Manufacturing method and manufacturing equipment for recycled asphalt mixture

The method and apparatus separate and classify old asphalt from recycled aggregates, enhancing their flexibility and durability by mixing with additives, resulting in high-quality asphalt mixtures with improved fatigue resistance.

JP7565694B2Active Publication Date: 2024-10-11NIPPO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020034616
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-02
Publication Date
2024-10-11
Estimated Expiration
2040-03-02

AI Technical Summary

Technical Problem

Recycled asphalt mixtures deteriorate quickly due to old asphalt hardening and loss of flexibility, leading to premature rutting and cracking.

Method used

A method and apparatus that separates old asphalt from recycled aggregates using a separator, classifies them into different particle sizes, and mixes them with additives and new asphalt to restore flexibility and durability.

Benefits of technology

Improves the fluidity and flexibility of recycled aggregates, enabling the production of high-quality asphalt mixtures with enhanced fatigue durability and extended pavement life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565694000002
    Figure 0007565694000002
  • Figure 0007565694000003
    Figure 0007565694000003
  • Figure 0007565694000004
    Figure 0007565694000004
Patent Text Reader

Abstract

To be able to restore flexibility and improve fatigue durability of deteriorated old asphalt.SOLUTION: A recycled asphalt mixture manufacturing device 1 classifies by a sieve 2 asphalt recycled aggregates into first recycled aggregates a with relatively large particle sizes of 13 mm to over 5 mm and second recycled aggregates b with relatively small particle sizes of 5 mm to over 0 mm. The first recycled aggregates a are put into a granulator 3 to separate parts of the old asphalt on the surface of the recycled aggregates. After that, with a sieve 4, the aggregates are classified into third recycled aggregates ab with relatively large particle sizes of 13 mm to over 5 mm and fourth recycled aggregates bb with relatively small particle sizes of 5 mm to 0 mm. The fourth recycled aggregates bb and the second recycled aggregates b, which have the same small particle sizes, are mixed, further, asphalt mortar is manufactured by mixing at least either new asphalt, or recycling additive d, or workability improving agent e. And asphalt mixture is manufactured by further mixing the third recycled aggregates ab.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for producing recycled asphalt mixture using recycled asphalt aggregate. [Background technology]

[0002] In recent years, recycled asphalt aggregate has been produced by crushing waste asphalt mixtures applied to the surface and base layers of asphalt pavement. This recycled asphalt aggregate is used as a material for recycled asphalt mixtures, and is widely used on asphalt pavement roads by mixing it with new asphalt and new aggregate to produce recycled asphalt mixtures. For example, in a conventional method for producing recycled asphalt mixture, asphalt recycled aggregate (hereinafter simply referred to as recycled aggregate) 100 is heated in a dryer 101, as shown in Fig. 5. The heated recycled aggregate 100 is then charged into a mixer 105 together with heated new fine aggregate 102, coarse aggregate 103, and new asphalt 104, and stirred and mixed to produce a recycled asphalt mixture, which is then laid on the road surface as recycled asphalt pavement.

[0003] Recycled aggregate 100 is made by coating the surface of old aggregate that has become waste with old asphalt. By repeatedly recycling recycled aggregate 100 for asphalt pavement, the old asphalt deteriorates due to reheating during production and ultraviolet rays during use, and the oil falls off. Therefore, the performance of recycled asphalt mixtures containing recycled aggregate 100 and the like gradually deteriorates, and the old asphalt hardens over time. This causes problems such as rutting and cracking to occur in the recycled asphalt pavement in a short period of time, making it impossible to use the old asphalt.

