Anti-rust paint composition, anti-rust coating film, coated product and method for producing same
A coating composition with a binder, zinc-based powder, and glass powder with a specific thermal expansion coefficient addresses the issue of zinc oxidation in high-temperature treatments, ensuring effective rust prevention and resistance to discoloration and white rust.
Patent Information
- Application Number
- JP2024100325
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Conventional inorganic zinc coating compositions lose rust-prevention properties when subjected to high-temperature heat treatments due to zinc oxidation, necessitating a coating that maintains effectiveness under such conditions.
A rust-preventing coating composition comprising a binder, zinc-based powder, and glass powder with a specific thermal expansion coefficient, which forms a film that withstands high temperatures and maintains rust-prevention properties.
The composition forms a coating film that exhibits high rust-prevention properties even after high-temperature heat treatments, resisting discoloration and white rust, and requires no secondary surface treatments.
Smart Images

Figure 0007567087000001 
Figure 0007567087000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an anti-rust paint composition, an anti-rust coating film, a coated article, and a method for producing the same. [Background technology]
[0002] In order to suppress rusting of large steel structures such as ships, marine structures, plants, tanks, and bridges, the substrate surface is usually coated with an anti-rust paint composition. Known examples of the anti-rust paint composition include organic anti-rust paint compositions such as wash primers, non-zinc epoxy primers, and epoxy zinc rich primers, as well as inorganic zinc anti-rust paint compositions containing siloxane binders and zinc powder. Among these, inorganic zinc anti-rust paint compositions are widely used (see, for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 047479 [Patent Document 2] International Publication No. 2016 / 047480 [Patent Document 3] Japanese Patent Application Publication No. 53-119932 Summary of the Invention [Problem to be solved by the invention]
[0004] A substrate coated with an inorganic zinc paint composition may be subjected to a heat treatment involving high heat, such as welding or cutting. A coating film formed from a conventional inorganic zinc paint composition tends to have zinc in the coating film oxidized and partially deactivated by such heat treatment, resulting in a decrease in rust prevention. Therefore, there is a demand for an anti-rust coating composition that can form a coating film that exhibits high rust prevention even when heated at high temperatures.
[0005] An object of the present disclosure is to provide a rust preventive paint composition capable of forming a coating film that exhibits high rust prevention performance even when heated at a high temperature.
Means for Solving the Problems
[0006] One aspect of the rust preventive paint composition of the present disclosure contains a binder (A), zinc-based powder (B), and glass powder (C) having a coefficient of thermal expansion of 120×10 -7 / °C or more.
Effects of the Invention
[0007] The rust preventive paint composition of the present disclosure can form a coating film that exhibits high rust prevention performance even when heated at a high temperature.
Modes for Carrying Out the Invention
[0008] Each component described in this specification can be used alone or in combination of two or more. In this specification, the numerical range n1~n2 means a numerical range of n1 or more and n2 or less when n1 < n2, and a numerical range of n2 or more and n1 or less when n1 > n2. In this specification, when a lower limit value and an upper limit value are each described for a certain element in a plurality, a numerical range formed by combining a value arbitrarily selected from the described lower limit values and a value arbitrarily selected from the described upper limit values is also regarded as being described.
[0009] [Rust Preventive Paint Composition] The rust preventive paint composition of the present disclosure (hereinafter also referred to as "the composition of the present disclosure") contains a binder (A), zinc-based powder (B), glass powder (C), and. Hereinafter, the coating film formed from the composition of the present disclosure is also referred to as "the rust preventive coating film of the present disclosure".
[0010] <Binder (A)> The composition of the present disclosure contains a binder (A). Examples of the binder (A) include silicon-based binders such as siloxane-based binders, butyral resins such as polyvinyl butyral resins, and (meth)acrylic resins. Among these, silicon-based binders are preferred, and siloxane-based binders are more preferred.
[0011] Examples of siloxane-based binders include alkoxysilane condensates, specifically, partial hydrolysis condensates of alkoxysilane and / or its low condensate. Alkoxysilane and / or its low condensate are also called alkyl silicates. Examples of alkoxysilane include tetraalkoxysilane and alkylalkoxysilane.
[0012] Tetraalkoxysilanes include, for example, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, and tetra-sec-butoxysilane. Examples of the alkylalkoxysilane include alkyltrialkoxysilanes, such as methyltrialkoxysilane, methyltrimethoxysilane, methyltriethoxysilane, and the like; and ethyltrialkoxysilane, such as ethyltrimethoxysilane, ethyltriethoxysilane, and the like. The number of carbon atoms in the alkoxy group contained in the alkoxysilane is preferably 1 to 5, and more preferably 1 to 3. The number of carbon atoms in the alkyl group contained in the alkylalkoxysilane is preferably 1 to 5, and more preferably 1 to 3.
[0013] Examples of the low condensation product of alkoxysilane include low condensation products of tetraalkoxysilane such as methyl polysilicate and ethyl polysilicate. The low condensation product refers to a condensation product having a condensation degree of 2 to 20 (number of silicon atoms: 2 to 20), preferably a condensation degree of 3 to 10 (number of silicon atoms: 3 to 10).
[0014] Among the alkoxysilane condensates, a condensate of tetraalkoxysilane and / or its low condensate is preferred, a condensate of tetraethoxysilane and / or its low condensate is more preferred, and a partial hydrolysis condensate of Ethyl Silicate 40 (trade name; manufactured by Colcoat Co., Ltd.), which is a low condensate of tetraethoxysilane, is particularly preferred.
[0015] The weight average molecular weight (Mw) of the siloxane binder is preferably 1,300 to 10,000, more preferably 1,400 to 8,000, and even more preferably 1,500 to 6,000. When Mw is within the above range, the paint can be cured at room temperature (e.g., 5 to 40°C) in a short time when drying, and the rust resistance of the coating film and the adhesive strength to the substrate and top coating film tend to be improved. When Mw is equal to or greater than the above lower limit, the curing reaction of the siloxane binder is fast, and even when curing is required in a short time, it is not necessary to perform heat curing at a high temperature (e.g., 200 to 400°C) when drying the coating film. When Mw is equal to or less than the above upper limit, the coating film tends to have excellent rust resistance.
[0016] The weight average molecular weight (Mw) of siloxane binders is measured by gel permeation chromatography (GPC). The value obtained by GPC is a value (polystyrene equivalent value) obtained using a calibration curve created using polystyrene as the standard substance.
