Photoresponsive polymer, adhesive, photoswitching material, toner and image forming method
A photoresponsive polymer with an azomethine structure addresses the low toughness and coloration issues of azobenzene derivatives by providing reversible fluidization and high toughness, suitable for toners, adhesives, and optical switching materials.
Patent Information
- Application Number
- JP2020135372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-06
- Filing Date
- 2020-08-07
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-08-07
AI Technical Summary
Azobenzene derivatives used in photoresponsive liquid crystal materials suffer from low toughness and significant coloration, making them unsuitable for industrial applications such as toners, adhesives, and optical switching materials.
A photoresponsive polymer containing a structural unit with an azomethine structure, which has an activation energy for isomerization between 60 kJ/mol and 100 kJ/mol, allowing it to become fluidized and reversibly non-fluidized upon light irradiation, while minimizing coloration.
The polymer achieves high toughness, reversible fluidization, and lack of significant coloration, enabling effective use in toners, adhesives, and optical switching materials.
Smart Images

Figure 0007567268000056 
Figure 0007567268000057 
Figure 0007567268000058
Abstract
Description
[Technical field]
[0001] The present invention relates to a photoresponsive polymer which is fluidized and reversibly non-fluidized by irradiation with light, an adhesive, a photoswitching material and a toner each using the same, and an image forming method using the toner. [Background technology]
[0002] Photoresponsive liquid crystal materials are known as materials whose fluidity changes when irradiated with light. For example, Patent Documents 1 and 2 propose polymer liquid crystal materials using azobenzene derivatives. These undergo a cis-trans isomerization reaction at the azobenzene moiety in response to light. It is believed that the resulting change in molecular structure induces a phase transition from a solid state to a fluid state. In addition, if the material is irradiated with light at a different wavelength again, heated, or left at room temperature in the dark, a reverse reaction will occur and the material will solidify again. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-256155 A [Patent Document 2] JP 2011-256291 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the azobenzene derivatives described in Patent Documents 1 and 2 above have a relatively low molecular weight, and therefore have a problem of low toughness as a material. In addition, all of the azobenzene derivatives described in Patent Documents 1 and 2 above are colored yellow to orange, and there is a problem that the desired color cannot be reproduced when applied to industrial products such as toners, adhesives, and optical switching materials. Furthermore, according to the study by the present inventors, it was found that although the color of the yellow to orange color can be adjusted to some extent by changing the substituent of the azobenzene derivative, it is fundamentally impossible to make it colorless or nearly colorless.
[0005] Therefore, an object of the present invention is to provide a polymer which is fluidized by light irradiation, reversibly non-fluidized, has high toughness, and is not significantly colored. [Means for solving the problem]
[0006] The present inventors have conducted extensive research in view of the above problems, and as a result have found that the above problems can be solved by providing a polymer containing a structural unit including a group having an azomethine structure, in which a hydrogen atom is bonded to the group having an azomethine structure, and in which the activation energy of isomerization from a cis form to a trans form is within a predetermined range, thereby completing the present invention.
[0007] That is, the present invention provides a photoresponsive polymer which contains a structural unit represented by the following general formula (1), which is fluidized and reversibly non-fluidized upon light irradiation,
[0008] [ka]
[0009] In general formula (1), r 1 is a hydrogen atom or a methyl group, A is a group having an azomethine structure represented by the following general formula (2),
[0010] [ka]
[0011] In general formula (2), Z 1 and Z 2 are each independently N or CH, and Z 1 ≠Z 2 and B 1 each independently represents a substituted or unsubstituted divalent aromatic hydrocarbon group or a substituted or unsubstituted divalent aromatic heterocyclic group, B 2 each independently represents a substituted or unsubstituted monovalent aromatic hydrocarbon group or a substituted or unsubstituted monovalent aromatic heterocyclic group, r 2 each independently represents an alkylene group having 1 to 18 carbon atoms, The photoresponsive polymer is characterized in that the activation energy Ea of a compound in which a hydrogen atom is bonded in place of the oxygen atom bonded to A in the general formula (1) is 60 kJ / mol or more, as represented by the following formula (1). Equation (1): Ea (kJ / mol) = (total energy of TS (kJ / mol)) - (total energy of cis isomer (kJ / mol)) In the above formula (1), TS indicates a transition state represented by general formula (3), and the cis form indicates an isomer represented by general formula (4).
[0012] [ka] Effect of the Invention
[0013] According to the present invention, it is possible to provide a polymer which is fluidized by light irradiation, reversibly non-fluidized, has excellent toughness, and is not significantly colored. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. [Diagram 2] 2 is a schematic configuration diagram of an irradiation unit 40 in the image forming apparatus 100. FIG. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus used in the photoresponsive adhesion test of the Examples for measuring the change in adhesiveness of a polymer due to light irradiation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention relates to a photoresponsive polymer that contains a structural unit represented by the following general formula (1), is fluidized and reversibly non-fluidized upon irradiation with light,
[0016] [ka]
[0017] In general formula (1), r 1 is a hydrogen atom or a methyl group, A is a group having an azomethine structure represented by the following general formula (2),
[0018] [ka]
[0019] In general formula (2), Z 1 and Z 2 are each independently N or CH, and Z 1 ≠Z 2 and B 1 each independently represents a substituted or unsubstituted divalent aromatic hydrocarbon group or a substituted or unsubstituted divalent aromatic heterocyclic group, B 2 each independently represents a substituted or unsubstituted monovalent aromatic hydrocarbon group or a substituted or unsubstituted monovalent aromatic heterocyclic group, r 2 each independently represents an alkylene group having 1 to 18 carbon atoms, The photoresponsive polymer is characterized in that the activation energy Ea of a compound in which a hydrogen atom is bonded in place of the oxygen atom bonded to A in the general formula (1) is 60 kJ / mol or more, as represented by the following formula (1). Equation (1): Ea (kJ / mol) = (total energy of TS (kJ / mol)) - (total energy of cis isomer (kJ / mol)) In the above formula (1), TS indicates a transition state represented by general formula (3), and the cis form indicates an isomer represented by general formula (4).
[0020] [ka]
[0021] By using a polymer that contains a structural unit that includes a group having an azomethine structure represented by the above general formula (1) and in which a compound in which a hydrogen atom is bonded to the structure represented by the above general formula (2) has a predetermined activation energy for cis-trans isomerization, it is possible to realize a photoresponsive polymer that is fluidized by light irradiation and reversibly non-fluidized, has excellent toughness, and has minimal coloring to the extent that it does not affect the reproduction of desired colors when applied to toners, adhesives, and photoswitching materials.
[0022] Although the details of why the polymer of the present invention provides the above-mentioned effects are unclear, the following mechanism is considered. Note that the following mechanism is based on speculation, and the present invention is not limited to the following mechanism in any way. In the following explanation, the structural unit represented by the above general formula (1) is also referred to as a "structural unit containing a group having an azomethine structure."
[0023] Azobenzene derivatives with long alkyl chains at their ends are known to absorb light and soften from a solid state (photochemical phase transition), i.e., to become fluid when irradiated with light, and this photochemical phase transition is thought to occur when the crystal structure collapses due to cis-trans isomerization. The azobenzene derivatives described in Patent Documents 1 and 2 undergo a phase change in association with an isomerization reaction caused by irradiation with light, but these compounds have a relatively low molecular weight, and therefore have the problem of low toughness as materials. In addition, there are n-π * Because it exhibits strong absorption due to transition and is colored orange, there is a problem in that it is difficult to reproduce the desired color when applied to industrial products.
[0024] In the present invention, by using a polymer containing a structural unit having an azomethine structure (a structural unit derived from an azomethine derivative), it has been possible to provide a polymer that is fluidized by light irradiation, reversibly non-fluidized, has high toughness, and is not significantly colored. By introducing a structural unit having an azomethine structure, it is possible to obtain a polymer that is fluidized by light irradiation, reversibly non-fluidized, has high toughness, and is not significantly colored. * Absorption can be significantly weakened, resulting in a polymer that is not significantly colored.
[0025] In polymers containing structural units with azomethine structures, the azomethine derivative absorbs light, and the heat energy released during the photoexcitation and deactivation process is transferred to the repeating units (structural units) to which it is bonded (photothermal conversion), inducing the fluidization and nonfluidization phenomenon. In particular, if the azomethine derivative contained in the polymer is a trans isomer, in addition to the above-mentioned photothermal conversion, the nonfluid trans isomer (E) is irradiated with light and isomerizes to the cis isomer (Z), and many of the trans isomers change to cis isomers with a low Tg, which destroys the ordered structure and induces a phase transition, inducing the fluidization phenomenon. In addition, when the cis isomer returns to the trans isomer, an ordered structure is formed again, inducing the nonfluidization phenomenon. Therefore, in order to induce the fluidization phenomenon, it is considered necessary for many of the trans isomers (E) to be isomerized to the cis isomer (Z). However, it is generally known that azomethine derivatives undergo a faster rate of isomerization from cis to trans isomers than azobenzene derivatives, and it was predicted that azomethine derivatives having unsubstituted benzene rings at both ends of the C=N bond would be disadvantageous in inducing fluidization and the subsequent reversible immobilization.
[0026] The fast rate of isomerization from Z to E isomer is considered to be due to the low energy barrier in the isomerization reaction from Z to E, which allows the isomer to quickly return to the trans isomer (E). The present inventors considered that the rate of isomerization from Z to E can be controlled by controlling the energy barrier (activation energy Ea) in the isomerization reaction from Z to E. They found that the reaction rate of the isomerization reaction from Z to E can be controlled by setting the energy barrier (activation energy Ea) in the isomerization reaction from Z to E to 60 kJ / mol or more, and that the isomer can be fluidized by light irradiation and reversibly immobilized.
[0027] Here, being fluidized by light irradiation and being reversibly non-fluidized means that being changed from a non-fluid state to a fluid state by light irradiation and then returning to a non-fluid state.
[0028] Furthermore, by polymerizing the azomethine derivative, the heat energy released during the photoexcitation and deactivation process when the azomethine derivative absorbs light is transferred to the bonded structural unit (photothermal conversion), which is believed to effectively melt or soften the azomethine derivative. Furthermore, by polymerizing the azomethine derivative, the toughness of the material can also be improved. Therefore, it is believed that excellent fixing properties (image strength) can be obtained, especially when used in toner.
[0029] In addition, the introduction of a structural unit containing an azomethine structure has been shown to be effective in enhancing the n-π coupling of azobenzene derivatives. * Absorption can be significantly weakened, resulting in a polymer that is not significantly colored.
[0030] For the above reasons, it is believed that the polymer of the present invention having a structural unit containing a group having an azomethine structure can induce the phenomenon of fluidization and reversible non-fluidization upon photoisomerization. In addition, the polymer of the present invention has excellent toughness and is not significantly colored, so it can be suitably used for toners, photoresponsive adhesives, and photoswitching materials.
[0031] In the present invention, the fluid state refers to a state in which the material deforms without any external force or with a small external force.
[0032] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, in this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0033] <Polymer containing a structural unit containing a group having an azomethine structure> The polymer of the present invention is a polymer that contains a structural unit represented by the following general formula (1) and is fluidized and reversibly non-fluidized upon irradiation with light.
[0034] [ka]
[0035] In general formula (1), r 1 is a hydrogen atom or a methyl group, A is a group having an azomethine structure represented by the following general formula (2),
[0036] [ka]
[0037] In general formula (2), Z 1 and Z 2 are each independently N or CH, and Z 1 ≠Z 2 and B 1 each independently represents a substituted or unsubstituted divalent aromatic hydrocarbon group or a substituted or unsubstituted divalent aromatic heterocyclic group, B 2 each independently represents a substituted or unsubstituted monovalent aromatic hydrocarbon group or a substituted or unsubstituted monovalent aromatic heterocyclic group, r 2 are each independently an alkylene group having 1 to 18 carbon atoms.
[0038] The polymer of the present invention is a photoresponsive polymer characterized in that the activation energy Ea of a compound in which a hydrogen atom is bonded in place of the oxygen atom bonded to A in general formula (1) is 60 kJ / mol or more, as represented by the following formula (1): Equation (1): Ea (kJ / mol) = (total energy of TS (kJ / mol)) - (total energy of cis isomer (kJ / mol)) In the above formula (1), TS indicates a transition state represented by general formula (3), and the cis form indicates an isomer represented by general formula (4).
[0039] [ka]
[0040] It is believed that the polymer of the present invention has an energy barrier (activation energy Ea) of 60 kJ / mol or more in the isomerization reaction from cis to trans of a compound having a hydrogen atom bonded to the structure represented by the above general formula (2), thereby slowing down the reaction rate of the isomerization reaction from Z to E, relatively increasing the amount of cis upon light irradiation, and effectively inducing fluidization associated with the photoisomerization reaction. The polymer of the present invention is not particularly limited, but is preferably a polymer containing a structural unit containing a group having an azomethine structure, from the viewpoint of reliably facilitating the introduction of an azomethine group into the molecule and efficiently inducing fluidization and reversible immobilization.
[0041] In addition, since the azomethine group portion expresses intermolecular packing (π-π interactions) and exhibits high thermal mobility when isomerized from the trans isomer to the cis isomer, the polymer of the present invention is considered to be more likely to induce fluidization while increasing the strength of the material.
[0042] When the activation energy Ea represented by the above formula (1) is less than 60 kJ / mol, the barrier to the isomerization reaction from cis to trans isomers is low, so that even if the isomerization occurs upon light irradiation, it quickly reverts to the trans isomer. As a result, fluidization upon light irradiation and the subsequent reversible immobilization cannot be achieved.
[0043] Preferably, the activation energy Ea is 63 kJ / mol or more, more preferably 65 kJ / mol or more, and even more preferably 67 kJ / mol or more. In addition, in view of the ease of reversion to the trans form, the activation energy Ea is preferably 100 kJ / mol or less, more preferably 95 kJ / mol or less, and even more preferably 90 kJ / mol or less. In this way, the effects of the present invention can be more easily obtained.
[0044] In the present invention, as shown in formula (1), the energy barrier (activation energy Ea) in the isomerization reaction from a cis isomer to a trans isomer is calculated as a value obtained by subtracting the total energy of the cis isomer from the total energy of the transition state of a compound in which a hydrogen atom is bonded in place of the oxygen atom bonded to the group A having an azomethine structure in general formula (1). The structure of the transition state can be represented by general formula (3), and the structure of the cis isomer can be represented by general formula (4). Note that general formulas (3) and (4) are Z 1 =Z 2 B for bond 1 and B. 2 It indicates the arrangement (position) of H, r 2 -H, Or 2 -H part is B 1 The structure of the compound depends on the structure of the group A having an azomethine structure, including the structure of the compound shown below.
[0045] This includes a range of snowflakes and snowflakes In the case of the wavelength and wavelength ranges, the Gaussian function of the Gaussian 16 (Revision B.01, Frisch MJ, GW Trucks, HB Schlegel, Scuseria GE, Robb MA, Cheeseman JR, Scalmani G, Barone V, Petersson GA, Nakatsuji H, Li X, Caricato M, Marenich AV, Bloino J, Janesko BG, Gomperts R, Mennucci, HP Hratchian, JV Ortiz, AF Izmaylov, JL Sonnenberg, D. Williams-Young, F. Ding, F. Lipparini, F. Egidi, J. Goings, B. Peng, A. Petrone, T. Henderson, D. Ranasinghe, VG Zakrzewski, J. Gao, N. Rega, G. Zheng, W. Liang, M. Hada, M. Ehara, K. Toyota, R.K. Fukuda , Hasegawa J , Ishida M , Nakajima T , Honda Y , Kitao O , Nakai H , Vreven T , Throssell K , Montgomery JA , Peralta JE , Ogliaro F MJ , Bearpark MJ , Heyd EN Brothers , Kudin KN , Staroverov VN , Keith TA , Kobayashi R , Normand J, Raghavachari K, Rendell AP, Burant JC, Iyengar SS, Tomasi J, Cossi M, Millam JM, Klene M, Adamo C, Cammi R, Ochterski JW, RLMartin, K. Morokuma, O. Farkas, JB Foresman, and DJ Fox, Gaussian, Inc., Wallingford CT, 2016.) software can be used, and the density functional theory (B3LYP / 6-31G(d)) can be used as the calculation method. For the molecular structure of the cis isomer, the most stable molecular structure of the isomer represented by general formula (4), i.e., the molecular structure with the lowest total energy, is calculated, and this total energy is taken as the total energy of the cis isomer. For the molecular structure of the transition state, the saddle point of the corresponding molecular structure is calculated for the transition state represented by general formula (3), and the total energy obtained at this time is taken as the total energy of the transition state. There is no particular limitation on the software or calculation method, and similar values can be obtained using any of them. From the calculated value obtained in this way, the value of the activation energy Ea can be obtained according to the above formula (1). .
[0046] In the polymer of the present invention, B 1 and B. 2 By appropriately selecting the structure, the activation energy Ea represented by the above formula (1) can be controlled to 60 kJ / mol or more.
[0047] Specifically, by introducing an electron donating structure into the group A having an azomethine structure, the electron density of the azomethine moiety can be increased, and the activation energy Ea can be increased. For example, 1 and B. 2 By making at least one of the groups a highly electron donating aromatic heterocyclic group, the activation energy Ea can be increased. 1 and B. 2 The activation energy Ea can be increased by introducing a highly electron-donating substituent into the aromatic hydrocarbon group or aromatic heterocyclic group as the aryl group.
[0048] Here, the aromatic hydrocarbon group is not particularly limited, but is preferably an aryl group having 6 to 30 carbon atoms, such as a phenyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, a pyrenyl group (B1 In particular, the phenyl group (B 1 In the above, a phenylene group is preferred.
