Substrate holding member and manufacturing method thereof

A ceramic-based substrate holding member with thermal spray coatings and a silicone adhesive layer addresses heat resistance and uniformity issues, ensuring stable operation at high temperatures by maintaining adhesive integrity and uniform temperature distribution.

JP7565734B2Active Publication Date: 2024-10-11NITERRA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020160678
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-25
Publication Date
2024-10-11
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing substrate holding members, such as electrostatic chucks, face issues with heat resistance and uniform temperature distribution due to the use of organic adhesives, which degrade at high temperatures, and metal cooling plates that interfere with uniform temperature distribution.

Method used

A substrate holding member composed of a ceramic member with thermal spray coatings and a silicone adhesive layer, which maintains the adhesive below its heat-resistant temperature and reduces thermal unevenness by adjusting thermal resistances through ceramic materials and thermal spray films.

Benefits of technology

The substrate holding member maintains uniform temperature distribution and prevents adhesive degradation at high temperatures, enabling stable use beyond the adhesive's heat-resistant limit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565734000001
    Figure 0007565734000001
  • Figure 0007565734000002
    Figure 0007565734000002
  • Figure 0007565734000003
    Figure 0007565734000003
Patent Text Reader

Abstract

To provide a substrate holding member and a method for manufacturing the same in which a temperature of the silicone adhesive layer is equal to or below a heat resistance temperature and temperature distribution uniformity of a substrate mounting surface is high, even when used in a process in which the substrate temperature is equal to or above the heat resistance temperature of the silicone adhesive layer.SOLUTION: A substrate holding member 10 comprises: a ceramic member 12 being formed into a flat shape and formed of ceramics and having a substrate mounting surface 28 on one main surface; a first thermal spray film 14 formed on the other main surface of the ceramic member 12; a metal cooling member 16 having a refrigerant flow channel 22 inside; a second thermal spray film 18 formed on a flat main surface of the cooling member 16; and a silicone adhesive layer 20 joining the first thermal spray film 14 and second thermal spray film 18.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate holding member and a method for manufacturing the same. [Background technology]

[0002] 2. Description of the Related Art Some substrate holding members used in semiconductor manufacturing equipment, such as electrostatic chucks, are equipped with a cooling member in order to maintain the substrate at a predetermined temperature during semiconductor processing.

[0003] Patent Document 1 discloses an electrostatic chuck in which a metal plate having an insulator film formed on its surface by thermal spraying and a dielectric substrate having electrodes formed on its surface are joined with an insulating adhesive so that the electrodes face each other, the insulator film having a thickness of 0.3 mm or more and 0.6 mm or less, the insulating adhesive having a thermal conductivity of 1 W / mK or more, and the thermal conductivity of the insulator film being greater than that of the insulating adhesive.

[0004] Patent Document 2 discloses a heater unit having a substrate having a cooling flow path, a heater section disposed above the substrate and having a heating element, and a heat insulating layer disposed between the substrate and the heater section. It also describes that the thermal conductivity of the heat insulating layer may be lower than that of the substrate, that the heat insulating layer may be SUS containing pores, that the heater unit further has an insulator covering the heating element, and that the thermal conductivity of the heat insulating layer may be lower than that of the insulator. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-243139 A [Patent Document 2] JP 2017-037721 A Summary of the Invention [Problem to be solved by the invention]

[0006] Traditionally, metal materials, especially aluminum alloys, have been used for the cooling plates of electrostatic chucks due to their workability and cooling effect. Electrostatic chucks have used ceramic sintered bodies made of Al2O3 and AlN. To integrate these, organic adhesives have been proposed because of their ease of integration. However, when using organic adhesives as a bonding layer, their heat resistance becomes an issue, and electrostatic chucks could not be used in processes at 200°C or higher, in particular, because the temperature reaches a point where the organic adhesive layer decomposes.

[0007] Furthermore, with the trend toward higher power processes in recent years, there has been an increasing demand for uniform temperature distribution on the substrate support surface of the electrostatic chuck. However, when a metal cooling plate is used, the metal plate itself has good thermal conductivity, and the influence of the coolant flow paths provided inside the metal plate appears on the support surface of the electrostatic chuck, thereby hindering the uniformity of the temperature distribution on the support surface.

[0008] However, Patent Document 1 does not take into account the heat resistance of the insulating adhesive layer. Patent Document 2 does not take into account the bonding between the heat insulating layer and the base material or the heat insulating layer and the heater part, and therefore does not take into account the heat resistance when an organic adhesive is used. In addition, neither Patent Document 1 nor Patent Document 2 takes into account the uniformity of the temperature distribution when cooling the substrate.

[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a substrate holding member and a method for manufacturing the same, which has a highly uniform temperature distribution on the substrate supporting surface, and in which the temperature of the silicone adhesive layer is below the heat resistance temperature even when used in a process in which the temperature of the substrate reaches or exceeds the heat resistance temperature of the silicone adhesive layer, and in which the temperature of the silicone adhesive layer is below the heat resistance temperature. [Means for solving the problem]

[0010] (1) In order to achieve the above object, the substrate holding member of the present invention is characterized by comprising a ceramic member formed in a flat plate shape from ceramics and having a substrate mounting surface on one main surface, a first sprayed film formed on the other main surface of the ceramic member, a metal cooling member having a coolant flow path inside, a second sprayed film formed on the planar main surface of the cooling member, and a silicone adhesive layer bonding the first sprayed film and the second sprayed film. In this way, by providing sprayed films on the bonding surface between the ceramic member and the silicone adhesive layer and the bonding surface between the cooling member and the silicone adhesive layer, even if the substrate holding member is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer, the temperature of the silicone adhesive layer can be kept below the heat resistance temperature, and deterioration of the silicone adhesive layer can be prevented and uneven heat distribution on the substrate mounting surface of the substrate holding member can be reduced. At the same time, the flexibility of the silicone adhesive layer can reduce stress generated between the substrate holding member and the cooling member. As a result, it becomes possible to use the substrate holding member in processes at temperatures higher than the heat resistance temperature of the silicone adhesive layer while uniformizing the temperature distribution on the substrate mounting surface of the substrate holding member.

