Production of sodium metal by a two-temperature electrolysis process.

The two-temperature electrolysis method with controlled heating and cooling in sodium ion conductive membrane cells addresses inefficiencies in sodium metal production by minimizing solvent decomposition, enhancing conductivity and extending cell life.

JP7566033B2Active Publication Date: 2024-10-11ENLIGHTEN INNOVATIONS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022552725
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-04
Filing Date
2021-03-04
Publication Date
2024-10-11
Estimated Expiration
2041-03-04

AI Technical Summary

Technical Problem

Existing methods for producing sodium metal from sodium sulfide/polysulfides are inefficient and have short cell lifetimes due to side reactions caused by temperature-sensitive solvents, leading to decomposition and reduced conductivity.

Method used

A two-temperature electrolysis method using a ceramic sodium ion conductive membrane separates anolyte and catholyte compartments, with controlled heating and cooling to minimize solvent decomposition and extend cell lifetime.

Benefits of technology

The method maintains high sodium ion conductivity and reduces solvent decomposition rates by 80% compared to single-temperature processes, extending cell life and improving throughput.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566033000001
    Figure 0007566033000001
  • Figure 0007566033000002
    Figure 0007566033000002
  • Figure 0007566033000003
    Figure 0007566033000003
Patent Text Reader

Abstract

We have discovered a new bi-temperature electrochemical method and system for producing sodium metal from sodium polysulfide. This technique provides high sodium ion conductivity and long electrochemical cell life.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 62 / 985,287, filed March 4, 2020, which is incorporated by reference in its entirety. [Background technology]

[0002] background Liquid hydrocarbons, including many petroleum feedstocks, contain sulfur, often in the form of organic sulfur compounds, which are difficult to remove, as well as metals and other heteroatom-containing compounds that prevent the use of the hydrocarbons. Sulfur can cause air pollution and can adversely affect catalysts used in petroleum processing or catalysts designed to remove hydrocarbons and nitrogen oxides from vehicle exhaust. Globally, there is a trend to limit the amount of sulfur in hydrocarbon fuels, such as fuel oils, including gasoline, diesel, and marine bunker fuels. Metals contained in hydrocarbon streams can also adversely affect hydrotreating catalysts, which are typically utilized for sulfur removal, whereby hydrogen reacts under extreme conditions to break down sulfur-containing organic sulfur molecules.

[0003] Sodium metal has been recognized as potentially useful in the treatment of high sulfur hydrocarbons, including petroleum fractions, crude oil, heavy oil, bitumen, and shale oil. Sodium can react with the oil and its contaminants to dramatically reduce the sulfur, nitrogen, oxygen, and metal content of the oil through the formation of sodium sulfide compounds (sulfides, polysulfides, and hydrosulfides) and other sodium-containing by-products. In order for such desulfurization techniques to be economically viable, sodium metal must be regenerated from sodium sulfides / polysulfides and other sodium-containing by-products. Although metallic sodium can be electrochemically regenerated from such sulfides / polysulfides and by-products, the short lifespan of the electrochemical cells used in these processes has prevented their commercial use. Thus, a cost-effective and robust electrochemical system and method for producing sodium metal from sulfides / polysulfides has not been available until now. Summary of the Invention

[0004] overview A new electrochemical method for producing sodium metal from sodium polysulfide has been discovered. The technique provides high conductivity of sodium ions and long life of the electrochemical cell. The inventors developed the technique after their extensive investigations revealed that sodium sulfide / diol anolytes are chemically unstable under the electrolysis conditions for producing sodium metal from sodium polysulfide salts. Surprisingly, the side reactions that caused the decomposition of the anolytes were found to exhibit extreme temperature dependence that had not been recognized before. The technique provides a new bi-temperature electrolysis method with high throughput and long life of the electrochemical cell. [The present invention 1001] The process is as follows: introducing an anolyte at a first temperature into an anolyte compartment of an electrochemical flow cell; the anolyte comprising an effective amount of a sodium salt dissolved in a temperature sensitive solvent; the anolyte compartment comprises an anode, the anode containing the sodium salt; The electrochemical flow cell comprises: Catholyte compartment and a ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment comprises a molten sodium cathode; The process of introducing; passing sodium ions from said sodium salt through said ceramic sodium ion conducting membrane from said anolyte compartment to said catholyte compartment; reducing the sodium ions to sodium metal at the molten sodium cathode; and cooling the anolyte outside the anolyte compartment to a second temperature. A method comprising: the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that occurs at the first temperature; method. [The present invention 1002] The process is as follows: introducing the anolyte at the second temperature into an anolyte compartment of an electrochemical flow cell; the anolyte comprising an effective amount of a sodium salt dissolved in a temperature sensitive solvent; the anolyte compartment comprises an anode, the anode containing the sodium salt; The electrochemical flow cell comprises: Catholyte compartment and a ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment comprises a molten sodium cathode; The process of introducing; passing sodium ions from the sodium salt through the ceramic sodium ion conductive membrane from the anolyte compartment to the catholyte compartment; and reducing said sodium ions to sodium metal at said molten sodium cathode. A method comprising: the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that would occur at the first temperature; method. [The present invention 1003] 13. The process of claim 1001 or 1002, wherein the sodium salt comprises, consists of, or consists essentially of sodium sulfide, sodium polysulfide, or a mixture of sodium sulfide and one or more sodium polysulfides. [The present invention 1004] The polysulfide has the formula Na 2 S x wherein x is an integer from 1 to 32. [The present invention 1005] Any of the methods of the preceding invention, wherein the amount of sodium in the anolyte ranges from about 1% to about 10% by weight. [The present invention 1006] Any of the methods of the preceding invention, wherein the amount of sodium in the anolyte ranges from about 3% to about 7% by weight. [The present invention 1007] The method of any of the preceding inventions, wherein the anolyte further comprises sulfur. [The present invention 1008] The process of claim 1007, further comprising the step of recovering said sulfur from said anolyte. [The present invention 1009] The temperature sensitive solvent is an alkyl diol, an alkyl triol, a cycloalkyl diol, a cycloalkyl triol, a lactam, a cyclic urea, a C 1~6 Any of the preceding methods of the present invention comprising, consisting of, or consisting essentially of an alkylamide, a carbonate, an ether, a mixture of any two or more thereof, or a mixture of any of the foregoing with water. [The present invention 1010] The method of any of the prior inventions, wherein the temperature sensitive solvent is selected from the group consisting of ethylene glycol, propylene glycol, butane-1,4-diol, diethylene glycol, triethylene glycol, tetraethylene glycol, glycerol, and mixtures of two or more thereof. [The present invention 1011] The method of any of the preceding inventions, wherein said temperature sensitive solvent comprises, consists of, or consists essentially of ethylene glycol. [The present invention 1012] The method of any of the preceding inventions, wherein an anode current collector in electrical contact with the anode is disposed within the anolyte compartment of the electrochemical cell. [The present invention 1013] The method of claim 1012, wherein said anode current collector comprises, consists of, or consists essentially of one or more of nickel, various carbon types, steel, kovar, or cobalt. [The present invention 1014] The method of claim 1013, wherein said anode current collector comprises, consists of, or consists essentially of nickel. [The present invention 1015] The method of any of the preceding inventions, wherein the electrochemical flow cell further comprises a cathode current collector. [The present invention 1016] The method of claim 1015, wherein said cathode current collector comprises, consists of, or consists essentially of nickel. [The present invention 1017] Any of the preceding methods of the present invention, wherein the ceramic sodium ion conductive membrane comprises, consists of, or consists essentially of a sodium ion conductive garnet-like ceramic, a Na conductive ceramic glass, NaSiCON, or Na-β″-alumina. [The present invention 1018] The method of any of the preceding inventions, wherein the first temperature is in the range of about 115°C to about 150°C. [The present invention 1019] The method of any of the preceding inventions, wherein the second temperature is in the range of 80°C to less than 115°C. [The present invention 1020] The method of any of the preceding inventions, wherein the ceramic sodium ion conductive membrane, or the ceramic sodium ion conductive membrane and the anolyte compartment, are heated to the first temperature. [The present invention 1021] The method of any of the preceding inventions, wherein the ceramic sodium ion conductive membrane, or the ceramic sodium ion conductive membrane and the anolyte compartment, are heated to the first temperature by a thermal enclosure. [The present invention 1022] The ceramic sodium ion conducting membrane has a current density of at least 10 mS cm when anolyte is present in the anolyte compartment. -1 The method of any of the preceding inventions, wherein the conductive material has a conductivity of [The present invention 1023] When anolyte is present in the anolyte compartment, the ceramic sodium ion conductive membrane has a current density of at least 50 mS cm -1 The method of any of the preceding inventions, wherein the conductive material has a conductivity of [The present invention 1024] The ceramic sodium ion conductive membrane has a conductivity of 10 mScm -1 ~100mScm -1 The method according to any one of claims 1001 to 1023, wherein the conductive material has a conductivity of 0.01 to 0.02. [The present invention 1025] 1. A system for producing sodium metal by bi-temperature electrolysis, comprising: The system further comprises: an anolyte source comprising anolyte; at least one pump for pumping the anolyte through the system; a heater for heating the anolyte to a first temperature; a chiller for cooling the anolyte to a second temperature lower than the first temperature; 1. An electrolytic flow cell comprising: an anolyte compartment and a catholyte compartment separated by a sodium ion conducting ceramic membrane; an anode comprising a sodium salt disposed within the anolyte compartment; a molten sodium cathode disposed within the catholyte compartment; and a power source electrically connected to the anode and the cathode; An electrolysis flow cell comprising: Equipped with the anolyte compartment further comprises an anolyte inlet and an anolyte outlet; and the catholyte compartment having an opening through which molten sodium can flow; Where: the anolyte source is in fluid communication with the pump and the anolyte inlet of the anolyte compartment; the heater is adapted to heat the anolyte from the anolyte source before or as the anolyte enters the anolyte compartment; and the chiller is adapted to cool the anolyte as it exits the anolyte compartment; system.

