Magnetic metamaterial, spin current control device and spin current control method

A magnetic metamaterial with controlled light irradiation enables precise control of spin current direction and magnitude, addressing limitations in existing spin current generation methods and enhancing spintronics applications.

JP7565563B2Active Publication Date: 2024-10-11TOHOKU UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023520945
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-14
Filing Date
2022-04-20
Publication Date
2024-10-11
Estimated Expiration
2042-04-20

AI Technical Summary

Technical Problem

Existing methods for generating and controlling spin current, such as the spin pumping effect, are limited in freely controlling the direction and magnitude of spin current.

Method used

A magnetic metamaterial with a perpendicularly magnetized film having periodic unit structures with three-fold rotational symmetry, which can be irradiated with light of controlled ellipticity and azimuth angles to control the spin current direction and magnitude using the magneto-optical galvano effect.

Benefits of technology

The magnetic metamaterial effectively controls the direction and magnitude of spin current, enabling applications in new spintronics devices like magnetic memories and thermoelectric conversion elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565563000004
    Figure 0007565563000004
  • Figure 0007565563000005
    Figure 0007565563000005
  • Figure 0007565563000006
    Figure 0007565563000006
Patent Text Reader

Abstract

This magnetic metamaterial includes a perpendicular magnetized film that is isotropic with respect to light, wherein: the perpendicular magnetized film includes a plurality of unit structures arranged periodically in an in-plane direction; and each of the plurality of unit structures has a size at most equal to the wavelength of radiated light, and has three-fold rotational symmetry.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic metamaterial, a spin current control device, and a spin current control method. This application claims priority based on Japanese Patent Application No. 2021-082127 filed in Japan on May 14, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, attention has been focused on spintronics. Spintronics is the engineering use of not only the charge degree of freedom of electrons in solids, but also their spin degree of freedom. Spintronics will contribute to the realization of new devices with functions and performance that could not be realized by electronics that only utilizes the charge degree of freedom.

[0003] Spin current is one of the elements used in spintronics. It is the difference between the current of spin-up electrons and spin-down electrons, and is called J S =J ↑ -J ↓ It is expressed as J S is the spin current, and J ↑ is the flow of electrons with spin up, and J ↓ is a flow of electrons with a downward spin. For example, Patent Document 1 describes that when a magnetic material is irradiated with microwaves, a spin current is generated due to the spin pumping effect. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-086448 A Summary of the Invention [Problem to be solved by the invention]

[0005] A spin current can also be generated by methods other than the spin pumping effect shown in Patent Document 1. For example, a spin current can be generated by the spin Hall effect caused by an electric current, the spin Seebeck effect caused by a heat current, the plasmonic spin pumping effect using light, the circularly polarized galvanic effect, etc. However, no matter which method is used, it is difficult to freely control the direction and magnitude of the generated spin current.

[0006] The present invention has been made in consideration of the above problems, and aims to provide a magnetic metamaterial, a spin current control device, and a spin current control method that are capable of controlling the direction and magnitude of a spin current. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides the following means.

[0008] (1) A magnetic metamaterial according to a first aspect has a perpendicular magnetization film that is isotropic with respect to light, the perpendicular magnetization film including a plurality of unit structures that are periodically arranged in an in-plane direction, each of the plurality of unit structures having a size equal to or smaller than the wavelength of the irradiated light and having three-fold rotational symmetry.

[0009] (2) In the magnetic metamaterial according to the above aspect, the perpendicular magnetization film may have a plurality of openings that form the plurality of unit structures.

[0010] (3) In the magnetic metamaterial according to the above aspect, each of the plurality of openings may be an equilateral triangle.

[0011] (4) A spin current control element according to a second aspect has a magnetic metamaterial according to the above aspect and a light irradiation unit that irradiates light onto the magnetic metamaterial, and the light irradiation unit can control the ellipticity angle and azimuth angle of the light irradiated onto the magnetic metamaterial.