[0011] (2) In the substrate holder of the present invention, the ceramic member is made of a ceramic material mainly composed of AlN, and the thermal resistance per unit area in the thickness direction of the ceramic member is Re(m 2 K / W), and the thermal resistance per unit area in the thickness direction of the first sprayed coating is Rf1 (m 2 K / W), and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb (m 2 K / W), and the thermal resistance per unit area in the thickness direction of the second sprayed coating is Rf2 (m 2 K / W), and the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member on the silicone adhesive layer side to the flow path of the refrigerant is Rm (m 2K / W), 0.75 ≧ (Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.24. In this way, by adjusting the thermal resistance per unit area of ​​the ceramic member, first sprayed film, silicone adhesive layer, second sprayed film, and cooling member according to the ceramic material that forms the ceramic member, the substrate holding member can be used even in high-temperature processes of 250°C or more.

[0012] (3) In the substrate holder of the present invention, the ceramic member is made of a ceramic material mainly composed of Al2O3, and the thermal resistance per unit area in the thickness direction of the ceramic member is Re(m 2 K / W), and the thermal resistance per unit area in the thickness direction of the first sprayed coating is Rf1 (m 2 K / W), and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb (m 2 K / W), and the thermal resistance per unit area in the thickness direction of the second sprayed coating is Rf2 (m 2 K / W), and the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member on the silicone adhesive layer side to the flow path of the refrigerant is Rm (m 2 K / W), 0.77 ≧ (Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.20. In this way, by adjusting the thermal resistance per unit area of ​​the ceramic member, first sprayed film, silicone adhesive layer, second sprayed film, and cooling member according to the ceramic material that forms the ceramic member, the substrate holding member can be used even in high-temperature processes of 250°C or more.

[0013] (4) Furthermore, the substrate holding member of the present invention is characterized in that, in the substrate holding member, the ceramic member is formed of a ceramic containing AlN as a main component, and (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.83. In this way, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member, the first sprayed film, the silicone adhesive layer, the second sprayed film, and the cooling member according to the ceramic material forming the ceramic member, the amount of heat supply required to maintain a predetermined process temperature can be reduced.

[0014] (5) Furthermore, in the substrate holding member of the present invention, the ceramic member is formed of a ceramic containing Al2O3 as a main component, and (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.63. In this way, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member, the first sprayed film, the silicone adhesive layer, the second sprayed film, and the cooling member according to the ceramic material forming the ceramic member, the amount of heat supply required to maintain a predetermined process temperature can be reduced.

[0015] (6) Furthermore, a method for manufacturing a substrate holding member of the present invention includes the steps of: forming and firing a ceramic raw material powder to produce a ceramic member; preparing a plurality of metal members and forming a groove portion which serves as a flow path for a coolant; joining the plurality of metal members with the groove portion formed therein to produce a cooling member having the flow path; spraying a first thermal spray raw material powder containing a predetermined ceramic onto a surface of the ceramic member facing the substrate mounting surface to form a first thermal sprayed film; spraying a second thermal spray raw material powder containing a predetermined ceramic onto one main surface of the cooling member to form a second thermal sprayed film; applying a silicone adhesive to at least one of the first thermal sprayed film or the second thermal sprayed film to bond the ceramic member and the cooling member together; and curing the silicone adhesive to form a silicone adhesive layer. In this way, by providing a thermal spray film on each of the bonding surfaces between the ceramic member and the silicone adhesive layer and between the cooling member and the silicone adhesive layer, even if the substrate holding member is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer, the temperature of the silicone adhesive layer can be kept below the heat resistance temperature, preventing deterioration of the silicone adhesive layer and reducing thermal unevenness on the substrate mounting surface of the substrate holding member. At the same time, the flexibility of the silicone adhesive layer can relieve stress generated between the substrate holding member and the cooling member. As a result, it is possible to use the electrostatic chuck in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer while uniforming the temperature distribution on the substrate mounting surface of the substrate holding member. Effect of the Invention

[0016] According to the present invention, even if the substrate holding member is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer, the temperature of the silicone adhesive layer can be kept below the heat resistance temperature, and deterioration of the silicone adhesive layer can be prevented, while thermal unevenness on the substrate mounting surface of the substrate holding member can be reduced. As a result, the electrostatic chuck can be stably used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer while the temperature distribution on the substrate mounting surface of the substrate holding member is made uniform. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a front cross-sectional view showing the substrate holding member of the embodiment. [Diagram 2] 1 is a table showing the manufacturing conditions and temperature measurements for each sample. [Diagram 3] 1 is a table showing the manufacturing conditions and temperature measurements for each sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Next, an embodiment of the present invention will be described with reference to the drawings. In order to facilitate understanding of the description, the same reference numerals are used for the same components in each drawing, and duplicated descriptions will be omitted. In the configuration diagrams, the size of each component is conceptually shown, and does not necessarily represent the actual dimensional ratio.