[0017] The measurement conditions for the GPC method are as follows: A small amount of a binder sample is taken and diluted with tetrahydrofuran, and the solution is filtered through a membrane filter to obtain a GPC measurement sample. Equipment: Tosoh Eco SEC Elite HLC-8420GPC Column: Tosoh TSKgel Super H4000 TSKgel Super H2000 TSKgel Super H2000 The above three were connected in series and measured. Eluent: Tetrahydrofuran (THF) ·Flow rate: 0.6ml / min Column thermostat temperature: 40℃ Standard material: polystyrene
[0018] The siloxane-based binder can be produced by using a conventionally known method, for example, by subjecting an alkoxysilane and / or a low condensate thereof to a partial hydrolysis and condensation reaction in an organic solvent in the presence of an appropriate amount of water and, if necessary, a catalyst, so that the weight average molecular weight (Mw) reaches the desired value.
[0019] Examples of the organic solvent include those described in the <Organic Solvent> section below. The amount of water used is preferably 5 to 20 parts by mass, and more preferably 6 to 18 parts by mass, based on 100 parts by mass of the alkoxysilane and / or its low condensate.
[0020] Examples of the catalyst include inorganic acids such as sulfuric acid, hydrochloric acid, nitric acid, and formic acid; organic tin compounds such as dibutyltin dilaurate, dibutyltin dimaleate, dioctyltin dilaurate, dioctyltin dimaleate, dioctyltin maleate, and tin octoate; phosphoric acid, monomethyl phosphate, monoethyl phosphate, monobutyl phosphate, monooctyl phosphate, monodecyl phosphate, dimethyl phosphate, diethyl phosphate, dibutyl phosphate, dioctyl phosphate, and didecyl phosphate; Examples of suitable organic acids include phosphoric acid or phosphoric acid esters; organic titanate compounds such as diisopropoxybis(acetylacetate)titanium and diisopropoxybis(ethylacetoacetate)titanium; organic aluminum compounds such as tris(ethylacetoacetate)aluminum and tris(acetylacetonate)aluminum; and organic zirconium compounds such as tetrabutyl zirconate, tetrakis(acetylacetonate)zirconium, tetraisobutyl zirconate, and butoxytris(acetylacetonate)zirconium. Among these, inorganic acids are preferred, and hydrochloric acid is more preferred, in view of the good storage stability of the first agent described below.
[0021] When a catalyst is used, the amount thereof is preferably 0.01 to 2.0 parts by mass, and more preferably 0.01 to 1.0 part by mass, based on 100 parts by mass of the alkoxysilane and / or its low condensate.
[0022] The binder (A) may be one type or two or more types. The content of the binder (A) is preferably 1 to 30 mass%, more preferably 2 to 25 mass%, further preferably 3 to 20 mass%, and particularly preferably 5 to 15 mass%, in the solid content of the composition of the present disclosure. The content of the component derived from the binder (A) is preferably 1 to 30 mass%, more preferably 2 to 25 mass%, further preferably 3 to 20 mass%, and particularly preferably 5 to 15 mass%, in the rust-preventive coating film formed from the composition of the present disclosure. When the binder (A) is a siloxane-based binder, the content of the binder (A) or a component derived therefrom is calculated by multiplying the mass of the siloxane-based binder by the amount of SiO 2 (i.e., the mass of the siloxane binder is converted to the mass of SiO 2 The mass of the material is calculated by converting the mass of the material into the mass of the material.
[0023] The solid content of a substance (e.g., a composition or a contained ingredient) refers to the heating residue when the substance is dried in an incubator at 125°C for 1 hour in accordance with the standard JIS K5601-1-2:2008. Specifically, the heating residue is the residue of the sample (including the residue attached to the wire) obtained by weighing out 1.0 g of the substance sample onto a flat-bottom dish, spreading it evenly using a wire of known mass, and drying it in an incubator at 1 atmosphere and 125°C for 1 hour.
[0024] <Zinc-based powder (B)> The composition of the present disclosure contains a zinc-based powder (B). The zinc-based powder (B) acts, for example, as an anti-rust pigment that inhibits rusting of steel materials.
[0025] Examples of the zinc-based powder (B) include zinc powder and zinc alloy powder. Examples of the zinc alloy include an alloy of zinc and at least one selected from the group consisting of aluminum, magnesium, and tin, specifically, an alloy of zinc and aluminum, and an alloy of zinc and tin.
[0026] The shape of the particles constituting the zinc-based powder (B) can be, for example, spherical, scaly, or other various shapes. That is, the zinc-based powder (B) can be, for example, a spherical zinc-based powder and a scaly zinc-based powder. As the zinc-based powder (B), one or both of zinc powder and zinc alloy powder can be used.
[0027] The particles constituting the flaky zinc-based powder preferably have a median diameter (D50) of 30 μm or less and an average thickness of 1 μm or less, more preferably a D50 of 5 to 20 μm and an average thickness of 0.2 to 0.9 μm. The aspect ratio (D50 / average thickness), which is the ratio of D50 to the average thickness, is preferably 10 to 150, more preferably 20 to 100.
[0028] The particles constituting the spherical zinc-based powder preferably have a D50 of 2 to 15 μm, more preferably a D50 of 2 to 7 μm. The aspect ratio of the particles constituting the spherical zinc-based powder is preferably 1 to 3. The spherical zinc-based powder is less expensive than the flaky zinc-based powder, and its use can reduce the cost of the coating composition.
[0029] The median diameter is calculated from the volumetric particle size distribution obtained using a laser scattering diffraction type particle size distribution measuring device, for example, "SALD 2200" (product name; manufactured by Shimadzu Corporation). The average thickness is calculated by observing the zinc-based powder using a scanning electron microscope (SEM), for example, "XL-30" (product name; manufactured by Philips), measuring the thicknesses of several tens to several hundreds of powder particles, and calculating the average value.
[0030] The zinc-based powder (B) may be of one type or of two or more types. The content of the zinc-based powder (B) in the solid content of the composition of the present disclosure or in the rust-preventive coating film formed from the composition is preferably 10 to 90 mass%, more preferably 20 to 80 mass%, and even more preferably 25 to 70 mass%. Such a composition can form a coating film with excellent rust prevention and weldability.
[0031] <Glass powder (C)> The composition of the present disclosure contains a glass powder (C). It is believed that the glass powder (C) acts as a component that inhibits oxidation of the zinc-based powder (B) when the coating film is heated at high temperatures (e.g., 400 to 900°C) and contributes to maintaining the rust prevention properties of the coating film.
[0032] Glass powder (C) is 120 x 10 -7 / °C or higher. For example, a substrate coated with an inorganic zinc paint composition may be subjected to a heat treatment involving high heat, such as welding or cutting. The composition of the present disclosure can form a coating film that exhibits high rust prevention properties even when placed outdoors or in a corrosive environment after high-temperature heat treatment. That is, the rust-preventive coating film of the present disclosure exhibits high rust prevention properties even when placed outdoors or in a corrosive environment after high-temperature heat treatment.
