Soundproofing paint

A soundproofing paint with hollow beads of varying elasticity and hardness forms a dense layer for effective sound insulation and heat reduction, addressing dust and heat issues in existing technologies.

JP7566231B2Active Publication Date: 2024-11-05TC UNION CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021030750
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-11-05
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Existing soundproofing methods for buildings and air conditioner outdoor units face issues such as dust accumulation and heat buildup, and existing soundproofing paints using metal powders face challenges with high temperatures and require thick coatings for effective sound isolation.

Method used

A soundproofing paint comprising first and second hollow beads with different elasticity and hardness properties, having a predetermined size difference, forms a dense layer that maintains soundproofing effectiveness over time, with a preferred particle size range of 50 to 100 μm for maximum beads and smaller sizes filling gaps between them.

Benefits of technology

The paint achieves long-lasting soundproofing by maintaining a dense bead layer and enhancing sound insulation, while also providing heat insulation and reducing external noise levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566231000003
    Figure 0007566231000003
  • Figure 0007566231000004
    Figure 0007566231000004
  • Figure 0007566231000005
    Figure 0007566231000005
Patent Text Reader

Abstract

To provide a sound-proof coating applicable to an architectural structure, an air conditioner outdoor unit or the like.SOLUTION: A sound-proof coating P containing, in a film formation material 1, an elastic first hollow bead 2, and a second hollow bead 3 of a material harder than the material of the first hollow bead 2, is used for sound-proofing. Hereby, even if hollow beads of each material are put into mutual contact, a hollow structure can be maintained to thereby contribute to sound-proofing.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a soundproofing coating for buildings, outdoor units of air conditioners, etc. [Background technology]

[0002] In recent years, in light of environmental and energy issues, energy conservation efforts have been made in various fields. For example, in the case of air conditioners, which account for a certain amount of energy consumption in buildings, efforts have become common from both a technical perspective, such as improving compressor performance and increasing the efficiency of equipment operation through sensors and inverter control, as well as an operational perspective, such as reviewing the set temperature. In addition, energy conservation efforts are also being made for the buildings themselves, such as insulating roofs and walls.

[0003] On the other hand, efforts to prevent noise have not progressed as much as efforts to save energy, etc. For example, it is a well-known fact that there are quite a few noise problems, such as the sound of compressor motors.

[0004] One example of tackling the above problem is to enclose the outdoor unit of an air conditioner in a soundproof cover. However, this method can lead to new problems, such as dust accumulating between the outdoor unit and the soundproof cover, and heat buildup that creates a high temperature environment around the device, resulting in increased power loss.

[0005] Under these circumstances, one technology for using paint to achieve soundproofing is vibration- and sound-proofing paint (Patent Document 1), which is made by mixing metallic powder such as lead into synthetic resin, heating it, melting and kneading it to uniformly disperse it, rapidly solidifying it, and crushing it to form powder in the form of metal-containing lumps, and then mixing this with epoxy resin or the like as a binder and kneading and dispersing it uniformly.

[0006] However, the technology described in Patent Document 1 has the problem that it is prone to high temperatures because it uses metal powder. In addition, although it is thought that the moldability is improved by using metal powder, there is a problem that the thickness of the coating film must be as large as possible to contribute to soundproofing and vibration proofing. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special Publication No. 62-058633 Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved is to provide a soundproofing coating material that can be applied to buildings, outdoor units of air conditioners, etc. [Means for solving the problem]

