Structure with microchannel, manufacturing method thereof, and microchannel device

The microchannel structure with controlled infrared absorption and water contact angles addresses the challenges of pattern complexity and fluid movement, improving the accuracy of microfluidic devices by minimizing capillary-induced fluid movement.

JP7565565B2Active Publication Date: 2024-10-11ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023554710
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-18
Filing Date
2022-10-18
Publication Date
2024-10-11
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Existing methods for producing microchannels in microfluidic devices face challenges such as the difficulty in creating various fine patterns and unintended fluid movement due to capillarity, which affects the accuracy of output results.

Method used

A microchannel structure is designed with specific infrared absorption characteristics and water contact angles, using a photosensitive resin composition that minimizes the ratio of certain peak intensities and includes a resin region derived from an alkali-soluble resin, reducing hydrophilicity and controlling fluid movement through capillary action.

Benefits of technology

This approach effectively reduces unintended fluid movement in microchannels, enhancing the accuracy of output results by suitably controlling fluid flow and improving the precision of microchannel devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565565000004
    Figure 0007565565000004
  • Figure 0007565565000005
    Figure 0007565565000005
  • Figure 0007565565000006
    Figure 0007565565000006
Patent Text Reader

Abstract

A structure 10 comprising a microchannel 14, said structure 10 including a base material 11, a partition material 12, and a cover material 13, wherein: at least part of the partition material 12 and the base material 11 have a resin region 21 derived from an alkali-soluble resin; in an infrared absorption spectrum of the resin region 21 as observed by infrared spectroscopy, the ratio (Aa / Ac) of the maximum peak intensity (Aa) in a first range of 1555-1575 cm-1 to the maximum peak intensity (Ac) in a second range of 1715-1735cm-1 is greater than 0 but less than or equal to 0.200; and the water contact angle of a channel formation surface 11a of the base material 11 is 40-150 degrees.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a structure having a microchannel, a manufacturing method thereof, and a microchannel device. [Background technology]

[0002] Microfluidic devices have been attracting increasing attention from the viewpoints of remote medical care and point-of-care testing (POCT), etc. Microfluidic devices are also called microfluidic devices, microfluidic chips, μTAS (Micro Total Analysis Systems), LOC (Lab on a Chip), microreactors, etc.

[0003] A microchannel device has a structure (hereinafter, simply referred to as "structure") equipped with a microchannel. In this type of structure, the microchannel has generally been produced by injection molding, mold forming, glass etching, or the like. On the other hand, a method of producing a microchannel using a photosensitive resin composition is also known. For example, Patent Document 1 discloses a method of producing a fine pattern by pouring a photosensitive resin composition into a mold and solidifying it by photopolymerization.

[0004] A method for fabricating a microchannel using a photosensitive resin laminate (also called a "dry film" or the like) is also known. For example, Patent Document 2 discloses a method for forming a fine pattern by developing (dissolving and removing) the unexposed parts (uncured parts) of a resin that exhibits alkali solubility due to the presence of carboxyl groups with an alkaline developer. In addition, for example, Patent Document 3 discloses a method for forming a microchannel by curing a patterning material in two stages with the aim of preventing the substrate in the channel from adhering to the side of the channel. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-46853 A [Patent Document 2] JP 2010-70614 A [Patent Document 3] International Publication No. 2015 / 012212 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the method of Patent Document 1 requires a mold corresponding to the flow path pattern in order to pour the photosensitive resin composition, and has a problem that it is disadvantageous in terms of producing various fine patterns compared to the method using a dry film.

[0007] On the other hand, in the case of the method using a dry film, there is a possibility that carboxylates are generated and remain in the obtained pattern due to the use of an alkaline developer. Patent Document 2 does not mention this point at all, and therefore, the method of Patent Document 2 has a problem in that the hydrophilic effect of the carboxylates makes it easier for the fluid to run unexpectedly in the microchannel, that is, it becomes difficult to control the movement of the fluid in the microchannel.

[0008] Furthermore, in recent years, there has been a strong demand for improved accuracy in output results from microchannel devices (such as synthesis results and test results in microchannel devices), and so there has been a need for a method that can improve various characteristics of microchannel devices using an approach other than preventing adhesion of a substrate to the sides of the channel, as in Patent Document 3.

[0009] Therefore, the problem to be solved by the present invention is to provide a structure having a microchannel that can reduce unintended fluid movement that may be induced by capillary action in a microchannel fabricated using a dry film, thereby enabling suitable control of fluid movement and ultimately improving the accuracy of output results in the obtained microchannel device. Another problem to be solved by the present invention is to provide a method for manufacturing the structure, and a microchannel device including the structure. [Means for solving the problem]

[0010] The present inventors have found that the above object can be achieved by the following technical means, and have arrived at the embodiments of the present invention. That is, the embodiments of the present invention are as follows. [1] A structure having a microchannel, The structure includes a substrate, a partition material, and a cover material, The substrate and at least a part of the partition material have a resin region derived from an alkali-soluble resin, The resin region has an infrared absorption spectrum according to infrared spectroscopy, 1555~1575cm -1 A maximum peak intensity (Aa) in the first range; 1715~1735cm -1 The maximum peak intensity (Ac) in the second range of The ratio (Aa / Ac) is greater than 0 and less than or equal to 0.200, The water contact angle of the flow path forming surface of the substrate is 40 to 150 degrees. A structure having a microchannel. [2] 2. The structure having a microchannel according to item 1, wherein the ratio (Aa / Ac) is 0.100 or less. [3] 3. The structure having a microchannel according to item 1 or 2, wherein the ratio (Aa / Ac) is 0.085 or less. [4] 4. The structure having a microchannel according to any one of items 1 to 3, wherein the ratio (Aa / Ac) is 0.050 or less. [5] 5. The structure equipped with a microchannel according to any one of items 1 to 4, wherein the first range includes an absorption intensity corresponding to a stretching vibration of a carbonyl (C═O) bond derived from a carboxylate. [6] 6. The structure equipped with a microchannel according to any one of items 1 to 5, wherein the second range includes an absorption intensity corresponding to the stretching vibration of a carbonyl (C═O) bond derived from an ester. [7] 1625~1645cm -1 The maximum peak intensity (Ad) in the third range; The maximum peak intensity (Ac); 7. The structure having a microchannel according to any one of items 1 to 6, wherein the ratio (Ad / Ac) is greater than 0 and not greater than 0.150. [8] 8. The structure having a microchannel according to item 7, wherein the third range includes an absorption intensity corresponding to a stretching vibration of a carbon-carbon (C=C) bond derived from a carbon-carbon double bond. [9] 9. The structure having a microchannel according to any one of items 1 to 8, wherein the resin region is substantially free of components derived from an alkali metal salt.

[10] 10. The structure having a microchannel according to any one of items 1 to 9, wherein the water contact angle is 60 to 130 degrees.

[11] 11. The structure having a microchannel according to any one of items 1 to 10, wherein the resin region is derived from a resin containing a (meth)acrylic resin.

[12] The resin region comprises the following components: (a) an alkali-soluble polymer containing a carboxyl group; (b) an addition polymerizable monomer; and (c) a photopolymerization initiator or its decomposition product; 12. The structure having a microchannel according to any one of items 1 to 11, which is derived from a resin made of a photosensitive resin composition containing:

[13] 13. The structure having a microchannel according to any one of items 1 to 12, wherein the partition material includes the resin region.

[14] The resin region has the following formula (1): P = [(1 / h) cos{(θs / 180) π} + (1 / h)·cos{(θb / 180)·π}+ (2 / w) cos{(θ / 180) π}] 10 6 ... (1) {In the formula, θs: Water contact angle (deg: degree) of the flow path forming surface of the lid material θb: Water contact angle (deg) of the flow path forming surface of the substrate θ: Water contact angle (deg) of the flow path forming surface of the partition material h: Length (μm) of the flow path forming surface of the partition material when the structure is cut along the thickness direction w: length (μm) of the flow channel forming surface of the substrate when the structure is cut along the thickness direction 14. A structure having a microchannel according to any one of items 1 to 13, wherein P(1 / μm) represented by the following formula is 1650 or less.

[15] (i-1) a step of applying a photosensitive resin composition solution containing a solvent having a boiling point of less than 100° C. to a support and drying the applied solution to form a photosensitive resin layer containing an alkali-soluble resin on the support; (i-2) laminating the photosensitive resin layer on a substrate; (ii) developing the laminated photosensitive resin layer with an organic base aqueous solution to form a flow path pattern; (iii) a step of subjecting the flow path pattern to a heat treatment to perform a surface treatment on the flow path pattern, thereby producing a resin region derived from an alkali-soluble resin; The resin region has an infrared absorption spectrum according to infrared spectroscopy, 1555~1575cm-1 A maximum peak intensity (Aa) in the first range; 1715~1735cm -1 The maximum peak intensity (Ac) in the second range of The ratio (Aa / Ac) is greater than 0 and not greater than 0.200.

[16] The step (ii) comprises: Item 16. The method for producing a structure provided with a microchannel according to item 15, further comprising a step of exposing the photosensitive resin layer to light before the development.

[17] Item 17. The method for producing a structure provided with a microchannel according to item 16, wherein in the step (ii), the exposing step is performed by direct imaging exposure without using a mask.

[18] After the step (iii), (iv) forming a lid material by lamination; 18. The method for producing a structure provided with a microchannel according to any one of items 15 to 17,

[19] 15. A microchannel device comprising a structure having a microchannel according to any one of items 1 to 14.

[20] A substrate having an electrode; an electrode protection layer provided on the base material for protecting the electrodes; a structure including the microchannel, which is laminated on the substrate and / or the electrode protection layer; 20. The microfluidic device according to item 19, comprising: Effect of the Invention

[0011] According to the present invention, it is possible to provide a structure having a microchannel that can reduce unintended fluid movement that may be induced by capillary action in a microchannel fabricated using a dry film, thereby enabling suitable control of fluid movement and ultimately improving the accuracy of output results in the obtained microchannel device. Furthermore, according to the present invention, it is possible to provide a method for manufacturing the structure and a microchannel device having the structure. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view and a plan view for explaining an example of a structure according to the present embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view for explaining one example and another example of the structure according to the present embodiment. [Diagram 3] FIG. 3 is a diagram for explaining an example of a structure according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, a structure having a microchannel according to this embodiment will be described with reference to the drawings. In this embodiment, a numerical range described using "~" represents a numerical range including the numerical values ​​before and after "~" as the lower limit and upper limit. In this embodiment, in a numerical range described in stages, the upper limit or lower limit described in a certain numerical range can be replaced with the upper limit or lower limit of another numerical range described in stages. Furthermore, in this embodiment, the upper limit or lower limit described in a certain numerical range can also be replaced with a value shown in an example. In this embodiment, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the function of the process is achieved. In the contents shown in FIG. 1 and FIG. 2, the scale, shape, and length may be exaggerated for further clarity.

[0014] [Microfluidic Device] <Structure with Microchannels> (Schematic configuration) FIG. 1(a) is a cross-sectional view showing an example of the configuration of a structure 10, and FIG. 1(b) is a plan view showing the example of the configuration of the structure 10. As shown in FIG.