[0005] In one aspect, the present technology provides a method for preparing sodium metal from a sodium salt, such as sodium sulfide / polysulfide or sodium halide / polyhalide. The method includes introducing an anolyte at a first temperature into an anolyte compartment of an electrochemical flow cell (or hybrid flow cell). The anolyte includes an effective amount of a sodium salt (e.g., a sulfur-containing sodium salt) dissolved in a temperature-sensitive solvent. The anolyte compartment includes an anode including a sodium salt. The electrochemical flow cell further includes a catholyte compartment and a ceramic sodium ion-conducting membrane separating the anolyte compartment from the catholyte compartment. The catholyte compartment includes a molten sodium cathode. The method further includes passing sodium ions from the sodium salt from the anolyte compartment to the catholyte compartment through the ceramic sodium ion conducting membrane, reducing the sodium ions to sodium metal at a molten sodium cathode, and cooling the anolyte outside the anolyte compartment to a second temperature. In an optional embodiment, the ceramic sodium ion conducting membrane has a current density of at least 10 mS cm when the anolyte is in the anolyte compartment (i.e., at the cell operating temperature). -1 Or at least 50 mScm -1 The second temperature causes decomposition of the temperature sensitive solvent at a rate less than 20% of that which occurs at the first temperature. Thus, by simply briefly heating a portion of the anolyte as it enters the electrochemical cell and quickly cooling the anolyte as it leaves the cell, side reactions of the anolyte are minimized and cell life is greatly extended.

[0006] In any embodiment, the method further comprises oxidizing the anion of the sodium salt at the anode. In any embodiment, the sodium salt includes sodium sulfide, sodium polysulfide, and mixtures of sodium sulfide and one or more sodium polysulfides. In some such embodiments, the method further comprises oxidizing the sulfide and / or polysulfide to higher polysulfides and / or sulfur at the anode. In any embodiment of the method, the anolyte comprises sulfur, which may optionally be recovered from the anolyte. In any embodiment, at least a portion of the sodium metal formed in the catholyte compartment may be removed and / or recovered.

[0007] In another aspect, the present technology provides a system for carrying out the method. Thus, a system for producing sodium metal by bi-temperature electrolysis is provided, comprising an anolyte source containing anolyte, at least one pump for pumping the anolyte in the system, a heater for heating the anolyte to a first temperature, a chiller for cooling the anolyte to a second temperature lower than the first temperature, and an electrolysis flow cell. The electrolysis flow cell comprises an anolyte compartment and a catholyte compartment separated by a sodium ion conductive ceramic membrane, an anode containing a sodium salt disposed in the anolyte compartment, a molten sodium cathode disposed in the catholyte compartment, and a power source electrically connected to the anode and the cathode. In the electrolysis flow cell, the anolyte compartment further comprises an anolyte inlet and an anolyte outlet, and the catholyte compartment comprises an opening through which the molten sodium can flow. The anolyte source is in fluid communication with the pump and the anolyte inlet of the anolyte compartment, the heater is adapted to heat the anolyte from the anolyte source before or as it enters the anolyte compartment, and the chiller is adapted to cool the anolyte as it exits the anolyte compartment. It will be understood that the system may optionally use any of the elements described herein, including but not limited to anolyte, anodes, catholytes, cathodes, current collectors, and other equipment in, for example, FIG. 8 and the accompanying text, including equipment for sulfur and / or sodium metal recovery. [Brief description of the drawings]

[0008] [Figure 1A] FIG. 1 is a schematic diagram of an exemplary embodiment of an electrochemical cell that may be used in the present methods and systems. [Figure 1B] FIG. 1 is a schematic diagram of an exemplary embodiment of an electrochemical cell that may be used in the present methods and systems. [Figure 1C]FIG. 1 illustrates an exemplary embodiment of a series electrochemical cell arranged to oxidize sodium sulfide to sodium polysulfide and ultimately to elemental sulfur while also removing sodium metal from the anolyte. [Diagram 2] 1 is a graph showing the conductivity of Na2S5 anolyte as a function of wt% Na and temperature. [Diagram 3] FIG. 1 shows FT-IR spectra of Na2S5 with 7% sodium dissolved in EG and incubated at different temperatures for 195 hours. [Figure 4] FT-IR peak heights normalized to the baseline for the peak at 1725 cm −1 wavenumber characteristic of 2-hydroxyethyl acetate are shown. [Diagram 5] FT-IR peak heights normalized to the baseline are shown for the peak at 3250 cm −1 wavenumber, which is the OH stretch from ethylene glycol. [Figure 6] 1 is a graph showing the observed mass loss of 3% and 7% sodium Na2S5 anolyte at 110° C., 125° C., and 150° C. during thermal incubation. [Figure 7] 1 is a graph showing the observed mass loss of an anolyte having Na2S5 in 5 wt% ethylene glycol anolyte at temperatures ranging from 80° C. to 150° C. [Figure 8] FIG. 1 shows a process flow diagram (PFD) of an exemplary embodiment of a system for performing an instant dual stage anolyte temperature electrolysis process. [Figure 9] 1 shows the applied voltage (right y-axis) required to achieve 57 mA / cm2 over time using an exemplary embodiment of the electrochemical cell and bi-temperature electrolysis method of the present technology. [Figure 10] As discussed in Example 1, voltage and current density over time are shown for high temperature operation (125-150° C.) of an exemplary embodiment of the present technology. [Figure 11]The normalized FT-IR peak height relative to the baseline for the peak at 1580 cm −1 wavenumber is shown. [Figure 12] The normalized FT-IR peak height relative to the baseline for the peak at 1725 cm −1 wavenumber is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Detailed Description The following terms are used throughout as defined below.

[0010] As used herein and in the appended claims, singular articles such as "a," "an," and "the" and similar referents in the context of describing an element (particularly in the context of the appended claims) should be construed to cover both the singular and the plural, unless otherwise stated herein or clearly contradicted by context. Recitations of ranges of values ​​herein are merely intended to serve as a shorthand method of individually referring to each individual value falling within the range, unless otherwise stated herein, and each individual value is incorporated herein as if it were individually recited herein. All methods described herein may be performed in any suitable order, unless otherwise stated herein or clearly contradicted by context. The use of any and all examples or exemplary language (e.g., "etc.") provided herein is intended merely to better illustrate the embodiments and does not pose limitations on the scope of the claims, unless otherwise stated. No language in this specification should be construed as indicating any non-claimed element as essential.

