Solid electrolyte material and battery using same

A solid electrolyte material with Li, M, O, X, and F composition addresses low conductivity and safety issues in sulfide electrolytes by enhancing lithium ion conductivity and stability, ensuring safe battery operation across varying temperatures.

JP7565544B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021552295
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-05
Filing Date
2020-09-28
Publication Date
2024-10-11
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Existing solid electrolyte materials for batteries, such as sulfide solid electrolytes, suffer from low lithium ion conductivity and can generate hazardous hydrogen sulfide when exposed to the atmosphere, posing safety concerns and limiting their effectiveness.

Method used

A solid electrolyte material composed of Li, M (Ta or Nb), O, X (Cl, Br, or I), and F is developed, with a specific molar ratio of these elements to enhance lithium ion conductivity and stability, avoiding sulfur to prevent hydrogen sulfide generation.

Benefits of technology

The new electrolyte material exhibits high lithium ion conductivity and electrochemical stability, maintaining performance across a wide temperature range and ensuring safety by preventing hydrogen sulfide formation, thus enabling stable battery operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565544000003
    Figure 0007565544000003
  • Figure 0007565544000004
    Figure 0007565544000004
  • Figure 0007565544000005
    Figure 0007565544000005
Patent Text Reader

Abstract

This solid electrolyte material according to the present disclosure contains Li, M, O, X, and F. M is at least one element selected from the group consisting of Ta and Nb. X is at least one element selected from the group consisting of Cl, Br, and I.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid electrolyte material and a battery using the same. [Background technology]

[0002] Patent Document 1 discloses an all-solid-state battery that uses a sulfide solid electrolyte material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-129312 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide a solid electrolyte material having high lithium ion conductivity. [Means for solving the problem]

[0005] The solid electrolyte material of the present disclosure comprises Li, M, O, X, and F, where M is at least one element selected from the group consisting of Ta and Nb, and X is at least one element selected from the group consisting of Cl, Br, and I. Effect of the Invention

[0006] The present disclosure provides a solid electrolyte material having high lithium ion conductivity. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 shows a cross-sectional view of a battery 1000 according to a second embodiment. [Diagram 2] FIG. 2 shows a cross-sectional view of an electrode material 1100 according to a second embodiment. [Diagram 3]FIG. 3 shows a schematic diagram of a pressing die 300 used to evaluate the ionic conductivity of a solid electrolyte material. [Figure 4] FIG. 4 is a graph showing the X-ray diffraction patterns of the solid electrolyte materials according to Examples 1 to 6 and Comparative Examples 1 and 2. [Diagram 5] FIG. 5 is a graph showing the X-ray diffraction patterns of the solid electrolyte materials according to Examples 7 to 11. [Figure 6A] FIG. 6A is a graph showing the results of cyclic voltammetry measurements of the solid electrolyte materials according to Examples 1 to 3. [Figure 6B] FIG. 6B is a graph showing the results of cyclic voltammetry measurement of the solid electrolyte material according to Example 4. [Figure 6C] FIG. 6C is a graph for explaining the reduction onset voltage obtained from the results of cyclic voltammetry measurement. [Figure 7] FIG. 7 is a graph showing the initial discharge characteristics of the battery according to Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0009] (First embodiment) The solid electrolyte material according to the first embodiment includes Li, M, O, X, and F. M is at least one element selected from the group consisting of Nb and Ta. X is at least one element selected from the group consisting of Cl, Br, and I.

[0010] The solid electrolyte material according to the first embodiment has high lithium ion conductivity.

[0011] The solid electrolyte material according to the first embodiment can be used to obtain a battery having excellent charge / discharge characteristics.

[0012] The solid electrolyte material according to the first embodiment can maintain high lithium ion conductivity in the expected temperature range for use of the battery (for example, a range of −30° C. to 80° C.). Therefore, the battery using the solid electrolyte material according to the first embodiment can operate stably even in an environment with temperature changes.

[0013] From the viewpoint of safety, it is desirable that the solid electrolyte material according to the first embodiment does not contain sulfur. A solid electrolyte material that does not contain sulfur is excellent in safety because hydrogen sulfide is not generated even when exposed to the atmosphere. It should be noted that hydrogen sulfide may be generated when the sulfide solid electrolyte material disclosed in Patent Document 1 is exposed to the atmosphere.

[0014] In order to enhance the ionic conductivity of the solid electrolyte material, the solid electrolyte material according to the first embodiment may be substantially composed of Li, M, O, X, and F. Here, "the solid electrolyte material according to the first embodiment is substantially composed of Li, M, O, X, and F" means that the molar ratio of the total amount of substance of Li, M, O, X, and F to the total amount of substance of all elements constituting the solid electrolyte material according to the first embodiment is 90% or more. As an example, the molar ratio may be 95% or more.

[0015] In order to enhance the ionic conductivity of the solid electrolyte material, the solid electrolyte material according to the first embodiment may consist of only Li, M, O, X, and F.

[0016] In order to enhance the ionic conductivity of the solid electrolyte material, in the solid electrolyte material according to the first embodiment, X may contain Cl. Desirably, X may be Cl.

[0017] The solid electrolyte material according to the first embodiment may contain a first crystalline phase having a peak in an X-ray diffraction pattern in a first range of a diffraction angle 2θ of 13.7° to 14.8°, for example, in a range of 13.7° to 13.96°.

[0018] The first crystal phase has high lithium ion conductivity. The solid electrolyte material according to the first embodiment contains the first crystal phase, which makes it easier for paths for lithium ions to diffuse. As a result, the solid electrolyte material according to the first embodiment has high lithium ion conductivity.

[0019] The X-ray diffraction pattern of the solid electrolyte material according to the first embodiment can be obtained by X-ray diffraction measurement by the θ-2θ method using Cu-Kα radiation (wavelengths of 1.5405 Å and 1.5444 Å, ie, wavelengths of 0.15405 nm and 0.15444 nm).