[0015] As shown in Fig. 1(a), the microchannel device 1 includes a structure 10. The structure 10 includes a base material 11, a partition material 12 provided on the base material 11, and a cover material 13 provided on the partition material 12, thereby forming a microchannel 14, which is a passage for a fluid (liquid or gas). The partition material 12 includes a resin layer 16 in which a flow channel pattern 15 is formed. In the figure, the partition material 12 has a three-layer structure, but it may have a single layer structure or another multiple layer structure (for example, a four-layer structure, a five-layer structure, a six-layer structure, a seven-layer structure, or an eight-layer structure).

[0016] (Partition wall material) 1(b), the flow path pattern 15 is configured to have an injection port 17, an injection port pattern 17a extended from the injection port 17, a waste liquid port 18, a waste liquid port pattern 18a extended from the waste liquid port 18, a main flow path pattern 19 connecting the injection port pattern 17a and the waste liquid port pattern 18a, and a plurality of weighing flow path patterns 20 extended in a comb shape from the main flow path pattern 19. Of these, the weighing flow path pattern 20 has long sides 20a, short sides 20b, a flow path pattern width 20c, and a partition width 20d. In this embodiment, the flow channel pattern 15 is configured as a micro flow channel pattern 15 for weighing purposes, but this configuration is merely an example. The configuration of the flow channel pattern can be modified in various ways depending on the purpose of the micro flow channel device, its overall structure, etc.

[0017] The flow path pattern 15 can be produced using a dry film. For example, in FIG. 1(b), the region within the frame of the flow path pattern 15 is an unexposed portion, and the region outside the frame is an exposed portion. The region outside the frame of the flow path pattern 15 is exposed to light to harden it, and the region within the frame is developed with an alkaline developer to obtain the flow path pattern 15. The method using the dry film is advantageous in terms of producing various fine patterns, and is also advantageous in terms of suitably selecting exposure conditions and / or development conditions according to the desired flow path pattern. The dry film may be a dry film resist. As described above, the method described here uses a so-called "negative" dry film, in which the unexposed areas can be removed by development, as an example. However, the present invention can also use a method using a so-called "positive" dry film.

[0018] One or more microchannel devices 1 can be arranged in a silicon wafer (not shown) so that, for example, the inlet 17 is positioned toward the center of the silicon wafer and the waste liquid outlet 18 is positioned in the circumferential direction.

[0019] Methods for moving the fluid in the microchannel 14 (including not only the movement of the fluid in various patterns but also the introduction of the fluid from the inlet 17 and the discharge of the fluid from the waste port 18) include, for example, a method using a micropump (not shown); a method using centrifugal force; and the like. In any liquid transfer method, energy is exerted on the fluid by capillary action to move the fluid in the microchannel 14. Therefore, reducing unintended fluid movement that may be induced by capillary action in the microchannel 14 and thereby achieving suitable control of the fluid movement is advantageous in terms of improving the accuracy of the output result from the microchannel device 1.

[0020] (Resin area) Fig. 2(a) is an enlarged cross-sectional view showing an example of the configuration within region A in Fig. 1(a). As shown in Fig. 2(a), a component of the microchannel 14 (in this embodiment, the partition material 12) at least partially has a resin region 21. The resin region 21 is derived from an alkali-soluble resin. Here, the resin region 21 has an infrared absorption spectrum according to infrared spectroscopy, 1555~1575cm -1 A maximum peak intensity (Aa) in the first range; 1715~1735cm -1 The maximum peak intensity (Ac) in the second range of The ratio (Aa / Ac) is greater than 0 and less than 0.200. The "maximum peak intensity" refers to the maximum peak intensity obtained.

[0021] First, the inventors have noticed that a composition having a main functional group in which energy absorption is observed in the first region has higher hydrophilicity than a composition having a main functional group in which energy absorption is observed in the second region. In this regard, if the maximum peak intensity (Ac) in the second region is considered to play a role as an internal standard for defining the ratio of the maximum peak intensity (Aa) in the first region in the resin region 21, it can also be understood that the structure region in which the energy absorption in the first region is large has high hydrophilicity. Therefore, by making the ratio (Aa / Ac) 0.200 or less, the degree of hydrophilicity of the component of the microchannel 14 (the partition material 12 in this embodiment) can be reduced, and thus unintended fluid movement that may be induced by capillary action can be reduced.

[0022] In addition, the main functional groups that exhibit energy absorption in the first range include those derived from functional groups that play a role in imparting alkali solubility. Therefore, the ratio (Aa / Ac) exceeding 0 means that the prerequisite for producing the flow path pattern 15 using the dry film is satisfied.

[0023] As described above, by controlling the ratio (Aa / Ac) to a relatively small range, the flow channel pattern 15 can be produced through development with an alkaline developer, while the degree of hydrophilicity of the component of the microchannel 14 (the partition material 12 in this embodiment) can be reduced. By reducing the degree of hydrophilicity, unintended fluid movement in the microchannel 14 that may be induced by capillary action can be reduced.

[0024] In this regard, the first range includes, for example, an absorption intensity corresponding to the stretching vibration of a carbonyl (C=O) bond derived from a carboxylate. Carboxylate salts have a high hydrophilic effect, and the amount of such components is relatively small, which makes it easier to reduce unintended fluid movement that may be induced by capillary action. The second range also includes, for example, an absorption intensity corresponding to the stretching vibration of a carbonyl (C=O) bond derived from an ester. Esters have a lower hydrophilic effect than carboxylates, and the relatively large amount of such components makes it easier to reduce unintended fluid movement that may be induced by capillary action. Furthermore, by clarifying that the first range and the second range each include the above absorption intensities, it becomes easier to synergistically reduce unintended fluid movement that may be induced by capillary action.

[0025] Here, the relationship between the main functional groups exhibiting energy absorption in the first range and the main functional groups exhibiting energy absorption in the second range, and the method for fabricating a microchannel using a dry film will be described. That is, when developing the uncured part of the alkali-soluble resin layer, an alkaline developer is used. Due to the use of the alkaline developer, a carboxylate may be generated and remain in the obtained pattern. Here, the absorption intensity corresponding to the stretching vibration of the carbonyl (C=O) bond derived from the carboxylate falls within the above-mentioned first range. When the uncured portion is developed with an alkaline developer, the development process conditions are appropriately selected, and the flow path pattern obtained by development is subjected to a heat treatment, whereby the carboxylate can be converted to a carboxylic acid or a carboxylate ester, of which the absorption intensity corresponding to the stretching vibration of the carbonyl (C=O) bond derived from the carboxylate ester falls within the above-mentioned second range.

[0026] From the above, it is assumed that in the process of producing a flow path pattern using a dry film, due to the use of an alkaline developer, a carboxylate related to the first range is generated and remains in the resulting pattern. However, the carboxylate can be converted to a carboxylate ester related to the second range by a subsequent heat treatment. That is, the component of the microflow path 14 (the partition material 12 in this embodiment) can be modified as if by performing a surface treatment, and thus a resin region 21 satisfying the ratio (Aa / Ac) can be obtained. Therefore, unintended fluid movement that may be induced by capillary action can be reduced.

[0027] The maximum peak intensity (Aa) and the maximum peak intensity (Ac) can be adjusted by appropriately changing the raw material composition of the component (partition material 12 in this embodiment) of the microchannel 14 having the resin region 21, the manufacturing method, etc. Among these, with regard to the manufacturing method, the type of alkaline developer, the exposure and development conditions, and further the subsequent heating conditions, etc. can be appropriately changed. If the conditions are such that carboxylate is easily generated and remains in the resulting pattern after development, the maximum peak intensity (Aa) can be adjusted to be large and the maximum peak intensity (Ac) can be adjusted to be small. On the other hand, if the conditions are such that carboxylate is easily converted to carboxylic acid or carboxylate ester, the maximum peak intensity (Aa) can be adjusted to be small and the maximum peak intensity (Ac) can be adjusted to be large.

[0028] From the viewpoint of reliably obtaining the effects according to this embodiment as described above, the ratio (Aa / Ac) is preferably 0.100 or less, more preferably 0.085 or less, and even more preferably 0.050 or less.

[0029] The resin region 21 further includes: 1625~1645cm -1 The maximum peak intensity (Ad) in the third range; Maximum peak intensity (Ac), It is preferable that the ratio (Ad / Ac) is greater than 0 and equal to or less than 0.150. Among the main functional groups that exhibit energy absorption in the third range, functional groups derived from photopolymerizable double bonds are included. Some of these are usually confirmed in the components of the microchannel 14 (the partition material 12 in this embodiment). Therefore, adjusting the ratio (Ad / Ac) using the maximum peak intensity (Ad) in the third range to a relatively small range leads to controlling the maximum peak intensity (Ac) to a relatively large value. This also leads to controlling the ratio (Aa / Ac) to a relatively small range. In particular, the smaller absorption derived from the photopolymerizable double bonds indicates that the crosslinking has progressed, which is preferable from the viewpoint of suppressing the outflow of materials from the partition material. Therefore, by making the ratio (Ad / Ac) satisfy the above range, it becomes easier to reduce unintended fluid movement that may be induced by capillary action.

[0030] The third range includes an absorption intensity corresponding to the stretching vibration of a carbon-carbon (C=C) bond derived from a carbon-carbon double bond. Such a bond is usually found in a component of the microchannel 14 (the partition material 12 in this embodiment). Therefore, from the above viewpoint, it becomes easier to reduce unintended fluid movement that may be induced by capillary action.

[0031] The resin region 21 is substantially free of components derived from an alkali metal salt, which makes it easier to reduce unintended fluid movement that may be induced by capillary action. Examples of alkali metal salts include those derived from an organic base aqueous solution, specifically, those derived from an alkali developer, such as sodium.

[0032] The resin region 21 is preferably derived from a resin containing a (meth)acrylic resin. This makes it easy to form the resin region 21 in a component of the microchannel 14 (the partition material 12 in this embodiment) after employing a technique for producing the flow channel pattern 15 using a dry film. In particular, from the above viewpoint, the resin region 21 is derived from the following components: (a) Alkali-soluble polymers; (b) addition polymerization monomers; and (c) a photopolymerization initiator or a decomposition product thereof (hereinafter simply referred to as “photopolymerization initiator”); It is preferable that the photosensitive resin composition is derived from a resin containing the photosensitive resin composition.

[0033] A component of the microchannel 14 (the partition material 12 in this embodiment) has a resin region 21 at least in a part. When the component has a region (other region: not shown) that does not correspond to the resin region 21, the boundary between the resin region 21 and the other regions in the component does not need to be clear. If the process for making the resin region 21 is applied only to a specific portion of the component, it is highly likely that the resin region 21 will be made only in the specific portion and its related portions. On the other hand, the process for making the resin region 21 can be applied to substantially the entire component, and in this case, the resin region 21 will be made substantially throughout the entire component. In this case, if it is confirmed that the resin region 21 has been made in a certain place in the component, it is highly likely that the resin region 21 has also been made in other places. In this regard, if the process for producing the resin region 21 is basically applied to the entire component, without being deliberately not applied to specific locations in the component, this falls under the term "substantially the entire component" above.