[0011] As used herein, "about" will be understood by those of ordinary skill in the art and will vary to some extent depending on the context in which it is used. If there are uses of the term that are not clear to persons of ordinary skill in the art, given the context in which it is used, "about" will mean up to plus or minus 10% of the particular term.

[0012] "Ceramic sodium ion conducting ceramic membrane" refers to any suitable ceramic membrane that prevents the molten sodium cathode from contacting the anode and anolyte, but allows sodium ions to be selectively transported from the anode / anolyte through the membrane to the cathode.

[0013] An "alkyl diol" or "alkane diol" refers to an alkene of 2 to 6 carbons (i.e., 2, 3, 4, 5, or 6 carbon atoms) or an alkylene ether of 4 to 8 carbons (i.e., 4, 5, 6, 7, or 8 carbon atoms) having two hydroxyl groups attached to different carbons. It is understood that an alkane is a saturated straight-chain or branched hydrocarbon. Similarly, an "alkyl triol" or "alkane triol" refers to an alkane of 3 to 6 carbons (i.e., 2, 3, 4, 5, or 6 carbon atoms) or an alkylene ether of 4 to 8 carbons (i.e., 4, 5, 6, 7, or 8 carbon atoms) having three hydroxyl groups attached to three different carbons. Examples of alkane diols and triols include, but are not limited to, ethylene glycol (i.e., ethane-1,2-diol), propylene diols (e.g., propane-1,2-diol, propane-1,3-diol), glycerol, butane diols (e.g., butane-1,2-diol, butane-1,3-diol, butane-2,3-diol, butane-1,4-diol, 2-methylpropane-1,3-diol, etc.), butane triols (e.g., butane-1,2,3-triol, butane-1,2,4-triol, 2-hydroxymethylpropane-1,3-diol, etc.), pentane diols (e.g., pentane-1,2-diol, pentane-1,3-diol, etc.), propylene diols (e.g., propane-1,2-diol, propane-1,3-diol, etc.), butane triols (e.g., butane-1,2,3-triol, butane-1,2,4-triol, 2-hydroxymethylpropane-1,3-diol, etc.), pentane diols (e.g., pentane-1,2-diol, pentane-1,3-diol, etc.), propylene ... ,3-diol, pentane-2,3-diol, pentane-1,4-diol, pentane-1,5-diol, 2-methylbutane-1,4-diol, etc.), pentanetriol (e.g., pentane-1,2,5-triol, pentane-1,3,5-triol, 2-hydroxymethylbutane-1,4-diol, etc.), hexanediol (e.g., hexane, 1,2-diol, hexane-1,6-diol, hexane-1,3-diol, hexane-2,3-diol, hexane-3,4-diol, etc.), hexanetriol (e.g., hexane-1,2,3-triol, hexane-1,2,6-triol, hexane-1,3,6-triol, etc.). Examples of alkylene diols and triols.

[0014] "Cycloalkyldiol" or "cycloalkanediol" refers to a cycloalkane of 3, 4, 5, or 6 carbons with two hydroxyl groups attached to different carbons. "Cycloalkyltriol" or "cycloalkanetriol" refers to a cycloalkane of 3, 4, 5, or 6 carbons with three hydroxyl groups attached to different carbons. Examples include cyclopropane-1,2-diol, cyclobutane-1,3-diol, cyclopentanes-1,2-diol, cyclohexane-1,2-diol, cyclohexane-1,3-diol, cyclohexane-1,4-diol, and the like.

[0015] As used herein, a "temperature sensitive solvent" refers to a solvent utilized in an electrolyte of an electrochemical cell to dissolve or partially dissolve one or more species (e.g., a salt or a neutral, uncharged compound) that becomes increasingly unstable as temperature increases and undergoes decomposition and / or other side reactions that adversely affect the performance of the electrolyte.

[0016] High sodium ion conductivity is desired to ensure high throughput in the electrolytic production of sodium metal from sodium salts such as sodium polysulfide. To achieve the desired conductivity with a particular combination of sodium sulfide and polysulfide salts, a balance must be struck between the selected anolyte, anode, and ceramic ion-conducting membrane, which are part of the electrochemical cell. The inventors have found that low molecular weight diols and triols (e.g., having a molecular weight of less than 400 Da, such as about 62 Da to less than about 200 Da) provide good solubility for sodium sulfide / polysulfide and lower solubility of elemental sulfur while maintaining maximum sodium ion conductivity of the cell. However, it has been found that the performance of such cells degrades within a few days, making the cells unsuitable for long-term commercial use.

[0017] Sodium polysulfide (Na2S xAt least the following side reactions of diols / triols such as ethylene glycol (EG) and / or ethylene glycol (EG) have been identified: 1.EG acts as an acid and Na2S x acts as a base, producing hydrogen sulfide gas. 2.Na2S x Abstraction of oxygen from glycol by acetone to form sodium sulfur oxygenates (sodium thiosulfate, sodium sulfate, etc.). 3.Na2S x The methylene group is abstracted from EG by S from the olefin to form vulcanized or inverse vulcanized oligomers of sulfur and methylene groups. 4. Electrochemical oxidation of EG in alkaline medium to form sodium carboxylates (sodium acetate, sodium glycolate, sodium formate, sodium oxalate, etc.). 5. Formation of gases such as dimethyl disulfide, carbon disulfide, and carbon dioxide.

[0018] Observations 1, 2, and 3 are consistent with the following side reactions shown below. Na2S.Sx+2(CH2OH-CH2OH)---->2H2S+Na2SO4+(CH2)2Sy

[0019] Observations 4 and 5 are consistent with the following side reactions shown below. Na2S.S x +2(CH2OH-CH2OH)------>(COONa)2+(CH3)2S x

[0020] Thus, it has been surprisingly found that the use of ethylene glycol results in an undesirable increase in the area specific resistance (ASR) of the electrolytic cell, causing the current to drop within a few days.

[0021] Thermal and electrolysis tests as a function of anolyte temperature showed a sudden drop in decomposition reaction rate and a shift in equilibrium to the left (favoring the reactants in the decomposition reaction) as the process temperature was decreased from above 125° C. to lower temperatures. Indeed, the decomposition rate dropped dramatically when the anolyte temperature was below 110° C., and especially when the anolyte temperature was below 100° C. See, for example, Figures 3-7, each of which shows electrolyte decomposition at the high end of this spectrum, i.e., temperatures favorable for superior conductivity and current density.

[0022] The above reactions become prominent at temperatures above 120° C., particularly at temperatures above 125° C. Nevertheless, considering that such temperatures are desirable to provide high sodium ion conductivity of the membrane during electrolysis, the present technology provides methods and systems that minimize anolyte decomposition at operating temperatures, for example, between 125° C. and 150° C., while maintaining high sodium ion conductivity.

[0023] Thus, in one aspect, the present technology comprises the steps of: introducing an anolyte at a first temperature into an anolyte compartment of an electrochemical flow cell; the anolyte comprising an effective amount of a sodium salt dissolved in a temperature sensitive solvent; the anolyte compartment comprises an anode containing a sodium salt; An electrochemical flow cell, Catholyte compartment and A ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment containing a molten sodium cathode; The process of introducing; passing sodium ions from the sodium salt through the ceramic sodium ion conducting membrane from the anolyte compartment to the catholyte compartment; reducing sodium ions to sodium metal at a molten sodium cathode; and cooling the anolyte outside the anolyte compartment to a second temperature. A method comprising: the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that occurs at the first temperature; A method is provided.

[0024] In another aspect, the present technology comprises the steps of: introducing the anolyte at the second temperature into an anolyte compartment of an electrochemical flow cell; the anolyte comprising an effective amount of a sodium salt dissolved in a temperature sensitive solvent; the anolyte compartment comprises an anode containing a sodium salt; An electrochemical flow cell, Catholyte compartment and A ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment containing a molten sodium cathode; The process of introducing; passing sodium ions from the sodium salt through the ceramic sodium ion conducting membrane from the anolyte compartment to the catholyte compartment; and Reducing sodium ions to sodium metal at a molten sodium cathode. A method comprising: the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that would occur at the first temperature; A method is provided.

