Electrolytic capacitors

By using an ionic conductor with specific solvent and component ratios, the electrolytic capacitor's low-temperature characteristics and voltage resistance are improved, addressing solidification issues in existing capacitors.

JP7565510B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2019561628
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-28
Filing Date
2018-12-21
Publication Date
2024-10-11
Estimated Expiration
2038-12-21

AI Technical Summary

Technical Problem

Existing electrolytic capacitors using organic acid onium salts with low solvent content face solidification in low-temperature environments, deteriorating their low-temperature characteristics and capacity.

Method used

Incorporating an ionic conductor with a solvent content of more than 10% to 60% by mass and a total acid and base component content of 40% to 90% by mass, with a melting point of -10°C or lower, to enhance the electrolytic capacitor's low-temperature performance.

Benefits of technology

The solution prevents solidification, improves low-temperature capacity, and enhances repairability and voltage resistance, maintaining performance in extreme conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565510000002
    Figure 0007565510000002
  • Figure 0007565510000003
    Figure 0007565510000003
  • Figure 0007565510000001
    Figure 0007565510000001
Patent Text Reader

Abstract

The electrolytic capacitor includes an anode body having a dielectric layer formed on its surface, a solid electrolyte layer in contact with the dielectric layer and containing a conductive polymer, and an ionic conductor that is liquid at room temperature. The ionic conductor contains a solvent, an acid component, and a base component, and the solvent content in the ionic conductor is more than 10% by mass and not more than 60% by mass, and the total content of the acid component and the base component in the ionic conductor is 40% by mass or more and less than 90% by mass. The melting point of the ionic conductor is -10°C or less. This allows for the provision of an electrolytic capacitor with excellent low-temperature characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic capacitor having a solid electrolyte layer containing a conductive polymer. [Background technology]

[0002] Electrolytic capacitors, which include an anode body having a dielectric layer and a solid electrolyte layer formed so as to cover at least a portion of the dielectric layer, are considered to be promising as small-sized, large-capacity capacitors with low equivalent series resistance (ESR). Patent Document 1 discloses that an organic acid onium salt is used as an electrolyte in order to increase the voltage resistance of the electrolytic capacitor. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-22938 A Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Document 1 proposes that when an organic acid onium salt is used as an electrolyte solution containing a solvent, the amount of the solvent should be small, 10 mass % or less of the electrolyte solution. However, since the electrolyte described in Patent Document 1 contains a small amount of solvent, the electrolyte may solidify in a low-temperature environment, which may result in a deterioration in the low-temperature characteristics of the electrolytic capacitor. [Means for solving the problem]

[0005] In view of the above, one aspect of the present invention Electrolytic capacitors related to The present invention relates to an anode body having a dielectric layer formed on its surface, a solid electrolyte layer in contact with the dielectric layer and containing a conductive polymer, and a liquid electrolyte that is liquid at room temperature. body and an ion conductor comprising do. The ionic conductor includes a solvent, an acid component, and a base component. nothing.The content of the solvent in the ion conductor is more than 10% by mass and not more than 60% by mass, and the total content of the acid component and the base component in the ion conductor is 40% by mass or more and less than 90% by mass. do. The melting point of the ionic conductor is −10° C. or lower. do. Effect of the Invention

[0006] According to the present invention, it is possible to provide an electrolytic capacitor having excellent low-temperature characteristics. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of an electrolytic capacitor according to one embodiment of the present invention. [Diagram 2] 2 is a schematic diagram for explaining the configuration of a capacitor element according to the same embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The electrolytic capacitor according to the present invention comprises an anode body having a dielectric layer formed on its surface, a solid electrolyte layer in contact with the dielectric layer and containing a conductive polymer, and a liquid electrolyte layer that is liquid at room temperature. body The ionic conductor includes a solvent, an acid component, and a base component. The content of the solvent in the ionic conductor is more than 10 mass% and not more than 60 mass%, and the total content of the acid component and the base component in the ionic conductor is 40 mass% or more and less than 90 mass%. The melting point of the ionic conductor is -10°C or less.

[0009] When the content of the solvent in the ionic conductor exceeds 10% by mass (the total content of the acid component and the base component in the ionic conductor is less than 90% by mass) and the melting point of the ionic conductor is -10°C or lower, solidification of the ionic conductor in a low-temperature environment is suppressed, and the low-temperature characteristics of the electrolytic capacitor are improved. For example, the decrease in capacity due to solidification of the ion conductor in a low-temperature environment and the decrease in the repairability of the dielectric layer are suppressed. In addition, the capacity appearance rate in a low-temperature environment (e.g., −55° C.) is increased. The melting point of the ion conductor is preferably −40° C. or lower, and more preferably −55° C. or lower. By providing the electrolytic capacitor with an ion conductor, the repairability of the dielectric layer is improved and the voltage resistance is increased.

