Manufacturing method of composite pressurized fluid container
By using a method with a temperature-controlled intermediate layer and a different resin for the third layer, the bonding issues of polyolefin resins are resolved, resulting in a strong and durable composite container structure.
Patent Information
- Application Number
- JP2022528669
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-20
- Filing Date
- 2020-11-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-11-02
AI Technical Summary
Polyolefin resins like polybutene-1, polyethylene, and polypropylene are difficult to bond with other layers due to their stable chemical structure, leading to poor bond quality and health risks from adhesives, and over time, the bond deteriorates.
A method involving a first polyolefin resin tape layer, an intermediate layer with temperature-dependent permeability, and a third layer of a different resin, where the intermediate layer is heated above its threshold temperature and cooled below the melting point of the other layers to facilitate bonding.
Creates a strong, durable bond between layers with improved adhesion and resistance to separation, enhancing the structural integrity of pressurized fluid composite containers.
Smart Images

Figure 0007566899000001 
Figure 0007566899000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a composite pressurized fluid container.
[0002] More particularly, the present invention relates to a method for manufacturing a composite pressurized fluid container, comprising the steps of winding a first polyolefin resin-based tape to form a first layer of the container, and depositing on the first layer an intermediate second layer of a material having variable permeability properties that are temperature dependent, in particular permeable below a predetermined temperature threshold and impermeable above the temperature threshold, the method further comprising winding a second resin-based tape onto the intermediate second layer to form a third layer.
[0003] FIELD OF THE DISCLOSURE The present invention relates to a thermoplastic composite container manufactured using a tape reinforced with a polyolefin resin.In some applications, various elements, such as supports or accessories, must be attached to the exterior surface of the container. [Background technology]
[0004] Polyolefin resins, such as polybutene-1, polyethylene, and polypropylene, are not suitable for forming bonds with additional layers during manufacture of the container.
[0005] Polyolefin resins have a fairly stable chemical structure (very stable outer electronic structure) and as a result, it is quite difficult to form the chemical bonds (structural bonds) to bond the resin to other layers or materials.
[0006] There are approaches to overcome this problem. To improve the ability of such resins to form bonds with other layers or materials, it is known practice to provide, for example, chemical attack, plasma treatment (for example "Matis" treatment), flame treatment or surface polishing to the surface of the material. The aim of these solutions is to change the chemical nature of the surface layer, allowing chemical bonding with adhesives.
[0007] Some adhesives give very good adhesion results on polyolefins, but have a very short open time (especially cyanoacrylate adhesives such as 3M DP 8005). These adhesives can also cause health problems.
[0008] Other adhesives must be applied according to very specific and complex protocols to produce maximum bond strength, making the quality of the bond operator dependent (temperature for applying the adhesive, exact ratios of the adhesive's ingredients, moisture levels, thickness of adhesive, etc.).
[0009] However, these known solutions do not provide the required results over time: over time, a deterioration in the quality of the bond is observed.
[0010] Despite these problems, the polyolefin resins are often the most widely used resins for making composite containers, especially due to their favorable cost. Summary of the Invention [Problem to be solved by the invention]
[0011] SUMMARY OF THE PRESENT EMBODIMENT One object of the present invention is to overcome all or part of the above-mentioned shortcomings of the prior art. [Means for solving the problem]
[0012] To that end, the method according to the invention, which also complies with the generic definition given in the preamble above, is essentially characterized in that the tape forming the third layer is based on a resin different from that of the first layer and in that, during the step of depositing the intermediate second layer and during the step of winding the second tape, the intermediate second layer is kept at a temperature higher than the threshold temperature, the method then comprising a step of cooling the intermediate second layer to a temperature lower than the threshold temperature, during which the first and third layers are each kept at a temperature higher than the melting point of their resins.
[0013] Furthermore, embodiments of the invention may include one or more of the following features: The first polyolefin resin-based tape contains reinforcing fibers, such as glass and / or carbon fibers. The thickness of the second layer is less than the thickness of the first layer. The tape forming the third layer is based on a thermoplastic resin. The tape forming the third layer is based on a resin comprising at least one of the following materials: PET, PBT, PA, polymers and copolymers. The melting points of the resins of the first and third layers are within a temperature range of 40°C. The melting point of the resin of the third layer is higher than the melting point of the resin of the first layer. - the intermediate second layer comprises or consists of fleece; The intermediate second layer is made of at least one of the following materials: polyester, polyamide, or a combination thereof. - The second layer has a weight per unit area of 50-800g / m 2 The material is The first layer of the container forms a sealing liner that will come into contact with the fluid to be stored in the container or is positioned on the outer surface of a sealing liner that will come into contact with the fluid to be stored in the container.