[0049] The aromatic heterocyclic group is not particularly limited, but is preferably one having 2 to 30 carbon atoms. In addition, those having high electron donating properties are preferred, such as a thienyl group, a furanyl group, a pyrrolyl group, a pyrazolyl group, an imidazolyl group, a pyridyl group, a pyrimidinyl group, a pyrazinyl group, a triazinyl group, a benzothienyl group, a benzimidazolyl group, an indolyl group, an isoindolyl group, a quinolinyl group, an isoquinolinyl group, a quinazolinyl group, a quinoxalinyl group, a naphthyridinyl group, an acridinyl group, a carbazolyl group, a dibenzothienyl group (B 1 In the case of , divalent groups derived from these groups) are included, but are not limited to these. Among them, thienyl group, pyrrolyl group, pyrazolyl group, imidazolyl group, indolyl group, carbazolyl group (B 1 In the above, divalent groups derived from these groups are preferred.
[0050] The above aromatic hydrocarbon group or aromatic heterocyclic group may each have a substituent. The substituent is not particularly limited, but examples thereof include a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. Preferred are a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0051] As described above, the photoinduced phase transition of azomethine derivatives is thought to occur due to the collapse of the crystal structure caused by cis-trans isomerization, as in the case of azobenzene derivatives. In general, the π-π interaction between molecules is strong, so the photoinduced phase transition occurs only on the very outermost surface of the crystal structure. Here, B in the above general formula (1) 1 and B. 2 When the aromatic hydrocarbon group or aromatic heterocyclic group represented by the formula (I) has a substituent, the polymer containing the structural unit containing the group having the azomethine structure of the present invention forms a specific crystal structure in which a structure isotropically disordered by the thermal motion of these substituents coexists in a periodic structure in which π-π interactions are dominant. Therefore, when the cis-trans isomerization reaction proceeds locally and the π-π interactions in the azomethine derivative portion are reduced, isotropic melting occurs in a chain-like manner throughout the system. Therefore, it is considered that the cis-trans isomerization proceeds more easily and fluidization is more likely to occur.
[0052] In this case, it is preferable that at least one of the above-mentioned substituents is a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 18 carbon atoms. It is considered that such a structure makes it easier for cis-trans isomerization to proceed and makes it easier for fluidization to occur. Among these, it is more preferable that the alkyl group having 1 to 18 carbon atoms, the alkoxy group having 1 to 18 carbon atoms, or the dialkylamino group having 2 to 10 carbon atoms have high thermal mobility.
[0053] As for the number of carbon atoms of the substituent, the alkyl group is more preferably an alkyl group having 1 to 12 carbon atoms, and even more preferably an alkyl group having 4 to 12 carbon atoms. The alkoxy group is more preferably an alkoxy group having 1 to 12 carbon atoms, and even more preferably an alkoxy group having 4 to 12 carbon atoms. The dialkylamino group is more preferably a dialkylamino group having 2 to 8 carbon atoms, and even more preferably a dialkylamino group having 4 to 6 carbon atoms. The acyl group is more preferably an acyl group having 2 to 13 carbon atoms, and even more preferably an acyl group having 5 to 13 carbon atoms. The alkoxycarbonyl group is more preferably an alkoxycarbonyl group having 2 to 13 carbon atoms, and even more preferably an alkoxycarbonyl group having 5 to 13 carbon atoms. In this way, by introducing a long-chain substituent, the crystal is easily broken, the light melting property is improved, and the fixability is improved.
[0054] Examples of the alkyl group having 1 to 18 carbon atoms are not particularly limited, and include linear alkyl groups such as a methyl group, an ethyl group, a n-propyl group, a n-butyl group, a n-hexyl group, a n-heptyl group, a n-octyl group, a n-nonyl group, a n-decyl group, a n-undecyl group, a n-dodecyl group, a n-tridecyl group, a n-tetradecyl group, a n-pentadecyl group, and a n-hexadecyl group; an isopropyl group, a sec-butyl group, an isobutyl group, a t Examples of branched alkyl groups include t-butyl, 1-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, 1-methylhexyl, t-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, 2,2-dimethylheptyl, 2,6-dimethyl-4-heptyl, 3,5,5-trimethylhexyl, 1-methyldecyl, and 1-hexylheptyl groups.
[0055] Examples of alkoxy groups having 1 to 18 carbon atoms include linear alkoxy groups such as methoxy group, ethoxy group, n-propoxy group, n-butoxy group, n-hexyloxy group, n-heptyloxy group, n-octyloxy group, n-nonyloxy group, n-decyloxy group, n-undecyloxy group, n-dodecyloxy group, n-tridecyloxy group, n-tetradecyloxy group, n-pentadecyloxy group, and n-hexadecyloxy group; 1-methylpentyloxy group, 4-methyl-2-methylpentyloxy group, and 5-methyl-2-methylpentyloxy group. Examples of branched alkoxy groups include t-pentyloxy group, 3,3-dimethylbutyloxy group, 2-ethylbutyloxy group, 1-methylhexyloxy group, t-octyloxy group, 1-methylheptyloxy group, 2-ethylhexyloxy group, 2-propylpentyloxy group, 2,2-dimethylheptyloxy group, 2,6-dimethyl-4-heptyloxy group, 3,5,5-trimethylhexyloxy group, 1-methyldecyloxy group, and 1-hexylheptyloxy group.
[0056] Examples of alkylamino groups having 1 to 10 carbon atoms include methylamino groups, ethylamino groups, n-propylamino groups, n-butylamino groups, isobutylamino groups, n-hexylamino groups, n-heptylamino groups, n-octylamino groups, n-nonylamino groups, and n-decylamino groups.
[0057] Examples of the dialkylamino group having 2 to 10 carbon atoms include a dimethylamino group, a diethylamino group, a di-n-propylamino group, a di-n-butylamino group, a di-isobutylamino group, and a methylethylamino group.
[0058] Examples of the acyl group having 2 to 19 carbon atoms include saturated or unsaturated straight-chain or branched-chain acyl groups, such as an acetyl group, a propanoyl group (propionyl group), a butanoyl group (butyryl group), an isobutanoyl group (isobutyryl group), a pentanoyl group (valeryl group), an isopentanoyl group (isovaleryl group), a sec-pentanoyl group (2-methylbutyryl group), a t-pentanoyl group (pivalyl group), and the like. Examples of such groups include hexanoyl, heptanoyl, octanoyl, t-octanoyl (2,2-dimethylhexanoyl), 2-ethylhexanoyl, nonanoyl, isononanoyl, decanoyl, isodecanoyl, undecanoyl, lauroyl, myristoyl, palmitoyl, stearoyl, behenoyl, undecylenoyl, and oleoyl groups.
[0059] Examples of the alkoxycarbonyl group having 2 to 19 carbon atoms include linear or branched alkoxycarbonyl groups such as a methoxycarbonyl group, an ethoxycarbonyl group, an n-butoxycarbonyl group, an n-hexyloxycarbonyl group, an n-heptyloxycarbonyl group, an n-octyloxycarbonyl group, an n-nonyloxycarbonyl group, an n-decyloxycarbonyl group, an n-undecyloxycarbonyl group, an n-dodecyloxycarbonyl group, an n-tridecyloxycarbonyl group, an n-tetradecyloxycarbonyl group, an n-pentadecyloxycarbonyl group, and an n-hexadecyloxycarbonyl group; Examples of branched alkoxycarbonyl groups include branched alkoxycarbonyl groups such as a 4-methyl-2-pentyloxycarbonyl group, a 3,3-dimethylbutyloxycarbonyl group, a 2-ethylbutyloxycarbonyl group, a 1-methylhexyloxycarbonyl group, a t-octyloxycarbonyl group, a 1-methylheptyloxycarbonyl group, a 2-ethylhexyloxycarbonyl group, a 2-propylpentyloxycarbonyl group, a 2,2-dimethylheptyloxycarbonyl group, a 2,6-dimethyl-4-heptyloxycarbonyl group, a 3,5,5-trimethylhexyloxycarbonyl group, a 1-methyldecyloxycarbonyl group, and a 1-hexylheptyloxycarbonyl group.
[0060] In the structural unit represented by the above general formula (1), one polymerizable group is provided for each group having an azomethine moiety, which makes it easy to obtain a polymer that is easily melted even with a low amount of light irradiation energy.
[0061] The polymerizable group in the monomer for synthesizing (polymerizing) the photoresponsive polymer represented by general formula (1) has a group represented by any one of the following formulae (i) to (iii). Having a group having such a polymerizable group is preferable because it is suitable for polymer synthesis. As a result, a polymer represented by general formula (2-a), (2-b), or (2-c) can be obtained in which A in general formula (1) has a group represented by general formula (2-a), (2-b), or (2-c), respectively. Among them, from the viewpoint of ease of softening and melting, it is preferable that A has a group represented by (ii) or (iii), and it is more preferable that A has a group represented by (iii). That is, in the above general formula (1), A is preferably a group having an azomethine structure represented by the above general formula (2-b) or (2-c), and it is more preferable that A has an azomethine structure represented by general formula (2-c).
[0062] [ka]
[0063] In the above formulas (i) to (iii), r 1 is r in general formula (1). 1 and each independently represents a hydrogen atom or a methyl group. 2 is r in general formulas (2-b) and (2-c) 2 Each of them is independently an alkylene group having 1 to 18 carbon atoms. 2 is an alkylene group having 3 to 12 carbon atoms. The alkylene group may be linear or branched, and is preferably linear. A part of the alkylene group may be substituted with a substituent. Examples of the substituent include a halogen group, a nitro group, a hydroxyl group, and a carboxyl group.
[0064] The polymer of the present invention is not particularly limited and can be prepared by any method. For example, a polymer in which A in the above general formula (1) is represented by the above general formula (2-a), (2-b), or (2-c) can be obtained by polymerizing a monomer represented by the following formula (i-2), (ii-2), or (iii-2). In the following formulas (i-2), (ii-2), and (iii-2), Z 1 , Z 2 , B 1 , B 2 is the same as in the above general formula (1), and r 1 and r 2 is the same as the above general formula (1) and the above formulas (i), (ii), and (iii). That is, in one embodiment of the present invention, the polymer of the present invention contains a structural unit derived from an azomethine derivative having a polymerizable group represented by the following formula (i-2), (ii-2), or (iii-2).
[0065] [ka]
[0066] Preferably, in the general formula (1), the B 1 are each independently a substituted or unsubstituted phenylene group or a substituted or unsubstituted divalent aromatic heterocyclic group, 2 are each independently a substituted or unsubstituted phenyl group or a substituted or unsubstituted monovalent aromatic heterocyclic group. By adopting such a structure, fluidization and non-fluidization can occur more effectively. In particular, B 1 Or B 2 When is an aromatic heterocyclic group, B 1 and B 2 In comparison with the case where the compound is a phenyl group, the molar absorption coefficient in the solution is smaller and, therefore, when light is irradiated, the light can reach a greater depth, so that not only the upper layer but also the lower layers can be optically melted, which is thought to be advantageous for inducing fluidization.
[0067] In addition, a preferred embodiment of the present invention is a compound represented by the general formula (1),1 are each independently 1 Para position to oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), B is a phenylene group bonded to 2 are each independently unsubstituted or 2 A phenyl group having a substituent selected from an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms at the para position to B. 1 is Z 1 or an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), a carbon atom other than the carbon atom bonded to the aryl group may have a substituent. Here, the specific form of each of the substituents is as described above.
[0068] In azomethine derivatives in which benzene rings are introduced at both ends of the C=N bond, the electron density of the azomethine moiety is lower and the activation energy is likely to be lower than when either one of the bonds is an electron-donating aromatic heterocyclic group. However, by introducing the above-mentioned substituents, the electron density of the azomethine moiety can be increased and the activation energy can be controlled within a specified range, effectively inducing fluidization and reversible non-fluidization phenomena. In addition, lattice defects that act favorably on cis-trans isomerization, free volume, and reduced π-π interactions occur. Therefore, it is believed that cis-trans isomerization proceeds more easily and fluidization is more likely to occur.
[0069] That is, in the azomethine derivatives having benzene rings at both ends of the C=N bond, B 2 When is an unsubstituted phenyl group or a phenyl group having one or more electron-donating substituents (alkoxy groups, dialkylamino groups, etc.), the electron density of the azomethine moiety is higher than when it has only electron-withdrawing substituents, which is preferable because it tends to increase the activation energy and effectively induces the fluidization and reversible non-fluidization phenomena.
[0070] As mentioned above, B 2 is unsubstituted or Z 2 When the phenyl group has a substituent selected from an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms at the para position to the phenyl group, the crystal is easily broken down, the light melting property is improved, and excellent fixability can be obtained when used as a toner. As the substituent at such a para position, an alkyl group having 4 to 12 carbon atoms, an alkoxy group having 4 to 12 carbon atoms, or a dialkylamino group having 4 to 10 carbon atoms is more preferable, since the introduction of a long-chain substituent makes the crystal easily broken down and has a high effect of improving the light melting property.
[0071] At this time, B 1 and B. 2 At least one of them is Z 1 or Z 2 It is preferable that the two ortho positions and the two meta positions are unsubstituted or substituted with a group selected from a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms. That is, all of the four carbon atoms in the two ortho positions and the two meta positions may be unsubstituted, or the four carbon atoms in total may be substituted with a group selected from a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms, or a part of the four carbon atoms in total may be unsubstituted and the remaining part may be substituted with a group selected from a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms. In addition, when substituted, the groups may be the same or different, as long as they are selected from a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms. The alkyl group and alkoxy group may be linear or branched. By adopting such a structure, the steric hindrance near the C=N bond can be controlled, and fluidization and non-fluidization can be effectively expressed. In addition, it is preferable because the melting point of the compound can be controlled within a suitable range.
[0072] Therefore, according to a preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 has the following structure:
[0073] [ka]
[0074] In the formula, Z 1 and Z 2 is N or CH, and Z 1 ≠Z 2 and R 53 represents an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), R 56 ~R 60 are all hydrogen atoms, or R 58 is an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a dialkylamino group having 2 to 10 carbon atoms, preferably an alkyl group having 4 to 12 carbon atoms, an alkoxy group having 4 to 12 carbon atoms, or a dialkylamino group having 4 to 10 carbon atoms; R 56 , R 57 , R 59 , R 60 each independently represents a hydrogen atom, a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, R 51 , R 52 , R 54 , R 55are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0075] More preferably, in the above formula, it is preferable that at least one of the following conditions is further satisfied: R 51 , R 52 , R 54 , R 55 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a dialkylamino group having 2 to 10 carbon atoms (in a preferred embodiment, R 51 , R 52 , R 54 , R 55 are all hydrogen atoms); or R 56 , R 57 , R 59 , R 60 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a dialkylamino group having 2 to 10 carbon atoms (in a preferred embodiment, R 56 , R 57 , R 59 , R 60 are all hydrogen atoms).
[0076] Another preferred embodiment of the present invention is a compound represented by the general formula (1), 1 However, each independently, Z 1 Para position to oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), B is a phenylene group bonded to 2are each independently an aromatic heterocyclic group that is unsubstituted or substituted with any one of a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0077] With the above-mentioned configuration, the electron density of the azomethine moiety is increased, the activation energy is controlled within a predetermined range, and the phenomenon of fluidization and reversible non-fluidization due to light irradiation can be effectively induced. In addition, lattice defects that act favorably on cis-trans isomerization, free volume, and reduced π-π interactions occur. Therefore, it is considered that cis-trans isomerization proceeds more easily and fluidization occurs more easily. Here, the specific forms of the aromatic heterocyclic group and each of the substituents are the same as those described above.
[0078] B 1 But, Z 1 Para position to oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), Z 1 By having a long chain substituent at the para position to the aryl group, the crystal is easily broken down, the light melting property is improved, and when used in a toner, the fixing property is improved.
[0079] Furthermore, B 2 It is preferable that the aromatic heterocyclic group is unsubstituted or substituted with a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms. With the above configuration, the activation energy can be easily controlled within a predetermined range, and fluidization and reversible non-fluidization phenomena can be effectively induced. In addition, lattice defects that act favorably on cis-trans isomerization, free volume, and π-π interaction are generated. Therefore, it is considered that cis-trans isomerization is more likely to proceed and fluidization is more likely to occur.
[0080] Here, B 1 is a phenylene group, B 2 In those embodiments in which Z is an aromatic heterocyclic group, 1 is N and Z 2 is preferably CH. In this embodiment, B 2 The aromatic heterocyclic group is preferably a substituted or unsubstituted thienyl group, pyrrolyl group, pyrazolyl group, imidazolyl group, or furanyl group.
[0081] In such structural units, the activation energy for isomerization from cis to trans can be easily controlled to 60 kJ / mol or more, and therefore the rate of the return reaction can be controlled, presumably enabling the production of sufficient cis isomers.
[0082] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Examples of the structure include the following structure.
[0083] [ka]
[0084] In the formula, Z 1 and Z 2 is N or CH, and Z 1 ≠Z 2 and R 53 represents an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), X is S, O, or NR 61 and preferably S or NR 61 and R 61 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, R 62~R 64 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms (in one embodiment, R 62 ~R 64 are all hydrogen atoms), R 51 , R 52 , R 54 , R 55 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0085] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Other examples of the structure include the following structures:
[0086] [ka]
[0087] In the formula, Z 1 , Z 2 , X, R 51 ~R 55 is the same as in Structural Example 2 above, R 65 ~R 67 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms. In one embodiment, R 65 ~R 67 are all hydrogen atoms.
[0088] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Other examples of the structure include the following structures:
[0089] [ka]
[0090] In the formula, Z 1 , Z 2 , R 51 ~R 55 is the same as in Structural Example 2 above, R 68 ~R 70 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms. In one embodiment, R 68 ~R 70 are all hydrogen atoms.
[0091] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Other examples of the structure include the following structures:
[0092] [ka]
[0093] In the formula, Z 1 , Z 2 , R 51 ~R 55 is the same as in Structural Example 2 above, R 71 ~R 73are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms. In one embodiment, R 71 ~R 73 are all hydrogen atoms.
