Isophthalate plasticizer composition and resin composition containing the same
A plasticizer composition using dihexyl isophthalate from a hexyl alcohol isomer mixture improves tensile strength, elongation, and migration resistance, while maintaining low viscosity and heat stability, overcoming the limitations of traditional plasticizers in PVC resins.
Patent Information
- Application Number
- JP2023518276
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-24
- Filing Date
- 2021-11-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-23
AI Technical Summary
Existing plasticizers, such as di(2-ethylhexyl) terephthalate (DEHTP), exhibit high hardness, slow absorption rate, poor migration and stress migration properties, and deteriorate mechanical properties when used in PVC resins, while alternatives like tri(2-ethylhexyl) trimellitate and triisononyl trimellitate increase costs and environmental concerns.
A plasticizer composition comprising dihexyl isophthalate derived from a hexyl alcohol isomer mixture, including 1-hexanol, 1-methylpentanol, and 2-methylpentanol, with a specific ratio of dihexyl isophthalate and di(2-ethylhexyl) isophthalate, enhances tensile strength, elongation, and migration resistance, and maintains low initial sol viscosity and viscosity stability.
The composition achieves equivalent plasticization efficiency with improved tensile strength, elongation, and reduced migration and heat loss, addressing environmental concerns and cost issues of traditional plasticizers.
Smart Images

Figure 0007566408000001 
Figure 0007566408000002 
Figure 0007566408000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0158965, filed on November 24, 2020, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a plasticizer composition containing an isophthalate derived from a mixed alcohol of isomers of hexyl alcohol and di(2-ethylhexyl)isophthalate, and a resin composition containing the same. [Background technology]
[0003] Plasticizers are usually made by reacting alcohol with polycarboxylic acids such as phthalic acid and adipic acid to form the corresponding esters. In addition, in consideration of domestic and international regulations on phthalate-based plasticizers, which are harmful to the human body, research is ongoing into plasticizer compositions that can be used to replace phthalate-based plasticizers, such as terephthalate-based, adipate-based, and other polymer-based plasticizers.
[0004] Meanwhile, the need for such environmentally friendly products is increasing in the plastisol industry, such as flooring, wallpaper, soft and hard sheets, the calendaring industry, and the extrusion / injection compounding industry. In order to enhance the quality characteristics, processability, and productivity of each finished product, it is necessary to use appropriate plasticizers taking into consideration discoloration, migration, mechanical properties, etc.
[0005] In these various areas of use, PVC resin is blended with secondary materials such as plasticizers, fillers, stabilizers, viscosity reducers, dispersants, defoamers, and foaming agents depending on the characteristics required by each industry, such as tensile strength, elongation, light resistance, migration, gelling properties, and absorption speed.
[0006] For example, when di(2-ethylhexyl) terephthalate (DEHTP), which is relatively inexpensive and most widely used among plasticizer compositions applicable to PVC, is applied, the hardness or sol viscosity is high, the absorption rate of the plasticizer is relatively slow, and the migration and stress migration properties are also poor.
[0007] One possible solution to this problem is to use the product of a transesterification reaction with butanol as a plasticizer in a composition containing DEHTP. However, although this improves the plasticization efficiency, it also leads to a deterioration in heat loss and thermal stability, and some decrease in mechanical properties, so improvements in physical properties are required. Therefore, there is currently no solution other than to supplement this by mixing it with another secondary plasticizer.
[0008] However, when using secondary plasticizers, it is difficult to predict the change in physical properties, which may lead to increased product costs, and there are drawbacks such as the occurrence of unpredictable problems, such as the improvement of physical properties being unclear except in specific cases and causing compatibility problems with resins.
[0009] In addition, when a trimellitate-based product such as tri(2-ethylhexyl) trimellitate or triisononyl trimellitate is used to improve the poor migration, weight loss and light resistance of the DEHTP product, the migration and weight loss properties are improved, but the plasticization efficiency is deteriorated and a considerable amount must be added to give the resin an appropriate plasticization effect. Therefore, the product is relatively expensive and cannot be commercially used.
[0010] In addition, when a substance such as dibutyl terephthalate is mixed into a terephthalate-based product, there is a problem that the use of the substance beyond a certain amount is restricted, since it causes environmental problems such as air pollution during processing due to deterioration in weight loss caused by heating, and thus the plasticization efficiency cannot be improved.
[0011] Therefore, there is a demand for development of products that solve the environmental problems of existing phthalate-based products or products that improve the poor physical properties of environmentally friendly products to improve the environmental problems of phthalate-based products. Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention provides a plasticizer composition characterized by being a mixture of dihexyl isophthalate, in which the hexyl group has an alkyl group derived from a mixture of hexyl alcohol isomers, and di(2-ethylhexyl)isophthalate, and an object of the present invention is to provide a plasticizer composition that, when applied to a resin, has equivalent plasticizing efficiency, improved tensile strength and elongation, and good migration resistance.
[0013] Another object of the present invention is to provide a plasticizer composition which has a low initial sol viscosity, little change in the sol viscosity over time, and excellent viscosity stability. [Means for solving the problem]
[0014] In order to solve the above problems, the present invention provides a plasticizer composition.
[0015] (1) The present invention provides a plasticizer composition that includes dihexyl isophthalate and di(2-ethylhexyl)isophthalate, wherein the hexyl group of the dihexyl isophthalate is derived from an isomeric mixture of hexyl alcohol, and the isomeric mixture of hexyl alcohol includes two or more selected from the group consisting of 1-hexanol, 1-methylpentanol, 2-methylpentanol, 3-methylpentanol, 4-methylpentanol, 1,1-dimethylbutanol, 1,2-dimethylbutanol, 1,3-dimethylbutanol, 2,2-dimethylbutanol, 2,3-dimethylbutanol, 3,3-dimethylbutanol, 1-ethylbutanol, 2-ethylbutanol, 3-ethylbutanol, and cyclopentylmethanol.
