graphene oxide nanocomposite on the electrospun layer of core-shell nanofibers.

20. The method of claim 9, wherein curing and drying the three-layered formed coating comprises: maintaining the three-layered formed coating at ambient temperature in a range of 20 ºC to 30 ºC for a time period in a range of 20 hours to 60 hours; and baking the three-layered formed coating at a temperature in a range of 55 ºC to 65 ºC for a time period in a range of 20 hours to 30 hours.

Citation Information

Cited By

  • Epoxy resin composite material based on flexible chain segments and rigid fiber particles and preparation method

    CN119775723A

  • Paint with high durability and preparation method thereof

    CN121203538A

  • Anti-fingerprint ceramic, manufacturing method of anti-fingerprint ceramic, switch panel and manufacturing method of switch panel

    CN121362043A

  • Water-based protective coating for wheel shaft surface and preparation method of water-based protective coating

    CN122168139A