[0020] The diffraction angle of a peak in an X-ray diffraction pattern is defined as the angle at which the signal-to-noise ratio (i.e., the ratio of the signal S to the background noise N) is 3 or more and the peak width is 10° or less, showing the maximum intensity. MAX When the intensity is I MAX This is the width expressed as the difference between the two diffraction angles that are half the value of

[0021] In the X-ray diffraction pattern of the solid electrolyte material according to the first embodiment, a peak derived from the first crystal phase may further exist in a second range of a diffraction angle 2θ of 24.0° or more and 25.3° or less. The peak may exist, for example, in a range of 24.84° or more and 24.98° or less. Such a first crystal phase has a higher lithium ion conductivity. Therefore, the solid electrolyte material containing the first crystal phase has a higher lithium ion conductivity.

[0022] In the solid electrolyte material according to the first embodiment, the molar ratio of F to the sum of X and F may be 1% or more and 50% or less. The molar ratio of F to the sum of X and F is calculated by the formula: {(amount of substance of F) / (total amount of substance of all elements constituting X+amount of substance of F)}×100. Hereinafter, the molar ratio of F to the sum of X and F will be referred to as "molar ratio F / (X+F)".

[0023] The solid electrolyte material according to the first embodiment contains fluorine and therefore has high electrochemical stability. That is, the solid electrolyte material according to the first embodiment has high reduction resistance. When the molar ratio F / (X+F) is 1% or more and 50% or less, the solid electrolyte material according to the first embodiment can maintain high ionic conductivity and improve electrochemical stability. That is, by virtue of the configuration in which the molar ratio F / (X+F) is 1% or more and 50% or less, the solid electrolyte material according to the first embodiment has both high ionic conductivity and high electrochemical stability.

[0024] In order to further increase the ionic conductivity of the solid electrolyte material, in the solid electrolyte material according to the first embodiment, the molar ratio F / (X+F) may be 1% or more and 10% or less. For example, the molar ratio F / (X+F) may be 1% or more and 4% or less.

[0025] In order to further enhance the electrochemical stability of the solid electrolyte material, in the solid electrolyte material according to the first embodiment, the molar ratio F / (X+F) may be 10% or more and 50% or less.

[0026] In order to further increase the ion conductivity of the solid electrolyte material, the solid electrolyte material according to the first embodiment may further include a second crystal phase different from the first crystal phase. That is, the solid electrolyte material according to the first embodiment may further include a second crystal phase having a peak at a diffraction angle 2θ different from the peak of the first crystal phase in the X-ray diffraction pattern. When the solid electrolyte material according to the first embodiment further includes a second crystal phase in addition to the first crystal phase, it is considered that the second crystal phase promotes the conduction of lithium ions between the first crystal phases. Therefore, the lithium ion conductivity is further improved.

[0027] The shape of the solid electrolyte material according to the first embodiment is not limited. Examples of the shape are needle-like, spherical, and elliptical. The solid electrolyte material according to the first embodiment may be in the form of particles. The solid electrolyte material according to the first embodiment may be formed to have a pellet or plate shape.

[0028] When the solid electrolyte material according to the first embodiment has a particulate shape (for example, a spherical shape), the solid electrolyte material may have a median diameter of 0.1 μm or more and 100 μm or less, or may have a median diameter of 0.5 μm or more and 10 μm or less. This allows the solid electrolyte material according to the first embodiment and other materials to be dispersed well. The median diameter of the particles means a particle diameter (d50) corresponding to a volume cumulative 50% in a volume-based particle size distribution. The volume-based particle size distribution can be measured by a laser diffraction measurement device or an image analysis device.

[0029] When the solid electrolyte material according to the first embodiment has a particulate (e.g., spherical) shape, the solid electrolyte material may have a smaller median diameter than the active material, which allows the solid electrolyte material according to the first embodiment and the active material to form a good dispersion state.

[0030] <Method of manufacturing solid electrolyte material> The solid electrolyte material according to the first embodiment can be produced by the following method.

[0031] A raw material powder is prepared to have a desired composition, for example an oxide, hydroxide, halide, or oxyhalide.

[0032] As an example, in a solid electrolyte material composed of Li, M, O, X, and F, M is Ta, X is Cl, and the molar ratios Li / M, O / (F+X), and F / (F+X) at the time of mixing the raw materials are 1.0, 0.2, and 0.1, respectively, Li2O2, TaCl5, and TaF5 are mixed in a Li2O2:TaCl5:TaF5 molar ratio of 1:1.8:0.2. M and X are determined by the selection of the raw material powder. The molar ratios of Li / M, O / (F+X), and F / (F+X) are determined by selecting the mixing ratio of the raw material powder.

[0033] The mixture of raw material powders is reacted with each other mechanochemically (by the method of mechanochemical milling) in a mixing device such as a planetary ball mill to obtain a reactant. The reactant may be sintered in a vacuum or in an inert atmosphere. Alternatively, the mixture may be sintered in a vacuum or in an inert gas atmosphere to obtain a reactant. By these methods, the solid electrolyte material according to the first embodiment is obtained. The inert atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere.

[0034] Sintering of the solid electrolyte material may cause a part of M or a part of X to evaporate. As a result, the molar ratios Li / M and O / (F+X) of the obtained solid electrolyte material may be larger than the values ​​calculated from the molar ratios of the prepared raw material powders. Specifically, the molar ratio Li / M may be about 20% larger, and the molar ratio O / (F+X) may be about 40% to 75% larger.

[0035] By selecting the raw material powders, the mixing ratio of the raw material powders, and the reaction conditions, the position of the X-ray diffraction peak in the solid electrolyte material according to the first embodiment, that is, the structure of the crystal phase, can be adjusted to a desired one.