[0016] (2) The present invention provides a plasticizer composition according to the above (1), wherein the mixture of hexyl alcohol isomers contains 1-hexanol and 2-methylpentanol.
[0017] (3) The present invention provides the plasticizer composition according to (1) or (2) above, wherein the isomer mixture of hexyl alcohol contains 30 parts by weight or more of a branched alcohol per 100 parts by weight of the isomer mixture.
[0018] (4) The present invention provides a plasticizer composition according to any one of the above items (1) to (3), wherein the isomer mixture of hexyl alcohol contains 40 to 95 parts by weight of a branched alcohol per 100 parts by weight of the isomer mixture.
[0019] (5) The present invention provides a plasticizer composition according to any one of the above items (1) to (4), wherein the isomer mixture of hexyl alcohol contains 40 parts by weight or less of 1-hexanol per 100 parts by weight of the isomer mixture.
[0020] (6) The present invention provides the plasticizer composition according to any one of the above (1) to (5), wherein the dihexyl isophthalate and di(2-ethylhexyl) isophthalate are present in a weight ratio of 90:10 to 10:90.
[0021] (7) The present invention provides a plasticizer composition in any one of the above (1) to (6), wherein the mixture of hexyl alcohol isomers contains 1-hexanol, 2-methylpentanol, and 3-methylpentanol.
[0022] (8) The present invention provides a resin composition comprising 100 parts by weight of a resin and 5 to 150 parts by weight of a plasticizer composition according to any one of (1) to (7) above.
[0023] (9) The present invention provides a resin composition according to (8) above, wherein the resin is at least one selected from the group consisting of straight vinyl chloride polymer, paste vinyl chloride polymer, ethylene-vinyl acetate copolymer, ethylene polymer, propylene polymer, polyketone, polystyrene, polyurethane, polylactic acid, natural rubber, and synthetic rubber. Effect of the Invention
[0024] When used in a resin composition, the plasticizer composition according to one embodiment of the present invention has the same plasticizing efficiency as existing plasticizers, and can have improved tensile strength and elongation, as well as good migration resistance.
[0025] In addition, the plasticizer composition according to the present invention has a low initial sol viscosity and little change in sol viscosity over time, and thus has excellent viscosity stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0027] Definition of Terms The term "composition" as used herein includes mixtures of materials which comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition.
[0028] The term "straight vinyl chloride polymer" as used herein means one type of vinyl chloride polymer, which may be polymerized by suspension polymerization, bulk polymerization, or the like, and which has the form of porous particles with a large number of pores having sizes of tens to hundreds of micrometers distributed therein, is non-aggregating, and has excellent fluidity.
[0029] The term "paste vinyl chloride polymer" as used herein refers to a type of vinyl chloride polymer, which may be polymerized by fine suspension polymerization, fine seed polymerization, emulsion polymerization, or the like, and is a polymer in the form of fine, dense, void-free particles having a size of tens to thousands of nanometers, which has agglomeration properties, and which has poor fluidity.
[0030] The terms "comprise", "have" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether specifically disclosed or not. To avoid any uncertainty, all compositions claimed by use of the term "comprise" may include any additional additives, adjuvants, or compounds, whether polymeric or otherwise, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any consecutive description any other component, step or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step or procedure not specifically described or listed.
[0031] Measurement method In this specification, the content of components in a composition is analyzed by gas chromatography measurement using a gas chromatography device manufactured by Agilent (product name: Agilent 7890 GC, column: HP-5, carrier gas: helium (flow rate 2.4 mL / min), detector: FID, injection volume: 1 μL, initial value: 70° C. / 4.2 min, final value: 280° C. / 7.8 min, program rate: 15° C. / min).
[0032] In this specification, "hardness" refers to Shore hardness (Shore "A" and / or Shore "D") at 25°C in accordance with ASTM D2240, measured under conditions of 3T 10s, and can be an index for evaluating plasticization efficiency, with a lower hardness indicating a more excellent plasticization efficiency.
[0033] In this specification, the "tensile strength" is calculated according to the ASTM D638 method by measuring the point where a test piece breaks after pulling it at a cross head speed of 200 mm / min (1T) using a UTM (manufacturer: Instron, model name: 4466) which is a test device, and calculating it according to the following mathematical formula 1.
[0034] [Mathematical formula 1] Tensile strength (kgf / cm 2 ) = Load value (kgf) / (Thickness (cm) x Width (cm))
[0035] In the present specification, the "elongation rate" is calculated by the following Equation 2 after measuring the point where the test piece breaks after pulling the test piece at a cross head speed of 200 mm / min (1T) using the UTM in accordance with the ASTM D638 method.
[0036] [Mathematical formula 2] Elongation rate (%) = length after elongation / initial length x 100
[0037] In this specification, the term "migration loss" refers to a test piece having a thickness of 2 mm or more, which is obtained according to KSM-3156, and after attaching glass plates to both sides of the test piece, the test piece is subjected to a pressure of 1 kgf / cm 2A load of 10 ...
[0038] [Mathematical formula 3] Migration loss (%) = {[(initial weight of test piece) - (weight of test piece after leaving in oven)] / (initial weight of test piece)} x 100
[0039] In this specification, the "volatile loss" is calculated by measuring the weight of a test piece after treating the test piece at 80°C for 72 hours.