[0004] To solve this problem, for example, the recycled aggregate described in Patent Document 1 heats the oil-covered surface with hot air and radiant heat in a rotating drum to promote combustion and deterioration, thereby reducing the amount of oil adhering to the old asphalt. Then, in the subsequent heating process, a recycling additive is added to the recycled aggregate and mixed with new asphalt, thereby improving the performance of the recycled asphalt mixture. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-102883 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the performance of the recycled asphalt mixture described in Patent Document 1 cannot be said to be fully restored. Therefore, even in this case, the recycled asphalt pavement surface deteriorates in a relatively short period of time, causing problems such as hardening and cracking of the pavement surface.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a manufacturing method and manufacturing apparatus for recycled asphalt mixture that can restore the flexibility of deteriorated old asphalt and improve fatigue durability. [Means for solving the problem]

[0008] The method for producing a recycled asphalt mixture according to the present invention is characterized in that a first recycled aggregate containing old asphalt is separated by peeling off the old asphalt on the surface from the first recycled aggregate using a separator. According to the present invention, the old asphalt on the surface of the first recycled aggregate is peeled off and separated into small particle size using a separator, thereby improving fluidity and enabling the first recycled aggregate to be reused as aggregate.

[0009] In addition, it is preferable to classify the separated first recycled aggregate containing the old asphalt by a classification means into a third recycled aggregate having a relatively large particle size and a fourth recycled aggregate having a relatively small particle size. By classifying the first recycled aggregate using a separator, the fluidity of the old asphalt having a small particle size is improved and the first recycled aggregate can be easily reused as aggregate.

[0010] It is also preferable to mix the fourth recycled aggregate with a second recycled aggregate having a relatively small particle size, which is obtained by classifying the base material, recycled asphalt aggregate. By mixing the second recycled aggregate and the fourth recycled aggregate, which have relatively small particle sizes, the particle sizes are approximately the same, so the fluidity is high and the efficiency of recycling the old asphalt is improved.

[0011] It is also preferable to produce asphalt mortar by mixing the second recycled aggregate and the fourth recycled aggregate with at least one of a workability improving agent, a recycling additive, and new asphalt. By mixing the mixture of the second recycled aggregate and the fourth recycled aggregate with at least one of a workability improving agent, a recycling additive, and new asphalt, an oil-based component is added, which makes it possible to restore the flexibility and fluidity of the old asphalt and produce a high-quality asphalt mortar.

[0012] In addition, a recycled asphalt mixture can be produced by mixing a third recycled aggregate with the asphalt mortar. By adding a third recycled aggregate with a relatively large particle size as coarse aggregate to asphalt mortar with high flexibility and fluidity, a recycled asphalt mixture with high flexibility and fatigue resistance can be produced.

[0013] The manufacturing apparatus for recycled asphalt mixture according to the present invention is characterized by including a separator that peels off and separates the old asphalt from the first recycled aggregate containing the old asphalt. According to the present invention, by using a separator to peel off the old asphalt on the surface of the first recycled aggregate, the old asphalt can be separated into particles with smaller particle sizes, improving fluidity and enabling the first recycled aggregate to be reused as aggregate.

[0014] The system is also characterized by being equipped with a classification means for classifying the first recycled aggregate containing the separated old asphalt into a third recycled aggregate having a relatively large particle size and a fourth recycled aggregate having a relatively small particle size. By classifying the first recycled aggregate containing the separated old asphalt by a classification means into a third recycled aggregate and a fourth recycled aggregate, a recycled asphalt mixture with high fatigue resistance can be easily produced.

[0015] It is also preferable to include a mixing kettle that produces asphalt mortar by mixing the second recycled aggregate and the fourth recycled aggregate, which have relatively small particle sizes, and by mixing at least one of a workability improvement agent, a recycling additive, and new asphalt, and a mixer that produces a recycled asphalt mixture by stirring and mixing the asphalt mortar and the third recycled aggregate. The first recycled aggregate, which has a relatively large particle size, is passed through a separator and then classified by a classification means, and the second and fourth recycled aggregates, which have similarly small particle sizes, are mixed in a mixing kettle to increase the fluidity of the old asphalt, and by further mixing at least one of a workability improving agent, a recycling additive, and new asphalt, an oily component is added to the old asphalt, restoring its flexibility and fluidity, thereby producing asphalt mortar. Furthermore, by mixing the asphalt mortar and the third recycled aggregate in a mixer, an asphalt mixture with high fatigue resistance can be produced. Effect of the Invention