[0034] FIG. 2(b) is an enlarged cross-sectional view showing another configuration example within the region A in FIG. 1(a). 2(b), in a structure 10A according to another configuration example, in a component of a microchannel 14A (partition material 12A in this embodiment), at least a part of a region exposed in the channel is covered with a coating layer 22 that does not correspond to the resin region 21A. The coating layer 22 is, for example, a fluorine coating layer. In this regard, the resin region 21A does not have to be exposed to the inner surface of the flow path as long as the effect of the present embodiment can be obtained. As long as the effect of the present embodiment can be obtained, most of the region exposed in the flow path (50% or more, 80% or more, 90% or more, or 95% or more of the total exposed area) may be covered by the coating layer 22 that does not correspond to the resin region 21A.

[0035] Here, the resin region 21 has the following formula (1): P = [(1 / h) cos{(θs / 180) π} + (1 / h)·cos{(θb / 180)·π}+ (2 / w) cos{(θ / 180) π}] 10 6 ... (1) {In the formula, θs: Water contact angle of the flow path forming surface 13a of the lid member 13 (deg: degrees) θb: Water contact angle (deg) of the flow path forming surface 11a of the base material 11 θ: Water contact angle of the flow path forming surface 12a of the partition material 12 (deg: degree) h: length (μm) of the flow path forming surface 12a of the partition material 12 when the structure 10 is cut along the thickness direction w: length (μm) of the flow channel forming surface 11a of the base material 11 when the structure 10 is cut along the thickness direction It is preferable that P(1 / μm) represented by the following formula is 1650 or less. In this case, by controlling the interfacial tension between the substrate 11, the partition material 12, and the cover material 13, which form the flow path forming surface, within a predetermined range, the stability of fluid transport is further improved, and it becomes easier to reduce unintended fluid movement that may be induced by capillary action.

[0036] FIG. 3 is a diagram for explaining an example of the structure 10, and the meaning of the above formula will be explained with reference to this diagram. First, the capillary force in a microchannel is affected by the interfacial tension on the channel formation surface (for example, the interfacial tension at room temperature). Also, The interfacial tension (N) of the flow path forming surface 13a of the cover member 13 is (T·10 -6 )·w·cos{(θs / 180)·π}; The interfacial tension (N) of the flow path forming surface 11a of the substrate 11 is (T·10 -6 )·w·cos{(θb / 180)·π}; The interfacial tension (N) of the flow passage forming surface 12a of the partition material 12 is (T·10 -6 )·2h·cos{(θ / 180)·π}; (In the formula, it is assumed that the partition material 12 has two flow path forming surfaces 12a facing each other. T: surface tension of water (N / m)) is affected.

[0037] And the mass of the fluid in the microchannel is the length h (μm) of the flow channel forming surface 12a of the partition material 12 when the structure 10 is cut along the thickness direction; the length w (μm) of the flow channel forming surface 11a of the substrate 11 when the structure 10 is cut along the thickness direction; Length of flow path H (μm); density of fluid ρ (Kg / m 3 );Gravity g(m / s 2 ); This is related to the product hwHρg.

[0038] In this case, when the surface tension of water, T (N / m), is used, the interfacial tension on the flow channel forming surface and the mass of the fluid in the micro flow channel are used to obtain the following relationship: hwHρg 10 -18 =T·[w·cos{(θs / 180)·π}+w·cos{(θb / 180)·π}+2h·cos{(θ / 180)·π}]·10 -6 is represented.

[0039] The present inventors have found that the above factors affecting the capillary force can be treated as a function of the water contact angle of the flow channel surface and the size of the micro flow channel. h, w and 10 for the size of the microchannel -12 Moving to the right side of the above equation and T to the left side, the equation becomes: (Hρg / T) 10 -6 =[(1 / h)·cos{(θs / 180)·π}+(1 / h)·cos{(θb / 180)·π}+(2 / w)·cos{(θ / 180)·π}]·10 6 The left side is expressed as a function of the water contact angle of the flow channel surface and the size of the micro flow channel, as shown on the right side. The right side in this case corresponds to the above (1). In this case, the left side is (Hρg / T)·10 -6 It is expressed as:

[0040] The interfacial tension between the flow channel surface and water can be derived from the water contact angle of the flow channel surface, and the tendency of the effect of these changes on P is as described above. Furthermore, as the size of the flow channel (cross-sectional area of ​​the flow channel) becomes smaller, liquid transfer tends to become difficult. Using these tendencies as indicators, it is possible to control P to be ≦ 1650 by appropriately adjusting the configuration of the microchannel and the respective constituent materials. In theory, P can be a negative value, and may be 0 or more.

[0041] The value "1650" expressed in terms of magnitude relationship with P is determined by taking into consideration the assumed structure and use of the structure of this embodiment, as well as the type of fluid, etc., and is expressed by (Hρg / T)·10 -6 This is a value calculated as the above, which is a value that makes it easier to reduce unintended fluid movement that may be induced by capillary action. Since the sum of the capillary forces on the four sides that make up the flow path is within a certain range, the value at which the target aqueous solution can be stopped in the flow path when no driving force for liquid transfer is applied corresponds to the above numerical value "1650".

[0042] The resin region 21 described above is provided in at least a part of the component of the microchannel 14. In the present embodiment, the partition material 12 is used as an example of the component in which the resin region 21 is provided, but the resin region 21 may be provided in the base material 11. That is, the resin region 21 is When provided on the substrate 11, When provided on the partition wall material 12, and When provided on the substrate 11 and the partition material 12, Either is acceptable.

[0043] (Other configurations) The substrate 11 may be made of either a light-transmitting material or a light-non-transmitting material, and is preferably made of a light-transmitting material such as resin or glass, and more preferably made of resin. Note that the term "light-transmitting" is broadly interpreted to mean that light can pass through, regardless of whether the material is colored or colorless, and regardless of the degree of light transmittance. The substrate 11 may have a multi-layer structure, in which a plurality of layers made of a light-transmitting material may be laminated, a plurality of layers made of a non-light-transmitting material may be laminated, or a layer made of a light-transmitting material and a layer made of a non-light-transmitting material may be laminated. The number of layers of the substrate 11 is not limited, but for example, FIG. 1(a) shows a multi-layer substrate 11 having a first layer 11A having an adhesive layer AD and a second layer 11B from the inside of the flow path. The layer constituting the flow path forming surface 11a of the substrate 11 is preferably made of a material that is advantageous for the stability of fluid delivery, for example, a light-transmitting material, particularly a resin. The layers after the first layer 11A (the second layer 11B in FIG. 1(a)) are preferably made of a material that is advantageous for heat resistance, for example, a light-transmitting material, particularly glass. The adhesive layer AD can be omitted, but it is preferable that the first layer 11A has the adhesive layer AD, since this improves the adhesion between the first layer 11A and the second layer 11B via the adhesive layer AD.

[0044] The flow channel forming surface 11a (for example, the surface of the first layer 11A) of the substrate 11 has a water contact angle of 40 to 150 degrees. In this manner, by controlling the degree of hydrophilicity, unintended fluid movement that may be induced by capillary action can be reduced. The water contact angle is preferably 60 to 130 degrees, more preferably 80 to 120 degrees, and even more preferably 90 to 120 degrees. In general, the larger the contact angle, the more likely it is that unintended fluid movement caused by capillary action is to be prevented. In this embodiment, even in such a situation where it is likely that prevention of unintended fluid movement caused by capillary action is desired, unintended fluid movement that may be induced by capillary action can be reduced.

[0045] The water contact angle can be adjusted by the composition and preparation conditions for obtaining the substrate 11, as well as the heat treatment conditions, etc. By adjusting the amount of hydrophilic components to be increased, the water contact angle tends to be smaller, and by adjusting the amount of hydrophilic components to be decreased, the water contact angle tends to be larger. When the resin region 21 is provided in the substrate 11, the region in the substrate 11 whose water contact angle is in the above range may overlap with the resin region 21 or may be different from the resin region 21.

[0046] From the viewpoint of suitability for forming a microchannel, examples of the resin constituting the base material 11 and / or the adhesive layer AD include acrylic resin, polypropylene, polycarbonate resin, cycloolefin resin, polystyrene resin, polyester resin, urethane resin, vinyl chloride resin, silicone resin, fluorine-based resin, etc. In addition, examples of the resin constituting the base material 11 and / or the adhesive layer AD include resins that can be used as the partition material 12.

[0047] Examples of non-transparent materials include silicon wafers and copper-clad laminates. When the state of the fluid in the flow path is detected by electrical conductivity or the like, for example, an electric circuit board on which metal wiring is formed is used. The substrate 11 may be smooth or have an uneven shape. Examples of the uneven shape include a micro flow path through which the fluid passes formed on the surface, and an electric circuit made of metal wiring formed on the surface. The thickness of the substrate 11 (the total thickness when the substrate 11 has a multi-layer structure) is not particularly limited, but is preferably 10 μm to 10 mm.

[0048] The size of the microchannel 14 is selected depending on the purpose, and may be, for example, a width of 1 to 1000 μm or 10 to 70 μm and a depth of 1 to 1000 μm or 5 to 750 μm. In one embodiment, the flow channel forming surface of the microchannel may be flat or uneven, and the angle between the bottom surface and the side surface, and between the side surface and the cover surface may be approximately right angles, but the shape of the microchannel is not limited to this and may be designed depending on the purpose.

[0049] The lid material 13 is preferably made of a material that is resistant to fluids, and when the state of the fluid in the flow path is detected by light, a lid material 13 that is highly transparent to the light is used. The thickness of the lid material 13 is selected depending on the purpose, and is, for example, 10 μm to 10 mm. The lid material 13 may be made of either the above-mentioned light-transmitting material or the above-mentioned non-light-transmitting material, and may be made of, for example, a light-transmitting material (such as glass).

[0050] (Microfluidic device to which the structure can be applied) A microchannel device 1 to which the structure 10 according to this embodiment can be applied will be described. The microchannel device 1 is a device equipped with micro-order size channels, and can be used as various microchannel devices such as a POCT kit, an ELISA (Enzyme-Linked ImmunoSorbent Assay) device, a microreactor, etc. The microchannel device 1 includes a substrate 1, a partition material 12 formed by photolithography using a photosensitive resin laminate, and a cover material 13 arranged to cover the partition material 12.

[0051] In a compact disc (CD) type ELISA device, a liquid tank for storing a liquid, an analysis section for detecting, reacting, adsorbing, desorbing or decomposing the liquid, and a microchannel for connecting the liquid tank and the analysis section and flowing the liquid between them are formed on a disk-shaped substrate, and the flow channel pattern is sealed with a lid. In this case, the diameter of the substrate is about 10 cm, the minimum flow channel width of the microchannel is about 45 μm, and the depth of the microchannel is about 300 μm. The number of analysis sections on the substrate is, for example, 4 to 20, or 14 to 16. The liquid is sent from the center to the outside in the radial direction by utilizing the centrifugal force caused by the rotation of the substrate, and is supplied to each analysis section from the liquid tank through the microchannel.