[0040] [Mathematical formula 4] Heat loss (%) = {[(initial weight of test piece) - (weight of test piece after treatment)] / (initial weight of test piece)} x 100
[0041] In the case of the various measurement conditions, the detailed conditions such as temperature, rotation speed, time, etc. may vary slightly depending on the case, and if they do vary, the measurement method and conditions will be separately specified.
[0042] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.
[0043] According to one embodiment of the present invention, the plasticizer composition comprises dihexyl isophthalate and di(2-ethylhexyl) isophthalate, wherein the hexyl group of the dihexyl isophthalate is derived from an isomeric mixture of hexyl alcohol.
[0044] According to one embodiment of the present invention, the isomeric mixture of hexyl alcohols of the plasticizer composition comprises two or more selected from the group consisting of 1-hexanol, 1-methylpentanol, 2-methylpentanol, 3-methylpentanol, 4-methylpentanol, 1,1-dimethylbutanol, 1,2-dimethylbutanol, 1,3-dimethylbutanol, 2,2-dimethylbutanol, 2,3-dimethylbutanol, 3,3-dimethylbutanol, 1-ethylbutanol, 2-ethylbutanol, 3-ethylbutanol, and cyclopentylmethanol.
[0045] The alkyl groups of the dihexyl isophthalate can be determined by the alcohols contained in the mixture of hexyl alcohol isomers, and the final composition can include various compositions in which the two alkyl groups are bonded to two isomeric alkyl groups of hexyl alcohol, one alkyl group is bonded to one alkyl group is bonded to the other alkyl groups, or none is bonded to the other alkyl groups. The ratio of the components in the final composition can be determined by the ratio of the reacting alcohol components.
[0046] In this way, when using isophthalate as a component of a plasticizer, if an alcohol with 6 carbon atoms is used, an appropriate level of absorption speed can be ensured, compared to when the carbon number is less than 6, thereby improving processability, and tensile strength, elongation, and heat loss can be greatly improved. In addition, compared to when the carbon number is more than 6, excellent plasticization efficiency can be achieved, and great migration resistance and stress resistance can be expected.
[0047] The branching degree of the hexyl alcohol isomer mixture of the plasticizer composition according to one embodiment of the present invention may be 2.0 or less, preferably 1.5 or less. Specifically, the branching degree may be 1.5 or less, 1.3 or less, and more preferably 1.1 or less. Also, it may be 0.1 or more, 0.2 or more, 0.3 or more, and most preferably 0.7 or more. The branching degree of the hexyl alcohol isomer mixture may be maintained even when it is converted to dihexyl isophthalate by esterification reaction. If the branching degree exceeds 2.0, the balance between physical properties may be lost, and a problem may occur in which the product does not meet one or more evaluation criteria. However, if the branching degree is 1.5 or less as a preferred range, the improvement of not only mechanical properties but also migration loss and heat loss may be more optimized, and the balance between physical properties may be excellent.
[0048] Here, the degree of branching may mean how many branched carbons the alkyl group bonded to a substance contained in the composition has, and the degree of branching may be determined according to the weight ratio of the substance. For example, assuming that an alcohol mixture contains 60% by weight of n-hexyl alcohol, 30% by weight of methylpentyl alcohol, and 10% by weight of ethylbutyl alcohol, the branched carbon numbers of each alcohol are 0, 1, and 2, respectively, so the branching degree can be calculated as [(60×0)+(30×1)+(10×2)] / 100, which is 0.5. Here, in the case of cyclopentylmethanol, the branched carbon number is considered to be 0.
[0049] The plasticizer composition according to one embodiment of the present invention may contain 1-hexanol and 2-methylpentanol in the hexyl alcohol isomer mixture. In this case, excellent effects can be obtained in terms of migration resistance and heat loss.
[0050] The branched hexyl alcohol including 2-methylpentanol may be included in an amount of 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, and preferably 60 parts by weight or more, 70 parts by weight or more, based on 100 parts by weight of the isomer mixture. The maximum amount may be entirely branched, and may be 99 parts by weight or less, 98 parts by weight or less, and preferably 95 parts by weight or less, or 90 parts by weight or less. When the branched hexyl alcohol is included in this range, improvement in mechanical properties can be expected.
[0051] In addition, the linear alcohol of 1-hexanol may be included in an amount of 50 parts by weight or less, 40 parts by weight or less, and preferably 30 parts by weight or less, based on 100 parts by weight of the isomer mixture. The 1-hexanol may not be present in the component, but may be included in an amount of at least 2 parts by weight, in which case, it is possible to obtain an advantage in that mechanical properties are improved while maintaining a balance between physical properties.
[0052] The plasticizer composition according to one embodiment of the present invention may contain 1-hexanol, 2-methylpentanol, and 3-methylpentanol in the isomer mixture of hexyl alcohol. By further containing 3-methylpentanol, the heat loss can be further improved while maintaining a balance between physical properties. In this case, 3-methylpentanol may be included as a component of the branched hexyl alcohol and may be present so as to satisfy the content of the branched hexyl alcohol described above.
[0053] More preferably, the mixture of isomers of hexyl alcohol may further contain cyclopentylmethanol, which is expected to have the effect of complementing migration resistance and stress migration.
[0054] In this case, the cyclopentylmethanol may be present independently in an amount of 20 parts by weight or less, preferably 15 parts by weight or less, and more preferably 10 parts by weight or less, per 100 parts by weight of the isomer mixture, and may be absent or the minimum amount for obtaining the effect thereof may be 2 parts by weight.