[0033] The reason why the composition of the present disclosure has such an excellent effect is unclear, but the present inventors speculate as follows. The above-mentioned thermal expansion coefficient is the rate at which the length of a substance increases when the temperature rises. The thermal expansion coefficient is a physical property inherent to a substance. For example, when two materials with similar thermal expansion coefficients are bonded together, they tend to expand or contract in response to a temperature change. On the other hand, when two materials with a large difference in thermal expansion coefficients are bonded together, they tend to peel off when a temperature change occurs. Glass powder (C) is 120 x 10 -7 The thermal expansion coefficient of the glass powder (C) is 120×10 -7Compared with the thermal expansion coefficient of less than 1000 / °C, the thermal expansion coefficient of the glass powder (C) is relatively close to that of the zinc-based powder (B). This allows the glass powder (C) to easily follow the expansion or contraction of the zinc-based powder (B) due to temperature changes, and the glass powder (C) can cover the surface of the zinc-based powder (B) during the heat treatment and the subsequent cooling treatment, thereby effectively suppressing its oxidation. Therefore, even if placed outdoors or in a corrosive environment after heat treatment at high temperatures, the rust-preventive coating film of the present disclosure exhibits high rust prevention properties. However, the above explanation is merely speculation and does not limit the contents of the present disclosure in any way.
[0034] The composition of the present disclosure can form a coating film that is resistant to discoloration when subjected to heat treatment at high temperatures. That is, the rust-preventive coating film of the present disclosure exhibits heat discoloration resistance, that is, is resistant to discoloration (small change in hue) when subjected to heat treatment at high temperatures.
[0035] The composition of the present disclosure can form a coating film that is less likely to develop white rust even when placed outdoors or in a corrosive environment after heat treatment at high temperatures. That is, the rust-preventive coating film of the present disclosure exhibits heat-resistant white rust resistance, that is, it is less likely to develop white rust even when placed outdoors or in a corrosive environment after heat treatment at high temperatures. In a conventional rust-preventive coating film, a portion that has been heat-treated at high temperatures is more likely to develop white rust when placed outdoors or in a corrosive environment. For this reason, a secondary surface treatment is required to remove white rust. The rust-preventive coating film of the present disclosure generates little white rust even when heated at high temperatures. Therefore, the above-mentioned secondary surface treatment can be eliminated.
[0036] A topcoat coating film may be provided on the rust-preventive coating film of the present disclosure. A laminated coating film having the rust-preventive coating film of the present disclosure and the topcoat coating film also exhibits high rust prevention properties even when placed outdoors or in a corrosive environment after heat treatment, or when exposed to a high-temperature environment.
[0037] The reason why the above-mentioned effects on heat discoloration resistance, heat white rust resistance and rust prevention properties of the laminated coating film are exhibited is presumably because, similarly to the reason mentioned above, oxidation of the zinc-based powder (B) during heat treatment can be suppressed.
[0038] The thermal expansion coefficient of the glass powder (C) is preferably 130×10-7 / ℃ or more, more preferably 140×10 -7 / ℃ or more, more preferably 145×10 -7 / °C or more, and particularly preferably 150×10 -7 / ℃ or higher. The thermal expansion coefficient of the glass powder (C) is preferably 220×10 -7 / ℃ or less, more preferably 210×10 -7 / ℃ or less, more preferably 200×10 -7 / °C or less, and even more preferably 195×10 -7 / ℃ or less, and particularly preferably 190×10 -7 / ℃ or less. Thermal expansion coefficient of glass powder (C) (unit: 10 -7 / °C) is preferably 120 to 220, more preferably 130 to 210, even more preferably 140 to 200, still more preferably 145 to 195, and particularly preferably 150 to 190.
[0039] The thermal expansion coefficient is measured using a push rod dilatometer or a thermomechanical analyzer (TMA). With a push rod dilatometer, the target sample is heated at 5°C per minute in the temperature range from 23°C to the yield point, and the average linear thermal expansion coefficient between 100 and 300°C is calculated. With a TMA, the target sample is heated at 5°C per minute in the temperature range from 23°C to the yield point, and the average linear thermal expansion coefficient between 50 and 300°C is calculated. In this specification, the thermal expansion coefficient of the glass powder (C) is the average linear thermal expansion coefficient obtained by the first measurement method using a push rod type thermal dilatometer, and when the first measurement method is difficult to apply, the average linear thermal expansion coefficient is the average linear thermal expansion coefficient obtained by the second measurement method using TMA. In either measurement method, when the glass transition temperature is lower than 350°C, the upper limit temperature for calculating the average linear thermal expansion coefficient is set to a temperature 50°C lower than the glass transition temperature, and the average linear thermal expansion coefficient is calculated.
[0040] The softening point of the glass powder (C) is preferably 480°C or less, more preferably 470°C or less, even more preferably 460°C or less, and even more preferably 450°C or less. The softening point of the glass powder (C) is particularly preferably 440°C or less, particularly preferably 430°C or less, and most preferably 420°C or less, and may be, for example, less than 400°C or 398°C or less. The softening point of the glass powder (C) is preferably 200°C or more, more preferably 250°C or more, even more preferably 300°C or more, and particularly preferably 350°C or more. By using the glass powder (C) having the above thermal expansion coefficient, even if the glass powder (C) has a softening point in the above range, the obtained anti-rust coating film can exhibit excellent anti-rust properties.
[0041] The softening point of the glass powder (C) is preferably 200 to 480°C, more preferably 250 to 470°C, even more preferably 300 to 460°C, still more preferably 350 to 450°C, particularly preferably 350 to 440°C, particularly preferably 350 to 430°C, and most preferably 350 to 420°C, and may be, for example, 350°C or higher but lower than 400°C, or 350°C or higher but 398°C or lower.
[0042] The softening point is measured using a push rod dilatometer or thermogravimetric differential thermal analysis (TG-DTA). With a push rod dilatometer, the softening point is the temperature at which the thermal expansion curve is at its maximum. With TG-DTA, the sample is heated at 10°C per minute in air to measure the DTA curve, and the softening point is the temperature of the fourth inflection point on the DTA curve. In this specification, the softening point of the glass powder (C) is a value obtained by a first measurement method using a push rod type thermal dilatometer, and when the first measurement method is difficult to apply, is a value obtained by a second measurement method using TG-DTA.
[0043] The components constituting the glass powder (C) include, for example, SiO 2 , B 2 O 3 , Al 2 O 3 , ZnO, BaO, MgO, CaO, SrO, Bi 2 O 3 , Li2 O, Na 2 OK 2 O, PbO, P 2 O 5 , In 2 O 3 , SnO, CuO, Ag 2 O, V 2 O 5 , and TeO 2 Although PbO can also be used as a compound constituting the glass powder (C), from the viewpoint of low environmental pollution, it is preferable that the glass powder (C) does not contain PbO.