[0012] (5) A method for controlling a spin current according to a third aspect includes a step of irradiating a magnetic metamaterial with light having a controlled ellipticity angle and azimuth angle, the magnetic metamaterial having a perpendicular magnetization film that is isotropic with respect to the light, the perpendicular magnetization film including a plurality of unit structures that are periodically arranged in an in-plane direction, each of the plurality of unit structures having a size equal to or smaller than the wavelength of the irradiated light and having three-fold rotational symmetry. Effect of the Invention

[0013] The magnetic metamaterial, the spin current control device, and the spin current control method according to the above aspects can control the direction and magnitude of the spin current. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a perspective view of a spin current control device according to a first embodiment. [Diagram 2] FIG. 1 is a perspective view of a magnetic metamaterial according to a first embodiment. [Diagram 3] FIG. 1 is a plan view of a magnetic metamaterial according to a first embodiment. [Figure 4] FIG. 13 is a plan view of a magnetic metamaterial according to a modified example. [Diagram 5] FIG. 2 is a conceptual diagram of an experimental system according to the first embodiment. [Figure 6] In Example 1, the response characteristics of the spin current generated after irradiating the magnetic metamaterial with laser light are shown. [Figure 7] In Example 1, the results of changing the intensity of the laser light irradiated onto the magnetic metamaterial are shown. [Figure 8] 1 shows the results of measuring the effect on the spin current when the magnetic field applied to the magnetic metamaterial is changed in Example 1. [Figure 9] 1 shows the results of measuring the direction of magnetization of a perpendicular magnetic film using the magnetic Faraday effect in Example 1. [Figure 10] FIG. 1 shows a comparison of the magnetization curves of a flat Co / Pt multilayer before the formation of multiple apertures and the magnetization curves of a magnetic metamaterial (MM). [Figure 11] These are the results of measuring the wavelength dependence of the transmittance (T), reflectance (R), and absorptance (A) of a magnetic metamaterial. [Figure 12] 1 shows the results of measuring the dependence of the magnitude of the spin current on the wavelength of the irradiated light in the experimental system of Example 1. [Figure 13] FIG. 1 is a conceptual diagram of an experimental system according to Example 2. [Figure 14] This shows the results when the azimuth angle θω of light irradiated to the magnetic metamaterial was changed in the experimental system of Example 2. [Figure 15] FIG. 13 is a conceptual diagram of an experimental system according to Example 3. [Figure 16] 13 shows the results of measuring the x and y components (Js,x, Js,y) of the magnitude of the spin current when the azimuth angle φω of the light irradiated to the optical element is changed in an experimental system according to Example 3. [Figure 17] This is a diagram in which the results of FIG. 16 are expressed as the relationship between the ellipticity angle εω and the magnitude of the spin current (|Js|). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.

[0016] First, the directions are defined. One direction within the plane in which the magnetic metamaterial 10 extends is defined as the x direction, the direction perpendicular to the x direction is defined as the y direction, and the direction perpendicular to the xy plane is defined as the z direction.

[0017] 1 is a perspective view of a spin current controlling device 100 according to the first embodiment. The spin current controlling device 100 has a magnetic metamaterial 10 and a light irradiation unit 20. The magnetic metamaterial may also be called a magnetic metamaterial or a magnetic metamaterial.

[0018] The light irradiating unit 20 irradiates the magnetic metamaterial 10 with light. The light irradiating unit 20 irradiates the magnetic metamaterial 10 with light, for example, from the z direction. The light irradiating unit 20 calculates an ellipticity angle ε ω and azimuth angle θ ω The light irradiation unit 20 includes, for example, a light source 21 and an optical element 22.

[0019] The light source 21 is, for example, a laser light source. The light source 21 is, for example, a pulse laser. There are no particular limitations on the central wavelength, pulse width, and repetition period of the light emitted from the light source 21. The central wavelength of the light emitted from the light source 21 is, for example, not less than 300 nm and not more than 2000 nm. The spot diameter of the light emitted from the light source 21 on the surface of the magnetic metamaterial 10 is matched to the size of the magnetic metamaterial 10. The spot diameter of the light is, for example, 250 μm.

[0020] The optical element 22 is, for example, a polarizer or a wave plate. The polarization state of the light emitted from the light source 21 changes as it passes through the optical element 22. The magnetic metamaterial 10 is irradiated with the light whose polarization state is controlled by the optical element 22.

[0021] The light irradiated to the magnetic metamaterial 10 has an ellipticity angle ε ω and azimuth angle θ ω The linear polarization is controlled by the ellipticity angle ε ω is 0° or 90°, which is one form of elliptically polarized light. ω The ellipticity angle ε is 45°, which is one form of elliptical polarization. The ellipticity is the ratio of the length a of the major axis of the elliptical polarization to the length b of the minor axis, and is expressed as b / a. ω is tan ε ω =b / a. Azimuth angle θω is the angle that the major axis of the elliptically polarized light makes with the y-axis, which is, for example, the transmission axis of the incident linearly polarized light.