[0036] The composition of the solid electrolyte material is determined by, for example, ICP emission spectroscopy, ion chromatography, inert gas fusion-infrared absorption spectroscopy, or EPMA (Electron Probe Micro Analyzer) method.

[0037] Second embodiment The second embodiment will be described below. The matters described in the first embodiment will be omitted as appropriate.

[0038] The battery according to the second embodiment includes a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is disposed between the positive electrode and the negative electrode. At least one selected from the group consisting of the positive electrode, the electrolyte layer, and the negative electrode contains the solid electrolyte material according to the first embodiment.

[0039] The battery according to the second embodiment has excellent charge / discharge characteristics.

[0040] FIG. 1 shows a cross-sectional view of a battery 1000 according to a second embodiment.

[0041] The battery 1000 includes a positive electrode 201, an electrolyte layer 202, and a negative electrode 203. The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203.

[0042] The positive electrode 201 contains positive electrode active material particles 204 and solid electrolyte particles 100 .

[0043] The electrolyte layer 202 contains an electrolyte material, for example, a solid electrolyte material.

[0044] The negative electrode 203 contains negative electrode active material particles 205 and solid electrolyte particles 100 .

[0045] The solid electrolyte particle 100 is a particle containing the solid electrolyte material according to the first embodiment. The solid electrolyte particle 100 may be a particle containing the solid electrolyte material according to the first embodiment as a main component. A particle containing the solid electrolyte material according to the first embodiment as a main component means a particle in which the most abundant component is the solid electrolyte material according to the first embodiment. The solid electrolyte particle 100 may be a particle made of the solid electrolyte material according to the first embodiment.

[0046] The positive electrode 201 contains a material capable of absorbing and releasing metal ions such as lithium ions. The positive electrode 201 contains, for example, a positive electrode active material (for example, positive electrode active material particles 204).

[0047] Examples of the positive electrode active material include a lithium-containing transition metal oxide, a transition metal fluoride, a polyanion material, a fluorinated polyanion material, a transition metal sulfide, a transition metal oxysulfide, or a transition metal oxynitride. Examples of the lithium-containing transition metal oxide include Li(NiCoAl)O2, Li(NiCoMn)O2, or LiCoO2.

[0048] From the viewpoints of battery cost and safety, lithium phosphate may be used as the positive electrode active material.

[0049] When the positive electrode 201 contains the solid electrolyte material according to the first embodiment and X contains I (i.e., iodine), lithium iron phosphate may be used as the positive electrode active material. The solid electrolyte material according to the first embodiment containing I is easily oxidized. If lithium iron phosphate is used as the positive electrode active material, the oxidation reaction of the solid electrolyte material is suppressed. That is, the formation of an oxide layer having low lithium ion conductivity is suppressed. As a result, the battery has high charge and discharge efficiency.

[0050] The positive electrode 201 may contain not only the solid electrolyte material according to the first embodiment but also a transition metal oxyfluoride as the positive electrode active material. Even if the solid electrolyte material according to the first embodiment is fluorinated by a transition metal fluoride, it is difficult to form a resistance layer. As a result, the battery has high charge and discharge efficiency.

[0051] The transition metal oxyfluoride contains oxygen and fluorine. As an example, the transition metal oxyfluoride may be a compound represented by the composition formula Li p Me q O m F n . Here, Me is at least one element selected from the group consisting of Mn, Co, Ni, Fe, Al, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si, and P, and the following mathematical formulas: 0.5 ≦ p ≦ 1.5, 0.5 ≦ q ≦ 1.0, 1 ≦ m < 2, and 0 < n ≦ 1 are satisfied. An example of such a transition metal oxyfluoride is Li 1.05 (Ni 0.35 Co 0.35 Mn 0.3 ) 0.95 O 1.9 F 0.1 .

[0052] The positive electrode active material particles 204 may have a median diameter of 0.1 μm or more and 100 μm or less. When the positive electrode active material particles 204 have a median diameter of 0.1 μm or more, the positive electrode active material particles 204 and the solid electrolyte particles 100 can form a good dispersion state in the positive electrode 201. This improves the charge / discharge characteristics of the battery. When the positive electrode active material particles 204 have a median diameter of 100 μm or less, the lithium diffusion speed in the positive electrode active material particles 204 improves. This allows the battery to operate at high output.

[0053] The positive electrode active material particles 204 may have a larger median diameter than the solid electrolyte particles 100. This allows the positive electrode active material particles 204 and the solid electrolyte particles 100 to form a well-dispersed state.

[0054] From the viewpoint of the energy density and output of the battery, in the positive electrode 201, the ratio of the volume of the positive electrode active material particles 204 to the total volume of the positive electrode active material particles 204 and the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.

[0055] 2 shows a cross-sectional view of an electrode material 1100 according to a second embodiment. The electrode material 1100 is included in, for example, a positive electrode 201. A coating layer 216 may be formed on the surface of the electrode active material particle 206 to prevent the electrode active material particle 206 from reacting with the solid electrolyte particle 100. This makes it possible to suppress an increase in the reaction overvoltage of the battery. Examples of the coating material included in the coating layer 216 include a sulfide solid electrolyte, an oxide solid electrolyte, or a halide solid electrolyte.

[0056] When the solid electrolyte particle 100 is a sulfide solid electrolyte, the coating material may be the solid electrolyte material according to the first embodiment, and X may be at least one element selected from the group consisting of Cl and Br. Such a solid electrolyte material according to the first embodiment is less susceptible to oxidation than the sulfide solid electrolyte. As a result, the increase in the reaction overvoltage of the battery can be suppressed.