[0025] In any embodiment, the sodium salts may include sodium sulfide, sodium polysulfide, a mixture of sodium sulfide and one or more sodium polysulfides, a sodium halide, a sodium polyhalide, or a mixture of sodium halide and one or more sodium polyhalides. In any embodiment, the sodium salts may include sodium sulfide, sodium polysulfide, a mixture of sodium sulfide and one or more sodium polysulfides. In any embodiment, the polysulfides have the formula Na2S x where x is an integer between 1 and 32, i.e., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, or a range inclusive between any two of the preceding values ​​(e.g., 1-7 or 1-5). However, it will be understood by those skilled in the art that in some embodiments, the measured x value will reflect the amount of sulfur in the mixture. It will also be understood that the sodium salt in the anolyte includes an anion, and that the method also includes a step of oxidizing the anion at the anode. For example, if the anolyte comprises sodium sulfide and / or sodium polysulfide, the method may include oxidizing the sulfide and polysulfide anions to higher polysulfides and / or sulfur, such that the anolyte comprises sulfur. In any embodiment of the method, the sulfur may be recovered from the anolyte, for example, by phase separating the sulfur as a solid and / or an immiscible liquid, and removing or otherwise recovering the sulfur from the anolyte. Phase separation and recovery may be accomplished by standard means, such as cooling and precipitating or crystallizing the sulfur, or cooling and settling the liquid sulfur, so that the sulfur may be removed from the remainder of the anolyte.

[0026] In any embodiment herein, the amount of sodium in the anolyte can be in the range of about 1% to about 10% by weight, such as about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 9%, about 10%, or a range inclusive of any two of the preceding values. For example, the amount of sodium in the anolyte can be in the range of about 3% to about 7% by weight.

[0027] In any embodiment herein, the temperature sensitive solvent of the present technology may include an alkyl diol, an alkyl triol, a cycloalkyl diol, and / or a cycloalkyl triol. For example, the temperature sensitive solvent may be selected from the group consisting of ethylene glycol, propylene glycol, butane-1,4-diol, diethylene glycol, triethylene glycol, tetraethylene glycol, and glycerol. In any embodiment, the temperature sensitive solvent may be a lactam (e.g., N-methyl-2-pyrrolidone, (NMP)), a cyclic urea (e.g., N,N'-dimethylpropylene urea, DMPU), a C 1~6 Examples of suitable solvents include alkylamides (e.g., formamide, N,N-dimethylformamide, acetamide), carbonates (e.g., dimethyl carbonate, diethyl carbonate), ethers (e.g., dimethyl ether, dioxane), or mixtures of any of the foregoing with water. In any embodiment, the temperature sensitive solvent may comprise a mixture of two or more of the foregoing solvents (or classes of solvents). Thus, for example, the anolyte may comprise a mixture of two solvents in a weight ratio of 1:99 to 99:1, 5:95 to 95:5, or more typically, 50:50 to 95:5, e.g., 50:50, 55:45, 60:40, 70:30, 80:20, 90:10, 95:5, or a range inclusive of any two of the foregoing ratios. In any embodiment, any compatible temperature sensitive solvent pair may be used, examples include ethylene glycol and NMP, ethylene glycol and water, tetraethylene glycol and dimethyl ether, ethylene glycol and glycerol.

[0028] In any embodiment herein, the anolyte optionally includes one or more sodium salts as sodium ion conductivity enhancers. The presence of these sodium salts in the anolyte along with sodium polysulfide increases the conductivity and current density of the electrolytic flow cell. The sodium ion conductivity enhancers of the present technology include sodium salts selected to be substantially (preferably completely) soluble, ionizable, and thermally stable at the concentrations used in the temperature sensitive solvent at both the first and second temperatures used in the method. Non-limiting examples of sodium ion conductivity enhancers include sodium halides (e.g., NaCl, NaBr, and NaI), sodium hydroxide, sodium carbonate, sodium sulfur oxides (Na2SO4, Na2SO3, Na2S2O3), sodium hydrosulfide (NaSH), and mixtures of any two or more thereof. In any embodiment, the anolyte may include sodium halides, sodium hydroxide, or mixtures of any two or more thereof. In any embodiment, 0.01% to 20% by weight of the sodium conductivity enhancer may be present in the anolyte. For example, the anolyte may include 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 16 wt%, 18 wt%, and 20 wt% of the sodium ion conductivity enhancer, or a range between any two of the preceding values ​​inclusive. Thus, for example, the anolyte may optionally include 0.1 wt% to 20 wt%, 1 wt% to 18 wt%, or 5 wt% to 15 wt% of the sodium ion conductivity enhancer. An improvement in conductivity of at least 10% to 100% may be obtained with an anolyte including such enhancers, as compared to the same anolyte without such enhancers present. In some embodiments, the improvement is at least 10%, at least 20%, at least 40%, at least 60%, at least 80%, at least 100%, or a range inclusive of any two of the preceding values.

[0029] In the present technology, the molten sodium cathode comprises sodium, and optionally is a sodium alloy. In any embodiment, the sodium of the molten sodium cathode may contain a small amount of extraneous impurities, but may still be substantially pure (e.g., at least 99% sodium, at least 99.5% sodium, or at least 99.9% sodium). It will be understood by those skilled in the art that a suitable sodium alloy is composed primarily of sodium metal. In any embodiment, the sodium alloy is at least 80% sodium metal by weight, such as at least 80% by weight, at least 85% by weight, at least 90% by weight, at least 95% by weight, at least 96% by weight, at least 97% by weight, at least 98% by weight, at least 99% by weight, or a range inclusive of any two of the preceding values. For example, in any embodiment, the sodium alloy may be 80% to 99% sodium metal by weight. The alloy of the alkali metal may include, for example, an alloy with one or more of Si, Ge, Sn, Pb, Hg, Cs, Sb, Bi, Zn, Al, Ti, Co, Ni, Mn, and Cd. In any embodiment, the liquid alkali metal may be a sodium alloy including Cs. The amount of non-sodium metal in the alloy may comprise, for example, 1-20% by weight of the total sodium alloy. Thus, the non-sodium metal may be 1%, 2%, 3%, 4%, 5%, 6%, 8%, 10%, 15%, 20% by weight, or any two of the preceding values ​​inclusive.

[0030] In any embodiment of the methods and systems herein, an anode current collector in electrical contact with the anode is disposed within the anolyte compartment of the electrochemical cell. In any such embodiment, the anode current collector may be or include one or more of nickel (e.g., foam or mesh), various carbon types (e.g., carbon foam, carbon felt), steel, kovar, or cobalt. In any embodiment, the anode current collector may include nickel.

[0031] In any embodiment, the electrochemical flow cell may further include a cathode current collector, which may comprise nickel or other suitable materials known in the art.

[0032] In any embodiment, the ceramic sodium ion conducting membrane can be a sodium superionic conductor, a sodium ion conducting garnet-like ceramic, a sodium β″-alumina, or a sodium conducting glass-ceramic. For example, when the negative electrode active material includes sodium, the alkali ion conducting membrane can include any suitable type of NaSICON membrane, a sodium ion conducting garnet-like ceramic, a Na-β″-alumina, or a sodium ion conducting glass-ceramic membrane. NaSICON compositions include, but are not limited to, Na3Zr2Si2PO 12 , Na 1+x S x Zr2P 3-x O 12 (wherein x=1.6 to 2.4), yttrium-doped NaSICON (e.g., Na 1+x+y Zr 2-y Y y S x P 3-x O 12 , Na 1+x Zr 2-y Y y , Si x P 3-x O 12-y , where x=1.6-2.4, y=0-0.25), Na 1+x Zr2X y (PO4)3, where x is 0-3, y is 0-1.5, and X is a dopant (e.g., Fe, Al, Ti, Hf, Co, Ni, Nb), and Fe-doped NaSICON (Na3Zr 2 / 3 Fe 4 / 3 P3O 12 A non-limiting example of a Na-β″-alumina membrane is Na (1.53-1.73) Li (0.28-0.32) Al (10.66-10.72) O 17 In any embodiment, the sodium ion conducting ceramic membrane has a x B2C3O 12A sodium ion conducting garnet-like ceramic having the general formula: 6+ , Ta 5+ , Nb 5+ , Zr 4+ , C=La 3+ , Y 3+ , Nd 3+ Non-limiting examples of Na-conducting ceramic glasses include sodium phosphates such as xNa2O.yP2O5, sodium silicates such as xNa2O.ySiO2, sodium borates such as xNa2O.yB2O3, sodium aluminates such as xNa2O.yAl2O3, and mixtures of any two or more thereof, in any of the above where the molar ratio of x:y can be in the range of 1:3 to 3:1, 1:2 to 3:1, 1:2 to 2:1, 1:2 to 1:1, 1:3 to 2:1, or 1:3 to 1:1.

