Substrate holding member, manufacturing method thereof, and electrostatic chuck member

A ceramic-based substrate holding member with a thermal sprayed film and adjusted thermal resistance ratios maintains adhesive integrity at high temperatures, addressing heat resistance issues and ensuring efficient operation.

JP7565735B2Active Publication Date: 2024-10-11NITERRA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020160682
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-25
Publication Date
2024-10-11
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing substrate holding members, such as electrostatic chucks, face issues with heat resistance when using organic adhesives due to temperature limitations, as they decompose at high processing temperatures, and existing technologies do not adequately address this challenge.

Method used

A substrate holding member composed of a ceramic member with a thermal sprayed film and a silicone adhesive layer, where the thermal resistance ratios are adjusted to maintain the adhesive layer below its heat-resistant temperature, alleviating stress and preventing deterioration, even at high processing temperatures.

Benefits of technology

The substrate holding member can operate at temperatures higher than the adhesive's heat-resistant limit, preventing deterioration and ensuring uniform temperature distribution, while reducing the required heat input.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565735000001
    Figure 0007565735000001
  • Figure 0007565735000002
    Figure 0007565735000002
  • Figure 0007565735000003
    Figure 0007565735000003
Patent Text Reader

Abstract

To provide a substrate holding member, a method for manufacturing the same, and an electrostatic chuck member in which a temperature of an adhesive layer is equal to or less than a heat resistance temperature of an organic adhesive, even when used in a process in which the temperature of the substrate is equal to or higher than the heat resistance temperature of the organic adhesive in the adhesive layer.SOLUTION: A substrate holding member 10 comprises: a ceramic member 12 being formed into a flat shape and formed of ceramics and having a substrate mounting surface 26 on one major surface; a thermal spray film 14 formed on the other major surface of the ceramic member 12; a metal cooling member 16 having a refrigerant flow path 20 inside; and a silicone adhesive layer 18 joining the thermal spray film 14 and the cooling member 16.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate holding member, a manufacturing method thereof, and an electrostatic chuck member. [Background technology]

[0002] 2. Description of the Related Art Some substrate holding members used in semiconductor manufacturing equipment, such as electrostatic chucks, are equipped with a cooling member in order to maintain the substrate at a predetermined temperature during semiconductor processing.

[0003] Patent Document 1 discloses a heater unit having a substrate having a cooling flow path, a heater section disposed above the substrate and having a heating element, and a heat insulating layer disposed between the substrate and the heater section. It also describes that the thermal conductivity of the heat insulating layer may be lower than that of the substrate, that the heat insulating layer may be SUS containing pores, that the heater unit further has an insulator covering the heating element, and that the thermal conductivity of the heat insulating layer may be lower than that of the insulator.

[0004] Patent Document 2 discloses a method for manufacturing a dissimilar material joint, which is characterized by interposing a third member having a Young's modulus of 150 GPa or less and a melting point of 1500 K or less between a first member and a second member having a thermal expansion coefficient different from that of the first member, via a metal brazing material, and brazing the first member to the second member.

[0005] Patent Document 3 discloses a heat dissipation component having a three-layer structure formed by bonding a flat aluminum-ceramic composite formed by impregnating a ceramic porous body with an aluminum alloy, the heat dissipation component being characterized in that a cooling groove penetrating the front and back is provided in the intermediate layer by water jet machining or electric discharge machining, the heat dissipation component being characterized in that the aluminum-ceramic composite is manufactured by a high-pressure forging method, and the ceramic porous body is composed of at least one material selected from the group consisting of silicon carbide, silicon nitride, aluminum nitride, and alumina.

[0006] Furthermore, Patent Document 4 discloses an electrostatic chuck in which a metal plate having an insulator film formed on its surface by thermal spraying and a dielectric substrate having an electrode formed on its surface are joined with an insulating adhesive so that the electrodes face each other, the insulator film having a thickness of 0.3 mm or more and 0.6 mm or less, the insulating adhesive having a thermal conductivity of 1 W / mK or more, and the thermal conductivity of the insulator film being greater than that of the insulating adhesive. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-037721 A [Patent Document 2] JP 2010-052011 A [Patent Document 3] JP 2008-071845 A [Patent Document 4] JP 2007-243139 A Summary of the Invention [Problem to be solved by the invention]

[0008] Traditionally, cooling plates for cooling substrate-holding members such as electrostatic chucks have been made of metal materials, especially Al alloys, due to their workability and cooling effect. In addition, ceramic sintered bodies made of Al2O3 or AlN have been used for substrate-holding members. To integrate these members, organic adhesives have been proposed because of their ease of integration. However, when using organic adhesives as a bonding layer, their heat resistance becomes an issue, and they could not be used, especially when using electrostatic chucks in processes above 200°C, because the temperature reaches a point where the organic adhesive layer decomposes.

[0009] However, Patent Document 1 does not take into account the bonding between the heat insulating layer and the base material or the heat insulating layer and the heater part, and therefore does not take into account the heat resistance when an organic adhesive is used. Patent Document 2 uses a metal brazing material for bonding, and therefore does not take into account the heat resistance when an organic adhesive is used. Patent Document 3 focuses on the thermal expansion coefficient of the heat dissipation component, but does not take into account the heat resistance when an organic adhesive is used. Patent Document 4 does not take into account the heat resistance of the insulating adhesive layer.

[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide a substrate holding member, a manufacturing method thereof, and an electrostatic chuck member, which ensure that the temperature of the adhesive layer is equal to or lower than the heat resistance temperature of the organic adhesive even when used in a process in which the temperature of the substrate reaches or exceeds the heat resistance temperature of the organic adhesive in the adhesive layer. [Means for solving the problem]

[0011] (1) In order to achieve the above object, the substrate holding member of the present invention is characterized by comprising a ceramic member formed in a flat plate shape from ceramics and having a substrate mounting surface on one main surface, a thermal spray film formed on the other main surface of the ceramic member, a metal cooling member having a coolant flow path inside, and a silicone adhesive layer bonding the thermal spray film and the cooling member. As a result, even if the substrate holding member is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer, the temperature of the silicone adhesive layer can be kept below the heat resistance temperature, preventing deterioration of the silicone adhesive layer, and the flexibility of the silicone adhesive layer can relieve stress generated between the substrate holding member and the cooling member. As a result, it becomes possible to use the substrate holding member in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer.

