Positive electrode material and battery using the same

By optimizing the volume ratio of positive electrode active material to solid electrolyte material in the positive electrode, the battery achieves improved discharge capacity and reduced internal resistance.

JP7565494B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020090435
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-04
Filing Date
2020-05-25
Publication Date
2024-10-11
Estimated Expiration
2040-05-25

AI Technical Summary

Technical Problem

Existing batteries do not achieve optimal discharge capacity due to improper volume ratios of positive electrode active material and solid electrolyte material, leading to increased internal resistance and reduced ionic conductivity.

Method used

The positive electrode material comprises a positive electrode active material and a first solid electrolyte material, with a volume ratio of 0.55 to 0.85, enhancing electronic and ionic conductivity by adjusting the volume ratio to improve contact between materials.

Benefits of technology

This configuration results in a battery with higher discharge capacity and reduced internal resistance, achieved by optimizing the volume ratio of positive electrode active material to solid electrolyte material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565494000002
    Figure 0007565494000002
  • Figure 0007565494000003
    Figure 0007565494000003
  • Figure 0007565494000001
    Figure 0007565494000001
Patent Text Reader

Abstract

To provide a battery having a high discharge capacity.SOLUTION: A positive electrode material contains a positive electrode active material and a first solid electrolyte material. The first solid electrolyte material is expressed by a following chemical formula (1): LiαMβXγ, and in here, each of α, β, and γ is a value larger than 0. M is at least one kind of elements formed by a group of a metal element other than lithium and a metalloid element. X is at least one kind of elements selected from a group of fluorine, chlorine, bromine, and iodine. A ratio of a volume of the positive electrode active material for a total of the volumes of the volume of the positive electrode active material and the volume of the solid electrolyte material is 0.55 or more and 0.85 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a positive electrode material and a battery using the same. [Background technology]

[0002] Patent Document 1 discloses an all-solid-state battery using a halide solid electrolyte. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 025582 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide a battery having a high discharge capacity. [Means for solving the problem]

[0005] The positive electrode material according to the present disclosure contains a positive electrode active material and a first solid electrolyte material, and the first solid electrolyte material is represented by the following chemical formula (1): Li α M β X γ (1) Here, α, β, and γ are all values ​​greater than 0, M is at least one element selected from the group consisting of metal elements and semi-metal elements other than lithium, X is at least one element selected from the group consisting of fluorine, chlorine, bromine, and iodine, and the ratio of the volume of the positive electrode active material to the sum of the volume of the positive electrode active material and the volume of the solid electrolyte material is 0.55 or more and 0.85 or less. Effect of the Invention

[0006] The present disclosure provides a battery having a high discharge capacity. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a graph showing the discharge capacity versus the volume ratio of the active material in the positive electrode of secondary batteries according to Examples 1 to 11 and Comparative Examples 1 and 2. [Diagram 2] FIG. 2 shows a cross-sectional view of a battery 1000 according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0009] (First embodiment) The positive electrode material according to the first embodiment contains a positive electrode active material and a first solid electrolyte material.

[0010] The first solid electrolyte material is a material represented by the following chemical formula (1). Li α M β X γ (1) Here, α, β, and γ are all greater than 0. M is at least one element selected from the group consisting of metal elements and metalloid elements other than lithium. X is at least one element selected from the group consisting of fluorine, chlorine, bromine, and iodine.

[0011] The ratio of the volume of the positive electrode active material to the total volume of the positive electrode active material and the first solid electrolyte material is 0.55 or more and 0.85 or less.

[0012] The positive electrode material according to the first embodiment can improve the discharge capacity of a battery.

[0013] Patent Document 1 discloses a battery using a halide solid electrolyte. However, the document does not mention the volume ratio of the halide solid electrolyte and the positive electrode active material in the positive electrode. In general, when the volume ratio of the active material contained in the positive electrode increases, the active materials are more likely to contact each other, and the electronic conductivity is improved. This reduces the internal resistance of the battery and improves the discharge capacity of the battery. Therefore, it is expected that the discharge capacity of the battery will also improve when the volume ratio of the active material in the positive electrode increases.

[0014] As a result of studies by the present inventors, it has been found that by adjusting the volume ratio of the positive electrode active material and the first solid electrolyte material (i.e., an example of a halide solid electrolyte) in the positive electrode as described above, the internal resistance of the battery is reduced and the discharge capacity of the battery is improved.

[0015] In the positive electrode, if the ratio of the volume of the positive electrode active material to the total volume of the positive electrode active material and the first solid electrolyte material is less than 0.55, the battery will not have a sufficient discharge capacity.

[0016] Since the halide solid electrolyte has high adhesion to the positive electrode active material, the surface of the positive electrode active material is easily covered with the first solid electrolyte material, which has very low electronic conductivity, which prevents contact between the positive electrode active materials and increases the internal resistance of the battery.

[0017] In the positive electrode, when the ratio of the volume of the positive electrode active material to the total volume of the positive electrode active material and the first solid electrolyte material exceeds 0.85, the battery does not have a sufficient discharge capacity.