[0033] In any embodiment, the ceramic sodium ion conducting membrane is a NaSiCON or Na-β″-alumina membrane. In any embodiment, the ceramic sodium ion conducting membrane has a conductivity of at least 10 mS cm -1 Or at least 50 mScm -1 Conductivity of, for example, 10 mScm -1 ~100mScm -1 For example, a ceramic sodium ion conducting membrane can have a conductivity of 10 cm -1 , 20cm -1 , 30cm -1 , 40cm -1 , 50mScm -1 , 60mScm -1 , 70mScm -1 , 80mScm -1 , 90mScm -1 , 100mScm -1 , or a range between any two of the aforementioned values, inclusive.

[0034] As disclosed herein, the bi-temperature method of the present technology reduces or avoids the decomposition of temperature-sensitive solvents used as electrolytes, e.g., anolytes in electrolytic flow cells to maintain high throughput and extend lifetime. Temperature control in the present method can be implemented in several ways. In any embodiment, the anolyte can be heated to a first temperature just before or as it enters the anolyte compartment, and cooled to a second temperature just after or shortly after it leaves the anolyte compartment. In any embodiment, the ceramic sodium ion conducting membrane, or the ceramic sodium ion conducting membrane and the anolyte compartment, are heated to a first temperature, e.g., by a thermal enclosure surrounding the anolyte compartment, or by a heat exchange element in the anolyte compartment. Thus, the anolyte can be heated to a first temperature by the anolyte compartment, or can be heated in whole or in part before entering the heated anolyte compartment.

[0035] In any embodiment, the first temperature can be in the range of about 115° C. to about 150° C., such as about 115° C., about 120° C., about 125° C., 130° C., 135° C., 140° C., 145° C., 150° C., or a range inclusive of any two of the preceding values. Thus, in any embodiment, the first temperature can be in the range of about 120° C. to about 150° C., or about 125° C. to about 150° C. or about 145° C.

[0036] In any embodiment, the second temperature can be in the range of about 80° C. to less than 115° C., such as about 80° C., about 85° C., about 90° C., about 95° C., about 110° C., less than 115° C., or a range inclusive of any two of the preceding values. Thus, in any embodiment, the second temperature can be in the range of about 80° C. or about 85° C. to about 110° C.

[0037] Given the guidance provided herein, it is within the skill of one in the art to select a first temperature to provide the desired conductivity and throughput, and to select a second temperature to limit the decomposition of the temperature-sensitive solvent in the anolyte to provide a long life at the desired throughput, while minimizing the energy consumption for heating / cooling the anolyte. Thus, in some embodiments, the second temperature will be selected to cause the decomposition of the temperature-sensitive solvent at a rate of less than 20% of the rate that occurs at the first temperature, although a second temperature to limit the decomposition to other rates can be readily selected by one of skill in the art. Thus, in some embodiments, the second temperature is selected to result in less than 25%, less than 20%, less than 15%, less than 10%, less than 5%, less than 4%, less than 3%, 2%, or 1% of the decomposition rate that occurs at the first temperature. In any embodiment, the.

[0038] Thus, in any embodiment, the method herein comprises the steps of: introducing an anolyte at a first temperature into an anolyte compartment of an electrochemical flow cell; the anolyte compartment comprises an anode containing a sodium salt; the anolyte comprising an effective amount of a sodium salt dissolved in a temperature sensitive solvent; An electrochemical flow cell, Catholyte compartment and A ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment containing a molten sodium cathode; The process of introducing; passing sodium ions from the sodium salt through the sodium ion conductive membrane from the anolyte compartment to the catholyte compartment; reducing sodium ions to sodium metal at a molten sodium cathode; and cooling the anolyte outside the anolyte compartment to a second temperature. Including, Ceramic sodium ion conducting membranes have a resistance of at least 50 mScm -1 and the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that occurs at the first temperature; the sodium salt is selected from the group consisting of sodium sulfide, sodium polysulfide, a combination of sodium sulfide and one or more sodium polysulfides, a sodium halide, a sodium polyhalide, and a combination of sodium halide and one or more sodium polyhalides; and The temperature sensitive solvent includes an alkyl diol and / or a cycloalkyl diol.

[0039] In some such embodiments, the sodium salt is selected from the group consisting of sodium sulfide, sodium polysulfide, or a combination of sodium sulfide and one or more sodium polysulfides.

[0040] The method may use a variety of electrochemical cell configurations. An exemplary embodiment of one such cell configuration is shown generally in FIG. 1A. The cell 100 includes a molten sodium cathode 110 (which may be sodium or a sodium alloy) disposed within a catholyte compartment 115. The cell also includes an anode 120 (i.e., a sodium salt) disposed within an anolyte compartment 125. A ceramic sodium ion conducting membrane 130 (e.g., NaSICON, Na-β″-alumina, sodium ion conducting garnet-like ceramic, sodium conducting glass ceramic, etc.) separates the catholyte and anolyte compartments and their contents. The membrane 130 may be secured to the cell housing with O-rings 140A and 140B. The cell may include cathode and anode current collectors 150A and 150B in electrical contact with the cathode and anode, respectively. During cell operation, anolyte may be circulated into and out of the anolyte compartment. Not shown is any external chamber fluidly connected to the catholyte compartment into which excess molten sodium may flow during sodium metal regeneration. It will be appreciated that the electrochemical cells of the present technology may be configured with sensors, controllers, monitors, regulators, flow meters, access ports, and alert mechanisms to allow concentrations and ratios of components such as sodium, elemental sulfur, temperature sensitive solvents, oxidation states, open cell voltages, and the like to be monitored, measured, and maintained.

[0041] Alternatively, FIG. 1B shows a schematic cross-sectional view of another exemplary embodiment of an electrolysis cell of the present technology. The cell is composed of a housing 310, which is typically an electrical insulator and chemically resistant to solvents and sodium sulfide. A ceramic sodium ion conducting membrane 312, in this case in the form of a tube, separates a catholyte compartment 314 from an anolyte compartment 316. Within the catholyte compartment is a cathode (molten sodium or sodium alloy) and a cathode current collector. The cathode current collector 324 can be configured to pass through the housing 310 or to have a lead 325 that passes through the housing 310 so that a connection can be made to the negative terminal of a DC power source (not shown). Within the anolyte compartment 316 is an anode current collector 326, which in this case is shown as a porous mesh-type electrode in the form of a cylinder surrounding the membrane tube 312. A lead 328 passes through the housing so that a connection can be made to the positive terminal of the DC power source. The anolyte solution flows through the anolyte inlet 330. The anolyte includes an anode (i.e., sodium salt) as described herein. As the anolyte flows through the inlet 330, the anolyte also flows out of the outlet 332. In some cases, a second liquid phase of molten sulfur may also exit with the anolyte. An optional second outlet from the anolyte compartment may be provided at a lower location than the anolyte outlet 332. The second lower outlet may be used well for removal of molten sulfur that has settled and accumulated at the bottom of the cell. The space between the cathode 324 and the membrane 312 is generally filled with molten alkali metal. When the cell is operated, alkali metal ions pass through the membrane 312 and are reduced at the cathode 324 to form alkali metal in the cathode compartment 314, resulting in a flow of alkali metal through the cathode outlet 334.