[0094] In still another preferred embodiment of the present invention, in the general formula (1), B 1 is a substituted or unsubstituted divalent aromatic heterocyclic group, Z 1 An oxygen atom (in the case of (2-a) or (2-c)) at a position not adjacent to the bond position with r 2 (In the case of (2-b)) and B 2 are each independently unsubstituted or a phenyl group substituted with any one of a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. With the above-mentioned configuration, it is possible to increase the electron density of the azomethine moiety and control the activation energy within a predetermined range, thereby effectively inducing the phenomenon of fluidization and reversible non-fluidization by light irradiation. In addition, lattice defects that act favorably on cis-trans isomerization, the appearance of free volume, and the reduction of π-π interactions occur. Therefore, it is considered that cis-trans isomerization proceeds more easily, and fluidization is more easily manifested. In addition, B 1 In the aromatic heterocyclic group of the formula 1 It is believed that by introducing a polymerizable group into a position that is not adjacent to the bonding position of B, the steric hindrance is reduced when the polymer is formed, and therefore the polymer is easily melted and softened. 1 is more preferably a divalent aromatic heterocyclic group substituted with an alkyl group having 4 to 12 carbon atoms, an alkoxy group having 4 to 12 carbon atoms, or a dialkylamino group having 4 to 10 carbon atoms. Here, the specific forms of the aromatic heterocyclic group and each of the substituents are the same as above.
[0095] At this time, B 2 is preferably a phenyl group substituted with a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a dialkylamino group having 2 to 10 carbon atoms. This results in the generation of lattice defects and the appearance of free volume, which act favorably on cis-trans isomerization, and the reduction of π-π interactions. It is therefore believed that cis-trans isomerization proceeds more easily, and fluidization is more likely to occur.
[0096] Here, B 1 is an aromatic heterocyclic group, B 2 In those embodiments where Z is a phenyl group, 1 is CH and Z 2 is preferably N. In this embodiment, B 1 The aromatic heterocyclic group is preferably a group having a substituted or unsubstituted thiophene ring, pyrrole ring, pyrazole ring, imidazole ring, or furan ring.
[0097] In such a structural unit, the activation energy of isomerization from cis to trans isomers is 60 kJ / mol or more, so the rate of the return reaction can be controlled, sufficient cis isomers can be obtained, and B 1 and B 2 Since the molar absorption coefficient in solution is smaller than that in the case where the compound has a six-membered ring, when light is irradiated, the light can reach a deeper direction, and therefore it is possible to optically melt not only the upper layer but also the lower layer, which is considered to be advantageous for inducing fluidization.
[0098] In still another preferred embodiment of the present invention, in the general formula (1), B 1 are each independently a substituted or unsubstituted divalent aromatic heterocyclic group, Z 1 An oxygen atom (in the case of (2-a) or (2-c)) at a position not adjacent to the bond position with r 2 (In the case of (2-b)) and B 2are each independently an aromatic heterocyclic group that is unsubstituted or substituted with a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0099] With the above-mentioned configuration, it is possible to increase the electron density of the azomethine moiety and control the activation energy within a predetermined range, thereby effectively inducing the phenomenon of fluidization and reversible non-fluidization by light irradiation. In addition, lattice defects that act favorably on cis-trans isomerization, the emergence of free volume, and the reduction of π-π interactions occur. Therefore, it is believed that cis-trans isomerization proceeds more easily and fluidization occurs more easily. In addition, B 1 In the aromatic heterocyclic group of the formula 1 It is believed that by introducing a polymerizable group into a position that is not adjacent to the bonding position of B, the steric hindrance is reduced when the polymer is formed, and therefore the polymer is easily melted and softened. 1 and B. 2 The aromatic heterocyclic groups constituting the formula (I) may have the same ring structure or different ring structures.
[0100] In this case, preferably, B 1 is an aromatic heterocyclic group having at least one substituent selected from an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms. By adopting such a structure, fluidization and non-fluidization can be effectively achieved. In addition, it is preferable because the melting point of the compound can be controlled within a suitable range.
[0101] In order to further improve the light melting property, B 1 and B. 2 It is more preferable that at least one of them is substituted with an alkyl group having 4 to 12 carbon atoms, an alkoxy group having 4 to 12 carbon atoms, or a dialkylamino group having 4 to 10 carbon atoms.
[0102] B 1 and B.2 The specific forms of the aromatic heterocyclic group constituting the ring and each of the substituents are the same as those described above.
[0103] Here, B 1 and B. 2 In those embodiments where B is an aromatic heterocyclic group, 1 and B. 2 The aromatic heterocyclic group is particularly preferably a group having a substituted or unsubstituted thiophene ring, pyrrole ring, pyrazole ring, imidazole ring, or furan ring.
[0104] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Examples of the structure include the following structure.
[0105] [ka]
[0106] In the formula, Z 1 and Z 2 is N or CH, and Z 1 ≠Z 2 and R 62 and R 63 each independently represents an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (in the case of (2-b)), or a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, and R 62 and R 63 In the general formula (1), either one of the following is an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), R64 is a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, X is S, O, or NR 61 and preferably S or NR 61 and R 61 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, R 68 ~R 70 are all hydrogen atoms, or R 68 ~R 70 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0107] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Other examples of the structure include the following structures:
[0108] [ka]
[0109] In the formula, Z 1 and Z 2 is N or CH, and Z 1 ≠Z 2 and R 62 and R 63 each independently represents an oxygen atom (in the case of (2-a) or (2-c)) or r 2(in the case of (2-b)), or a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, and R 62 and R63 is an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), R 64 is a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, X is S, O, or NR 61 and preferably S or NR 61 and R 61 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, R 71 ~R 73 are all hydrogen atoms, or R 71 ~R 73 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0110] According to the above-mentioned preferred embodiment of the present invention, -B in the group A having an azomethine structure of general formula (1) 1 -Z 1 =Z 2 -B 2 Other examples of the structure include the following structures:
[0111] [ka]
[0112] In the formula, Z 1 and Z 2 is N or CH, and Z 1 ≠Z 2 and R' 68 and R' 69 each independently represents an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (in the case of (2-b)), or a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, and R' 68 and R' 69 In the general formula (1), either one of the following is an oxygen atom (in the case of (2-a) or (2-c)) or r 2 (In the case of (2-b)), R' 70 is a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, R 71 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms, R 72 , R 73 are all hydrogen atoms, or R 72 , R 73 are each independently a hydrogen atom, a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0113] In the polymer of the present invention, the structural unit represented by formula (1) may be used alone or in combination of two or more kinds.
[0114] Specific examples of the structural unit represented by general formula (1) include the structural units shown in the table below. The table also shows the activation energy Ea of photoisomerization from cis to trans for compounds containing these structural units (compounds in which a hydrogen atom is bonded in place of the oxygen atom bonded to A in general formula (1)).
[0115] [Table 1-1]
[0116] [Table 1-2]
[0117] [Table 1-3]
[0118] [Table 1-4]
[0119] [Table 1-5]
[0120] [Table 1-6]
[0121] [Table 1-7]
[0122] [Table 1-8]
[0123] [Table 1-9]
[0124] [Table 1-10]
[0125] [Table 1-11]
[0126] [Table 1-12]
[0127] <Method for preparing azomethine derivatives having a polymerizable group> The method for preparing the azomethine derivative having a polymerizable group is not particularly limited. For example, the azomethine derivative can be prepared by first preparing a desired azomethine derivative and then introducing a polymerizable group into the azomethine derivative.
[0128] For example, in the case of preparing an azomethine derivative containing a thiophene ring, in the first step, an aniline derivative is reacted with a thiophene carboxaldehyde derivative as a compound having a thiophene ring. In this case, if either the raw material aniline derivative or the thiophene carboxaldehyde derivative has an OH group as a substituent, a polymerizable group can be easily introduced at the position of the OH group.
[0129] For example, Z in the above general formula (1) 1 is N and Z 2 is CH, X is S, and B 1 is a phenylene group, and in the phenylene group, Z 1 A polymerizable group is introduced at the para position of B 2 is a 2-methylthienyl group, and Z is at the 5-position 2 In the case of an azomethine derivative bound to the compound, intermediate A can be obtained by the following reaction scheme.
[0130] Specifically, 4-hydroxyaniline and 5-methylthiophene-2-carboxaldehyde are treated (heated to reflux to react) in a solvent such as ethanol (EeOH) or methanol (MeOH), the reaction liquid is filtered, the resulting powder is washed with cooled ethanol, and recrystallized from methanol / ethanol to obtain the desired compound.
[0131] [ka]
[0132] Then, in the second step, a polymerizable group is introduced into the intermediate A. The method for introducing the polymerizable group is not particularly limited. For example, 6 H 12 When introducing -, use a halogenated alcohol compound such as Cl-C 6 H 12 By reacting with -OH, intermediate B shown below is obtained.
[0133] The reaction conditions are not particularly limited, but for example, the reaction is carried out in a solvent such as dimethylformamide (DMF) in the presence of potassium carbonate and potassium iodide at a temperature preferably within the range of 0°C to 100°C, more preferably within the range of 0°C to 60°C, and even more preferably within the range of 0°C to 40°C.
[0134] [ka]
[0135] Then, in the third step, the intermediate B is reacted with a compound for forming a polymerizable group, for example, acrylic acid chloride or methacrylic acid chloride. The reaction conditions are not particularly limited. For example, it is preferable to carry out the reaction in a known organic solvent in the presence of tertiary amines such as triethylamine and triethanolamine. Preferably, while keeping the mixed liquid containing the intermediate B, tertiary amines, and solvent at 0 to 10°C, a compound for forming a polymerizable group, such as acrylic acid chloride or methacrylic acid chloride, is dropped into the mixed liquid and mixed. Then, the mixed liquid is reacted at room temperature for about 5 to 10 hours, for example, to obtain an azomethine derivative having a polymerizable group.
[0136] [ka]
[0137] In the first step, by changing the raw material to be used to another compound, it is possible to obtain an azomethine derivative having a desired substituent. For example, by reacting a benzaldehyde derivative with an aminothiophene derivative, Z in the general formula (1) can be obtained. 1 is CH and Z 2 is N and B 1 is a phenylene group, and B 2 In addition, by using other aromatic hydrocarbon compounds or aromatic heterocyclic compounds (carboxaldehyde derivatives) instead of compounds having a thiophene ring (thiophene carboxaldehyde derivatives) as raw materials, it is possible to obtain azomethine derivatives in which B is a thienyl group. 2 Similarly, by changing the raw material aniline derivative to another aromatic hydrocarbon compound or aromatic heterocyclic compound having an amino group, it is possible to obtain azomethine derivatives with different structures. 1 It is possible to obtain azomethine derivatives having different structures.
[0138] In addition, groups having polymerizable groups with different structures can be introduced by changing the compounds added in the second and third steps. A person skilled in the art can synthesize an azomethine derivative having a desired polymerizable group by appropriately making the above changes and selecting appropriate reaction conditions.
[0139] Furthermore, by appropriately selecting the raw materials used in the first step, it is also possible to introduce a polymerizable group into intermediate A without carrying out the second step.
[0140] <Structural units other than structural units containing a group having an azomethine structure> The polymer of the present invention may contain structural units (other structural units) other than the structural unit containing a group having an azomethine structure having a polymerizable group represented by the above general formula (1). When the polymer is a copolymer containing other structural units, the arrangement of the repeating units of the copolymer is not particularly limited, and may be any of a random copolymer, a block copolymer, and an alternating copolymer.
[0141] The other structural units are preferably those not containing an azomethine group, and are more preferably structural units constituting a thermoplastic resin that is softened by heating.
[0142] As the other structural unit, it is preferable that it has a vinyl-based polymerizable group because it is easy to synthesize the copolymer.Specifically, for example, a styrene derivative, a (meth)acrylic acid derivative, an olefin derivative, a vinyl ester derivative, a vinyl ether derivative, a vinyl ketone derivative, etc. are used, and it is preferable that it is a structural unit derived from a styrene derivative, a (meth)acrylic acid derivative, or an olefin derivative.
[0143] Examples of styrene derivatives include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pt-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.
[0144] Examples of (meth)acrylic acid derivatives include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.
[0145] Examples of the olefin derivative include ethylene, propylene, n-butylene, isobutylene, n-pentene, 3-methyl-1-pentene, etc. The olefin derivative may be linear or branched, and the number of carbon chains is not particularly limited.
[0146] Examples of the vinyl ester derivatives include vinyl propionate, vinyl acetate, vinyl benzoate, etc. Examples of the vinyl ether derivatives include vinyl methyl ether, vinyl ethyl ether, etc. Examples of the vinyl ketone derivatives include vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc.
[0147] The content of the other structural units in the polymer is not particularly limited and can be selected as appropriate, but is preferably 70% by mass or less, and more preferably 40% by mass or less, relative to 100% by mass of the total amount of all structural units constituting the polymer.
[0148] The number average molecular weight Mn of the polymer of the present invention is not particularly limited, but is preferably 1000 or more, more preferably 3500 or more, even more preferably 3500 to 100000, even more preferably 3500 to 70000, even more preferably 3500 to 50000, and particularly preferably 5000 to 50000. If the number average molecular weight of the polymer is 3500 or more, it is preferable because it has excellent toughness and, when used as a toner, a toner image with excellent fixability can be more easily obtained. In addition, if the number average molecular weight is 100000 or less, it is preferable because the efficiency of isomerization and softening and melting is high.
[0149] The number average molecular weight of the polymer of the present invention can be measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples below.
[0150] <Method of preparing polymer> The method for synthesizing the polymer of the present invention is not particularly limited, and a method of polymerizing the above-mentioned azomethine derivative having a polymerizable group as a monomer using a known polymerization initiator, such as anionic polymerization, cationic polymerization, living radical polymerization, etc., may be used. A known chain transfer agent may be used as necessary.
[0151] As the polymerization initiator, for example, the following azo-based or diazo-based polymerization initiators and peroxide-based polymerization initiators can be used.
[0152] Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile.
[0153] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.
[0154] Examples of the chain transfer agent include benzyl dithiobenzoate, 1-phenylethyl dithiobenzoate, 2-phenylprop-2-yl dithiobenzoate, 1-acetoxyethyl dithiobenzoate, hexakis(thiobenzoylthiomethyl)benzene, 1,4-bis(thiobenzoylthiomethyl)benzene, 1,2,4,5-tetrakis(thiobenzoylthiomethyl)benzene, 1,4-bis-(2-(thiobenzoylthio)prop-2-yl)benzene, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate; ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)prop-2-yl dithiobenzoate, 2-cyano prop-2-yl dithiobenzoate, t-butyl dithiobenzoate, 2,4,4-trimethylpent-2-yl dithiobenzoate, 2-(4-chlorophenyl)prop-2-yl dithiobenzoate, 3- and 4-vinylbenzyl dithiobenzoate, S-benzyl diethoxyphosphinyl dithioformate, t-butyl trithioperbenzoate, 2-phenylprop-2-yl 4-chlorodithiobenzoate, 2-phenylprop-2-yl 1-dithionaphthalate, 4-cyanopentanoic acid dithiobenzoate, dibenzyl tetrathioterephthalate, dibenzyl trithiocarbonate, carboxymethyl dithiobenzoate, and the like.
[0155] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 60 hours.
[0156] Regarding the copolymer containing structural units (other structural units) other than the structural unit containing a group having an azomethine structure represented by the above general formula (1), the preparation method thereof is not particularly limited.
[0157] For example, when preparing a random copolymer, the monomers for constituting the structural unit represented by the general formula (1) and the monomers for constituting the other structural units are mixed with a chain transfer agent, a polymerization initiator, etc. as raw material monomers to obtain a desired copolymer by carrying out a polymerization reaction. The specific form of the monomers for constituting the other structural units is as described above.
[0158] A preferred embodiment of the polymer of the present invention is a polymer (block copolymer) represented by the following general formula (5).
[0159] [ka]
[0160] In the above general formula (5), α is a polymer block containing a structural unit represented by the above general formula (1), and β is an azomethine structure (B 1 -Z 1 =Z 2 -B 2 ) is a polymer block that does not contain.
[0161] When the polymer of the present invention is polymerized, the azomethine structure absorbs light, and the heat energy released during the photoexcitation and deactivation process is transferred to the repeating units (structural units) to which it is bonded (photothermal conversion), which can cause melting or softening. In addition, by forming a block copolymer, the azomethine structure is more likely to form a domain within the polymer, which is thought to efficiently induce softening and melting. Therefore, the effects of the present invention can be obtained even more significantly.
[0162] Of the above block copolymer structures, from the viewpoints of ease of softening and melting and image strength when used as a toner, an α-β-α (also represented as 2α-β) or β-α-β (also represented as 2β-α) block copolymer structure is preferred, and an α-β-α block copolymer structure is more preferred.
[0163] The specific form of the structural unit represented by the general formula (1) constituting the polymer block α is as described above.
[0164] The structural unit constituting the polymer block β is an azomethine structure (B 1 -Z 1 =Z 2 -B 2 ). Specifically, the above-described structural units other than the structural unit containing a group having an azomethine structure can be preferably used. In particular, from the viewpoint of application to the synthesis of block copolymers by living radical polymerization methods such as ATRP, ARGET-ATRP, or RAFT, it is preferable that the polymerizable group has a vinyl-based polymerizable group. Specifically, for example, styrene derivatives, (meth)acrylic acid derivatives, olefin derivatives, vinyl ester derivatives, vinyl ether derivatives, vinyl ketone derivatives, etc. are used, and styrene derivatives, (meth)acrylic acid derivatives, or olefin derivatives are preferable. That is, the polymer block β is preferably a polymer block containing at least one of structural units derived from styrene derivatives, (meth)acrylic acid derivatives, and olefin derivatives.
[0165] The number average molecular weight (total number average molecular weight) of the polymer block α contained in the polymer represented by the general formula (5) is not particularly limited, but is preferably 1000 or more, more preferably 1000 to 100,000, even more preferably 1000 to 70,000, even more preferably 1000 to 50,000, and particularly preferably 3000 to 50,000. If the total number average molecular weight of the polymer blocks α is 1000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. In addition, if the total number average molecular weight of the polymer blocks α is 100,000 or less, it is preferable because the efficiency of softening and melting is high. Here, the total number average molecular weight of the polymer blocks α refers to the number average molecular weight of the polymer block α when the polymer represented by the general formula (5) contains a single polymer block α, and refers to the sum of the number average molecular weights of the polymer blocks α when the polymer represented by the general formula (5) contains multiple polymer blocks α.