[0022] Fig. 2 is a perspective view of the magnetic metamaterial 10. Fig. 3 is a plan view of the magnetic metamaterial 10. The magnetic metamaterial 10 has broken spatial inversion symmetry and time reversal symmetry. The magnetic metamaterial 10 has, for example, a substrate 11 and a perpendicular magnetization film 12 laminated on the substrate 11.

[0023] There is no particular limitation on the substrate 11. The substrate 11 is, for example, quartz glass. Other layers may be present between the substrate 11 and the perpendicular magnetization film 12. For example, an adhesion layer may be formed between the substrate 11 and the perpendicular magnetization film 12 to improve adhesion between the substrate 11 and the perpendicular magnetization film 12. The adhesion layer may be, for example, silicon nitride. Also, for example, an underlayer may be formed between the substrate 11 and the perpendicular magnetization film 12 to improve the crystallinity of the perpendicular magnetization film 12. The underlayer may be, for example, platinum.

[0024] The perpendicular magnetization film 12 is a magnetic film having an easy axis of magnetization in a direction intersecting (orthogonal to) the xy plane. The magnetic film may be a ferromagnetic film or a ferrimagnetic film. The magnetic film has broken time reversal symmetry. This is because in a magnetically ordered state, the magnetic moment created by the angular momentum of spin and orbit is reversed by a time reversal operation. The magnetic film is preferably, for example, a ferromagnetic film.

[0025] The perpendicular magnetic film 12 has isotropy to light before the unit structures are formed. Having isotropy to light means that the perpendicular magnetic film 12 has the property of responding in the same way regardless of the direction from which light is irradiated onto the perpendicular magnetic film 12.

[0026] The perpendicular magnetic film 12 is, for example, a multilayer film of 3d transition metal and noble metal, a sandwich film, an L10-type or L11-type ordered alloy, a rare earth-transition metal amorphous alloy, etc. The multilayer film of 3d transition metal and noble metal is, for example, a multilayer film of Co and Pt, a multilayer film of Co and Pd, a multilayer film of Co and Au, a multilayer film of Fe and Pt, etc. The sandwich film is, for example, a film in which CoFeB is sandwiched between MgO and Ta, a film in which Co is sandwiched between Ta and Pt, etc. The ordered alloy of L10 type or L11 type is, for example, FePt, FePd, CoPt, MnGa, MnAl, etc. The rare earth-transition metal amorphous alloy is, for example, GdFeCo, etc. The multilayer film of 3d transition metal and noble metal is particularly preferable because it has high corrosion resistance, high perpendicular magnetic anisotropy, and can be formed at room temperature.

[0027] The perpendicular magnetization film 12 has a plurality of unit structures 13. The plurality of unit structures 13 are formed in the perpendicular magnetization film 12, which is isotropic to light, before the unit structures are formed. The plurality of unit structures 13 are periodically arranged in the in-plane direction of the magnetic metamaterial 10. The plurality of unit structures 13 are periodically arranged, for example, in one direction among the in-plane directions of the magnetic metamaterial 10. The plurality of unit structures 13 may be periodically arranged, for example, in a plurality of different directions among the in-plane directions of the magnetic metamaterial 10. The plurality of unit structures 13 are formed, for example, by a plurality of openings 14. The arrangement state of the plurality of unit structures 13 is not particularly limited. For example, a line connecting the centers of gravity of adjacent unit structures 13 may draw a triangle or other polygon.

[0028] The size of each of the unit features 13 is equal to or smaller than the wavelength of the irradiated light. The size of each of the unit features 13 is, for example, equal to or smaller than 1 μm. The size of each of the unit features 13 refers to the maximum width of each of the unit features 13 in the x direction and the maximum width of each of the unit features 13 in the y direction.

[0029] The unit structure 13 has three-fold rotational symmetry. The opening 14 also has three-fold rotational symmetry. Three-fold rotational symmetry means that when the unit structure 13 is rotated by ±120°, it becomes the same structure as before the rotation. Since the unit structure 13 has three-fold rotational symmetry, the perpendicular magnetic film 12 breaks spatial inversion symmetry. Spatial inversion symmetry means point symmetry, and means that when the coordinates (x, y, z) are inverted to (-x, -y, -z), it becomes the same structure as before the inversion.

