Wiring board and manufacturing method thereof
The wiring board design with nanometer-order meandering grooves on the insulating layer surface addresses the adhesion and transmission loss issues by using a seed layer and metal plating layer to improve contact and reduce signal path expansion, achieving strong adhesion and efficient signal transmission.
Patent Information
- Application Number
- JP2020174190
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-25
- Filing Date
- 2020-10-15
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-10-15
AI Technical Summary
Existing methods for improving adhesion between insulating and wiring layers in wiring boards while minimizing transmission loss are inadequate, particularly for high-frequency signals, and the techniques for forming primer layers have limited material versatility.
A wiring board design featuring nanometer-order grooves with a meandering shape on the insulating layer surface, where the wiring layer includes a seed layer that fills these grooves, forming anchor portions for enhanced adhesion, and a metal plating layer is used to improve contact between the insulating and wiring layers.
This design enhances adhesion strength between the insulating and wiring layers while maintaining good transmission characteristics for high-frequency signals, reducing signal path expansion due to the skin effect.
Smart Images

Figure 0007567134000002 
Figure 0007567134000003 
Figure 0007567134000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a wiring board and a manufacturing method thereof. [Background technology]
[0002] In the manufacture of wiring boards, a desmear process may be performed on the insulating layer. The desmear process forms micrometer-order irregularities on the surface of the insulating layer, improving the adhesion between the insulating layer and the wiring layer. However, when micrometer-order irregularities are formed on the surface of the insulating layer, the faster the signal transmission speed becomes, the longer the signal transmission path becomes due to the skin effect, and the transmission loss increases.
[0003] A method for improving adhesion between an insulating layer and a wiring layer while suppressing transmission loss is described in Patent Document 1. Also known is a technique for improving adhesion with a wiring layer by forming a primer layer on the surface of an insulating layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-192864 A Summary of the Invention [Problem to be solved by the invention]
[0005] Although the method described in Patent Document 1 achieves the intended purpose, sufficient adhesion may not be obtained. In addition, the technology for forming a primer layer is limited to only certain materials, and is therefore not very versatile.
[0006] An object of the present disclosure is to provide a wiring board having excellent transmission characteristics for high frequency signals and high adhesion strength between an insulating layer and a wiring layer, and a manufacturing method thereof. [Means for solving the problem]
[0007] According to one embodiment of the present disclosure, an insulating layer; Part of the upper surface of a wiring layer formed on the insulating layer; above a surface of the insulating layer having a meandering groove of nanometer order in a plan view, the groove having an average width of 1 nm or more and less than 100 nm; the wiring layer having a seed layer in contact with the insulating layer and a metal plating layer on the seed layer, the wiring layer having an anchor portion formed by filling the groove with the seed layer; The upper surface of the insulating layer has a first region covered by the wiring layer and a second region not covered by the wiring layer, and the upper surface of the insulating layer in the first region protrudes upwardly relative to the upper surface of the insulating layer in the second region. A wiring board is provided. Effect of the Invention
[0008] According to the present disclosure, it is possible to improve the adhesive strength between an insulating layer and a wiring layer while obtaining good transmission characteristics for high frequency signals. [Brief description of the drawings]
[0009] [Figure 1] FIG. [Diagram 2] 1 is a cross-sectional view illustrating a structure of a wiring board according to a first embodiment. [Diagram 3] 1 is a cross-sectional view illustrating a structure of a wiring board according to a first embodiment. [Figure 4] 3 is a plan view illustrating an example of a surface of an insulating layer in the first embodiment. FIG. [Diagram 5] 1A to 1C are cross-sectional views (part 1) illustrating the method for manufacturing the wiring board according to the first embodiment. [Figure 6] 5A to 5C are cross-sectional views (part 2) illustrating the method for manufacturing the wiring board according to the first embodiment. [Figure 7] 5A to 5C are cross-sectional views (part 3) illustrating the method for manufacturing the wiring board according to the first embodiment; [Figure 8] 4A to 4C are cross-sectional views (part 1) illustrating a method for forming a wiring layer and an insulating layer in the first embodiment. [Figure 9] 5A to 5C are cross-sectional views (part 2) illustrating a method for forming a wiring layer and an insulating layer in the first embodiment. [Figure 10]5A to 5C are cross-sectional views (part 3) illustrating a method for forming a wiring layer and an insulating layer in the first embodiment. [Figure 11] FIG. 1 is a plan view (part 1) illustrating a mask film. [Figure 12] FIG. 2 is a plan view (part 2) illustrating the mask film. [Figure 13] 5A to 5C are cross-sectional views illustrating a method for forming a wiring layer and an insulating layer in a first modified example of the first embodiment. [Figure 14] 11 is a cross-sectional view illustrating a structure of a wiring board according to a second modified example of the first embodiment. FIG. [Figure 15] 6A to 6C are cross-sectional views illustrating a method for manufacturing a wiring board according to a second modified example of the first embodiment. [Figure 16] 11 is a cross-sectional view illustrating a structure of a wiring board according to a third modified example of the first embodiment. FIG. [Figure 17] 10A to 10C are cross-sectional views illustrating a method for manufacturing a wiring board according to a third modified example of the first embodiment. [Figure 18] 6 is a cross-sectional view illustrating the structure of a wiring board according to a second embodiment. [Figure 19] 11A to 11C are cross-sectional views illustrating a method for manufacturing a wiring board according to a second embodiment; [Figure 20] 11A to 11C are cross-sectional views (part 2) illustrating the method for manufacturing the wiring board according to the second embodiment; [Figure 21] 11A to 11C are cross-sectional views (part 3) illustrating the method for manufacturing the wiring board according to the second embodiment; [Figure 22] 13A to 13C are cross-sectional views (part 4) illustrating the method for manufacturing a wiring board according to the second embodiment; [Figure 23] FIG. 11 is a diagram illustrating a method for calculating a pitch. [Figure 24] FIG. 2 is a diagram illustrating a scanning electron microscope (SEM) photograph of a surface of an insulating layer. [Diagram 25] FIG. 25 is a diagram showing the result of binarization processing of the SEM photograph shown in FIG. 24. [Figure 26] FIG. 1 shows the results of a 90° peel test. [Figure 27]FIG. 13 is a diagram showing the results of a reliability test. [Figure 28] FIG. 1 is a diagram (part 1) illustrating an SEM photograph of the surface of a mask film. [Figure 29] FIG. 2 is a diagram (part 2) illustrating an SEM photograph of the surface of a mask film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments will be described in detail with reference to the attached drawings. In this specification and the drawings, components having substantially the same functional configuration may be denoted by the same reference numerals to avoid repetitive description. In addition, for convenience, the drawings may show characteristic parts in an enlarged manner to make the characteristics easier to understand, and the dimensional ratios of each component may not be the same as in reality. In this disclosure, the term "planar view" refers to viewing an object from a vertical direction (up and down directions in the drawing) such as in FIG. 2, and the term "planar shape" refers to the shape of an object viewed from a vertical direction such as in FIG. 1.
[0011] (Grooves in this disclosure) In the present disclosure, a groove is defined as a recess formed on the surface of a layer or film, and has an elongated shape such that the length of the planar shape of the recess is 2.0 times or more the average width of the recess.
[0012] The recess 12 shown in Fig. 1 is formed on a surface 11 of a layer. A medial axis (MA) 13 can be defined for the recess 12. The recess 12 may be branched. In the present disclosure, the total length of the medial axis 13 of the recess 12, including the branched portion, is defined as the length of the recess 12.