[0009] The first invention is a soundproof paint including first hollow beads having elasticity and second hollow beads made of a material harder than that of the first hollow beads. The second invention is the soundproof paint of the first invention, in which either or both of the first and second hollow beads are composed of a predetermined size with a particle size difference of 30 μm or more, and the content (volume basis) of hollow beads with the largest particle size is the largest. Here, the composition of a predetermined size with a particle size difference of 30 μm or more can be, for example, a composition of hollow beads with a maximum particle size of 80 μm to a minimum particle size of 50 μm. However, the maximum particle size and the minimum particle size are not limited. The third invention is the soundproof paint of the second invention, in which the particle size of the hollow beads with the maximum particle size is within the range of 50 to 100 μm. The fourth invention is the soundproof paint of the second or third invention, in which the particle size fits into the gap between the hollow beads with the maximum particle size adjacent to each other. It is preferable that the specified size of the hollow beads is equal to or smaller than a size that allows the hollow beads to be adequately held by the coating film formed when applied, and is equal to or larger than a size that allows a gas such as air to be held therein and that can exhibit soundproofing properties, etc. Effect of the Invention

[0010] In the present invention, the coating film contains first hollow beads having elasticity and second hollow beads made of a harder material, so that the first hollow beads can reversibly maintain their shape even when they come into contact with each other, and the hollow beads can maintain their internal space without breaking even when they come into contact with each other due to external pressure or the like. That is, a dense layer of hollow beads can be formed and maintained, and soundproofing effects can be expected to be achieved over a long period of time. In addition, since the coating film is composed of hollow beads with different particle sizes and has the largest content of the maximum particle size, the beads can be made denser, and a dense layer of beads can be formed and maintained. That is, the amount of space useful for soundproofing in the coating film can be increased, and the soundproofing effect can be expected to be further improved. In addition, by setting the maximum particle size of the hollow beads within the range of 50 to 100 μm and using hollow beads with a particle size that fits into the gaps between the hollow beads with the maximum particle size, the above effect can be expected to be stably obtained. In addition, in the present invention, soundproofing means reducing or blocking sound (vibrations of various wavelengths, waveforms, and frequencies) propagating from a source. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a paint according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of a layer of hollow beads in a paint. [Diagram 3] This is a conceptual diagram showing the relationship between the target equipment, coating, and sound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the present invention will be described in detail based on the embodiments.

[0013] <Paint> As shown in Fig. 1, paint P, which is an example of a paint for soundproofing according to this embodiment, has a coating film-forming material 1 such as a water-based or solvent-based material, hollow beads 2 (an example of the first hollow beads) made of a soft material having elasticity, and hollow beads 3 (an example of the second hollow beads) made of a hard material. Note that Fig. 1 is an image diagram showing that there are multiple types of hollow beads, and that each type of hollow bead has a range of particle diameters.

[0014] An example of the coating film-forming material 1 is an acrylic emulsion resin. The coating film-forming material 1 may be a resin mainly composed of a urethane-based, silicone-based, or fluorine-based component other than an acrylic-based material.

[0015] Examples of materials for the soft hollow beads 2, which are an example of the first hollow beads having elasticity, include plastics such as acrylic, polystyrene, polycarbonate, etc., and elastomers such as rubber, etc. The soft hollow beads 2 are preferably made of the same material as the coating film-forming material 3, and for example, when the coating film-forming material 3 is an acrylic emulsion resin, the soft hollow beads 2 are acrylic hollow beads.

[0016] The hard hollow beads 3 are, for example, ceramic hollow beads or glass hollow beads. Ceramic hollow beads include those made from volcanic ash containing 65 to 73% silicon dioxide and 12 to 18% aluminum oxide as main components.

[0017] The ratio of the soft hollow beads 2 to the hard hollow beads 3 is preferably 1:1 on a weight basis or a volume basis. The ratio of the soft hollow beads 2 to the hard hollow beads 3 should be close to 1:1 on a weight basis. If the ratio of the soft hollow beads 2 is high, the flexibility of the paint film is high when the paint dries, but the thickness of the paint film from one application is not sufficient. It is necessary to increase the number of applications. On the other hand, if the ratio of the hard hollow beads 3 is high, the thickness of the paint film from one application is thick when the paint dries, but the flexibility of the paint film is impaired. Taking into account the passage of time, the ratio of the soft hollow beads 2 is preferably 50% or more on a volume basis or a weight basis.