[0016] According to the method for producing a recycled asphalt mixture of the present invention, for recycled aggregate containing asphalt, the old asphalt on the surface of the first recycled aggregate is peeled off using a separator, thereby separating the old asphalt into particles with smaller particle sizes, improving fluidity and flexibility, and allowing the remaining first recycled aggregate to be reused as aggregate. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing a manufacturing apparatus for recycled asphalt mixture according to an embodiment of the present invention. [Diagram 2] FIG. [Diagram 3] FIG. 1 is a flow diagram showing a process for producing an asphalt mixture based on recycled aggregate containing old asphalt. [Figure 4] FIG. 1 is a diagram showing a test example of a method for producing an asphalt mixture according to an embodiment. [Diagram 5] FIG. 1 is a schematic diagram showing a conventional manufacturing apparatus and method for recycled asphalt mixture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, a manufacturing apparatus and a manufacturing method for recycled asphalt mixture according to an embodiment of the present invention will be described with reference to the attached drawings from FIG. 1 to FIG. First, recycled asphalt aggregate is produced by crushing waste asphalt excavated during repair or replacement of existing asphalt pavement to an appropriate size as recycled aggregate to be added to produce recycled asphalt mixture A. The crushed recycled asphalt aggregate is used as a base material having a suitable particle size range, for example, a particle size (R) range of 13 mm to 0 mm.

[0019] The manufacturing apparatus 1 for the recycled asphalt mixture A will be described with reference to Figs. 1 to 3. 1 shows an apparatus 1 for manufacturing recycled asphalt mixture A according to an embodiment of the present invention. In the apparatus 1 for manufacturing recycled asphalt mixture A, recycled aggregate containing asphalt is used as a base material, and the base material asphalt recycled aggregate B is classified into a first recycled aggregate (coarse aggregate) a having a particle size of more than 5 mm, i.e., a particle size of 13 mm to 5 mm, and a second recycled aggregate (fine aggregate) b having a particle size of 5 mm to 0 mm, using a classification device consisting of a sieve 2 with a mesh size of, for example, 6.3 mm. The first recycled aggregate a may contain aggregates with particle sizes in the range of 5 mm to 0 mm. The first recycled aggregate a contains old asphalt in an amount of, for example, about 2 mass %, and the second recycled aggregate b contains old asphalt in an amount of, for example, about 8 mass %.

[0020] The first recycled aggregate a is processed in a separator 5 equipped with a sieve 4 as a classification means and is classified again. The sieve 3 is a device that inputs the first recycled aggregate a and strips off a part of the old asphalt located on its outer periphery. As shown in FIG. 2, the first recycled aggregate a is input into an opening 8 of the sieve 3 from a raw material input port 7, and is rotated at an appropriate speed by a rotating rotor 9. The first recycled aggregate a is scattered into a crushing chamber 10 by centrifugal force through a discharge port 9a of the rotating rotor 9. The scattered first recycled aggregate a is dead-stocked on the inner wall of the crushing chamber 10, and when it collides with the next scattered first recycled aggregate a, the old asphalt on the surface is crushed and peeled off, and the particle size is adjusted to a shape close to a sphere. The peeled old asphalt becomes small-diameter granules or powder. In addition, not only the old asphalt on the surface of the first recycled aggregate a but also part of the aggregate part may be crushed and separated as stone powder, etc. By passing through the granulator 3, part of the old asphalt on the surface of the first recycled aggregate a is crushed, peeled off, or stripped away, and separated.

[0021] In order to separate a part of the old asphalt on the surface without crushing the first recycled aggregate a by the granulator 3, the rotor 9 is adjusted to an appropriate peripheral speed, for example, in the range of 10 to 60 m / sec. Preferably, the granulator 3 is set to a peripheral speed of about 20 to 50 m / sec. By selecting an appropriate speed from low to high, the crushing ratio of the first recycled aggregate a can be adjusted. If the time spent in the granulator 3 is long, the fourth recycled aggregate (fine aggregate) bb with a particle size of, for example, 5 mm to 0 mm will relatively increase, so the operating time must be adjusted as necessary. The first recycled aggregate a that has passed through the granulator 3 is classified again by the sieve 4 into a third recycled aggregate (coarse aggregate) ab having a particle size of 13 mm to over 5 mm, and a fourth recycled aggregate (fine aggregate) bb having a particle size of 5 mm to 0 mm. The asphalt content of the third recycled aggregate ab and the fourth recycled aggregate bb is, for example, 2 to 8 mass %, preferably 3 to 6 mass %.