[0013] The length of a line segment 14 that is a part of a straight line perpendicular to the intermediate axis 13 and connects two intersections with the contour of the recess 12 is defined as the width of the recess 12 at the intersection with the line segment 14 of the intermediate axis 13. If the interval between the line segments 14 on the intermediate axis 13 is made infinitesimally small, the average value of the lengths of these infinite number of line segments 14 becomes substantially equal to the value obtained by dividing the area of the recess 12 in a plan view by the total length of the intermediate axis 13, i.e., the length of the recess 12. In the present disclosure, the value obtained by dividing the area of the recess 12 by the total length of the intermediate axis 13, i.e., the length of the recess 12, is defined as the average width of the recess 12.
[0014] Regarding an opening formed in a layer or film, a groove-like opening is defined as an elongated opening whose planar length is 2.0 times or more the average width of the opening.
[0015] (First embodiment) A first embodiment will be described below. The first embodiment relates to a wiring board including a core substrate.
[0016] [Wiring board structure] The structure of the wiring board will be described below with reference to Fig. 2, which is a cross-sectional view illustrating the structure of the wiring board according to the first embodiment.
[0017] As shown in FIG. 2, the wiring board 100 according to the first embodiment includes a core wiring board 101 as a support. The core wiring board 101 includes a core board 102 formed of an insulating material such as glass epoxy resin or bismaleimide triazine resin. A first wiring layer 104 made of copper or the like is formed on both sides of the core board 102. A through hole 103A is formed in the core board 102 penetrating in the thickness direction, and a through conductor 103 is provided in the through hole 103A. The first wiring layers 104 on both sides of the core board 102 are connected to each other via the through conductor 103. A through hole plating layer is formed on the side wall of the through hole 103A, and the remaining hole of the through hole 103A may be filled with a resin body. In this case, the first wiring layers 104 on both sides of the core board 102 are connected to each other via the through hole plating layer.
[0018] A first insulating layer 105 is formed on both sides of the core substrate 102. The first insulating layer 105 has a surface 105a on the opposite side to the core substrate 102 and a surface 105b on the core substrate 102 side. A via hole 106 reaching the connection portion of the first wiring layer 104 is formed in the first insulating layer 105, and a second wiring layer 107 connected to the first wiring layer 104 through a via conductor in the via hole 106 is formed on the first insulating layer 105. Furthermore, a second insulating layer 108 is formed on the first insulating layer 105 on both sides of the core substrate 102. The second insulating layer 108 has a surface 108a on the opposite side to the core substrate 102 and a surface 108b on the core substrate 102 side. A via hole 109 is formed in the second insulating layer 108, reaching the connection portion of the second wiring layer 107, and a third wiring layer 110 is formed on the second insulating layer 108, and is connected to the second wiring layer 107 through a via conductor in the via hole 109.
[0019] On both sides of core substrate 102, solder resist layers 150 are formed on second insulating layer 108. Openings 151 reaching the connecting portions of third wiring layer 110 are formed in solder resist layer 150 on the side of core substrate 102 that is to be connected to the semiconductor chip. Openings 152 reaching the connecting portions of third wiring layer 110 are formed in solder resist layer 150 on the opposite side of core substrate 102.
[0020] Here, the structures of the first insulating layer 105 and the second wiring layer 107 will be described in detail. FIG. 3 is a cross-sectional view illustrating the structure of the wiring board according to the first embodiment. FIG. 3 illustrates an enlarged view of part A in FIG. 2. FIG. 4 is a plan view illustrating the surface 105a of the first insulating layer 105 in the first embodiment. A cross section taken along line III-III in FIG. 4 appears in FIG. 3.
[0021] As shown in FIG. 3 and FIG. 4, a plurality of grooves 105x are formed on the surface 105a of the first insulating layer 105. The grooves 105x have a meandering shape in plan view. That is, the grooves 105x have a meandering portion in plan view. In the present disclosure, a meandering groove (concave) refers to a groove (concave) that extends in a random direction without direction dependency. The meandering shape also includes a mesh shape and a labyrinth shape. The grooves 105x are grooves on the order of nanometers. That is, the average width of the grooves 105x is 1 nm or more and less than 100 nm, and preferably 3 nm or more and 50 nm or less. In FIG. 3, the width of the grooves 105x varies depending on the location, but this is because the grooves 105x have a meandering shape. As shown in FIG. 4, the appearance of the grooves 105x varies depending on the position at which the cross section is observed, but the width of the grooves 105x when viewed in plan is generally uniform.
[0022] The surface 105a has a covered region 105s covered by the second wiring layer 107 and an exposed region 105t exposed from the second wiring layer 107. Grooves 105x are formed in both the covered region 105s and the exposed region 105t. The second wiring layer 107 has an anchor portion 107y that fits into the groove 105x and is in direct contact with the covered region 105s. The second insulating layer 108 has an anchor portion 108y that fits into the groove 105x and is in direct contact with the exposed region 105t.
[0023] Although not shown, grooves having a shape similar to that of the grooves 105x are also formed on the surface 108a of the second insulating layer 108. The third wiring layer 110 has anchor portions that fit into the grooves formed on the surface 108a. The solder resist layer 150 has anchor portions that fit into the grooves formed on the surface 108a.
[0024] The first wiring layer 104, the second wiring layer 107, and the third wiring layer 110 are conductive layers including, for example, a copper layer. The first insulating layer 105 and the second insulating layer 108 are resin layers including, for example, an insulating resin such as an epoxy resin or a polyimide resin. The first insulating layer 105 and the second insulating layer 108 may contain a filler such as silica.
[0025] In the first embodiment, a groove 105x is formed on the surface 105a, and the second wiring layer 107 has an anchor portion 107y that fits into the groove 105x, thereby improving the adhesion between the first insulating layer 105 and the second wiring layer 107.
[0026] The grooves 105x have a meandering shape, filling the surface with high density, and the anchor portions 107y that penetrate into the grooves have a root-like structure that spreads to a certain length in any direction (all directions) in the plane. Therefore, even if local stress is applied to the portion on the anchor portion 107y of the second wiring layer 107, the stress is dispersed in all directions, so that the anchor portion 107y is less likely to break, and excellent adhesion can be obtained. For example, when the recess is pinhole-shaped, the anchor portion becomes pile-shaped, and when the diameter of the pile is nano-sized, the breaking strength of the anchor portion itself becomes small, and it easily breaks when stress is concentrated. Also, when the grooves are linear, the anchor portion has a long, elongated shape as in the present disclosure, so that although the stress is dispersed, directional dependency of adhesion strength may occur in the surface.
[0027] Similarly, a groove having a shape similar to groove 105x is formed on surface 108a of second insulating layer 108, and third wiring layer 110 has an anchor portion that enters the groove formed on surface 108a, thereby improving adhesion between second insulating layer 108 and third wiring layer 110.
[0028] In addition, since grooves 105x are formed in surface 105a and second insulating layer 108 has anchor portions 108y that fit into grooves 105x, adhesion between first insulating layer 105 and second insulating layer 108 can also be improved.
[0029] Furthermore, since the grooves 105x are grooves on the order of nanometers, the expansion of the signal transmission path due to the skin effect can be suppressed, and good transmission characteristics for high-frequency signals can be obtained.
[0030] Note that, on the side of core substrate 102 that is connected to the semiconductor chip, a connection terminal that protrudes above solder resist layer 150 through opening 151 may be formed on the connection portion of third wiring layer 110.
[0031] [Method of manufacturing wiring board] Next, a method for manufacturing the wiring board will be described. Figures 5 to 7 are cross-sectional views illustrating the method for manufacturing the wiring board according to the first embodiment.