[0012] (2) In addition, in the substrate holding member of the present invention, the ceramic member is formed of a ceramic mainly composed of AlN, and when the thermal resistance per unit area in the thickness direction of the sprayed film is Rf and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb, Rf / Rb ≧ 0.32. In this way, by adjusting the ratio of the thermal resistance per unit area of ​​the sprayed film to the thermal resistance per unit area of ​​the silicone adhesive layer according to the ceramic material forming the ceramic member, the substrate holding member can be used even in high-temperature processes of 250°C or higher.

[0013] (3) In addition, in the substrate holding member of the present invention, the ceramic member is formed of a ceramic mainly composed of Al2O3, and when the thermal resistance per unit area in the thickness direction of the sprayed film is Rf and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb, Rf / Rb ≧ 0.25. In this way, by adjusting the ratio of the thermal resistance per unit area of ​​the sprayed film to the thermal resistance per unit area of ​​the silicone adhesive layer according to the ceramic material forming the ceramic member, the substrate holding member can be used even in high-temperature processes of 250°C or higher.

[0014] (4) In addition, in the substrate holding member of the present invention, when the thermal resistance per unit area in the thickness direction of the ceramic member is Re, and the thermal resistance per unit area in the thickness direction of the region from the main surface of the cooling member on the silicone adhesive layer side to the coolant flow path is Rm, (Rf+Rb) / (Re+Rf+Rb+Rm)≧0.84 is satisfied. In this way, by adjusting the thermal resistance per unit area of ​​the ceramic member, the sprayed film, the silicone adhesive layer, and the cooling member according to the ceramic material forming the ceramic member, the amount of heat supply required to maintain a predetermined process temperature can be reduced.

[0015] (5) In addition, in the substrate holding member of the present invention, when the thermal resistance per unit area in the thickness direction of the ceramic member is Re, and the thermal resistance per unit area in the thickness direction of the region from the main surface of the cooling member on the silicone adhesive layer side to the coolant flow path is Rm, (Rf+Rb) / (Re+Rf+Rb+Rm)≧0.71 is satisfied. In this way, by adjusting the thermal resistance per unit area of ​​the ceramic member, the sprayed film, the silicone adhesive layer, and the cooling member according to the ceramic material forming the ceramic member, the amount of heat supply required to maintain a predetermined process temperature can be reduced.

[0016] (6) The electrostatic chuck member of the present invention is an electrostatic chuck member, comprising a ceramic member formed in a flat plate shape from ceramics mainly composed of AlN, having a substrate mounting surface on one main surface, and having an electrode embedded therein, and a thermal spray film formed on the other main surface of the ceramic member, characterized in that, when the thermal resistance per unit area in the thickness direction of the ceramic member is Re and the thermal resistance per unit area in the thickness direction of the thermal spray film is Rf, 0.38≧Re / Rf≧0.03 is satisfied. In such an electrostatic chuck member having a thermal spray film on the back surface, the thermal resistance per unit area of ​​the ceramic member and the thermal spray film can be adjusted according to the ceramic material forming the ceramic member, so that when the heat input to the electrostatic chuck surface is transferred to the cooling member, the temperature difference (temperature gradient) between the front and back of the thermal spray film can be increased. As a result, when the electrostatic chuck member is bonded to the cooling member by a heat-resistant adhesive, the temperature of the lower surface (adhesive side) of the thermal spray film can be made lower than the heat-resistant temperature of the heat-resistant adhesive.

[0017] (7) The electrostatic chuck member of the present invention is an electrostatic chuck member, comprising a ceramic member formed in a flat plate shape from ceramics mainly composed of Al2O3, having a substrate mounting surface on one main surface, and an electrode embedded therein, and a thermal spray film formed on the other main surface of the ceramic member, characterized in that, when the thermal resistance per unit area in the thickness direction of the ceramic member is Re and the thermal resistance per unit area in the thickness direction of the thermal spray film is Rf, 1.33≧Re / Rf≧0.13 is satisfied. In such an electrostatic chuck member having a thermal spray film on the back surface, the thermal resistance per unit area of ​​the ceramic member and the thermal spray film can be adjusted according to the ceramic material forming the ceramic member, so that when the heat input to the electrostatic chuck surface is transferred to the cooling member, the temperature difference (temperature gradient) between the front and back of the thermal spray film can be increased. As a result, when the electrostatic chuck member is bonded to the cooling member by a heat-resistant adhesive, the temperature of the lower surface (adhesive side) of the thermal spray film can be made lower than the heat-resistant temperature of the heat-resistant adhesive.