[0019] [Embodiment] [Configuration of the substrate holding member] 1 is a front cross-sectional view showing a substrate holding member 10. The substrate holding member 10 includes a ceramic member 12, a first sprayed film 14, a cooling member 16, a second sprayed film 18, and a silicone adhesive layer 20. The substrate holding member 10 may also have one or more electrodes embedded therein as necessary. The substrate holding member 10 can be used, for example, in an electrostatic chuck, a heater, etc.

[0020] The ceramic member 12 is formed of ceramics in a flat plate shape, and has a substrate mounting surface 28 on one of its main surfaces. The ceramics constituting the ceramic member 12 are preferably ceramics containing AlN or Al2O3 as the main component. "Mainly containing" means that the weight ratio of the main component to the weight of the ceramic member 12 is 90 wt% or more. In addition to the ceramics as the main component, the ceramic member 12 may contain additives for various purposes, such as increasing thermal conductivity. For example, additives made of oxides of Group 2a elements or Group 3a elements or transition metal oxides may be added to adjust thermal conductivity or volume resistivity.

[0021] In general, in the case of ceramics mainly composed of AlN, it is known that the thermal conductivity increases with increasing amount of additives such as Y2O3, but adding more than a certain amount causes a decrease in thermal conductivity. Therefore, it is desirable to keep the content of additives consisting of oxides of 2a group elements and 3a group elements and transition metal oxides to 10wt% or less. In the case of ceramics mainly composed of Al2O3, it is also desirable to keep the content of additives consisting of oxides of 2a group elements and 3a group elements and transition metal oxides to 10wt% or less. Examples of additives of 2a group elements include Mg, Ca, Sr, Ba, etc., and examples of additives of 3a group elements include Y, La, Sm, Ce, etc. Examples of additives of transition metals include Ti, Cr, Mn, Ni, etc.

[0022] The first sprayed film 14 is formed on the surface of the ceramic member 12 facing the substrate mounting surface 28. The first sprayed film 14 is made of ceramics. The first sprayed film 14 is preferably made of ceramics with low thermal conductivity, such as Al2O3, Y2O3, or ZrO2. The first sprayed film 14 can be produced by a known spraying method, such as a plasma spraying method or a dry plasma spraying method. The thickness of the first sprayed film 14 is preferably 0.05 mm or more and 2 mm or less.

[0023] It is preferable that the first sprayed coating 14 has a predetermined porosity. This enhances the heat insulating effect. The porosity is preferably 2% or more, and more preferably 5% or more. The upper limit of the porosity does not need to be particularly limited as long as the thermal conductivity of the first sprayed coating 14 is within a predetermined range, but it can be, for example, 10% or less.

[0024] The cooling member 16 is made of metal and has a coolant flow path 22 inside. The metal constituting the cooling member 16 is most preferably an Al alloy because of its workability and high thermal conductivity, but alloys containing copper, titanium, nickel, SUS, etc. may also be used. The coolant may be water, ethylene glycol, fluorocarbon, etc., and the coolant temperature may be below the boiling point.

[0025] The second sprayed film 18 is formed on one of the main surfaces of the cooling member 16. The main surface of the cooling member 16 on which the second sprayed film 18 is formed is flat. The second sprayed film 18 is made of ceramics. The second sprayed film 18 is preferably made of ceramics such as Al2O3, Y2O3, and ZrO2. If the thermal conductivity of the second sprayed film is too low, the effect of the cooling member is weakened, so it is preferable that the thermal conductivity of the second sprayed film is relatively high. Therefore, the porosity is preferably 5% or less, and more preferably 2% or less. The thickness of the second sprayed film 18 is preferably 0.05 mm or more and 2 mm or less. The materials and thicknesses of the first sprayed film 14 and the second sprayed film 18 may be the same or different.

[0026] The porosity of the first sprayed coating 14 and the second sprayed coating 18 may be the same value or different values.

[0027] The silicone adhesive layer 20 bonds the first sprayed film 14 and the second sprayed film 18. This allows the ceramic member 12 and the cooling member 16 to be bonded. The silicone adhesive layer 20 is formed of a silicone adhesive containing silicone as a main component, such as silicone resin or modified silicone resin. The curing type of the silicone adhesive can be selected from dehydration, dealcoholization, and addition polymerization types. In addition, one-component curing, two-component curing, and ultraviolet curing can be selected. The silicone adhesive may contain ceramics such as Al2O3 and AlN or metal fillers such as Cu to adjust thermal conductivity. The thickness of the silicone adhesive layer 20 is preferably 0.1 mm or more and 2.0 mm or less. The silicone adhesive layer has a sufficiently small Young's modulus compared to ceramics and metals, so it can maintain flexibility.

[0028] The ceramic member 12 shown in Fig. 1 has two electrodes 24, 26 embedded therein. The electrode 24 in Fig. 1 is an electrode for electrostatic attraction, and the electrode 26 is an electrode serving as a heating resistor. In this manner, the substrate holding member 10 may have one or more electrodes embedded therein as necessary. The substrate holding member 10 shown in Fig. 1 is an electrostatic chuck having a heating resistor.

[0029] In this way, by providing the first sprayed film 14 and the second sprayed film 18 on the bonding surface between the ceramic member 12 and the silicone adhesive layer 20 and on the bonding surface between the cooling member 16 and the silicone adhesive layer 20, respectively, even if the substrate holding member 10 is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer 20, the temperature of the silicone adhesive layer 20 can be kept below the heat resistance temperature, and deterioration of the silicone adhesive layer 20 can be prevented and uneven heat distribution on the substrate mounting surface 28 of the substrate holding member 10 can be reduced. At the same time, the flexibility of the silicone adhesive layer can relieve stress generated between the substrate holding member and the cooling member. As a result, the substrate holding member 10 can be used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer 20 while uniformizing the temperature distribution on the substrate mounting surface 28 of the substrate holding member 10.