[0032] First, as shown in FIG. 5(a), a core wiring board 101 is prepared as a support. The core wiring board 101 includes a core board 102 and a first wiring layer 104. A through hole 103A is formed in the core board 102 penetrating in the thickness direction, and a through conductor 103 is provided in the through hole 103A. For example, the through hole 103A can be formed by processing using a drill or a laser, and the through conductor 103 and the first wiring layer 104 can be formed by plating, photolithography, or the like. Note that a large-sized board from which a plurality of wiring boards 100 can be obtained is used as the core wiring board 101. That is, the core wiring board 101 has a plurality of regions in which structures corresponding to the wiring boards 100 are formed.
[0033] Next, as shown in FIG. 5(b), uncured resin films are attached to both sides of the core substrate 102 and cured by heat treatment to form a first insulating layer 105. The first insulating layer 105 is made of insulating resin such as epoxy resin or polyimide resin. The first insulating layer 105 may be formed by applying a liquid resin. Thereafter, the first insulating layer 105 on both sides of the core substrate 102 is processed with a laser to form a via hole 106 in the first insulating layer 105 that reaches the connection portion of the first wiring layer 104.
[0034] Next, as shown in FIG. 6(a), second wiring layers 107 connected to the first wiring layer 104 through via conductors in the via holes 106 are formed on the first insulating layer 105 on both sides of the core substrate 102.
[0035] 6(b), a second insulating layer 108 is formed on the first insulating layer 105 on both sides of the core substrate 102. The second insulating layer 108 can be formed in the same manner as the first insulating layer 105.
[0036] Here, a method for forming the second wiring layer 107 and the second insulating layer 108 will be described in detail. The second wiring layer 107 can be formed by a semi-additive method. Figs. 8 to 10 are cross-sectional views illustrating a method for forming the second wiring layer 107 and the second insulating layer 108 in the first embodiment. Figs. 8 to 10 show the same parts as Fig. 3.
[0037] As described above, the via hole 106 reaching the connection part of the first wiring layer 104 is formed in the first insulating layer 105 (see FIG. 8(a)). After that, the surface 105a of the first insulating layer 105, the side surface of the via hole 106, and the exposed surface 104a exposed from the via hole 106 of the first wiring layer 104 are cleaned. In this cleaning, for example, reverse sputtering plasma etching is performed in a sputtering device. In this plasma etching, for example, argon gas or nitrogen gas can be used as a process gas. A mixed gas of argon gas and nitrogen gas may be used as a process gas. In addition, in order to remove the residue (smear) of the insulating resin generated at the bottom of the via hole 106, plasma etching may be performed before cleaning. In this plasma etching, for example, tetrafluoromethane gas, oxygen gas, nitrogen gas, or argon gas, or a mixed gas thereof can be used as a process gas.
[0038] Next, as shown in FIG. 8(b), a mask film 910 having a recess 911 and a protrusion 912 is formed on the surface 105a and the exposed surface 104a. The mask film 910 has a surface 910a on the opposite side to the core substrate 102 and a surface 910b on the core substrate 102 side. FIG. 11 is a plan view illustrating the mask film 910. For example, a copper film can be formed as the mask film 910. For example, the mask film 910 can be formed by a sputtering method in the sputtering device used for cleaning. That is, the mask film 910 can be formed following cleaning without removing the structure shown in FIG. 8(a) from the sputtering device. For example, a film of aluminum, zinc, tin, titanium, nickel, or a copper-nickel alloy may be formed as the mask film 910. The surface 105a is an example of a first surface.
[0039] The average thickness of the mask film 910 is, for example, about 5 nm to 15 nm. When the mask film 910 is formed by a sputtering method, the material of the mask film 910 is selected and the film formation conditions are adjusted so that the film grows nuclei. For example, it is preferable to use a metal having a melting point of 1100° C. or less, such as copper, aluminum, or zinc, as the material of the mask film 910. In the early stage of growth, nuclei of the mask film 910 are formed at multiple locations on the surface 105a and the exposed surface 104a. Thereafter, the nuclei grow larger and bond with each other, so that the entire surface 105a and the exposed surface 104a are covered with the mask film 910. At the stage where the average thickness of the mask film 910 is about 5 nm to 15 nm, the bonding between the nuclei is completed and the surface 105a and the exposed surface 104a are covered with the mask film 910, but there is a variation in the thickness of the mask film 910. The mask film 910 has recesses 911 and protrusions 912 due to thickness variations. Nucleation and bonding between nuclei occur irregularly, so the recesses 911 and protrusions 912 are also formed irregularly. Therefore, as shown in FIG. 11, the recesses 911 have a meandering shape in plan view. That is, the recesses 911 have a meandering portion in plan view. The recesses 911 are recesses on the order of nanometers. That is, the average width of the recesses 911 is 1 nm or more and less than 100 nm, and preferably 3 nm or more and 50 nm or less. The surface 910a is an example of a second surface, and the recesses 911 are an example of a first groove.
[0040] The lower the melting point of the material of the mask film, the larger the nuclei tend to grow due to aggregation during film formation, and the larger the pitch of the recesses 911 and the protrusions 912 tend to be. The melting points of aluminum and zinc are lower than that of copper. For this reason, when aluminum or zinc is used for the mask film 910, the pitch of the recesses 911 and the protrusions 912 tends to be larger than when copper is used for the mask film 910. By increasing the pitch of the recesses 911 and the protrusions 912, it becomes easier to insert the seed layer into the grooves 105x to be formed later (see FIG. 9(b)).
[0041] After the formation of the mask film 910, as shown in FIG. 8(c), the recess 911 is penetrated to the first insulating layer 105 to form a groove-shaped opening 913. Although an opening may exist in the mask film 910 even before this treatment, if this treatment is not performed, the opening 913 cannot be sufficiently formed in the mask film 910, and it becomes difficult to sufficiently etch the first insulating layer 105 in the subsequent treatment (see FIG. 9(a)). The opening 913 can be formed, for example, in the sputtering device used for forming the mask film 910. In forming the opening 913, for example, reverse sputtering plasma etching is performed in the sputtering device. In this way, the opening 913 can be formed following the formation of the mask film 910 without taking out the structure shown in FIG. 8(b) from the sputtering device. In this plasma etching, for example, argon gas can be used as a process gas. When argon gas is used, for example, the etching rate of the metal mask film 910 can be increased, so that the time required for etching can be shortened and mask deformation due to heat during plasma etching can be suppressed. When the opening 913 is formed, the recess 911 becomes deeper, the recess 911 widens, and the protrusion 912 becomes lower and narrower. FIG. 12 is a plan view illustrating the mask film 910. The above-mentioned FIG. 11 illustrates the mask film 910 before the opening 913 is formed, and FIG. 12 illustrates the mask film 910 after the opening 913 is formed. The opening 913 is an opening on the order of nanometers. That is, the average width of the opening 913 is 1 nm or more and less than 100 nm, and preferably 3 nm or more and 50 nm or less.
[0042] Next, as shown in FIG. 9(a), a groove 105x is formed on the surface 105a so as to follow the opening 913 in a plan view. The groove 105x can be formed, for example, in the sputtering device used to form the opening 913. In forming the groove 105x, for example, reverse sputtering plasma etching is performed in the sputtering device. That is, the groove 105x can be formed following the formation of the opening 913 without removing the structure shown in FIG. 8(c) from the sputtering device. In this plasma etching, for example, oxygen gas can be used as a process gas. Nitrogen gas or carbon tetrafluoride gas may be used as a process gas. A mixed gas of two or three of oxygen gas, nitrogen gas, and carbon tetrafluoride gas may be used as a process gas. The groove 105x is a groove on the order of nanometers. That is, the average width of the groove 105x is 1 nm or more and less than 100 nm, and preferably 3 nm or more and 50 nm or less. The groove 105x is an example of a second groove.