[0014] The invention may also relate to any other device (container) or method including any combination of the features set out above or below within the scope of the claims.
[0015] Other specific features and advantages will become apparent from the following description taken in conjunction with the drawings, in which: [Brief description of the drawings]
[0016] [Figure 1] 1 shows a schematic partial cross-sectional view illustrating an example of a structure of a container according to the invention; [Diagram 2] 1 shows schematic partial views illustrating examples of steps of a manufacturing method according to the invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The method of manufacturing a composite pressurized fluid container includes winding a first polyolefin resin-based tape to form a first layer 2 of the container.
[0018] As shown in FIG. 1, this first layer 2 can form a sealing liner that will come into contact with the fluid to be stored in the reservoir. Of course, this first layer 2 can wrap the outer surface of the sealing liner and come into contact with the fluid to be stored in the container (storage space 5). This preformed sealing liner can be made, for example, from plastic or metal. That is, the final container can be, for example, a type III, IV, or V container. As shown, the container can be provided with a base, to which a valve 6 is attached.
[0019] The first tape may be configured to form a layer that ensures the mechanical strength of the container under internal pressure.
[0020] The method then comprises depositing on the first layer 2 an intermediate second layer 3 of a material having variable permeability properties that are temperature dependent, in particular permeable below a given temperature threshold and impermeable above the temperature threshold, these permeable / impermeable states being preferably reversible.
[0021] For example, this intermediate second layer 3 comprises or consists of a breather or fleece. The intermediate second layer 3 may in particular consist of at least one of the following materials: polyester, polyamide, or a combination thereof. The intermediate second layer 3 has a weight per unit area of 50 to 800 grams / m 2 It can be said that:
[0022] This second layer is deposited over the first layer, for example by hand application, and preferably is wrinkle-resistant.
[0023] The method also includes a step of winding a second resin-based tape onto the intermediate second layer 3 to form a third layer 4. The tape forming the third layer 4 is based on a different resin than the first layer 2. The tape forming the third layer 4 is for example based on a thermoplastic resin and in particular comprises at least one of the following materials: PET, PBT, PA, polymers and copolymers.
[0024] During the steps of depositing the intermediate second layer 3 and wrapping the second tape, the intermediate second layer 3 is kept above a temperature threshold (i.e. impermeable, in particular impermeable to resins). The two resin-based layers 2, 4 are heated or kept above their melting points (e.g. via a heating element 7).
[0025] The method then includes cooling the intermediate second layer 3 to a temperature below the temperature threshold (ie, impregnated with respect to the resin) but above the melting point of the resin in the first layer 2 and the third layer 4 .
[0026] This makes it possible to achieve a mechanical bond between the first layer 2 and the third layer 4 in the second layer 3. These two resins migrate into the permeable or porous structure of the intermediate second layer 3. When the assembly is subsequently cooled, solidification ensures that the intermediate second layer 3 bonds and seals between all of the layers.
[0027] The two tapes encasing ultimately behave structurally as one entity or wall.
[0028] The resin of the third layer 4 preferably has a melting point close to that of the polyolefin resin used in the first layer 2. This allows for an airtight and structurally bonded construction of the composite container to be achieved.
[0029] For example, the melting point of the resin of the tape forming the third layer 4 preferably differs by 0 to 40 degrees from the melting point of the resin (polyolefin resin) of the layer forming the first layer 2. The melting point of the resin of the tape forming the third layer 4 preferably is higher than the melting point of the resin (polyolefin resin) of the layer forming the first layer 2.
[0030] The intermediate second layer 3 therefore enables a bond between two types of tapes made from different resins (and which may also have reinforcing fibres, preferably the same reinforcing fibres).
[0031] The resin of the second tape (optionally on the exterior surface of the container) can be a thermoplastic resin such as PET, PBT, PA, copolymers, polymers, etc. This outer layer is therefore more suitable for bonding (adhering) to other layers or accessories than layers based on polyolefin resins.