[0055] Specifically, depending on the ratio of branched alkyl groups to the total alkyl radicals in the final composition, and further, the ratio of a specific branched alkyl radical among the branched alkyl groups, the physical properties of plasticization efficiency and migration / weight loss characteristics can be balanced, and mechanical properties such as tensile strength and elongation and stress resistance can be maintained at the same or higher levels. Excellent viscosity characteristics can be achieved by the interaction between dihexyl isophthalates having various types of alkyls in the composition, which can be achieved by the components of the above-mentioned hexyl alcohol isomers and their component ratios.
[0056] This makes it possible to eliminate the environmental problems associated with existing phthalate-based products and realize products with improved weight loss properties, and it is possible to significantly improve the migration and weight loss properties of existing terephthalate-based products, thereby enabling the realization of products with significantly improved mechanical properties compared to existing commercial products.
[0057] According to an embodiment of the present invention, the dihexyl isophthalate is mixed with di(2-ethylhexyl) isophthalate and used as a plasticizer. Di(2-ethylhexyl) isophthalate can complement the mechanical properties and thermal stability of dihexyl isophthalate by being mixed with dihexyl isophthalate. Meanwhile, when dihexyl phthalate is used instead of dihexyl isophthalate, it is not appropriate because dihexyl phthalate is not a substance regulated due to environmental concerns, but it has potential environmental concerns and many restrictions on use, and it has very poor mechanical properties such as tensile strength and elongation compared to isophthalate, and its plasticization efficiency is also low.
[0058] The plasticizer composition according to an embodiment of the present invention is characterized by being a mixture of dihexyl isophthalate and di(2-ethylhexyl) isophthalate having the above-mentioned characteristics. In this case, the mixing weight ratio may be 90:10 to 10:90, and various other weight ratios may be applied, with the upper limit being 85:15, 80:20, 75:25, 70:30, 65:35, or 60:40, and the lower limit being 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, or 50:50. When dihexyl isophthalate and di(2-ethylhexyl) isophthalate are mixed within the above-mentioned weight ratio range, one physical property is not significantly deteriorated, and the overall physical properties can be maintained at a balanced and excellent level. In particular, in the plasticizer composition according to one embodiment of the present invention, when the amount of di(2-ethylhexyl)isophthalate is equal to or greater than that of dihexylisophthalate, it may be particularly advantageous in terms of mechanical properties and heat loss.
[0059] The method for producing the plasticizer composition according to one embodiment of the present invention is a method well known in the art and can be applied without any particular limitation as long as it can produce the above-mentioned plasticizer composition.
[0060] First, in the case of dihexyl isophthalate, for example, the composition can be prepared by directly esterifying an isophthalic acid or an anhydride thereof with an isomeric mixture of hexyl alcohol, or the composition can be prepared by transesterifying an isophthalate with an isomeric mixture of hexyl alcohol.
[0061] The plasticizer composition according to one embodiment of the present invention is a material prepared by appropriately carrying out the esterification reaction, and as long as it satisfies the above-mentioned conditions, in particular, the ratio of branched alcohol in the isomer mixed alcohol is controlled and specific components are included, there is no particular limitation on the preparation method.
[0062] For example, the direct esterification reaction can be carried out by the steps of: introducing isophthalic acid or a derivative thereof and two or more mixed alcohols, adding a catalyst, and reacting under a nitrogen atmosphere; removing unreacted raw materials; neutralizing (or inactivating) the unreacted raw materials and the catalyst; and removing impurities (e.g., distillation under reduced pressure) and filtering.
[0063] The components and weight ratios of the isomer mixture of hexyl alcohol are as described above. The isomer mixture of alcohol can be used in a range of 200-900 mol%, 200-700 mol%, 200-600 mol%, 250-500 mol%, or 270-400 mol% relative to 100 mol% of the acid, and the component ratio in the final composition can be controlled by controlling the content of this alcohol.
[0064] The catalyst may be one or more selected from acid catalysts such as sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, paratoluenesulfonic acid, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, alkylsulfuric acid, etc., metal salts such as aluminum lactate, lithium fluoride, potassium chloride, cesium chloride, calcium chloride, iron chloride, aluminum phosphate, etc., metal oxides such as heteropolyacids, natural / synthetic zeolites, cation and anion exchange resins, and organic metals such as tetraalkyl titanate and its polymers. As a specific example, the catalyst may be tetraalkyl titanate. Preferably, paratoluenesulfonic acid, methanesulfonic acid, etc. are suitable as acid catalysts with low activation temperatures.
[0065] The amount of catalyst used may vary depending on the type. For example, in the case of a homogeneous catalyst, the amount may be within the range of 0.01 to 5 wt%, 0.01 to 3 wt%, 1 to 5 wt%, or 2 to 4 wt%, relative to 100 wt% of the total amount of reactants. In the case of a heterogeneous catalyst, the amount may be within the range of 5 to 200 wt%, 5 to 100 wt%, 20 to 200 wt%, or 20 to 150 wt%, relative to the total amount of reactants.
[0066] At this time, the reaction temperature can be within the range of 100°C to 280°C, 100°C to 250°C, or 120°C to 230°C.
[0067] As another example, the transesterification reaction can be a reaction of an isophthalate with an alcohol having an alkyl radical different from the alkyl radical of the isophthalate, where the alkyl groups of the isophthalate and the alcohol can be crossed.
[0068] The term "transesterification reaction" as used herein means a reaction in which an alcohol reacts with an ester to exchange the alkyl groups of the ester and the alkyl groups of the alcohol, as shown in Reaction Scheme 1 below.