[0043] Next, as shown in FIG. 9(b), a seed layer 920 is formed on the first insulating layer 105 and on the inner surface of the via hole 106. A part of the seed layer 920 enters the groove 105x, and the groove 105x is filled with the seed layer 920. The seed layer 920 can be formed, for example, in the sputtering device used to form the groove 105x. That is, the seed layer 920 can be formed following the formation of the groove 105x without removing the structure shown in FIG. 9(a) from the sputtering device. As the seed layer 920, for example, a copper-nickel alloy layer can be formed. The copper-nickel alloy layer has excellent corrosion resistance and oxidation resistance. If the proportion of nickel in the copper-nickel alloy layer is 20% by mass or more and 50% by mass or less, the copper-nickel alloy layer can be removed in a later process using an etching solution for copper. When forming the seed layer 920, it is preferable to apply a bias to the core substrate 102. This is because the seed layer 920 is more likely to enter the groove 105x. 9(a) from the sputtering device and then electroless plating may be used to form the seed layer 920. A copper layer may be formed as the seed layer 920.
[0044] 9(c), a plating resist layer 930 having an opening 931 is formed in a portion where the second wiring layer 107 is to be formed. The plating resist layer 930 can be formed outside the sputtering apparatus used for forming the grooves 105x.
[0045] Next, as shown in FIG. 10(a), a metal plating layer 940 is formed in the openings 931 of the plating resist layer 930 by electrolytic plating using the seed layer 920 as a plating power supply path.
[0046] 10(b), the plating resist layer 930 is removed. Furthermore, the seed layer 920 and the mask film 910 are removed by wet etching using the metal plating layer 940 as a mask. In this manner, the second wiring layer 107 can be formed, which includes the seed layer 920 and the metal plating layer 940 and has an anchor portion 107y that enters the groove 105x.
[0047] 10(c), a second insulating layer 108 is formed on the first insulating layer 105. The second insulating layer 108 has an anchor portion 108y that fits into the groove 105x exposed from the second wiring layer 107.
[0048] In this manner, the second wiring layer 107 and the second insulating layer 108 can be formed.
[0049] After the second insulating layer 108 is formed, as shown in FIG. 7(a), the second insulating layer 108 on both sides of the core substrate 102 is processed with a laser to form via holes 109 in the second insulating layer 108, the via holes 109 reaching the connection portions of the second wiring layer 107. Furthermore, on both sides of the core substrate 102, a third wiring layer 110 connected to the second wiring layer 107 through the via conductors in the via holes 109 is formed on the second insulating layer 108. The third wiring layer 110 can be formed in the same manner as the second wiring layer 107. That is, a groove having a shape similar to the groove 105x can be formed on the surface 108a of the second insulating layer 108, and the third wiring layer 110 having an anchor portion that enters the groove can be formed.
[0050] 7(b), solder resist layers 150 are formed on the second insulating layer 108 on both sides of the core substrate 102. After that, openings 151 reaching the connection portions of the third wiring layer 110 are formed in the solder resist layer 150 on the side of the core substrate 102 that is to be connected to the semiconductor chip. In addition, openings 152 reaching the connection portions of the third wiring layer 110 are formed in the solder resist layer 150 on the opposite side of the core substrate 102.
[0051] The solder resist layer 150 is formed from an insulating resin such as a photosensitive epoxy resin or an acrylic resin. The solder resist layer 150 may be formed by attaching a resin film or applying a liquid resin. The openings 151 and 152 can be formed by exposure and development. The solder resist layer 150 may be formed from an insulating resin such as a non-photosensitive epoxy resin or a polyimide resin. In this case, the openings 151 and 152 can be formed by laser processing or blasting.
[0052] Next, the structure shown in Fig. 7(b) is cut with a slicer or the like. As a result, structures corresponding to the wiring boards 100 are separated into individual pieces, and a plurality of wiring boards 100 according to the first embodiment are obtained from the large-sized core wiring board 101. In this manner, the wiring board 100 according to the first embodiment shown in Fig. 2 can be manufactured.
[0053] According to this method, meander-shaped grooves 105x on the nanometer order can be easily formed on the surface 105a of the first insulating layer 105. Also, the second wiring layer 107 having anchor portions 107y that enter the grooves 105x can be easily formed. Similarly, meander-shaped grooves on the nanometer order can be easily formed on the surface 108a of the second insulating layer 108. Also, the third wiring layer 110 having anchor portions that enter the grooves can be easily formed.
[0054] Furthermore, the processes from cleaning after the formation of the via holes 106 (see FIG. 8(a)) to the formation of the seed layer 920 can be performed using a single sputtering apparatus. That is, these processes can be performed continuously in a single sputtering apparatus without removing the structure including the core substrate 102 from the sputtering apparatus.
[0055] In addition, after the formation of the solder resist layer 150 and before singulation, a connection terminal that protrudes above the solder resist layer 150 through the opening 151 may be formed on the connection portion of the third wiring layer 110 on the side of the core substrate 102 that is to be connected to the semiconductor chip.
[0056] (First Modification of the First Embodiment) A first modified example of the first embodiment will be described. The first modified example differs from the first embodiment mainly in the method of forming the second wiring layer 107 and the second insulating layer 108. Fig. 13 is a cross-sectional view illustrating the method of forming the second wiring layer 107 and the second insulating layer 108 in the first modified example of the first embodiment. Fig. 13 illustrates the same part as Fig. 3.
[0057] In the first modification, similarly to the first embodiment, the processes up to the formation of the grooves 105x are performed (see FIG. 9(a)). In the first modification, as shown in FIG. 13(a), the mask film 910 is oxidized during the formation of the grooves 105x to form an oxide film 915.
[0058] In the first modification, after the formation of the groove 105x, the oxide film 915 is removed as shown in FIG. 13(b). The oxide film 915 can be removed in the sputtering device used for the formation of the groove 105x. In removing the oxide film 915, for example, reverse sputtering plasma etching is performed in the sputtering device. In this way, the oxide film 915 can be removed following the formation of the groove 105x without removing the structure shown in FIG. 13(a) from the sputtering device. In removing the oxide film 915, for example, argon gas can be used as a process gas. When removing the oxide film 915, a damaged layer 916 can be generated in the vicinity of the surface 105a.
[0059] Next, as shown in FIG. 13(c), a damaged layer 916 generated in the vicinity of the surface 105a during removal of the oxide film 915 is removed. The damaged layer 916 can be removed in the sputtering device used for removing the oxide film 915. In removing the damaged layer 916, for example, reverse sputtering plasma etching is performed at low power in the sputtering device. In this way, the damaged layer 916 can be removed following removal of the oxide film 915 without removing the structure shown in FIG. 13(b) from the sputtering device. In removing the damaged layer 916, for example, nitrogen gas can be used as a process gas. By performing plasma etching using nitrogen gas as a process gas, the damaged layer 916 can be removed and a modified layer 917 having functional groups such as hydroxyl groups and carboxyl groups can be formed in the vicinity of the surface 105a. The process gas may further contain oxygen gas.
[0060] Thereafter, the processes subsequent to the formation of the seed layer 920 are carried out in the same manner as in the first embodiment.
[0061] The first modified example can also provide the same effects as those of the first embodiment. In addition, the modified layer 917 having the functional group can improve the adhesion between the seed layer 920 and the first insulating layer 105, so that better adhesion can be obtained.
[0062] The wiring substrate 100 manufactured by the method of the first modification does not include the mask film 910.
[0063] Even if the mask film 910 is not oxidized, as in the first modification, the mask film 910 may be removed after the formation of the grooves 105x and before the formation of the seed layer 920. In this case, it is also preferable to remove the damaged layer 916 and form the modified layer 917.
[0064] When the mask film 910 is oxidized to form an oxide film 915, the oxide film 915 may be reduced using hydrogen gas instead of being removed.