[0052] A microchannel device that can use the structure according to this embodiment is not limited to the above example, and typically includes: A substrate having an electrode; an electrode protection layer provided on the substrate for protecting the electrodes; and a structure having a microchannel, which is laminated on the substrate and / or the electrode protection layer.

[0053] The electrodes can be made of, for example, a conductive material and are electrically connected to any suitable control circuit or sensor mounted on the microchannel device. The electrode protection layer can be made of, for example, various resin materials. A dry film may be used as the electrode protection layer.

[0054] [Photosensitive resin laminate] The above structure can be obtained by utilizing the photosensitive resin laminate according to this embodiment. That is, this embodiment provides a photosensitive resin laminate for a microchannel device, which is composed of a support film and a photosensitive resin layer. The phrase "composed of a support film and a photosensitive resin layer" means that the laminate is substantially composed of a support film and a photosensitive resin layer, but does not exclude the possibility that other elements may be present within a range that does not impair the effects of the present invention. The photosensitive resin laminate for a microchannel device according to this embodiment (hereinafter, also simply referred to as "photosensitive resin laminate") has properties that are particularly suitable for forming a microchannel by photolithography, and can be used, for example, as a substrate for a microchannel (for example, the first layer 11A in FIG. 1(a)), a partition material, a cover material, etc.

[0055] In a preferred embodiment, the photosensitive resin layer is composed of a photosensitive resin composition having a ratio (I / O) of inorganic value (I) to organic value (O) of 1.0 or less.

[0056] The ratio (I / O) of inorganic value (I) to organic value (O), also called the I / O value or inorganic value / organic value, is a value that represents the polarity of a component or compound in terms of an organic concept, and is a type of functional group contribution method in which parameters are set for each functional group.

[0057] The ratio (I / O) is explained in detail in documents such as Organic Concept Diagram (Koda Yoshio, Sankyo Publishing (1984)); KUMAMOTO PHARMACEUTICAL BULLETIN, No. 1, pages 1-16 (1954); and Chemistry Area, Vol. 11, No. 10, pages 719-725 (1957). The ratio (I / O) is a measure that classifies the properties of a component or compound broadly into organic groups that exhibit covalent bonding and inorganic groups that exhibit ionic bonding, and indicates the positions of these groups on a rectangular coordinate system named the organic axis and inorganic axis.

[0058] The inorganic value (I) is a numerical value of the influence of various substituents or bonds on the boiling point of an organic compound, based on the hydroxyl group. Specifically, the distance between the boiling point curve of a straight-chain alcohol and that of a straight-chain paraffin is about 100°C when taken around the carbon number of 5, so the influence of one hydroxyl group is set to 100, and the value obtained by quantifying the influence of various substituents or various bonds on the boiling point based on this value is the inorganic value (I) of the substituents of the organic compound. For example, the inorganic value (I) of a -COOH group is 150, and the inorganic value (I) of a double bond is 2. Therefore, the inorganic value (I) of a certain organic compound means the sum of the inorganic values ​​(I) of various substituents or bonds that the compound has.

[0059] The organic value (O) is determined based on the influence of the carbon atom representing the methylene group on the boiling point, using the methylene group in the molecule as a unit. In other words, the average boiling point rise caused by the addition of one carbon atom in linear saturated hydrocarbon compounds with carbon numbers of 5 to 10 is 20°C, so based on this, the organic value of one carbon atom is set to 20, and the organic value (O) is a value that quantifies the influence of various substituents or bonds on the boiling point based on this. For example, the organic value (O) of the nitro group (-NO2) is 70.

[0060] In general, the closer the ratio (I / O) is to 0, the more non-polar (more hydrophobic, more organic) the organic material is, while the larger the value, the more polar (more hydrophilic, more inorganic) the organic material is. The ratio (I / O) of the photosensitive resin layer is preferably 1.0 or less, more preferably 0.9 or less, even more preferably 0.8 or less, and particularly preferably 0.7 or less, from the viewpoint of the resistance (fluid resistance) of the photosensitive resin laminate to the fluid flowing through the microchannel. The ratio (I / O) is preferably 0.0 from the viewpoint of fluid resistance, but may be 0.1 or more, 0.2 or more, or 0.3 or more, from the viewpoint of the ease of manufacture and developability of the photosensitive resin laminate. The above ratio (I / O) is a value calculated based on the base resin and monomer of the photosensitive resin composition (i.e., excluding the photopolymerization initiator and additives).

[0061] The components of the photosensitive resin laminate for a microchannel device according to this embodiment will be described below.

[0062] <Photosensitive resin layer> The photosensitive resin layer can be formed by applying a photosensitive resin composition to a support film, drying and laminating the composition. The photosensitive resin composition can contain any polymer and / or monomer as long as it can impart photosensitivity to the photosensitive resin laminate, and may further contain a photopolymerization initiator, other additives, and the like, as desired.

[0063] From the viewpoints of formability of a microchannel device member by photolithography, lamination property between the photosensitive resin laminate and the substrate of the microchannel device, etc., the photosensitive resin composition preferably contains (a) an alkali-soluble polymer containing a carboxyl group, (b) an addition-polymerizable monomer, and (c) a photopolymerization initiator, as described above. In addition, the photosensitive resin composition may contain an epoxy resin such as EPON (registered trademark) SU-8 type resin or bisphenol A novolac epoxy resin, so long as the photosensitive resin layer can be formed into a film using the photosensitive resin composition.

[0064] (a) Alkali-soluble polymers containing carboxyl groups (a) The alkali-soluble polymer containing a carboxyl group has an α,β-unsaturated carboxyl group-containing monomer as a polymerization component, and the acid equivalent of the alkali-soluble polymer is preferably 100 to 600 and the weight average molecular weight is preferably 5,000 to 500,000. The carboxyl group in the alkali-soluble polymer containing a carboxyl group is necessary for the photosensitive resin composition to have developability or strippability with respect to an organic base aqueous solution (for example, a developer or stripper containing an alkaline aqueous solution). The acid equivalent refers to the mass of the alkali-soluble polymer having one equivalent of a carboxyl group therein. The more preferred lower limit of the acid equivalent is 250, and the more preferred upper limit is 450. The acid equivalent of (a) the alkali-soluble polymer containing a carboxyl group is preferably 100 or more from the viewpoints of improving development resistance, improving resolution and adhesion between the cured product of the photosensitive resin layer (also referred to as "cured resist film" in this disclosure) and other members, and further ensuring compatibility with the solvent or other components in the photosensitive resin composition, particularly the (b) addition polymerizable monomer described below, and is preferably 600 or less from the viewpoint of improving developability and peelability. The acid equivalent is measured by potentiometric titration using 0.1 mol / L sodium hydroxide using a Hiranuma automatic titrator (COM1750) manufactured by Hiranuma Sangyo Co., Ltd.

[0065] The weight average molecular weight of the (a) alkali-soluble polymer containing a carboxyl group is preferably 5,000 to 500,000. The weight average molecular weight is preferably 5,000 or more from the viewpoint of improving the fluid resistance of the photosensitive resin laminate, suppressing air from entering the microchannel during lamination, and obtaining resistance to the developer by making the thickness of the photosensitive resin laminate uniform, and is preferably 500,000 or less from the viewpoint of maintaining developability. In order to achieve both fluid resistance and developability, the lower limit of the weight average molecular weight of the (a) alkali-soluble polymer containing a carboxyl group is more preferably 10,000 or more, 20,000 or more, or 40,000 or more, and the upper limit is more preferably 250,000 or less, 200,000 or less, 150,000 or less, or 100,000 or less.

[0066] The weight average molecular weight in this specification means a weight average molecular weight measured by gel permeation chromatography (GPC) using a calibration curve of polystyrene (Shodex STANDARD SM-105 manufactured by Showa Denko K.K.). (a) The weight average molecular weight of an alkali-soluble polymer containing a carboxyl group can be measured using a gel permeation chromatography manufactured by JASCO Corporation under the following conditions: Differential Refractometer: RI-1530 Pump: PU-1580 Degasser: DG-980-50 Column oven: CO-1560 Columns: KF-8025, KF-806M x 2, KF-807 Eluent: THF.

[0067] The (a) alkali-soluble polymer containing a carboxyl group is preferably a (co)polymer containing, as a component, one or more monomers selected from the first and second monomers described below.

[0068] The first monomer is a carboxylic acid or an acid anhydride having one polymerizable unsaturated group in the molecule. Examples include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, maleic anhydride, and maleic acid half ester. Among them, (meth)acrylic acid is preferred from the viewpoint of alkaline developability.

[0069] The second monomer is a monomer that is non-acidic and has at least one polymerizable unsaturated group in the molecule. Examples of the second monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, esters of vinyl alcohol such as vinyl acetate, (meth)acrylonitrile, styrene, and polymerizable styrene derivatives. Among these, from the viewpoint of the resolution of the flow path pattern, at least one selected from the group consisting of methyl (meth)acrylate, n-butyl (meth)acrylate, styrene, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and benzyl (meth)acrylate is preferred, and benzyl (meth)acrylate is more preferred.

[0070] In this specification, "(meth)acrylic" means "acrylic" and the corresponding "methacrylic", "(meth)acrylate" means "acrylate" and the corresponding "methacrylate", and "(meth)acryloyl" means "acryloyl" and the corresponding "methacryloyl".

[0071] (a) The alkali-soluble polymer containing a carboxyl group can be synthesized by mixing the above-mentioned monomers, diluting the solution with a solvent such as acetone, methyl ethyl ketone, or isopropanol, adding an appropriate amount of a radical polymerization initiator such as benzoyl peroxide or azoisobutyronitrile, and heating and stirring. In some cases, the synthesis is performed while dropping a part of the mixture into the reaction solution. After the reaction is completed, further solvent is added to the reactants to adjust the concentration to the desired level. As a synthesis method, bulk polymerization, suspension polymerization, or emulsion polymerization may be used in addition to solution polymerization.

[0072] In the (a) alkali-soluble polymer containing a carboxyl group, the copolymerization ratio of the first monomer and the second monomer is preferably 10 to 60 mass % of the first monomer and 40 to 90 mass % of the second monomer, and more preferably 15 to 35 mass % of the first monomer and 65 to 85 mass % of the second monomer.

[0073] More specific examples of the (a) alkali-soluble polymer containing a carboxyl group include a polymer containing methyl methacrylate, methacrylic acid, and styrene as copolymerization components, a polymer containing methyl methacrylate, methacrylic acid, and n-butyl methacrylate as copolymerization components, a polymer containing methacrylic acid, benzyl methacrylate, and styrene as copolymerization components, a polymer containing methacrylic acid and benzyl methacrylate as copolymerization components, and a polymer containing methacrylic acid, 2-ethylhexyl acrylate, 2-hydroxyethyl methacrylate, and styrene as copolymerization components.

[0074] The content of (a) the alkali-soluble polymer containing a carboxyl group in the photosensitive resin composition is preferably 20 to 90 mass %, more preferably 40 to 60 mass %, based on the total solid content of the photosensitive resin composition. The content of (a) the alkali-soluble polymer containing a carboxyl group is preferably 20 mass % or more from the viewpoint of maintaining the resistance of the photosensitive resin composition in photolithography, and is preferably 90 mass % or less from the viewpoint of the flexibility of the photosensitive resin composition before curing and the resist pattern after curing.