[0018] Since the first solid electrolyte material is hard and difficult to deform, the contact area between the first solid electrolyte material and the positive electrode active material may be small. Furthermore, the volume ratio of the first solid electrolyte material in the positive electrode is small, so the ion conductivity is low. It is considered that the internal resistance of the battery increases because the decrease in ion conductivity due to the increase in the positive electrode active material is more noticeable than the increase in electronic conductivity. The above-mentioned deformation means elastic deformation or plastic deformation.

[0019] Examples of solid electrolyte materials include halide solid electrolytes such as the first solid electrolyte material, sulfide solid electrolytes, and oxide solid electrolytes. The softness of the solid electrolyte material and its adhesion to the positive electrode active material vary depending on the material.

[0020] The sulfide solid electrolyte and the oxide solid electrolyte have a lower adhesion to the positive electrode active material than the halide solid electrolyte, and therefore are less likely to prevent contact between the positive electrode active materials. In addition, the sulfide solid electrolyte is softer than the halide solid electrolyte. This ensures a sufficient contact area between the sulfide solid electrolyte and the positive electrode active material, and between the sulfide solid electrolytes themselves, and therefore the ion conductivity is less likely to decrease.

[0021] When the positive electrode contains a halide solid electrolyte, it is believed that by adjusting the volume ratio of the positive electrode active material and the halide solid electrolyte as described above, the contact area between the positive electrode active materials, the contact area between the halide solid electrolytes, and the contact area between the positive electrode active material and the halide solid electrolyte are all sufficiently ensured.

[0022] In order to further increase the discharge capacity of the battery, in the positive electrode material, the ratio of the volume Vpa of the positive electrode active material to the sum of the volume Vpa of the positive electrode active material and the volume Vpe of the first solid electrolyte material may be 0.60 or more and 0.72 or less, and preferably 0.65 or more and 0.72 or less. That is, 0.60≦Vpa / (Vpa+Vpe)≦0.72 or 0.65≦Vpa / (Vpa+Vpe)≦0.72 may be satisfied.

[0023] In this disclosure, "metalloid elements" means B, Si, Ge, As, Sb, and Te.

[0024] In the present disclosure, a "metal element" is (i) All elements in groups 1 to 12 of the periodic table (except hydrogen); and (ii) All elements in groups 13 to 16 (except B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se) means.

[0025] In order to improve the ionic conductivity of the first solid electrolyte material, M in chemical formula (1) may contain yttrium (i.e., Y). That is, the first solid electrolyte material may contain Y as a metal element. The improvement in ionic conductivity reduces the internal resistance of the battery, and can improve the discharge capacity of the battery.

[0026] The first solid electrolyte material containing Y is, for example, Li a Me b Y c X6, where a+mb+3c=6 and c>0 are satisfied. Me is at least one element selected from the group consisting of metal elements and metalloid elements other than Li and Y. m represents the valence of Me.

[0027] Me may be at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.

[0028] In order to improve the ionic conductivity of the first solid electrolyte material, M in chemical formula (1) may contain zirconium (i.e., Zr). That is, the first solid electrolyte material may contain Zr as a metal element. The improvement in ionic conductivity reduces the internal resistance of the battery, and the discharge capacity of the battery can be improved.

[0029] The first solid electrolyte material containing Zr is, for example, Li p Me' q Zr rIt may be a compound represented by the chemical formula of X6. Here, p + m’q + 4r = 6 and c > 0 are satisfied. Me’ is at least one element selected from the group consisting of metal elements and metalloid elements other than Li, Y, and Zr. m’ represents the valence of Me’.

[0030] Me’ may be at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Hf, Ti, Sn, Ta, and Nb.

[0031] In order to increase the ionic conductivity of the first solid electrolyte material, in Chemical Formula (1), 2.5 ≦ α ≦ 3, β = 1, and γ = 6 may be satisfied. Due to the improvement of the ionic conductivity, the battery has a high discharge capacity.

[0032] In order to enhance the potential stability of the first solid electrolyte material and the discharge capacity of the battery, in Chemical Formula (1), X may contain chlorine (i.e., Cl).

[0033] In order to increase the ionic conductivity of the first solid electrolyte material, in Chemical Formula (1), X may contain bromine (i.e., Br).

[0034] In order to increase the ionic conductivity of the first solid electrolyte material, in Chemical Formula (1), X may contain iodine (i.e., I).

[0035] The first solid electrolyte material may be a material represented by the following chemical formula (A1). Li 6-3d Y d X6···(A1) Here, X is two or more elements selected from the group consisting of F, Cl, Br, and I. Further, 0 < d < 2 is satisfied.

[0036] The material represented by Formula (A1) has a high ionic conductivity. Thereby, the discharge capacity of the battery can be further improved.

[0037] The first solid electrolyte material may be a material represented by the following chemical formula (A2): Li 3-3δ Y 1+δ Cl6···(A2) Here, 0<δ≦0.15 is satisfied.

[0038] The material represented by formula (A2) has high ionic conductivity, which can improve the discharge capacity of the battery.

[0039] The first solid electrolyte material may be a material represented by the following chemical formula (A3): Li 3-3δ Y 1+δ Br6···(A3) Here, 0<δ≦0.25 is satisfied.