[0018] The reason for using multiple materials with different properties in this way is to take advantage of the bead characteristics of each material (soundproofing effect, molding effect, heat insulation effect, durability, etc. obtained from the shape and components.) In the following examples, for example, acrylic hollow beads and ceramic hollow beads were used in a 1:1 ratio by weight for the hollow beads.

[0019] Here, hollow beads refer to particles that have voids or spaces inside the beads, and may be either a closed system in which air is blocked from the inside and outside of the beads, or an open system in which the inside and outside of the beads are connected, such as a porous structure or doughnut structure.

[0020] The particle size of hollow beads such as the soft hollow beads 2 and the hard hollow beads 3 preferably has a predetermined range of particle size difference (for example, a range of particle size from 80 μm to 50 μm) based on the maximum particle size. If the particle size distribution has a predetermined range, when a solvent such as water evaporates from the paint P to form a paint film, hollow beads with smaller particle sizes will get in between the hollow beads with the largest particle size, making the hollow beads more dense. The maximum particle size of the hollow beads may be determined by the coarseness, mesh size, etc. of the filter used to filter the hollow beads.

[0021] The hollow beads for each component have a lineup of three particle sizes (particle size lineup). Here, the particle size lineup means that the particle sizes of the hollow beads are configured to have multiple intended particle sizes. In this example, the hollow beads of each material have peaks in hollowness (the ratio of the total volume of the hollow parts for each particle size in the coating film) at particle sizes of 80 μm, 60 μm, and 50 μm, and the weight ratio is 5:3:2 (including fine beads generated during the manufacturing process).

[0022] In this embodiment, the hollow beads of 80 μm are the largest in both volume and weight. The membrane thickness of the hollow beads of each diameter ranges from about 1 μm to several μm, and the volume of the hollow part inside the bead is generally 80% or more of the bead.

[0023] There are various methods for confirming the particle size distribution of hollow beads. For example, there is a method for measuring the particle size from the area of ​​hollow beads in the enlarged image of Figure 2. There is also the Coulter method, which measures the volume of each particle to determine the corresponding particle size, as well as the so-called centrifugal sedimentation method and laser diffraction / scattering method. Note that hollow beads are very fine, so it is technically difficult to manufacture hollow beads with an accurate particle size. Therefore, the particle size distribution should be confirmed assuming manufacturing errors. For example, there is a method in which all hollow beads with a particle size of 80 μm ± 5 μm are counted as hollow beads with a particle size of 80 μm.

[0024] The density of the hollow beads in the coating film is preferably at the level shown in Figure 2. A coating film with this density level can provide soundproofing, sound insulation, vibration control, and other effects. Figure 3 is a conceptual diagram. A coating film containing soft hollow beads 2 and hard hollow beads 3 is formed on the surface of equipment 4 by coating film forming material 1. In this way, the coating film blocks and reduces sound 5 transmitted from the outside.

[0025] The shape of the hollow beads such as the soft hollow beads 2 and the hard hollow beads 3 is preferably spherical as shown in Fig. 2, but may not be spherical. When the hollow beads are distorted like fragments and are not spherical, the particle size may be the average of the maximum and minimum widths of the hollow beads, the maximum width, or the minimum width of the hollow beads.

[0026] <Coating agent> Methanol (90% by weight or more), water (4% by weight or more), tin oxide (SnO 2 ) (0.1% by weight) is the main coating agent. The coating agent may be the hydrophilic coat described in JP 2019-002671 A or a similar one. However, it is not necessarily required.

[0027] The coating agent may contain components for purposes other than soundproofing, such as photocatalysts such as titanium oxide, zinc oxide, and tin oxide. In this case, the coating film has a multifunctional structure with a lower layer for soundproofing and an upper layer that has a different function. For example, photocatalysts such as titanium oxide in the coating agent clean the painted surface by their hydrophilicity and photocatalytic reaction.