[0044] The thermal expansion coefficient and softening point of the glass powder (C) can be appropriately adjusted, for example, by the type, combination and content ratio of the components constituting the glass powder (C). The glass powder (C) can be obtained, for example, by heating and melting the compounds constituting the glass at about 1000 to 1100°C for a predetermined time, cooling, and then granulating the resulting mixture into a powder shape using a grinding device.
[0045] The median diameter (D50) of the glass powder (C) is preferably 1 to 30 μm, more preferably 1.5 to 25 μm, and further preferably 2 to 20 μm. The median diameter is calculated from the volume-based particle size distribution obtained using a laser scattering diffraction type particle size distribution measuring device, for example, "SALD 2200" (product name; manufactured by Shimadzu Corporation).
[0046] The content of the glass powder (C) in the solid content of the composition of the present disclosure or in the anticorrosive coating film formed from the composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 15 mass%, and even more preferably 0.2 to 10 mass%. Such a composition and anticorrosive coating film tend to exhibit the above-mentioned effects more satisfactorily.
[0047] In the composition of the present disclosure or the rust-preventive coating film formed from the composition, the ratio of the content of the glass powder (C) to the content of the zinc-based powder (B) ((C) / (B)) is preferably 0.005 to 0.10, more preferably 0.010 to 0.09, and even more preferably 0.013 to 0.08, based on mass. Such a composition and rust-preventive coating film tend to be able to exhibit the above-mentioned effects more satisfactorily.
[0048] <Pigment components> The composition of the present disclosure may further contain, for example, a pigment component other than the zinc-based powder (B) and the glass powder (C). Examples of the pigment component include a metal-based powder other than the zinc-based powder (B), an anti-rust pigment other than the zinc-based powder (B), an inorganic powder other than the zinc-based powder (B), molybdenum, a molybdenum compound, an extender pigment, and a color pigment. The pigment component may be one type or two or more types.
[0049] Metal-based powders other than the zinc-based powder (B) have electrical conductivity and facilitate the movement of iron ions or zinc ions to enhance the rust-preventive effect of the coating film. Examples of the metal-based powder include metal powders and metal alloy powders. Examples of the metal-based powder include Fe-Si powder, Fe-Mn powder, Fe-Cr powder, magnetic iron powder, and iron phosphide powder.
[0050] From the viewpoint of further improving the rust prevention of the coating film, the composition of the present disclosure may further contain an anti-rust pigment other than the zinc-based powder (B). Examples of the anti-rust pigment include zinc phosphate compounds, calcium phosphate compounds, aluminum phosphate compounds, magnesium phosphate compounds, zinc phosphite compounds, calcium phosphite compounds, aluminum phosphite compounds, strontium phosphite compounds, aluminum tripolyphosphate compounds, zinc cyanamide compounds, borate compounds, nitro compounds, and composite oxides.
[0051] Examples of inorganic powders other than the zinc-based powder (B) include zinc compound powders (excluding zinc phosphate-based compounds, zinc phosphite-based compounds, and zinc cyanamide-based compounds), and inorganic compound powders that generate gas upon thermal decomposition.
[0052] Zinc compound powder is the ionized form of zinc-based powder (B) (Zn 2+ It is believed that the zinc compound has the effect of adjusting the activity of oxidation reactions, such as the degree of oxidation reaction (the formation of zinc oxide, zinc chloride, zinc sulfide, zinc sulfate, etc.). The above composition containing the zinc compound powder has even better rust prevention properties. Examples of the zinc compound powder include zinc oxide, zinc chloride, zinc sulfide, and zinc sulfate.
[0053] The composition of the present disclosure will be described below in the case where it contains a zinc compound powder. The content of the zinc compound powder in the solid content of the composition or in the rust-preventive coating film formed from the composition is preferably 0.1 to 20 mass%, more preferably 0.2 to 15 mass%, and even more preferably 0.3 to 10 mass%.
[0054] Inorganic powders that generate gases by pyrolysis are compounds that generate gases (e.g., CO) by pyrolysis (e.g., pyrolysis at 500 to 1,500°C). 2 , F 2 ) is a powder of an inorganic compound that generates the above-mentioned. By using the above-mentioned inorganic compound powder, bubbles generated from gas generated from organic components contained in the binder (A) and the like in the molten pool during welding of a coated product can be removed from the molten pool together with the gas derived from the above-mentioned inorganic compound powder. Examples of the above-mentioned inorganic compound powder include calcium fluoride, calcium carbonate, magnesium carbonate, and strontium carbonate.
[0055] The composition of the present disclosure will be described below in the case where it contains an inorganic compound powder that generates a gas upon thermal decomposition. The content of the inorganic compound powder that generates a gas upon thermal decomposition is preferably 0.1 to 8 mass %, more preferably 0.2 to 4 mass %, in the solid content of the composition or in the rust-preventive coating film formed from the composition.
[0056] The composition of the present disclosure may further contain at least one component selected from the group consisting of molybdenum (metallic molybdenum) and molybdenum compounds (hereinafter also referred to as "molybdenum component"). The molybdenum component acts as an antioxidant (so-called white rust inhibitor) for the zinc-based powder (B) to reduce the occurrence of white rust in the coating film.
[0057] Examples of the molybdenum compound include molybdenum oxides such as molybdenum trioxide, molybdenum sulfide, molybdenum halides, metal salts of molybdic acid such as molybdic acid, ammonium molybdate, phosphomolybdic acid, silicomolybdic acid, and zinc molybdate, alkali metal salts of molybdic acid, alkali metal salts of phosphomolybdic acid, alkali metal salts of silicomolybdic acid, alkaline earth metal salts of molybdic acid such as calcium molybdate, alkaline earth metal salts of phosphomolybdic acid, alkaline earth metal salts of silicomolybdic acid, manganese salts of molybdic acid, manganese salts of phosphomolybdic acid, manganese salts of silicomolybdic acid, basic nitrogen-containing compound salts of molybdic acid, basic nitrogen-containing compound salts of phosphomolybdic acid, and basic nitrogen-containing compound salts of silicomolybdic acid.
[0058] The case where the composition of the present disclosure contains a molybdenum component will be described. The content of the molybdenum component is preferably 0.05 to 5.0 parts by mass, more preferably 0.3 to 3.0 parts by mass, and even more preferably 0.5 to 2.0 parts by mass, relative to 100 parts by mass of the zinc-based powder (B). Such a composition can sufficiently suppress the oxidation of the zinc-based powder (B) and can form a coating film with excellent rust prevention properties.