[0030] (Thermal resistance design) The above-mentioned configuration allows the substrate holding member 10 to be used in processes at temperatures higher than the heat resistance temperature of the silicone adhesive layer 20. However, when considering use in processes at higher temperatures or reducing the amount of heat required to maintain a given process temperature, it is preferable to design the thermal resistance of the substrate holding member 10. The thermal resistance per unit area in the thickness direction of the substrate holding member 10 (m 2 The thermal resistance Re(m 2 The thermal resistance Rf1 (m 2 The thermal resistance Rm (m 2 The thermal resistance Rb (m 2The thermal conductivity of the silicone adhesive layer is defined as the thickness (m) of the silicone adhesive layer divided by the thermal conductivity (W / mK) of the silicone adhesive layer. The thickness direction is defined as the direction perpendicular to the substrate mounting surface 28 of the substrate holding member 10.

[0031] Here, when the ceramic member 12 is formed of a ceramic mainly composed of AlN, it is preferable that 0.75 ≧ (Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.24. In this way, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member 12, the first sprayed film 14, the silicone adhesive layer 20, the second sprayed film 18, and the cooling member 16 according to the ceramic material forming the ceramic member 12, the substrate holding member 10 can be used even in a high-temperature process of 250°C or more. The value of (Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm) is considered to indicate the temperature of the silicone adhesive layer 20. The value of (Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm) is related to the temperature at the interface between the silicone adhesive layer 20 and the first sprayed film 14; when this value is large, the temperature of the silicone adhesive layer 20 tends to be low, and when this value is small, the temperature tends to be high.

[0032] Furthermore, when the ceramic member is formed of a ceramic containing Al2O3 as a main component, it is preferable that 0.77 ≧ (Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.20. In this way, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member 12, the first sprayed film 14, the silicone adhesive layer 20, the second sprayed film 18, and the cooling member 16 according to the ceramic material forming the ceramic member 12, the substrate holding member 10 can be used even in high-temperature processes of 250°C or more.

[0033] In addition, when the ceramic member 12 is formed of ceramics mainly composed of AlN, it is preferable that (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm)≧0.83. In this way, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member 12, the first sprayed film 14, the silicone adhesive layer 20, the second sprayed film 18, and the cooling member 16 according to the ceramic material forming the ceramic member 12, it is possible to reduce the amount of heat supply required to maintain a predetermined process temperature. The value of (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) is considered to indicate the degree of ease of application to semiconductor processes. If the value of (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) is small, the amount of heat supply required to reach a predetermined substrate processing temperature becomes excessive, and it tends to be difficult to use in semiconductor processes.

[0034] Furthermore, when the ceramic member 12 is made of ceramics containing Al2O3 as a main component, it is preferable that (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm)≧0.63 is satisfied, where Re is the thermal resistance per unit area in the thickness direction of the ceramic member 12, and Rm is the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member 16 on the silicone adhesive layer 18 side to the refrigerant flow path. In this way, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member 12, the first sprayed film 14, the silicone adhesive layer 20, the second sprayed film 18, and the cooling member 16 according to the ceramic material forming the ceramic member 12, the amount of heat supply required to maintain a predetermined process temperature can be reduced.

[0035] In designing the above thermal resistance, the thickness and thermal conductivity of each member are preferably within the following ranges. The ceramic member 12 is preferably 1 mm or more and 30 mm or less in thickness, and the ceramic member 12 is preferably 4 W / mK or more and 250 W / mK in thermal conductivity. The first ceramic sprayed film 14 is preferably 0.3 mm or more and 2.0 mm or less in thickness, and the first ceramic sprayed film 14 is preferably 0.4 W / mK or more and 16.0 W / mK or less in thermal conductivity. The second ceramic sprayed film 18 is preferably 0.1 mm or more and 2.0 mm or less in thickness, and the second ceramic sprayed film 18 is preferably 0.4 W / mK or more and 16.0 W / mK or less in thermal conductivity. The thickness of the silicone adhesive layer 20 is preferably 0.1 mm or more and 2.0 mm or less, and the thermal conductivity of the silicone adhesive layer 20 is preferably 0.1 W / mK or more and 4.0 W / mK or less. The thickness (shortest distance) from the main surface of the cooling member 16 on the silicone adhesive layer side to the refrigerant flow path is preferably 2 mm or more and 30 mm or less, and the thermal conductivity of the cooling member 16 is preferably 10 W / mK or more and 300 W / mK or less. The thermal conductivity of each part is measured at 25°C.

[0036] [Method of manufacturing the substrate holding member] Next, a method for manufacturing the substrate holder configured as described above will be described in the following order: a method for manufacturing the ceramic member, a method for manufacturing the cooling member, a thermal spraying method, and a method for forming the silicone adhesive layer.

[0037] (Method of manufacturing ceramic members) The following manufacturing method for ceramic members will be described as a method for producing ceramic members from raw materials whose main component is AlN by powder hot pressing, but the raw materials and manufacturing method are not limited to this method and can also be applied to ceramic members whose main component is Al2O3. In addition to the powder hot pressing method, it is also possible to adopt green sheet lamination methods and other conventional manufacturing methods. First, the AlN ceramic raw material powder is granulated. The granulated powder is added with 0.3 wt% to 6 wt% Y2O3 in an internal ratio, and a binder is added to granulate the granulated powder. Next, the granulated powder is filled into a bottomed carbon mold (molding die), a carbon punch is placed on it, and then sintered.