[0028] Example 1 The evaluation of the soundproofing effect of the paint according to the present invention will be described below. In this example, the evaluation targets are offices of multiple companies (railroad, electric power, manufacturing), factory roofs and exterior walls, air conditioning and electrical equipment (air conditioner outdoor units, substation control panels, railway communication equipment, server rooms), and beverage vending machines.

[0029] The coating process consists of a process of removing dirt from the surface of the target equipment with a high-pressure water wash, and a process of applying paint with a roller brush to a film thickness of approximately 400 μm (when dry). There are no limitations on the coating method. For example, coating by spraying can be used. With a roller brush, a film thickness of approximately 200 μm (when dry) was formed with the first coat, and approximately 400 μm (when dry) with the second coat.

[0030] Table 1 shows the results of a year-round observation of the soundproofing effect of the coating. Painting the exterior walls of the office reduced external noise. [Table 1]

[0031] In Table 1, the facility being evaluated is an office located near a source of low-frequency noise. Table 1 shows the results of a sensory evaluation indicating the extent to which paint applied to the office walls reduced low-frequency noise. The condition before the paint was applied ("Sound can be heard" under "Before application" in Table 1) is the subject of comparison. The index for this sensory evaluation is a five-point scale: "Very unpleasant sound can be heard," "Unpleasant sound can be heard," "Sound can be heard," "Slight sound can be heard," and "Almost no sound can be heard." As Table 1 shows, the paint reduced low-frequency noise by one level.

[0032] No visible stains were observed on the exterior of the areas where the paint was applied (Table 2). [Table 2]

[0033] Table 2 shows the results of a sensory evaluation of the appearance of the painted areas of the office walls. The areas that were not painted were used for comparison. Table 2 shows the extent to which the dirtiness of the office walls differed depending on whether or not they were painted. Similar results were obtained for all of the equipment tested this time.

[0034] In addition, for all equipment, including the office exterior walls and air conditioner outdoor units, the temperature difference between the areas where paint was applied and those where it was not was approximately 30 to 40 degrees Celsius in the summer (the areas where paint was applied remained cool).

[0035] Example 2 Verification of useful forms of the coating material according to the present invention will be described below. As described above, the hollow beads in this embodiment are made of ceramic beads, which are a hard material, and acrylic resin beads, which are a soft material. By using two types of materials in this way, it is possible to take advantage of the characteristics of each material.

[0036] Generally, hollow beads made of ceramics or glass, which have excellent heat resistance, are used for various purposes. However, when only hollow beads made of these hard materials are used in paint, the hollow beads often break due to contact with each other. In another test, it was found that most of the beads break when only glass beads are used in the same amount as the hollow beads used in this embodiment.

[0037] On the other hand, in this example, almost no cracking of the beads was observed, suggesting that the combination of hollow beads made of a hard material and hollow beads made of a soft material can form a dense layer of hollow beads.

[0038] What materials are hard and what materials are soft, and how to select the materials, is a matter of relative importance between the materials. In this embodiment, no cracks occurred when the ceramic hollow beads and the acrylic hollow beads were combined. This is thought to be due to the elasticity of the acrylic hollow beads. In this way, it is sufficient to select a material that can withstand the stress of the hollow beads of the other material.

[0039] Here, Young's modulus is an index of the elasticity of a material. Synthetic resins often have a Young's modulus of 4 or less. It is said that glass has a Young's modulus of 80, and inorganic compounds such as silicon dioxide and aluminum oxide that form ceramics have a Young's modulus of 100 or more. Taking into account this technical common knowledge and the results of this example, it is suggested that a combination of at least a soft material with a Young's modulus of 4 or less and a hard material with a Young's modulus of 80 or more can form a dense hollow bead layer in the paint.

[0040] It was also confirmed that, in addition to acrylic, urethane, silicone, and fluorine-based coating materials have similar soundproofing effects. In other words, it was suggested that synthetic resins in general can be used as coating materials according to the present invention. However, in terms of formability of the coating, acrylic is the best coating material according to the present invention.