[0069] [ka]
[0070] The mixture produced by the transesterification reaction can control the composition ratio of the mixture according to the amount of alcohol added. The amount of alcohol added can be 0.1 to 200 parts by weight, specifically 1 to 150 parts by weight, and more specifically 5 to 100 parts by weight, relative to 100 parts by weight of isophthalate. For reference, the component ratio in the final composition can be determined by the amount of alcohol added, as in the direct esterification reaction.
[0071] According to one embodiment of the present invention, the transesterification reaction is carried out at a reaction temperature of 120°C to 190°C, preferably 135°C to 180°C, more preferably 141°C to 179°C, for 10 minutes to 10 hours, preferably 30 minutes to 8 hours, more preferably 1 to 6 hours. Within the above temperature and time ranges, the component ratio of the final plasticizer composition can be efficiently controlled. In this case, the reaction time can be calculated from the time when the reactants reach the reaction temperature after heating.
[0072] The transesterification reaction can be carried out in the presence of an acid catalyst or a metal catalyst, which has the effect of shortening the reaction time.
[0073] The acid catalyst may be, for example, sulfuric acid, methanesulfonic acid, or p-toluenesulfonic acid, and the metal catalyst may be, for example, an organometallic catalyst, a metal oxide catalyst, a metal salt catalyst, or a metal itself.
[0074] The metal component may be, for example, any one selected from the group consisting of tin, titanium, and zirconium, or a mixture of two or more of these.
[0075] Di(2-ethylhexyl)isophthalate can be prepared in the same manner as above, and dihexylisophthalate and di(2-ethylhexyl)isophthalate can be prepared in the plasticizer composition according to one embodiment of the present invention by mixing the two components according to the weight ratio described above.
[0076] According to another embodiment of the present invention, there is provided a resin composition comprising the above-described plasticizer composition and a resin.
[0077] The resin may be any resin known in the art, including, but not limited to, a mixture of one or more selected from the group consisting of straight vinyl chloride polymer, paste vinyl chloride polymer, ethylene-vinyl acetate copolymer, ethylene polymer, propylene polymer, polyketone, polystyrene, polyurethane, polylactic acid, natural rubber, synthetic rubber, and thermoplastic elastomer.
[0078] The plasticizer composition can be contained in an amount of 5 to 150 parts by weight, preferably 5 to 130 parts by weight, or 10 to 120 parts by weight, based on 100 parts by weight of the resin.
[0079] Generally, the resin in which the plasticizer composition is used can be manufactured as a resin product by melt processing or plastisol processing, and melt-processed resins and plastisol-processed resins can be produced differently depending on the polymerization method.
[0080] For example, when vinyl chloride polymer is used in melt processing, solid resin particles with a large average particle size produced by suspension polymerization or the like are used, and such vinyl chloride polymer is called "straight vinyl chloride polymer."When it is used in plastisol processing, a resin in a sol state as fine resin particles produced by emulsion polymerization or the like is used, and such vinyl chloride polymer is called "paste vinyl chloride resin."
[0081] In this case, in the case of the straight vinyl chloride polymer, the plasticizer is preferably contained in a range of 5 to 80 parts by weight per 100 parts by weight of the polymer, and in the case of a paste vinyl chloride polymer, the plasticizer is preferably contained in a range of 40 to 120 parts by weight per 100 parts by weight of the polymer.
[0082] The resin composition may further contain a filler, the amount of the filler being 0 to 300 parts by weight, preferably 50 to 200 parts by weight, and more preferably 100 to 200 parts by weight, relative to 100 parts by weight of the resin.
[0083] The filler can be any filler known in the art, and is not particularly limited.For example, the filler can be one or more mixtures selected from silica, magnesium carbonate, calcium carbonate, hard carbon, talc, magnesium hydroxide, titanium dioxide, magnesium oxide, potassium hydroxide, aluminum hydroxide, aluminum silicate, magnesium silicate and barium sulfate.
[0084] Furthermore, the resin composition may further contain other additives such as a stabilizer, if necessary. The amount of each of the other additives such as the stabilizer may be, for example, 0 to 20 parts by weight, preferably 1 to 15 parts by weight, per 100 parts by weight of the resin.
[0085] The stabilizer may be, for example, a calcium-zinc (Ca-Zn) stabilizer such as a calcium-zinc complex stearate or a barium-zinc (Ba-Zn) stabilizer, but is not particularly limited thereto.
[0086] As described above, the resin composition may be applied to both melt processing and plastisol processing. For example, the melt processing may be a calendaring process, an extrusion process, or an injection process, and the plastisol processing may be a coating process.
[0087] Working Example Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0088] Manufacturing Example 1-1 Into a four-necked 3-liter reactor equipped with a cooler, condenser, decanter, reflux pump, temperature controller, stirrer, etc., 516.5 g of isophthalic acid, 1,170 g of hexanol (n-hexanol and 2-methylpentanol mixed at a weight ratio of 1:9), and 1.55 g of tetraisopropyl titanate as a catalyst were added, the reaction temperature was set to 230°C, and nitrogen gas was continuously added to carry out a direct esterification reaction for about 6 hours, and the reaction was completed when the acid value reached 0.1.
[0089] After the reaction was completed, distillation extraction was carried out under reduced pressure to remove unreacted raw materials. After distillation extraction, a neutralization process, a dehydration process, and a filtration process were performed to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nH2MPIP), and di(2-methylpentyl)isophthalate (D2MPIP).
[0090] Manufacturing Example 1-2 The same procedure was carried out as in Preparation Example 1-1, except that 1,170 g of a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 3:7 was used as hexanol, to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nHMPIP), and di(2-methylpentyl)isophthalate (DMPIP).