[0022] The manufacturing device 1 for the recycled asphalt mixture A is equipped with an asphalt storage silo 13 capable of storing and heating new asphalt c, and a mixing kettle 14 for heating and mixing the new asphalt c, the recycled additive d, the second recycled aggregate b, and the fourth recycled aggregate bb. The mixing kettle 14 has a built-in stirring blade 15. Note that a workability improving agent e may be added in place of the recycled additive d, or together with the recycled additive d. The manufacturing apparatus 1 is also provided with a mixer 18 that mixes the asphalt mortar produced by mixing in the mixing kettle 14 with the third recycled aggregate ab using a mixing blade 19. The mixer 18 produces the recycled asphalt mixture A.

[0023] Next, a method for producing recycled asphalt mixture A using the manufacturing apparatus 1 for recycled asphalt mixture A will be described with reference to a flow diagram using blocks shown in FIG. 1 and FIG. In Fig. 3, asphalt recycled aggregate B is classified into a first recycled aggregate (coarse aggregate) a having a particle size of 13 mm to over 5 mm and a second recycled aggregate (fine aggregate) b having a particle size of 5 mm to 0 mm using a sieve 2 with a mesh size of, for example, 6.3 mm (step S1). The first recycled aggregate a may include aggregates with particle sizes in the range of 5 mm to 0 mm. The first recycled aggregate a contains old asphalt at, for example, about 2 mass%, and the second recycled aggregate b contains old asphalt at, for example, about 8 mass%.

[0024] Next, in FIG. 3, the first recycled aggregate a is processed and classified in a separator 5 equipped with a granulator 3 and a sieve 4. First, the first recycled aggregate a is fed into the granulator 3 to crush and peel off the old asphalt part on the surface (step S2). For example, if the first recycled aggregate a has sharp asphalt parts, it is likely to crack or chip, so the particle size can be smoothed by feeding it into the granulator 3 to peel off the sharp parts and corners. The peeled old asphalt on the surface becomes powder or fine particles and is separated from the first recycled aggregate a, and the first recycled aggregate a is granulated so that the corners and sharp parts are scraped off to approximate a smooth curved shape. In addition, some of the aggregate exposed on the surface may be crushed together with the old asphalt to become fine aggregate, stone powder, etc.

[0025] The first recycled aggregate a crushed by the granulator 3 is classified again by the sieve 4 (step S3) into third recycled aggregate ab with a particle size of 13 mm to over 5 mm from which the old asphalt has been stripped, and fourth recycled aggregate bb with a particle size of 5 mm to 0 mm. In this case, the third recycled aggregate ab contains less old asphalt than the first recycled aggregate a. Next, in the mixing tank 14, the second recycled aggregate b and the fourth recycled aggregate bb, each classified to the same extent (particle size 5 mm to 0 mm), are mixed (step S4). In this case, the fourth recycled aggregate bb contains old asphalt powder and the like because the old asphalt has been peeled off from the first recycled aggregate a by the granulator 3. Therefore, the mixture of the second recycled aggregate b and the fourth recycled aggregate bb has a fine particle size, improved fluidity, and high asphalt recycling efficiency.

[0026] Next, for example, new asphalt c is charged from the asphalt storage silo 13 into the mixing vessel 14 and mixed with the mixture of the second recycled aggregate b and the fourth recycled aggregate bb (step S5). This allows the production of high-quality asphalt mortar with high fluidity. Alternatively, instead of new asphalt c, one or both of the regeneration additive d and the workability improving agent e are added and mixed. This also adds an oily component, making it possible to produce a high-quality asphalt mortar with a fine particle size, high flexibility and fluidity (step S5).