[0057] When the solid electrolyte particle 100 is the solid electrolyte material according to the first embodiment and X contains I, the coating material may be the solid electrolyte material according to the first embodiment and X may be at least one element selected from the group consisting of Cl and Br. The solid electrolyte material according to the first embodiment that does not contain I is less susceptible to oxidation than the solid electrolyte material according to the first embodiment that contains I. As a result, the battery has high charge / discharge efficiency.

[0058] When the solid electrolyte particle 100 is the solid electrolyte material according to the first embodiment and X includes I, the coating material may include an oxide solid electrolyte. The oxide solid electrolyte may be lithium niobate, which has excellent stability even at high potentials, so that the battery has high charge / discharge efficiency.

[0059] The positive electrode 201 may be composed of a first positive electrode layer containing a first positive electrode active material and a second positive electrode layer containing a second positive electrode active material. Here, the second positive electrode layer is disposed between the first positive electrode layer and the electrolyte layer 202, the first positive electrode layer and the second positive electrode layer contain a solid electrolyte material according to the first embodiment containing I, and a coating layer 216 is formed on the surface of the second positive electrode active material. According to the above configuration, the solid electrolyte material according to the first embodiment contained in the electrolyte layer 202 can be suppressed from being oxidized by the second positive electrode active material. As a result, the battery has a high charging capacity. Examples of the coating material contained in the coating layer 206 are a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, or a halide solid electrolyte. However, when the coating material is a halide solid electrolyte, it does not contain I as a halogen element. The first positive electrode active material may be the same material as the second positive electrode active material, or may be a material different from the second positive electrode active material.

[0060] From the viewpoint of the energy density and output of the battery, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.

[0061] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte material. The electrolyte layer 202 may be a solid electrolyte layer. The solid electrolyte material contained in the electrolyte layer 202 may contain the solid electrolyte material according to the first embodiment. The solid electrolyte material contained in the electrolyte layer 202 may consist only of the solid electrolyte material according to the first embodiment.

[0062] The solid electrolyte material contained in the electrolyte layer 202 may be composed only of a solid electrolyte material different from the solid electrolyte material according to the first embodiment. Examples of the solid electrolyte material different from the solid electrolyte material according to the first embodiment include Li2MgX'4, Li2FeX'4, Li(Al, Ga, In)X'4, Li3(Al, Ga, In)X'6, or LiI. Here, X' is at least one element selected from the group consisting of F, Cl, Br, and I.

[0063] Hereinafter, the solid electrolyte material according to the first embodiment will be referred to as a first solid electrolyte material, and a solid electrolyte material different from the solid electrolyte material according to the first embodiment will be referred to as a second solid electrolyte material.

[0064] The electrolyte layer 202 may contain not only the first solid electrolyte material but also the second solid electrolyte material. The first solid electrolyte material and the second solid electrolyte material may be uniformly dispersed.

[0065] The electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less. When the electrolyte layer 202 has a thickness of 1 μm or more, the positive electrode 201 and the negative electrode 203 are less likely to short-circuit. When the electrolyte layer 202 has a thickness of 100 μm or less, the battery can operate at high output.

[0066] Another electrolyte layer may be further provided between the electrolyte layer 202 and the negative electrode 203. For example, when the electrolyte layer 202 includes a first solid electrolyte material, an electrolyte layer made of another solid electrolyte material that is electrochemically more stable than the first solid electrolyte material may be further provided in order to more stably maintain the high ionic conductivity of the solid electrolyte material.

[0067] The negative electrode 203 contains a material capable of absorbing and releasing metal ions (for example, lithium ions). The negative electrode 203 contains, for example, a negative electrode active material (for example, negative electrode active material particles 205).

[0068] Examples of the negative electrode active material are metal materials, carbon materials, oxides, nitrides, tin compounds, or silicides. The metal material may be a single metal or an alloy. Examples of the metal material are lithium metal or a lithium alloy. Examples of the carbon material are natural graphite, coke, partially graphitized carbon, carbon fiber, spherical carbon, artificial graphite, or amorphous carbon. From the viewpoint of capacity density, suitable examples of the negative electrode active material are silicon (i.e., Si), tin (i.e., Sn), silicides, or tin compounds.

[0069] The negative electrode active material may be selected based on the reduction resistance of the solid electrolyte material contained in the negative electrode 203. When the negative electrode 203 contains a first solid electrolyte material, a material capable of absorbing and releasing lithium ions at 0.27 V or more relative to lithium may be used as the negative electrode active material. If the negative electrode active material is such a material, it is possible to suppress the reduction of the first solid electrolyte material contained in the negative electrode 203. As a result, the battery has high charge and discharge efficiency. Examples of such materials are titanium oxide, indium metal, or lithium alloy. An example of titanium oxide is Li4Ti5O 12 , LiTi2O4, or TiO2.

[0070] The negative electrode active material particles 205 may have a median diameter of 0.1 μm or more and 100 μm or less. When the negative electrode active material particles 205 have a median diameter of 0.1 μm or more, the negative electrode active material particles 205 and the solid electrolyte particles 100 can form a good dispersion state in the negative electrode 203. This improves the charge and discharge characteristics of the battery. When the negative electrode active material particles 205 have a median diameter of 100 μm or less, the lithium diffusion speed in the negative electrode active material particles 205 improves. This allows the battery to operate at a high output.

[0071] The negative electrode active material particles 205 may have a larger median diameter than the solid electrolyte particles 100. This allows the negative electrode active material particles 205 and the solid electrolyte particles 100 to form a well-dispersed state.

[0072] From the viewpoint of the energy density and output of the battery, in the negative electrode 203, the ratio of the volume of the negative electrode active material particles 205 to the total volume of the negative electrode active material particles 205 and the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.

[0073] The electrode material 1100 shown in FIG. 2 may be contained in the negative electrode 203. In order to prevent the solid electrolyte particles 100 from reacting with the negative electrode active material (i.e., the electrode active material particles 206), a coating layer 216 may be formed on the surface of the electrode active material particles 206. This allows the battery to have high charge / discharge efficiency. Examples of the coating material contained in the coating layer 216 include a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, or a halide solid electrolyte.