[0040] The material represented by formula (A3) has high ionic conductivity, which can improve the discharge capacity of the battery.

[0041] The first solid electrolyte material may be a material represented by the following chemical formula (A4): Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y (A4) Here, Me is at least one element selected from the group consisting of Mg, Ca, Sr, Ba, and Zn. -1<δ<2, 0 <a<3、 0<(3-3δ+a), 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6, is satisfied.

[0042] The material represented by formula (A4) has high ionic conductivity, which can improve the discharge capacity of the battery.

[0043] The first solid electrolyte material may be a material represented by the following chemical formula (A5): Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y (A5) Here, Me is at least one element selected from the group consisting of Al, Sc, Ga, and Bi. -1<δ<1, 0 <a<2、 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6, is satisfied.

[0044] The material represented by formula (A5) has high ionic conductivity, which can improve the discharge capacity of the battery.

[0045] The first solid electrolyte material may be a material represented by the following chemical formula (A6): Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y (A6) Here, Me is at least one element selected from the group consisting of Zr, Hf, and Ti. -1<δ<1, 0 <a<1.5、 0<(3-3δ-a), 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6, is satisfied.

[0046] The material represented by formula (A6) has high ionic conductivity, which can improve the discharge capacity of the battery.

[0047] The first solid electrolyte material may be a material represented by the following chemical formula (A7): Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Br x I y (A7) Here, Me is at least one element selected from the group consisting of Ta and Nb. -1<δ<1, 0 <a<1.2、 0<(3-3δ-2a), 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6, is satisfied.

[0048] The material represented by formula (A7) has high ionic conductivity, which can improve the discharge capacity of the battery.

[0049] As the first solid electrolyte material, for example, Li3YX6, Li2MgX4, Li2FeX4, Li(Al, Ga, In)X4, or Li3(Al, Ga, In)X6 may be used, where "(Al, Ga, In)" means "at least one element selected from the group consisting of Al, Ga, and In."

[0050] The positive electrode active material is a material capable of absorbing and releasing metal ions (for example, lithium ions).

[0051] Examples of the positive electrode active material include lithium-containing transition metal oxides (e.g., Li(NiCoAl)O2, Li(NiCoMn)O2, or LiCoO2), transition metal fluorides, polyanions, fluoride polyanion materials, transition metal sulfides, transition metal oxysulfides, or transition metal oxynitrides. When a lithium-containing transition metal oxide is used as the positive electrode active material, the manufacturing cost can be reduced and the average discharge voltage of the battery can be increased.

[0052] To increase the discharge capacity and energy density of the battery, the positive electrode active material may be lithium nickel-cobalt-manganese oxide, which may be Li(NiCoMn)O2.

[0053] To increase the discharge capacity and energy density of the battery, the positive electrode active material may be lithium nickel-cobalt-aluminum oxide, which may be Li(NiCoAl)O2.

[0054] In order to improve the charge / discharge efficiency of the battery, at least a portion of the surface of the positive electrode active material may be coated with a coating material.

[0055] The coating material may be a material with low electronic conductivity, such as an oxide material or an oxide solid electrolyte material.

[0056] Examples of oxide materials are SiO2, Al2O3, TiO2, B2O3, Nb2O5, WO3, or ZrO2. Examples of oxide solid electrolyte materials are Li-Nb-O compounds such as LiNbO3, Li-BO compounds such as LiBO2 or Li3BO3, Li-Al-O compounds such as LiAlO2, Li-Si-O compounds such as Li4SiO4, Li-SO compounds such as Li2SO4, Li4Ti5O 12Li-Ti-O compounds such as Li2ZrO3, Li-Zr-O compounds such as Li2MoO3, Li-VO compounds such as LiV2O5, or Li-WO compounds such as Li2WO4.

[0057] From the viewpoint of ion conductivity and potential stability, the coating material may be an oxide solid electrolyte. By using an oxide solid electrolyte as the coating material, the charge / discharge efficiency of the battery can be further improved.

[0058] The oxide solid electrolyte material used for the coating material may be lithium niobate (LiNbO3), which has high ionic conductivity and high potential stability.

[0059] When the surface of the positive electrode active material is coated with a coating material, the positive electrode active material and the first solid electrolyte material are separated by the coating material and do not contact each other. The coating layer containing the coating material may have a thickness of 1 nm or more and 100 nm or less. When the coating layer has a thickness of 1 nm or more, contact between the positive electrode active material and the first solid electrolyte material is suppressed, and side reactions of the first solid electrolyte material can be suppressed. Therefore, the charge and discharge efficiency of the battery can be improved. When the coating layer has a thickness of 100 nm or less, the internal resistance of the battery can be sufficiently small. Therefore, the discharge capacity of the battery can be increased.

[0060] In order to increase the output of the battery, a part of the surface of the positive electrode active material may be coated. By contacting each other with the positive electrode active material through the part not having a coating layer, the electronic conductivity between the positive electrode active materials is improved.