[0065] The oxide film 915 or the mask film 910 may be removed by wet etching. When the oxide film 915 or the mask film 910 is removed by wet etching, the damaged layer 916 is unlikely to be formed, so the seed layer 920 may be formed as is. When copper or zinc is used as the material of the mask film 910, the oxide film 915 or the mask film 910 is easily removed by wet etching. After the oxide film 915 or the mask film 910 is removed by wet etching, the seed layer 920 may be formed by a wet process such as an electroless plating process.
[0066] (Second Modification of the First Embodiment) A second modification of the first embodiment will be described below. The second modification differs from the first embodiment and the like mainly in the configurations of the first insulating layer 105 and the second insulating layer .
[0067] [Wiring board structure] The structure of the wiring board will be described. Fig. 14 is a cross-sectional view illustrating the structure of a wiring board according to a second modified example of the first embodiment. Fig. 14 illustrates a portion corresponding to Fig. 3.
[0068] As described above, in the first embodiment, the grooves 105x are formed in both the covered region 105s and the exposed region 105t. Also, in the first embodiment, the second insulating layer 108 has an anchor portion 108y that fits into the groove 105x.
[0069] On the other hand, in the second modified example, as shown in FIG. 14, the grooves 105x are formed in the covered region 105s but not in the exposed region 105t. In the exposed region 105t, the surface 105a is a substantially flat surface. The second insulating layer 108 is in direct contact with the exposed region 105t of the substantially flat surface 105a. Moreover, the exposed region 105t is located closer to the core substrate 102 than the covered region 105s.
[0070] The other configuration is similar to that of the first embodiment.
[0071] The second modification can improve the adhesion between the first insulating layer 105 and the second wiring layer 107 while obtaining good transmission characteristics for high frequency signals, as in the first embodiment. In the first embodiment, there is a risk that the resin contained in the first insulating layer 105 may be altered or that a compound of a metal contained in the mask film 910 or the seed layer 920 may be present around the groove 105x in the exposed region 105t. However, the second modification can reduce such a risk. Therefore, the second modification can provide the first insulating layer 105 with more stable insulation.
[0072] As for the second insulating layer 108, the exposed area of the surface 108a that is exposed from the third wiring layer 110 may be a substantially flat surface similar to the exposed area 105t. This allows the second insulating layer 108 to have more stable insulation properties.
[0073] [Method of manufacturing wiring board] Next, a method for manufacturing a wiring board will be described with reference to Fig. 15, which is a cross-sectional view illustrating a method for manufacturing a wiring board according to a second modification of the first embodiment.
[0074] In the second modified example, similarly to the first embodiment, the process up to the removal of the seed layer 920 and the mask film 910 is performed (see FIG. 10(b)). Next, as shown in FIG. 15(a), the second wiring layer 107 is used as a mask to remove the surface portion of the first insulating layer 105 around the groove 105x in the exposed region 105t. In removing the surface portion of the first insulating layer 105, for example, plasma etching is performed in a plasma etching device. In removing the first insulating layer 105, for example, oxygen gas or carbon tetrafluoride gas can be used as a process gas. A mixed gas of oxygen gas and carbon tetrafluoride gas may also be used as the process gas. As a result of removing the surface portion of the first insulating layer 105, the surface 105a becomes a substantially flat surface in the exposed region 105t. As a result, even if there are altered portions of the resin contained in the first insulating layer 105 or metal compounds contained in the mask film 910 or the seed layer 920 around the groove 105x in the exposed region 105t, these are removed.
[0075] 15(b), a second insulating layer 108 is formed on the first insulating layer 105. The second insulating layer 108 is in direct contact with the exposed region 105t of the substantially flat surface 105a.
[0076] Thereafter, the processes subsequent to the formation of the via hole 109 are carried out in the same manner as in the first embodiment.
[0077] According to the second modified example, even if there are altered portions of the resin contained in the first insulating layer 105 or metal compounds contained in the mask film 910 or the seed layer 920 around the groove 105x in the exposed region 105t, these can be removed to obtain more stable insulation.
[0078] In the second modified example as well, the mask film 910 or the oxide film 915 may be removed after the formation of the grooves 105x and before the formation of the seed layer 920. In this case as well, it is preferable to remove the damaged layer 916 and form the modified layer 917. When the oxide film 915 is formed, a reduction treatment of the oxide film 915 may be performed using hydrogen gas.
[0079] Regarding the second insulating layer 108, the exposed region of the surface 108a that is exposed from the third wiring layer 110 may be made to be a substantially flat surface, similar to the exposed region 105t.
[0080] (Third Modification of the First Embodiment) A third modified example of the first embodiment will be described. The third modified example differs from the first embodiment and the like mainly in the configurations of the first insulating layer 105 and the second insulating layer .
[0081] [Wiring board structure] The structure of the wiring board will be described. Fig. 16 is a cross-sectional view illustrating the structure of a wiring board according to a second modified example of the first embodiment. Fig. 16 illustrates a portion corresponding to Fig. 3.
[0082] 16, in the third modified example, like the second modified example, the exposed region 105t is located closer to the core substrate 102 than the covered region 105s. Unlike the second modified example, in the third modified example, a groove 105z having a similar shape to the groove 105x is formed in the exposed region 105t. The second insulating layer 108 has an anchor portion 108y that fits into the groove 105z in the exposed region 105t.
[0083] The other configuration is similar to that of the second modified example of the first embodiment.
[0084] According to the third modification, it is possible to obtain the same effects as those of the first embodiment. Furthermore, like the second modification, it is possible to obtain more stable insulation properties for the first insulating layer 105.
[0085] The second insulating layer 108 may also have a groove formed in an exposed area of the surface 108a that is exposed from the third wiring layer 110, the groove having a shape similar to that of the groove 105z.
[0086] [Method of manufacturing wiring board] Next, a method for manufacturing a wiring board will be described with reference to Fig. 17, which is a cross-sectional view illustrating a method for manufacturing a wiring board according to a third modification of the first embodiment.
[0087] In the third modified example, similar to the first embodiment, the processes up to removal of the seed layer 920 and the mask film 910 are performed (see FIG. 10(b)). Next, as shown in FIG. 17(a), similar to the second modified example, the second wiring layer 107 is used as a mask to remove the surface portion of the first insulating layer 105 around the groove 105x in the exposed region 105t. As a result, the surface 105a in the exposed region 105t becomes a substantially flat surface.
[0088] Next, as shown in Fig. 17(b), a groove 105z having a similar shape to the groove 105x is formed in the surface 105a in the exposed region 105t. In forming the groove 105z, for example, similar to the first modified example, processes from forming the mask film 910 to forming the modified layer 917 are performed (see Figs. 8(b), 8(c), 9(a), and 13(a)-(c)). If the mask film 910 is not oxidized, it is sufficient to remove the mask film 910 instead of the oxide film 915. The groove 105z is an example of a third groove.
[0089] 17(c), a second insulating layer 108 is formed on the first insulating layer 105. The second insulating layer 108 has an anchor portion 108y that fits into the groove 105z exposed from the second wiring layer 107.
[0090] Thereafter, the processes subsequent to the formation of the via hole 109 are carried out in the same manner as in the first embodiment.
[0091] In the third modified example as well, the mask film 910 or the oxide film 915 may be removed after the formation of the grooves 105x and before the formation of the seed layer 920. In this case as well, it is preferable to remove the damaged layer 916 and form the modified layer 917. When the oxide film 915 is formed, a reduction treatment of the oxide film 915 may be performed using hydrogen gas.
[0092] Regarding the second insulating layer 108, a groove having a shape similar to that of the groove 105z may be formed in an exposed area of the surface 108a that is exposed from the third wiring layer 110.
[0093] Second embodiment The second embodiment relates to a wiring board that does not include a core substrate, a so-called coreless board.