[0030] The shape of the unit structure 13 in plan view in the z direction is, for example, an equilateral triangle that shares a corner with an adjacent unit structure 13. The shape of the opening 14 in plan view in the z direction is, for example, an equilateral triangle. There is no particular limit to the shapes of the unit structure 13 and the opening 14 in plan view as long as they each have three-fold rotational symmetry. For example, the relationship between the unit structure 13 and the opening 14 may be inverted, or the opening 14 may be of the Mitsubishi type as shown in FIG. 4.

[0031] The unit structure 13 and the opening 14 belong to the point group 3m. Furthermore, these planar periodic structures belong to the space group p3m1.

[0032] The magnetic metamaterial 10 is obtained by processing a unit structure into a formed perpendicular magnetization film.

[0033] First, a perpendicular magnetic film is formed on the substrate 11. The perpendicular magnetic film can be formed by a known method such as sputtering or chemical vapor deposition (CVD). For example, when the perpendicular magnetic film is a multilayer film of a 3d transition metal and a noble metal, the 3d transition metal and the noble metal are alternately formed. An adhesion layer and an underlayer may be formed between the substrate 11 and the perpendicular magnetic film.

[0034] Next, an opening 14 having three-fold rotational symmetry is formed in the formed perpendicular magnetic film. The opening 14 can be made by, for example, electron beam lithography.

[0035] The spin current control device 100 according to the first embodiment has a magnetic metamaterial 10 with an ellipticity angle ε ω and azimuth angle θ ωBy irradiating the magnetic metamaterial with light having a controlled ellipticity angle ε, the direction and magnitude of the spin current generated on the surface of the magnetic metamaterial 10 can be controlled. ω and azimuth angle θ ω By irradiating the material with light with controlled spin current, the spin current can be controlled.

[0036] When light is irradiated onto a material that does not have spatial inversion symmetry, a current is generated by optical excitation without an external field. This phenomenon is called the optogalvanic effect. A similar phenomenon is the magneto-optical galvanic effect. The magneto-optical galvanic effect is a phenomenon in which, when light is irradiated onto a material that does not have spatial inversion symmetry or time reversal symmetry, a spin current is generated by optical excitation without an external field.

[0037] The magneto-optical galvanic effect is a second-order nonlinear optical effect and is expressed by the following relational expression (1).

[0038]

number

[0039] In the above formula, E j (ω), E k * (ω)=E k (-ω) denotes the j-polarized and k-polarized electric fields of the incident light at ω, respectively, which induce zero-bias photocurrents in the i-direction proportional to the square of the AC electric field. β ijk is a third-rank polar tensor whose sign changes with space and time reversal operations and whose value is determined by the symmetry of the material.

[0040] The magnetic metamaterial 10 is a perpendicular magnetization film having three-fold rotational symmetry and an ellipticity angle ε ω and azimuth angle θ ω When light with controlled spin current is irradiated, the spin current J s As described above, since the magnetic metamaterial 10 belongs to the point group 3m, the following relations (2) and (3) are derived.

[0041]

number

[0042]

number

[0043] |J s | denotes the magnitude of the spin current, and cos2ε ω In other words, the magnitude of the spin current is proportional to the ellipticity angle ε ω In other words, the ellipticity angle ε ω By controlling θ s is the main direction in which the spin current occurs, and is the angle between the y axis and the main direction of the spin current. The direction in which the spin current occurs is the azimuth angle θ ω In other words, the azimuth angle θ ω By controlling this, the direction in which the spin current is generated can be controlled.

[0044] The above relationship is obtained when the magnetic metamaterial 10 is applied to the symmetry of the point group 3m, and when the magnetic metamaterial 10 has three-fold rotational symmetry, the magnitude and direction of the spin current can be controlled.

[0045] Spin current is applied to magnetic memories, thermoelectric conversion elements, oscillators, sensors, etc. If the direction of the spin current can be controlled, it may be possible to give directionality to signals, for example. The spin current control device 100 can be applied to new spintronics devices.