[0075] (b) Addition-polymerizable monomer The (b) addition polymerizable monomer is a compound having at least one polymerizable ethylenically unsaturated bond in the molecule. The ethylenically unsaturated bond is preferably a terminal ethylenically unsaturated group. From the viewpoint of high resolution of the flow path pattern and the shape of the partition wall, it is preferable to use, as the (b) addition polymerizable monomer, at least one selected from the group consisting of bisphenol A-based (meth)acrylate compounds, polyfunctional monomers, monomers having a repeating unit of alkylene oxide, cyclic monomers, and aromatic monomers.

[0076] In this specification, a bisphenol A-based (meth)acrylate compound refers to a compound having a (meth)acryloyl group or a carbon-carbon unsaturated double bond derived from a (meth)acryloyl group and a -C6H4-C(CH3)2-C6H4- group derived from bisphenol A. Specific examples include dimethacrylate of polyethylene glycol having an average of 1 mole unit of ethylene oxide added to each end of bisphenol A, dimethacrylate of polyethylene glycol having an average of 2 mole units of ethylene oxide added to each end of bisphenol A (NK Ester BPE-200 manufactured by Shin-Nakamura Chemical Co., Ltd.) or dimethacrylate of polyethylene glycol having an average of 5 mole units of ethylene oxide added to each end of bisphenol A (NK Ester BPE-500 manufactured by Shin-Nakamura Chemical Co., Ltd.), dimethacrylate of polyalkylene glycol having an average of 6 mole units of ethylene oxide and an average of 2 mole units of propylene oxide added to each end of bisphenol A, and dimethacrylate of polyalkylene glycol having an average of 15 mole units of ethylene oxide and an average of 2 mole units of propylene oxide added to each end of bisphenol A.

[0077] Examples of the (b) addition polymerizable monomer other than bisphenol A (meth)acrylate compounds include 4-nonylphenylheptaethylene glycol dipropylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, phenoxyhexaethylene glycol acrylate, a reaction product of a half ester compound of phthalic anhydride and 2-hydroxypropyl acrylate with propylene oxide (manufactured by Nippon Shokubai Kagaku, product name OE-A200), dimethacrylate of polyethylene glycol having an average of 4 moles of ethylene oxide added thereto, dimethacrylate of glycol having an average of 3 moles of ethylene oxide added to each end of polypropylene glycol having an average of 12 moles of propylene oxide added thereto, and dimethacrylate of polybutylene glycol having an average of 28 moles of butylene oxide added thereto; polyoxyalkylene glycol di(meth)acrylates such as 4-n-octylphenoxypentapropylene glycol acrylate, 1,6-hexanediol (meth)acrylate, 1,4-cyclohexanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate, 2-di(p-hydroxyphenyl)propane di(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri-, tetra-, or penta(meth)acrylate, and trimethylolpropane triglycidyl ether tri(meth)acrylate; 2,2-bis(4-(meth)acryloxypentaethoxyphenyl)propane, 2,2-bis(4-((meth)acryloxypentaethoxy)cyclohexyl)propane; Examples of the polyfunctional (meth)acrylates include those containing a urethane group, such as a urethane compound of hexamethylene diisocyanate and nonapropylene glycol monomethacrylate, dimethacrylates of polyurethane diols synthesized from polybutylene glycol to which an average of 28 moles of butylene oxide has been added and hexamethylene diamine, and polyfunctional (meth)acrylates of isocyanuric acid ester compounds. Examples of the polyfunctional (meth)acrylates include triacrylates in which an average of 3 moles of ethylene oxide has been added to trimethylolpropane. These may be used alone or in combination of two or more kinds, and may also be used in combination with bisphenol A-based (meth)acrylate compounds.

[0078] The content of the (b) addition polymerizable monomer in the photosensitive resin composition is preferably 5 to 75 mass %, more preferably 15 to 70 mass %, and even more preferably 20 to 55 mass %, based on the total solid content of the photosensitive resin composition. The content of the (b) addition polymerizable monomer is preferably 5 mass % or more from the viewpoints of resolution and adhesion between the cured resist film and other members, and is preferably 75 mass % or less from the viewpoint of flexibility of the cured resist film.

[0079] (c) Photopolymerization initiator (c) As the photopolymerization initiator, any of those commonly used as photopolymerization initiators for photosensitive resins can be used as appropriate, for example, hexaarylbisimidazole (hereinafter also referred to as triarylimidazolyl dimer).

[0080] Examples of triaryl imidazolyl dimers include 2-(o-chlorophenyl)-4,5-diphenylimidazolyl dimer (hereinafter also referred to as "2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,1'-bisimidazole"), 2,2',5-tris-(o-chlorophenyl)-4-(3,4-dimethoxyphenyl)-4',5'-diphenylimidazolyl dimer, and 2,4-bis-(o-chlorophenyl)-5-(3,4-dimethoxyphenyl)-diphenylimidazolyl dimer; 2,4,5-tris-(o-chlorophenyl)-diphenylimidazolyl dimer, 2-(o-chlorophenyl)-bis-4,5-(3,4-dimethoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2-fluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3-difluoromethylphenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,4-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer; 2,2'-bis-(2,5-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,6-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3,4-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer; 2,2'-bis-(2,3,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,4,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,4,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer; Examples include 2,2'-bis-(2,3,4,5-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3,4,6-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, and 2,2'-bis-(2,3,4,5,6-pentafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer.

[0081] Among them, 2-(o-chlorophenyl)-4,5-diphenylimidazolyl dimer is preferred because it has a high effect on the resolution and strength of the cured resist film. These may be used alone or in combination of two or more kinds, and may also be used in combination with an acridine compound, a pyrazoline compound, etc. described below.

[0082] (c) As the photopolymerization initiator, an acridine compound or a pyrazoline compound can also be used. Examples of the acridine compound include acridine, 9-phenylacridine, 9-(4-tolyl)acridine, 9-(4-methoxyphenyl)acridine, 9-(4-hydroxyphenyl)acridine, 9-ethylacridine, 9-chloroethylacridine, 9-methoxyacridine, and 9-ethoxyacridine; 9-(4-methylphenyl)acridine, 9-(4-ethylphenyl)acridine, 9-(4-n-propylphenyl)acridine, 9-(4-n-butylphenyl)acridine, 9-(4-tert-butylphenyl)acridine, 9-(4-ethoxyphenyl)acridine, 9-(4-acetylphenyl)acridine, 9-(4-dimethylaminophenyl)acridine, 9-(4-chlorophenyl)acridine; Examples of such acridine include 9-(4-bromophenyl)acridine, 9-(3-methylphenyl)acridine, 9-(3-tert-butylphenyl)acridine, 9-(3-acetylphenyl)acridine, 9-(3-dimethylaminophenyl)acridine, 9-(3-diethylaminophenyl)acridine, 9-(3-chlorophenyl)acridine, 9-(3-bromophenyl)acridine, 9-(2-pyridyl)acridine, 9-(3-pyridyl)acridine, and 9-(4-pyridyl)acridine. Of these, 9-phenylacridine is preferred. It is preferable to use the acridine compound in combination with a halogen compound from the viewpoint of the curing property after exposure of the photosensitive resin layer. Examples of the halogen compound include amyl bromide, isoamyl bromide, isobutylene bromide, ethylene bromide, diphenylmethyl bromide, benzal bromide, methylene bromide, tribromomethylphenylsulfone, carbon tetrabromide, tris(2,3-dibromopropyl)phosphate, trichloroacetamide, amyl iodide, isobutyl iodide, 1,1,1-trichloro-2,2-bis(p-chlorophenyl)ethane, hexachloroethane, and chlorinated triazine compounds. Among them, tribromomethylphenylsulfone is preferable from the viewpoint of curing property.

[0083] As the pyrazoline compound, 1-phenyl-3-(4-tert-butyl-styryl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-(4-(benzoxazol-2-yl)phenyl)-3-(4-tert-butyl-styryl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-octyl-phenyl)-pyrazoline are preferred.

[0084] Other photopolymerization initiators include, for example, quinones such as 2-ethylanthraquinone, octaethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, 2,3-dimethylanthraquinone, and 3-chloro-2-methylanthraquinone; aromatic ketones such as benzophenone, Michler's ketone [4,4'-bis(dimethylamino)benzophenone], and 4,4'-bis(diethylamino)benzophenone; benzoin ethers such as benzoin, benzoin ethyl ether, benzoin phenyl ether, methylbenzoin, and ethylbenzoin; Examples of the oxime esters include benzil dimethyl ketal, benzil diethyl ketal, combinations of thioxanthones and alkylaminobenzoic acids, and oxime esters such as 1-phenyl-1,2-propanedione-2-O-benzoin oxime and 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime. In cases where colorless transparency of the microchannel is required or from the viewpoint of suppressing fluorescence emission and facilitating detection of the luminescence signal of the microchannel device, an oxime compound is preferred. Examples thereof include Irgacure OXE01 and Irgacure OXE02 manufactured by BASF Japan Ltd. and ADEKA Arcles NCI-831 manufactured by ADEKA Corporation.

[0085] In addition, the combination of the above-mentioned thioxanthones and alkylaminobenzoic acids includes, for example, a combination of ethylthioxanthones and ethyl dimethylaminobenzoate, a combination of 2-chlorothioxanthones and ethyl dimethylaminobenzoate, and a combination of isopropylthioxanthones and ethyl dimethylaminobenzoate. In addition, N-arylamino acids may be used. Examples of N-arylamino acids include N-phenylglycine, N-methyl-N-phenylglycine, and N-ethyl-N-phenylglycine. Among them, N-phenylglycine is particularly preferred.

[0086] The content of the (c) photopolymerization initiator in the photosensitive resin composition is preferably within the range of 0.01 to 30 mass% based on the total solid content of the photosensitive resin composition, with a more preferred lower limit of 0.05 mass% or more, an even more preferred lower limit of 0.1 mass% or more, and a more preferred upper limit of 15 mass% or less, and an even more preferred upper limit of 10 mass% or less. The content of the (c) photopolymerization initiator is preferably 0.01 mass% or more from the viewpoint of obtaining sufficient sensitivity during photopolymerization by exposure, and is preferably 30 mass% or less from the viewpoint of sufficiently transmitting light to the bottom surface of the photosensitive resin composition (i.e., the part far from the light source) during photopolymerization, obtaining good resolution and good adhesion between the cured resist film and other members.

[0087] (d) Other additives The photosensitive resin composition may contain various additives in addition to the above components (a) to (c).

[0088] For example, in order to improve the thermal stability and storage stability of the photosensitive resin composition, it is preferable to incorporate at least one compound selected from the group consisting of radical polymerization inhibitors, benzotriazoles, carboxybenzotriazoles, and hindered phenol-based antioxidants in the photosensitive resin composition.