[0041] The amount of hollow beads used varies depending on the thickness of the coating and the particle size of the beads. The density level of the hollow beads shown in Figure 2 is a guide for forming a desired coating thickness.

[0042] In this embodiment, the hollow beads of each material have particle sizes of 80 μm, 60 μm, and 50 μm, with a weight ratio of 5:3:2. As shown in Figure 2, the proportion of hollow beads with the largest particle size is also the highest in terms of volume ratio. Thus, it has been found that the greatest soundproofing effect is achieved when the volume ratio of hollow beads with the largest particle size is maximized.

[0043] In this embodiment, hollow beads with a maximum particle size of 80 μm and a minimum particle size of 50 μm (particle size difference 30 μm) were mainly used. Empirically, the maximum particle size is preferably within the range of 50 to 100 μm. The minimum particle size is not limited and may be less than 1 μm. This is because it can contribute to increasing the density of the hollow beads.

[0044] The particle size lineup also allows for a dense structure of hollow beads, which increases the soundproofing effect. A combination of hollow beads with two or more peaks in the particle size distribution may also contribute to the soundproofing effect. Such peaks may be 60 μm, 50 μm, or even smaller. For example, they may be of a particle size that fills the gap between adjacent hollow beads of the largest particle size. Theoretically, hollow beads of such a particle size can maximize the dense state of the hollow beads.

[0045] Also, the hollow beads with the largest particle size may be acrylic hollow beads, and the beads with a particle size that fills the gaps between the acrylic hollow beads may be ceramic hollow beads. If the beads with the largest particle size are ceramic, the acrylic hollow beads may be of a particle size that can separate the ceramic hollow beads so that they do not come into contact with each other. In this way, it is sufficient that the particle size and material composition are such that adverse effects such as cracks caused by contact between the hollow beads can be avoided.

[0046] In addition, the thickness of the paint film changes depending on various factors. For example, the thickness of the paint film immediately after painting is smaller than that after the paint has dried. This is because the water in the paint evaporates. The thickness of the film also expands and contracts due to the influence of temperature, humidity, etc. Therefore, when the paint film shrinks between adjacent hard and soft hollow beads, it is expected that the former will deform the latter into a concave shape. It is important to select a material that can withstand the stress associated with this paint film shrinkage and maintain the hollow structure of the beads.

[0047] Furthermore, the paint of the present invention lowered the surface temperature of the target equipment by 30 to 40°C compared to the surrounding area in summer. This result suggests that the hollow bead layer in the coating film is formed uniformly.

[0048] In this example, a coating film of about 400 μm formed on the surface of the target equipment achieved a year-round soundproofing effect. A coating film with a larger amount of hollow beads or a coating film thickness of more than 400 μm is expected to have an even greater soundproofing effect. Empirically, a coating film thickness of 300 to 600 μm is useful as a soundproofing paint without significantly affecting moldability and durability. [Industrial Applicability]

[0049] The present invention can be used in the field of soundproofing of buildings, outdoor units of air conditioners, etc. In addition, the present invention can be used not only for the equipment according to the present embodiment, but also for various objects such as vehicles, aircraft, ships, etc. [Explanation of symbols]

[0050] 1 Paint film forming material 2. First hollow bead 3. Second hollow bead P Paint (Soundproof Paint)

Claims

[Claim 1] A soundproofing paint comprising a first hollow bead made of a synthetic resin material and a second hollow bead made of an inorganic compound material in a coating film forming material, A soundproofing paint in which either or both of the first and second hollow beads are composed of particles of a specified size with a particle size difference of 30 μm or more, and which has the largest content (on a volume basis) of hollow beads with a particle size of 80 μm.

Citation Information

Patent Citations

  • Industrial thermal insulation coating and preparation method thereof

    CN102093788A

  • Dry etching device

    JP1987058633A

  • Paint and painted product

    JP2017186452A

  • Crack resistance insulating paint

    KR1020200073695A