[0074] When the solid electrolyte particle 100 is the first solid electrolyte material, the coating material may be a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer solid electrolyte. An example of a sulfide solid electrolyte is Li2S-P2S5. An example of an oxide solid electrolyte is trilithium phosphate. An example of a polymer solid electrolyte is a composite compound of polyethylene oxide and a lithium salt. An example of such a polymer solid electrolyte is lithium bis(trifluoromethanesulfonyl)imide.

[0075] From the viewpoint of the energy density and output of the battery, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.

[0076] At least one selected from the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a second solid electrolyte material for the purpose of increasing ion conductivity. Examples of the second solid electrolyte material include a sulfide solid electrolyte, an oxide solid electrolyte, a halide solid electrolyte, or an organic polymer solid electrolyte.

[0077] In the present disclosure, a "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur. An "oxide solid electrolyte" refers to a solid electrolyte containing oxygen. The oxide solid electrolyte may contain anions other than oxygen (excluding sulfur anions and halogen anions). A "halide solid electrolyte" refers to a solid electrolyte containing a halogen element and not containing sulfur. The halide solid electrolyte may contain not only a halogen element but also oxygen.

[0078] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4, or Li 10 GeP2S 12 It is.

[0079] Examples of oxide solid electrolytes include: (i) NASICON-type solid electrolytes such as LiTi2(PO4)3 or elemental substitutions thereof; (ii) Perovskite-type solid electrolytes such as (LaLi)TiO3; (iii) Li 14 ZnGeO 16 LISICON-type solid electrolytes such as Li4SiO4, LiGeO4 or elemental substitutes thereof; (iv) Li7La3Zr2O 12 or a garnet-type solid electrolyte such as an elemental substitution product thereof; or (v) Li3PO4 or its N-substituted derivatives It is.

[0080] An example of a halide solid electrolyte is Li a Me' b Y cZ6, where the formula: a+mb+3c=6, and c>0 is satisfied. Me' is at least one selected from the group consisting of metal elements other than Li and Y and metalloid elements. Z is at least one element selected from the group consisting of F, Cl, Br, and I. The value of m represents the valence of Me'.

[0081] The "metalloid elements" are B, Si, Ge, As, Sb, and Te. The "metal elements" are all elements in groups 1 to 12 of the periodic table (except hydrogen) and all elements in groups 13 to 16 of the periodic table (except B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se). Me' may be at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.

[0082] Examples of halide solid electrolytes are Li3YCl6 or Li3YBr6.

[0083] When the electrolyte layer 202 contains the first solid electrolyte material, the negative electrode 203 may contain a sulfide solid electrolyte. This allows the sulfide solid electrolyte, which is electrochemically stable with respect to the negative electrode active material, to prevent the first solid electrolyte material and the negative electrode active material from contacting each other. As a result, the battery has low internal resistance.

[0084] An example of the organic polymer solid electrolyte is a compound of a polymer compound and a lithium salt. The polymer compound may have an ethylene oxide structure. The polymer compound having an ethylene oxide structure can contain a large amount of lithium salt, and therefore has a higher ionic conductivity.

[0085] Examples of the lithium salt are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.

[0086] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a nonaqueous electrolyte solution, a gel electrolyte, or an ionic liquid for the purpose of facilitating the exchange of lithium ions and improving the output characteristics of the battery.

[0087] The non-aqueous electrolyte includes a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent are a cyclic carbonate ester solvent, a chain carbonate ester solvent, a cyclic ether solvent, a chain ether solvent, a cyclic ester solvent, a chain ester solvent, or a fluorine solvent. Examples of the cyclic carbonate ester solvent are ethylene carbonate, propylene carbonate, or butylene carbonate. Examples of the chain carbonate ester solvent are dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. Examples of the cyclic ether solvent are tetrahydrofuran, 1,4-dioxane, or 1,3-dioxolane. Examples of the chain ether solvent are 1,2-dimethoxyethane or 1,2-diethoxyethane. Examples of the cyclic ester solvent are γ-butyrolactone. Examples of the chain ester solvent are methyl acetate. Examples of fluorine-containing solvents include fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate. One non-aqueous solvent selected from these may be used alone. Alternatively, a mixture of two or more non-aqueous solvents selected from these may be used.

[0088] Examples of the lithium salt are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), or LiC(SO2CF3)3. One type of lithium salt selected from these may be used alone. Alternatively, a mixture of two or more types of lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 mol / liter to 2 mol / liter.

[0089] The gel electrolyte may be a polymer material impregnated with a non-aqueous electrolyte, such as polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.

[0090] Examples of cations contained in ionic liquids are: (i) Aliphatic chain quaternary salts such as tetraalkylammonium or tetraalkylphosphonium salts, (ii) aliphatic cyclic ammonium such as pyrrolidiniums, morpholiniums, imidazoliniums, tetrahydropyrimidiniums, piperaziniums, or piperidiniums, or (iii) nitrogen-containing heterocyclic aromatic cations such as pyridiniums or imidazoliums It is.

[0091] An example of an anion contained in an ionic liquid is PF6 - , BF4 - , SbF6 - , AsF6 - , SO3CF3 - , N(SO2CF3)2 - , N(SO2C2F5)2 - , N(SO2CF3)(SO2C4F9) - , or C(SO2CF3)3 - It is.

[0092] The ionic liquid may contain a lithium salt.

[0093] At least one selected from the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a binder for the purpose of improving adhesion between particles.