[0010] When the total content of acid components and base components in the ionic conductor is 40 mass% or more (the solvent content in the ionic conductor is 60 mass% or less), the number of dissociated anions (anions derived from the acid components) increases, and the effect of improving the repairability of the dielectric layer can be sufficiently obtained.

[0011] From the viewpoint of improving low-temperature properties, the content of the solvent in the ionic conductor is preferably 11% by mass to 60% by mass, more preferably 20% by mass to 60% by mass, and even more preferably 40% by mass to 60% by mass. The total content of the acid component and the base component in the ionic conductor is preferably 40% by mass to 89% by mass, more preferably 40% by mass to 80% by mass, and even more preferably 40% by mass to 60% by mass.

[0012] (Acid and base components) It is preferable that the acid component contains a carboxylic acid and the base component contains an amidine compound. It is also preferable that the acid component contains a sulfonic acid and the base component contains at least one selected from the group consisting of amine compounds (primary amines, secondary amines, and tertiary amines) and amidine compounds.

[0013] The salts containing the above-mentioned acidic and basic components can exist as liquids at room temperature (24°C) in the state of neutralized salts, and are unlikely to precipitate even in low-temperature environments even when contained in high concentrations in the ionic conductor, which further suppresses solidification of the ionic conductor and further improves the low-temperature characteristics of the electrolytic capacitor.

[0014] Even if the solvent is reduced by evaporating through the sealing member to the outside of the electrolytic capacitor, the salt containing the above-mentioned acid component and base component can remain as a liquid, so the solid electrolyte is sufficiently covered with the ion conductor. Therefore, deterioration of the solid electrolyte layer caused by contact of the solid electrolyte layer (conductive polymer) with moisture or oxygen as the solvent is reduced, and the resulting shortening of the life of the electrolytic capacitor are suppressed. Even if the solvent is reduced due to the application of heat from outside the electrolytic capacitor or heat generation due to ripple current, deterioration of the solid electrolyte layer is suppressed due to the presence of the above-mentioned acid component and base component. Therefore, heat resistance and resistance to ripple current are also improved.

[0015] In cases where the acid component contains a carboxylic acid and the base component contains an amidine compound, the ionic conductor preferably contains more acid components than base components in molar ratio and has a pH of 4.5 or less. In this case, dedoping of the dopant contained in the solid electrolyte layer from the conductive polymer is suppressed, and an increase in ESR due to dedoping of the dopant is suppressed.

[0016] In the case where the acid component contains a carboxylic acid and the base component contains an amidine compound, the content of the base component in the ion conductor is preferably 10% by mass or more and the content of the acid component in the ion conductor is preferably 30% by mass or more. In this case, dedoping of the dopant contained in the solid electrolyte layer from the conductive polymer is suppressed, and an increase in ESR due to dedoping of the dopant is suppressed.

[0017] The acid component includes a sulfonic acid, and the base component includes at least an amine compound and an amidine compound. When the ionic conductor contains either one of the acid component and the base component, the ionic conductor preferably contains the acid component in an amount equal to or greater than the base component in molar ratio, and the pH of the ionic conductor is preferably less than 7.0. In this case, dedoping of the dopant contained in the solid electrolyte layer from the conductive polymer is suppressed, and an increase in ESR due to dedoping of the dopant is suppressed.

[0018] The carboxylic acid preferably includes an aromatic carboxylic acid (aromatic dicarboxylic acid) having two or more carboxyl groups. Examples of aromatic carboxylic acids include phthalic acid (ortho form), isophthalic acid (meta form), terephthalic acid (para form), maleic acid, benzoic acid, salicylic acid, trimellitic acid, and pyromellitic acid. Among them, aromatic dicarboxylic acids such as phthalic acid (ortho form) and maleic acid are more preferable. The carboxyl group of aromatic dicarboxylic acid is stable and does not easily cause side reactions. Therefore, it exerts the effect of stabilizing the conductive polymer for a long period of time, which is advantageous for extending the life of the electrolytic capacitor. From the viewpoint of the repairability and thermal stability of the dielectric layer, phthalic acid (ortho form) is more preferable. The carboxylic acid may also be an aliphatic carboxylic acid, such as adipic acid.