[0059] The composition of the present disclosure may further contain a body pigment. The body pigment is not particularly limited as long as it is an inorganic pigment used as a component of general paints, and examples thereof include potassium feldspar, soda feldspar, kaolin, mica, silica, talc, barium sulfate, aluminum oxide, zirconium silicate, wollastonite, and diatomaceous earth. The body pigment may be an inorganic pigment that generates gas by thermal decomposition.
[0060] The case where the composition of the present disclosure contains an extender pigment will be described below. The content of the extender pigment in the solid content of the composition or in the rust-preventive coating film formed from the composition is preferably 0.1 to 60 mass %, more preferably 1 to 50 mass %, and even more preferably 5 to 40 mass %.
[0061] The composition of the present disclosure may further contain a color pigment. The color pigment can, for example, impart a desired hue to the coating film. Examples of the color pigment include inorganic pigments such as titanium oxide, red iron oxide, iron oxide, iron hydroxide, carbon black, copper chromium, ultramarine blue, iron oxide-manganese oxide, iron oxide-chromium oxide, iron oxide-cobalt oxide-chromium oxide, copper oxide-magnesium oxide, manganese oxide-bismuth oxide, and manganese oxide-yttrium oxide; and organic pigments such as phthalocyanine green and phthalocyanine blue.
[0062] The composition of the present disclosure containing a color pigment will be described below. The content of the color pigment in the solid content of the composition or in the rust-preventive coating film formed from the composition is preferably 0.1 to 20 mass%, more preferably 0.2 to 15 mass%, and even more preferably 0.3 to 10 mass%.
[0063] <Additives> The composition of the present disclosure may further contain additives. Additives are materials used to improve or maintain the performance of a paint or coating film. Examples of additives include anti-settling agents, thickeners, anti-sagging agents, drying agents, flow control agents, defoamers, dispersants, color separation inhibitors, skinning inhibitors, plasticizers, and ultraviolet absorbers. The additive may be of one type or of two or more types.
[0064] Examples of anti-settling agents include organic bentonite-based anti-settling agents, polyethylene oxide-based anti-settling agents, fumed silica-based anti-settling agents, and amide-based anti-settling agents. The anti-settling agent may be one type or two or more types. The composition of the present disclosure containing an anti-settling agent will be described below. The content of the anti-settling agent in the solid content of the composition or in the anti-rust coating film formed from the composition is preferably 0.5 to 8 mass %, more preferably 1 to 6 mass %.
[0065] Examples of the thickening agent include known thickening agents such as tricalcium phosphate. The thickener may be one type or two or more types. The composition of the present disclosure containing a thickener will be described below. The content of the thickener in the solid content of the composition or in the rust-preventive coating film formed from the composition is preferably 0.5 to 8 mass %, more preferably 1 to 6 mass %.
[0066] <Organic solvent> The composition of the present disclosure may further contain an organic solvent. Such a composition has excellent dispersibility of each component such as the zinc-based powder (B), has good compatibility with the substrate during coating, and can form a coating film with excellent adhesion to the substrate.
[0067] Examples of the organic solvent include organic solvents that are commonly used in the field of paints, such as alcohol-based solvents, ester-based solvents, ketone-based solvents, aromatic solvents, and glycol-based solvents.
[0068] Examples of the alcohol-based solvent include methanol, ethanol, propanol, and butanol. Examples of the ester-based solvent include ethyl acetate and butyl acetate. Examples of the ketone-based solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Examples of the aromatic solvent include benzene, xylene, and toluene. Examples of the glycol-based solvent include propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate. The organic solvent may be one type or two or more types.
[0069] The composition of the present disclosure contains an organic solvent in an amount of preferably 20 to 90% by mass, more preferably 25 to 85% by mass, and further preferably 30 to 80% by mass.
[0070] <Form of Antirust Coating Composition> The composition of the present disclosure may be, for example, a sachet type composition having a first agent containing a binder (A) and a second agent containing a zinc-based powder (B) and a glass powder (C), a sachet type composition having a first agent containing a binder (A) and a glass powder (C) and a second agent containing a zinc-based powder (B), or a sachet type composition having a first agent containing a binder (A), a second agent containing a zinc-based powder (B), and a third agent containing a glass powder (C). The sachet type composition may further have another agent containing at least one component selected from the group consisting of the above-mentioned components.
[0071] Each agent, such as the first agent, the second agent, the third agent, and other agents, is usually stored, preserved, or transported in a separate container. At the time of use (e.g. immediately before painting), the mixture obtained by mixing the first agent, the second agent, and other agents used as needed, or the first agent, the second agent, the third agent, and other agents used as needed, is used.
[0072] The composition of the present disclosure may be, for example, a two-part composition consisting of a liquid first part and a powder, paste or liquid second part. The composition of the present disclosure may be, for example, a three-part composition consisting of a liquid first part, a powder, paste or liquid second part, and a powder, paste or liquid third part.
[0073] The first agent contains a binder (A) and preferably further contains an organic solvent. The first agent may further contain a glass powder (C). The first agent may further contain at least one selected from the group consisting of the pigment components and additives described above. The first agent may be in a liquid form or a paste form, and is preferably in a liquid form.
[0074] The case where the first agent contains a siloxane-based binder as the binder (A) will be described. The first agent may be prepared, for example, by mixing a siloxane-based binder with an organic solvent. The first agent may be prepared, for example, by adding hydrochloric acid or the like to a mixed solution of at least one selected from the group consisting of alkoxysilanes and their low condensates and an organic solvent, and stirring the mixture to generate a partial hydrolysis condensate.
[0075] The second agent contains a zinc-based powder (B) and preferably further contains an organic solvent. The second agent may further contain a glass powder (C). The second agent may further contain at least one selected from the group consisting of the pigment components and additives described above. The second agent may be in a liquid, paste, or powder form, preferably in a paste or powder form, and more preferably in a paste form.
[0076] The third agent contains a glass powder (C) and preferably further contains an organic solvent. The third agent may further contain at least one selected from the group consisting of the pigment components and additives described above. The third agent may be in the form of a liquid, a paste, or a powder, preferably in the form of a paste or powder, and more preferably in the form of a paste.
[0077] The content ratio of each component contained in the first agent can be appropriately set so that the content ratio of each component in the coating composition or its solid content when the coating composition is prepared by mixing each agent such as the first agent and the second agent falls within the above-mentioned range. The same applies to the content ratio of each component contained in the second agent and the content ratio of each component contained in the third agent.
[0078] The first agent, for example, when it is a mixture, can be prepared by mixing the respective components to be blended. The second agent, for example, when it is a mixture, can be prepared by mixing the respective components to be blended. The third agent, for example, when it is a mixture, can be prepared by mixing the respective components to be blended. When mixing, each component may be added at once or may be added in several portions.