[0089] Examples of the radical polymerization inhibitor include p-methoxyphenol, hydroquinone, pyrogallol, naphthylamine, tert-butylcatechol, cuprous chloride, 2,6-di-tert-butyl-p-cresol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), nitrosophenylhydroxylamine aluminum salt (N-nitroso-N-phenylhydroxylamine aluminum), and diphenylnitrosamine.

[0090] Examples of benzotriazoles include 1,2,3-benzotriazole, 1-chloro-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-tolyltriazole, and bis(N-2-hydroxyethyl)aminomethylene-1,2,3-benzotriazole.

[0091] Examples of carboxybenzotriazoles include 4-carboxy-1,2,3-benzotriazole, 5-carboxy-1,2,3-benzotriazole, (N,N-dibutylamino)carboxybenzotriazole, N-(N,N-di-2-ethylhexyl)aminomethylenecarboxybenzotriazole, N-(N,N-di-2-hydroxyethyl)aminomethylenecarboxybenzotriazole, and N-(N,N-di-2-ethylhexyl)aminoethylenecarboxybenzotriazole.

[0092] Examples of the hindered phenol-based antioxidant include the IRGANOX series from BASF Japan Ltd. and the Adeka STAB (AO) series from ADEKA Corporation.

[0093] Other examples of polymerization inhibitors include ethylene bis(oxyethylene) bis(3-5-tert-butyl-4-hydroxy-m-tolyl) propionate (trade name IRGANOX 245).

[0094] The total amount of radical polymerization inhibitor, benzotriazoles, carboxybenzotriazoles and / or hindered phenol antioxidant is preferably 0.001 to 3 mass% based on the total solid content of the photosensitive resin composition, with a more preferred lower limit of 0.05 mass% or more and a more preferred upper limit of 1 mass% or less. From the viewpoint of imparting storage stability to the photosensitive resin composition, this total amount is preferably 0.001 mass% or more, and from the viewpoint of maintaining sensitivity, preferably 3 mass% or less.

[0095] The photosensitive resin composition may contain other coloring substances as necessary, such as phthalocyanine green, crystal violet, methyl orange, Nile blue 2B, Victoria blue, malachite green, basic blue 20, diamond green, etc., or color-developing dyes such as leuco dyes or combinations of fluoran dyes and halogen compounds. Leuco dyes include, for example, tris(4-dimethylamino-2-methylphenyl)methane [leuco crystal violet], tris(4-dimethylamino-2-methylphenyl)methane [leucomalachite green], and fluoran dyes. Examples of halogen compounds include amyl bromide, isoamyl bromide, isobutylene bromide, ethylene bromide, diphenylmethyl bromide, benzal bromide, methylene bromide, tribromomethylphenylsulfone, carbon tetrabromide, tris(2,3-dibromopropyl)phosphate, trichloroacetamide, amyl iodide, isobutyl iodide, 1,1,1-trichloro-2,2-bis(p-chlorophenyl)ethane, hexachloroethane, and chlorinated triazine compounds.

[0096] The photosensitive resin composition may contain a plasticizer as necessary. Examples of the plasticizer include compounds obtained by modifying bisphenol A with polyalkylene oxide. Other examples of the plasticizer include sorbitan derivatives such as polyoxyethylene sorbitan laurate and polyoxyethylene sorbitan oleate, polyalkylene glycols such as polyethylene glycol and polypropylene glycol, phthalic acid esters such as diethyl phthalate, o-toluenesulfonic acid amide, p-toluenesulfonic acid amide, tributyl citrate, triethyl citrate, triethyl acetyl citrate, tri-n-propyl acetyl citrate, and tri-n-butyl acetyl citrate. In particular, it is preferable to use sorbitan derivatives and polyalkylene glycols.

[0097] The content of the plasticizer in the photosensitive resin composition is preferably 1 to 50 mass% based on the total solid content of the photosensitive resin composition, more preferably 3 mass% as the lower limit and 30 mass% as the upper limit. From the viewpoint of suppressing delay in development time and imparting flexibility to the cured film, the content is preferably 1 mass% or more, and from the viewpoint of suppressing insufficient curing, the content is preferably 50 mass% or less.

[0098] In one embodiment, the thickness of the photosensitive resin layer is preferably 100 μm or more, more preferably 120 μm or more, and even more preferably 240 μm or more, and may be preferably 720 μm or less, and more preferably 480 μm or less.

[0099] <Support film> The support film supports the photosensitive resin layer in the form of a film. The support film is preferably one that transmits light with wavelengths of 510 nm and 600 nm, as well as light emitted from an exposure light source. Examples of such support films include polyethylene terephthalate films, polyvinyl alcohol films, polyvinyl chloride films, vinyl chloride copolymer films, polyvinylidene chloride films, vinylidene chloride copolymer films, polymethyl methacrylate copolymer films, polystyrene films, polyacrylonitrile films, styrene copolymer films, polyamide films, and cellulose derivative films. These films may be stretched as necessary. From the viewpoint of resolution, films with a haze value of 5 or less are preferred. A haze value of 3 or less is more preferred, a haze value of 2.5 or less is even more preferred, and a haze value of 1 or less is even more preferred. The thinner the support film, the more advantageous it is in terms of image forming properties and economic efficiency, but from the viewpoint of the film thickness of the photosensitive resin laminate or the viewpoint of reducing the influence of thermal shrinkage during coating of the photosensitive resin layer, a film with a haze value of 10 to 30 μm is preferably used. For example, GR-19 and GR-16 manufactured by Teijin Films Limited, R310-16 and R340G16 manufactured by Mitsubishi Plastics, Inc., FB40 (16 μm film thickness) and FB60 (16 μm film thickness) manufactured by Toray Polyester Film Co., Ltd., and the like can be mentioned.

[0100] <Protective film> In one embodiment, the photosensitive resin laminate of the present embodiment is preferably combined with a protective film. In one embodiment, the protective film may be disposed on the photosensitive resin layer. The protective film may be any film as long as the protective film has a smaller adhesive force with the photosensitive resin layer than the supporting film and is peelable. For example, a polyethylene film, a polypropylene film, an oriented polypropylene film, etc. can be used as the protective film. In addition, a film having excellent peelability, such as that disclosed in JP-A-59-202457, can be used. The protective film is preferably a polypropylene film or a plastic film that has been subjected to a release treatment, from the viewpoint of good peelability, from the viewpoint of being peeled off from the photosensitive resin laminate when forming a microchannel device.

[0101] The thickness of the protective film is preferably 10 to 100 μm, more preferably 10 to 50 μm, from the viewpoint of the thickness and dimensional stability of the laminate of the photosensitive resin laminate and the protective film. Specific examples of the protective film include release-treated PET film 25X (thickness 25 μm) manufactured by Lintec Corporation, and GF-18, GF-818, and GF-858 manufactured by Tamapoly Co., Ltd.

[0102] <Method for producing photosensitive resin laminate> A known method can be used as a method for producing the photosensitive resin laminate. For example, the photosensitive resin composition constituting the photosensitive resin layer is mixed with a solvent to prepare a photosensitive resin composition preparation liquid, which is then applied to a support film using a blade coater or roll coater and dried, and a photosensitive resin layer made of the photosensitive resin composition is laminated on the support film to obtain the photosensitive resin laminate. If desired, a protective film may be further laminated on the photosensitive resin layer.

[0103] The photosensitive resin composition preparation is preferably prepared by adding a solvent so that the viscosity of the photosensitive resin composition preparation is 500 to 4000 mPa·sec at 25° C. The solvent may be appropriately selected from methyl ethyl ketone, acetone, ethanol, methanol, propanol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, toluene, etc., in view of the viscosity, drying property, remaining solvent amount, coatability, or foamability of the photosensitive resin composition preparation.

[0104] The photosensitive resin laminate can be used in a roll state by being wound around a core, optionally laminated with a protective film. The photosensitive resin laminate can be covered with a light-shielding sheet such as a polyethylene film from the viewpoint of suppressing adhesion of foreign matter and light exposure during storage or transportation.

[0105] [Method for manufacturing a microchannel device] <Summary> In a typical embodiment, the photosensitive resin laminate of the present embodiment is included in the microchannel device as a permanent film after exposure. In one embodiment, after exposure of the photosensitive resin layer, the support film is removed and only the cured resist film is included in the microchannel device. In another embodiment, after exposure of the photosensitive resin layer, the support film is not removed and the support film and the cured resist film are included in the microchannel device.

[0106] The microchannel device can be manufactured, for example, by a method including a step of forming a channel pattern on a substrate and a step of sealing the channel pattern by laminating a cover material onto the microchannel. Here, an example in which the photosensitive resin laminate of the present embodiment is used as a partition wall material will be described.

[0107] A method for producing a microfluidic device includes the steps of: (i-1) a step of applying a photosensitive resin composition solution containing a solvent having a boiling point of less than 100° C. to a support and drying the applied solution to form a photosensitive resin layer containing an alkali-soluble resin on the support; (i-2) laminating the photosensitive resin layer on a substrate; A step of preparing a photosensitive resin layer containing an alkali-soluble resin; (ii) developing the laminated photosensitive resin layer with an organic base aqueous solution to form a flow path pattern; (iii) A step of subjecting the flow path pattern to a heat treatment to perform a surface treatment on the flow path pattern, thereby producing a resin region derived from an alkali-soluble resin.

[0108] Here, the resin region is, in an infrared absorption spectrum by infrared spectroscopy, 1555~1575cm -1 A maximum peak intensity (Aa) in the first range; 1715~1735cm -1 The maximum peak intensity (Ac) in the second range of The ratio (Aa / Ac) is greater than 0 and less than 0.200.

[0109] The ratio (Aa / Ac) is as explained above. It should be noted that, without being limited to matters relating to the ratio (Aa / Ac), the preferred aspects relating to the structure explained above are also understood to be preferred aspects for the production method according to this embodiment.

[0110] In the step (i-1), a photosensitive resin composition solution containing a solvent having a boiling point of less than 100° C. is applied to a support and then dried. This makes it possible to produce a photosensitive resin layer containing an alkali-soluble resin on the support. The photosensitive resin composition solution may contain 80 mass % or more of the solvent having a boiling point of less than 100° C. based on the total amount of the solvent. In the step (i-2), the photosensitive resin layer is laminated on a substrate. For example, the photosensitive resin layer of the photosensitive resin laminate can be laminated on the substrate with the photosensitive resin layer side facing the substrate.

[0111] In the step (ii), the partition material is exposed in a pattern corresponding to a desired shape, and the support film is removed and developed. That is, the step (ii) can include a step of exposing the photosensitive resin layer before development. This makes it possible to suitably form a plurality of partition materials that are made of a cured resist film and that define microchannels.

[0112] In the above step (ii), the exposure step is preferably performed by direct imaging exposure without using a mask. Even for a fine pattern obtained by direct imaging exposure, the above structure can reduce unintended fluid movement that may be induced by capillary action.

[0113] In the above step (ii), the organic base aqueous solution may be an aqueous solution that functions as an alkaline developer capable of developing an alkali-soluble polymer containing a carboxyl group, such as an aqueous solution of tetramethylammonium hydroxide (TMAH), dimethylaminoethanol (DMAE), ammonia, monoethanolamine, diethanolamine, triethanolamine, or triethylamine.