[0094] [Wiring board structure] The structure of the wiring board will be described below with reference to Fig. 18. Fig. 18 is a cross-sectional view illustrating the structure of the wiring board according to the second embodiment.
[0095] As shown in FIG. 18, the wiring board 200 according to the second embodiment includes a first wiring layer 204, a first insulating layer 205, a second wiring layer 207, and a second insulating layer 208. The first insulating layer 205 has a surface 205a on the side connected to the semiconductor chip and a surface 205b opposite to the surface 205a. The first wiring layer 204 is formed on the surface 205b. A via hole 206 reaching the connection portion of the first wiring layer 204 is formed in the first insulating layer 205, and a second wiring layer 207 connected to the first wiring layer 204 through a via conductor in the via hole 206 is formed on the first insulating layer 205. A second insulating layer 208 is formed on the first insulating layer 205. The second insulating layer 208 has a surface 208a on the side connected to the semiconductor chip and a surface 208b opposite to the surface 208a. A via hole 209 is formed in the second insulating layer 208, reaching the connection portion of the second wiring layer 207, and a third wiring layer 210 is formed on the second insulating layer 208, and is connected to the second wiring layer 207 through a via conductor in the via hole 209.
[0096] A solder resist layer 250 is formed on the second insulating layer 208. A via hole 251 reaching the connection portion of the third wiring layer 210 is formed in the solder resist layer 250.
[0097] The first wiring layer 204, the second wiring layer 207, and the third wiring layer 210 are, for example, conductive layers including a copper layer or the like. The first insulating layer 205 and the second insulating layer 208 are, for example, resin layers including an insulating resin such as an epoxy resin or a polyimide resin. The first insulating layer 205 and the second insulating layer 208 may contain a filler such as silica.
[0098] A groove having a shape similar to the groove 105x shown in Fig. 3 and Fig. 4 is formed on a surface 205a of the first insulating layer 205 and a surface 208a of the second insulating layer 208. The second wiring layer 207 has an anchor portion that enters the groove formed on the surface 205a, and the second insulating layer 208 also has an anchor portion that enters the groove formed on the surface 205a. The third wiring layer 210 has an anchor portion that enters the groove formed on the surface 208a, and the solder resist layer 250 also has an anchor portion that enters the groove formed on the surface 208a.
[0099] According to the second embodiment, it is also possible to improve the adhesion between the first insulating layer 205 and the second wiring layer 207, and between the second insulating layer 208 and the third wiring layer 210. In addition, it is also possible to improve the adhesion between the first insulating layer 205 and the second insulating layer 208.
[0100] In addition, since the grooves are on the order of nanometers, the expansion of the signal transmission path due to the skin effect can be suppressed, and good transmission characteristics for high-frequency signals can be obtained.
[0101] Note that a connection terminal protruding above the solder resist layer 250 through the via hole 251 may be formed on the connection portion of the third wiring layer 210.
[0102] [Method of manufacturing wiring board] Next, a method for manufacturing the wiring board will be described. Figures 19 to 22 are cross-sectional views illustrating the method for manufacturing the wiring board according to the second embodiment.
[0103] First, as shown in Fig. 19(a), a support 201 is prepared. The support 201 includes, for example, a support substrate, and an adhesive layer and a metal layer provided on both sides of the support substrate. For example, a woven or nonwoven fabric (not shown) made of glass fiber, aramid fiber, or the like, impregnated with an insulating resin such as an epoxy resin can be used as the support substrate. For example, a metal foil such as copper foil, aluminum foil, nickel foil, or zinc foil, a ceramic plate, or a resin sheet mainly made of a resin such as acrylic or polyimide can be used as the adhesive layer. For example, a copper foil can be used as the metal layer.
[0104] 19(a), a first wiring layer 204 is formed on both sides of the support 201. The first wiring layer 204 can be formed by, for example, a semi-additive method.
[0105] Next, as shown in FIG. 19(b), uncured resin films are attached to both sides of the support 201 and cured by heat treatment to form a first insulating layer 205. The first insulating layer 205 is made of insulating resin such as epoxy resin or polyimide resin. The first insulating layer 205 may be formed by applying a liquid resin. Thereafter, the first insulating layer 205 on both sides of the support 201 is processed with a laser to form a via hole 206 in the first insulating layer 205 that reaches the connection portion of the first wiring layer 204.
[0106] Next, as shown in FIG. 20(a), second wiring layers 207 connected to the first wiring layer 204 through via conductors in the via holes 206 are formed on the first insulating layer 205 on both sides of the support 201.
[0107] Next, as shown in FIG. 20(b), a second insulating layer 208 is formed on the first insulating layer 205 on both sides of the support 201.
[0108] The second wiring layer 207 and the second insulating layer 208 can be formed by a method similar to the method for forming the second wiring layer 107 and the second insulating layer 108 in the first embodiment shown in Figures 8 to 10. That is, a groove having a similar shape to the groove 105x can be formed on the surface 205a of the first insulating layer 205, and the second wiring layer 207 and the second insulating layer 208 having an anchor portion that fits into this groove can be formed.
[0109] Next, as shown in FIG. 21(a), the second insulating layer 208 on both sides of the support 201 is processed with a laser to form via holes 209 in the second insulating layer 208, which reach the connection parts of the second wiring layer 207. Furthermore, on both sides of the support 201, a third wiring layer 210 connected to the second wiring layer 207 through a via conductor in the via hole 209 is formed on the second insulating layer 208. The third wiring layer 210 can be formed in the same manner as the second wiring layer 207. That is, a groove having a form similar to the groove 105x can be formed on the surface 208a of the second insulating layer 208, and the third wiring layer 210 having an anchor part that enters the groove can be formed.
[0110] 21(b), a solder resist layer 250 is formed on the second insulating layer 208 on both sides of the support 201. Thereafter, via holes 251 reaching the connection portions of the third wiring layer 210 are formed in the solder resist layer 250 on both sides of the support 201. The solder resist layer 250 and the via holes 251 can be formed in the same manner as the solder resist layer 150 and the openings 151 in the first embodiment.
[0111] 21(b) is cut by a slicer or the like. As a result, structures including the support 201 and corresponding to the wiring substrate 200 are separated. After a carrier is attached to the structure shown in FIG. 21(b), it may be cut by a slicer or the like.
[0112] 22, structures corresponding to wiring board 200 are separated from both sides of support 201. In this manner, wiring board 200 according to the second embodiment shown in FIG.
[0113] According to this method, meandering grooves on the order of nanometers can be easily formed on surface 205a of first insulating layer 205 and surface 208a of second insulating layer 208. Also, second wiring layer 207 and third wiring layer 210 having anchor portions that enter these grooves can be easily formed.
[0114] The first to third modified examples of the first embodiment may be applied to the second embodiment.
[0115] In the present disclosure, when a thermoplastic resin is used as the material of the insulating layer 105, the grooves 105x, 105z are preferably formed in the insulating layer 105 by microwave plasma etching. Microwave plasma etching can be performed at a low temperature, and damage to the insulating layer 105 can be suppressed. On the other hand, when reactive ion etching (RIE) is performed to etch the insulating layer 105 made of a thermoplastic resin, there is a risk that the insulating layer 105 may be altered or deformed due to the influence of plasma, heat, and the like. If the insulating layer 105 is altered or deformed, the shape of the grooves 105x, 105z may be distorted or fibrils may be generated on the surface of the insulating layer 105, and sufficient adhesion strength may not be obtained.
[0116] Alternatively, the process from forming the mask film 910 to forming the grooves 105x may be performed by dry processing, and the process from removing the mask film 910 or the oxide film 915 to forming the seed layer 20 may be performed by wet processing. In this case, if an amphoteric metal with a low melting point such as zinc is used as the material for the mask film 910, the mask film 910 or the oxide film 915 can be easily removed by a plating pretreatment such as pickling, and the pitch of the recesses 911 and the protrusions 912 can be increased. By increasing the pitch of the recesses 911 and the protrusions 912, the seed layer 20 can be easily formed to enter the grooves 105x even by wet processing (electroless plating processing). An existing device can be used for the wet processing.