[0019] Examples of sulfonic acids include aromatic sulfonic acids such as benzenesulfonic acid, alkylbenzenesulfonic acid (e.g., toluenesulfonic acid), naphthalenesulfonic acid, and alkylnaphthalenesulfonic acid (e.g., ethylnaphthalenesulfonic acid, butylnaphthalenesulfonic acid), and aliphatic sulfonic acids such as alkylsulfonic acids (e.g., methanesulfonic acid, ethanesulfonic acid). Among these, naphthalenesulfonic acid and 1,4-naphthalenedisulfonic acid are preferred from the viewpoint of the repairability of the dielectric layer and the thermal stability of the molecular structure. When the sulfonic acid has an alkyl group, the number of carbon atoms of the alkyl group is preferably 1 or more and 10 or less.

[0020] Carboxylic acids are thermally decomposed in extremely high temperature environments such as during reflow soldering to generate carbon dioxide gas, which can cause the sealing portion of the capacitor to swell. On the other hand, sulfonic acids do not generate the above-mentioned carbon dioxide gas. In this respect, sulfonic acids are advantageous in extremely high temperature environments such as during reflow soldering.

[0021] Examples of the amine compounds (primary to tertiary amines) include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, N,N-diisopropylethylamine, tetramethylethylenediamine, hexamethylenediamine, spermidine, spermine, amantadine, aniline, phenethylamine, toluidine, pyrrolidine, piperidine, piperazine, morpholine, imidazole, pyridine, pyridazine, pyrimidine, pyrazine, and 4-dimethylaminopyridine. These may be used alone or in combination of two or more. Among them, tertiary amines are preferred, and triethylamine and monoethyldimethylamine are particularly preferred.

[0022] The amidine compound is a compound having an alkyl-substituted amidine group, and examples thereof include cyclic amidine compounds or their quaternized derivatives (amidinium compounds).Specific examples include 1,2,3,4-tetramethylimidazolinium, 1-ethyl-2,3-dimethylimidazolinium, and 1-ethyl-3-methylimidazolium.

[0023] (solvent) From the viewpoint of improving the low-temperature characteristics of the electrolytic capacitor, the melting point of the solvent is preferably −10° C. or lower. In this case, it is easy to adjust the melting point of the ion conductor to −10° C. or lower.

[0024] The solvent preferably contains at least one glycol compound selected from the group consisting of alkylene glycol and polyalkylene glycol, because the melting point of the solvent can be easily adjusted to -10°C or lower. Since glycol compounds are unlikely to permeate through the sealing material of the electrolytic capacitor, the evaporation of the solvent to the outside of the electrolytic capacitor is suppressed, and deterioration of the solid electrolyte layer (conductive polymer) due to evaporation of the solvent is prevented. This also suppresses the deterioration of the life span of the electrolytic capacitor. Even when heat is applied from the outside of the electrolytic capacitor, such as in reflow, or when heat is generated due to ripple current, the evaporation of the solvent to the outside of the electrolytic capacitor is suppressed. Therefore, the heat resistance and resistance to ripple current are also improved.

[0025] From the viewpoint of suppressing permeation of the plugging material, the alkylene glycol preferably has 5 or less carbon atoms. From the viewpoint of improving the low-temperature characteristics of the electrolytic capacitor and suppressing evaporation of the solvent, it is preferable that the alkylene glycol contains at least one of propylene glycol (melting point -50°C or less) and butylene glycol (melting point -50°C or less). The alkylene glycol may also contain ethylene glycol (melting point -12.9°C) or the like.

[0026] From the viewpoint of improving the low-temperature characteristics of the electrolytic capacitor and suppressing evaporation of the solvent, the polyalkylene glycol preferably contains a copolymer of ethylene glycol (EG) and propylene glycol (PG). The number average molecular weight of the copolymer of ethylene glycol and propylene glycol is, for example, 88 or more and 5000 or less. The mass ratio of ethylene glycol and propylene glycol used as monomers constituting the copolymer is preferably 10 parts by mass or more and 10,000 parts by mass or less of propylene glycol per 100 parts by mass of ethylene glycol.

[0027] The polyalkylene glycol may include polyethylene glycol, polypropylene glycol, etc. The number average molecular weight of the polyethylene glycol is, for example, 300 or less. The number average molecular weight of the polypropylene glycol is, for example, 102 or more and 5000 or less.

[0028] From the viewpoint of improving the low-temperature characteristics of the electrolytic capacitor and suppressing evaporation of the solvent, it is preferable to use the above-mentioned glycol compound as the main solvent. The content of the glycol compound in the solvent is preferably 20 mass % or more, more preferably 40 mass % or more.

[0029] The solvent may contain other components such as a sulfone compound, a lactone compound, and a carbonate compound in addition to the glycol compound. As the sulfone compound, sulfolane, dimethyl sulfoxide, diethyl sulfoxide, etc. can be used. As the lactone compound, γ-butyrolactone, γ-valerolactone, etc. can be used. As the carbonate compound, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), fluoroethylene carbonate (FEC), etc. can be used.