[0018] (8) The method for manufacturing a substrate holding member of the present invention is characterized by including the steps of forming and firing a ceramic raw material powder to prepare a ceramic member, preparing a plurality of metal members and forming a groove portion that serves as a flow path for a coolant, joining the plurality of metal members with the groove portion to prepare a cooling member having the flow path, spraying a spray raw material powder containing a predetermined ceramic on a surface of the ceramic member facing the substrate mounting surface to form a sprayed film, applying a silicone adhesive to at least one of the sprayed film or the joining surface of the cooling member to bond the ceramic member and the cooling member, and curing the silicone adhesive to form a silicone adhesive layer. This allows the temperature of the silicone adhesive layer to be kept below the heat-resistant temperature, preventing deterioration of the silicone adhesive layer, and alleviating stress generated between the substrate holding member and the cooling member due to the flexibility of the silicone adhesive layer. As a result, it becomes possible to use the substrate holding member in a process at a temperature higher than the heat-resistant temperature of the silicone adhesive layer. Effect of the Invention

[0019] According to the present invention, even if the substrate holding member is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer, the temperature of the silicone adhesive layer can be kept below the heat resistance temperature, and deterioration of the silicone adhesive layer can be prevented. As a result, the substrate holding member can be used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a front cross-sectional view showing the substrate holding member of the embodiment. [Diagram 2] FIG. 2 is a front cross-sectional view showing the electrostatic chuck member of the embodiment. [Diagram 3] 1 is a table showing the manufacturing conditions and temperature measurements for each sample. [Figure 4] 1 is a table showing the manufacturing conditions and temperature measurements for each sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Next, an embodiment of the present invention will be described with reference to the drawings. In order to facilitate understanding of the description, the same reference numerals are used for the same components in each drawing, and duplicated descriptions will be omitted. In the configuration diagrams, the size of each component is conceptually shown, and does not necessarily represent the actual dimensional ratio.

[0022] [Embodiment] [Configuration of the substrate holding member] 1 is a front cross-sectional view showing a substrate holding member 10. The substrate holding member 10 includes a ceramic member 12, a sprayed film 14, a cooling member 16, and a silicone adhesive layer 18. The substrate holding member 10 may also have one or more electrodes embedded therein as necessary. The substrate holding member 10 can be used, for example, in an electrostatic chuck, a heater, etc.

[0023] The ceramic member 12 is formed of ceramics in a flat plate shape, and has a substrate mounting surface 26 on one of its main surfaces. The ceramics constituting the ceramic member 12 are preferably ceramics containing AlN or Al2O3 as the main component. "Mainly containing" means that the weight ratio of the main component to the weight of the ceramic member 12 is 90 wt% or more. The ceramic member 12 may contain additives for various purposes, such as increasing thermal conductivity, in addition to the ceramics as the main component. For example, additives made of oxides of Group 2a elements or Group 3a elements or transition metal oxides may be added to adjust thermal conductivity or volume resistivity.

[0024] In general, in the case of ceramics mainly composed of AlN, it is known that the thermal conductivity increases with increasing amount of additives such as Y2O3, but adding more than a certain amount causes a decrease in thermal conductivity. Therefore, it is desirable to keep the content of additives consisting of oxides of 2a group elements and 3a group elements and transition metal oxides to 10wt% or less. In the case of ceramics mainly composed of Al2O3, it is also desirable to keep the content of additives consisting of oxides of 2a group elements and 3a group elements and transition metal oxides to 10wt% or less. Examples of additives of 2a group elements include Mg, Ca, Sr, Ba, etc., and examples of additives of 3a group elements include Y, La, Sm, Ce, etc. Examples of additives of transition metals include Ti, Cr, Mn, Ni, etc.

[0025] The sprayed film 14 is formed on the surface of the ceramic member 12 facing the substrate mounting surface 26. The sprayed film 14 is made of ceramics. The sprayed film 14 is preferably made of ceramics with low thermal conductivity, such as Al2O3, Y2O3, or ZrO2. The sprayed film 14 can be produced by a plasma spraying method, a dry plasma spraying method, or other known spraying methods. The thickness of the sprayed film 14 is preferably 0.3 mm or more and 3 mm or less.

[0026] It is preferable that the sprayed film 14 has a predetermined porosity. This enhances the heat insulating effect. The porosity is preferably 2% or more, and more preferably 5% or more. The upper limit of the porosity does not need to be particularly limited as long as the thermal conductivity of the sprayed film 14 can be within a predetermined range, but it can be, for example, 10% or less.

[0027] The cooling member 16 is made of metal and has a coolant flow path 20 inside. The metal constituting the cooling member 16 is most preferably an Al alloy because of its workability and high thermal conductivity, but alloys containing copper, titanium, nickel, SUS, etc. may also be used. The coolant may be water, ethylene glycol, fluorocarbon, etc., and the coolant temperature may be below the boiling point.

[0028] The silicone adhesive layer 18 bonds the sprayed film 14 and the cooling member 16. This allows the ceramic member 12 and the cooling member 16 to be bonded. The silicone adhesive layer 18 is formed of a silicone adhesive containing silicone as a main component, such as silicone resin or modified silicone resin. The curing type of the silicone adhesive can be selected from dehydration, dealcoholization, and addition polymerization types. One-component curing, two-component curing, and ultraviolet curing types can also be selected. The silicone adhesive may contain ceramics such as Al2O3 and AlN or metal fillers such as Cu to adjust thermal conductivity. The thickness of the silicone adhesive layer 18 is preferably 0.1 mm or more and 2.0 mm or less. The silicone adhesive layer 18 has a sufficiently small Young's modulus compared to ceramics and metals, so it can maintain flexibility.

[0029] The ceramic member 12 shown in Fig. 1 has two electrodes 22, 24 embedded therein. The electrode 22 in Fig. 1 is an electrode for electrostatic attraction, and the electrode 24 is an electrode that functions as a heating resistor. In this manner, the substrate holding member 10 may have one or more electrodes embedded therein, as necessary. The substrate holding member 10 shown in Fig. 1 is an electrostatic chuck having a heating resistor.

[0030] In this way, by providing the thermal spray film 14 on the bonding surface between the ceramic member 12 and the silicone adhesive layer 18, even if the substrate holding member 10 is used in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer 18, the temperature of the silicone adhesive layer 18 can be kept below the heat resistance temperature, and deterioration of the silicone adhesive layer 18 can be prevented. At the same time, the flexibility of the silicone adhesive layer can reduce stress generated between the substrate holding member and the cooling member. As a result, it is possible to use the substrate holding member 10 in a process at a temperature higher than the heat resistance temperature of the silicone adhesive layer 18 while making the temperature distribution of the substrate mounting surface 26 of the substrate holding member 10 uniform.