[0091] Manufacturing Example 1-3 The same procedure was carried out as in Preparation Example 1-1, except that 1,170 g of a mixture of n-hexanol and 2-methylpentanol in a weight ratio of 7:3 was used as hexanol, to obtain a composition containing di(n-hexyl)isophthalate (DnHIP), (n-hexyl)(2-methylpentyl)isophthalate (nHMPIP), and di(2-methylpentyl)isophthalate (DMPIP).
[0092] Manufacturing Example 1-4 A composition was obtained in the same manner as in Preparation Example 1-1, except that 1,170 g of a mixture of n-hexanol, 2-methylpentanol, and 3-methylpentanol in a weight ratio of 2:3:5 was used as hexanol.
[0093] Manufacturing Example 1-5 A composition was obtained in the same manner as in Preparation Example 1-1, except that 1,170 g of a mixture of n-hexanol, 2-methylpentanol, 3-methylpentanol and cyclopentylmethanol in a weight ratio of 7:37:44:12 was used as hexanol.
[0094] Manufacturing Example 2 516.5g of isophthalic acid, 1,170g of 2-ethylhexanol, and 1.55g of tetraisopropyl titanate as a catalyst were added to a four-necked 3-liter reactor equipped with a cooler, condenser, decanter, reflux pump, temperature controller, stirrer, etc., and the reaction temperature was set to 230°C. Nitrogen gas was continuously added, and a direct esterification reaction was carried out for about 6 hours. The reaction was completed when the acid value reached 0.1.
[0095] After the reaction was completed, distillation extraction was carried out under reduced pressure to remove unreacted raw materials. After distillation extraction, the mixture was neutralized, dehydrated, and filtered to obtain di(2-ethylhexyl)isophthalate (DnHIP).
[0096] Production Example 3 A composition containing di(2-methylpentyl)isophthalate (D2MPIP) was obtained in the same manner as in Preparation Example 1-1, except that 1,170 g of 2-methylpentanol was used instead of hexanol.
[0097] Production Example 4 A composition containing dibutyl isophthalate (DBIP) was obtained in the same manner as in Preparation Example 1-1, except that 1,170 g of n-butanol was used instead of hexanol.
[0098] Production Example 5 A composition containing diheptyl isophthalate (DHpIP) was obtained in the same manner as in Preparation Example 2, except that 1,170 g of n-heptanol was used instead of 2-ethylhexanol.
[0099] Production Example 6 The same procedure was carried out as in Preparation Example 1-1, except that 516.5 g of terephthalic acid was used instead of isophthalic acid, to obtain a composition containing di(n-hexyl) terephthalate (DnHTP), (n-hexyl)(2-methylpentyl) terephthalate (nH2MPTP) and di(2-methylpentyl) terephthalate (D2MPTP).
[0100] The types of alcohols and acids used in the above Production Examples 1-1 to 1-5 and 2 to 6 are summarized in Table 1 below.
[0101] [Table 1]
[0102] Example 1-1 The dihexyl isophthalate (mixture) of Preparation Example 1-1 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 1:9 to prepare a plasticizer composition.
[0103] Example 1-2 The dihexyl isophthalate (mixture) of Preparation Example 1-1 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 2:8 to prepare a plasticizer composition.
[0104] Examples 1-3 The dihexyl isophthalate (mixture) of Preparation Example 1-1 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 3:7 to prepare a plasticizer composition.
[0105] Examples 1-4 The dihexyl isophthalate (mixture) of Preparation Example 1-1 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 5:5 to prepare a plasticizer composition.
[0106] Examples 1-5 The dihexyl isophthalate (mixture) of Preparation Example 1-1 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 7:3 to prepare a plasticizer composition.
[0107] Example 2-1 The dihexyl isophthalate (mixture) of Preparation Example 1-2 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 3:7 to prepare a plasticizer composition.
[0108] Example 2-2 The dihexyl isophthalate (mixture) of Preparation Example 1-3 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 3:7 to prepare a plasticizer composition.
[0109] Example 2-3 The dihexyl isophthalate (mixture) of Preparation Example 1-4 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 3:7 to prepare a plasticizer composition.
[0110] Examples 2-4 The dihexyl isophthalate (mixture) of Preparation Example 1-5 and di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 3:7 to prepare a plasticizer composition.
[0111] Comparative Example 1 Dioctyl phthalate (DOP), manufactured by LG Chem, was used as the plasticizer composition.
[0112] Comparative Example 2 Diisononyl phthalate (DINP), manufactured by LG Chem, was used as the plasticizer composition.
[0113] Comparative Example 3 Di(2-ethylhexyl) terephthalate (DEHTP, LGflex GL300) manufactured by LG Chem was used as the plasticizer composition.
[0114] Comparative Example 4 A mixture (LGflex GL500) of di(2-ethylhexyl) terephthalate (DEHTP), butyl(2-ethylhexyl) terephthalate (BEHTP), and dibutyl terephthalate (DBTP) manufactured by LG Chem was used as the plasticizer composition.
[0115] Comparative Example 5 The composition of Preparation Example 1-1 was used alone.
[0116] Comparative Example 6 The composition of Preparation Example 2 was used alone.
[0117] Comparative Example 7 The di(2-methylpentyl)isophthalate (D2MPIP) of Preparation Example 3 and the di(2-ethylhexyl)isophthalate of Preparation Example 2 were mixed in a weight ratio of 5:5 to prepare a plasticizer composition.