[0061] In order to improve the charge / discharge efficiency of the battery, the entire surface of the positive electrode active material may be covered with a coating material. By suppressing contact between the positive electrode active material and the first solid electrolyte material, side reactions of the first solid electrolyte material can be suppressed.

[0062] The shape of the first solid electrolyte material is not limited. Examples of the shape include a needle shape, a sphere shape, and an oval sphere shape. The shape of the first solid electrolyte material may be a particle shape.

[0063] When the first solid electrolyte material is particulate (e.g., spherical), the first solid electrolyte particles may have a median diameter of 100 μm or less. Desirably, the first solid electrolyte particles may have a median diameter of 10 μm or less. This allows the positive electrode active material and the first solid electrolyte particles to be well dispersed in the positive electrode material. This can improve the charge / discharge characteristics of the battery.

[0064] The median diameter of the first solid electrolyte particles may be smaller than the median diameter of the positive electrode active material. This allows the first solid electrolyte particles and the positive electrode active material to be better dispersed in the positive electrode material. As a result, the charge / discharge characteristics of the battery can be improved.

[0065] The positive electrode active material may have a median diameter of 0.1 μm or more and 100 μm or less. When the positive electrode active material has a median diameter of 0.1 μm or more, the positive electrode active material and the first solid electrolyte particles can be well dispersed in the positive electrode material. This can improve the charge and discharge characteristics of the battery. When the positive electrode active material has a median diameter of 100 μm or less, the diffusion speed of lithium in the positive electrode active material is improved. This can allow the battery to operate at high power.

[0066] [Method for producing the first solid electrolyte material] The first solid electrolyte material according to the first embodiment can be produced, for example, by the following method.

[0067] The raw material powder of the halide is prepared taking into consideration the composition ratio of the product. For example, to produce Li3YCl6, LiCl and YCl3 are prepared in a molar ratio of 3:1.

[0068] The selection of the raw material powder type determines the elements M, Me, Me', and X in the above chemical formula. The values ​​of α, β, γ, a, b, c, and d are determined by adjusting the raw material powder, the compounding ratio, and the synthesis process.

[0069] The raw powders are mixed to obtain a mixed powder. The mixed powders are reacted with each other mechanochemically (i.e., by the method of mechanochemical milling) in a mixing device such as a planetary ball mill to obtain a reactant. The reactant may be fired in a vacuum or in an inert atmosphere. Alternatively, the mixed powder may be sintered in a vacuum or in an inert atmosphere to obtain a reactant.

[0070] By these methods, the first solid electrolyte material is obtained.

[0071] Second embodiment The second embodiment will be described below. Descriptions that overlap with the first embodiment will be omitted as appropriate.

[0072] The battery according to the second embodiment includes a positive electrode, a negative electrode, and an electrolyte layer. The positive electrode contains the positive electrode material according to the first embodiment. The electrolyte layer is disposed between the positive electrode and the negative electrode. The electrolyte layer contains a second solid electrolyte material. The battery according to the second embodiment has a high discharge capacity.

[0073] 2 shows a cross-sectional view of a battery 1000 according to a second embodiment. The battery 1000 includes a positive electrode 101, an electrolyte layer 102, and a negative electrode 103. The positive electrode 101 includes first solid electrolyte particles 110 and positive electrode active material particles 111. The electrolyte layer 102 is disposed between the positive electrode 101 and the negative electrode 103. The electrolyte layer 102 contains a second solid electrolyte material.

[0074] From the viewpoint of the energy density and output of the battery, the positive electrode 101 may have a thickness of 10 μm or more and 500 μm or less.

[0075] To enhance the discharge capacity of the battery, the second solid electrolyte material may be a halide solid electrolyte.

[0076] The halide solid electrolyte may be the compound exemplified as the first solid electrolyte material in the first embodiment. The second solid electrolyte material may be the same material as the first solid electrolyte material, or may be a material different from the first solid electrolyte material.

[0077] The second solid electrolyte material may be a sulfide solid electrolyte. By using a sulfide solid electrolyte with excellent reduction stability, a low potential negative electrode material can be used. This can improve the energy density of the battery.

[0078] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4, or Li 10 GeP2S 12 In addition, LiX, Li2O, MO, or Li p MO q may be added. Here, M is at least one element selected from the group consisting of P, Si, Ge, B, Al, Ga, In, Fe, and Zn. p and q are both natural numbers. X is at least one element selected from the group consisting of F, Cl, Br, and I.

[0079] The second solid electrolyte material may be an oxide solid electrolyte.

[0080] Examples of oxide solid electrolytes include: (i) NASICON-type solid electrolytes such as LiTi2(PO4)3 or other element-substituted solid electrolytes quality, (ii) (LaLi)TiO3-based perovskite solid electrolytes, (iii) Li 14 ZnGeO 16 LISICON-type solid electrolytes such as Li4SiO4, LiGeO4 or elemental substitutes thereof; (iv) Li7La3Zr2O 12Or other element-substituted garnet-type solid electrolytes , (v) Li3PO4 or its N-substituted derivatives, or (vi) Glasses or glass ceramics containing Li-BO compounds such as LiBO2 or Li3BO3 with the addition of Li2SO4 or Li2CO3 It is.