[0031] (Thermal resistance design) The above-mentioned configuration allows the substrate holding member 10 to be used in processes at temperatures higher than the heat resistance temperature of the silicone adhesive layer 18. However, when considering use in processes at higher temperatures or reducing the amount of heat required to maintain a given process temperature, it is preferable to design the thermal resistance of the substrate holding member 10. The thermal resistance per unit area in the thickness direction of the substrate holding member 10 (m 2 The thermal resistance Re(m 2 The thermal resistance Rf (m 2 The thermal resistance Rm (m 2 The thermal resistance Rb (m 2 The thermal conductivity of the silicone adhesive layer (W / mK) is defined as the thickness (m) of the silicone adhesive layer divided by the thermal conductivity of the silicone adhesive layer (W / mK). The thickness direction is defined as the direction perpendicular to the substrate mounting surface 26 of the substrate holding member 10.

[0032] When the ceramic member 12 is mainly composed of AlN, the substrate holding member 10 preferably has Rf / Rb≧0.32. In this way, by adjusting the ratio of the thermal resistance per unit area of ​​the sprayed film 14 to the thermal resistance per unit area of ​​the silicone adhesive layer 18 according to the ceramic material forming the ceramic member 12, the substrate holding member 10 can be used even in high-temperature processes of 250° C. or more. The value of Rf / Rb is considered to indicate the temperature of the silicone adhesive layer 18. The value of Rf / Rb is related to the temperature of the interface between the silicone adhesive layer 18 and the sprayed film 14, and the higher the value, the lower the temperature of the silicone adhesive layer 18 tends to be, and the lower the value, the higher the temperature tends to be.

[0033] When the ceramic member of the substrate holding member 10 is mainly composed of Al2O3, it is preferable that Rf / Rb ≧ 0.25. In this way, by adjusting the ratio of the thermal resistance per unit area of ​​the sprayed film 14 to the thermal resistance per unit area of ​​the silicone adhesive layer 18 according to the ceramic material forming the ceramic member 12, the substrate holding member 10 can be used even in high temperature processes of 250°C or more.

[0034] In addition, when the ceramic member 12 is made of ceramics mainly composed of AlN, the substrate holding member 10 preferably has (Rf+Rb) / (Re+Rf+Rb+Rm)≧0.84. In this way, the amount of heat required to maintain a predetermined process temperature can be reduced by adjusting the thermal resistance per unit area of ​​the ceramic member 12, the sprayed film 14, the silicone adhesive layer 18, and the cooling member 16 according to the ceramic material forming the ceramic member 12. The value of (Rf+Rb) / (Re+Rf+Rb+Rm) is considered to indicate the degree of ease of application to semiconductor processes. If the value of (Rf+Rb) / (Re+Rf+Rb+Rm) is small, the amount of heat required to reach a predetermined substrate processing temperature becomes excessively large, and it tends to be difficult to use in semiconductor processes.

[0035] Furthermore, when the ceramic member of the substrate holding member 10 is made of ceramics containing Al2O3 as a main component, it is preferable that (Rf+Rb) / (Re+Rf+Rb+Rm)≧0.71. In this manner, by adjusting the thermal resistance per unit area of ​​the ceramic member 12, the sprayed film 14, the silicone adhesive layer 18, and the cooling member 16 according to the ceramic material forming the ceramic member 12, the amount of heat supply required to maintain a predetermined process temperature can be reduced.

[0036] In designing the thermal resistance, the thickness and thermal conductivity of each member are preferably within the following ranges. The ceramic member 12 is preferably 1 mm or more and 30 mm or less in thickness, and the thermal conductivity of the ceramic member 12 is preferably 4 W / mK or more and 250 W / mK or less in thickness. The sprayed film 14 is preferably 0.3 mm or more and 3.0 mm or less in thickness, and the thermal conductivity of the sprayed film 14 is preferably 0.4 W / mK or more and 16.0 W / mK or less in thickness. The silicone adhesive layer 18 is preferably 0.1 mm or more and 2.0 mm or less in thickness, and the thermal conductivity of the silicone adhesive layer 18 is preferably 0.1 W / mK or more and 4.0 W / mK or less in thickness. The cooling member 16 is preferably 2 mm or more and 30 mm or less in thickness, and the cooling member 16 is preferably 10 W / mK or more and 300 W / mK or less in thermal conductivity. The thermal conductivity of each part is measured at 25°C.

[0037] [Method of manufacturing the substrate holding member] Next, a method for manufacturing the substrate holder configured as described above will be described in the following order: a method for manufacturing the ceramic member, a method for manufacturing the cooling member, a thermal spraying method, and a method for forming the silicone adhesive layer.

[0038] (Method of manufacturing ceramic members) The following manufacturing method for ceramic members will be described as a method for producing ceramic members from raw materials whose main component is AlN by powder hot pressing, but the raw materials and manufacturing method are not limited to this method and can also be applied to ceramic members whose main component is Al2O3. In addition to the powder hot pressing method, it is also possible to adopt green sheet lamination methods and other conventional manufacturing methods. First, the AlN ceramic raw material powder is granulated. The granulated powder is added with 0.3 wt% to 6 wt% Y2O3 in an internal ratio, and a binder is added to granulate the granulated powder. Next, the granulated powder is filled into a bottomed carbon mold (molding die), a carbon punch is placed on it, and then sintered.

[0039] At this time, an electrode for electrostatic attraction or an electrode serving as a heating resistor may be embedded in the ceramic member. Heat-resistant metals such as tungsten and molybdenum can be used as the electrode for electrostatic attraction or the heating resistor. For example, an electrode for electrostatic attraction or a heating resistor formed of a plate, foil, wire, mesh, or the like is embedded during molding and sintered. For example, when embedding one layer of electrodes, a molding die is filled with granulated powder corresponding to the insulating layer of the ceramic member, and the electrode is placed on the molded body after uniaxial pressing. The same granulated powder is filled on top of it, a carbon punch is placed on it, and then sintered. When embedding two or more layers of electrodes, the process of filling with granulated powder and placing the electrode on the molded body after uniaxial pressing is repeated.