[0046] When light is irradiated onto a metamaterial made of a non-magnetic material (e.g., Pt) that does not have spatial inversion symmetry, a photocurrent is generated by the optogalvanic effect. The photocurrent can be converted into a spin current by utilizing the spin Hall effect. The spin Hall effect is a phenomenon in which, when a current flows in one direction, a spin current is generated in a direction perpendicular to the direction of the current flow. That is, a spin current can be obtained by irradiating light onto a non-magnetic metamaterial that does not have spatial inversion symmetry. However, the conversion efficiency from photocurrent to spin current is not sufficient, and it is difficult to obtain a spin current that can be applied to measurements and device use. The spin current control device 100 according to the first embodiment directly controls and detects the spin current by the magneto-optogalvanic effect, so that a sufficiently large spin current can be controlled by light.

[0047] So far, one embodiment of the spin current controlling device 100 has been illustrated, but the present invention is not limited to this embodiment. EXAMPLES

[0048] Example 1 5 is a conceptual diagram of an experimental system according to Example 1. The experimental system of Example 1 includes a magnetic metamaterial 10, a light irradiation unit 20, a measurement system 30, and a magnetic field generation unit (not shown). The experiment was carried out at room temperature.

[0049] The specific configuration of the magnetic metamaterial 10 is the same as that shown in Fig. 2 and Fig. 3. The magnetic metamaterial 10 is a SiO 2 The device has a substrate and a perpendicular magnetic film in which equilateral triangular openings having three-fold rotational symmetry are periodically formed. 2 Between the substrate and the perpendicular magnetic film, SiO 2 From the substrate side, there is an adhesion layer (SiN with a thickness of 5 nm) and an underlayer (Pt with a thickness of 2 nm), and these also have equilateral triangular openings formed periodically. The perpendicular magnetic film is a multilayer film in which Pt with a thickness of 0.9 nm and Co with a thickness of 0.5 nm are alternately laminated. The number of Pt layers and Co layers is 5 each. The perpendicular magnetic film has magnetization M in the z direction. zIn addition, a cap layer (2 nm thick Pt) is formed on the perpendicular magnetic film, and equilateral triangular openings are periodically formed in the cap layer. Each layer is formed by radio frequency sputtering.

[0050] The equilateral triangular openings were formed in an area of ​​250 μm × 250 μm by electron beam lithography. After the openings were formed, they were etched with Ar ions. Each side of the openings was 480 nm, and they were periodically arranged at intervals of 558 nm.

[0051] The light irradiation unit 20 has a Ti:sapphire laser (Spectra-Physics, Mai Tai (registered trademark)). The laser light used had a central wavelength of 800 nm, a pulse width of 100 fs, and a repetition period of 80 MHz. The spot diameter of the laser light on the surface of the magnetic metamaterial 10 was 250 μm. The laser light after passing through the magnetic metamaterial 10 was monitored by a CCD camera. The laser light was adjusted so that it was irradiated to the center of the magnetic metamaterial 10 in order to eliminate the influence of the Seebeck effect and the Nernst effect. The intensity of the laser light was modulated to 1 kHz by an optical chopper. The light irradiated to the magnetic metamaterial 10 had an ellipticity angle ε ω and azimuth angle θ ω The light was linearly polarized at 0°.

[0052] When the magnetic metamaterial 10 is irradiated with light, a spin current is generated on the surface of the magnetic metamaterial 10. The spin current was measured separately in the x and y directions with a two-phase lock-in amplifier (Stanford Research Systems, SR865) using a reference signal from an optical chopper. The spin current was obtained by time averaging. The magnitude of the spin current |J s | is |J s |=((J s,y ) 2 +(J s,x ) 2 ) 1 / 2 The calculation was done by J s,y is the y-component of the spin current, and J s,x is the x-component of the spin current. The direction of spin current generation θ sθ s =tan -1 (J s,x / J s,y ) was calculated.

[0053] Fig. 6 shows the response characteristics of the spin current generated after irradiating the magnetic metamaterial 10 with laser light in Example 1. Also, Fig. 7 shows the results of changing the intensity of the laser light irradiated to the magnetic metamaterial 10 in Example 1.

[0054] As shown in Fig. 6, after the magnetic metamaterial 10 is irradiated with laser light, a spin current is generated in about 2 nsec. In other words, the spin current control device shown in Example 1 has a fast response characteristic. Note that, although it takes 2 nsec to detect the spin current in Fig. 6, this time depends on the spin current measurement system, and in principle, it is considered that the response is on the order of fsec. Furthermore, as shown in Fig. 7, the magnitude of the spin current increases when the intensity of the laser light is increased.