[0042] A cell may have multiple anodes, anode current collectors, cathodes, cathode current collectors, and membranes. In a cell, the anodes / current collectors will all be in parallel and the cathodes / current collectors will all be in parallel.

[0043] 1B, the electrolysis cell housing 310 can be an electrically insulating material such as most polymers. This material is also preferably chemically resistant to solvents. Polytetrafluoroethylene (PTFE) is particularly suitable, as is Kynar® polyvinylidene fluoride, or high density polyethylene (HDPE). The cell housing 310 may be made from a non-insulating and non-chemically resistant material, provided that the interior of the housing 310 is lined with such an insulating and chemically resistant material. Other suitable materials would be inorganic materials such as alumina, silica, aluminosilicates, and other insulating refractory or ceramic materials.

[0044] The ceramic sodium ion conducting membrane 312 is preferably substantially permeable only to sodium and substantially impermeable to anions, polyanions, and dissolved sulfur. The membrane 312 may be partially fabricated from an alkali metal ion conducting material. When the metal recovered by the cell is sodium, a useful material for the divider is NaSICON, which has relatively high ionic conductivity. Exemplary NaSICON compositions may be as disclosed herein. The membrane 312 may have a portion of its thickness with negligible through porosity such that liquids in the anolyte compartment 316 and catholyte compartment 314 cannot pass from one compartment to the other, but substantially only sodium ions can pass from the anolyte compartment 316 to the catholyte compartment 314. The membrane may also be partially constructed of an alkali metal (i.e., sodium) ion conducting glass ceramic, such as the material manufactured by Ohara Glass of Japan.

[0045] An anode current collector 326 is located within the anolyte compartment 316. The anode current collector 326 may be made of a conductive material such as stainless steel, nickel, iron, iron alloys, nickel alloys, and other anode materials known in the art. The anode 326 is connected to the positive terminal of a DC power source. The anode 326 may be a mesh, foam, monolithic structure, or may be monolithic with features that allow the anolyte (including sodium salt anodes) to pass through the anode structure. The anolyte solution is fed into the anolyte compartment through an inlet 330, passes through the compartment, and exits through an outlet 332. The electrolysis cell 300 may also be operated in a semi-continuous mode where the anolyte compartment is fed and partially drained through the same passageway.

[0046] The electronically conductive cathode current collector 324 may be in the form of a strip, band, rod, or mesh. The cathode current collector 324 may be composed of most electronic conductors such as nickel, steel, iron, copper, or graphite. A portion of the cathode current collector may be disposed within the catholyte compartment 314 and a portion may be disposed outside the catholyte compartment 314 and cell housing 310 for electrical contact. Alternatively, a lead 325 may extend from the cathode current collector outside the cell housing 310 for electrical contact. Within the catholyte compartment 314 is a bath of molten sodium.

[0047] One non-limiting example of the operation of the electrolysis cell 300 is described below, in which an anolyte solution is provided to the anolyte compartment 316. The electrode current collectors 324, 326 are connected to a Na2S solution having a potential ranging between about 1.8 V and about 2.5 V, depending on the composition, between the anode current collector 326 and the cathode current collector 324. xThe anolyte is connected to a voltage source such that there is a potential greater than the dissociation voltage of the anolyte. For example, the dissociation voltage can be 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5 V, or a range inclusive between any two of the preceding values. At the same time, sodium ions pass through the membrane 312 into the catholyte compartment 314, where they are reduced to the metallic state with electrons supplied through the cathode current collector 324, and sulfides and polysulfides are oxidized at the anode current collector 326, resulting in lower polysulfide anions becoming higher polysulfide anions and / or elemental sulfur forms. While sulfur is being formed, it is dissolved in whole or in part in the anolyte solvent. Upon sulfur saturation or cooling, sulfur may form its second liquid phase and settle to the bottom of the anolyte compartment 316 of the electrolytic cell. The sulfur may be removed with the anolyte solution and settle in a vessel outside the cell, or, as shown, may be removed directly from the settling zone 336 via optional sulfur outlet 338. Alternatively, cell 300 may be part of an electrochemical system that removes sulfur from the anode in other ways, and sulfur outlet 338 is not present.

[0048] The cells of the present technology can be arranged in series, i.e., the anolyte of one electrolytic cell can flow into a second cell, with the ratio of sodium to sulfide decreasing in each successive cell as the polysulfide form becomes more highly concentrated. Such an embodiment is shown in FIG. 1C.

[0049] The methods disclosed herein may be implemented in various types of electrochemical systems. The process flow diagram (PFD) shown in FIG. 8 as an exemplary embodiment only illustrates one possible system 200 for implementing the bi-temperature anolyte process of the present technology. Solids 205 from the desulfurization process, including sodium sulfide, sodium heavy metal salts, and other sodium-containing salts, are added to an anolyte tank 210 containing a temperature sensitive anolyte solvent, for example, an alkyl diol as described herein, such as, but not limited to, ethylene glycol or propylene glycol. Anolyte 212 is pumped from the anolyte tank 210 via a fluid driver 215 (e.g., a pump) to a splitter 220 where a portion 225 is then directed to an anolyte filter 230, which filters out any undissolved solids. The filtered anolyte 232 is then conducted to a heat exchanger 235 where the filtered anolyte 232 is heated to a temperature above 120° C., e.g., about 125° C. to about 150° C., as described herein. A heated fluid is conducted into (236A) and out of (236B) the heat exchanger to maintain the appropriate temperature. The heated anolyte 234 is conducted to an anolyte compartment of an electrochemical cell or series of cells 240 (see, e.g., FIGS. 1A-1C) where sodium metal 245 is regenerated from the sodium salts and removed from the cell. Upon exiting the electrochemical cell, the spent anolyte 242 is cooled in a second heat exchanger 250 to a temperature below 110° C., e.g., about 80 to about 100° C., as described herein. The cooled anolyte 255 , which may contain some dissolved elemental sulfur, is recycled to the anolyte tank 210 .

[0050] At splitter 220, a portion 260 of the anolyte leaving the anolyte tank is sent to a crystallizer 265 where the anolyte is cooled to a temperature of about 15° C.-80° C. by a cooling fluid circulating into (266A) and out of (266B) the crystallizer. Other suitable temperatures in this range may be used, including, for example, 15° C.-60° C., 30° C.-80° C., or 40° C.-80° C. The sulfur 277 precipitates, such as as crystals, and the crystals are then filtered out as the anolyte 270 passes through sulfur filter 275. The lower temperature in this part of the system and process not only reduces the solubility of sulfur in the anolyte, resulting in the precipitation / crystallization of sulfur (S8), but also reduces the solubility of Na2S x to destabilize the sulfur to promote the formation and precipitation / crystallization of S8. The desulfurized anolyte 280 is then recycled back to the anolyte tank 210. It will be understood by those skilled in the art that other methods of removing dissolved sulfur from the anolyte 260 may be used, such as gravimetric methods (e.g., centrifugation). Alternatively, a different anolyte solvent system with lower sulfur solubility may be used at a temperature above the melting point of sulfur so that elemental sulfur may be removed as a liquid. Still other sulfur removal techniques may be used, such as extraction with a non-polar solvent immiscible with the anolyte. It is within the purview of one skilled in the art to modify the present system and process to use any suitable sulfur removal technique, and to make other minor changes, such as including additional fluid drivers (e.g., pumps), filters, heat exchangers, etc. as needed, and arranging such components to serve the needs at hand. EXAMPLES

[0051] material Ethylene glycol was obtained from Univar.