[0038] At this time, an electrode for electrostatic attraction or an electrode serving as a heating resistor may be embedded in the ceramic member. Heat-resistant metals such as tungsten and molybdenum can be used as the electrode for electrostatic attraction or the heating resistor. For example, an electrode for electrostatic attraction or a heating resistor formed of a plate, foil, wire, mesh, or the like is embedded during molding and sintered. For example, when embedding one layer of electrodes, a molding die is filled with granulated powder corresponding to the insulating layer of the ceramic member, and the electrode is placed on the molded body after uniaxial pressing. The same granulated powder is filled on top of it, a carbon punch is placed on it, and then sintered. When embedding two or more layers of electrodes, the process of filling with granulated powder and placing the electrode on the molded body after uniaxial pressing is repeated.

[0039] The firing process is preferably atmospheric firing or uniaxial hot press firing. Normal pressure firing is performed at 1800°C or higher, and uniaxial hot press firing is performed at 1700°C or higher and 1 MPa or higher pressure and temperature conditions. However, the firing method is not limited to these. After firing, the substrate mounting surface on which the substrate is mounted and the back surface on which the first sprayed film is provided are formed, and the ceramic member is processed into a predetermined shape. The outer shape of the ceramic member can be selected from circular, rectangular, etc., depending on the shape of the substrate to be mounted.

[0040] (Method of manufacturing cooling member) First, a plurality of metal members are prepared, and grooves are formed as the flow paths of the refrigerant. Next, the plurality of metal members with the grooves formed therein are joined to produce a cooling member having a flow path. The flow paths are formed by performing a predetermined machining process on the plurality of metal members, and then using a conventional metal joining method such as brazing, electron beam welding, or diffusion bonding. The most suitable metal is an Al alloy because of its workability and high thermal conductivity, but alloys containing copper, titanium, and nickel, and SUS can also be used. A flow path for the refrigerant is formed inside the metal cooling member. The size and shape of the flow path of the refrigerant may be any size and shape that can uniformly cool the ceramic member.

[0041] (Thermal spraying method) A first sprayed raw material powder containing a predetermined ceramic is sprayed on the surface of the ceramic member facing the substrate mounting surface to form a first sprayed film. Separately, a second sprayed raw material powder containing a predetermined ceramic is sprayed on one main surface of the cooling member to form a second sprayed film. The sprayed film can be produced by a known spraying method, such as an air plasma spraying method using a slurry containing a ceramic raw material powder, or a dry plasma spraying method in which the raw material powder is granulated and fed. The film type of the first sprayed film and the second sprayed film is preferably Al2O3, Y2O3, ZrO2, or the like. The sprayed film has a certain porosity, and the pores exert a heat insulating effect. Therefore, the porosity of the first sprayed film in particular is preferably 2% or more, and more preferably 5% or more. The thermal conductivity of the first sprayed film and the second sprayed film can be adjusted to 0.4 to 16 W / mK by these raw materials and porosity. The thickness of the sprayed film is preferably 0.05 mm or more and 2 mm or less.

[0042] (Method of forming silicone adhesive layer) The curing type of the silicone adhesive can be selected from dehydration, dealcoholization, addition polymerization, etc. Also, one-component curing, two-component curing, ultraviolet curing, etc. can be selected. Of these, the silicone adhesive forming the silicone adhesive layer is preferably a heat-curing one. The following description will explain a method of forming a silicone adhesive layer using a heat-curing silicone adhesive.

[0043] The silicone adhesive is applied to at least one of the first ceramic sprayed film or the second ceramic sprayed film after weighing and stirring an appropriate amount, and after degassing, the two are laminated and heat-cured in an oven under air, nitrogen atmosphere, or reduced pressure with a load. In order to suppress outgassing of siloxane components from the silicone adhesive, it is preferable to cure at 100°C or higher and then treat at 200°C or higher for a certain period of time. In addition, a spacer of a predetermined thickness may be placed at the same time to adjust the thickness of the silicone adhesive layer. By the above treatment, the ceramic member coated with the first ceramic sprayed film on the back side and the metal cooling member coated with the second ceramic sprayed film on the front side are bonded with the silicone adhesive to form a silicone adhesive layer. Note that if the center line average roughness Ra of the sprayed film is 1 μm or more, the silicone adhesive can penetrate into the gaps in the roughness curve of the sprayed film and adhere well.

[0044] By this method, a substrate holding member can be manufactured.

[0045] [Examples and Comparative Examples] [Samples a1-a15] Next, examples and comparative examples will be described. First, as a sample using AlN as the material of the ceramic member, an electrostatic chuck was produced in which a ceramic member mainly composed of AlN in which an electrode for an electrostatic chuck is embedded and a cooling member made of an Al alloy are bonded with a silicone adhesive layer. Samples a1 to a15 were produced by varying the presence or absence, material, thickness, and thermal conductivity and thickness of the first sprayed film or the second sprayed film. Hereinafter, samples a1 to a15 are collectively referred to as sample a. FIG. 2 is a table showing the manufacturing conditions and measured temperatures of each of samples a1 to a15.