[0114] Here, in the above step (iii), the flow path pattern is subjected to a heat treatment to perform a surface treatment on the flow path pattern, thereby producing a resin region derived from an alkali-soluble resin. The heat treatment can be carried out, for example, using a hot air circulation oven (such as SF-100C manufactured by Asahi Scientific Co., Ltd.). The heating temperature (curing temperature) is preferably from 90 to 180°C, more preferably from 110 to 160°C, and further preferably from 120 to 150°C. The heating time (curing time) is preferably from 30 to 700 minutes, more preferably from 60 to 450 minutes, and even more preferably from 90 to 400 minutes. Such a heat treatment makes it easier to convert the carboxylates that are generated and remain in the obtained pattern into carboxylic acids or carboxylate esters, and thus makes it easier to produce resin regions in which the ratio (Aa / Ac) is greater than 0 and less than or equal to 0.200.

[0115] After the above step (iii), a microchannel sealing step (iv) may be performed. In this step, the photosensitive resin laminate is laminated on at least the partition material so as to cover the channel pattern with the photosensitive resin layer side facing the partition material, and exposed to light throughout the entire surface, typically without removing the support film, to form a cover material composed of the support film and the cured resist film.

[0116] The lamination of the photosensitive resin laminate is preferably carried out under reduced pressure, more preferably at a vacuum degree of 30 to 70 Pa, and even more preferably at a vacuum degree of 40 to 60 Pa, from the viewpoint of forming a cured resist film with good dimensional accuracy.

[0117] When forming a cured resist film having a multi-layer structure, lamination of a single photosensitive resin layer, exposure and development may be repeated several times, or multiple photosensitive resin layers may be laminated in advance and then exposed at once. The batch exposure is preferable in that a cured resist film having excellent dimensional accuracy (i.e., little misalignment between layers) can be formed.

[0118] The photosensitive resin laminate according to this embodiment is particularly preferably applied to the partition material and / or the lid material of a compact disk (CD)-type microchannel device for ELISA. Hereinafter, an example of the configuration of a CD-type ELISA device will be described.

[0119] <Manufacturing Method of CD-Type ELISA Device> In an exemplary embodiment, the manufacturing method of a CD-type ELISA device includes the following steps: (1) A step of forming a plurality of partitions on a substrate to form a flow path pattern; (2) A step of providing through holes in the substrate; (3) A step of fitting an analysis part through the through holes from the back side of the substrate; (4) A step of laminating a lid material from the front side of the substrate; (5) Optionally, a step of partially cutting the substrate on which the flow path pattern is formed to trim the outer shape; and (6) Optionally, a step of cleaning the partitions. The order of each step can be freely changed before and after according to the efficiency of the manufacturing process.

[0120] When step (1) is performed by photolithography, if there is a protective film on the photosensitive resin laminate (when using the photosensitive resin laminate of this embodiment as the partition material, this photosensitive resin laminate), the protective film is peeled off, and the support film is maintained and laminated on the substrate. After exposure and development, the support film is removed to form a plurality of partition materials that define the microchannels.

[0121] Furthermore, when step (4) is performed by photolithography, the photosensitive resin laminate (when the photosensitive resin laminate of the present embodiment is used for a lid material, this photosensitive resin laminate) can be laminated onto a substrate and cured by exposure to form a permanent film consisting of a support film and a cured resist film. Specifically, the protective film (if present) is peeled off from the photosensitive resin laminate, and while maintaining the support film, lamination can be performed at about 0.18 m / min by a biaxial roll in the stacking order of the support film, the photosensitive resin layer, the CD-type ELISA device substrate, the CD-type ELISA device analysis part, and a jig that aligns the surface irregularities of the ELISA substrate as necessary on a single plane. The aforementioned jig is preferably made of a material that has low adhesion to the resist even during lamination, such as Teflon (registered trademark).

[0122] The structure including a microchannel, the manufacturing method thereof, and the microchannel device according to the present embodiment have been described above. The above embodiment is one aspect of the present invention, and various modifications can be made without departing from the scope of the present invention.

[0123] For example, in the present embodiment, the partition material includes a resin region. However, the base material may include a resin region, or the lid material may include a resin region. In either case, the base material includes a resin region, or the lid material includes a resin region, the manufacturing method thereof can be appropriately applied to the method of the partition material including a resin region described above. For example, when the substrate contains a resin region, the method may include a step of developing a substrate made of an alkali-soluble resin with an organic base aqueous solution to form a flow path pattern. Furthermore, for example, when the lid material includes a resin region, the method may include a step of developing a lid material made of an alkali-soluble resin with an organic base aqueous solution to form a flow path pattern. In either case, as described in the above embodiment, a resin region derived from a soluble resin may then be formed in the substrate and / or lid material by carrying out a process for producing the resin region. EXAMPLES

[0124] The present invention will be described below with reference to examples and comparative examples.

[0125] [Preparation of evaluation samples] The evaluation samples in the examples and comparative examples were prepared as follows.

[0126] <Preparation of Photosensitive Resin Laminate 1> A photosensitive resin composition 1A having the composition shown in Table 1 (in the table, "blended amount" indicates the blended amount (parts by mass) as solid content) and ethanol as a solvent were mixed and stirred to obtain a prepared solution. This prepared solution was applied to the surface of a 16 μm-thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., FB40) as a support using a blade coater. Thereafter, the mixture was dried at 95° C. for 40 minutes to form a photosensitive resin layer 1B, thereby obtaining a photosensitive resin laminate 1. The thickness of the photosensitive resin layer 1B was 120 μm. Next, a protective film (GF-818 manufactured by Tamapoly Co., Ltd.) was attached to the surface of the photosensitive resin layer 1B opposite to the support.

[0127] <Preparation of Photosensitive Resin Laminate 2> A photosensitive resin composition 2A having the composition shown in Table 2 (in the table, "blended amount" indicates the blended amount (parts by mass) as solid content) and ethanol as a solvent were mixed and stirred to obtain a prepared solution. This prepared solution was applied to the surface of a 16 μm-thick polyethylene terephthalate film (FB40, manufactured by Toray Industries, Inc.) as a support using a blade coater. Thereafter, the mixture was dried at 95° C. for 5 minutes to form a photosensitive resin layer 2B, thereby obtaining a photosensitive resin laminate 2. The thickness of the photosensitive resin layer 2B was 5 μm. Next, a protective film (GF-818 manufactured by Tamapoly Co., Ltd.) was attached to the surface of the photosensitive resin layer 2B opposite to the support.

[0128] <Preparation of Photosensitive Resin Laminate 3> A photosensitive resin composition 3A having the composition shown in Table 2 (in the table, "blended amount" indicates the blended amount (parts by mass) as solid content) and ethanol as a solvent were mixed and stirred to obtain a prepared solution. This prepared solution was applied to the surface of a 16 μm-thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., FB40) as a support using a blade coater. Thereafter, the mixture was dried at 95° C. for 5 minutes to form a photosensitive resin layer 3B, thereby obtaining a photosensitive resin laminate 3. The thickness of the photosensitive resin layer 3B was 50 μm. Next, a protective film (GF-818 manufactured by Tamapoly Co., Ltd.) was attached to the surface of the photosensitive resin layer 3B opposite to the support.

[0129] [Table 1]

[0130] [Example 1] <Preparation of substrate> The protective film on the photosensitive resin laminate 3 was peeled off, and the photosensitive resin laminate was laminated on a glass substrate (0.9 mm thick) so that the peeled surface was overlapped with the substrate. This resulted in a laminate in which the substrate, a 50 μm photosensitive resin layer, and a support were laminated. The lamination was performed using a normal pressure laminator (VA-400III manufactured by Taisei Laminator Co., Ltd.) under conditions of a speed of 0.2 m / min, a cylinder pressure of 0.2 MPa, and a roll temperature of 70°C. Next, the support on the photosensitive resin laminate 3 was peeled off. Next, the protective film on the photosensitive resin laminate 1 was peeled off, and the photosensitive resin laminate was laminated so that the peeled surface was overlapped with the photosensitive resin layer of the photosensitive resin laminate 3. This resulted in a laminate in which the substrate, the 50 μm photosensitive resin layer 3, the photosensitive resin layer 1, and the support were laminated. The lamination was performed using a normal pressure laminator (VA-400III manufactured by Taisei Laminator Co., Ltd.) under conditions of a speed of 0.2 m / min, a cylinder pressure of 0.2 MPa, and a roll temperature of 70° C.

[0131] Next, the photosensitive resin layer of this laminate was exposed to light using a scattered light exposure machine HMW-201KB manufactured by Oak Manufacturing Co., Ltd., at 500 mJ / cm 2 As described above, a multi-layered substrate having a photosensitive resin layer (first layer), an adhesive layer, and a glass substrate (second layer) was prepared.

[0132] <Formation of flow path pattern> The protective film on the photosensitive resin laminate 1 (also referred to as the first photosensitive resin laminate 1-1) was peeled off, and the first photosensitive resin laminate 1-1 was laminated on the first layer so that the peeled surface overlapped the first layer. This resulted in a laminate in which the substrate, the 120 μm photosensitive resin layer, and the support were laminated. The lamination was performed using a normal pressure laminator (VA-400III manufactured by Taisei Laminator Co., Ltd.) under conditions of a speed of 0.2 m / min, a cylinder pressure of 0.2 MPa, and a roll temperature of 70°C.

[0133] The support film was peeled off from the first photosensitive resin laminate 1-1 to expose the photosensitive resin layer 1B. Then, the protective film on another photosensitive resin laminate 1 (also referred to as the second photosensitive resin laminate 1-2) was peeled off, and the second photosensitive resin laminate 1-2 was laminated so that the photosensitive resin layer 1B (photosensitive resin layer 1B of the second photosensitive resin laminate 1-2) on the peeled surface overlaps the photosensitive resin layer 1B (photosensitive resin layer 1B of the first photosensitive resin laminate 1-1) laminated on the substrate. This resulted in a laminate in which the substrate, the photosensitive resin layer of 240 μm (i.e., 120 μm × 2), and the support were laminated. The lamination was performed in the same manner as above.

[0134] The above procedure was further repeated to obtain a laminate X in which a substrate, a 720 μm (that is, 120 μm×6) photosensitive resin layer, and a support were laminated. Next, the laminate X was exposed to a photosensitive resin pattern shown in FIG. 1. The exposure was performed using Nuvogo fine 10 manufactured by Orbotech Japan Co., Ltd. at 2000 mJ / cm. 2 The test was performed under conditions of ih light ratio of 0-100%.

[0135] Next, after peeling off the support film from the laminate X, a pattern was produced by spray developing for a developing time 1.5 times the minimum developing time. The development was carried out using a wafer developing machine AD-1200 manufactured by Takizawa Sangyo Co., Ltd., and the developer shown in the table. The "minimum developing time" referred to here is the time when the substrate surface was first visually confirmed during the development process. After development, the pattern was washed with pure water for 60 seconds and dried. The pattern was then heated (cured) in a hot air circulating oven under the conditions shown in Table 2. Next, the partition material was sealed by laminating it with a microchannel sealing material #9795 manufactured by 3M (referred to as "sealing material" in Table 3) at room temperature, thereby producing a structure equipped with a microchannel according to Example 1.