[0079] <Preparation of Antirust Coating Composition> The composition of the present disclosure can be prepared, for example, by mixing the binder (A), the zinc-based powder (B), the glass powder (C), and, if necessary, other components, such as the pigment components, additives, and organic solvents described above.
[0080] In the case of the above-mentioned divided-package composition, the first agent, the second agent, and optionally other agents are mixed before coating the substrate to obtain a coating composition. The mixing ratio of each agent can be appropriately set so that the content ratio of each component after mixing falls within the above-mentioned range. The obtained coating composition is used to coat the substrate.
[0081] When mixing, a conventionally known device such as a mixer, disperser, or stirrer can be used. Examples of the device include a disperser, a mixing / dispersing mill, a mortar mixer, a roll, a paint shaker, and a homogenizer. Mixing may be performed while heating or cooling depending on the season or environment.
[0082] The composition of the present disclosure may be diluted before use depending on the coating method, etc. All descriptions in this specification, except for those related to such dilution, are descriptions of the composition before dilution.
[0083] [Anti-rust coatings and painted products] The anti-rust coating film of the present disclosure is formed from the composition of the present disclosure. The coated article of the present disclosure has a substrate and the anti-rust coating film of the present disclosure provided on the substrate. For example, the composition of the present disclosure can be applied to the substrate and cured to obtain the anti-rust coating film and coated article of the present disclosure.
[0084] The anticorrosive coating film of the present disclosure contained in the above-mentioned coated article may consist of one layer, or two or more layers. The average thickness of the rust-preventive coating film of the present disclosure is preferably 1 to 100 μm, more preferably 3 to 80 μm, further preferably 5 to 60 μm, and particularly preferably 7 to 40 μm. The average thickness is measured using an electromagnetic coating thickness meter. The rust-preventive coating film having the above average thickness may be formed by one coating, or may be formed by two or more coatings.
[0085] Examples of the material of the substrate include iron and steel (e.g., iron, steel, ferroalloy, carbon steel, mild steel, alloy steel, stainless steel) and non-ferrous metals (e.g., zinc, aluminum, copper, brass, zinc plating, zinc spraying), as well as plastics (e.g., polypropylene, polyamide, polycarbonate, polyurethane, polyester, polystyrene, polyvinyl chloride resin), ceramics, glass, and concrete. Among these, iron and steel are preferred.
[0086] Specific examples of the substrate include ships (e.g., ship decks, superstructures or outer hulls, engines, chimneys, etc.), marine structures (e.g., marine buoys, undersea pipelines), structures (e.g., plants, tanks, containers), bridges, and outdoor equipment (e.g., guard fences, industrial machinery). Steel structures are preferred as substrates.
[0087] The substrate may be a substrate that has been pretreated by a cleaning treatment for removing rust, dirt, coating film (old coating film), etc., attached to the substrate, or a blasting treatment, etc. If necessary, the substrate may be blasted under conditions equivalent to a rust removal degree Sa2 1 / 2 or more in ISO 8501-1.
[0088] The coated article of the present disclosure may have an additional coating film (hereinafter also referred to as "topcoat coating film") on the rust-preventive coating film of the present disclosure. That is, the coated article of the present disclosure may have a substrate, the rust-preventive coating film of the present disclosure, and a topcoat coating film in this order. Examples of the topcoat coating film include silicone resin-based, epoxy resin-based, epoxy ester resin-based, polyurethane resin-based, fluororesin-based, (meth)acrylic resin-based, vinyl resin-based, chlorinated rubber-based, or inorganic zinc-based coating films. The average thickness of the topcoat coating film is not particularly limited, but is preferably 1 to 100 μm, more preferably 3 to 90 μm, and even more preferably 5 to 80 μm.
[0089] The coated article of the present disclosure can be produced, for example, by a method having a step of applying the composition of the present disclosure to a substrate and curing the composition to form an anti-rust coating film. Specifically, the coated article of the present disclosure can be produced by a method having a step of applying the composition of the present disclosure to a substrate to form an uncured coating film, and a step of curing the coating film to form an anti-rust coating film.
[0090] First, the composition of the present disclosure (in the case of a packaged composition, a composition obtained by mixing each agent such as the first agent and the second agent) is applied to a substrate to form an uncured coating film. Examples of methods for applying the composition include air spray coating, airless spray coating, roll coater coating, brush coating, and dip coating. When coating a substrate at a shipyard or steelworks, a line coater may be used as the coater. The line coater controls the film thickness by coating conditions such as the line speed, the coating pressure of the air spray or airless spray installed inside the coater, and the size (diameter) of the spray tip.
[0091] Next, the composition or the coating film is cured. The curing temperature (drying temperature) is preferably 5 to 40° C., more preferably 10 to 30° C., and may be, for example, ambient temperature. The curing time (drying time) is usually 3 minutes to 100 hours, preferably 5 minutes to 60 hours.
[0092] The method for curing the composition or the coating film is not particularly limited, and a conventionally known curing method may be adopted. For example, a composition containing a siloxane-based binder as the binder (A) will be described. When the composition applied to the substrate is left in air (with heating as necessary), the organic solvent evaporates, and the siloxane-based binder undergoes a hydrolysis and condensation reaction with the water in the composition or the moisture (humidity) in the air, thereby curing.
[0093] As described above, the coated article of the present disclosure has excellent rust prevention, heat discoloration resistance, and heat white rust resistance even when subjected to heat treatment (for example, heat treatment at high temperatures such as 400 to 900°C). For example, anti-rust paints used in steel processing processes and the like are required to protect steel from rust without interfering with melting, welding, and the like in the construction process, and are also required to have small changes in hue due to oxidation of zinc during heat treatment. For this reason, the composition of the present disclosure is suitable as an anti-rust paint used in steel processing processes and the like.