[0046] (Preparation of ceramic members for use in sample a) The raw material was AlN with 5wt% Y2O3 added as an additive, and an electrode made of cut Mo mesh (wire diameter 0.1mm, mesh size #50) was embedded as an electrode. After uniaxial hot press sintering, it was machined into a specified shape, and a substrate mounting surface was provided on the front side, and a flat surface on which the thermal spray coating was sprayed was provided on the back side opposite the front side, to produce a ceramic component with a diameter of 300mm and a thickness of 15mm. The surface roughness Ra of the substrate mounting surface was 0.5μm, and the surface roughness Ra of the sprayed surface was 1.5μm. These were measured in accordance with JIS B 0601 and ISO25178. The thermal conductivity measured for the ceramic component alone was 160W / mK at 25℃. The thermal conductivity was measured using the laser flash method in accordance with JIS R 1611-1997.

[0047] [Samples b1-b6] In addition, as a sample using Al2O3 as the material of the ceramic member, an electrostatic chuck was fabricated in which a ceramic member mainly composed of Al2O3 in which an electrostatic chuck electrode is embedded is bonded to an Al alloy cooling member by a silicone adhesive layer. Samples b1 to b6 were produced by varying the material and thickness of the first sprayed film or the second sprayed film, and the thermal conductivity and thickness of the silicone adhesive layer. Hereinafter, samples b1 to b6 are collectively referred to as sample b. Figure 3 is a table showing the manufacturing conditions and measured temperatures for each of samples b1 to b6.

[0048] (Preparation of ceramic members for use in sample b) The raw material was Al2O3 with 0.05wt% MgO added as an additive, and an electrode made from cut Mo mesh (wire diameter 0.1mm, mesh size #50) was embedded as the electrode. After uniaxial hot press sintering, it was machined into the specified shape, and a substrate mounting surface was provided on the front surface, and a flat surface on which the thermal spray film was sprayed was provided on the back surface opposite the front surface, producing a ceramic component with a diameter of 300mm and a thickness of 15mm. The surface roughness Ra of the substrate mounting surface was 0.4μm, and the surface roughness Ra of the sprayed surface was 1.2μm. The thermal conductivity measured on the ceramic component alone was 30W / mK at 25℃.

[0049] (Production of cooling components) An Al alloy (6061T6) was used as the metal. The coolant flow paths were rectangular with a cross section of 10 mm wide and 5 mm high, and were arranged at a radial distance of 20 mm. The shortest vertical distance from the surface of the cooling member to the flow paths was 15 mm. The surface roughness Ra of the sprayed surface of the cooling member was 1.6 μm. The cooling member was the same for sample a and sample b. The thermal conductivity of the cooling member was 138 W / mK at 25°C.

[0050] (Formation of thermal spray coating) Al2O3, Y2O3, or ZrO2 was used as a slurry raw material for forming a first sprayed film or a second sprayed film on the surface of the ceramic member facing the substrate mounting surface and the main surface formed by the flat surface of the cooling member. The porosity was adjusted so that the thermal conductivity of the ZrO2 sprayed film was 0.8 (W / mK), the thermal conductivity of the Y2O3 sprayed film was 2 (W / mK), and the thermal conductivity of the Al2O3 sprayed film was 4 (W / mK). The above thermal conductivities were measured at 25°C for a single sprayed film produced under the same conditions. The thickness of the sprayed film was 300 μm to 2000 μm.

[0051] The manufacturing method of the sprayed film of the sample is explained in detail. A high-speed plasma spraying machine was used to irradiate or spray a non-oxidizing gas plasma onto the back surface of the ceramic electrostatic chuck to preheat the surface. A mixture of Ar gas, N2 gas, and H2 gas was used as the non-oxidizing gas. The supply rate of Ar gas to the nozzle constituting the spraying machine was controlled to 100 l / min, the supply rate of N2 gas was controlled to 70 l / min, and the supply rate of H2 gas was controlled to 60 l / min. The current applied to the nozzle constituting the high-speed plasma spraying machine was controlled to 250 A, thereby adjusting the power supplied to the nozzle to 65 kW. The distance between the tip of the nozzle and the surface of the ceramic member or cooling member to be sprayed was adjusted to 75 mm. The scanning speed or displacement speed of the nozzle relative to the ceramic member or cooling member was adjusted to 850 mm / s. This generated plasma from a mixture of Ar gas, N2 gas, and H2 gas, and the plasma was irradiated or sprayed from the tip of the nozzle onto the surface to be sprayed, which was the ceramic member or the cooling member. The surface to be sprayed was preheated by irradiating or spraying the plasma for 10 minutes.

[0052] Then, the high-speed plasma spraying machine was used as it was, and the ceramic slurry containing the spraying raw material powder was plasma sprayed onto the sprayed surface on the back side of the ceramic electrostatic chuck using a non-oxidizing gas. The slurry was prepared by mixing 300 g of ceramic raw material powder with a purity of 99.9% or more and an average particle diameter D50 of 0.5 μm with 700 g of water. A mixed gas of Ar gas, N2 gas, and H2 gas was used as the non-oxidizing gas. The supply amount of Ar gas to the nozzle constituting the spraying machine was controlled to 100 l / min, the supply amount of N2 gas was controlled to 70 l / min, and the supply amount of H2 gas was controlled to 60 l / min. As a result, the spraying speed was controlled to 600 to 700 mm / s. The applied current to the nozzle constituting the high-speed plasma spraying machine was controlled to 250 A, and the power supplied to the nozzle was adjusted to 65 kW. The distance between the tip of the nozzle and the surface of the ceramic member or cooling member to be sprayed was adjusted to 75 mm. The scanning speed or displacement speed of the nozzle relative to the ceramic member or cooling member was adjusted to 850 mm / s. This generated a plasma of a mixed gas of Ar gas, N2 gas, and H2 gas, and the raw material powder melted by the plasma was sprayed from the tip of the nozzle onto the surface of the ceramic member or cooling member to be sprayed. In this way, a ceramic member or cooling member was formed in which one surface of the ceramic member or cooling member was covered with a ceramic sprayed film.