[0081] The second solid electrolyte material may be a polymer solid electrolyte.

[0082] Examples of the polymer solid electrolyte include a polymer compound and a lithium salt compound. The polymer compound may have an ethylene oxide structure. The polymer solid electrolyte having an ethylene oxide structure can contain a large amount of lithium salt, and therefore can further improve the ion conductivity.

[0083] Examples of the lithium salt are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. A mixture of two or more lithium salts selected from these may be used.

[0084] The second solid electrolyte material may be a complex hydride solid electrolyte.

[0085] Examples of complex hydride solid electrolytes are LiBH4-LiI or LiBH4-P2S5.

[0086] The electrolyte layer 102 may be made of only one of the materials exemplified as the second solid electrolyte material, or may be made of two or more of the materials. For example, the electrolyte layer 102 may include a halide solid electrolyte material and a sulfide solid electrolyte material.

[0087] When the electrolyte layer 102 is made of two or more materials, the materials may be uniformly dispersed, or multiple layers made of a single material may be stacked in the stacking direction of the battery.

[0088] From the viewpoints of suppressing short circuits between the positive electrode 101 and the negative electrode 103 and of the battery output, the electrolyte layer 102 may have a thickness of 1 μm or more and 300 μm or less.

[0089] The negative electrode 103 includes a material capable of absorbing and releasing metal ions (e.g., lithium ions). An example of such a material is a negative electrode active material.

[0090] Examples of the negative electrode active material are metal materials, carbon materials, oxides, nitrides, tin compounds, or silicon compounds. The metal material may be a single metal or an alloy. Examples of the metal material are lithium metal or lithium alloys. Examples of the carbon material are natural graphite, coke, partially graphitized carbon, carbon fiber, spherical carbon, artificial graphite, or amorphous carbon. From the viewpoint of capacity density, silicon (i.e., Si), tin (i.e., Sn), silicon compounds, or tin compounds may be used as the negative electrode active material.

[0091] The negative electrode 103 may contain a solid electrolyte material. This improves the lithium ion conductivity in the negative electrode 103, and the battery may operate at high power. The solid electrolyte material may be any of the materials exemplified as the second solid electrolyte material.

[0092] The negative electrode active material may have a median diameter of 0.1 μm or more and 100 μm or less. When the negative electrode active material has a median diameter of 0.1 μm or more, the negative electrode active material and the solid electrolyte material can be well dispersed in the negative electrode 103. This improves the charge / discharge characteristics of the battery. When the negative electrode active material has a median diameter of 100 μm or less, the diffusion speed of lithium in the negative electrode active material improves. This allows the battery to operate at high power.

[0093] The negative electrode active material may have a larger median diameter than the solid electrolyte material, which allows the negative electrode active material and the solid electrolyte material to be dispersed well.

[0094] From the viewpoint of the energy density and output of the battery, in the negative electrode 103, the ratio of the volume of the negative electrode active material to the total volume of the negative electrode active material and the solid electrolyte material may be 0.30 or more and 0.95 or less.

[0095] From the viewpoint of the energy density and output of the battery, the negative electrode 103 may have a thickness of 10 μm or more and 500 μm or less.

[0096] At least one selected from the group consisting of the positive electrode 101, the electrolyte layer 102, and the negative electrode 103 may contain a binder for the purpose of improving adhesion between particles.

[0097] Examples of binders are polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylic acid methyl ester, polyacrylic acid ethyl ester, polyacrylic acid hexyl ester, polymethacrylic acid, polymethacrylic acid methyl ester, polymethacrylic acid ethyl ester, polymethacrylic acid hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene butadiene rubber, or carboxymethylcellulose. Copolymers may also be used as binders. Examples of such binders are copolymers of two or more materials selected from the group consisting of tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene.

[0098] A mixture of two or more of the above materials may be used as the binder.

[0099] At least one selected from the positive electrode 101 and the negative electrode 103 may contain a conductive assistant for the purpose of improving electronic conductivity.

[0100] Examples of the conductive additive include: (i) Graphite, either natural or synthetic; (ii) carbon black, such as acetylene black or ketjen black; (iii) conductive fibers, such as carbon or metal fibers; (iv) fluorocarbons, (v) metal powders such as aluminum; (vi) conductive whiskers such as zinc oxide or potassium titanate; (vii) a conductive metal oxide, such as titanium dioxide; or (viii) A conductive polymer compound such as polyaniline, polypyrrole, or polythiophene. For cost reduction, the conductive assistant of (i) or (ii) above may be used.

[0101] Examples of the shape of the battery according to the second embodiment are a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminate type.

[0102] (Example) The present disclosure will now be explained in more detail with reference to examples.

[0103] Example 1 [Preparation of the first solid electrolyte material] In an argon atmosphere having a dew point of -60°C or less (hereinafter referred to as "dry argon atmosphere"), LiBr, LiCl, YCl3, and YBr3 were prepared as raw material powders in a molar ratio of LiBr:LiCl:YCl3:YBr3 = 1:5:1:1. The mixture was treated to react mechanochemically at 600 rpm for 25 hours using a planetary ball mill (Fritsch, P-7 type). In this manner, a powder of the first solid electrolyte material according to Example 1 was obtained. The first solid electrolyte material according to Example 1 had a composition represented by Li3YBr2Cl4.