[0166] The number average molecular weight (total number average molecular weight) of the polymer block β contained in the polymer represented by the general formula (5) is not particularly limited, but is preferably 1000 or more, more preferably 1000 to 100,000, even more preferably 1000 to 70,000, even more preferably 1000 to 50,000, and particularly preferably 3000 to 50,000. If the total number average molecular weight of the polymer blocks β is 1000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. In addition, if the total number average molecular weight of the polymer blocks β is 100,000 or less, it is preferable because the efficiency of softening and melting is high. Here, the total number average molecular weight of the polymer blocks β refers to the number average molecular weight of the polymer block β when the polymer represented by the general formula (5) contains a single polymer block β, and refers to the sum of the number average molecular weights of the polymer blocks β when the polymer represented by the general formula (5) contains multiple polymer blocks β.
[0167] The total number average molecular weight Mn of the polymer represented by formula (5) is preferably 3500 or more, more preferably 3500 to 100000, even more preferably 3500 to 70000, even more preferably 3500 to 50000, and particularly preferably 5000 to 50000. If the total number average molecular weight of the polymer represented by formula (5) is 3500 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. If the total number average molecular weight is 100000 or less, it is preferable because the efficiency of softening and melting is high.
[0168] Therefore, according to a preferred embodiment of the present invention, the total number average molecular weight of the polymer blocks α contained in the polymer represented by general formula (5) is 1000 or more, the total number average molecular weight of the polymer blocks β is 1000 or more, and the total number average molecular weight Mn of the polymer represented by general formula (5) is 3500 or more.
[0169] In the polymer represented by general formula (5), the ratio of the total number average molecular weight of the polymer blocks α to the total number average molecular weight of the polymer blocks β is not particularly limited, but from the viewpoints of ease of softening and melting and image strength, the ratio of the total number average molecular weight of the polymer blocks α to the total number average molecular weight of the polymer blocks β is preferably 1:20 to 20:1, and more preferably 1:15 to 15:1.
[0170] The total number average molecular weight of the polymer represented by formula (5) and the total number average molecular weight of the polymer blocks α and β can be measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples below.
[0171] The method for synthesizing the block copolymer represented by the general formula (5) is not particularly limited, and known methods such as anionic polymerization, cationic polymerization, living radical polymerization, etc. can be used. Among them, as a simple synthesis method, a living radical polymerization method such as an atom transfer radical polymerization method (ATRP method), an ARGET-ATRP method, or a RAFT method can be preferably used.
[0172] Taking the ATRP method as an example, the method can be carried out by using a monofunctional, difunctional, trifunctional, or tetrafunctional compound containing a halogen element as an initiator as a starting material, and polymerizing a monomer that becomes a structural unit of the polymer block α or β in the presence of a catalyst.
[0173] In the step of polymerizing the monomer, for example, a macroinitiator is produced by polymerizing a monomer that will be a structural unit of either one of the polymer blocks α or β (the block that will be the core part of the block copolymer) in the presence of an initiator, a catalyst, and a ligand.
[0174] Examples of the initiator include, but are not limited to, 2-bromoisobutyrate butyl, 2-bromoisobutyrate ethyl, ethylene bis(2-bromoisobutyrate), 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane, pentaerythritol tetrakis(2-bromoisobutyrate), α,α'-dibromo-p-xylene, ethyl bromoacetate, 2-bromoisobutyryl bromide, and mixtures thereof.
[0175] Examples of the catalyst include copper (I) catalysts and iron (II) catalysts, such as Cu(I)Cl, Cu(I)Br, Fe(II)Cl, Fe(II)Br, and mixtures thereof.
[0176] As the ligand, known ligands can be used, but one or more selected from the group consisting of 2,2'-bipyridyl, 4,4'-dimethyl-2,2'-bipyridyl, 4,4'-di-tert-butyl-2,2'-bipyridyl, 1,1,4,7,10,10-hexamethyltriethylenetetramine, N,N,N',N",N"-pentamethyldiethylenetriamine, cyclam (1,4,8,11-tetraazacyclotetradecane), 1,4,8,11-tetramethylcyclam (1,4,8,11-tetramethyl-1,4,8,11-tetraazacyclotetradecane), tris[2-(dimethylamino)ethyl]amine, and the like are preferred.
[0177] The amounts of the catalyst and ligand used are not particularly limited, and can be appropriately determined with reference to conventionally known knowledge.
[0178] Next, the macroinitiator obtained by the above polymerization is isolated and used as an initiator, and the monomer that is to become the structural unit of the polymer block α or β, which is not used in the synthesis of the macroinitiator, is polymerized again in the presence of a catalyst and a ligand. Alternatively, when the monomers have been almost completely consumed in the synthesis of the macroinitiator, the macroinitiator may be left as it is without isolating it, and the monomer that was not used in the synthesis of the macroinitiator may be added to continue the polymerization. By these operations, the desired block copolymer can be obtained.
[0179] Each of the above reactions is preferably carried out in an inert atmosphere, such as nitrogen or a rare gas such as argon. Each of the above reactions can be carried out at a temperature of, for example, 25 to 160° C., preferably 35 to 130° C. Each of the above reactions may be carried out without using a solvent, or in a solvent such as an organic solvent.
[0180] In the reaction for obtaining a macroinitiator by polymerizing a monomer that will become a structural unit of either one of the polymer blocks α or β, and the reaction for obtaining a block copolymer by reacting the macroinitiator with a monomer that will become a structural unit of the other polymer block, the conditions such as the type and amount of catalyst and ligand used, and the reaction temperature may be the same or different.
[0181] <Fluidization and reversible non-fluidization by light irradiation> The wavelength of the irradiated light when the polymer of the present invention is fluidized by light irradiation is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. Within the above range, the crystals are easily broken (improved light melting property), and the fixability is improved. When fluidizing, in addition to light irradiation, heat or pressure may be applied to promote fluidization. By irradiating with light of the above wavelength, even when heat or pressure is applied, it is possible to fluidize with less heat or pressure. Therefore, by introducing the polymer of the present invention into a toner, fixation at the above wavelength is possible, and a toner with excellent fixability and high color reproducibility can be obtained.
[0182] The above wavelength range includes a part of visible light. Therefore, it is desirable that the polymer of the present invention does not become fluid only by being exposed to light such as sunlight (natural light) or fluorescent light, and that the polymer is made more fluid under low-cost conditions with as low an irradiation dose and irradiation time as possible. From this viewpoint, the irradiation conditions for the above-mentioned polymer to become fluid are preferably an irradiation dose of 0.1 J / cm. 2 More than 200J / cm 2 Within the range of 0.1 J / cm 2 More than 100J / cm 2 Within the range below, more preferably 0.1 J / cm 2 More than 50J / cm 2 It is within the following range.
[0183] When the polymer is fluidized, the polymer may be heated in addition to the light irradiation. This allows the polymer to be fluidized with a lower irradiation dose. The heating temperature in this case is, for example, in the range of 20°C to 200°C, preferably in the range of 20°C to 150°C.
[0184] On the other hand, the conditions for immobilizing (resolidifying) the polymer of the present invention are preferably left at room temperature (within the range of 25±15° C.) (in a natural environment). In this case, it is preferable to leave it in a dark place, but it may be exposed to natural light or visible light such as fluorescent light. It is more preferable to apply heat during the immobilization process. Light may also be applied.
[0185] When the polymer is heated to make it non-fluid, the heating temperature is preferably in the range of 0°C or more and 200°C or less, more preferably in the range of 20°C or more and 150°C or less.
[0186] [Toner composition] One embodiment of the present invention is a toner containing the polymer of the present invention. By introducing the polymer of the present invention into a toner, it is possible to obtain a toner that can be fixed by light irradiation, has excellent fixability, and has high color reproducibility. The term "toner" refers to toner base particles or an aggregate of toner particles. The toner particles are preferably toner base particles to which an external additive has been added, but the toner base particles can also be used as they are as toner particles. In the present invention, when there is no particular need to distinguish between toner base particles, toner particles, and toner, they are also simply referred to as "toner".
[0187] The content of the polymer in the toner is determined by the amount of the azomethine structure (B 1 -Z 1 =Z 2 -B 2 ) and other structural units, from the viewpoint of efficient fluidization and image strength, it is, for example, in the range of 5 to 95% by mass based on the total amount of the binder resin, colorant, release agent, and polymer of the present invention that constitute the toner.
[0188] <Binding resin> The toner of the present invention may further contain a binder resin. The binder resin is a resin that does not have a structure derived from an azomethine derivative, i.e., a resin that does not have an azomethine structure (B 1 -Z 1 =Z 2 -B 2), and resins generally used as binder resins constituting toners can be used without any restrictions. Examples of binder resins that can be used include styrene resins, acrylic resins, styrene-acrylic resins, polyester resins, silicone resins, olefin resins, amide resins, and epoxy resins. These binder resins can be used alone or in combination of two or more.
[0189] Among these, from the viewpoint of having a low viscosity when melted and having high sharp melting properties, the binder resin preferably contains at least one selected from the group consisting of a styrene resin, an acrylic resin, a styrene-acrylic resin, and a polyester resin, and more preferably contains at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.
[0190] (styrene acrylic resin) The styrene-acrylic resin in the present invention is a polymer containing at least a structural unit derived from a styrene monomer and a structural unit derived from a (meth)acrylic acid ester monomer. Here, the styrene monomer is CH 2 =CH-C 6 H 5 In addition to styrene represented by the structural formula above, structures having known side chains or functional groups in the styrene structure are also included.
[0191] Examples of the styrene monomer include the same styrene monomers capable of forming the above-mentioned polymer.
[0192] The (meth)acrylic acid ester monomer is a monomer having a functional group having an ester bond in the side chain. 2 In addition to the acrylic ester monomer represented by =CHCOOR (R is an alkyl group), 2 =C(CH 3(Meth)acrylic acid in the (meth)acrylic acid ester monomer means acrylic acid and methacrylic acid.
[0193] Examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.
[0194] The styrene monomer and the (meth)acrylic acid ester monomer can be used either alone or in combination of two or more kinds.
[0195] The content of the structural unit derived from the styrene monomer and the structural unit derived from the (meth)acrylic acid ester monomer in the styrene-acrylic resin is not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point and glass transition temperature of the binder resin. Specifically, the content of the structural unit derived from the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total structural units constituting the styrene-acrylic resin. In addition, the content of the structural unit derived from the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total structural units constituting the styrene-acrylic resin.
[0196] The styrene-acrylic resin may further contain structural units derived from other monomers than the styrene monomer and the (meth)acrylic acid ester monomer, if necessary. Examples of other monomers include vinyl monomers. Below, examples of vinyl monomers that can be used in combination when forming the styrene-acrylic copolymer of the present invention are shown, but the vinyl monomers that can be used in combination are not limited to those shown below.
[0197] (1) Olefins Ethylene, propylene, isobutylene, etc. (2) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (3) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (4) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (5) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (6)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile and acrylamide, and the like.
[0198] It is also possible to prepare a resin having a crosslinked structure by using a polyfunctional vinyl monomer. Furthermore, it is also possible to use a vinyl monomer having an ionic dissociation group in the side chain. Specific examples of the ionic dissociation group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group. Specific examples of the vinyl monomer having these ionic dissociation groups are shown below.
[0199] Specific examples of vinyl monomers having a carboxyl group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.
[0200] When forming the styrene-acrylic resin used in the present invention, the contents of the styrene monomer and the (meth)acrylic acid ester monomer are not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point temperature and the glass transition temperature of the binder resin. Specifically, the content of the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total monomers constituting the styrene-acrylic resin. In addition, the content of the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total monomers constituting the styrene-acrylic resin.
[0201] The method for forming the styrene-acrylic resin is not particularly limited, and may be a method of polymerizing a monomer using a known oil-soluble or water-soluble polymerization initiator. If necessary, a known chain transfer agent such as n-octyl mercaptan may be used. As the oil-soluble polymerization initiator, for example, the following azo-based or diazo-based polymerization initiator or peroxide-based polymerization initiator may be used.
[0202] Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile.
[0203] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.
[0204] In addition, when forming styrene-acrylic resin particles by emulsion polymerization, a water-soluble radical polymerization initiator can be used. Examples of the water-soluble radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, and hydrogen peroxide.
[0205] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 12 hours.
[0206] The styrene-acrylic resin particles formed by emulsion polymerization can be made to have two or more layers made of resins with different compositions. In this case, the manufacturing method can be a multi-stage polymerization method in which a polymerization initiator and a polymerizable monomer are added to a dispersion of resin particles prepared by emulsion polymerization treatment (first stage polymerization) according to a conventional method, and this system is polymerized (second stage, third stage polymerization).
[0207] (polyester resin) The polyester resin is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (a polyvalent carboxylic acid component) and a divalent or higher alcohol (a polyhydric alcohol component). The polyester resin may be amorphous or crystalline.
[0208] The valence of each of the polyvalent carboxylic acid component and the polyhydric alcohol component is preferably 2 to 3, and more preferably 2. That is, the polyvalent carboxylic acid component preferably contains a dicarboxylic acid component, and the polyhydric alcohol component preferably contains a dialcohol component.
[0209] Examples of the dicarboxylic acid component include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and methylenesuccinic acid. unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid; unsaturated aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylenediacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and anthracenedicarboxylic acid; and lower alkyl esters and acid anhydrides of these may also be used. The dicarboxylic acid component may be used alone or in combination of two or more.
[0210] In addition, trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid, and their anhydrides or alkyl esters having 1 to 3 carbon atoms can also be used.
[0211] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, and neopentanediol. Examples of the diol component include saturated aliphatic diols such as ethyl glycol; unsaturated aliphatic diols such as 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, and 9-octadecene-7,12-diol; and aromatic diols such as bisphenols such as bisphenol A and bisphenol F, and alkylene oxide adducts of bisphenols such as ethylene oxide adducts and propylene oxide adducts thereof, and derivatives thereof can also be used. The diol component may be used alone or in combination of two or more kinds.
[0212] The method for producing the polyester resin is not particularly limited, and the polyester resin can be produced by polycondensing (esterifying) the polyvalent carboxylic acid component and the polyhydric alcohol component using a known esterification catalyst.
[0213] Catalysts that can be used in the production of polyester resins include alkali metal compounds such as sodium and lithium; compounds containing Group 2 elements such as magnesium and calcium; compounds of metals such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds. Specific examples of tin compounds include dibutyltin oxide (dibutyltin oxide), tin octoate, tin dioctoate, and salts thereof. Titanium compounds include tetra-normal-butyl titanate (Ti(On-Bu) 4Examples of the titanium compounds include titanium alkoxides such as titanium tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanol aminate. Examples of the germanium compounds include germanium dioxide. Examples of the aluminum compounds include polyaluminum hydroxide, aluminum alkoxides, and tributylaluminate. These compounds may be used alone or in combination of two or more.
[0214] The polymerization temperature is not particularly limited, but is preferably 70 to 250° C. The polymerization time is also not particularly limited, but is preferably 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0215] When the toner of the present invention contains a binder resin in addition to the polymer of the present invention, the content ratio of the polymer to the binder resin is not particularly limited.
[0216] From the viewpoints of fixability and heat-resistant storage stability, the glass transition temperature (Tg) of the toner is preferably 25 to 100° C., and more preferably 30 to 80° C. The glass transition temperature (Tg) of the toner can be adjusted by the molecular weight of the polymer, and when a structural unit other than a structural unit containing a group having an azomethine structure is contained, by the type and content of the structural unit. When the toner contains a binder resin, it can be further adjusted by the content ratio of the polymer and the binder resin, the type and molecular weight of the binder resin, etc.
[0217] The toner of the present invention may be particles having a single layer structure or particles having a core-shell structure. The types of binder resins used for the core particles and shell part of the core-shell structure are not particularly limited.
[0218] <Coloring agent> The toner of the present invention may further contain a colorant. Since the polymer of the present invention does not have a significant coloring, a toner having high color reproducibility of the colorant can be obtained. As the colorant, generally known dyes and pigments can be used.
[0219] Examples of colorants for obtaining black toner include carbon black, magnetic materials, iron-titanium composite oxide black, etc. Examples of carbon black include channel black, furnace black, acetylene black, thermal black, and lamp black, and examples of magnetic materials include ferrite and magnetite.
[0220] Colorants for obtaining yellow toners include dyes such as CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; and pigments such as CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, and 185.
[0221] Colorants for obtaining magenta toner include dyes such as CI Solvent Red 1, 49, 52, 58, 63, 111, and 122; and pigments such as CI Pigment Red 5, 48:1, 53:1, 57:1, 122, 139, 144, 149, 166, 177, 178, and 222.
[0222] Colorants for obtaining cyan toner include dyes such as CI Solvent Blue 25, 36, 60, 70, 93, and 95; and pigments such as CI Pigment Blue 1, 7, 15, 15:3, 60, 62, 66, and 76.
[0223] The colorants for obtaining the toner of each color may be used alone or in combination of two or more kinds for each color.
[0224] The content of the colorant in the toner particles (toner base particles) before addition of external additives is preferably 0.5 to 20% by mass, and more preferably 2 to 10% by mass.
[0225] <Release agent> The toner according to the present invention may further contain a release agent. By incorporating a release agent into the toner, a toner having superior fixability and color reproducibility can be obtained when heat fixing is performed together with light irradiation.
[0226] The release agent used is not particularly limited, and various known waxes can be used. Examples of the wax include polyolefins such as low molecular weight polypropylene, polyethylene, or oxidized low molecular weight polypropylene, polyethylene, paraffin wax, and synthetic ester wax. Among them, it is preferable to use paraffin wax from the viewpoint of improving the storage stability of the toner.
[0227] The content of the release agent in the toner base particles is preferably 1 to 30% by mass, and more preferably 3 to 15% by mass.
[0228] <Charge control agent> The toner according to the present invention may contain a charge control agent. The charge control agent used is a substance capable of imparting positive or negative charge by frictional charging, and is colorless, and is not particularly limited. Any of various known positively and negatively chargeable charge control agents can be used.