[0053] (Silicone adhesive layer) A general silicone resin was used with fillers such as alumina and metal dispersed to increase thermal conductivity. The thermal conductivity of the silicone adhesive layer was 0.9W / mK~2.0W / mK, and the thickness of the silicone adhesive layer was 500μm~2000μm.

[0054] (Evaluation method) The obtained electrostatic chuck was subjected to a predetermined evaluation process. The coolant used was a mixture of water and ethylene glycol, and the heat transfer coefficient was adjusted to 2500 W / mK. The coolant temperature was set to 20°C, and the flow rate of the coolant was set to 3 L / min. The following evaluations were performed.

[0055] The electrostatic chuck mounting surface was heated by placing another plate-shaped external heater made of AlN ceramics for supplying heat. For samples a1 to a7, a11 to a13, a15 and samples b1, b2, b4, and b6, the average temperature of the electrostatic chuck substrate mounting surface was controlled to be in a steady state of 250°C. For samples a8, a9, and a14, the amount of heat supplied was 10,000 (W / m 2 ) was used. In sample a10, the average temperature of the substrate mounting surface of the electrostatic chuck was controlled to be in a steady state of 300°C. In sample b3, the average temperature of the substrate mounting surface of the electrostatic chuck was controlled to be in a steady state of 240°C. In sample b3, the temperature of the silicone adhesive layer exceeded 200°C when the temperature of the substrate mounting surface of the electrostatic chuck was 250°C. In sample b5, the average temperature of the substrate mounting surface of the electrostatic chuck was controlled to be in a steady state of 400°C. The temperature of each part exposed on the side surface of the electrostatic chuck at that time was measured by directly contacting the silicone adhesive layer with a thermocouple, or the temperature of each part on the side surface was measured with an optical thermometer, as appropriate.

[0056] (Evaluation Results) Sample a8 is an electrostatic chuck on which the first sprayed film is not formed. In sample 8, when the temperature of the substrate mounting surface of the electrostatic chuck reached 232°C, the temperature of the silicone adhesive layer reached 206°C, exceeding the heat resistance temperature of the silicone adhesive layer. In contrast, in samples a1 to a6, a9 to a15, and samples b1 to b6 on which the first sprayed film and the second sprayed film were formed, the temperature of the silicone adhesive layer could be kept below 200°C when the temperature of the substrate mounting surface of the electrostatic chuck was set to 240°C or higher. In sample a6, the temperature of the silicone adhesive layer exceeded 200°C when the temperature of the substrate mounting surface of the electrostatic chuck was 250°C, but the temperature of the silicone adhesive layer was below 200°C when the temperature of the substrate mounting surface was 240°C. In other words, it was found that for samples a1 to a6, a9 to a15 and samples b1 to b6 on which a first and second sprayed films were formed, the temperature of the silicone adhesive layer could be kept below the heat-resistant temperature even when an electrostatic chuck (substrate holding member) was used in a process at a temperature higher than the heat-resistant temperature of the silicone adhesive layer, and deterioration of the silicone adhesive layer could be prevented.

[0057] Sample a7 is an electrostatic chuck without the second sprayed film. Samples a1 and b1 on which the first and second sprayed films are formed have a temperature distribution ΔT of 1.2°C and 1.0°C, respectively, on the substrate mounting surface, whereas sample a7 has a temperature distribution ΔT of 2.1°C. This is presumed to be because the heat flow from the electrostatic chuck toward the refrigerant flow path of the cooling member is affected by the second ceramic sprayed film formed on the surface of the cooling member, and this effect is also seen on the substrate mounting surface of the electrostatic chuck. As a result, it was found that samples a1 and b1 on which the first and second sprayed films are formed can reduce the thermal unevenness on the substrate mounting surface of the electrostatic chuck. It is presumed that samples a2 to a6, a9 to a15, and samples b2 to b6 on which the first and second sprayed films are formed have the same effect. The temperature distribution ΔT on the substrate mounting surface was obtained as the maximum value-minimum value in the inner region of a diameter of 290 mm using an infrared (IR) camera.

[0058] In addition, in the samples a1 to a5 and a9 to a15, the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C by adjusting the amount of heat supplied, and the temperature of the silicone adhesive layer at that time could be set to 200°C or less. In this case, the ceramic members of the samples a1 to a5 and a11 to a13 were made of ceramics containing AlN as the main component, and 0.75 ≧ (Re + Rf1) / (Re + Rf1 + Rb + Rf2 + Rm) ≧ 0.24 was satisfied. This confirmed that the substrate holding member, whose ceramic member is made of ceramics containing AlN as the main component and satisfies 0.75 ≧ (Re + Rf1) / (Re + Rf1 + Rb + Rf2 + Rm) ≧ 0.24, can be used in processes at least at 250°C or higher. In addition, the samples a9 and a14, which satisfy this condition, were able to be used in processes at 250°C or higher by adjusting the amount of heat supplied of 10,000 (W / m 2 ), the temperature of the substrate mounting surface could not reach 250°C, but samples a11 and a15, which were produced by increasing the amount of heat supplied using the same electrostatic chuck as samples a9 and a14, respectively, were able to reach a temperature of 250°C on the substrate mounting surface. Sample a10, which satisfied the above conditions, was able to keep the temperature of the silicone adhesive layer below 200°C even when the temperature of the substrate mounting surface was set to 300°C.