[0104] [Preparation of positive electrode material] In a dry argon atmosphere, a powder of a positive electrode active material Li(NiCoMn)O2 (hereinafter referred to as "NCM") and a powder of a first solid electrolyte material according to Example 1 were prepared in a volume ratio of 85:15. These materials were mixed in an agate mortar. In this manner, a positive electrode material according to Example 1 was obtained.

[0105] Example 2 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 1 were prepared in a volume ratio of 80:20. Except for this, the positive electrode material according to Example 2 was obtained in the same manner as in Example 1.

[0106] Example 3 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 1 were prepared in a volume ratio of 72:28. Except for this, the positive electrode material according to Example 3 was obtained in the same manner as in Example 1.

[0107] Example 4 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 1 were prepared in a volume ratio of 65:35. Except for this, the positive electrode material according to Example 4 was obtained in the same manner as in Example 1.

[0108] Example 5 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 1 were prepared in a volume ratio of 55:45. Except for this, the positive electrode material according to Example 5 was obtained in the same manner as in Example 1.

[0109] Example 6 [Preparation of the first solid electrolyte material] In a dry argon atmosphere, LiBr, LiCl, YCl3, and YBr3 were prepared as raw material powders in a molar ratio of LiBr:LiCl:YCl3:YBr3=3:3:1:1. Except for this, the powder of the first solid electrolyte material according to Example 6 was obtained in the same manner as in Example 1. The first solid electrolyte material according to Example 6 had a composition represented by Li3YBr3Cl3.

[0110] [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 6 were prepared in a volume ratio of 60.6:39.4. Except for this, the positive electrode material according to Example 6 was obtained in the same manner as in Example 1.

[0111] Example 7 [Preparation of the first solid electrolyte material] In a dry argon atmosphere, LiCl and YCl3 were prepared as raw material powders in a molar ratio of LiCl:YCl3 = 3:1. Except for this, the powder of the first solid electrolyte material according to Example 7 was obtained in the same manner as in Example 1. The first solid electrolyte material according to Example 7 had a composition represented by Li3YCl6.

[0112] [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 7 were prepared in a volume ratio of 58.5:41.5. Except for this, the positive electrode material according to Example 7 was obtained in the same manner as in Example 1.

[0113] Example 8 [Preparation of the first solid electrolyte material] In a dry argon atmosphere, LiBr and YBr3 were prepared as raw material powders in a molar ratio of LiBr:YBr3 = 3:1. Except for this, the powder of the first solid electrolyte material according to Example 8 was obtained in the same manner as in Example 1. The first solid electrolyte material according to Example 8 had a composition represented by Li3YBr6.

[0114] [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 8 were prepared in a volume ratio of 68.8:31.2. Except for this, the positive electrode material according to Example 8 was obtained in the same manner as in Example 1.

[0115] Example 9 [Preparation of the first solid electrolyte material] In a dry argon atmosphere, LiCl, ZrCl4, and YCl3 were prepared as raw material powders in a molar ratio of LiCl:ZrCl4:YCl3=5:1:1. Except for this, the powder of the first solid electrolyte material according to Example 9 was obtained in the same manner as in Example 1. The solid electrolyte material according to Example 9 was Li 2.5 Zr 0.5 Y 0.5 It had a composition represented by Cl6.

[0116] [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 9 were prepared in a volume ratio of 65:35. Except for this, the positive electrode material according to Example 9 was obtained in the same manner as in Example 1.

[0117] Example 10 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 9 were prepared in a volume ratio of 60:40. Except for this, the positive electrode material according to Example 10 was obtained in the same manner as in Example 1.

[0118] Example 11 [Preparation of the first solid electrolyte material] In a dry argon atmosphere, LiCl and YCl3 were prepared as raw material powders in a molar ratio of LiCl:YCl3=3:1. Except for this, the powder of the first solid electrolyte material according to Example 11 was obtained in the same manner as in Example 1. The solid electrolyte material according to Example 11 had a composition represented by Li3YCl6.

[0119] [Preparation of positive electrode material] In a dry argon atmosphere, a positive electrode active material Li(NiCoAl)O2 (hereinafter referred to as "NCA") and the first solid electrolyte material according to Example 11 were prepared in a volume ratio of 58.5:41.5. Except for this, the positive electrode material according to Example 11 was obtained in the same manner as in Example 1.

[0120] Comparative Example 1 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 1 were prepared in a volume ratio of 90:10. Except for this, the positive electrode material according to Comparative Example 1 was obtained in the same manner as in Example 1.

[0121] Comparative Example 2 [Preparation of positive electrode material] In a dry argon atmosphere, powders of NCM and the first solid electrolyte material according to Example 1 were prepared in a volume ratio of 50:50. Except for this, the positive electrode material according to Comparative Example 2 was obtained in the same manner as in Example 1.