[0040] The firing process is preferably atmospheric firing or uniaxial hot press firing. Normal pressure firing is performed at 1800°C or higher, and uniaxial hot press firing is performed at 1700°C or higher and 1 MPa or higher pressure and temperature conditions. However, the firing method is not limited to these. After firing, the substrate mounting surface on which the substrate is mounted and the back surface on which the sprayed film is provided are formed, and the ceramic member is processed into a predetermined shape. The outer shape of the ceramic member can be selected according to the shape of the substrate to be mounted, such as circular or rectangular.

[0041] (Method of manufacturing cooling member) First, a plurality of metal members are prepared, and grooves are formed as the flow paths of the refrigerant. Next, the plurality of metal members with the grooves formed therein are joined to produce a cooling member having a flow path. The flow paths are formed by performing a predetermined machining process on the plurality of metal members, and then using a conventional metal joining method such as brazing, electron beam welding, or diffusion bonding. The most suitable metal is an Al alloy because of its workability and high thermal conductivity, but alloys containing copper, titanium, and nickel, and SUS can also be used. A flow path for the refrigerant is formed inside the metal cooling member. The size and shape of the flow path of the refrigerant may be any size and shape that can uniformly cool the ceramic member.

[0042] (Thermal spraying method) A sprayed film is formed by spraying a spraying raw material powder containing a predetermined ceramic on the surface of the ceramic member facing the substrate mounting surface. The sprayed film can be produced by a known spraying method, such as a plasma spraying method using a slurry containing ceramic raw material powder, a dry plasma spraying method in which raw material powder is granulated and fed, or other known methods. The film type of the sprayed film is preferably Al2O3, Y2O3, ZrO2, etc. The sprayed film has a certain porosity, and the pores exert a heat insulating effect. Therefore, the porosity of the sprayed film is preferably 2% or more, and more preferably 5% or more. The thermal conductivity of the sprayed film can be adjusted to 0.4 to 16 W / mK depending on these raw materials and porosity. The thickness of the sprayed film is preferably 0.3 mm or more and 3.0 mm or less.

[0043] (Method of forming silicone adhesive layer) The curing type of the silicone adhesive can be selected from dehydration, dealcoholization, addition polymerization, etc. Also, one-component curing, two-component curing, ultraviolet curing, etc. can be selected. Of these, the silicone adhesive forming the silicone adhesive layer is preferably a heat-curing one. The following description will explain a method of forming a silicone adhesive layer using a heat-curing silicone adhesive.

[0044] The silicone adhesive is applied to at least one of the joint surfaces of the sprayed film or the cooling member after weighing and stirring an appropriate amount, and after degassing, the two are laminated and a load is applied to heat cure in an oven in air, nitrogen atmosphere, or reduced pressure. In order to suppress the outgassing of siloxane components from the silicone adhesive, it is preferable to cure at 100°C or higher and then treat at 200°C or higher for a certain period of time. In addition, a spacer of a specified thickness may be placed at the same time to adjust the thickness of the silicone adhesive layer. The ceramic member coated with the sprayed film on the back side by the above treatment and the metal cooling member are bonded with the silicone adhesive to form a silicone adhesive layer. Note that if the center line average roughness Ra of the sprayed film is 1 μm or more, the silicone adhesive can penetrate into the gaps in the roughness curve of the sprayed film and adhere well.

[0045] By this method, the substrate holding member can be manufactured.

[0046] [Electrostatic chuck component configuration] 2 is a front cross-sectional view showing an electrostatic chuck member 30. The electrostatic chuck member 30 includes a ceramic member 12 in which an electrode 22 is embedded, and a thermal sprayed film 14. Details of the ceramic member 12 and the thermal sprayed film 14 are similar to those of the above-described substrate holding member 10. The electrode 22 is an electrode for electrostatic attraction. In addition, the electrostatic chuck member 30 may have other electrodes, such as a heater electrode, embedded therein as necessary.

[0047] In order to provide an electrostatic chuck member 30 of the present invention that can be used in processes that have a temperature equal to or higher than the heat resistance of the heat-resistant adhesive when attached to a general cooling member using a heat-resistant adhesive not limited to a silicone adhesive, the thermal resistances of the ceramic member 12 and the sprayed film 14 are designed according to the ceramic material that forms the ceramic member 12. The thermal resistance Re per unit area in the thickness direction of the ceramic member 12 and the thermal resistance Rf per unit area in the thickness direction of the sprayed film 14 are similar to those of the substrate holding member 10 described above.

[0048] (Thermal resistance design) When the ceramic member 12 is formed of a ceramic containing AlN as a main component, the electrostatic chuck member 30 satisfies 0.38≧Re / Rf≧0.03. In this manner, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member 12 and the sprayed film 14 according to the ceramic material forming the ceramic member 12, any adhesive having a heat resistance of 200° C. or higher, not limited to silicone adhesive, can be bonded and integrated with a general cooling plate and used in processes at temperatures above the heat resistance temperature.

[0049] Furthermore, when the ceramic member 12 of the electrostatic chuck member 30 is formed of a ceramic containing Al2O3 as a main component, Re / Rf satisfies 1.33≧Re / Rf≧0.13. In this manner, by adjusting the thermal resistance per unit area in the thickness direction of the ceramic member 12 and the sprayed film 14 according to the ceramic material forming the ceramic member 12, any adhesive having a heat resistance of 200° C. or higher, not limited to silicone adhesive, can be used to bond and integrate with a general cooling plate and can be used in processes at temperatures above the heat resistance temperature.