[0118] Comparative Example 8 The dibutyl isophthalate (DBIP) of Preparation Example 4 and the di(2-ethylhexyl) isophthalate of Preparation Example 2 were mixed in a weight ratio of 5:5 to prepare a plasticizer composition.
[0119] Comparative Example 9 The dihexyl isophthalate (mixture) of Preparation Example 1-1 and diheptyl isophthalate (DHpIP) of Preparation Example 5 were mixed in a weight ratio of 5:5 to prepare a plasticizer composition.
[0120] Comparative Example 10 The dihexyl terephthalate (mixture) of Preparation Example 6 and di(2-ethylhexyl)isophthalate of Preparation Example 2 were mixed in a weight ratio of 5:5 to prepare a plasticizer composition.
[0121] The components of the plasticizer compositions prepared in the above Examples and Comparative Examples and their weight ratios are summarized in Table 2 below.
[0122] [Table 2]
[0123] Experimental example 1: Evaluation of seat performance Using the plasticizers of the Examples and Comparative Examples, test pieces were prepared according to the following recipes and preparation conditions in accordance with ASTM D638.
[0124] (1) Formulation: 100 parts by weight of straight vinyl chloride polymer (LS100), 50 parts by weight of plasticizer, and 3 parts by weight of stabilizer (BZ-153T)
[0125] (2) Mixing: Mix at 98℃ and 700 rpm
[0126] (3) Preparation of test pieces: 1T, 2T and 3T sheets were prepared by treating in a roll mill at 160°C for 4 minutes, and in a press at 180°C for 2.5 minutes (low pressure) and 2 minutes (high pressure).
[0127] (4) Evaluation items 1)Hardness In accordance with ASTM D2240, Shore hardness (Shore "A" and "D") at 25°C was measured for 10 seconds using a 3T test piece. The smaller the value, the better the plasticization efficiency.
[0128] 2) Tensile strength According to ASTM D638, the test equipment UTM (manufacturer: Instron, model name: 4466) was used to measure the point at which the 1T test piece broke after pulling at a cross head speed of 200 mm / min. The tensile strength was calculated as follows: Tensile strength (kgf / cm 2 ) = Load value (kgf) / thickness (cm) x width (cm)
[0129] 3) Measurement of elongation rate According to the ASTM D638 method, the UTM was used to measure the point at which the 1T test piece broke after pulling at a cross head speed of 200 mm / min, and the elongation was calculated as follows: The elongation rate (%) was calculated as follows: length after elongation / initial length×100.
[0130] 4) Measurement of migration loss According to KSM-3156, a test piece with a thickness of 2 mm or more is obtained, and a glass plate is attached to both sides of the 1T test piece, and then the specimen is subjected to a pressure of 1 kgf / cm 2 A load of 10 ... Migration loss (%) = [{(initial weight of test piece at room temperature) - (weight of test piece after leaving in oven)} / (initial weight of test piece at room temperature)] × 100
[0131] 5) Measurement of volatile loss The prepared test piece was treated at 80° C. for 72 hours, and then the weight of the test piece was measured. The weight loss on heating (%) was calculated as follows: [{(initial weight of test piece)-(weight of test piece after treatment)} / (initial weight of test piece)]×100.
[0132] (5) Evaluation results The evaluation results for the above items are shown in Table 3 below.
[0133] [Table 3]
[0134] Referring to the results in Table 3, it can be seen that the plasticizer compositions according to the embodiments of the present invention exhibit excellent plasticizing efficiency, excellent mechanical properties, and good results in terms of migration loss and heat loss.
[0135] Comparative Examples 1 and 2 were the most commonly used plasticizer products in the past, but are now prohibited from use due to environmental regulations, and it can be confirmed that the plasticizers according to the examples of the present invention show similar or superior plasticizing efficiency compared to these existing plasticizers, and that no performance problems arise when the plasticizer compositions of the present invention are used in place of existing plasticizers, and although the plasticizer compositions of the examples of the present invention show somewhat inferior migration resistance and heat loss, they show excellent results in terms of elongation. Considering that the plasticizer compositions of Comparative Examples 1 and 2 are currently difficult to use due to environmental regulations, it can be confirmed that the plasticizer compositions of the present invention can be fully used as environmentally friendly products in place of existing plasticizer products.
[0136] In addition, Comparative Examples 3 and 4 are environmentally friendly plasticizers used in place of Comparative Examples 1 and 2, and Comparative Example 3 has excellent mechanical properties, but is very poor in migration resistance and plasticization efficiency, and it can be inferred that the excellent performance of mechanical properties cannot be fully demonstrated. In addition, in the case of Comparative Example 4, none of the tensile strength, elongation, migration loss, and heat loss are superior to the Examples, and migration resistance and heat loss are relatively inferior, confirming the superiority of the plasticizer composition of the Examples of the present invention.
[0137] On the other hand, in Comparative Examples 5 and 6, dihexyl isophthalate or di(2-ethylhexyl) isophthalate, which are components contained in the plasticizer composition of the present invention, were used alone. In the case of Comparative Example 5, in which dihexyl isophthalate was used alone, it was confirmed that the plasticization efficiency was excellent, but the mechanical properties were significantly inferior and the heat loss was also significantly inferior. In addition, it was confirmed that Comparative Example 6, in which di(2-ethylhexyl) isophthalate was used alone, also showed inferior mechanical properties and migration resistance compared to the plasticizer composition according to the embodiment of the present invention. From this, it is determined that the fact that the plasticizer composition of the present invention exhibits good properties overall, as well as excellent plasticization efficiency, mechanical properties, migration resistance and heat loss, is an effect achieved by using a mixture of dihexyl isophthalate and di(2-ethylhexyl) isophthalate.