[0122] [Preparation of sulfide solid electrolyte] In a dry argon atmosphere, Li2S and P2S5 were prepared in a molar ratio of Li2S:P2S5=75:25. The mixture was treated to react mechanochemically for 10 hours at 510 rpm using a planetary ball mill (Fritsch, P-7 type). In this way, a glassy solid electrolyte was obtained. The obtained glassy solid electrolyte was heat-treated at 270°C for 2 hours in an inert atmosphere to obtain a glass-ceramic sulfide solid electrolyte. The sulfide solid electrolyte had a composition represented by Li2S-P2S5. The Li2S-P2S5 used in the examples and comparative examples is simply called a sulfide solid electrolyte.

[0123] [Preparation of negative electrode material] In a dry argon atmosphere, graphite and a sulfide solid electrolyte were prepared in a mass ratio of 60:40. These materials were mixed in an agate mortar. In this manner, a negative electrode material was obtained. This negative electrode material was used in Examples 1 to 5.

[0124] [Preparation of secondary battery] (Secondary Batteries of Examples 1 to 5 and Comparative Examples 1 and 2) A sulfide solid electrolyte (40 mg) and the first solid electrolyte material (55 mg) according to Example 1 were laminated in this order in an insulating cylinder having an inner diameter of 9.5 mm to obtain a laminate. A pressure of 160 MPa was applied to the laminate to form a solid electrolyte layer.

[0125] Next, the above-mentioned negative electrode material (15.74 mg) was laminated on the sulfide solid electrolyte side, and the positive electrode material according to Example 1 (corresponding to 14.17 mg of positive electrode active material) was laminated on the first solid electrolyte material according to Example 1. A pressure of 720 MPa was applied to the laminate, and the negative electrode and the positive electrode were formed.

[0126] Current collectors made of stainless steel were placed on the positive and negative electrodes, and current collecting leads were attached to the current collectors.

[0127] Finally, the inside of the insulating cylinder was isolated from the outside atmosphere by using an insulating ferrule, and the inside of the cylinder was sealed. In this manner, the secondary battery according to Example 1 was obtained.

[0128] Secondary batteries according to Examples 2 to 5 and Comparative Examples 1 and 2 were obtained in the same manner as in the production of the secondary battery according to Example 1, except that the positive electrode materials according to Examples 2 to 5 and Comparative Examples 1 and 2 were used instead of the positive electrode material according to Example 1.

[0129] (Secondary battery according to Example 6) After the first solid electrolyte material (80 mg) according to Example 6 was placed in an insulating cylinder having an inner diameter of 9.5 mm, a pressure of 80 MPa was applied. Next, the positive electrode material (corresponding to 7 mg of positive electrode active material) according to Example 6 was placed in the cylinder, and a pressure of 360 MPa was applied to the solid electrolyte material according to Example 6 and the positive electrode material according to Example 6. In this manner, a solid electrolyte layer and a positive electrode were formed.

[0130] Next, a metal In foil (thickness 200 μm), a metal Li foil (thickness 300 μm), and a metal In foil (thickness 200 μm) were laminated on the solid electrolyte layer in this order to obtain a laminate. A pressure of 80 MPa was applied to the laminate to form a negative electrode.

[0131] Except for the above, the secondary battery of Example 6 was obtained in the same manner as in the production of the secondary battery of Example 1.

[0132] (Secondary batteries according to Examples 7 and 11) A secondary battery of Example 7 was obtained in the same manner as in the production of the secondary battery of Example 6, except that the positive electrode material of Example 7 (corresponding to 7 mg of positive electrode active material) and the first solid electrolyte material of Example 7 were used instead of the positive electrode material of Example 6 and the first solid electrolyte material of Example 6.

[0133] A secondary battery according to Example 11 was obtained in the same manner as in the production of the secondary battery according to Example 7, except that the positive electrode material according to Example 11 was used instead of the positive electrode material according to Example 7.

[0134] (Secondary battery according to Example 8) A secondary battery of Example 8 was obtained in the same manner as in the production of the secondary battery of Example 6, except that the positive electrode material of Example 8 (corresponding to 7 mg of positive electrode active material) and the first solid electrolyte material of Example 8 were used instead of the positive electrode material of Example 6 and the first solid electrolyte material of Example 6.

[0135] (Secondary batteries according to Examples 9 and 10) In an insulating cylinder having an inner diameter of 9.5 mm, a sulfide solid electrolyte (40 mg) and the first solid electrolyte material (40 mg) according to Example 9 were laminated in this order. A pressure of 80 MPa was applied to the obtained laminate, and a solid electrolyte layer was formed.

[0136] Next, the positive electrode material of Example 9 (corresponding to 7 mg of positive electrode active material) was laminated on the first solid electrolyte material of Example 9 to obtain a laminate. A pressure of 360 MPa was applied to this laminate to form a positive electrode.

[0137] Except for the above, the secondary battery of Example 9 was obtained in the same manner as in the production of the secondary battery of Example 6.

[0138] A secondary battery of Example 10 was obtained in the same manner as in the production of the secondary battery of Example 9, except that the positive electrode material of Example 10 was used instead of the positive electrode material of Example 9.