[0027] The old asphalt of the base material, recycled asphalt aggregate B, has hardened due to aging, but the mixture of the second recycled aggregate b and the fourth recycled aggregate bb contains fine-grained old asphalt, sand, stone powder, etc. Therefore, by mixing at least one of new asphalt c, recycling additive d, and workability improvement agent e, a high-quality asphalt mortar with fine grain size and improved fluidity and flexibility can be manufactured. This can be used as a product or by adding other materials for paving work, repair work, etc.

[0028] Next, the produced asphalt mortar is fed from the mixing vessel 14 into the mixer 18, and the third recycled aggregate ab with a particle size of 13 mm to over 5 mm is fed into the mixer 18 and mixed to produce the recycled asphalt mixture A (step S6). The third recycled aggregate ab is a coarse aggregate containing a small amount of old asphalt, and by mixing it with the high-quality produced asphalt mortar, a recycled asphalt mixture A that is less likely to crack and has high fatigue durability can be obtained. Note that a workability improving agent may be added during the production of the recycled asphalt mixture A.

[0029] The recycled asphalt mixture A obtained by mixing for a predetermined time with the mixing blades 19 in the mixer 18 is, for example, dropped into a dump truck 20 and transported to an asphalt pavement construction site. Alternatively, the recycled asphalt mixture A may be discharged directly from the mixer 18 at the construction site and used for construction.

[0030] As described above, according to the manufacturing device 1 and manufacturing method of the recycled asphalt mixture A of this embodiment, the old asphalt on the surface can be partially peeled off from the first recycled aggregate a, which is a relatively large particle size obtained by classifying the base material, the asphalt recycled aggregate B, by the granulator 3. This allows classification into the third recycled aggregate ab, which has a particle size of 13 mm to over 5 mm, and the fourth recycled aggregate bb, which contains a large amount of fine particle size old asphalt, which has a particle size of 5 mm to 0 mm. Therefore, by mixing the fourth recycled aggregate bb with the second recycled aggregate b, it is possible to manufacture an asphalt mortar with high flexibility and durability. Furthermore, by mixing it with the third recycled aggregate ab, which contains almost no old asphalt, a high-quality recycled asphalt mixture A with high flexibility and fatigue resistance can be produced.

[0031] Next, a test example carried out on the manufacturing method of the recycled asphalt mixture A according to the above-mentioned embodiment will be described with reference to FIG. In FIG. 4, the asphalt recycled aggregate B as the base material has a particle size of, for example, 13 mm to 0 mm, and contains 5.4% asphalt by mass. This recycled aggregate is classified by a sieve 2 into a first recycled aggregate a having a large particle size (particle size 13 mm to over 5 mm) and a second recycled aggregate b having a small particle size (particle size 5 mm to 0 mm). The first recycled aggregate a having a large particle size is 40% by mass, and the second recycled aggregate b having a small particle size is 60% by mass. The ratio of the amount of old asphalt in the amount of the second recycled aggregate b is 6.5% by mass, and 3.9% by mass with respect to the total recycled aggregate. Since the amount of old asphalt in the recycled aggregate before classification is 5.4% by mass, the content ratio is 72%.

[0032] The amount of old asphalt in the first recycled aggregate a with a large particle size is 3.8% by mass, and 1.5% by mass in the total recycled aggregate. The first recycled aggregate a is fed into the granulator 3 of the separator 5 to be peeled off, and is further classified into the third recycled aggregate ab with a large particle size (particle size 13 mm to over 5 mm) and the fourth recycled aggregate bb with a small particle size (particle size 5 mm to 0 mm) using the sieve 4 of the separator 5. Moreover, the ratio of the amount of asphalt in the second recycled aggregate b and the fourth recycled aggregate bb (particle size 5 mm to 0 mm) with a small particle size classified using the sieve 4 of the separator 5 to the asphalt recycled aggregate B of the base material is 4.7% by mass / 5.4% by mass x 100 = 87%.

[0033] As a result, the large particle size was 25% by mass, and the small particle size was 75% by mass. The large particle size had an old asphalt content of 2.7% by mass, and the amount of old asphalt was 0.7% by mass relative to the entire recycled asphalt aggregate B. The small particle size had an old asphalt content of 6.3% by mass, and the amount of old asphalt was 4.7% by mass relative to the entire recycled aggregate. The change in asphalt amount in this test example is shown in Table 1 below. The asphalt amount is indicated by the As amount.