[0030] The ionic conductor may contain water in an amount of more than 1% by mass and less than 10% by mass. When the water content in the ionic conductor is more than 1% by mass, the repairability of the dielectric layer is ensured. When the water content in the ionic conductor is less than 10% by mass, corrosion of the anode body is suppressed. The water content in the ionic conductor is more preferably more than 1% by mass and not more than 5% by mass.

[0031] The conductive polymer contained in the solid electrolyte layer is a π-conjugated conductive polymer, and polypyrrole, polythiophene, polyaniline, etc. are preferable. In this specification, polypyrrole, polythiophene, polyaniline, etc. refer to polymers having polypyrrole, polythiophene, polyaniline, etc. as their basic skeletons, respectively. Therefore, polypyrrole, polythiophene, polyaniline, etc. may also include their respective derivatives. For example, polythiophene includes its derivative, poly(3,4-ethylenedioxythiophene) (PEDOT), etc. These may be used alone or in combination of two or more kinds, or may be copolymers of two or more kinds of monomers. There is no particular limit to the weight average molecular weight of the conductive polymer. Although not limited thereto, it is, for example, 1,000 to 100,000. The solid electrolyte layer may further contain a dopant.

[0032] The present invention will be described in more detail below based on the embodiments, however, the present invention is not limited to the following embodiments.

[0033] FIG. 1 is a schematic cross-sectional view of the electrolytic capacitor according to this embodiment, and FIG. 2 is a schematic exploded view of a portion of a capacitor element of the electrolytic capacitor.

[0034] The electrolytic capacitor includes, for example, a capacitor element 10, a bottomed case 11 that houses the capacitor element 10, a sealing member 12 that closes the opening of the bottomed case 11, a seat plate 13 that covers the sealing member 12, lead wires 14A, 14B that are led out from the sealing member 12 and pass through the seat plate 13, lead tabs 15A, 15B that connect the lead wires to electrodes of the capacitor element 10, and an ion conductor (not shown). The vicinity of the open end of the bottomed case 11 is drawn inward, and the open end is curled so as to be crimped to the sealing member 12.

[0035] Capacitor element 10 is produced from a wound body as shown in Fig. 2. The wound body includes an anode body 21 connected to lead tab 15A, a cathode body 22 connected to lead tab 15B, and a separator 23. The wound body is a semi-finished product in which a solid electrolyte layer is not formed between anode body 21 and cathode body 22.

[0036] The anode body 21 and the cathode body 22 are wound with a separator 23 interposed therebetween. The outermost periphery of the wound body is fixed with a stop tape 24. Note that FIG. Tome The separator 23 is shown in a partially expanded state before being folded in. The material for the separator 23 may be, for example, a nonwoven fabric containing cellulose, polyethylene terephthalate, vinylon, aramid fiber, or the like as a main component.

[0037] The anode body 21 comprises a metal foil that has been roughened so that the surface has projections and recesses, and a dielectric layer is formed on the metal foil having projections and recesses. A conductive polymer is attached to at least a portion of the surface of the dielectric layer to form a solid electrolyte layer. The solid electrolyte layer may cover at least a portion of the surface of the cathode body 22 and / or the surface of the separator 23. The capacitor element 10 on which the solid electrolyte layer has been formed is heated to 3000° C. together with an electrolytic solution. Bottomed Case 11 will be housed in.

[0038] Hereinafter, an example of a method for manufacturing the electrolytic capacitor according to this embodiment will be described step by step. (i) preparing an anode body 21 having a dielectric layer First, prepare a metal foil as the raw material of the anode body 21. Although the type of metal is not particularly limited, it is preferable to use a valve metal such as aluminum, tantalum, or niobium, or an alloy containing a valve metal, because this facilitates the formation of a dielectric layer.

[0039] Next, the surface of the metal foil is roughened. By roughening, a plurality of projections and recesses are formed on the surface of the metal foil. The roughening is preferably performed by etching the metal foil. The etching may be performed by, for example, DC electrolysis or AC electrolysis.

[0040] Next, a dielectric layer is formed on the roughened surface of the metal foil. The method of formation is not particularly limited, but the dielectric layer can be formed by subjecting the metal foil to a chemical conversion treatment. In the chemical conversion treatment, for example, the metal foil is immersed in a chemical conversion solution such as an ammonium adipate solution and heat-treated. Alternatively, the metal foil may be immersed in the chemical conversion solution and a voltage may be applied.