[0229] The content of the charge control agent in the toner base particles is preferably 0.01 to 30% by mass, and more preferably 0.1 to 10% by mass.
[0230] <External additives> In order to improve the fluidity, chargeability, cleaning properties, etc. of the toner, external additives such as a fluidizing agent, a cleaning aid, etc., which are so-called post-treatment agents, may be added to the toner base particles to form the toner according to the present invention.
[0231] Examples of the external additive include inorganic oxide particles such as silica particles, alumina particles, and titanium oxide particles, inorganic stearic acid compound particles such as aluminum stearate particles and zinc stearate particles, and inorganic titanic acid compound particles such as strontium titanate particles and zinc titanate particles. If necessary, these inorganic particles may be hydrophobized. These may be used alone or in combination of two or more.
[0232] Among these, preferred external additives are, for example, sol-gel silica particles, silica particles whose surfaces have been hydrophobized (hydrophobic silica particles), or titanium oxide particles (hydrophobic titanium oxide particles), and it is more preferred to use at least two or more types of external additives among these.
[0233] The number average primary particle size of the external additive is preferably within the range of 1 to 200 nm, and more preferably 10 to 180 nm.
[0234] The amount of these external additives added is preferably 0.05 to 5% by mass, and more preferably 0.1 to 3% by mass, in the toner.
[0235] <Average particle size of toner> The average particle size of the toner (and the average particle size of the toner base particles) is preferably 4 to 20 μm, more preferably 5 to 15 μm, in terms of volume-based median diameter (D50). When the volume-based median diameter (D50) is within the above range, the transfer efficiency is increased, and the image quality of halftones and fine lines, dots, etc. is improved.
[0236] The volume-based median diameter (D50) can be measured and calculated using a measuring device consisting of a "Coulter Counter 3" (Beckman Coulter, Inc.) connected to a computer system (Beckman Coulter, Inc.) equipped with the data processing software "Software V3.51."
[0237] Specifically, 0.02 g of the measurement sample (toner or toner base particles) is added to 20 mL of surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing surfactant components 10 times with pure water in order to disperse toner particles), and after mixing, ultrasonic dispersion is performed for 1 minute to prepare a dispersion liquid. This dispersion liquid is then pipetted into a beaker containing an "ISOTON II" (manufactured by Beckman Coulter, Inc.) in the sample stand until the concentration indicated on the measuring device reaches 8%.
[0238] Here, by setting the display concentration to the above value, a reproducible measurement value can be obtained. In the measurement device, the number of measured particles is set to 25,000, the aperture diameter is set to 50 μm, the measurement range of 1 to 30 μm is divided into 256 parts to calculate the frequency value, and the particle size of the largest volume cumulative fraction, which is 50%, is set as the volume-based median diameter (D50).
[0239] [Toner manufacturing method] The method for producing the toner of the present invention is not particularly limited. For example, when the toner is made from only the polymer of the present invention, a production method including pulverizing the polymer using an apparatus such as a hammer mill, a feather mill, or a counter jet mill, and then classifying the polymer to a desired particle size using a dry classifier such as a spin air sieve, a classifier, or a micron classifier can be used. When a toner further containing a colorant is produced, the polymer and the colorant are dissolved in a solvent in which both the polymer of the present invention and the colorant are soluble to obtain a solution, the solvent is removed, and then the solution is pulverized and classified in the same manner as above.
[0240] In particular, the toner containing the polymer of the present invention and, if necessary, a binder and a colorant is preferably produced by a production method utilizing an emulsion aggregation method, which allows easy control of particle size and shape.
[0241] Such a manufacturing method is as follows: (1A) a binder resin particle dispersion preparation step for preparing a binder resin particle dispersion as required; (1B) a polymer particle dispersion preparation step for preparing a polymer particle dispersion of the present invention; (1C) A colorant particle dispersion preparation step of preparing a colorant particle dispersion as required. (2) An association step in which a flocculant is added to an aqueous medium in which polymer particles, and if necessary, binder resin particles and colorant particles are present, to promote salting out and simultaneously cause aggregation and fusion to form associated particles. (3) Aging process to form toner base particles by controlling the shape of aggregated particles (4) A filtering and washing process for filtering the toner base particles from the aqueous medium and removing surfactants and the like from the toner base particles. (5) A drying process for drying the washed toner base particles. (6) Additive addition step of adding additives to the dried toner base particles It is preferable that the method includes each of the steps of:
[0242] The steps (1A) to (1C) are described below.
[0243] (1A) Binder resin particle dispersion preparation process In this process, resin particles are formed by a conventional emulsion polymerization or the like, and the resin particles are aggregated and fused to form binder resin particles. As an example, polymerizable monomers constituting the binder resin are introduced into an aqueous medium, dispersed therein, and polymerized by a polymerization initiator to prepare a dispersion of binder resin particles.
[0244] As a method for obtaining a binder resin particle dispersion, in addition to the above-mentioned method of polymerizing a polymerizable monomer in an aqueous medium by a polymerization initiator, for example, a method of performing a dispersion treatment in an aqueous medium without using a solvent, or a method of dissolving a crystalline resin in a solvent such as ethyl acetate to prepare a solution, emulsifying and dispersing the solution in an aqueous medium using a disperser, and then performing a solvent removal treatment, can be mentioned.
[0245] In this case, if necessary, a release agent may be added to the binder resin in advance. For dispersion, it is also preferable to carry out the polymerization in the presence of a known surfactant (for example, an anionic surfactant such as polyoxyethylene (2) dodecyl ether sodium sulfate, sodium dodecyl sulfate, or dodecylbenzenesulfonic acid).
[0246] The volume-based median diameter of the binder resin particles in the dispersion is preferably 50 to 300 nm. The volume-based median diameter of the binder resin particles in the dispersion can be measured by a dynamic light scattering method using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).
[0247] (1B) Polymer particle dispersion preparation process The polymer particle dispersion preparation step is a step of dispersing the polymer of the present invention in the form of fine particles in an aqueous medium to prepare a dispersion of the polymer particles.
[0248] In preparing the dispersion of the polymer particles, first, an emulsion of the polymer is prepared. For example, the emulsion of the polymer is prepared by dissolving the polymer in an organic solvent and then emulsifying the obtained solution in an aqueous medium.
[0249] The method for dissolving the polymer in the organic solvent is not particularly limited, and examples thereof include a method of adding the polymer to the organic solvent and stirring and mixing the polymer so as to dissolve it. The amount of the polymer added is preferably 5 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the organic solvent.
[0250] Next, the obtained solution of the polymer is mixed with an aqueous medium and stirred using a known dispersing machine such as a homogenizer, whereby the polymer becomes droplets and is emulsified in the aqueous medium to prepare an emulsion of the polymer.
[0251] The amount of the polymer solution added is preferably 10 parts by mass or more and 110 parts by mass or less with respect to 100 parts by mass of the aqueous medium.
[0252] The temperatures of the polymer solution and the aqueous medium when the polymer solution and the aqueous medium are in a temperature range below the boiling point of the organic solvent, and are preferably from 20° C. to 80° C., more preferably from 30° C. to 75° C. When the polymer solution and the aqueous medium are mixed, the temperatures of the polymer solution and the aqueous medium may be the same or different, and are preferably the same.
[0253] Regarding the stirring conditions of the dispersing machine, when the capacity of the stirring vessel is 1 to 3 L, for example, the rotation speed is preferably 7000 rpm or more and 20000 rpm or less, and the stirring time is preferably 10 minutes or more and 30 minutes or less.
[0254] The dispersion of the polymer particles is prepared by removing the organic solvent from the polymer emulsion. Examples of the method for removing the organic solvent from the polymer emulsion include known methods such as blowing air, heating, reducing pressure, or a combination of these.
[0255] As an example, the polymer emulsion is heated, for example, in an inert gas atmosphere such as nitrogen, preferably at 25° C. to 90° C., more preferably at 30° C. to 80° C., until, for example, about 80% by mass to 95% by mass of the initial amount of organic solvent is removed, thereby removing the organic solvent. As a result, the organic solvent is removed from the aqueous medium, and a dispersion of the polymer particles in which the polymer particles are dispersed in the aqueous medium is prepared.
[0256] The mass average particle diameter of the polymer particles in the dispersion of the polymer particles is preferably 90 nm or more and 1200 nm or less. The mass average particle diameter can be set within the above range by appropriately adjusting the viscosity when the polymer is mixed with an organic solvent, the mixing ratio of the polymer solution to the aqueous medium, the stirring speed of a disperser when preparing the polymer emulsion, etc. The mass average particle diameter of the polymer particles in the dispersion of the polymer particles can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0257] <Organic solvent> The organic solvent used in this step is not particularly limited as long as it can dissolve the polymer.Specific examples of the organic solvent include esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, diisopropyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, saturated hydrocarbons such as hexane and heptane, and halogenated hydrocarbons such as dichloromethane, dichloroethane, and carbon tetrachloride.
[0258] Such organic solvents can be used alone or in combination of two or more kinds. Among these organic solvents, ketones and halogenated hydrocarbons are preferred, and methyl ethyl ketone and dichloromethane are more preferred.
[0259] <Aqueous medium> The aqueous medium used in this step may be water, or an aqueous medium containing water as the main component and water-soluble solvents such as alcohols and glycols, and optional components such as surfactants and dispersants. The aqueous medium used is preferably a mixture of water and a surfactant.
[0260] Examples of the surfactant include cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of the cationic surfactant include dodecyl ammonium chloride, dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, and hexadecyl trimethyl ammonium bromide. Examples of the anionic surfactant include fatty acid soaps such as sodium stearate and sodium dodecanoate, sodium dodecyl benzene sulfonate, and sodium dodecyl sulfate. Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl ether, polyoxyethylene sorbitan monooleate ether, and monodecanoyl sucrose.
[0261] Such surfactants can be used alone or in combination of two or more. Among the surfactants, anionic surfactants are preferred, and sodium dodecylbenzenesulfonate is more preferred.
[0262] The amount of the surfactant added is preferably from 0.01 to 10 parts by mass, more preferably from 0.04 to 1 part by mass, based on 100 parts by mass of the aqueous medium.
[0263] (1C) Colorant particle dispersion preparation process The colorant particle dispersion preparation step is a step of dispersing a colorant in the form of fine particles in an aqueous medium to prepare a colorant particle dispersion.
[0264] The colorant can be dispersed by utilizing mechanical energy. The median diameter based on the number of colorant particles in the dispersion is preferably 10 to 300 nm, and more preferably 50 to 200 nm. The median diameter based on the number of colorant particles can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0265] The steps from (2) association step to (6) external additive addition step can be carried out according to various conventionally known methods.
[0266] The flocculant used in the (2) association step is not particularly limited, but is preferably selected from metal salts. Examples of metal salts include monovalent metal salts such as salts of alkali metals such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum. Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, and manganese sulfate. Among these, it is particularly preferable to use divalent metal salts because they can promote flocculation with a smaller amount. These can be used alone or in combination of two or more.
[0267] [Developer] The toner according to the present invention can be suitably used in various cases, including when it contains a magnetic material and is used as a one-component magnetic toner, when it is mixed with a so-called carrier and used as a two-component developer, and when it is used alone as a non-magnetic toner.
[0268] As the magnetic material, for example, magnetite, γ-hematite, or various ferrites can be used.
[0269] The carrier contained in the two-component developer may be magnetic particles made of conventionally known materials such as metals such as iron, steel, nickel, cobalt, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead.
[0270] The carrier may be a coated carrier in which the surface of the magnetic particles is coated with a coating agent such as a resin, or a resin-dispersed carrier in which magnetic powder is dispersed in a binder resin. The resin for coating is not particularly limited, but for example, olefin resin, acrylic resin, styrene resin, styrene-acrylic resin, silicone resin, polyester resin, or fluororesin is used. The resin for constituting the resin-dispersed carrier particles is not particularly limited, and known resins can be used, for example, acrylic resin, styrene-acrylic resin, polyester resin, fluororesin, phenolic resin, etc. can be used.
[0271] The volume-based median diameter of the carrier is preferably 20 to 100 μm, and more preferably 25 to 80 μm. The volume-based median diameter of the carrier can be measured typically by a laser diffraction particle size distribution measuring device "HELOS" (manufactured by SYMPATEC) equipped with a wet disperser.
[0272] The mixed amount of the toner is preferably 2 to 10% by mass, with the total mass of the toner and carrier being 100% by mass.
[0273] [Image forming method] The toner of the present invention can be used in various known electrophotographic image forming methods. For example, it can be used in monochrome image forming methods and full-color image forming methods. In the full-color image forming method, it can be applied to any image forming method, such as a four-cycle image forming method that is composed of four types of color developing devices for yellow, magenta, cyan, and black, and one photoconductor, and a tandem image forming method that is equipped with image forming units having color developing devices and photoconductors for each color, respectively.
[0274] That is, an image forming method according to one embodiment of the present invention includes: 1) a step of forming a toner image made of the toner of the present invention on a recording medium; and 2) a step of irradiating the toner image with light to soften the toner image.
[0275] Regarding step 1) In this process, a toner image made of the toner of the present invention is formed on a recording medium.
[0276] (Recording medium) The recording medium is a member for holding a toner image. Examples of the recording medium include plain paper, high-quality paper, art paper, coated printing paper such as coated paper, commercially available Japanese paper and postcard paper, resin films for overhead projectors or packaging materials, and cloth.
[0277] The recording medium may be in the form of a sheet (foliage) having a predetermined size, or may be in the form of a long piece that is wound up in a roll after the toner image is fixed thereon.
[0278] As described later, the toner image can be formed, for example, by transferring the toner image on the photoconductor onto a recording medium.
[0279] Regarding step 2) In this process, the formed toner image is irradiated with light to soften the toner image, thereby allowing the toner image to adhere to the recording medium. Heating may be performed in addition to the light irradiation.
[0280] The wavelength of the irradiated light is not particularly limited as long as it can sufficiently soften the toner image by photothermal conversion by the polymer in the toner, but is preferably 280 nm or more and 480 nm or less. If it is in the above range, the toner image can be softened more efficiently. From the same viewpoint, the amount of light irradiation is preferably 0.1 to 200 J / cm. 2 , more preferably 0.1 to 100 J / cm 2 , and more preferably 0.1 to 50 J / cm 2 It is.
[0281] The light irradiation can be carried out using a light source such as a light emitting diode (LED) or a laser light source, as described below.
[0282] After the step 2), a step 3) of pressing the softened toner image may be further carried out, if necessary.
[0283] Regarding step 3) In this process, the softened toner image is pressed.
[0284] The pressure when pressing the toner image on the recording medium is not particularly limited, but is preferably 0.01 to 5.0 MPa, and more preferably 0.05 to 1.0 MPa. By setting the pressure to 0.01 MPa or more, the deformation amount of the toner image can be increased, so that the contact area between the toner image and the recording paper S increases, and it is easy to further improve the fixability of the image. In addition, by setting the pressure to 5.0 MPa or less, shock noise during pressing can be suppressed.
[0285] The pressurizing step may be carried out before or simultaneously with the step of irradiating the toner image with light and softening it (step 2) described above), but it is preferable to carry it out after the light irradiation, since this allows pressure to be applied to the toner image that has already been softened, thereby further improving the fixability of the image.
[0286] In the pressurizing step, the softened toner image may be further heated, that is, the pressurizing step may be performed while the toner image is being heated.
[0287] The heating temperature of the toner image (the surface temperature of the toner image during heating) is preferably (Tg+20) to (Tg+100)° C., and more preferably (Tg+25) to (Tg+80)° C., where Tg is the glass transition temperature of the toner. If the surface temperature of the toner image is (Tg+20)° C. or higher, the toner image is easily deformed by pressure, and if it is (Tg+100)° C. or lower, hot offset is easily suppressed. Note that hot offset refers to a phenomenon in which part of the toner is transferred to a pressure member such as a roller during the fixing process, causing the toner layer to break up.
[0288] Furthermore, before the step 2), a step 4) of heating the toner image in advance may be further carried out as necessary. By carrying out the step 4) of heating the toner image in advance before the step 2), the sensitivity of the polymer of the present invention to light can be further increased. This makes it easy to promote melting or softening of the toner image by light irradiation, since the sensitivity to light is unlikely to be impaired even in the case of a polymer.
[0289] The image forming method of the present invention can be carried out by using, for example, the following image forming apparatus.
[0290] Fig. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. However, the image forming apparatus used in the present invention is not limited to the following form and illustrated example. Fig. 1 shows an example of a monochrome image forming apparatus 100, but the present invention can also be applied to a color image forming apparatus.
[0291] The image forming apparatus 100 is an apparatus for forming an image on a recording paper S as a recording medium, and is equipped with an image reading device 71 and an automatic document feeder 72, and performs image formation on the recording paper S transported by a paper transport system 7 using an image forming unit 10, an irradiation unit 40, and a pressing unit 9.
[0292] Furthermore, while image forming apparatus 100 uses recording paper S as a recording medium, the medium on which an image is formed may be something other than paper.
[0293] An original d placed on the platen of the automatic document feeder 72 is scanned and exposed by the optical system of the scanning exposure device of the image reading device 71 and read into the image sensor CCD. An analog signal photoelectrically converted by the image sensor CCD is subjected to analog processing, A / D conversion, shading correction, image compression processing, etc. in the image processing unit 20, and then input to the exposure device 3 of the image forming unit 10.
[0294] The paper transport system 7 includes a plurality of trays 16, a plurality of paper feed units 11, transport rollers 12, a transport belt 13, etc. The trays 16 each store recording paper S of a predetermined size, and operate the paper feed unit 11 of the specified tray 16 in response to an instruction from the control unit 90 to supply the recording paper S. The transport rollers 12 transport the recording paper S sent out from the tray 16 by the paper feed unit 11 or the recording paper S brought in from the manual paper feed unit 15 to the image forming unit 10.
[0295] The image forming unit 10 is configured by arranging a charger 2, an exposure unit 3, a developing unit 4, a transfer unit 5 and a cleaning unit 8 in this order around the photoreceptor 1 along the direction of rotation of the photoreceptor 1.