[0055] 6 and 7 also show that when the magnetization orientation of the perpendicular magnetic film is reversed, the direction of the spin current is reversed. z indicates the case where the magnetization of the perpendicular magnetic film is oriented in the +z direction, and -M z indicates the case where the magnetization of the perpendicular magnetic film is oriented in the -z direction. The +z direction is the direction from the magnetic metamaterial 10 to the light irradiation unit 20, and the -z direction is the direction from the light irradiation unit 20 to the magnetic metamaterial 10. The orientation direction of the magnetization of the perpendicular magnetic film was changed by applying a magnetic field to the magnetic metamaterial 10 by a magnetic field generating unit (not shown).

[0056] Fig. 8 shows the results of measuring the effect on the spin current when the magnetic field applied to the magnetic metamaterial 10 is changed in Example 1. As shown in Fig. 8, the spin current draws a hysteresis loop with respect to the external magnetic field. Even when the absolute value of the magnitude of the external magnetic field applied to the perpendicular magnetization film is increased to about 1000 Oe, the magnitude and direction of the spin current do not change, but when the absolute value exceeds 1000 Oe, the direction of the spin current is reversed.

[0057] 9 shows the results of measuring the magnetization direction of the perpendicular magnetic film using the magnetic Faraday effect in Example 1. The light irradiated to the perpendicular magnetic film rotates after passing through the perpendicular magnetic film due to the Faraday effect. The Faraday rotation angle θ F was measured by the balance detection method. As shown in Figure 9, when the magnetization direction of the perpendicular magnetization film is reversed, the Faraday rotation angle θ F In other words, when the magnitude of the external magnetic field exceeds 1000 Oe, the magnetization direction of the perpendicular magnetic film is reversed. As can be seen from Figures 8 and 9, the reversal of the direction in which the spin current is generated is caused by the reversal of the magnetization orientation of the perpendicular magnetic film.

[0058] Figure 10 compares the magnetization curve of the flat Co / Pt multilayer before the formation of multiple openings with that of the magnetic metamaterial (MM). As shown in Figure 10, the coercive force Hc of the magnetic metamaterial (Hc ≒ 1000 Oe) was greater than the coercive force Hc' (Hc' ≒ 600 Oe) of the flat Co / Pt multilayer. This is believed to be because the openings in the magnetic metamaterial prevented magnetization reversal.

[0059] In addition, Figure 11 shows the results of measuring the wavelength dependence of the transmittance (T), reflectance (R), and absorptance (A) of the magnetic metamaterial. The absorptance (A) was calculated as 1 - transmittance (T) - reflectance (R). As shown in Figure 11, the magnetic metamaterial has little dependence on the wavelength of light.

[0060] FIG. 12 shows the results of measuring the dependence of the magnitude of the spin current on the wavelength of the irradiated light in the experimental system of Example 1. Even if the irradiated wavelength is changed, the spin current (J s,y ) does not occur, and spin current (J s,x ) was generated. That is, the ellipticity angle ε ω and azimuth angle θ ω When linearly polarized light with a polarization of 0° was irradiated onto the magnetic metamaterial, the relationship that spin current occurs only in the x direction did not change.

[0061] Example 2 13 is a conceptual diagram of an experimental system according to Example 2. The experimental system of Example 2 is the same as that of Example 1 in that the magnetic metamaterial 10 is irradiated with light from a light irradiating unit 20, and the spin current generated on the surface of the magnetic metamaterial 10 is measured by a measurement system 30. On the other hand, the azimuth angle θ of the light irradiated to the magnetic metamaterial 10 ω This differs from Example 1 in that

[0062] FIG. 14 shows the azimuth angle θ of light irradiated onto the magnetic metamaterial 10 in the experimental system according to the second embodiment. ω The vertical axis of the graph in Fig. 14 represents, from the top, the x and y components of the magnitude of the spin current (J s,x , J s,y ), the magnitude of the spin current (|J s |), the direction of spin current generation θ s The horizontal axis of the graph shown in FIG. ω It is.

[0063] As shown in FIG. 14, the azimuth angle θ ω Even if the spin current magnitude (|J s |) did not change, but the azimuth angle θ ω By changing the direction of spin current generation θ s changed continuously. The results show the relations (2) and (3). According to the relation (2), the magnitude of the spin current (|J s |) is the azimuth angle θ ω The results are consistent with the experimental results. s is the azimuth angle θ ω , which is in agreement with the actual experimental results.