[0094] Examples of the binder include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylic acid methyl ester, polyacrylic acid ethyl ester, polyacrylic acid hexyl ester, polymethacrylic acid, polymethacrylic acid methyl ester, polymethacrylic acid ethyl ester, polymethacrylic acid hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene butadiene rubber, and carboxymethylcellulose. A copolymer may be used as the binder. An example of the binder is a copolymer of two or more materials selected from the group consisting of tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. A mixture of two or more materials selected from the above materials may be used.

[0095] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive assistant for the purpose of increasing electronic conductivity.

[0096] Examples of the conductive additive include: (i) Graphites, such as natural or synthetic graphite; (ii) Carbon blacks such as acetylene black or ketjen black; (iii) conductive fibers, such as carbon or metal fibers; (iv) fluorocarbons, (v) Metal powders such as aluminum; (vi) conductive whiskers such as zinc oxide or potassium titanate; (vii) a conductive metal oxide, such as titanium dioxide; or (viii) Conductive polymers such as polyaniline, polypyrrole, or polythiophene In order to reduce costs, the above-mentioned conductive assistant (i) or (ii) may be used.

[0097] Examples of shapes of the battery according to the second embodiment are a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, and a laminate type. EXAMPLES

[0098] Hereinafter, the present disclosure will be described in more detail using examples.

[0099] Example 1 [Preparation of solid electrolyte materials] In a dry atmosphere having a dew point of -30°C or less (hereinafter referred to as "dry atmosphere"), Li2O2, TaCl5 and TaF5 were prepared as raw material powders in a molar ratio of Li2O2:TaCl5:TaF5 of 1:1.9:0.1. These raw material powders were ground and mixed in a mortar to obtain a mixed powder. The obtained mixed powder was milled at 600 rpm for 24 hours using a planetary ball mill (Fritsch, P-7 type). The mixed powder was then fired at 200°C for 6 hours. In this manner, a powder of the solid electrolyte material according to Example 1 containing a crystalline phase consisting of Li, Ta, O, Cl, and F was obtained.

[0100] [Evaluation of ionic conductivity] FIG. 3 shows a schematic diagram of a pressing die 300 used to evaluate the ionic conductivity of the solid electrolyte material.

[0101] The pressure molding die 300 had an upper punch 301, a frame 302, and a lower punch 303. The frame 302 was made of insulating polycarbonate. Both the upper punch 301 and the lower punch 303 were made of electronically conductive stainless steel.

[0102] Using the pressure molding die 300 shown in FIG. 3, the ionic conductivity of the solid electrolyte material according to Example 1 was measured by the following method.

[0103] In a dry atmosphere, the powder of the solid electrolyte material according to Example 1 (i.e., the powder of the solid electrolyte material 101 in FIG. 3) was filled into the inside of the pressure molding die 300. In the inside of the pressure molding die 300, a pressure of 300 MPa was applied to the solid electrolyte material according to Example 1 using the upper punch 301.

[0104] While the pressure was applied, the punch was connected to a potentiostat (Princeton Applied Research VersaSTAT4) equipped with a frequency response analyzer via the upper punch 301 and the lower punch 303. The upper punch 301 was connected to a working electrode and a terminal for measuring potential. The lower punch 303 was connected to a counter electrode and a reference electrode. The ionic conductivity of the solid electrolyte material according to Example 1 was measured at room temperature by an electrochemical impedance measurement method. As a result, the ionic conductivity measured at 22°C was 7.7 mS / cm.

[0105] [X-ray diffraction] Figure 4 is a graph showing the X-ray diffraction pattern of the solid electrolyte material according to Example 1. The results shown in Figure 4 were measured by the following method.

[0106] The X-ray diffraction pattern of the solid electrolyte material according to Example 1 was measured using an X-ray diffractometer (RIGAKU, MiniFlex600) in a dry atmosphere having a dew point of -45°C or less. Cu-Kα radiation (wavelengths 1.5405 Å and 1.5444 Å) was used as the X-ray source.

[0107] The solid electrolyte material according to Example 1 had diffraction peaks at 13.70° (i.e., the first range) and 25.30° (i.e., the second range). Therefore, the solid electrolyte material according to Example 1 contained a first crystal phase having high lithium ion conductivity.

[0108] The solid electrolyte material according to Example 1 also had a diffraction peak derived from LiCl. Therefore, the solid electrolyte material according to Example 1 also contained a second crystal phase.

[0109] [Evaluation of reduction resistance] The reduction resistance of the solid electrolyte material was evaluated based on the onset voltage of the reduction reaction of the solid electrolyte material (hereinafter referred to as the "reduction onset voltage"). The reduction onset voltage of the solid electrolyte material was determined by cyclic voltammetry measurement (hereinafter referred to as the CV measurement).

[0110] Fig. 6A is a graph showing the results of CV measurement of the solid electrolyte material according to Example 1. The results shown in Fig. 6A were measured by the following method.

[0111] In an insulating cylinder having an inner diameter of 9.5 mm, the solid electrolyte material (120 mg, thickness: 500 μm) according to Example 1 and a sulfide solid electrolyte (50 mg) were laminated in this order to obtain a laminate. Li2S-P2S5 was used as the sulfide solid electrolyte. A pressure of 360 MPa was applied to this laminate to form a solid electrolyte layer.

[0112] Next, Li metal (thickness: 300 μm) was laminated on the solid electrolyte layer formed from the sulfide solid electrolyte, and a pressure of 80 MPa was applied to this laminate.

[0113] Next, current collectors made of stainless steel were placed on the top and bottom of the laminate, and current collecting leads were attached to the current collectors.

[0114] In this manner, the CV measurement cell according to Example 1 was obtained.

[0115] The obtained CV measurement cell was placed in a thermostatic chamber at 25°C. A voltage was applied to Li from the open circuit voltage (i.e., OCV) to 0.5 V at a scanning voltage rate of -2 mV / sec. When the solid electrolyte material is reduced, a current accompanying the reduction reaction is observed. The reduction onset voltage is the ratio of the current I x is defined as the voltage at which I0 is 10 times or more. In the case of the above measurement method, the current value is a negative value. Figure 6C is a graph for explaining the reduction onset voltage obtained from the results of CV measurement.