[0050] The electrostatic chuck member 30 can be used in processes at 250°C or higher when bonded with a silicone adhesive, a polyimide-based varnish adhesive, or a heat-resistant inorganic adhesive mainly composed of fire-resistant ceramics and an inorganic polymer. Although an Al alloy is often used for the cooling member, other metals such as SUS, Ti, Cu, brass, and ceramics may also be used. In any of these cases, the electrostatic chuck member 30 of the present invention can keep the temperature of the adhesive below the heat-resistant temperature because the temperature difference between the front and back of the sprayed film is large.

[0051] [Examples and Comparative Examples] [Samples a1-a14] Next, examples and comparative examples will be described. First, as a sample using AlN as the material of the ceramic member, an electrostatic chuck was produced in which a ceramic member mainly composed of AlN in which an electrode for an electrostatic chuck is embedded and a cooling member made of an Al alloy are bonded with a silicone adhesive layer. Samples a1 to a14 were produced by varying the presence or absence of a sprayed film, the material, the thickness, the thermal conductivity and the thickness of the silicone adhesive layer. Hereinafter, samples a1 to a14 are collectively referred to as sample a. FIG. 3 is a table showing the manufacturing conditions and the measured temperature of each sample a1 to a14.

[0052] (Preparation of ceramic members for use in sample a) The raw material was AlN with 5wt% Y2O3 added as an additive, and an electrode made of cut Mo mesh (wire diameter 0.1mm, mesh size #50) was embedded as an electrode. After uniaxial hot press sintering, it was machined into a specified shape, and a substrate mounting surface was provided on the front side, and a flat surface on which the thermal spray coating was sprayed was provided on the back side opposite the front side, to produce a ceramic component with a diameter of 300mm and a thickness of 15mm. The surface roughness Ra of the substrate mounting surface was 0.5μm, and the surface roughness Ra of the sprayed surface was 1.5μm. These were measured in accordance with JIS B 0601 and ISO25178. The thermal conductivity measured for the ceramic component alone was 160W / mK at 25℃. The thermal conductivity was measured using the laser flash method in accordance with JIS R 1611-1997.

[0053] [Samples b1-b13] In addition, as a sample using Al2O3 as the material of the ceramic member, an electrostatic chuck was fabricated in which a ceramic member mainly composed of Al2O3 with an electrode for electrostatic chuck embedded therein and a cooling member made of an Al alloy were bonded with a silicone adhesive layer. Samples b1 to b13 were created by varying the presence or absence of a thermal sprayed film, the material, thickness, and the thermal conductivity and thickness of the silicone adhesive layer. Hereinafter, samples b1 to b13 are collectively referred to as sample b. Figure 4 is a table showing the manufacturing conditions and measured temperatures for each of samples b1 to b13.

[0054] (Preparation of ceramic members for use in sample b) The raw material was Al2O3 with 0.05wt% MgO added as an additive, and an electrode made from cut Mo mesh (wire diameter 0.1mm, mesh size #50) was embedded as the electrode. After uniaxial hot press sintering, it was machined into the specified shape, and a substrate mounting surface was provided on the front surface, and a flat surface on which the thermal spray film was sprayed was provided on the back surface opposite the front surface, producing a ceramic component with a diameter of 300mm and a thickness of 15mm. The surface roughness Ra of the substrate mounting surface was 0.4μm, and the surface roughness Ra of the sprayed surface was 1.2μm. The thermal conductivity measured on the ceramic component alone was 30W / mK at 25℃.

[0055] (Production of cooling components) An Al alloy (6061T6) was used as the metal. The coolant flow paths were rectangular with a cross section of 10 mm wide and 5 mm high, and were arranged at a radial distance of 20 mm. The shortest vertical distance from the surface of the cooling member to the flow paths was 15 mm. The surface roughness Ra of the sprayed surface of the cooling member was 1.6 μm. The cooling member was the same for sample a and sample b. The thermal conductivity of the cooling member was 138 W / mK at 25°C.

[0056] (Formation of thermal spray coating) Al2O3, Y2O3, or ZrO2 was used as the slurry raw material for forming a thermal sprayed film on the surface of the ceramic member opposite to the substrate mounting surface. The porosity was adjusted so that the thermal conductivity of the ZrO2 thermal sprayed film was 0.8 (W / mK), the thermal conductivity of the Y2O3 thermal sprayed film was 2 (W / mK), and the thermal conductivity of the Al2O3 thermal sprayed film was 4 (W / mK). The above thermal conductivities were measured at 25°C for a single thermal sprayed film produced under the same conditions. The thickness of the thermal sprayed film was 300 μm to 3000 μm.

[0057] The manufacturing method of the sprayed film of the sample is explained in detail. A high-speed plasma spraying machine was used to irradiate or spray a non-oxidizing gas plasma onto the back surface of the ceramic electrostatic chuck to preheat the surface. A mixture of Ar gas, N2 gas, and H2 gas was used as the non-oxidizing gas. The supply rate of Ar gas to the nozzle constituting the spraying machine was controlled to 100 l / min, the supply rate of N2 gas was controlled to 70 l / min, and the supply rate of H2 gas was controlled to 60 l / min. The current applied to the nozzle constituting the high-speed plasma spraying machine was controlled to 250 A, thereby adjusting the power supplied to the nozzle to 65 kW. The distance between the tip of the nozzle and the surface of the ceramic member to be sprayed was adjusted to 75 mm. The scanning speed or displacement speed of the nozzle relative to the ceramic member was adjusted to 850 mm / s. This generated plasma from a mixture of Ar gas, N2 gas, and H2 gas, and the plasma was irradiated or sprayed from the tip of the nozzle onto the surface of the ceramic member to be sprayed. The surface to be sprayed was preheated by irradiating or spraying the plasma for 10 minutes.