[0296] The photoconductor 1, which is an image carrier, is an image carrier having a photoconductive layer formed on its surface, and is configured to be rotatable in the direction of the arrow in Fig. 1 by a driving device (not shown). A thermo-hygrometer 17 that detects the temperature and humidity inside the image forming apparatus 100 is provided near the photoconductor 1.
[0297] The charger 2 uniformly charges the surface of the photoreceptor 1, thereby uniformly charging the surface of the photoreceptor 1. The exposure unit 3 is equipped with a beam emission source such as a laser diode, and irradiates the charged surface of the photoreceptor 1 with a beam of light, thereby dissipating the charge in the irradiated area and forming an electrostatic latent image on the photoreceptor 1 according to the image data. The development unit 4 supplies the toner contained therein to the photoreceptor 1, and creates a toner image on the surface of the photoreceptor 1 based on the electrostatic latent image.
[0298] The transfer unit 5 faces the photoreceptor 1 via the recording paper S, and transfers the toner image onto the recording paper S. The cleaning unit 8 includes a blade 85. The blade 85 cleans the surface of the photoreceptor 1 to remove developer remaining on the surface of the photoreceptor 1.
[0299] The recording paper S onto which the toner image has been transferred is transported by a transport belt 13 to a pressing unit 9. The pressing unit 9 may be installed arbitrarily, and performs a fixing process on the recording paper S onto which the toner image has been transferred by applying pressure alone or heat and pressure with pressure members 91 and 92, thereby fixing the image onto the recording paper S. The recording paper S onto which the image has been fixed is transported by transport rollers to a paper discharge unit 14, and is discharged from the paper discharge unit 14 to the outside of the machine.
[0300] In addition, the image forming apparatus 100 is equipped with a paper inversion section 24, so that the recording paper S that has been subjected to the heat fixing process is transported to the paper inversion section 24 just before the paper discharge section 14, and the recording paper S is either inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10, so that images can be formed on both sides of the recording paper S.
[0301] <Irradiation unit> FIG. 2 is a schematic diagram of the irradiation unit 40 in the image forming apparatus 100. As shown in FIG.
[0302] The image forming apparatus 100 according to one embodiment of the present invention includes an irradiation unit 40. The irradiation unit 40 irradiates light onto a toner image formed on a recording paper S. Examples of devices constituting the irradiation unit 40 include a light emitting diode (LED) and a laser light source.
[0303] The irradiation section 40 irradiates the toner image formed on the recording medium with light to soften the toner image. The conditions of the light irradiation are not particularly limited as long as they melt and fluidize the polymer of the present invention contained in the toner of the developer. The wavelength of the light irradiated to the toner image may be sufficient to sufficiently fluidize the polymer, and is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. The amount of light irradiated in the irradiation section may also be sufficient to sufficiently fluidize the polymer, and is, for example, 0.1 J / cm. 2 More than 200J / cm 2 Within the range below, preferably 0.1 J / cm 2 More than 100J / cm 2 Within the range of 0.1 J / cm 2 More than 50J / cm 2 It is within the following range.
[0304] When the toner image is softened by irradiating the toner image with light from the irradiation unit 40, the toner image may be heated by a heating member (not shown) in addition to the light irradiation. This allows the toner image to be softened and melted more efficiently. The heating temperature at this time is, for example, in the range of 20°C to 200°C, and preferably in the range of 20°C to 150°C.
[0305] The softened toner image can be solidified and fixed to the recording medium by leaving it at room temperature (within the range of 25±15° C.), heating it, or irradiating it with visible light. As described below, the fixing step preferably further includes a step of applying pressure to the softened toner image. In the pressurizing step, it is preferable to further heat the softened toner image.
[0306] The irradiation unit 40 irradiates light toward the first surface of the recording paper S holding the toner image, which is on the photosensitive member side, and is positioned on the photosensitive member side relative to the surface of the recording paper S nipped between the photosensitive member 1 and the transfer unit (transfer roller) 5.
[0307] The irradiation unit 40 is disposed downstream of the nip position between the photoconductor 1 and the transfer unit 5 in the paper transport direction and upstream of the pressure bonding unit 9 in the paper transport direction.
[0308] According to an image forming method according to an embodiment of the present invention, the photoconductor 1 is charged by applying a uniform potential to it using the charger 2, and then the photoconductor 1 is scanned with a light beam irradiated by the exposure device 3 based on original image data to form an electrostatic latent image. Next, the developing unit 4 supplies a developer containing the toner of the present invention onto the photoconductor 1.
[0309] When recording paper S is transported from tray 16 to image forming unit 10 in time with the rotation of photoconductor 1 causing the toner image carried on the surface of photoconductor 1 to reach the position of transfer unit 5, the toner image on photoconductor 1 is transferred onto recording paper S nipped between transfer unit 5 and photoconductor 1 by a transfer bias applied to transfer unit 5.
[0310] The transfer unit 5 also functions as a pressure member, and can transfer the toner image from the photoreceptor 1 to the recording paper S while reliably bringing the polymer contained in the toner image into close contact with the recording paper S.
[0311] After the toner image is transferred onto the recording paper S, the blade 85 of the cleaning unit 8 removes the developer remaining on the surface of the photoconductor 1 .
[0312] In the process in which the recording paper S onto which the toner image has been transferred is transported by the transport belt 13 to the pressing unit 9, the irradiation unit 40 irradiates light onto the toner image transferred onto the recording paper S. By irradiating light onto the toner image on the first surface of the recording paper S by the irradiation unit 40, the toner image can be melted more reliably, and the fixability of the toner image to the recording paper S can be improved.
[0313] When the recording paper S carrying the toner image reaches the pressing unit 9 by the conveyor belt 13, the pressure members 91 and 92 press the toner image onto the first surface of the recording paper S. Before the toner image is fixed by the pressing unit 9, it is softened by light irradiation by the irradiation unit 40, so that energy consumption for pressing the image onto the recording paper S can be reduced.
[0314] The pressure when pressing the toner image is as described above. The pressing step may be performed before, simultaneously with, or after the step of softening the toner image by irradiating light. From the viewpoint of being able to pressurize a toner image in a pre-softened state and facilitating the enhancement of image strength, it is preferable to perform the pressing step after the light irradiation.
[0315] In addition, the pressure member 91 can heat the toner image on the recording paper S when the recording paper S passes between the pressure members 91 and 92. The toner image softened by the light irradiation is further softened by this heating, and as a result, the fixability of the toner image to the recording paper S is further improved.
[0316] The heating temperature of the toner image is as described above. The heating temperature of the toner image (surface temperature of the toner image) can be measured by a non-contact temperature sensor. Specifically, for example, a non-contact temperature sensor may be installed at a position where the recording medium is discharged from the pressure member, and the surface temperature of the toner image on the recording medium may be measured.
[0317] The toner image pressed by the pressure members 91 and 92 is solidified and fixed onto the recording paper S.
[0318] (Photoresponsive adhesive) Since the polymer of the present invention becomes fluid when irradiated with light and becomes non-fluid reversibly, a photoresponsive adhesive (photosensitive adhesive) that can be used repeatedly can be produced using the polymer of the present invention. For example, it can be applied to various bonding techniques as a photoresponsive adhesive that can be repeatedly attached and detached by light in response to changes in viscosity (friction coefficient). That is, one embodiment of the present invention is a photoresponsive adhesive that includes the polymer of the present invention.
[0319] The light-responsive adhesive of the present invention can be used for temporary fixing that allows repeated use, and is also suitable for recycling, but is not limited thereto.
[0320] (Photoswitching Materials) Since the polymer of the present invention is fluidized by light irradiation and reversibly non-fluidized, a light-switching material can be prepared using the polymer of the present invention. For example, a light-switching material can be prepared by utilizing the change in color or polarity, mass transfer, change in orientation, change in viscosity, or change in surface tension associated with photoisomerization. For example, in liquid crystal materials, it is possible to apply the material to patterning drawings that can be repeatedly rewritten in response to the change in molecular orientation associated with photoisomerization. In addition, for example, the change in surface tension associated with light irradiation and the resulting mass transfer can be utilized to perform microfabrication of the surface of a polymer film. That is, one embodiment of the present invention is a light-switching material that includes the polymer of the present invention.
[0321] The optical switching material of the present invention can be used for liquid crystal display materials and surface processing of polymer films, but is not limited thereto. EXAMPLES
[0322] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0323] [Example 4] <Synthesis of azomethine derivative monomer 6> 4-Aminophenol (5 g, 0.046 mol), 5-methylthiophene-2-carboxaldehyde (5.8 g, 0.046 mol), and 100 ml of ethanol were added to a 100 ml four-neck flask and heated and stirred. The reaction solution was suction filtered, and the resulting powder was washed with cooled ethanol. Further, recrystallization was performed with methanol / ethanol to obtain target product 1.
[0324] [ka]
[0325] Next, in a 200 ml four-neck flask, the target product 1 (5 g, 0.023 mol) obtained above was dissolved in 25 ml of dimethylformamide (DMF). To this, 4.88 g (0.035 mol) of potassium carbonate was added, and the mixture was stirred while maintaining the temperature at 30°C. To this, 10.2 mg (0.06 mmol) of potassium iodide and 6-chloro-1-hexanol (3.54 g, 0.026 mol) were added, and the mixture was reacted at 110°C. This was cooled to room temperature, added to 650 g of ice, and then filtered. The crystals were dispersed in 400 ml of water, stirred overnight, washed, filtered, and dried. Furthermore, recrystallization was performed with ethanol to obtain target product 2.
[0326] [ka]
[0327] Next, the target product 2 (3 g, 0.001 mol) obtained above, 1.34 ml (0.001 mol) of triethylamine, and 30 ml of dichloromethane were added to a 100 ml four-neck flask. At this time, the raw materials were in a dispersed state. While maintaining the internal temperature at 0°C, a solution of 1.04 g (0.011 mol) of acrylic acid chloride dissolved in 10 ml of dichloromethane was added dropwise while maintaining the internal temperature at 0 to 5°C. As the mixture was added dropwise, the raw materials dissolved.
[0328] After the dropwise addition, the reaction solution was returned to room temperature and stirred. After the reaction was completed, the dichloromethane was concentrated and removed, and the solution was dissolved in ethyl acetate and washed with dilute hydrochloric acid, aqueous sodium bicarbonate solution, and saturated saline. The organic layer was dried over magnesium sulfate and then concentrated. The orange crystals obtained were purified using a silica gel column (ethyl acetate / heptane=1 / 5) to obtain azomethine derivative monomer 6 having structural unit 6 in Table 1 below.
[0329] [ka]
[0330] <Synthesis of Polymer 4> In a 100 ml four-neck flask, 1.5 g (4.04 mmol) of the azomethine derivative monomer 6 obtained above, 5 mg (0.023 mmol) of 4-cyanopentanoic acid dithiobenzoate, and 1 mg (0.006 mmol) of AIBN were dissolved in 4 ml of anisole. Then, after creating an argon gas atmosphere by freeze degassing, the mixture was heated to 75°C and polymerized by stirring. 40 ml of methanol was gradually added dropwise to the obtained polymer solution, and then THF was added to remove unreacted azomethine derivative monomer 6. The separated polymer solution was dried in a vacuum drying oven at 40°C for 24 hours to obtain polymer 4. The number average molecular weight Mn of the obtained polymer 4 was measured by GPC and found to be 7300.
[0331] [ka]
[0332] <Preparation of Polymer Particle Dispersion 4> 80 parts by mass of dichloromethane and 20 parts by mass of the polymer 4 obtained above were mixed and stirred while being heated at 50° C. to obtain a solution containing polymer 4. A mixed liquid of 99.5 parts by mass of distilled water heated to 50° C. and 0.5 parts by mass of a 20% by mass aqueous solution of sodium dodecylbenzenesulfonate was added to 100 parts by mass of the obtained solution. Thereafter, the mixture was emulsified by stirring at 16,000 rpm for 20 minutes using a homogenizer (manufactured by Heidolph) equipped with a shaft generator 18F to obtain an emulsion of polymer 4.
[0333] The obtained emulsion was charged into a separable flask, and the organic solvent was removed by heating and stirring at 40° C. for 90 minutes while supplying nitrogen into the gas phase, to obtain polymer particle dispersion 4. The particle size of the polymer particles in polymer particle dispersion 4 was measured using an electrophoretic light scattering photometer “ELS-800” (manufactured by Otsuka Electronics Co., Ltd.) and found to be 155 nm in mass average particle size.
[0334] (Preparation of Black Colorant Particle Dispersion (Bk-1)) 11.5 parts by mass of sodium n-dodecyl sulfate was dissolved in 160 parts by mass of pure water, 25 parts by mass of carbon black "Mogul L (manufactured by Cabot Corporation)" was gradually added, and then the mixture was dispersed using "Clearmix (registered trademark) W Motion CLM-0.8 (manufactured by M Technique Co., Ltd.)" to prepare a black colorant particle dispersion (Bk-1). The volume-based median diameter of the colorant particles in the black colorant particle dispersion (Bk-1) was 110 nm.
[0335] <Preparation of Toner 4> The polymer particle dispersion 4 prepared above (602 parts by mass, calculated as solid content), the black colorant particle dispersion (Bk-1) (52 parts by mass, calculated as solid content), and 900 parts by mass of ion-exchanged water were charged into a reaction apparatus equipped with a stirrer, a temperature sensor, and a cooling tube. The temperature inside the vessel was kept at 30° C., and a 5 mol / L aqueous solution of sodium hydroxide was added to adjust the pH to 10.
[0336] Next, an aqueous solution of 2 parts by mass of magnesium chloride hexahydrate dissolved in 1000 parts by mass of ion-exchanged water was added dropwise under stirring over a period of 10 minutes, and then heating was started. The temperature of this system was raised to 70°C over a period of 60 minutes, and the particle growth reaction was continued while maintaining the temperature at 70°C. In this state, the particle size of the associated particles was measured using a "Multisizer 3" (manufactured by Beckman Coulter, Inc.), and when the volume-based median diameter (D50) reached 6.5 μm, an aqueous solution of 190 parts by mass of sodium chloride dissolved in 760 parts by mass of ion-exchanged water was added to stop the particle growth. After stirring at 70°C for 1 hour, the temperature was further raised, and the particles were heated and stirred at 75°C to promote fusion of the particles. The mixture was then cooled to 30°C to obtain a dispersion of toner base particles.
[0337] The obtained dispersion liquid of the toner base particles was subjected to solid-liquid separation using a centrifuge to form a wet cake of the toner base particles. The wet cake was washed with ion-exchanged water at 35°C until the electrical conductivity of the filtrate in the centrifuge reached 5 μS / cm, and then transferred to a "Flash Jet Dryer (manufactured by Seishin Enterprise Co., Ltd.)" and dried until the moisture content reached 0.5% by mass to produce the toner base particles.
[0338] Toner 4 was obtained by adding 1% by mass of hydrophobic silica (number average primary particle size: 12 nm) and 0.3% by mass of hydrophobic titania (number average primary particle size: 20 nm) to 100% by mass of the obtained toner base particles and mixing them using a Henschel mixer (registered trademark).
[0339] [Examples 1 to 3, 5 to 19] Using the corresponding raw materials and the same method as in Example 4, azomethine derivative monomers 1, 2, 3, 7, 8, 10, 12, 14, 15, 16, 17, 19, 22, 24, 28, 32, and 34 having structural units 1, 2, 3, 7, 8, 10, 12, 14, 15, 16, 17, 19, 22, 24, 28, 32, and 34 shown in Table 1 below were synthesized. Next, polymers 1 to 3 and 5 to 19 shown in Table 2 below were obtained in the same manner as in Example 4, except that the azomethine derivative monomers 1, 2, 3, 7, 8, 10, 12, 14, 15, 16, 17, 19, 22, 24, 28, 32, and 34 were used instead of the azomethine derivative monomer 6. Next, toners 1 to 3 and 5 to 19 were produced in the same manner as in Example 4, except that polymers 1 to 3 and 5 to 19 were used instead of polymer 4. However, in the preparation of azomethine derivative monomers 1, 2, 3, 7, 8, 10, 12, 14, 15, 16, 17, 19, 22, 24, 28, 32, and 34 and polymers 1 to 3 and 5 to 19, the amount of each raw material added and the reaction conditions were appropriately adjusted.
[0340] Polymer 19 was prepared by using the same raw materials as polymer 12 and appropriately adjusting the polymerization time to obtain a polymer having the same structural unit as polymer 12 but different number average molecular weight.
[0341] [Example 20] Polymer 20 was obtained in the same manner as in Example 12, except that the amount of azomethine derivative monomer 17 was changed from 1.5 g to 1.2 g and 0.3 g of styrene was added in the synthesis of polymer 12. Toner 20 was produced in the same manner as in Example 12, except that polymer 20 was used instead of polymer 12.
[0342] [Example 21] Polymer 21 was obtained in the same manner as in the synthesis of Polymer 20 in Example 20, except that styrene was changed to ethyl acrylate. Toner 21 was produced in the same manner as in Example 20, except that Polymer 21 was used instead of Polymer 20.
[0343] [Example 22] Polymer 22 was obtained in the same manner as in the synthesis of Polymer 20 in Example 20, except that styrene was changed to n-butyl methacrylate. Toner 22 was produced in the same manner as in Example 20, except that Polymer 22 was used instead of Polymer 20.
[0344] [Example 23] Polymer 23 was obtained in the same manner as in Example 20, except that the amount of styrene was changed from 0.3 g to 0.15 g and 0.15 g of methyl acrylate was added in the synthesis of Polymer 20. Toner 23 was prepared in the same manner as in Example 20, except that Polymer 23 was used instead of Polymer 20.
[0345] [Example 24] <Synthesis of macroinitiator 24> In a 100 ml eggplant flask, 2,2'-bipyridyl (230 mg, 1.47 mmol) was added, and in a glove box under a nitrogen atmosphere, Cu(I)Br (95 mg, 0.66 mmol), styrene (15 g, 144 mmol), and ethyl 2-bromoisobutyrate (35 mg, 0.18 mmol) were added and sealed. This was heated and stirred in an oil bath at 100°C. Then, an appropriate amount of tetrahydrofuran was added, and the mixture was passed through a neutral alumina column. This was purified by reprecipitation with methanol and centrifugation to obtain macroinitiator 24. The number average molecular weight (β Mn) of the obtained macroinitiator 24 was measured by GPC method and found to be 1000.