[0059] In addition, in the samples b1, b2, and b4 to b6, the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C by adjusting the amount of heat supplied, and the temperature of the silicone adhesive layer at that time could be set to 200°C or less. In this case, the ceramic members of the samples b1, b2, and b4 to b6 were formed of ceramics mainly composed of Al2O3, and satisfied 0.77≧(Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm)≧0.20. This confirmed that the substrate holding member, whose ceramic member is formed of ceramics mainly composed of Al2O3 and satisfies 0.77≧(Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm)≧0.20, can be used in processes at least at 250°C or more. In addition, the sample b5, which satisfies this condition, was able to keep the temperature of the silicone adhesive layer to 200°C or less even when the temperature of the substrate mounting surface was set to 400°C.

[0060] In addition, in samples a1 to a5, a10, a12, and a13, the amount of heat supplied was 10,000 (W / m 2 ), the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C. In this case, the ceramic members of the samples a1 to a5, a10, a12, and a13 were formed of ceramics containing AlN as the main component, and satisfied (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.83. This confirmed that an electrostatic chuck whose ceramic members are formed of ceramics containing AlN as the main component and which satisfies (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.83 can reduce the amount of heat supply required to maintain a predetermined process temperature.

[0061] In addition, for samples b1, b2, b4 to b6, the amount of heat supplied was 10,000 (W / m 2 ), the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C. In this case, samples b1, b2, and b4 to b6 had ceramic members formed of ceramics containing Al2O3 as the main component, and satisfied (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.63. This confirmed that an electrostatic chuck whose ceramic member is formed of ceramics containing Al2O3 as the main component and satisfies (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm) ≧ 0.63 can reduce the amount of heat supply required to maintain a specified process temperature.

[0062] From the above, it was confirmed that the substrate holding member of the present invention has a silicone adhesive layer temperature that is equal to or lower than the heat-resistant temperature of the silicone adhesive layer even when used in a process in which the substrate temperature exceeds the heat-resistant temperature of the silicone adhesive layer, and that the substrate mounting surface has a high uniformity of temperature distribution. It was also confirmed that the manufacturing method of the present invention can manufacture such a substrate holding member.

[0063] The present invention is not limited to the above-described embodiment, and it goes without saying that various modifications and equivalents are included within the spirit and scope of the present invention. In addition, the structure, shape, number, position, size, etc. of the components shown in each drawing are for convenience of explanation and may be changed as appropriate. [Explanation of symbols]

[0064] 10 Substrate holding member 12 Ceramic materials 14 First sprayed coating 16 Cooling material 18 Second spray coating 20 Silicone adhesive layer 22 Flow Path 24, 26 electrodes 28 Substrate mounting surface

Claims

1. A substrate holding member, a ceramic member formed in a flat plate shape from ceramics, having a substrate mounting surface on one main surface thereof and having an electrode embedded therein; a first thermal spray coating formed on the other main surface of the ceramic member; A metal cooling member having a coolant flow path therein; A second sprayed film formed on the planar main surface of the cooling member; a silicone adhesive layer that bonds the first sprayed film and the second sprayed film.

2. The ceramic member is formed of a ceramic mainly composed of AlN, The thermal resistance per unit area in the thickness direction of the ceramic member is Re (m 2 K / W), and the thermal resistance per unit area in the thickness direction of the first sprayed coating is Rf1 (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the second sprayed coating is Rf2 (m 2 K / W, and the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member on the silicone adhesive layer side to the flow path of the coolant is Rm (m 2 K / W), 0.75≧(Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm)≧0.24 2. The substrate holding member according to claim 1,

3. The ceramic member is Al 2 O 3 It is made of ceramics whose main component is The thermal resistance per unit area in the thickness direction of the ceramic member is Re (m 2 K / W), and the thermal resistance per unit area in the thickness direction of the first sprayed coating is Rf1 (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the second sprayed coating is Rf2 (m 2 K / W, and the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member on the silicone adhesive layer side to the flow path of the coolant is Rm (m 2 K / W), 0.77≧(Re+Rf1) / (Re+Rf1+Rb+Rf2+Rm)≧0.20 2. The substrate holding member according to claim 1,

4. In the substrate holding member, (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm)≧0.83 3. The substrate holding member according to claim 2, wherein

5. In the substrate holding member, (Rf1+Rb+Rf2) / (Re+Rf1+Rb+Rf2+Rm)≧0.63 4. The substrate holding member according to claim 3, wherein:

6. A method for manufacturing a substrate holding member, comprising the steps of: forming a ceramic raw material powder and firing the powder to produce a ceramic member having an electrode embedded therein; A step of preparing a plurality of metal members and forming grooves that serve as a flow path for a coolant; a step of joining the plurality of metal members having the grooves formed therein to fabricate a cooling member having the flow passage; spraying a first thermal spraying raw material powder containing a predetermined ceramic onto a surface of the ceramic member facing the substrate mounting surface to form a first thermal sprayed film; spraying a second thermal spraying raw material powder containing a predetermined ceramic onto one main surface of the cooling member to form a second thermal sprayed film; applying a silicone adhesive to at least one of the first sprayed film and the second sprayed film to bond the ceramic member and the cooling member; and curing the silicone adhesive to form a silicone adhesive layer.

Citation Information

Patent Citations

  • Wafer-mounting stage

    JP2003258065A

  • Susceptor

    JP2004079588A

  • Electrostatic chuck

    JP2007243139A

  • Bonding method, mounting table and substrate processing apparatus

    JP2014139989A

  • Plasma processing device

    JP2016031956A