[0034] [Table 1]

[0035] The manufacturing method of the recycled asphalt mixture A according to the present invention is not limited to the above-mentioned embodiment, and the configuration of the above-mentioned embodiment can be appropriately replaced or modified without departing from the gist of the present invention. Below, the recycled asphalt mixture A according to this embodiment and modified examples of the manufacturing method thereof will be described, but the same reference numerals will be used to describe the same or similar parts as those in the above-mentioned embodiment.

[0036] For example, in the method for producing an asphalt mixture according to the present embodiment, the produced asphalt mortar can be used as a surface treatment material for pavement surfaces. This makes it possible to extend the life of the pavement surface at low cost. The asphalt mortar is included in the asphalt mixture. In addition, in the above-described embodiment, the first recycled aggregate a is separated by peeling off the old asphalt on the surface using a granulator 3, but the means for separating the old asphalt is not limited to the granulator 3 and any appropriate separator such as a crusher or crusher can be used.

[0037] In this embodiment, the asphalt recycled aggregate B as the base material and the first recycled aggregate a are classified into relatively large recycled aggregates with a particle size of 13 mm to over 5 mm and relatively small recycled aggregates with a particle size of 5 mm to 0 mm by the sieves 2 and 4 as classification means. However, the classification of the particle size is not limited to the above embodiment, and the recycled aggregates can be classified into appropriate particle sizes. [Explanation of symbols]

[0038] 1. Recycled asphalt mixture manufacturing equipment 2, 4 sieves 3 Graining machine 5 Separation device 13 Asphalt storage silo 14 Mixing pot 18 Mixer A Recycled asphalt mixture a. First recycled aggregate B. Recycled asphalt aggregate b. Secondary recycled aggregate ab The third recycled aggregate bb The fourth recycled aggregate c New asphalt d. Regeneration additives e. Workability improvement agent

Claims

1. Classifying recycled asphalt aggregate into a first recycled aggregate having a particle size of 13 mm to over 5 mm and a second recycled aggregate having a particle size of 5 mm to 0 mm, The first recycled aggregate containing old asphalt is separated by peeling off the old asphalt on the surface from the first recycled aggregate using a separator; The first recycled aggregate containing the separated old asphalt is classified by a classification means into a third recycled aggregate having a particle size of 13 mm to more than 5 mm and a fourth recycled aggregate having a particle size of 5 mm to 0 mm; The fourth recycled aggregate is mixed with the second recycled aggregate obtained by classifying the asphalt recycled aggregate, which is a base material; The second recycled aggregate and the fourth recycled aggregate are mixed with at least one of a workability improving agent, a regeneration additive, and a new asphalt in a mixing kettle to produce an asphalt mortar; A method for producing a recycled asphalt mixture, characterized in that the third recycled aggregate is mixed with the produced asphalt mortar in a mixer to produce a recycled asphalt mixture.

2. A sieve for classifying recycled asphalt aggregate into a first recycled aggregate having a particle size of 13 mm to over 5 mm and a second recycled aggregate having a particle size of 5 mm to 0 mm; A separator that peels off and separates the old asphalt from the first recycled aggregate containing the old asphalt; A classification means for classifying the first recycled aggregate containing the separated old asphalt into a third recycled aggregate having a particle size of 13 mm to more than 5 mm and a fourth recycled aggregate having a particle size of 5 mm to 0 mm; A mixing kettle for producing asphalt mortar by mixing the second recycled aggregate and the fourth recycled aggregate and mixing at least one of a workability improving agent, a recycling additive, and a new asphalt; A mixer that produces a recycled asphalt mixture by stirring and mixing the asphalt mortar and the third recycled aggregate; A manufacturing apparatus for recycled asphalt mixture, comprising:

Citation Information

Patent Citations

  • Method for regenerating aggregate from destruction rubbish of asphalt

    JP1998057834A

  • Method of collecting aggregate from waste asphalt mixture

    JP2003247208A

  • Method of manufacturing asphalt mixture

    JP2009102883A