[0052] Example 1 - Electrochemical cell with NaSICON ceramic membrane for producing sodium metal from sodium polysulfide A hybrid electrochemical flow cell was constructed for use in the disclosed method. The flow cell has an anolyte compartment, a catholyte compartment, and a 4.5 mm thick NaSICON ceramic membrane separating the anolyte compartment from the catholyte compartment. The anolyte compartment includes a nickel anode current collector disposed therein, as well as an anolyte inlet and an anolyte outlet. The catholyte compartment includes a molten sodium cathode and a nickel cathode current collector. A power source (Ametek Sorensen XHR Series Programmable, 7.5V, 130A) was electrically connected to the current collectors in each compartment. During operation of the cell, anolyte, which includes ethylene glycol with dissolved Na2S and sulfur, flowed into the anolyte compartment through the inlet. The anolyte was heated (e.g., in a heat exchanger as shown in FIG. 8) to a temperature of 115° C. (or 125° C.) to 150° C. immediately prior to entering the cell, and entered the anolyte compartment at this temperature. The sulfides / polysulfides are partially or fully oxidized to form higher polysulfides and elemental sulfur, which at least partially dissolve in the ethylene glycol of the anolyte. Sodium ions from the oxidized sulfides / polysulfides are transported across the NaSICON membrane to the catholyte compartment where the molten sodium cathode and nickel current collector are located. The sodium ions are reduced to sodium metal at the cathode and excess sodium flows through an outlet of the catholyte compartment. The "spent" anolyte containing the higher polysulfides and elemental sulfur exits the compartment through the anolyte outlet. A portion of the anolyte is sent to a crystallizer where it is further cooled to precipitate / crystallize the elemental sulfur, the precipitated / crystallized elemental sulfur is filtered from the anolyte, and the anolyte is then returned to the storage tank. A portion of the spent anolyte is returned to the storage tank where additional sodium sulfide / polysulfide is dissolved in the anolyte, and the anolyte is then circulated back to the electrochemical cell to produce more sodium, higher polysulfides, and elemental sulfur.FIG. 9 shows the current draw of 57 mA / cm over time for this cell in a dual temperature system of the present technology operated at low temperature (110° C.), dual temperatures (100° C. and 125° C.), and 125° C. 2 Figure 10 shows the applied voltage and current density for cell inlet temperatures from 125°C to 150°C. After over 350 hours of exposure to high temperatures (>125°C), the cell performance was 57 mA / cm 2 and back to the baseline conditions of 3.08 V, demonstrating that the two-temperature system prevents anolyte decomposition over the entire temperature range.

[0053] Example 2 - XRD analysis of spent anolyte The electrochemical cell of Example 1 was operated at an anolyte temperature of about 130° C. The spent anolyte was recovered, the ethylene glycol was vacuum distilled, and the remaining solid was dried and examined by X-ray powder diffraction (XRD). Oxygenated sodium sulfur (sodium thiosulfate, sodium sulfate, etc.) is Na2S x In addition, sodium carboxylates (sodium acetate, sodium glycolate, sodium formate, sodium oxalate, etc.) were identified as being due to the electrochemical oxidation of EG in alkaline medium.

[0054] Example 3 - Effect of temperature on anolytes containing Na2S5 The effect of temperature on an anolyte containing the model polysulfide Na2S5 in the model anolyte solvent ethylene glycol was investigated by FT-IR using a Bruker Tensor 37. Na2S5 was prepared by mixing a 1:4 molar mixture of Na2S and S8 in EG until the mixture dissolved to nominally provide Na2S5. Figure 3 shows the FT-IR spectra of Na2S5 at 7 wt% sodium dissolved in EG and incubated at 110°C, 125°C, and 150°C for 195 hours compared to the baseline (i.e., prepared without thermal incubation). The data show a slight shift in peak heights for the 110°C data, but larger shifts at 125°C and 150°C, including the appearance of new peaks indicating the formation of new compounds.

[0055] In Figs. 4 and 5, -1 and 3250cm -1 The change in peak height relative to the baseline (i.e., normalized) in the FT-IR spectrum at wavenumbers of about 1725 cm is plotted. -1 The absorption band at 3250 cm is associated with the by-product 2-hydroxyethyl acetate. -1 The absorption band at 1725 cm is associated with EG. The data show that during the first 65 hours of incubation, the anolyte is similarly affected at the three test temperatures of 110°C, 125°C, and 150°C. However, further incubation showed no further degradation at 110°C, but further degradation was observed at 125°C and 150°C. Specifically, the absorption band at 1725 cm increases with increasing temperature. -1 The increase in absorption at 3250 cm indicates an increase in the side reaction producing 2-hydroxyethyl acetate. -1The decrease in absorption at 110°C indicates the disappearance of EG with increasing temperature, likely due to its conversion to by-products such as 2-hydroxyethyl acetate. Figure 6 shows the mass loss as a percentage of the baseline amount after 195 hours at three temperatures for two groups of anolytes with sodium contents of 3 and 7 wt%. The data show minimal mass loss at 110°C compared to 125 and 150°C.

[0056] In another study, Na2S5 anolytes in EG were prepared with 5 wt% sodium and incubated at various temperatures from 80°C to 150°C. The results are shown in Figure 7 as a plot of % mass loss versus incubation time. The data show similar trends to the 7% and 3% Na samples, with samples below 110°C showing negligible weight loss.

[0057] Anolytes from cells (from Example 1) operated at low temperature (110° C.), dual temperature (100° C. and 125° C.), and 125° C. (as shown in FIG. 9) were analyzed by FT-IR. Results for the three samples showed a peak at 1580 cm -1 and 1725 cm -1 11 and 12 as normalized peak heights at 100° C., demonstrating the presence of decomposition products in the anolyte. The data show that at a constant temperature of 125° C. (no temperature swing test), there was much greater degradation compared to the 110° C. and dual temperature tests.

[0058] Example 4 - Electrochemical cell with β''-alumina ceramic membrane for producing sodium metal from sodium polysulfide A hybrid electrochemical flow cell as in Example 1 is constructed using a β″-alumina ceramic membrane of the same thickness as the NaSICON ceramic membrane to separate the anolyte and catholyte compartments. Due to the lower conductivity of the β″-alumina membrane, the cell operates at approximately one-third the current density of the corresponding cell using NaSICON of Example 1.

[0059] Alternatively, a hybrid electrochemical flow cell as in Example 1 is constructed using a β''-alumina membrane that is approximately one-quarter to one-half the thickness of the NaSICON ceramic membrane to separate the anolyte and catholyte compartments. The current density of this electrochemical flow cell is expected to be comparable to that of the corresponding cell using NaSICON in Example 1.

[0060] Example 5 - Electrochemical cell with NaSICON ceramic membrane and temperature sensitive solvent mixture for producing sodium metal from sodium polysulfide A hybrid electrochemical flow cell is constructed as in Example 1 using different temperature sensitive solvents in the anolyte. In this cell, an 80:20 w / w mixture of ethylene glycol and NMP is used as the temperature sensitive solvent. The cell is operated under similar conditions as in Example 1. The addition of NMP to ethylene glycol is expected to increase the sodium ion conductivity of the anolyte.

[0061] Equivalent While particular embodiments have been illustrated and described, those skilled in the art, after reading the foregoing specification, may make modifications, substitutions of equivalents, and other types of changes to the methods, electrolytic cells, electrolytes, electrodes, systems, and operating conditions as described herein. Each of the above aspects and embodiments may also include or incorporate variations or aspects as disclosed with respect to any or all of the other aspects and embodiments.

[0062] Also, the present technology should not be limited with respect to the specific embodiments described herein, which are intended as single illustrations of individual embodiments of the present technology. Many modifications and variations of the present technology can be made without departing from its spirit and scope, as will be apparent to those skilled in the art. In addition to those enumerated herein, functionally equivalent methods within the scope of the present technology will be apparent to those skilled in the art from the foregoing description. Such modifications and variations are intended to be within the scope of the appended claims. It is understood that the present technology is not limited to specific methods, solvents, electrolyte reagents, compounds, compositions, cells, and conditions, which can, of course, vary. All methods described herein can be performed in any suitable order unless otherwise indicated herein or clearly contradicted by context. It is also understood that the terms used herein are for the purpose of describing particular embodiments only, and are not intended to be limiting. Thus, it is intended that the specification be considered as exemplary only, with the breadth, scope, and spirit of the present technology being indicated only by the appended claims, definitions therein, and any equivalents thereof. No language in the specification should be construed as indicating any non-claimed element as essential.