[0094] [Example of the situation] The present disclosure relates to, for example, the following [1] to
[12] . [1] Binder (A), zinc-based powder (B), and 120×10 -7 and a glass powder (C) having a thermal expansion coefficient of at least 1 / °C. [2] The rust-preventive coating composition according to [1] above, wherein the glass powder (C) has a softening point of 480° C. or lower. [3] The thermal expansion coefficient of the glass powder (C) is 120×10 -7 / ℃~220×10 -7 / °C. The anticorrosive coating composition according to [1] or [2] above. [4] The rust-preventive coating composition according to any one of the above [1] to [3], wherein the binder (A) is a siloxane-based binder. [5] The rust-preventive coating composition according to [4], wherein the siloxane-based binder is a condensate of at least one compound selected from the group consisting of tetraalkoxysilanes and alkyltrialkoxysilanes. [6] The rust-preventive coating composition according to [4] or [5] above, wherein the siloxane-based binder has a weight-average molecular weight (Mw) of 1,300 to 10,000. [7] The anti-rust coating composition according to any one of [1] to [6], wherein the content of the binder (A) is 1 to 30 mass%, the content of the zinc-based powder (B) is 10 to 90 mass%, and the content of the glass powder (C) is 0.01 to 20 mass%, based on the solid content of the anti-rust coating composition. [8] The rust-preventive coating composition according to any one of [1] to [7], wherein a ratio ((C) / (B)) of the content of the glass powder (C) to the content of the zinc-based powder (B) is 0.005 to 0.10 by mass. [9] The rust-preventive coating composition according to any one of the above items [1] to [8], which is a sachet-type composition having a first agent containing the binder (A) and a second agent containing the zinc-based powder (B) and the glass powder (C), a sachet-type composition having a first agent containing the binder (A) and the glass powder (C) and a second agent containing the zinc-based powder (B), or a sachet-type composition having a first agent containing the binder (A), a second agent containing the zinc-based powder (B), and a third agent containing the glass powder (C).
[10] An anti-rust coating film formed from the anti-rust coating composition according to any one of [1] to [9] above.
[11] A coated article having a substrate and the rust-preventive coating film according to
[10] provided on the substrate.
[12] A method for producing a coated product, comprising the steps of applying the anti-rust coating composition according to any one of [1] to [9] above to a substrate and curing the composition to form an anti-rust coating film. EXAMPLES
[0095] The composition of the present disclosure will be described in more detail below by way of examples, but the composition of the present disclosure is not limited to these examples.
[0096] [raw materials] The raw materials used in the examples and comparative examples are listed below. Alkyl silicate Ethyl silicate 40, manufactured by Colcoat Co., Ltd. ·Anti-settling agent AEROESIL 200, manufactured by Nippon Aerosil Co., Ltd. ·Thickener Tricalcium phosphate, manufactured by Taihei Chemical Industry Co., Ltd. Zinc oxide Three types of zinc oxide, manufactured by Hakusui Tech Co., Ltd. Potassium feldspar Feldspar PG-K10, manufactured by Sibelco ·Black pigment Dipyroxide Black #9510, manufactured by Dainichi Seika Color & Chemicals Co., Ltd. ·Zirconium Silicate A-PAX 45M, manufactured by Kinsei Matec Co., Ltd. Zinc powder Larvik Superfine 25, made by EverZinc Particle size (D50): 4.2μm Glass powder CY5401, manufactured by Takara Standard Co., Ltd. Softening point: 641℃, Thermal expansion coefficient: 67×10 -7 / ℃ Composition: SiO 2 -B 2 O 3 , particle size (D50): 10μm Glass powder TMX-302F, manufactured by TOMATEC Co., Ltd. Softening point: 490℃, Thermal expansion coefficient: 88×10 -7 / ℃ Composition: ZnO-B 2 O 3 -Bi 2 O 3 , particle size (D50): 2μm Glass powder TMX-501F, manufactured by TOMATEC Co., Ltd. Softening point: 545℃, Thermal expansion coefficient: 79×10 -7 / ℃ Composition: Bi 2 O 3 -ZnO-B 2 O 3 , particle size (D50): 2μm Glass powder 01-4102P, manufactured by TOMATEC Co., Ltd. Softening point: 384℃, Thermal expansion coefficient: 166×10 -7 / ℃ Composition: P-Al-B-Na-KF, particle size (D50): 9μm Glass powder VY0047M2, manufactured by Takara Standard Co., Ltd. Softening point: 420℃, Thermal expansion coefficient: 177×10 -7 / ℃ Composition:P 2 O 5 -Al 2 O 3 -R 2 O, particle size (D50): 9μm Glass powder VY0144, manufactured by Takara Standard Co., Ltd. Softening point: 404℃, Thermal expansion coefficient: 163×10 -7 / ℃ Composition:P 2 O 5 -Al 2 O 3 -R 2 O, particle size (D50): 10μm (R 2 O is Li 2 O, Na 2 O and K 2 O represents an alkali metal oxide.
[0097] [Preparation Example 1] 55g of ethyl silicate 40, 25g of ethanol, 5g of deionized water, and 0.03g of 35% hydrochloric acid were placed in a container. The mixture in the container was stirred at 50°C for 3 hours, and then 15g of isopropyl alcohol was added to the mixture to obtain a solution of alkyl silicate condensate (Mw: 1,700) (hereinafter also referred to as "Solution A").
[0098] [Preparation Example 2] 31.5 g of ethyl silicate 40, 13.4 g of isobutyl alcohol, 5 g of deionized water, and 0.05 g of 35% hydrochloric acid were charged into a container. The mixture in the container was stirred at 50° C. for 3 hours, and then 50 g of isopropyl alcohol was added to the mixture to obtain a solution of alkyl silicate condensate (Mw: 3,000) (hereinafter also referred to as “Solution B”).
[0099] [Preparation Example 3. Paste] The raw materials (except zinc powder) shown as the pastes in Table 1 were each placed in a polyethylene container, glass beads were added, and the mixture was shaken for about 2 hours using a paint shaker. Next, zinc powder was added to the polyethylene container, and the mixture was shaken for 10 minutes using a paint shaker. Next, the glass beads were removed using a 120 mesh filter, and a paste was obtained.
[0100] [Examples 1 to 7 and Comparative Examples 1 to 4] In the examples and comparative examples shown in Table 1, a coating composition was obtained by mixing solution A of the alkyl silicate condensate and a pasting agent in the ratio shown in Table 1. In the examples and comparative examples shown in Table 2, solution B of the alkyl silicate condensate, zinc powder, and glass powder were mixed in the ratio shown in Table 2, and the resulting mixture was stirred for about 1 minute to obtain a coating composition.
[0101] [Evaluation test] <Preparation of test plate> A sandblasted plate (JIS G3101:2024, SS400, dimensions: 150mm x 70mm x 2.3mm) was prepared. The blasted surface of the sandblasted plate was painted with an air spray using the coating composition of the example or comparative example. The painted sandblasted plate was then aged for one week in a thermostatic chamber at a temperature of 23°C and a relative humidity of 50% in accordance with the JIS K5600-1-6:1999 standard. In this way, a test plate having a sandblasted plate and an anti-rust coating film having an average film thickness shown in each table was obtained. The average film thickness was measured using an electromagnetic film thickness meter "Deltascope FMP-30" (Fisher Instruments).