[0116] In the solid electrolyte material according to Example 1, I0 is 3.0 × 10 -7 A, and the reduction onset voltage was 2.3V.

[0117] [Battery construction] In an argon atmosphere having a dew point of -60°C or less, the solid electrolyte material according to Example 1 and the positive electrode active material LiCoO2 were prepared in a volume ratio of 50:50. These materials were mixed in a mortar to obtain a positive electrode mixture.

[0118] In an insulating cylinder having an inner diameter of 9.5 mm, the solid electrolyte material (120 mg, thickness: 500 μm) according to Example 1 and the above positive electrode mixture (10.6 mg) were laminated in this order to obtain a laminate. A pressure of 360 MPa was applied to this laminate to form a solid electrolyte layer and a first electrode.

[0119] Next, a Li-In alloy having a thickness of 200 μm was laminated on the solid electrolyte layer, and a pressure of 80 MPa was applied to this laminate to form a second electrode.

[0120] The first electrode was the positive electrode and the second electrode was the negative electrode.

[0121] A current collector formed from stainless steel was attached to the first and second electrodes, and a current collecting lead was attached to the current collector.

[0122] Finally, an insulating ferrule was used to isolate the inside of the insulating tube from the outside atmosphere, and the inside of the tube was sealed.

[0123] In this manner, the battery according to Example 1 was obtained.

[0124] [Charge / discharge test] Fig. 7 is a graph showing the initial discharge characteristics of the battery according to Example 1. The results shown in Fig. 7 were measured by the following method.

[0125] The battery according to Example 1 was placed in a thermostatic chamber at 25° C. The battery according to Example 1 was charged at a current value of 56 μA until a voltage of 3.6 V was reached. The current density corresponds to a 0.05 C rate. The battery was then discharged at a current value of 56 μA until a voltage of 2.5 V was reached. The battery according to Example 1 was charged and discharged at room temperature.

[0126] As a result of the charge / discharge test, the battery according to Example 1 had an initial discharge capacity of 0.80 mAh.

[0127] (Examples 2 to 6) [Preparation of solid electrolyte materials] In Example 2, Li2O2, TaCl5, and TaF5 were prepared as raw material powders so that the molar ratio of Li2O2:TaCl5:TaF5 was 1:1.8:0.2.

[0128] In Example 3, Li2O2, TaCl5, and TaF5 were prepared as raw material powders in a molar ratio of Li2O2:TaCl5:TaF5 of 1:1:1.

[0129] In Example 4, Li2O2, NbCl5, and NbF5 were prepared as raw material powders so that the molar ratio of Li2O2:NbCl5:NbF5 was 1:1.9:0.1.

[0130] In Example 5, Li2O2, NbCl5, and NbF5 were prepared as raw material powders in a molar ratio of Li2O2:NbCl5:NbF5 of 1:1.8:0.2.

[0131] In Example 6, Li2O2, NbCl5, and NbF5 were prepared as raw material powders in a molar ratio of Li2O2:NbCl5:NbF5 of 1:1:1.

[0132] Except for the above, the solid electrolyte materials according to Examples 2 to 6 were obtained in the same manner as in Example 1.

[0133] Example 7 In a dry atmosphere having a dew point of -30°C or less (hereinafter referred to as "dry atmosphere"), Li2O2, TaCl5, and TaF5 were prepared as raw material powders so as to have a molar ratio of Li2O2:TaCl5:TaF5 of 1:1.98:0.02. These raw material powders were mixed in a mortar to obtain a mixed powder. The obtained mixed powder was sealed in a container made of quartz glass and filled with argon gas, and was fired at 350°C for 6 hours. In this manner, a powder of the solid electrolyte material according to Example 7 containing a crystalline phase consisting of Li, Ta, O, Cl, and F was obtained.

[0134] (Examples 8 to 11) In Example 8, Li2O2, TaCl5, and TaF5 were prepared as raw material powders so that the molar ratio of Li2O2:TaCl5:TaF5 was 1:1.96:0.04.

[0135] In Example 9, Li2O2, TaCl5, and TaF5 were prepared as raw material powders in a molar ratio of Li2O2:TaCl5:TaF5 of 1:1.94:0.06.

[0136] In Example 10, Li2O2, TaCl5, and TaF5 were prepared as raw material powders in a molar ratio of Li2O2:TaCl5:TaF5 of 1:1.92:0.08.

[0137] In Example 11, Li2O2, TaCl5, NbCl5, and TaF5 were prepared as raw material powders in a molar ratio of Li2O2:TaCl5:NbCl5:TaF5 of 1:0.92:1:0.08.

[0138] Except for the above, the solid electrolyte materials according to Examples 8 to 11 were obtained in the same manner as in Example 1.

[0139] (Comparative Examples 1 and 2) In Comparative Example 1, LiCl, Li2O2, and LiF were prepared as raw material powders so that the molar ratio of LiCl:Li2O2:LiF was 0.9:1:0.1.

[0140] In Comparative Example 2, LiCl, TaCl5, and LiF were prepared as raw material powders so that the molar ratio of LiCl:TaCl5:LiF was 0.4:1:0.6.

[0141] Except for the above, the solid electrolyte materials according to Comparative Examples 1 and 2 were obtained in the same manner as in Example 1.

[0142] [Evaluation of ionic conductivity] The ionic conductivity of the solid electrolyte materials according to Examples 2 to 11 and Comparative Examples 1 and 2 was measured in the same manner as in Example 1. The measurement results are shown in Tables 1 and 2.