[0063] The embodiments illustratively described herein may suitably be practiced in the absence of any element or elements, or limitation or limitations not specifically disclosed herein. Thus, for example, the terms "comprising," "including," "containing," and the like, shall be read expansively and without limitation. Furthermore, the terms and expressions used herein are used as terms of description and not of limitation, and in using such terms and expressions, there is no intention to exclude any equivalents of the features shown and described or portions thereof, but it is recognized that various modifications are possible within the scope of the claimed technology. Furthermore, the phrase "consisting essentially of" will be understood to include the elements specifically recited and additional elements that do not substantially affect the basic and novel characteristics of the claimed technology (e.g., the conductivity or current density of the claimed embodiment). The phrase "consisting of" excludes any elements not specified. Furthermore, the use of any of the foregoing terms in the description of a particular element or embodiment contemplates the use of any of the other terms. For example, it will be understood that the use of "comprising" with respect to an element or embodiment also discloses the use of "consisting essentially of" or "consisting of" with respect to the same element or embodiment, and vice versa.

[0064] Furthermore, where features or aspects of the disclosure are described in terms of a Markush group, one of skill in the art will recognize that the disclosure is also described thereby in terms of any individual member or subgroup of members of the Markush group. Each of the narrower species and subgeneric groupings falling within the generic disclosure also form part of the present technology. This includes the generic description of the technology with a proviso or negative limitation removing any subject matter from the genus, regardless of whether the excluded material is specifically recited herein.

[0065] As will be understood by those skilled in the art, for any and all purposes, particularly in terms of providing a written description, all ranges disclosed herein also encompass any and all possible subranges thereof, as well as combinations of subranges. Any recited range can be readily recognized as fully descriptive and allowing the same range to be broken down into at least two, three, four, five, ten, etc. As a non-limiting example, each range discussed herein can be readily broken down into a lower third, a middle third, and an upper third, etc. Also, as will be understood by those skilled in the art, all language such as "up to," "at least," "greater than," "less than," etc. refers to a range that includes the recited numbers and can be broken down into subranges as described above. Finally, as will be understood by those skilled in the art, a range includes each individual member, and each individual value is incorporated herein as if it were individually recited herein.

[0066] All publications, patent applications, issued patents, and other documents (e.g., journals, articles, and / or textbooks) mentioned herein are incorporated by reference herein as if each individual publication, patent application, issued patent, or other document was specifically and individually indicated to be incorporated by reference in its entirety. Definitions contained in the texts incorporated by reference are excluded to the extent they conflict with definitions in this disclosure.

[0067] Other embodiments are defined in the appended claims, along with the full scope of equivalents to which such claims are entitled.

Claims

1. The following steps: introducing an anolyte at a first temperature into an anolyte compartment of an electrochemical flow cell; the anolyte comprising sulfur and an effective amount of a sodium salt dissolved in a temperature sensitive solvent; the anolyte compartment comprises an anode, the anode containing the sodium salt; The electrochemical flow cell comprises: Catholyte compartment and a ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment comprises a molten sodium cathode; Introducing; passing sodium ions from said sodium salt through said ceramic sodium ion conducting membrane from said anolyte compartment to said catholyte compartment; reducing the sodium ions to sodium metal at the molten sodium cathode; and cooling the anolyte outside the anolyte compartment to a second temperature without recovering sulfur. A method comprising: the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that occurs at the first temperature; method.

2. 2. The method of claim 1, wherein the sodium salt comprises sodium sulfide, sodium polysulfide, or a mixture of sodium sulfide and one or more sodium polysulfides.

3. The sodium polysulfide has the formula Na 2 S x 3. The method of claim 2, wherein x is an integer from 1 to 32.

4. 2. The method of claim 1, wherein the amount of sodium in the anolyte ranges from about 1% to about 10% by weight.

5. 2. The method of claim 1, wherein the amount of sodium in the anolyte ranges from about 3% to about 7% by weight.

6. 10. The method of claim 1 further comprising recovering the sulfur from the anolyte at a temperature of about 15°C to 80°C.

7. The temperature sensitive solvent is an alkyl diol, an alkyl triol, a cycloalkyl diol, a cycloalkyl triol, a lactam, a cyclic urea, a C 1~6 2. The method of claim 1, wherein the organic solvent is selected from the group consisting of alkyl amides, carbonates, ethers, mixtures of any two or more thereof, or mixtures of any of the foregoing with water.

8. 2. The method of claim 1, wherein the temperature sensitive solvent is selected from the group consisting of ethylene glycol, propylene glycol, butane-1,4-diol, diethylene glycol, triethylene glycol, tetraethylene glycol, glycerol, and mixtures of two or more thereof.

9. The method of claim 1 , wherein the temperature sensitive solvent is ethylene glycol.

10. 10. The method of claim 1, wherein an anode current collector in electrical contact with the anode is disposed within the anolyte compartment of the electrochemical flow cell.

11. The method of claim 10 , wherein the anode current collector comprises one or more of nickel, various carbon types, steel, kovar, or cobalt.

12. The method of claim 11 , wherein the anode current collector comprises nickel.

13. The method of claim 1 , wherein the electrochemical flow cell further comprises a cathode current collector.

14. The method of claim 13 , wherein the cathode current collector comprises nickel.

15. 2. The method of claim 1, wherein the ceramic sodium ion conductive membrane comprises a sodium ion conductive garnet-like ceramic, a Na conductive ceramic glass, NaSiCON, or Na-β″-alumina.

16. 2. The method of claim 1, wherein the ceramic sodium ion conductive membrane, or the ceramic sodium ion conductive membrane and the anolyte compartment, are heated to the first temperature.

17. 2. The method of claim 1, wherein the ceramic sodium ion conductive membrane, or the ceramic sodium ion conductive membrane and the anolyte compartment, are heated to the first temperature by a thermal enclosure.

18. When anolyte is present in the anolyte compartment, the ceramic sodium ion conducting membrane has a conductivity of at least 10 mS cm -1 The method of claim 1 , wherein the conductive material has a conductivity of

19. When anolyte is present in the anolyte compartment, the ceramic sodium ion conducting membrane has a conductivity of at least 50 mS cm -1 The method of claim 1 , wherein the conductive material has a conductivity of

20. The ceramic sodium ion conductive membrane has a conductivity of 10 mScm -1 ~100 mScm -1 The method of claim 1 , wherein the conductive material has a conductivity of

21. The following steps: introducing an anolyte at a first temperature of from 115° C. to about 150° C. into an anolyte compartment of an electrochemical flow cell; the anolyte comprising an effective amount of a sulfur-containing sodium salt dissolved in a temperature sensitive solvent comprising an alkyl diol; the anolyte compartment comprises an anode, the anode comprising the sulfur-containing sodium salt; The electrochemical flow cell comprises: Catholyte compartment and a ceramic sodium ion conducting membrane separating the anolyte compartment from the catholyte compartment; and the catholyte compartment comprises a molten sodium cathode; Introducing; passing sodium ions from said sodium salt through said ceramic sodium ion conducting membrane from said anolyte compartment to said catholyte compartment; reducing the sodium ions to sodium metal at the molten sodium cathode; and cooling the anolyte outside the anolyte compartment to a second temperature of from 80° C. to less than 115° C. without recovering sulfur. A method comprising: the second temperature causes decomposition of the temperature sensitive solvent at a rate that is less than 20% of the rate that occurs at the first temperature; method.

22. A dual-temperature electrochemical system comprising: The system further comprises: an anolyte source comprising anolyte; at least one pump for pumping the anolyte through the system; a heater for heating the anolyte to a first temperature; a chiller for cooling the anolyte to a second temperature lower than the first temperature; 1. An electrolytic flow cell comprising: an anolyte compartment and a catholyte compartment separated by a sodium ion conducting ceramic membrane; an anode comprising a sodium salt disposed within the anolyte compartment; a molten sodium cathode disposed within the catholyte compartment; and a power source electrically connected to the anode and the cathode; Equipped with the anolyte compartment further comprises an anolyte inlet and an anolyte outlet; and the catholyte compartment includes an opening through which molten sodium can flow; Electrolysis flow cell Equipped with the anolyte source is in fluid communication with the pump and the anolyte inlet; system.

Citation Information

Patent Citations

  • Method for recovering alkali metal and sulfur from alkali metal sulfides and polysulfides

    JP2016519712A

  • Method and apparatus for recovering metals and sulfur from feedstreams containing metal sulfides and polysulfides

    JP2019500501A