[0346] <Synthesis of polymer 24> In a 100 ml eggplant flask, the above-obtained azomethine derivative monomer 17 (16 g, 38 mmol) and the above-mentioned macroinitiator 24 (0.92 g, 0.18 mmol) were placed, and in a glove box under a nitrogen atmosphere, Cu(I)Cl (29 mg, 0.29 mmol), 1,1,4,7,10,10-hexamethyltriethylenetetramine (136 mg, 0.59 mmol), and anisole (4.9 g, 41.1 mmol) as a solvent were added and sealed. Then, the mixture was heated and stirred in an oil bath at 80°C. Then, an appropriate amount of chloroform was added, and the mixture was passed through a basic alumina column. This was purified by reprecipitation with methanol and centrifugation to obtain polymer 24. The total number average molecular weight Mn of the obtained polymer 24 was 5400 when measured by GPC method. From this, the number average molecular weight (α Mn) of the structural unit containing a group having an azomethine structure (structural unit derived from an azomethine derivative) is determined to be 4,400.
[0347] Toner 24 was prepared in the same manner as in Example 1, except that Polymer 24 was used instead of Polymer 1.
[0348] [Example 25] <Synthesis of macroinitiator 25> Macroinitiator 25 was obtained in the same manner as in the synthesis of macroinitiator 24, except that ethyl 2-bromoisobutyrate was changed to α,α'-dibromo-p-xylene.
[0349] <Synthesis of polymer 25> Polymer 25 was obtained in the same manner as in the synthesis of Polymer 24, except that Macroinitiator 24 was changed to Macroinitiator 25.
[0350] However, in preparing Macroinitiator 25, Macroinitiators 26 to 35 described below, and Polymer 25, and Polymers 26 to 35 described below, the amount of each raw material added and reaction conditions were appropriately adjusted.
[0351] Next, toner 25 was prepared in the same manner as in Example 1, except that polymer 25 was used instead of polymer 1.
[0352] [Example 26] <Synthesis of macroinitiator 26> Macroinitiator 26 was obtained in the same manner as in the synthesis of macroinitiator 24, except that ethyl 2-bromoisobutyrate was changed to ethylene bis(2-bromoisobutyrate), 2,2'-bipyridyl was changed to 1,1,4,7,10,10-hexamethyltriethylenetetramine, styrene was changed to azomethine derivative monomer 17, and anisole was further added.
[0353] <Synthesis of polymer 26> Polymer 26 was obtained in the same manner as in the synthesis of polymer 24, except that macroinitiator 24 was changed to macroinitiator 26, 1,1,4,7,10,10-hexamethyltriethylenetetramine was changed to 2,2'-bipyridyl, azomethine derivative monomer 17 was changed to styrene, and anisole was omitted.
[0354] Next, toner 26 was prepared in the same manner as in Example 1, except that polymer 26 was used instead of polymer 1.
[0355] [Example 27] <Synthesis of macroinitiator 27> Macroinitiator 27 was obtained in the same manner as in the synthesis of macroinitiator 24, except that ethyl 2-bromoisobutyrate was changed to 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane.
[0356] <Synthesis of polymer 27> Polymer 27 was obtained in the same manner as in the synthesis of Polymer 24, except that macroinitiator 24 was changed to macroinitiator 27.
[0357] Next, toner 27 was prepared in the same manner as in Example 1, except that polymer 27 was used instead of polymer 1.
[0358] [Example 28] <Synthesis of macroinitiator 28> Macroinitiator 28 was obtained in the same manner as in the synthesis of macroinitiator 26, except that ethylene bis(2-bromoisobutyric acid) was changed to 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane.
[0359] <Synthesis of polymer 28> Polymer 28 was obtained in the same manner as in the synthesis of Polymer 26, except that macroinitiator 26 was changed to macroinitiator 28.
[0360] Next, toner 28 was prepared in the same manner as in Example 1, except that polymer 28 was used instead of polymer 1.
[0361] [Example 29] <Synthesis of macroinitiator 29> Macroinitiator 29 was obtained in the same manner as in the synthesis of macroinitiator 24, except that ethyl 2-bromoisobutyrate was changed to pentaerythritol tetrakis(2-bromoisobutyrate).
[0362] <Synthesis of polymer 29> Polymer 29 was obtained in the same manner as in the synthesis of Polymer 24, except that macroinitiator 24 was changed to macroinitiator 29.
[0363] Next, toner 29 was prepared in the same manner as in Example 1 except that polymer 29 was used instead of polymer 1.
[0364] [Example 30] <Synthesis of macroinitiator 30> Macroinitiator 30 was obtained in the same manner as in the synthesis of macroinitiator 26, except that ethylene bis(2-bromoisobutyric acid) was changed to pentaerythritol tetrakis(2-bromoisobutyrate).
[0365] <Synthesis of polymer 30> Polymer 30 was obtained in the same manner as in the synthesis of Polymer 26, except that macroinitiator 26 was changed to macroinitiator 30.
[0366] Next, toner 30 was prepared in the same manner as in Example 1, except that polymer 30 was used instead of polymer 1.
[0367] [Example 31] <Synthesis of macroinitiator 31> In the synthesis of macroinitiator 24, by appropriately adjusting the time of heating and stirring in a 100° C. oil bath, macroinitiator 31 was obtained which has the same structure as macroinitiator 24 and a number average molecular weight (β Mn) of 5000.
[0368] <Synthesis of Polymer 31> In the synthesis of polymer 24, the time of heating and stirring in an 80°C oil bath was appropriately adjusted to obtain polymer 31, which is composed of structural units similar to those of polymer 24 and has a total number average molecular weight Mn of 5,500. In polymer 31, the number average molecular weight (α Mn) of the structural unit containing a group having an azomethine structure (structural unit derived from an azomethine derivative) was 500.
[0369] Next, toner 31 was prepared in the same manner as in Example 1, except that polymer 31 was used instead of polymer 1.
[0370] [Example 32] <Synthesis of macroinitiator 32> Macroinitiator 32 was obtained in the same manner as in the synthesis of macroinitiator 25, except that styrene was changed to methyl acrylate.
[0371] <Synthesis of polymer 32> Polymer 32 was obtained in the same manner as in the synthesis of Polymer 25, except that macroinitiator 25 was changed to macroinitiator 32.
[0372] Next, toner 32 was prepared in the same manner as in Example 1, except that polymer 32 was used instead of polymer 1.
[0373] [Example 33] <Synthesis of macroinitiator 33> Macroinitiator 33 was obtained in the same manner as in the synthesis of macroinitiator 25, except that styrene was changed to n-hexyl methacrylate.
[0374] <Synthesis of polymer 33> Polymer 33 was obtained in the same manner as in the synthesis of Polymer 25, except that Macroinitiator 25 was changed to Macroinitiator 33.
[0375] Next, toner 33 was prepared in the same manner as in Example 1, except that polymer 33 was used instead of polymer 1.
[0376] [Example 34] <Synthesis of macroinitiator 34> Macroinitiator 34 was obtained in the same manner as in the synthesis of macroinitiator 25, except that styrene was changed to 3-methyl-1-pentene.
[0377] <Synthesis of polymer 34> Polymer 34 was obtained in the same manner as in the synthesis of Polymer 25, except that macroinitiator 25 was changed to macroinitiator 34.
[0378] Next, toner 34 was prepared in the same manner as in Example 1, except that polymer 34 was used instead of polymer 1.
[0379] [Example 35] <Synthesis of macroinitiator 35> Macroinitiator 35 was obtained in the same manner as in the synthesis of macroinitiator 25, except that styrene was changed to a mixture of styrene:methyl acrylate with a molar ratio of 5:5.
[0380] <Synthesis of polymer 35> Polymer 35 was obtained in the same manner as in the synthesis of Polymer 25, except that Macroinitiator 25 was changed to Macroinitiator 35.
[0381] Next, toner 35 was prepared in the same manner as in Example 1, except that polymer 35 was used instead of polymer 1.
[0382] [Example 36] Toner 36 was obtained in the same manner as in preparation of Toner 12, except that the amount of polymer particle dispersion 12 was changed from 602 parts by mass in solid content to 421 parts by mass, and 181 parts by mass of the following styrene acrylic resin particle dispersion was added in solid content equivalent.
[0383] <Preparation of styrene acrylic resin particle dispersion> (First stage polymerization) A solution of 8 parts by mass of sodium dodecyl sulfate dissolved in 3000 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirring device, a temperature sensor, a cooling tube, and a nitrogen introduction device, and the internal temperature was raised to 80 ° C. while stirring at a stirring speed of 230 rpm under a nitrogen gas flow. After the temperature was raised, a solution of 10 parts by mass of potassium persulfate dissolved in 200 parts by mass of ion-exchanged water was added, the liquid temperature was again raised to 80 ° C., and a polymerizable monomer solution consisting of 480 parts by mass of styrene, 250 parts by mass of n-butyl acrylate, 68.0 parts by mass of methacrylic acid, and 16.0 parts by mass of n-octyl-3-mercaptopropionate was dropped over 1 hour, and the mixture was heated and stirred at 80 ° C. for 2 hours to polymerize, thereby preparing a styrene acrylic resin particle dispersion liquid (1A) containing styrene acrylic resin particles (1a).
[0384] (Second stage polymerization) A solution of 7 parts by mass of sodium polyoxyethylene (2) dodecyl ether sulfate dissolved in 800 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98°C. After that, a polymerizable monomer solution of 260 parts by mass of the styrene acrylic resin particle dispersion (1A) obtained above, 245 parts by mass of styrene, 120 parts by mass of n-butyl acrylate, 1.5 parts by mass of n-octyl-3-mercaptopropionate, and 67 parts by mass of paraffin wax "HNP-11" (manufactured by Nippon Seiro Co., Ltd.) as a release agent was added at 90°C, and the mixture was mixed and dispersed for 1 hour using a mechanical disperser "CREARMIX (registered trademark)" (manufactured by M Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). Next, an initiator solution prepared by dissolving 6 parts by mass of potassium persulfate in 200 parts by mass of ion-exchanged water was added to this dispersion, and the system was heated and stirred at 82°C for 1 hour to carry out polymerization, thereby preparing a styrene-acrylic resin particle dispersion (1B) containing styrene-acrylic resin particles (1b).
[0385] (Third stage polymerization) A solution of 11 parts by mass of potassium persulfate dissolved in 400 parts by mass of ion-exchanged water was added to the obtained styrene-acrylic resin particle dispersion liquid (1B), and then a polymerizable monomer solution consisting of 435 parts by mass of styrene, 130 parts by mass of n-butyl acrylate, 33 parts by mass of methacrylic acid, and 8 parts by mass of n-octyl-3-mercaptopropionate was added dropwise over 1 hour under a temperature condition of 82°C. After the dropwise addition, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28°C to obtain a styrene-acrylic resin particle dispersion liquid containing styrene-acrylic resin 1. The glass transition temperature (Tg) of styrene-acrylic resin 1 was measured and found to be 45°C.
[0386] [Example 37] Toner 37 was obtained in the same manner as in preparation of Toner 12, except that the amount of polymer particle dispersion 12 was changed from 602 parts by mass in terms of solid content to 421 parts by mass, and 181 parts by mass of the following polyester resin particle dispersion was added in terms of solid content.
[0387] (Preparation of polyester resin particle dispersion containing polyester resin) In a 10-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 524 parts by mass of bisphenol A propylene oxide 2-mol adduct, 105 parts by mass of terephthalic acid, 69 parts by mass of fumaric acid, and 2 parts by mass of tin octylate (esterification catalyst) were added, and a polycondensation reaction was carried out at a temperature of 230°C for 8 hours. The polycondensation reaction was further continued at 8 kPa for 1 hour, and then cooled to 160°C to obtain polyester resin 1. 100 parts by mass of polyester resin 1 was pulverized with a "Landermill Type: RM" (manufactured by Tokuju Machinery Co., Ltd.), mixed with 638 parts by mass of a 0.26% by mass aqueous solution of sodium lauryl sulfate prepared in advance, and ultrasonically dispersed for 30 minutes at V-LEVEL and 300 μA using an ultrasonic homogenizer "US-150T" (manufactured by Nippon Seiki Co., Ltd.) while stirring, to obtain a polyester resin particle dispersion. The particle size of the polyester resin particles in the polyester resin particle dispersion was measured by dynamic light scattering using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.) to find that the volume-based median diameter was 135 nm. The glass transition temperature (Tg) of this polyester resin 1 was measured to find that it was 42°C.
[0388] [Comparative Example 1] Using the corresponding raw materials and the same method as in Example 4, an azomethine derivative monomer 37 of Comparative Example 1 having the structural unit 37 of Comparative Example 1 shown in Table 1 below was synthesized. Then, a polymer of Comparative Example 1 (also referred to as polymer 36) was obtained in the same manner as in Example 4, except that the azomethine derivative monomer 37 of Comparative Example 1 was used instead of the azomethine derivative monomer 6 in Example 4. Then, a toner of Comparative Example 1 (also referred to as toner 38) was produced in the same manner as in Example 4, except that the polymer of Comparative Example 1 (polymer 36) was used instead of the polymer 4.
[0389] [Comparative Example 2] <Comparative compounds (azobenzene derivatives)> The following comparative compound (azobenzene derivative, number average molecular weight Mn: 2870) was obtained by the method described in paragraphs 0217 to 0227 of JP2014-191078A.
[0390] [ka]
[0391] <Preparation of Comparative Compound Dispersion> A comparative compound dispersion was obtained in the same manner as in <Preparation of polymer particle dispersion 4> of Example 4, except that polymer 4 was changed to a comparative compound (azobenzene derivative).
[0392] <Preparation of Toner in Comparative Example 2> A toner of Comparative Example 2 (also referred to as toner 39) was obtained in the same manner as in Example 4, except that the polymer particle dispersion 4 in Example 4 was replaced with the comparative compound dispersion prepared above.
[0393] [Theoretical calculation] For the polymers of each Example and the polymer of Comparative Example 1, the activation energy Ea of photoisomerization of the azomethine derivative in the structural unit (energy barrier in the isomerization reaction from cis to trans) was calculated. In detail, for each polymer, the total energy of the transition state of a compound in which a hydrogen atom is bonded in place of the oxygen atom bonded to group A having the azomethine structure of general formula (1) above and the total energy of the cis form were calculated, and the difference between them was taken as the activation energy. Here, the transition state of the compound is represented by general formula (3) above, and the cis form is represented by general formula (4) above. Note that general formulas (3) and (4) are Z 1 =Z 2 B for bond 1 and B. 2 It indicates the arrangement (position) of H, r 2 -H, Or 2 -H part is B 1 The structure of the compound depends on the structure of the group A having an azomethine structure, including the structure of the compound shown below.
[0394] The snowflake of the snowflake is the snowflake ) is a slightly less expensive solution The intrinsic wavelengths of the independent wavelengths of the Gaussian waveform are Gaussian16 (Revision B.01, Frisch MJ, GW Trucks, HB Schlegel, Scuseria GE, Robb MA, Cheeseman JR, Scalmani G, Barone V, Petersson GA, Nakatsuji H, Li X, Caricato M, Marenich AV, Bloino J, Janesko BG, Gomperts R, Mennucci, HP Hratchian, Ortiz JV, AF Izmaylov, JL Sonnenberg, D Williams-Young, F Ding, F Lipparini, F Egidi, J Goings, B Peng, A Petrone, T Henderson, D Ranasinghe, VG Zakrzewski, J Gao, N Rega, G Zheng, W Liang, M Hada, M Ehara, K Toyota, R Fukuda, Hasegawa J, Ishida M, Nakajima T, Honda Y, Kitao O, Nakai H, Vreven T, Throssell K, Montgomery, Jr., Peralta JE, Ogliaro F, Bearpark MJ, Heyd JJ, EN Brothers, Kudin KN, Staroverov VN, Keith TA, Kobayashi R, Normand , K , Raghavachari , AP Rendell , JC Burant , SS Iyengar , J Thomas , M Cossi , Millam JM , Klene M , Adamo C , Cammi R , J .The calculation was performed using the software (W. Ochterski, RL Martin, K. Morokuma, O. Farkas, JB Foresman, and DJ Fox, Gaussian, Inc., Wallingford CT, 2016.). The density functional theory (B3LYP / 6-31G(d)) was used as the calculation method. From the calculated values, the activation energy Ea was calculated according to the above formula (1). .
[0395] For the molecular structure of the cis isomer, the most stable molecular structure of the isomer represented by the above general formula (4), i.e., the molecular structure with the lowest total energy, was calculated, and this total energy was taken as the total energy of the cis isomer. For the molecular structure of the transition state, the saddle point of the corresponding molecular structure was calculated for the transition state represented by general formula (3), and the total energy obtained at this time was taken as the total energy of the transition state. From the calculated value thus obtained, the value of the activation energy Ea was calculated according to the above formula (1).
[0396] The activation energies of the structural units constituting the polymers of Examples 1 to 19 and Comparative Example 1, and the compounds in which a hydrogen atom is bonded to the structure represented by the above general formula (2) are shown in Table 1 below.
[0397] (Number average molecular weight Mn) The number average molecular weights Mn of polymers 1 to 35, the polymer of Comparative Example 1, and the comparative compound (azobenzene derivative) were measured by the GPC method. Specifically, an apparatus "HLC-8120GPC" (manufactured by Tosoh Corporation) and a column "TSKguardcolumn+TSKgelSuperHZ-M3 series" (manufactured by Tosoh Corporation) were used, and tetrahydrofuran (THF) was passed as a carrier solvent at a flow rate of 0.2 mL / min while maintaining the column temperature at 40°C. The measurement sample was dissolved in tetrahydrofuran to a concentration of 1 mg / ml. The solution was prepared by treating the solution at room temperature for 5 minutes using an ultrasonic disperser. Next, the sample solution was treated with a membrane filter having a pore size of 0.2 μm to obtain a sample solution, and 10 μL of this sample solution was injected into the apparatus together with the above carrier solvent, and detected using a refractive index detector (RI detector). The molecular weight distribution of the measurement sample was calculated based on a calibration curve created using monodisperse polystyrene standard particles. Ten polystyrene points were used for the above calibration curve measurement.