[0058] Then, the high-speed plasma spraying machine was used as it was, and the ceramic slurry containing the spraying raw material powder was plasma sprayed onto the sprayed surface on the back side of the ceramic electrostatic chuck using a non-oxidizing gas. The slurry was prepared by mixing 300 g of ceramic raw material powder with a purity of 99.9% or more and an average particle diameter D50 of 0.5 μm with 700 g of water. A mixed gas of Ar gas, N2 gas, and H2 gas was used as the non-oxidizing gas. The supply amount of Ar gas to the nozzle constituting the spraying machine was controlled to 100 l / min, the supply amount of N2 gas was controlled to 70 l / min, and the supply amount of H2 gas was controlled to 60 l / min. As a result, the spraying speed was controlled to 600 to 700 mm / s. The applied current to the nozzle constituting the high-speed plasma spraying machine was controlled to 250 A, and the power supplied to the nozzle was adjusted to 65 kW. The distance between the tip of the nozzle and the surface of the ceramic member or cooling member to be sprayed was adjusted to 75 mm. The scanning speed or displacement speed of the nozzle relative to the ceramic member or cooling member was adjusted to 850 mm / s. This generated a plasma of a mixed gas of Ar gas, N2 gas, and H2 gas, and the raw material powder melted by the plasma was sprayed from the tip of the nozzle onto the surface of the ceramic member to be sprayed. In this way, a ceramic member was formed in which one side of the ceramic member was covered with a ceramic sprayed film.

[0059] (Silicone adhesive layer) A general silicone resin was used with fillers such as alumina and metal dispersed to increase thermal conductivity. The thermal conductivity of the silicone adhesive layer was 0.9W / mK~2.0W / mK, and the thickness of the silicone adhesive layer was 500μm~2000μm.

[0060] (Evaluation method) The obtained electrostatic chuck was subjected to a predetermined evaluation process. At this time, a mixture of water and ethylene glycol was used as the coolant, and the heat transfer coefficient was adjusted to 2000 to 3000 W / mK. The coolant temperature was set to 20°C, and the flow rate of the coolant was set to 3 L / min. Then, the following evaluations were performed.

[0061] A separate plate-shaped external heater made of AlN ceramics was placed on the electrostatic chuck mounting surface to supply heat and heat it. For samples a1 to a8, a11 to a14 and samples b1 to b8, b10 to b12, the average temperature of the electrostatic chuck substrate mounting surface was controlled to be in a steady state of 250°C. For samples a9 and b9, the amount of heat supplied was 10,000 (W / m 2 ) for sample a10, the average temperature of the substrate mounting surface of the electrostatic chuck was controlled to be in a steady state of 300° C. Then, the temperature of each part exposed on the side surface of the electrostatic chuck was measured together with the temperature of the silicone adhesive layer by directly contacting the electrostatic chuck with a thermocouple, or the temperature of each part on the side surface was measured by using an optical pyrometer in combination as appropriate.

[0062] (Evaluation Results) In samples a1 to a13 and samples b1 to b12, in which a sprayed film was formed on a ceramic member, the temperature of the silicone adhesive layer could be kept below 200° C. when the temperature of the substrate mounting surface of the electrostatic chuck was set to 220° C. or higher. In other words, it was found that in samples a1 to a13 and samples b1 to b12, in which a sprayed film was formed, the temperature of the silicone adhesive layer could be kept below the heat-resistant temperature even when the electrostatic chuck (substrate holding member) was used in a process at a temperature higher than the heat-resistant temperature of the silicone adhesive layer, and deterioration of the silicone adhesive layer could be prevented.

[0063] On the other hand, in samples a14 and b13, in which no sprayed film was formed on the ceramic member, the temperature of the silicone adhesive layer could not be reduced below 200°C when the temperature of the substrate mounting surface of the electrostatic chuck was set to 250°C.

[0064] In addition, in the samples a1 to a8 and a10 to a13, the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C by adjusting the amount of heat supplied, and the temperature of the silicone adhesive layer at that time could be set to 200°C or less. In the samples a1 to a5 and a11 to a13, the ceramic member was formed of ceramics mainly composed of AlN, and Rf / Rb≧0.32 was satisfied. In the sample a9, Rf / Rb≧0.32 was satisfied, and in the sample a11, which had the same thermal resistance design as the sample a9 but had an increased amount of heat supplied, the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C, and the temperature of the silicone adhesive layer at that time could be set to 200°C or less. This shows that the electrostatic chuck, in which the ceramic member is formed of ceramics mainly composed of AlN and Rf / Rb≧0.32 is satisfied, can use the substrate holding member even in a high-temperature process of 250°C or more.

[0065] In addition, in the samples b1 to b8 and b10 to b12, the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C by adjusting the amount of heat supplied, and the temperature of the silicone adhesive layer at that time could be set to 200°C or less. In the samples b1 to b8 and b10 to b12, the ceramic member was formed of ceramics mainly composed of Al2O3, and Rf / Rb≧0.25 was satisfied. In the sample b9, Rf / Rb≧0.25 was satisfied, and in the sample b10, which had the same thermal resistance design as the sample b9 but had an increased amount of heat supplied, the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C, and the temperature of the silicone adhesive layer at that time could be set to 200°C or less. This shows that the electrostatic chuck, in which the ceramic member is formed of ceramics mainly composed of Al2O3 and Rf / Rb≧0.25 is satisfied, can use the substrate holding member even in a high-temperature process of 250°C or more.

[0066] In addition, in samples a1 to a8, a10, a12, and a13, the amount of heat supplied was 10,000 (W / m 2), the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C. In this case, in samples a1 to a8, a10, a12, and a13, the ceramic member was formed of ceramics containing AlN as the main component, and satisfied (Rf+Rb) / (Re+Rf+Rb+Rm) ≧ 0.84. This confirmed that an electrostatic chuck whose ceramic member is formed of ceramics containing AlN as the main component and satisfies (Rf+Rb) / (Re+Rf+Rb+Rm) ≧ 0.84 can reduce the amount of heat supply required to maintain a specified process temperature.