[0064] Example 3 15 is a conceptual diagram of an experimental system according to Example 3. The experimental system of Example 3 is the same as that of Example 1 in that the magnetic metamaterial 10 is irradiated with light from a light irradiating unit 20, and the spin current generated on the surface of the magnetic metamaterial 10 is measured by a measurement system 30. On the other hand, the ellipticity angle ε ω and azimuth angle θ ω The difference from Example 1 is that the ellipticity angle ε ω and azimuth angle θ ω was changed by inserting the optical element 22 into the optical path. The optical element 22 was a quarter-wave plate. The azimuth angle φ of the light irradiated to the optical element 22 was also changed. ω was also changed.

[0065] The rotation angle α of the quarter-wave plate was set to 0° and 45°. The ellipticity angle ε of the excitation light was set to ω and azimuth angle θ ω is the azimuth angle φ of the light irradiated onto the optical element 22 ω and the rotation angle α. When the rotation angle α=0°, the azimuth angle θ ω is 0° or 90°. Ellipticity angle ε ω changes continuously from -45° to 45°. When the rotation angle α=45°, the azimuth angle θ ω is 45° or 135°. Ellipticity angle ε ω changes continuously from -45° to 45°.

[0066] FIG. 16 shows the azimuth angle φ of light irradiated onto the optical element 22 in the experimental system according to the third embodiment. ω The x and y components of the magnitude of the spin current when J s,x , J s,y ) are the results when the rotation angle α is 0°. The upper graph in Fig. 16 shows the results when the rotation angle α is 0°, and the lower graph in Fig. 16 shows the results when the rotation angle α is 45°.

[0067] When the rotation angle α = 0°, the x component of the magnitude of the spin current (J s,x ) is -cos2φ ω When the rotation angle α = 0°, the y component of the magnitude of the spin current (J s,y) remains constant at 0. When the rotation angle α is 45°, the y component of the magnitude of the spin current (J s,y ) is -sin2φ ω When the rotation angle α is 45°, the x component of the magnitude of the spin current (J s,x ) remains constant at 0.

[0068] Figure 17 shows the results of Figure 16 with respect to the ellipticity angle ε ω and the magnitude of the spin current (|J s As shown in Figure 17, the magnitude of the spin current is expressed as cos2ε ω This relationship is proportional to equation (2). [Explanation of symbols]

[0069] 10...magnetic metamaterial, 11...substrate, 12...perpendicular magnetization film, 13...unit structure, 14...opening, 20...light irradiation unit, 21...light source, 22...optical element, 30...measurement system, 100...spin current control device

Claims

1. A perpendicular magnetization film having isotropy with respect to light is included. the perpendicular magnetic film includes a plurality of unit structures periodically arranged in an in-plane direction, A magnetic metamaterial, wherein each of the plurality of unit structures has a size equal to or smaller than the wavelength of irradiated light and has three-fold rotational symmetry.

2. The magnetic metamaterial of claim 1 , wherein the perpendicular magnetization film has a plurality of openings that form the plurality of unit structures.

3. The magnetic metamaterial of claim 2 , wherein each of the plurality of apertures is an equilateral triangle.

4. A magnetic metamaterial according to any one of claims 1 to 3; A light irradiation unit that irradiates the magnetic metamaterial with light, The light irradiation unit is a spin current control device capable of controlling the ellipticity angle and azimuth angle of the light irradiated to the magnetic metamaterial.

5. A step of irradiating a magnetic metamaterial with light having a controlled ellipticity angle and azimuth angle, The magnetic metamaterial has a perpendicular magnetization film having isotropy with respect to light, the perpendicular magnetic film includes a plurality of unit structures periodically arranged in an in-plane direction, A method for controlling a spin current, wherein each of the plurality of unit structures has a size equal to or smaller than the wavelength of the irradiated light and has three-fold rotational symmetry.

Citation Information

Patent Citations

  • magnetic material

    JP2002541614A

  • Spintronics device

    JP2014086448A

  • Magnetic storage element

    JP2017195269A

  • Laminate, thermoelectric conversion element, usage method of thermoelectric conversion element, power generation device, waste heat recovery system, and method

    JP2021040066A

  • Spin torque device

    US20200395532A1