[0117] (Preferred groove shape) Next, a preferred form of the groove having a meandering shape in a plan view, which is formed in the insulating layer, will be described.
[0118] Groove pitch The groove pitch is preferably 10 nm or more and 100 nm or less. If the groove pitch is less than 10 nm, the groove and the convex part of the insulating resin may become too thin, and the strength of the anchor part may decrease. If the groove pitch exceeds 100 nm, when the wiring becomes fine, the adhesion may decrease due to the small number of anchors. In addition, according to the above-mentioned example of the manufacturing method, it is difficult to form a mask film having grooves with a pitch of less than 10 nm or more than 100 nm, and it is difficult to make the pitch of the grooves of the insulating layer less than 10 nm or more than 100 nm. It is more preferable that the groove pitch is 20 nm or more and 60 nm or less. The groove pitch can be calculated by the following method. FIG. 23 is a diagram illustrating a method of calculating the pitch.
[0119] FIG. 23 illustrates an insulating layer 50 in which grooves 50x are formed. In the surface in which the grooves 50x are formed, 10 or more line segments 21 extending in a first direction and arranged at equal intervals in a second direction perpendicular to the first direction are set, and the number of grooves 50x intersecting with each line segment 21 is identified. Furthermore, 10 or more line segments 22 extending in a second direction and arranged at equal intervals in the first direction are set, and the number of grooves 50x intersecting with each line segment 22 is identified. Then, the number of grooves 50x intersecting with 10 or more line segments 21 and the average number of grooves 50x intersecting with 10 or more line segments 22 are calculated. The length of the line segments 21 and 22 is constant L, and the value obtained by dividing the length L of the line segments 21 and 22 by the average number of grooves 50x is defined as the pitch of the grooves 50x.
[0120] If the length L of the line segments 21 and 22 is too short, the distribution of the grooves 50x may not be fully reflected in the calculation result of the pitch of the grooves 50x. Therefore, the length L of the line segments 21 and 22 is set to 200 nm or more. The length L of the line segments 21 and 22 may be 200 nm or more and 1 μm or less. The length L of the line segments 21 and 22 is set to, for example, 250 nm.
[0121] If the distance between the line segments 21 or the distance between the line segments 22 is too small, the distribution of the grooves 50x may not be fully reflected in the calculation result of the pitch of the grooves 50x. Therefore, the distance between the line segments 21 and 22 is set to 20 nm or more. The distance between the line segments 21 and 22 may be 20 nm or more and 100 nm or less.
[0122] [Average groove width] The average width of the groove is preferably 3 nm or more and 50 nm or less. If the average width of the groove is less than 3 nm, it becomes difficult to fill the inside of the groove with a seed layer, making it difficult to form the anchor part of the wiring layer, or the anchor part of the wiring layer itself becomes thin, so that the anchor part of the wiring layer may not have excellent strength. In addition, if the average width of the groove exceeds 50 nm, the aspect ratio of the groove (ratio of the depth and width of the groove) becomes small, and the anchor effect may be reduced. It is more preferable that the average width of the groove is 10 nm or more and 40 nm or less.
[0123] [Relationship between groove length and average groove width] A structure having many elongated grooves whose length is several times longer than the average width of the grooves is preferable. Specifically, when the ratio of (groove length) / (average groove width) in plan view is calculated for grooves present in an area of 200 nm square or more of the insulating layer, the average value of the ratio is preferably 4.0 or more. If the average value of the ratio is less than 4.0, the surface structure will be dominated by short grooves, and the anchor part of the wiring layer may not have excellent strength. Note that the surface of the wiring layer may include short grooves or pinhole-shaped recesses.
[0124] [Groove Occupancy Rate] The ratio of the area occupied by the grooves in a plan view to the total area of the surface on which the grooves are formed (groove occupancy) is preferably 10% or more and 60% or less. If the groove occupancy is less than 10% by area, the anchor portion of the wiring layer may be insufficient, and excellent adhesion may not be obtained. If the groove occupancy is more than 60% by area, the protrusions of the insulating layer supporting the anchor portion of the wiring layer may be insufficient, and the strength of the insulating layer may be reduced. It is more preferable that the groove occupancy is 20% or more and 50% or less by area. It is preferable that the groove occupancy is approximately the same as the value (%) obtained by dividing the breaking strength S1 of the resin of the insulating layer by the sum (S1+S2) of the breaking strength S1 and the breaking strength S2 of the metal of the wiring layer.
[0125] Groove Depth The depth of the groove is preferably 10 nm or more and 50 nm or less. If the depth of the groove is less than 10 nm, the anchor effect may not be fully exerted, and excellent adhesion may not be obtained. If the depth of the groove is more than 50 nm, the unevenness of the insulating layer surface may become large, and the transmission loss may increase. In addition, it may become difficult to fill the inside of the groove with the seed layer, and the formation of the anchor part of the wiring layer may become insufficient, resulting in a decrease in adhesion. The depth of the groove is more preferably 20 nm or more and 40 nm or less.
[0126] (Observation example) Here, an observation example of an actually produced sample will be described. Fig. 24 is a diagram showing an example of a scanning electron microscope (SEM) photograph of the surface of an insulating layer. Fig. 25 is a diagram showing the result of binarization processing of the SEM photograph shown in Fig. 24.
[0127] The SEM photographs shown in Fig. 24(a) to (d) are SEM photographs of the surface of the insulating layer in the sample prepared by changing the forming conditions of the mask film and the etching conditions. These SEM photographs were binarized to obtain the images shown in Fig. 25(a) to (d), respectively. Then, from the images shown in Fig. 25(a) to (d), the median axis was identified, and the average width of the recesses, the average ratio of the length of the recesses to the average width of the recesses (ratio of (length of recesses) / (average width of recesses)), the pitch of the recesses, and the occupancy rate of the recesses were calculated. The results are shown in Table 1. Here, the average value of the ratio of (length of recesses) / (average width of recesses) is the average value of the ratio when the ratio of (length of recesses) / (average width of recesses) is calculated for all recesses (including grooves) present in the observed image.
[0128] [Table 1]
[0129] 24(a) and 25(a), the average ratio of (recess length) / (recess average width) is 1.6, which is less than 4.0, and therefore the surface structure of the insulating layer of sample No. 1 does not correspond to the groove-containing structure of the present disclosure. The recesses formed on the surface of the insulating layer of sample No. 1 are pinhole-shaped recesses and do not have elongated grooves.
[0130] 24(b) and 25(b), the average ratio of (recess length) / (recess average width) is 4.6, which is greater than 4.0, and therefore the surface structure of the insulating layer of sample No. 2 corresponds to the groove-containing structure of the present disclosure. The recesses are formed in a maze shape and have a meandering shape.
[0131] 24(c) and 25(c), the average ratio of (recess length) / (recess average width) is 18.1, which is greater than 4.0, and therefore the surface structure of the insulating layer of sample No. 3 corresponds to the groove-containing structure of the present disclosure. The recesses are formed in a maze shape and have a meandering shape.
[0132] 24(d) and 25(d), the average ratio of (recess length) / (recess average width) is 61.0, which is greater than 4.0, and therefore the surface structure of the insulating layer of sample No. 4 corresponds to the groove-containing structure of the present disclosure. The recesses are formed in a mesh pattern and have a meandering shape.