[0067] In addition, in samples b1 to b8, b11, and b12, the amount of heat supplied was 10,000 (W / m 2 ), the temperature of the substrate mounting surface of the electrostatic chuck could be set to 250°C. In this case, samples b1 to b8, b11, and b12 had ceramic members formed of ceramics containing Al2O3 as the main component, and satisfied (Rf+Rb) / (Re+Rf+Rb+Rm) ≧ 0.71. This confirmed that an electrostatic chuck whose ceramic member is formed of ceramics containing Al2O3 as the main component and satisfies (Rf+Rb) / (Re+Rf+Rb+Rm) ≧ 0.71 can reduce the amount of heat supply required to maintain a specified process temperature.

[0068] In addition, in the samples a1 to a13, the ceramic members in which the electrodes are embedded are formed of ceramics containing AlN as the main component, and satisfy 0.38 ≧ Re / Rf ≧ 0.03. It was found that such electrostatic chuck members are optimal for integration with cooling members using various types of heat-resistant adhesives.

[0069] In addition, for samples b1 to b12, the ceramic members in which the electrodes are embedded are formed of ceramics mainly composed of Al2O3, and satisfy 1.33 ≧ Re / Rf ≧ 0.13. It was found that such electrostatic chuck members are optimal for integration with cooling members using various types of heat-resistant adhesives.

[0070] From the above, it was confirmed that the substrate holding member of the present invention has a temperature of the silicone adhesive layer below its heat-resistant temperature even when used in a process in which the substrate temperature is equal to or higher than the heat-resistant temperature of the silicone adhesive layer. It was also confirmed that the manufacturing method of the present invention can manufacture such a substrate holding member. It was also found that the electrostatic chuck member of the present invention is an optimal electrostatic chuck member for integration with a cooling member using various types of heat-resistant adhesives.

[0071] The present invention is not limited to the above-described embodiment, and it goes without saying that various modifications and equivalents are included within the spirit and scope of the present invention. In addition, the structure, shape, number, position, size, etc. of the components shown in each drawing are for convenience of explanation and may be changed as appropriate. [Explanation of symbols]

[0072] 10 Substrate holding member 12 Ceramic materials 14 Thermal spray coating 16 Cooling material 18 Silicone adhesive layer 20 Flow Path 22, 24 electrodes 26 Substrate mounting surface 30 Electrostatic chuck member

Claims

1. A substrate holding member, a ceramic member formed in a flat plate shape from ceramics, having a substrate mounting surface on one main surface thereof and having an electrode embedded therein; a thermal spray coating formed on the other main surface of the ceramic member; A metal cooling member having a coolant flow path therein; a silicone adhesive layer that bonds the thermal sprayed film and the cooling member.

2. The ceramic member is formed of a ceramic mainly composed of AlN, The thermal resistance per unit area in the thickness direction of the sprayed film is Rf (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb (m 2 K / W), Rf / Rb≧0.32 2. The substrate holding member according to claim 1,

3. The ceramic member is Al 2 O 3 It is made of ceramics whose main component is The thermal resistance per unit area in the thickness direction of the sprayed film is Rf (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the silicone adhesive layer is Rb (m 2 K / W), Rf / Rb≧0.25 2. The substrate holding member according to claim 1,

4. The thermal resistance per unit area in the thickness direction of the ceramic member is Re (m 2 K / W, and the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member on the silicone adhesive layer side to the flow path of the coolant is Rm (m 2 K / W), (Rf+Rb) / (Re+Rf+Rb+Rm)≧0.84 3. The substrate holding member according to claim 2, wherein

5. The thermal resistance per unit area in the thickness direction of the ceramic member is Re (m 2 K / W, and the thermal resistance per unit area in the thickness direction in the region from the main surface of the cooling member on the silicone adhesive layer side to the flow path of the coolant is Rm (m 2 K / W), (Rf+Rb) / (Re+Rf+Rb+Rm)≧0.71 4. The substrate holding member according to claim 3, wherein:

6. An electrostatic chuck member, a ceramic member formed in a flat plate shape from a ceramic mainly composed of AlN, having a substrate mounting surface on one main surface thereof, and having an electrode embedded therein; a thermal spray coating formed on the other main surface of the ceramic member, The thermal resistance per unit area in the thickness direction of the ceramic member is Re (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the sprayed film is Rf (m 2 K / W), 0.38≧Re / Rf≧0.03 Electrostatic chuck member characterized by:

7. An electrostatic chuck member, A 2 O 3 a ceramic member formed in a flat plate shape from a ceramic material containing the above-mentioned as a main component, having a substrate mounting surface on one of its main surfaces, and having an electrode embedded therein; a thermal spray coating formed on the other main surface of the ceramic member, The thermal resistance per unit area in the thickness direction of the ceramic member is Re (m 2 K / W, and the thermal resistance per unit area in the thickness direction of the sprayed film is Rf (m 2 K / W), 1.33≧Re / Rf≧0.13 Electrostatic chuck member characterized by:

8. A method for manufacturing a substrate holding member, comprising the steps of: forming a ceramic raw material powder and firing the powder to produce a ceramic member having an electrode embedded therein; A step of preparing a plurality of metal members and forming grooves that serve as a flow path for a coolant; a step of joining the plurality of metal members having the grooves formed therein to fabricate a cooling member having the flow passage; a step of spraying a thermal spray raw material powder containing a predetermined ceramic onto a surface of the ceramic member facing the substrate mounting surface to form a thermal sprayed film; applying a silicone adhesive to at least one of the joining surfaces of the thermal sprayed film and the cooling member to bond the ceramic member and the cooling member; and curing the silicone adhesive to form a silicone adhesive layer.

Citation Information

Patent Citations

  • Wafer-mounting stage

    JP2003258065A

  • Susceptor

    JP2004079588A

  • Electrostatic chuck

    JP2007243139A

  • Heat-dissipating part and its manufacturing method

    JP2008071845A

  • Method for producing resin molding having through hole

    JP2010052011A