[0138] Comparative Examples 7 and 8 relate to the case where, instead of the dihexyl isophthalate used in the compositions of the examples of the present invention, an isophthalate derived from a single branched C6 alcohol (Comparative Example 7) or an isophthalate derived from a C4 alcohol (Comparative Example 8) is used. In the case of Comparative Example 7, since the structure of the hexyl group contained in the dihexyl isophthalate is not diverse, it is inferior in mechanical properties, and in the case of Comparative Example 8, since the number of carbon atoms of the alkyl group bonded to the isophthalate is small, it is significantly inferior in mechanical properties and heat loss compared to Comparative Example 7. Therefore, from the above results, it can be seen that the fact that the alkyl group of the dihexyl isophthalate contained in the examples of the present invention is derived from an isomer mixture of hexyl alcohol contributes to the excellent effect of the plasticizer composition of the present invention.
[0139] Finally, Comparative Example 9 uses diheptyl isophthalate instead of di(2-ethylhexyl) isophthalate used in the compositions of the examples of the present invention, but it can be confirmed that Comparative Example 9 also has poor mechanical properties and heat loss, and Comparative Example 10 uses a composition prepared by using an isomer mixture of terephthalic acid and hexyl alcohol instead of isophthalic acid, and it can be confirmed that it also shows poor mechanical properties and heat loss. From this, it can be seen that the effects achieved by the plasticizer composition of the present invention are achieved by the specific types of components contained in the plasticizer composition and the weight ratio between them.
[0140] Example 2: Evaluation of plastisol performance Using the plasticizers of the Examples and Comparative Examples, test pieces were prepared according to the following recipe and preparation conditions in accordance with ASTM D638.
[0141] (1) Formulation: Paste vinyl chloride polymer (KH-10) 100 parts by weight, plasticizer 60 parts by weight and stabilizer (CZ400) 3 parts by weight
[0142] (2) Mixing: Mix at 1000 rpm for 15 minutes
[0143] (3) Preparation of test specimens: The compounded plastisol was spread to a thickness of 0.3 mm and cured in an oven at 230°C for 2 minutes to prepare test specimens.
[0144] (4) Evaluation items 1) Viscosity Brookfield viscosity was measured using a Brookfield (LV type) viscometer, using a #64 spindle, at measurement speeds of 6 rpm and 60 rpm, and at a measurement temperature of 25°C.
[0145] (5) Evaluation results The evaluation results for the above items are shown in Table 4 below.
[0146] [Table 4]
[0147] Referring to Table 4, it can be seen that when the plasticizer compositions of the Examples are used, the initial viscosity is low and the rate of change in viscosity is not large. Therefore, it can be seen that the plasticizer compositions of the present invention can be used as a complete substitute for existing plasticizers in plastisol processing.
Claims
1. dihexyl isophthalate and di(2-ethylhexyl) isophthalate, The hexyl group of the dihexyl isophthalate is derived from an isomeric mixture of hexyl alcohol, The plasticizer composition, wherein the isomer mixture of hexyl alcohol comprises two or more selected from the group consisting of 1-hexanol, 1-methylpentanol, 2-methylpentanol, 3-methylpentanol, 4-methylpentanol, 1,1-dimethylbutanol, 1,2-dimethylbutanol, 1,3-dimethylbutanol, 2,2-dimethylbutanol, 2,3-dimethylbutanol, 3,3-dimethylbutanol, 1-ethylbutanol, 2-ethylbutanol, 3-ethylbutanol, and cyclopentylmethanol.
2. 2. The plasticizer composition of claim 1, wherein the isomeric mixture of hexyl alcohols comprises 1-hexanol and 2-methylpentanol.
3. 2. The plasticizer composition according to claim 1, wherein the isomer mixture of hexyl alcohol contains 30 parts by weight or more of a branched alcohol per 100 parts by weight of the isomer mixture.
4. 2. The plasticizer composition according to claim 1, wherein the isomer mixture of hexyl alcohol contains 40 to 95 parts by weight of a branched alcohol per 100 parts by weight of the isomer mixture.
5. 2. The plasticizer composition according to claim 1, wherein the isomer mixture of hexyl alcohol contains 40 parts by weight or less of 1-hexanol per 100 parts by weight of the isomer mixture.
6. 2. The plasticizer composition of claim 1, wherein the dihexyl isophthalate and di(2-ethylhexyl) isophthalate are in a weight ratio of 90:10 to 10:
90.
7. 2. The plasticizer composition of claim 1, wherein the isomeric mixture of hexyl alcohols comprises 1-hexanol, 2-methylpentanol, and 3-methylpentanol.
8. A resin composition comprising 100 parts by weight of a resin and 5 to 150 parts by weight of the plasticizer composition according to claim 1 relative to 100 parts by weight of the resin.
9. 9. The resin composition according to claim 8, wherein the resin is at least one selected from the group consisting of straight vinyl chloride polymer, paste vinyl chloride polymer, ethylene-vinyl acetate copolymer, ethylene polymer, propylene polymer, polyketone, polystyrene, polyurethane, polylactic acid, natural rubber, and synthetic rubber.
Citation Information
Patent Citations
Mixed alcohol for producing plasticizer and method for producing plasticizer using the same
JP2001322959A
Production of ester mixture
JP2016150940A
Ester-based compound, plasticizer composition containing the same, method for producing the same, and resin composition containing the same
JP2017506216A
Ester-based compound, plasticizer composition containing the same, method for producing the same, and resin composition containing the same
JP2017509592A
Cyclohexane triester plasticizer composition and resin composition comprising same
WO2020222536A1