[0136] The partition wall material can also be sealed by the following method. That is, the protective film on the photosensitive resin laminate 2 is peeled off, and the photosensitive resin layer 2B on the peeled surface is laminated so as to overlap the above-mentioned structure (photosensitive resin layer). Then, the partition wall material is exposed to 500 mJ / cm2 of a scattered light exposure machine (HMW-201KB manufactured by Oak Seisakusho). 2 The partition wall material is then sealed with a lid material.

[0137] [Example 2] to [Example 6] and [Comparative Example 1] to [Comparative Example 4] A structure provided with a microchannel was produced in the same manner as in Example 1, except that the conditions shown in Table 2 were adopted.

[0138] [Comparative Example 3] A structure having a microchannel according to Comparative Example 3 was fabricated in the same manner as Example 1, except that the conditions shown in Table 2 were employed. Here, Comparative Example 3 differs from Example 1 in, for example, the temperature and time required for heating (curing). Furthermore, in Table 3, the process conditions of Example 2 were employed, and Example 4 in which the bottom surface of the channel is made of acrylic resin, Example 5 in which a photosensitive resin laminate is used on the cover surface, Example 6 in which the height of the partition material is different, and Comparative Example 4 in which the bottom surface of the channel is made of a silicon wafer were fabricated.

[0139] <Evaluation> The above structure was evaluated by the following methods. In this embodiment in which the resin region is formed in the partition material, the evaluation of the resin region can be performed on the structure before sealing the lid material. Similarly, the water contact angle of the flow path forming surface of the substrate can be performed on the structure before sealing the lid material. Since the contact angle is measured using droplets dropped from a syringe, it is difficult to directly measure the contact angle of the flow path surface of the partition wall having a height of several tens to several hundreds of μm. On the other hand, since the cured product of the photosensitive resin composition layer of this embodiment has high uniformity, the contact angle of the surface of the photosensitive resin composition layer, that is, the surface that will later come into contact with the lid material, is considered to be equal to the contact angle of the flow path surface in this specification. Therefore, in this embodiment, for the convenience of measurement, the surface of the flow path pattern of the above structure before sealing with the lid material (photosensitive resin laminate 2) was evaluated. In this regard, in a practical application as a microchannel device, the structure after sealing with the lid is used. On the other hand, the formation of the lid does not significantly change the results or trends of the evaluations below, so long as it is within the scope of the present embodiment. Therefore, it is understood that the evaluation results and trends below also apply to microchannel devices in practical applications.

[0140] (Infrared absorption spectrum) For the above structure before sealing with the photosensitive resin laminate 2, an infrared absorption (IR) spectrum was measured by infrared spectroscopy under the following conditions. Equipment: Thermo Fisher Scientific Nicolet iN10 infrared microscope Measurement method: Attenuated total reflection measurement method (ATR reflection method), Prism: Tip ATR 350 (Ge ATR slide plate) Accumulation count: 64 Identification: Maximum peak intensity (Aa): 1565 cm -1 Periphery (e.g., 1555~1575cm -1 The first range includes the absorption intensity corresponding to the stretching vibration of the carbonyl (C=O) bond derived from the carboxylate. Maximum peak intensity (Ab): 1700cm -1 Periphery (e.g., 1690~1710cm -1 The fourth range includes the absorption intensity corresponding to the stretching vibration of the carbonyl (C=O) bond derived from the carboxylic acid. Maximum peak intensity (Ac): 1725 cm -1 Periphery (e.g. 1715~1735cm -1 The second range includes the absorption intensity corresponding to the stretching vibration of the carbonyl (C=O) bond derived from the ester. Maximum peak intensity (Ad): 1635 cm -1 Perimeter (e.g. 1625~1645cm -1 The third range includes the absorption intensity corresponding to the stretching vibration of the carbon-carbon (C=C) bond derived from the carbon-carbon double bond.

[0141] (contact angle) The contact angle was measured under the following conditions for the above-mentioned structure before sealing with the photosensitive resin laminate 2. The measurement was performed on the flow path surface of the substrate. Contact angle meter: LSE-A110 manufactured by NIC Co., Ltd. Droplet: Pure water, 2μL Measurement: 60 seconds after contact

[0142] (Confirmation of capillary action) A 10 μL droplet (pure water) was dropped onto the flow path pattern of the above structure before sealing with the photosensitive resin laminate 2, and the strength of the capillary phenomenon was observed under an environment of 23° C. and 50% RH. It was evaluated that the larger the amount of liquid transported by capillary phenomenon, the more difficult it was to control the liquid transport. A (good): Almost no droplets are sent. B (Acceptable): The droplet spreads along the pattern, but the tip of the droplet can be seen. C (Poor): The droplets spread along the pattern, and the tips of the droplets cannot be seen.

[0143] The results of the above measurements are shown in Tables 2 and 3. [Table 2] [Table 3] [Industrial Applicability]

[0144] The present invention can be utilized in fields relating to structures having microchannels, manufacturing methods thereof, and microchannel devices. [Explanation of symbols]

[0145] 1: Microfluidic device 10 :Structure 11: Base material 11A: 1st layer 11B: 2nd layer 11a: Flow path forming surface of substrate 12: Partition material 12a: Flow path forming surface of partition material 13: Lid material 13a: Flow path forming surface of the lid material 14: Microchannel 15: Flow channel pattern (micro flow channel pattern for weighing purposes) 16: Resin layer 17: Inlet 17a: Inlet pattern 18: Waste water outlet 18a: Waste water outlet pattern 19: Main flow pattern 20: Weighing flow path pattern 20a: Long side 20b: Short side 20c: Flow path pattern width 20d: Partition width 21:Resin area 22: Coating layer AD: Adhesive layer h: Length of the flow passage surface of the partition material w: Length of the flow channel forming surface of the substrate H: Length of flow path

Claims

1. A structure having a microchannel, The structure includes a substrate, a partition material, and a cover material, The substrate and at least a part of the partition material have a resin region derived from an alkali-soluble resin, The resin region has an infrared absorption spectrum according to infrared spectroscopy, 1555-1575cm -1 A maximum peak intensity (Aa) in the first range; 1715-1735cm -1 A maximum peak intensity (Ac) in the second range; The ratio (Aa / Ac) is greater than 0 and not greater than 0.200, The water contact angle of the flow path forming surface of the substrate is 40 to 150 degrees. A structure having a microchannel.

2. The structure having a microchannel according to claim 1 , wherein the ratio (Aa / Ac) is 0.100 or less.

3. The structure having a microchannel according to claim 1 , wherein the ratio (Aa / Ac) is 0.085 or less.

4. The structure having a microchannel according to claim 1 , wherein the ratio (Aa / Ac) is 0.050 or less.

5. The structure having a microchannel according to claim 1 , wherein the first range includes an absorption intensity corresponding to a stretching vibration of a carbonyl (C═O) bond derived from a carboxylate.

6. The structure having a microchannel according to claim 1 , wherein the second range includes an absorption intensity corresponding to a stretching vibration of a carbonyl (C═O) bond derived from an ester.

7. 1625-1645cm -1 A maximum peak intensity (A d ) in the third range; The maximum peak intensity (Ac); 2. The structure having a microchannel according to claim 1, wherein the ratio (Ad / Ac) is greater than 0 and is 0.150 or less.

8. 8. The structure equipped with a microchannel according to claim 7, wherein the third range includes an absorption intensity corresponding to a stretching vibration of a carbon-carbon (C=C) bond derived from a carbon-carbon double bond.

9. The structure having a microchannel according to claim 1 , wherein the resin region is substantially free of components derived from an alkali metal salt.

10. 2. The structure having a microchannel according to claim 1, wherein the water contact angle is 60 to 130 degrees.

11. The structure having a microchannel according to claim 1 , wherein the resin region is derived from a resin containing a (meth)acrylic resin.

12. The resin region comprises the following components: (a) an alkali-soluble polymer containing a carboxyl group; (b) an addition polymerizable monomer; and (c) a photopolymerization initiator or a decomposition product thereof; The structure having a microchannel according to claim 1 , which is derived from a resin made of a photosensitive resin composition containing:

13. The structure having a microchannel according to claim 1 , wherein the partition material includes the resin region.

14. The resin region has the following formula (1): P=[(1 / h)・cos{(θs / 180)・π}+ (1 / h)・cos{(θb / 180)・π}+ (2 / w)・cos{(θ / 180)・π}]・10 6 ・・・ (1) {During the ceremony, θs: Water contact angle (deg: degree) of the flow path forming surface of the lid material θb: Water contact angle (deg) of the flow path forming surface of the substrate θ: Water contact angle (deg) of the flow path forming surface of the partition material h: Length (μm) of the flow path forming surface of the partition material when the structure is cut along the thickness direction w : the length (μm) of the flow path forming surface of the substrate when the structure is cut along the thickness direction.

2. The structure having a microchannel according to claim 1, wherein P(1 / μm) expressed by the following formula is 1650 or less.

15. (i-1) a step of applying a photosensitive resin composition solution containing a solvent having a boiling point of less than 100° C. to a support and drying the applied solution to form a photosensitive resin layer containing an alkali-soluble resin on the support; (i-2) laminating the photosensitive resin layer on a substrate; (ii) developing the laminated photosensitive resin layer with an organic base aqueous solution to form a flow path pattern; (iii) subjecting the flow path pattern to a heat treatment to perform a surface treatment on the flow path pattern, thereby producing a resin region derived from an alkali-soluble resin; The resin region has an infrared absorption spectrum according to infrared spectroscopy, 1555-1575cm -1 A maximum peak intensity (Aa) in the first range; 1715-1735cm -1 A maximum peak intensity (Ac) in the second range; The method for producing a structure having a microchannel, wherein the ratio (Aa / Ac) is greater than 0 and not greater than 0.

200.

16. The step (ii) comprises: The method for producing a structure provided with a microchannel according to claim 15, further comprising a step of exposing the photosensitive resin layer to light before the development.

17. The method for producing a structure provided with a microchannel according to claim 16 , wherein the exposing step in the step (ii) is performed by direct imaging exposure without using a mask.

18. After the step (iii), (iv) forming a lid material by lamination; The method for producing a structure provided with a microchannel according to claim 15, comprising the steps of:

19. A microchannel device comprising a structure having a microchannel according to any one of claims 1 to 14.

20. A substrate having an electrode; an electrode protection layer provided on the base material for protecting the electrodes; a structure including the microchannel, the structure being laminated on the substrate and / or the electrode protection layer; The microfluidic device according to claim 19 , comprising:

Citation Information

Patent Citations

  • Material for forming micropattern, micropattern composite material, method for producing the composite material, and method for manufacturing three-dimensional microstructural substrate

    JP2010070614A

  • Microstructure having functionality

    JP2011046853A

  • Method for producing multi-layered type micro flow channel device using photosensitive resin laminate

    JP2020204769A

  • JPP4442335B

  • Microfluidic device and process for producing same, and photosensitive resin composition for forming flow path

    WO2015012212A1