[0102] <(1) Rust prevention test: Salt spray test (single film)> The test plate was heated in a heating furnace at 800°C for 3 minutes, and then removed from the furnace and cooled to room temperature. The test plate was then placed in a salt spray tester as specified in item "4. Apparatus" of JIS K5600-7-1:1999. The temperature inside the tester was 35°C ± 2°C, and the sodium chloride concentration of the salt water was 5%. After continuously spraying salt water on the rust-proof coating surface of the test plate for 720 hours, the state of red rust on the test plate was confirmed. The ratio of the area where red rust occurred to the evaluation area of the test plate (rust occurrence ratio) (%) was calculated, and the state of red rust occurrence was evaluated on a scale of 0 to 10 based on the following evaluation criteria in accordance with ASTM D610.
[0103] <(2) Heat discoloration test> In each of the examples and comparative examples, two test plates were prepared. One test plate was heated in a heating furnace at 800°C for 3 minutes, and then removed from the furnace and cooled to room temperature. The other test plate was not subjected to this heat treatment. The color difference (ΔE represented by the following formula) of the test plate after the heat treatment relative to the test plate that was not subjected to the heat treatment was measured using a spectrophotometer (SPECTROPHOTOMETER CM-3700, manufactured by Konica Minolta, Inc.) under conditions of a C light source of D65 and a viewing angle of 10°, and then calculated. It was determined that the smaller the color difference, the better the heat discoloration resistance. ΔE = {(L * 1 -L * 0 ) 2 +(a * 1 -a * 0 ) 2 +(b * 1 -b * 0 ) 2} 1 / 2 L * 1 , a * 1 , b * 1is the L of the test plate after heat treatment * , a * , b * and L * 0 , a * 0 , b * 0 is the L of the test plate that has not been heat treated. * , a * , b * respectively.
[0104] <(3) Heat resistance test> The test plate was heated in a heating furnace at 800°C for 3 minutes, and then removed from the furnace and cooled to room temperature. Next, water was sprayed thoroughly using a sprayer until the surface of the rust-preventive coating film on the test plate was completely wet. After the surface of the rust-preventive coating film on the test plate had dried, it was sprayed in the same manner. Spraying was performed three times. After spraying, the test plate was left for about 16 hours. The state of red rust and the state of white rust on the test plate were confirmed. The state of red rust was evaluated on a scale of 0 to 10 based on the following evaluation criteria in accordance with ASTM D610, and the state of white rust was evaluated on a scale of 0 to 10 based on the following evaluation criteria.
[0105] <(4) Rust prevention test after topcoat painting> A silicone topcoat paint (Silicon Tainetsu Black (K), manufactured by Chugoku Toryo Co., Ltd.) was applied to the surface of the rust-preventive coating film of the above test plate, and heated at 200°C for 2 hours to form a topcoat coating film with an average thickness of 20 μm. The test plate was then heated at 400°C for 2 hours. After continuously spraying salt water on the topcoat coating surface of the test plate under the same conditions as in (1) above for 50 hours, the state of red rust and the state of white rust on the test plate were confirmed. The state of red rust was evaluated on a scale of 0 to 10 based on the following evaluation criteria in accordance with ASTM D610, and the state of white rust was evaluated on a scale of 0 to 10 based on the following evaluation criteria.
[0106] The evaluation criteria for the state of red rust occurrence are as follows. 10: No rust or rust rate is 0.01% or less 9: The rust rate is more than 0.01% and less than 0.03% 8: The rust rate is more than 0.03% and less than 0.1% 7: Rust ratio is more than 0.1% and less than 0.3% 6: Rust ratio is more than 0.3% and less than 1% 5: Rust ratio is more than 1% and less than 3% 4: Rust ratio is more than 3% and less than 10% 3: Rust ratio is over 10% and 16% or less 2: Rust ratio is over 16% and 33% or less 1: Rust ratio is over 33% and 50% or less 0: Rust area is over 50% and 100% or less
[0107] The evaluation criteria for the occurrence of white rust are as follows: Although the evaluation is based on even points, if the state of white rust on the test plate is intermediate between the two even points, odd points may be used. 10: No white rust is observed. 8: A small amount of white rust is observed. 6: White rust is partially observed. 4: White rust is observed over a wide area. 2: White rust is observed over a significantly wide area. 0: White rust is observed over the entire surface.
[0108] [Table 1]
[0109] [Table 2]
Claims
1. A binder (A); Zinc-based powder (B); 120 x 10 -7 / ° C. or more; and A rust-preventive coating composition comprising:
2. 2. The rust-preventive coating composition according to claim 1, wherein the glass powder (C) has a softening point of 480° C. or lower.
3. The thermal expansion coefficient of the glass powder (C) is 120×10 -7 / ℃~220×10 -7 The rust-preventive coating composition according to claim 1, wherein the temperature is 100° C. / ° C.
4. 2. The rust-preventive coating composition according to claim 1, wherein the binder (A) is a siloxane-based binder.
5. 5. The rust-preventive coating composition according to claim 4, wherein the siloxane-based binder is a condensate of at least one compound selected from the group consisting of tetraalkoxysilanes and alkyltrialkoxysilanes.
6. The rust-preventive coating composition according to claim 4, wherein the weight average molecular weight (Mw) of the siloxane-based binder is 1,300 to 10,000.
7. In the solid content of the anticorrosive coating composition, The content of the binder (A) is 1 to 30 mass %, The content of the zinc-based powder (B) is 10 to 90 mass%, The content of the glass powder (C) is 0.01 to 20 mass%. The anticorrosive coating composition according to claim 1.
8. The anticorrosive coating composition according to claim 1, wherein the ratio ((C) / (B)) of the content of the glass powder (C) to the content of the zinc-based powder (B) is 0.005 to 0.10 on a mass basis.
9. A first agent containing the binder (A); A second agent containing the zinc-based powder (B) and the glass powder (C); A packaged composition comprising: A first agent containing the binder (A) and the glass powder (C); A second agent containing the zinc-based powder (B); A packaged composition having the formula: A first agent containing the binder (A); A second agent containing the zinc-based powder (B); A third agent containing the glass powder (C); A packaged composition comprising The rust-preventive coating composition according to claim 1,
10. An anti-rust coating film formed from the anti-rust coating composition according to any one of claims 1 to 9.
11. A substrate; The rust-preventive coating film according to claim 10 provided on the substrate; A coated product having the above structure.
12. A method for producing a coated product, comprising a step of applying the anti-rust coating composition according to any one of claims 1 to 9 to a substrate and curing the composition to form an anti-rust coating film.
Citation Information
Patent Citations
Coating filmmforming composition
JP1978119932A
Method for manufacturing steel plate with anticorrosive coating film
JP2017186480A
Anti-corrosive coating composition
JP2021187864A
JPP7467453B
Rust-inhibiting paint composition and application for same
WO2016047479A1
Cited By
Laminated coating for methanol tanks
JP2026147065A