[0133] (Adhesion test) Next, we will explain the results of an experiment on the relationship between the surface condition of the insulating layer and the adhesion with the wiring layer. In this experiment, a wiring layer was formed on the insulating layer for samples No. 1, No. 2, No. 3, and No. 4, and a 90° peel test was performed. The insulating layer was a polyimide layer, and the seed layer and metal plating layer included in the wiring layer were both copper layers. In addition, as a reference sample, a wiring layer was formed on an insulating layer that did not intentionally have a recess on the surface, and a 90° peel test was performed. The results are shown in Figure 26.
[0134] As shown in FIG. 26, samples No. 2, No. 3, and No. 4, in which meandering grooves were formed, had significantly higher peel strengths than the reference sample and sample No. 1, in which pinhole-shaped recesses were formed.
[0135] (Reliability test) Next, the results of the reliability test will be described. In the reliability test, for sample No. 4, a wiring layer was formed on an insulating layer, and a 90° peel test was performed after applying a thermal load. In addition, for the first reference sample, a wiring layer was formed on an insulating layer that was not intentionally formed with a groove-shaped recess on the surface, and a 90° peel test was performed after applying a thermal load. In the reliability test, for sample No. 4 and the first reference sample, the insulating layer was a polyimide layer, the seed layer included in the wiring layer was a copper-nickel alloy layer, and the metal plating layer included in the wiring layer was a copper layer. Furthermore, a second reference sample was prepared that had the same configuration as the first reference sample except that a copper layer was used for the seed layer, and a 90° peel test was performed on the second reference sample after applying a similar thermal load.
[0136] There were two types of heat load conditions. In the first condition, the device was held in an atmosphere with a temperature of 125°C for 24 hours, then held in an atmosphere with a humidity of 60% RH and a temperature of 60°C for 40 hours, and then reflow was performed three times at 265°C. The first condition was in accordance with JEDEC Lv.3A. In the second condition, the device was held in an atmosphere with a humidity of 85% RH and a temperature of 130°C for 100 hours. The second condition was in accordance with the high-speed accelerated test (HAST). The results are shown in Figure 27.
[0137] 27, compared to the second reference sample in which a copper layer was used as the seed layer, the first reference sample and sample No. 4 in which a copper-nickel layer was used as the seed layer exhibited good peel strength. Furthermore, the first reference sample exhibited a decrease in peel strength after the heat load under the first condition and after the heat load under the second condition, but the decrease in peel strength in sample No. 4 was small, and a peel strength of 1.0 kgf / cm or more was maintained.
[0138] (Relationship between the material of the mask film and the pitch of the protrusions and openings) Next, the relationship between the material of the mask film and the pitch of the projections and openings will be described. Figures 28 and 29 are diagrams showing examples of SEM photographs of the surface of the mask film. Figures 28(a) and 29(a) show SEM photographs of the surface of a copper mask film, and Figures 28(b) and 29(b) show SEM photographs of the surface of an aluminum mask film. Figures 28(a) and 28(b) show an example where the openings are formed in a maze shape, and Figures 29(a) and 29(b) show an example where the openings are formed in a mesh shape.
[0139] 28 and 29, whether the openings are maze-shaped or mesh-shaped, the pitch of the projections and openings formed in the aluminum mask film is larger than the pitch of the projections and openings formed in the copper mask film. Therefore, by using the aluminum mask film, grooves can be formed in the insulating layer at a larger pitch than when the copper mask film is used.
[0140] Although preferred embodiments have been described above in detail, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims. [Explanation of symbols]
[0141] 11: Face 12: Recess 13: Intermediate shaft 14, 21, 22: Line segments 100, 200 Wiring board 104, 107, 110, 204, 207, 210: Wiring layer 105, 108, 205, 208: Insulating layer 105x, 105z: Groove 107y, 108y: Anchor section
Claims
1. An insulating layer; a wiring layer formed on a portion of an upper surface of the insulating layer; having a nanometer-order groove having a meandering shape in a plan view is formed on the upper surface of the insulating layer; The average width of the groove is equal to or greater than 1 nm and less than 100 nm, The wiring layer is a seed layer in contact with the insulating layer; a metal plating layer on the seed layer; having the wiring layer has an anchor portion formed by filling the groove with the seed layer, The top surface of the insulating layer is a first region covered by the wiring layer; a second region that is not covered by the wiring layer; having A wiring board, characterized in that the upper surface of the insulating layer in the first region protrudes above the upper surface of the insulating layer in the second region.
2. 2. The wiring board according to claim 1, wherein the average pitch of the grooves is 10 nm or more and 100 nm or less.
3. 3. The wiring board according to claim 1, wherein the average width of the groove is 3 nm or more and 50 nm or less.
4. The wiring board according to any one of claims 1 to 3, characterized in that the insulating layer has a surface structure in which, when the ratio of (groove length) / (average groove width) for grooves present on the upper surface is calculated, the average value of the ratio is 4.0 or more.
5. 5. The wiring board according to claim 1, wherein the grooves occupy an area of the upper surface of the wiring board in a range of 10% to 60% by area.
6. 6. The wiring board according to claim 1, wherein the average depth of the groove is 10 nm or more and 50 nm or less.
7. 7. The wiring board according to claim 1, wherein the seed layer is made of a copper-nickel alloy.
8. forming an insulating layer; forming a first film on a first surface of the insulating layer, the first film including a first groove on a nanometer order on a second surface opposite to the surface on the insulating layer side; forming a groove-shaped opening in the first film by penetrating the first groove to the insulating layer; a step of etching the insulating layer using the first film in which the opening is formed as a mask to form a second groove of nanometer order following the opening in the first surface; forming a wiring layer having an anchor portion that enters the second groove; 2. A method for manufacturing a wiring board comprising the steps of:
9. 9. The method for manufacturing a wiring board according to claim 8, wherein the first film is formed by a sputtering method.
10. 10. The method for manufacturing a wiring board according to claim 8, wherein the first groove has a meandering shape in a plan view.
11. 11. The method for manufacturing a wiring board according to claim 8, wherein the formation of the first film, the formation of the opening, and the formation of the second groove are carried out in a single sputtering apparatus.
12. The step of forming the wiring layer includes: forming a seed layer in the sputtering apparatus; forming a metal plating layer on the seed layer; The method for manufacturing a wiring board according to claim 11, further comprising the steps of:
13. The step of forming the wiring layer includes: forming a seed layer by wet processing; forming a metal plating layer on the seed layer; 12. The method for manufacturing a wiring board according to claim 8, further comprising the steps of:
14. 14. The method for manufacturing a wiring board according to claim 12, wherein a copper-nickel alloy layer is formed as the seed layer.
15. 15. The method for manufacturing a wiring board according to claim 8, further comprising a step of removing the first film between the step of forming the second groove and the step of forming the wiring layer.
16. 16. The method for manufacturing a wiring board according to claim 15, further comprising a step of performing a plasma treatment using nitrogen gas on the first surface between the step of removing the first film and the step of forming the wiring layer.
17. 17. The method for manufacturing a wiring board according to claim 15, wherein the first film is removed by wet etching.
18. 18. The method for manufacturing a wiring board according to claim 8, further comprising the step of etching a surface portion of the insulating layer in which the second groove is formed and which is exposed from the wiring layer, after the step of forming the wiring layer.
19. 20. The method for manufacturing a wiring board according to claim 18, further comprising the step of forming a third groove on the order of nanometers in a portion of the insulating layer exposed from the wiring layer after the step of etching the surface layer.
20. 20. The method for manufacturing a wiring board according to claim 8, wherein a metal film having a melting point of 1100[deg.] C. or less is formed as the first film.
Citation Information
Patent Citations
Method of producing electric circuit, and electric circuit board obtained by the method
JP2010080946A
Method of manufacturing multilayer wiring board
JP2010192864A
Surface suppressing substrate and substrate with conductor
JP2016082036A