[0032] The thickness of the second layer 4 is less than the thickness of the first layer 2 .
[0033] For example, the thickness of the second layer 4 may be between 0.3 and 1.5 mm. This thickness may be uniform across the surface of the container or may vary across the surface of the container.
[0034] Thus, in one possible example, the method could proceed as follows: A first tape is wound to form a first layer 2. The intermediate second layer 3 is formed at a temperature above the temperature threshold. - A second tape is wrapped to form a third layer 4. - Cool below the temperature threshold.
[0035] Once the second tape wrapping step is complete, the assembly can be cooled, allowing the material of the middle second layer 3 to regain its permeable properties. The resin of the other two layers 2, 4 is still above its melting point and can therefore penetrate into the permeable middle second layer. The result is an entity with very high bond strength, which prevents separation unless the container wall is completely intact.
[0036] The third layer 4 may thus consist of a resin on its outer surface that is more capable of bonding with the adhesive.
[0037] The manufacturing method can be localized to a portion of the container, if desired.
[0038] The final container therefore comprises a structure incorporating an intermediate second layer 3 of a material having permeability properties that vary depending on temperature, sandwiched between two layers 2, 4, namely a first polyolefin resin-based layer 2 and a third layer 4 based on a resin different from the first layer 2, the second layer 3 being permeated with the resin from the other two layers.
Claims
1. 1. A method for manufacturing a composite container for pressurized fluid, comprising the steps of winding a first polyolefin resin-based tape to form a first layer (2) of the composite container for pressurized fluid, and depositing on said first layer (2) an intermediate second layer (3) of a material having variable permeability properties depending on temperature, in particular permeability below a predefined temperature threshold and impermeability above said temperature threshold, said method comprising winding a second resin-based tape on said intermediate second layer (3) to form a third layer (4), and depositing said third layer (5) of a material having variable permeability properties depending on temperature, in particular permeability below a predefined temperature threshold and impermeability above said temperature threshold. the tape forming the intermediate second layer (4) is based on a resin different from that of the first layer (2), and during the steps of depositing the intermediate second layer (3) and of winding the second tape, the intermediate second layer (3) is kept at a temperature higher than the threshold temperature, the method then comprising a step of cooling the intermediate second layer (3) to a temperature lower than the threshold temperature, during which the first layer (2) and the third layer (4) are each kept at a temperature higher than the melting point of their resins.
2. 10. The method of claim 1, wherein the first polyolefin resin-based tape includes reinforcing fibers, such as glass and / or carbon fibers.
3. 3. A method according to claim 1 or 2, characterized in that the thickness of the intermediate second layer (3) is less than the thickness of the first layer (2).
4. Method according to any one of claims 1 to 3, characterized in that the tape forming the third layer (4) is based on a thermoplastic resin.
5. Method according to any one of the preceding claims, characterized in that the tape forming the third layer (4) is based on a resin comprising at least one of the following materials: PET, PBT, PA.
6. The method according to any one of claims 1 to 5, characterized in that the melting points of the resins of the first layer (2) and the third layer (4) are within a temperature range of 40°C.
7. The method according to any one of claims 1 to 6, characterized in that the melting point of the resin of the third layer (4) is higher than the melting point of the first layer (2).
8. Method according to any one of the preceding claims, characterised in that the intermediate second layer (3) comprises or consists of a fleece.
9. The method according to any one of the preceding claims, characterized in that the intermediate second layer (3) consists of at least one of the following materials: polyester, polyamide, or a combination thereof.
10. The weight per unit area of the intermediate second layer (3) is 50 to 800 grams / m 2 The method according to any one of claims 1 to 9, characterized in that
11. 11. The method according to any one of claims 1 to 10, characterized in that the first layer (2) of the container forms a sealing liner that will come into contact with the fluid to be stored in the container or is positioned on the outer surface of a sealing liner that will come into contact with the fluid to be stored in the container.
Citation Information
Patent Citations
Method to produce a multi-layer composite vessel, and composite vessel obtained thereof
EP3747626A1
RESERVOIR COMPOSITE AND CONTROL AND REPAIR METHOD
FR3037633A1
BOTTLE AND STORAGE DEVICE FOR PRESSURIZED FLUID
FR3076594A1
Hard adhesive plastic adhered product and its manufacture
JP2000263671A
Filter device and method for manufacturing the same
JP2019051475A