[0143] [X-ray diffraction] The X-ray diffraction patterns of the solid electrolyte materials according to Examples 2 to 11 and Comparative Examples 1 and 2 were measured in the same manner as in Example 1. The measurement results are shown in FIGS.

[0144] The solid electrolyte material according to Example 2 had diffraction peaks at 13.74° (i.e., the first range) and 24.52° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0145] The solid electrolyte material according to Example 3 did not have any diffraction peaks in the first and second ranges.

[0146] The solid electrolyte material according to Example 4 had diffraction peaks at 13.86° (i.e., the first range) and 24.55° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0147] The solid electrolyte material according to Example 5 had diffraction peaks at 13.96° (i.e., the first range) and 24.56° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0148] The solid electrolyte material according to Example 6 had diffraction peaks at 14.79° (ie, the first range) and 24.02° (ie, the second range).

[0149] The solid electrolyte material according to Example 7 had diffraction peaks at 13.84° (i.e., the first range) and 24.90° (i.e., the second range), and further had diffraction peaks derived from LiCl.

[0150] The solid electrolyte material according to Example 8 had diffraction peaks at 13.83° (i.e., the first range) and 24.89° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0151] The solid electrolyte material according to Example 9 had diffraction peaks at 13.88° (i.e., the first range) and 24.93° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0152] The solid electrolyte material according to Example 10 had diffraction peaks at 13.84° (i.e., the first range) and 24.89° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0153] The solid electrolyte material according to Example 11 had diffraction peaks at 13.90° (i.e., the first range) and 24.93° (i.e., the second range). In addition, a diffraction peak due to LiCl was also observed.

[0154] Thus, the solid electrolyte materials according to Examples 2 and 4 to 11 contained a first crystalline phase. The solid electrolyte materials according to Examples 2, 4 and 5 to 11 also contained a second crystalline phase.

[0155] [Evaluation of reduction resistance] CV measurements were carried out on the solid electrolyte materials according to Examples 2 to 4 in the same manner as in Example 1. The measurement results are shown in FIGS.

[0156] In Example 2, I0 is 3.6 x 10 -7 A, and the reduction onset voltage was 2.2V.

[0157] In Example 3, I0 is 2.6 x 10 -7 A, and the reduction onset voltage was 2.0V.

[0158] In Example 4, I0 is 5.1 x 10 -7 A, and the reduction onset voltage was 2.8V.

[0159] [Table 1]

[0160] [Table 2]

[0161] (Consideration) As is clear from Table 1, the solid electrolyte materials according to Examples 1 to 11 have a melting point of 1×10 -3 The solid electrolyte material has a high ionic conductivity of at least mS / cm. As is clear from the reduction onset voltages of the solid electrolyte materials according to Examples 1 to 4, the solid electrolyte material containing Li, M, O, X, and F has high electrochemical stability.

[0162] As is clear from a comparison between Examples 1 to 3, as the molar ratio F / (X+F) increases, the reduction onset voltage decreases. In other words, as the molar ratio F / (X+F) increases, the electrochemical stability of the solid electrolyte material improves.

[0163] As is clear from a comparison of Examples 1, 2, and 7 to 10 with Example 3, when the molar ratio F / (X+F) is 1% or more and 10% or less, the ionic conductivity of the solid electrolyte material becomes higher.

[0164] As is clear from a comparison of Examples 2 and 3 with Example 1, when the molar ratio F / (X+F) is 10% or more and 50% or less, the electrochemical stability of the solid electrolyte material is higher.

[0165] The solid electrolyte materials according to Examples 1 to 11 do not contain sulfur and therefore do not generate hydrogen sulfide.

[0166] As described above, the solid electrolyte material according to the present disclosure has high lithium ion conductivity and is therefore suitable for providing a battery with excellent charge / discharge characteristics. [Industrial Applicability]

[0167] The battery of the present disclosure is used, for example, in an all-solid-state lithium ion secondary battery. [Explanation of symbols]

[0168] 100 solid electrolyte particles 101 Solid electrolyte material powder 201 Positive electrode 202 Electrolyte layer 203 Negative electrode 204 Positive electrode active material particles 205 Negative electrode active material particles 206 Electrode active material particles 216 Covering layer 300 Pressure forming die 301 Punch top 302 Frame type 303 Punch bottom 1000 Battery 1100 Electrode Material

Claims

1. Li, M, O, X, and F; Where: M is at least one element selected from the group consisting of Ta and Nb; X is at least one element selected from the group consisting of Cl, Br, and I; In an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, a first crystal phase is contained, in which a peak exists in a first range in which the value of the diffraction angle 2θ is 13.7° or more and 14.8° or less. Solid electrolyte material.

2. X contains Cl; The solid electrolyte material according to claim 1 .

3. In the X-ray diffraction pattern, a peak derived from the first crystal phase is further present in a second range where the value of the diffraction angle 2θ is 24.0° or more and 25.3° or less. The solid electrolyte material according to claim 1 .

4. The molar ratio of F to the sum of X and F is 1% or more and 50% or less; The solid electrolyte material according to claim 1 .

5. The molar ratio is 1% or more and 10% or less. The solid electrolyte material according to claim 4 .

6. The molar ratio is 10% or more and 50% or less. The solid electrolyte material according to claim 4 .

7. Further comprising a second crystal phase different from the first crystal phase; The solid electrolyte material according to claim 1 .

8. positive electrode, a negative electrode, and an electrolyte layer provided between the positive electrode and the negative electrode; Equipped with At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte layer contains the solid electrolyte material according to any one of claims 1 to 7. battery.

Citation Information

Patent Citations

  • Method of manufacturing sulfide solid electrolyte material, sulfide solid electrolyte material, and lithium battery

    JP2011129312A

  • Positive electrode active material and battery

    JP2019125574A

  • Solid electrolyte material and battery

    WO2019135348A1