[0139] [Charge / discharge test] (Secondary batteries according to Examples 1 to 5, Comparative Example 1, and Comparative Example 2) The obtained secondary battery was placed in a thermostatic chamber at 25°C.

[0140] The secondary battery was charged at a current value of 142 μA, corresponding to a 0.05 C rate (20 hour rate), until a voltage of 4.2 V was reached.

[0141] Next, the secondary battery was discharged at a current value of 142 μA, which corresponds to a rate of 0.05 C, until the voltage reached 2.5 V.

[0142] (Secondary batteries according to Examples 6 to 11) The obtained secondary battery was placed in a thermostatic chamber at 25°C.

[0143] The secondary battery was charged at a current value of 70 μA, corresponding to a 0.05 C rate (20 hour rate), until a voltage of 3.7 V was reached.

[0144] Next, the secondary battery was discharged at a current value of 70 μA, which corresponds to a rate of 0.05 C, until the voltage reached 1.9 V.

[0145] The measurement results of the discharge capacity of the secondary batteries according to Examples 1 to 11, Comparative Example 1, and Comparative Example 2 are shown in Fig. 1 and Table 1. "Volume ratio of active material in positive electrode" in Fig. 1 and Table 1 means the ratio of the volume of the positive electrode active material to the total volume of the positive electrode active material and the solid electrolyte material in the positive electrode.

[0146] In FIG. 1, plots corresponding to Examples 1 to 5, Comparative Example 1, and Comparative Example 2 are connected by dotted lines.

[0147] [Table 1]

[0148] (Consideration) As is clear from Table 1, the batteries containing the positive electrode materials according to Examples 1 to 11 have high discharge capacities.

[0149] As is clear from a comparison of Comparative Examples 1 and 2 with Examples 1 to 5, when the ratio of the volume of the positive electrode active material to the total volume of the positive electrode active material and the solid electrolyte material in the positive electrode is outside the range of 0.55 or more and 0.85 or less, the discharge capacity of the battery is significantly reduced.

[0150] As is clear from a comparison of Examples 3 and 4 with Examples 1, 2, and 5, when the ratio of the volume of the positive electrode active material to the sum of the volume of the positive electrode active material and the volume of the solid electrolyte material in the positive electrode is 0.65 or more and 0.72 or less, the battery has a higher discharge capacity.

[0151] As described above, the positive electrode material according to the present disclosure is suitable for providing a battery having a high discharge capacity. [Industrial Applicability]

[0152] The positive electrode materials and batteries of the present disclosure are utilized, for example, in all-solid-state lithium ion secondary batteries. [Explanation of symbols]

[0153] 1000 batteries 101 Positive electrode 102 Electrolyte layer 103 Negative electrode 110 First solid electrolyte particle 111 Positive electrode active material particles

Claims

1. Contains a positive electrode active material and a first solid electrolyte material, The first solid electrolyte material is represented by the following chemical formula (1): Li α M β X γ ・・・(1) Here, α, β, and γ are all greater than 0. M is at least one element selected from the group consisting of metal elements and metalloid elements other than lithium, and contains yttrium; X is at least one element selected from the group consisting of fluorine, chlorine, bromine, and iodine; a ratio of the volume of the positive electrode active material to the sum of the volume of the positive electrode active material and the volume of the first solid electrolyte material is 0.55 or more and 0.85 or less; Positive electrode material.

2. The ratio is 0.60 or more and 0.72 or less. The positive electrode material according to claim 1 .

3. The ratio is equal to or greater than 0.65 and equal to or less than 0.

72. The positive electrode material according to claim 2 .

4. The M includes zirconium. The positive electrode material according to any one of claims 1 to 3.

5. In the above chemical formula (1), 2.5≦α≦3, β=1, and γ=6 are satisfied; The positive electrode material according to any one of claims 1 to 4.

6. The X includes chlorine. The positive electrode material according to any one of claims 1 to 5.

7. X contains bromine; The positive electrode material according to any one of claims 1 to 6.

8. The positive electrode active material is lithium nickel-cobalt-manganese oxide. The positive electrode material according to any one of claims 1 to 7.

9. The positive electrode active material is nickel-cobalt-lithium aluminum oxide. The positive electrode material according to any one of claims 1 to 8.

10. A positive electrode comprising the positive electrode material according to any one of claims 1 to 9. a negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode and containing a second solid electrolyte material; battery.

11. The second solid electrolyte material is a halide solid electrolyte. The battery of claim 10.

12. The second solid electrolyte material is the same material as the first solid electrolyte material.

12. The battery of claim 11.

13. The second solid electrolyte material is a sulfide solid electrolyte. The battery of claim 10.

Citation Information

Patent Citations

  • Lithium-ion secondary battery and its manufacturing method

    JP2010140725A

  • Method of manufacturing solid electrolyte layer

    JP2010186682A

  • Sulfide solid electrolyte material and cell using the same

    JP2019003927A

  • Solid electrolyte material, and cell

    WO2018025582A1

  • All-solid lithium battery and method of manufacturing same

    WO2019093222A1