[0041] Generally, from the viewpoint of mass production, a roughening treatment is performed on large-sized valve metal foils (metal foils). Then, a chemical conversion treatment is performed. In this case, the treated foil is cut to a desired size to prepare the anode body 21.

[0042] (ii) A step of preparing the cathode body 22 As with the anode body, a metal foil can be used for the cathode body 22. There are no particular limitations on the type of metal, but it is preferable to use a valve metal such as aluminum, tantalum, or niobium, or an alloy containing a valve metal. If necessary, the surface of the cathode body 22 may be roughened.

[0043] (iii) Preparation of the roll Next, a wound body is produced using the anode body 21 and the cathode body 22. First, anode body 21 and cathode body 22 are wound with separator 23 interposed therebetween. At this time, lead tabs 15A, 15B are wound while being wound, so that lead tabs 15A, 15B can be planted from the wound body as shown in FIG.

[0044] The material of the separator 23 may be, for example, a nonwoven fabric containing natural cellulose, synthetic cellulose, polyethylene terephthalate, vinylon, aramid fiber, or the like as a main component.

[0045] The material of the lead tabs 15A and 15B is not particularly limited as long as it is a conductive material. The material of the lead wires 14A and 14B connected to the lead tabs 15A and 15B, respectively, is also not particularly limited as long as it is a conductive material.

[0046] Next, of the wound anode body 21, cathode body 22, and separator 23, a stop tape 24 is placed on the outer surface of cathode body 22, which is the outermost layer, and an end of cathode body 22 is fixed with stop tape 24. When anode body 21 is prepared by cutting a large-sized metal foil, a chemical conversion treatment may be further performed on the wound body in order to provide a dielectric layer on the cut surface of anode body 21.

[0047] (iv) Step of forming capacitor element 10 Next, the polymer dispersion is impregnated into the dielectric layer to form a film covering at least a part of the dielectric layer. The polymer dispersion includes a liquid component and a conductive polymer dispersed in the liquid component. The polymer dispersion may be a solution in which a conductive polymer is dissolved in the liquid component, or a dispersion in which particles of a conductive polymer are dispersed in the liquid component. Next, the liquid component is volatilized from the formed film by drying to form a dense solid electrolyte layer covering at least a part of the dielectric layer. Since the polymer dispersion is uniformly distributed in the liquid component, it is easy to form a uniform solid electrolyte layer. In this way, the capacitor element 10 is obtained.

[0048] The polymer dispersion can be obtained, for example, by dispersing a conductive polymer in a liquid component, or by polymerizing a precursor monomer in the liquid component to generate conductive polymer particles, etc. A preferred polymer dispersion is, for example, poly(3,4-ethylenedioxythiophene) (PEDOT) doped with polystyrene sulfonate (PSS), i.e., PEDOT / PSS.

[0049] The liquid component may be water, a mixture of water and a non-aqueous solvent, or a non-aqueous solvent. The non-aqueous solvent is not particularly limited, and for example, a protic solvent or an aprotic solvent can be used. Examples of protic solvents include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, and propylene glycol, and ethers such as formaldehyde and 1,4-dioxane. Examples of aprotic solvents include amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone, esters such as methyl acetate, and ketones such as methyl ethyl ketone. Examples include:

[0050] A method for applying the polymer dispersion to the surface of the dielectric layer is, for example, a simple and preferred method of immersing the wound body in the polymer dispersion contained in a container. The immersion time depends on the size of the wound body, but is, for example, 1 second to 5 hours, preferably 1 minute to 30 minutes. The impregnation is preferably carried out under reduced pressure, for example, in an atmosphere of 10 to 100 kPa, preferably 40 to 100 kPa. After the wound body is removed from the polymer dispersion, drying is preferably carried out at, for example, 50 to 300°C, more preferably 100 to 200°C.

[0051] The step of applying the polymer dispersion to the surface of the dielectric layer and the step of drying the wound body may be repeated two or more times. By performing these steps multiple times, the coverage of the solid electrolyte layer on the dielectric layer can be increased. In this case, the solid electrolyte layer may be formed not only on the surface of the dielectric layer but also on the surfaces of the cathode body 22 and the separator 23.

[0052] In this manner, a solid electrolyte layer is formed between anode body 21 and cathode body 22, producing capacitor element 10. The solid electrolyte layer formed on the surface of the dielectric layer actually functions as a cathode material.

[0053] (v) Ions transmission A body is prepared, and an ion is placed in the capacitor element 10. transmission The process of impregnating the body Next, an acid component and a base component are dissolved in a solvent to prepare an ion conductor, and then the ion conductor is impregnated into the capacitor element 10. There is no particular limitation on the method for impregnating the capacitor element 10 with the ion conductor. For example, a method of immersing the capacitor element 10 in the ion conductor contained in a container is simple and preferable. The immersion time depends on the size of the capacitor element 10, but is, for example, 1 second to 5 minutes. The impregnation is preferably performed under reduced pressure, for example, in an atmosphere of 10 to 100 kPa, preferably 40 to 100 kPa.

[0054] (vi) Encapsulating the capacitor element Next, capacitor element 10 is sealed. Specifically, capacitor element 10 is first housed in bottomed case 11 so that lead wires 14A and 14B are located on the upper surface of bottomed case 11, which is open. The material of bottomed case 11 can be a metal such as aluminum, stainless steel, copper, iron, brass, or an alloy of these metals.

[0055] Next, sealing member 12, which is formed so that lead wires 14A, 14B pass through it, is placed above capacitor element 10, and capacitor element 10 is sealed in bottomed case 11. Next, a horizontal drawing process is performed near the open end of bottomed case 11, and the open end is crimped to sealing member 12 to curl it. Then, seat plate 13 is placed on the curled portion, completing the electrolytic capacitor as shown in Fig. 1. Thereafter, an aging process may be performed while applying a rated voltage.

[0056] In the above embodiment, a wound-type electrolytic capacitor has been described, but the scope of application of the present invention is not limited to the above, and the present invention can also be applied to other electrolytic capacitors, for example, chip-type electrolytic capacitors that use a metal sintered body as an anode body, and stacked-type electrolytic capacitors that use a metal plate as an anode body. EXAMPLES

[0057] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0058] 《Electrolytic capacitor A1》 Wound electrolytic capacitor with rated voltage of 25V and rated capacitance of 330μF (Φ (diameter) A specific method for producing the electrolytic capacitor is described below.

[0059] (Preparation of anode body) An aluminum foil having a thickness of 105 μm was subjected to an etching treatment to roughen the surface of the aluminum foil. Then, a dielectric layer was formed on the surface of the aluminum foil by chemical conversion treatment. The chemical conversion treatment was performed by immersing the aluminum foil in an ammonium adipate solution and applying a voltage of 45 V to the solution. Then, the aluminum foil was ( vertical ) 5.3mm x (beside) The anode body was prepared by cutting to a size of 180 mm.

[0060] (Preparation of the cathode body) An aluminum foil having a thickness of 50 μm was subjected to an etching treatment to roughen the surface of the aluminum foil. ( vertical ) 5.3mm x (beside) The cathode body was prepared by cutting to a length of 180 mm.

[0061] (Making of the roll) An anode lead tab and a cathode lead tab were connected to the anode body and the cathode body, and the anode body and the cathode body were wound with the lead tabs interposed therebetween. An anode lead wire and a cathode lead wire were connected to the ends of the lead tabs protruding from the wound body, respectively. The wound body was then subjected to a chemical conversion treatment again to form a dielectric layer on the cut end of the anode body. Next, the ends of the outer surface of the wound body were fixed with a winding stop tape to produce the wound body.

[0062] (Preparation of polymer dispersion) 3,4-Ethylenedioxythiophene and polystyrene sulfonic acid (PSS, weight average molecular weight 100,000), a polymer dopant, were dissolved in ion-exchanged water (liquid component) to prepare a mixed solution. While stirring the mixed solution, iron sulfate (III) dissolved in ion-exchanged water (acid After the reaction, the reaction solution was dialyzed to remove unreacted monomers and excess oxidizing agent, and a polymer dispersion containing poly(3,4-ethylenedioxythiophene) doped with approximately 5% by mass of PSS (PEDOT / PSS) was obtained.

[0063] (Formation of solid electrolyte layer) The wound body was immersed in a polymer dispersion contained in a specified container in a reduced pressure atmosphere (40 kPa) for 5 minutes, and then the wound body was pulled out from the polymer dispersion. Next, the wound body impregnated with the polymer dispersion was dried in a drying oven at 150°C for 20 minutes to form a solid electrolyte layer that covers at least a part of the dielectric layer, thereby obtaining a capacitor element.

[0064] (Preparation of ionic conductor) An ionic conductor containing a solvent, an acid component, and a base component was prepared. Propylene glycol was used as the solvent. Phthalic acid was used as the acid component, and 1,2,3,4-tetramethylimidazolinium was used as the base component. The content of the solvent in the ionic conductor was 11% by mass, and the total content of the acid component and the base component in the ionic conductor was 89% by mass. The molar ratio of the acid component to the base component: (acid component / base component) was 2.5. At least a part of the acid component was added as a salt with the base component. The pH of the ionic conductor was 4.5, and the melting point of the ionic conductor was -10°C or lower.

[0065] (Impregnation of ionic conductor) The capacitor element was immersed in the ionic conductor for 5 minutes in a reduced pressure atmosphere (40 kPa) to impregnate the capacitor element with the ionic conductor.

[0066] (Sealing of capacitor elements) The capacitor element impregnated with the ion conductor was sealed to complete electrolytic capacitor A1. Specifically, the capacitor element was housed in a bottomed case so that the lead wires were located on the open side of the bottomed case, and a sealing member (elastic material containing butyl rubber as a rubber component) formed so that the lead wires could pass through was placed above the capacitor element to seal the capacitor element in the bottomed case. Then, a drawing process was performed near the open end of the bottomed case, and the open end was further curled, and a seat plate was placed on the curled portion to complete electrolytic capacitor A1 as shown in Figure 1. Thereafter, an aging process was performed at 100°C for 2 hours while a voltage of 39V was applied.

[0067] [evaluation] (a) Measurement of initial low-temperature capacity appearance rate After the solid electrolyte layer was formed and before the ion conductor was impregnated, the capacitor element was measured for capacitance C1 in a 15 mass % aqueous solution of ammonium adipate at 30°C. After the aging treatment, the electrostatic capacitance C2 of the electrolytic capacitor A1 was measured in an environment of -55°C. Using the capacitance C1 and capacitance C2 obtained above, the initial low-temperature capacitance appearance rate was calculated according to the following formula. Initial low-temperature capacity appearance rate (%) = (C2 / C1) x 100 When the initial low-temperature capacity appearance rate was 70% or more, the initial low-temperature characteristics were evaluated as being good.

[0068] (b) Measurement of low-temperature capacitance appearance rate after exposure to high temperatures After the aging treatment, the electrolytic capacitor A1 was left for 4000 hours in a high-temperature environment at 145° C. After being left in the high-temperature environment, the capacitance C3 of the electrolytic capacitor A1 was measured in an environment at −55° C. Using the capacitance C3 obtained above and the capacitance C1 obtained in (a) above, the low-temperature capacitance appearance rate after standing at high temperature was calculated according to the following formula. Low-temperature capacitance appearance rate after high-temperature storage (%) = (C3 / C1) x 100 When the low-temperature capacity appearance rate after high-temperature storage was 30% or more, the low-temperature characteristics after high-temperature storage were evaluated as good. The low-temperature capacity appearance rate after high-temperature storage was measured under harsher conditions that made it easier for the solvent to decrease, compared to the initial measurement of the low-temperature capacity appearance rate.

[0069] (c) Measurement of discharge voltage of ionic conductor (evaluation of voltage resistance) Etched and chemically treated high-voltage aluminum foil (area 10 cm) was used as the anode. 2 ), and a flat aluminum foil (area 10 cm) as the cathode. 2 ) was used, and the anode and cathode were immersed in the ionic conductor to prepare a sample for evaluating the voltage resistance of the ionic conductor. At 25°C, a load was applied between the electrodes of the sample by the constant current method (2 mA), and the change in voltage over time was measured. The voltage at which continuous sparks or scintillation began to be observed was calculated as the discharge voltage of the ionic conductor. In Table 1, cases where the discharge voltage of the ionic conductor was over 100V are indicated as "○", and cases where the discharge voltage of the ionic conductor was 100V or less are indicated as "△".

[0070] Electrolytic capacitors A2 to A8, B1 to B3 An ionic conductor was prepared containing a solvent, an acid component, and a base component as shown in Table 1. The content of the solvent in the ionic conductor and the total content of the acid component and the base component in the ionic conductor were the values ​​shown in Table 1. The pH of the ionic conductor was the value shown in Table 1. Other than the above, electrolytic capacitors A2 to A8 and B1 to B3 were fabricated and evaluated in the same manner as electrolytic capacitor A1.

[0071] 《Electrolytic capacitor B4》 Electrolytic capacitor B4 was produced and evaluated in the same manner as electrolytic capacitor A1, except that the capacitor element was not impregnated with a solvent but was impregnated with only the acid component and the base component. The evaluation results are shown in Table 1. In Table 1, the ionic conductor having a melting point of -10°C or lower is indicated as "◯", and the ionic conductor having a melting point of more than -10°C is indicated as "×".

[0072] [Table 1]

[0073] The electrolytic capacitors A1 to A8 had higher initial low-temperature capacitance appearance rates and low-temperature capacitance appearance rates after high-temperature storage than the electrolytic capacitors B1, B3, and B4, and exhibited excellent low-temperature characteristics both initially and after storage at high temperatures. The electrolytic capacitors A1 to A8 also exhibited excellent voltage resistance.

[0074] In electrolytic capacitor B1, in which the content of the solvent in the ion conductor is small, at 10 mass % or less, the ion conductor solidified in a low-temperature environment, and the low-temperature characteristics deteriorated initially and after being left at high temperature. In electrolytic capacitor B4, the capacitor element was not impregnated with a solvent, and therefore the low-temperature characteristics deteriorated initially and after being left at high temperature. In electrolytic capacitor B2, in which the total content of the acid component and the base component in the ion conductor is small, at less than 40 mass %, the voltage resistance was lower than that of electrolytic capacitors A1 to A8. In electrolytic capacitor B3, the content of the solvent in the ion conductor is more than 10 mass %, but the melting point of the ion conductor is more than -10°C, and therefore the low-temperature characteristics deteriorated after being left at high temperature. [Industrial Applicability]

[0075] The present invention can be applied to electrolytic capacitors which are required to perform well in low temperature environments. [Explanation of symbols]

[0076] 10: capacitor element, 11: bottomed case, 12: sealing member, 13: seat plate, 14A, 14B: lead wires, 15A, 15B: lead tabs, 21: anode body, 22: cathode body, 23: separator, 24: winding stop tape

Claims

1. an anode body having a dielectric layer formed on a surface thereof, a solid electrolyte layer in contact with the dielectric layer and containing a conductive polymer, and an ion conductor that is liquid at room temperature; The ionic conductor includes a solvent, an acid component, and a base component, The content of the solvent in the ion conductor is more than 10% by mass and not more than 60% by mass, The total content of the acid component and the base component in the ion conductor is 40% by mass or more and less than 90% by mass, The melting point of the ionic conductor is −10° C. or lower; the solvent comprises at least one glycol compound selected from the group consisting of alkylene glycols and polyalkylene glycols; The content of the glycol compound in the solvent is 40% by mass or more, The acid component comprises a carboxylic acid, The electrolytic capacitor, wherein the base component includes an amidine compound.

2. the ionic conductor comprises, in a molar ratio, more of the acid component than the base component; 2. The electrolytic capacitor according to claim 1, wherein the ionic conductor has a pH of 4.5 or less.

3. The content of the base component in the ion conductor is 10% by mass or more, 3. The electrolytic capacitor according to claim 1, wherein the content of the acid component in the ion conductor is 30 mass % or more.

4. An anode body having a dielectric layer formed on a surface thereof, a solid electrolyte layer in contact with the dielectric layer and including a conductive polymer, and an ion conductor that is liquid at room temperature, The ionic conductor includes a solvent, an acid component, and a base component, The content of the solvent in the ion conductor is more than 10% by mass and not more than 60% by mass, The total content of the acid component and the base component in the ion conductor is 40% by mass or more and less than 90% by mass, The melting point of the ionic conductor is −10° C. or lower; the solvent comprises at least one glycol compound selected from the group consisting of alkylene glycols and polyalkylene glycols; The content of the glycol compound in the solvent is 40% by mass or more, The acid component comprises a sulfonic acid, The electrolytic capacitor, wherein the base component includes at least one selected from the group consisting of primary amines, secondary amines, tertiary amines and amidine compounds.

5. the ionic conductor contains, in terms of molar ratio, the acid component in an amount equal to or greater than the base component; 5. The electrolytic capacitor of claim 4, wherein the ionic conductor has a pH of less than 7.

0.

6. 6. The electrolytic capacitor according to claim 1, wherein the melting point of the solvent is −10° C. or lower.

7. 7. The electrolytic capacitor according to claim 6, wherein the melting point of the solvent is −50° C. or lower.

8. 5. The electrolytic capacitor according to claim 1, wherein the alkylene glycol includes at least one of propylene glycol and butylene glycol.

9. 5. The electrolytic capacitor of claim 1, wherein the polyalkylene glycol comprises a copolymer of ethylene glycol and propylene glycol.

10. The ionic conductor contains water, The electrolytic capacitor according to any one of claims 1 to 9, wherein the content of the water in the ion conductor is more than 1% by mass and less than 10% by mass.

11. The content of the solvent in the ionic conductor is, except for the case where the content is 40% by mass or more, The electrolytic capacitor according to any one of claims 1 to 10, wherein the total content of the acid component and the base component in the ion conductor is 60 mass % or less, except for cases where the total content of the acid component and the base component in the ion conductor is 60 mass % or less.

Citation Information

Patent Citations

  • Electrolytic capacitor

    JP2003022938A

  • Sample carrier device

    JP2017069357A

  • Electrolytic capacitor

    WO2011099261A1