[0398] In addition to the total number average molecular weight, the number average molecular weight of the macroinitiator was also measured by the above method for polymers 24 to 35. The number average molecular weight of the macroinitiator was taken as the number average molecular weight of polymer block α or β, and the total number average molecular weight of the other polymer block (number average molecular weight of the other polymer block × number of blocks) was obtained by subtracting (number average molecular weight of macroinitiator × number of blocks) from the total number average molecular weight of the polymer for each block structure. The results are shown in Table 2 below. In Table 2, Mn represents the total number average molecular weight of the polymer, αMn represents the total number average molecular weight of polymer block α, and βMn represents the total number average molecular weight of polymer block β.
[0399] (Glass transition temperature (Tg)) The glass transition temperature (Tg) of the binder resin was measured using a DSC7000X manufactured by Hitachi High-Tech Science Corporation. Specifically, about 3 mg of the binder resin was weighed out to two decimal places, sealed in an aluminum pan, and set. An empty aluminum pan was used as a reference. The measurement conditions were a first heating process in which the temperature was raised from 0°C to 200°C at a heating rate of 10°C / min; a cooling process in which the temperature was lowered from 200°C to 0°C at a heating rate of 10°C / min; and a second heating process in which the temperature was raised from 0°C to 200°C at a heating rate of 10°C / min, in that order. Then, analysis was performed based on the data from the second heating process. The value of the intersection between the extension line of the baseline before the rise of the first endothermic peak and the tangent line showing the maximum slope from the rise part of the first endothermic peak to the peak apex was taken as the glass transition temperature. The glass transition temperatures of the polymers and toners produced in each of the examples and comparative examples can also be measured by the same method.
[0400] [Evaluation: Photoresponsive adhesion test of polymers] The change in adhesiveness accompanying light irradiation of the polymers 1 to 35 prepared in each Example, the polymer of Comparative Example 1 synthesized in Comparative Example 1, and the azobenzene derivative synthesized in Comparative Example 2 was evaluated by the following photoresponsive adhesive test using the apparatus shown in FIG. 3. As shown in FIG. 3, 2 mg of the polymer was placed on a 18 mm square cover glass 1 within a radius of 6 mm from the center of the glass, and a cover glass 2 of the same size was placed at a position shifted about 4 mm in a parallel direction to the cover glass 1 so as to completely cover the polymer. This was heated to melt the sample, and the cover glass 1 and the cover glass 2 were bonded together. Each of the obtained samples was subjected to the following non-fluidity → fluidity test, and then the following fluidity → non-fluidity test.
[0401] <Testing non-fluidity to fluidity (fluidity test)> Part (A) shown in Figure 3 was fixed to the stand with cellophane tape, and a 30 cm long vinyl string with a 100 g weight attached was fixed to part (C) with cellophane tape. Part (B) was irradiated with light of 365 nm wavelength at a dose of 30 J / cm. 2It was confirmed whether cover glass 2 peeled off from cover glass 1, and the peeling was judged according to the following evaluation criteria. The obtained results are shown in Table 2 below.
[0402] - Evaluation criteria for testing non-liquidity to liquidity (fluidity test) - ○: Cover glass 2 was completely peeled off from cover glass 1 △: Cover glass 2 is displaced ×: The cover glass 2 did not move.
[0403] <Testing from liquidity to non-liquidity (non-liquidity test)> After the non-fluidity → fluidity test was completed, the following experiment was performed on the samples where the cover glass 2 had completely peeled off and on the samples where it had shifted. For the shifted samples, the cover glasses 1 and 2 were peeled off by hand. Five minutes after the light irradiation for the non-fluidity → fluidity test had finished (the sample was left in a dark room at room temperature for five minutes), a cover glass 3 (same size as cover glasses 1 and 2) was placed over the sample portion (part (B)) of the cover glass 1 used in the above test, and it was confirmed whether the cover glass 1 and the cover glass 3 were adhered to each other, and the evaluation was made according to the following criteria. The results are shown in Table 2.
[0404] -Evaluation criteria for liquidity to non-liquidity testing (non-liquidity testing)- 〇: Did not adhere (had become non-fluid) △: Partially adhered (partially maintained in a fluid state) ×: Adhered (fluid state was maintained).
[0405] In addition, it was confirmed that all of the polymers 1 to 35 prepared in Examples 1 to 31, which were evaluated as "good" in the above-mentioned fluidity to non-fluidity (reversion) test, re-solidified after the non-fluidity to fluidity test was performed.
[0406] [Evaluation: Fixation test] (Preparation of developer) For the toners 1 to 35 and the toners of Comparative Examples 1 and 2 prepared above, ferrite carrier particles having a volume average particle size of 30 μm coated with a copolymer resin of cyclohexane methacrylate and methyl methacrylate (monomer mass ratio 1:1) were mixed so that the toner particle concentration was 6 mass%, thereby obtaining developers 1 to 35 and the developers of Comparative Examples 1 and 2. Mixing was performed for 30 minutes using a V-type mixer.
[0407] (Fixation test) Fixing tests were carried out under normal temperature and humidity conditions (temperature 20°C, relative humidity 50% RH) using the above-obtained developers 1 to 35 and the developers of Comparative Examples 1 and 2. The developer was placed on one side, and plain paper (basis weight: 64 g / m2) was placed on the other side as a recording medium. 2 The developer is placed between a pair of parallel flat plate (aluminum) electrodes with a magnetic force, and the gap between the electrodes is 0.5 mm. The DC bias and AC bias are used to control the toner adhesion amount to 6 g / m. 2 The toner was developed under the above conditions, a toner layer was formed on the surface of the plain paper, and the toner was fixed by each fixing device to obtain a print (image formation). The 1 cm square toner image on the print was rubbed 11 times with a "JK Wiper (registered trademark)" (manufactured by Nippon Paper Crecia Co., Ltd.) at a pressure of 50 kPa to evaluate the fixation rate of the image. A fixation rate of 60% or more was considered to be acceptable. The fixation rate of the image is a numerical value obtained by measuring the reflection density of the image after printing and the image after rubbing with a fluorescent spectrodensitometer "FD-7" (manufactured by Konica Minolta, Inc.), and dividing the reflection density of the solid image after rubbing by the reflection density of the solid image after printing, expressed as a percentage.
[0408] The fixing devices used were the following three types of fixing devices, which were constructed by appropriately modifying the device shown in FIG. 2: No. 1: There is no bonding part 9 in FIG. 2. The wavelength of the ultraviolet light irradiated from the irradiation part 40 is 365 nm (light source: LED light source with an emission wavelength of 365 nm ± 10 nm), and the irradiation dose is 11 J / cm 2 is; No. 2: The pressure bonding unit 9 in FIG. 2 is included, the temperature of the pressure member 91 is 20° C., and the pressure during pressing is 0.2 MPa. The light source and the irradiation amount of the irradiation unit 40 are the same as those of No. 1; No. 3: The pressure bonding unit 9 in FIG. 2 is included, the temperature of the pressure member 91 is 80° C., and the pressure during pressing is 0.2 MPa. The light source and the irradiation amount of the irradiation unit 40 are the same as those of No. 1; No. 4: No compression part 9 in FIG. 2 was absent, and the sample was heated to 50° C. by a heating member (not shown) simultaneously with light irradiation by the irradiation part 40, and the wavelength and irradiation amount of the irradiation part 40 were the same as those of No. 1.
[0409] [Color reproducibility evaluation] The color reproducibility of the images of the examples and comparative examples obtained above was evaluated by visual evaluation by 10 monitors according to the following evaluation criteria. Specifically, as a sample for evaluation comparison, a toner was prepared in which the polymer 12 in the toner 32 of Example 32 was changed entirely to a styrene acrylic resin. Using this, a developer was prepared in the same manner as above, and development was performed in the same manner as in the image formation in the fixing property test above, and fixing was performed using the fixing device No. 5 described below: Fixing device No. 5: The pressing unit 9 in FIG. 2 was included, the temperature of the pressure member 91 was 150° C., the pressure during pressing was 0.2 MPa, and light irradiation was not performed.
[0410] The 10 monitors were shown the sample for evaluation and comparison, and the images obtained in the above-mentioned Examples and Comparative Examples in turn, and asked whether the colors of the two images were clearly different. The results of the evaluation based on the following color reproducibility evaluation criteria are shown in Table 3 below: -Evaluation criteria for color reproducibility- ◎: Less than 2 people answered that it was clearly different ○: 3 to 4 people answered that it was clearly different △: 5 to 7 people answered that it was clearly different ×: Eight or more people answered that it was clearly different.
[0411] [Table 2-1]
[0412] [Table 2-2]
[0413]
Table 2-3
[0414]
Table 2-4
[0415]
Table 2-5
[0416]
Table 2-6
[0417]
Table 2-7
[0418]
Table 2-8
[0419]
Table 2-9
[0420]
Table 3
[0421]
Table 4
[0422] As is clear from Table 2, it was confirmed that the polymers of each Example, which contain a structural unit represented by the above general formula (1) and have an activation energy Ea of 60 kJ / mol or more in the isomerization reaction from cis to trans of a compound having a structure represented by the above general formula (2) bonded to a hydrogen atom, are fluidized and reversibly non-fluidized by light irradiation. In contrast, the polymer prepared in Comparative Example 1 has an activation energy Ea of less than 60 kJ / mol in the isomerization reaction from cis to trans of a compound corresponding to the azomethine structure. It was found that such polymers are not fluidized or non-fluidized by light irradiation. In addition, reversible non-fluidization after fluidization was not confirmed in the comparative compound (azobenzene derivative) in Comparative Example 2.
[0423] Moreover, as shown in Table 3, all of the toners using the polymers prepared in the Examples could be fixed by light irradiation, and showed high fixability and excellent color reproducibility. On the other hand, the toner using the polymer prepared in Comparative Example 1 had insufficient fixability. It was also found that the toner using the comparative compound (azobenzene derivative) in Comparative Example 2 had poor fixability and color reproducibility. Since the ultraviolet light source and ultraviolet irradiation conditions used in the fixability test were constant, it can be said that the toners of each Example fully exhibited the effect of the polymer, which was fluidized by light irradiation, reversibly non-fluidized, and did not show significant coloring, compared to the toners of Comparative Examples 1 and 2.
[0424] When comparing the fixing devices, it was found that, using the same toner 12 and irradiating ultraviolet rays under the same conditions, higher fixability was obtained when using fixing device No. 2, which was pressurized with a pressure member, and fixing device No. 3, which was pressurized while being heated with a pressure member, were used than fixing device No. 1, which did not use a pressure member (comparison of Examples 12, 38, and 39).
[0425] As shown in each example, it can be seen that any polymer that contains a structural unit represented by general formula (1) containing a group having an azomethine structure, and has an activation energy Ea of 60 kJ / mol or more in an isomerization reaction from cis to trans isomers of a compound in which a hydrogen atom is bonded to the azomethine structure, is fluidized and reversibly non-fluidized by light irradiation, has little coloring, and shows an excellent fixation rate of 60% or more in a fixation test of a toner image using the toner.
[0426] From the comparison of the fixing properties of the toners of the respective examples, it is found that in the structural unit of the general formula (1), B 1 Or B 2 When either one of B has an aromatic heterocyclic group, the fixability tends to be higher than when both are aromatic hydrocarbon groups. 1 is a phenylene group, and B 2 When is an aromatic heterocyclic group, as in Examples 4 to 8, B 1 Z 1 When the polymerizable group is bonded to the para position of B, the fixability tends to be higher. 1 is a divalent aromatic heterocyclic group, and B 2 When is a monovalent aromatic heterocyclic group, as in Example 10, B 1 Z 1 When the bond to the polymerizable group is at a position that is not adjacent to the bond to the polymerizable group, the fixing property tends to be higher.
[0427] Not only structural units containing a group having an azomethine structure, but also combinations of other structural units can similarly obtain fluidization and reversible non-fluidization by light irradiation. In addition, when used in toner, good fixing rate can be obtained. In this case, it was found that excellent performance can be obtained whether the copolymer is a random copolymer or a block copolymer. In particular, it was found that the fixing property is superior in the case of block copolymers.
[0428] Furthermore, a comparison between Example 12 and Example 19 revealed that, even though the polymers have the same structural units, the polymer of Example 12 having a number average molecular weight of 3500 or more has superior toner fixing properties.
[0429] In the case of block copolymers, a comparison between Examples 24 and 31 revealed that even though they have the same structural units, the polymer of Example 24, in which the number average molecular weight of the polymer block α containing the structural unit represented by general formula (1) is 1000 or more and the number average molecular weight of the polymer block β not containing an azomethine structure is 1000 or more, has superior toner fixing properties.
[0430] In addition to the polymer, a binder resin can be further contained in the toner. It has been confirmed that a good fixing rate and color reproducibility can be obtained when a binder resin is further used. By using the above polymer, a good fixing rate can be obtained even if the binder resin content is low.
[0431] In particular, the toners of Examples 4, 5, 8, 12, and 13, which used polymers having structural units 6, 7, 12, 17, and 19, respectively, shown in Table 1, exhibited particularly good image fixing rates. The toners of Examples 24 to 26, which used block copolymers containing structural unit 17, also exhibited excellent fixing rates. [Explanation of symbols]
[0432] 1 photoreceptor, 2 Charger, 3 Exposure device, 4 Development section, 5 Transcription unit, 7 Paper transport system, 8 Cleaning section, 9 Crimping part, 10 Image forming unit, 11 Paper feed section, 12 Transport roller, 13 conveyor belt, 14 Paper ejection section, 15 Manual feed unit, 16 trays, 17 Thermohygrometer, 20 Image processing unit, 24 Paper reversing section, 40 Irradiation unit, 71 Image reading device, 72 Automatic document feeder, 85 blades, 90 control section, 91, 92 Pressurizing member, 100 Image forming apparatus, d manuscript, S Recording paper.
Claims
1. A photoresponsive polymer that contains a structural unit represented by the following general formula (1), which is fluidized and reversibly non-fluidized upon light irradiation, 【Chemistry 1】 In general formula (1), r 1 is a hydrogen atom or a methyl group, A is a group having an azomethine structure represented by the following general formula (2), 【Chemistry 2】 In general formula (2), Z 1 and Z 2 are each independently N or CH, and Z 1 ≠Z 2 and B 1 each independently represents a substituted or unsubstituted phenylene group or a substituted or unsubstituted divalent aromatic heterocyclic group, B 2 are each independently a substituted or unsubstituted phenyl group or a substituted or unsubstituted monovalent aromatic heterocyclic group, and satisfy any one of the following (i) to (iv): (i) each B 1 is independently a phenylene group bonded to an oxygen atom (in the case of (2-c)) or to r 2 (in the case of (2-b)) at the para position relative to Z 1 , and each B 2 is independently a phenyl group having a substituent selected from an alkoxy group having 4 to 18 carbon atoms and a dialkylamino group having 2 to 10 carbon atoms at the para position relative to Z 2 ; (ii) each B 1 is independently a phenylene group bonded to an oxygen atom (in the case of (2-c)) or to r 2 (in the case of (2-b)) at the para position relative to Z 1 ; B 2 s each independently represent an aromatic heterocyclic group that is unsubstituted or substituted with a halogen atom, a cyano group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms; (iii) each B 1 is independently a substituted or unsubstituted divalent aromatic heterocyclic group, which is bonded to an oxygen atom (in the case of (2-c)) or to r 2 (in the case of (2-b)) at a position not adjacent to the position bonded to Z 1 ; B 2 s are each independently an unsubstituted phenyl group or a phenyl group substituted with a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms; (iv) each B 1 is independently a substituted or unsubstituted divalent aromatic heterocyclic group, which is bonded to an oxygen atom (in the case of (2-c)) or to r 2 (in the case of (2-b)) at a position not adjacent to the position bonded to Z 1 ; B 2 s each independently represent an aromatic heterocyclic group which is unsubstituted or substituted with a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms; r 2 each independently represents an alkylene group having 1 to 18 carbon atoms, A photoresponsive polymer, characterized in that a compound in which a hydrogen atom is bonded in place of the oxygen atom bonded to A in the general formula (1) has an activation energy Ea represented by the following formula (1) of 60 kJ / mol or more: Equation (1): Ea (kJ / mol) = (total energy of TS (kJ / mol)) - (total energy of cis isomer (kJ / mol)) In the above formula (1), TS indicates a transition state represented by general formula (3), and the cis form indicates an isomer represented by general formula (4). 【Chemistry 3】
2. Each B 1 is independently a phenylene group bonded to an oxygen atom (in the case of (2-c)) or to r 2 (in the case of (2-b)) at the para position relative to Z 1 , each B 2 is independently a phenyl group having a substituent selected from an alkoxy group having 4 to 18 carbon atoms and a dialkylamino group having 2 to 10 carbon atoms at the para position relative to Z 2 , 1 and B 2 At least one of 1 Or Z 2 The polymer according to claim 1, wherein the two ortho-positions and the two meta-positions relative to the above are unsubstituted or substituted with a group selected from a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms.
3. The polymer according to claim 1 or 2, having a number average molecular weight Mn of 3,500 or more.
4. The polymer according to any one of claims 1 to 3, further comprising another structural unit having a vinyl-based polymerizable group.
5. The polymer according to claim 4 , wherein the other structural unit is a structural unit derived from a styrene derivative, an acrylic acid derivative, a methacrylic acid derivative, or an olefin derivative.
6. The polymer according to any one of claims 1 to 5, represented by the following general formula (5): 【Chemistry 4】 In the above general formula (5), α is a polymer block containing a structural unit represented by the above general formula (1), and β is an azomethine structure (B 1 -Z 1 =Z 2 -B 2 ) is a polymer block that does not contain
7. The polymer according to claim 6, wherein the total number average molecular weight of the polymer blocks α and β contained in the polymer represented by the general formula (5) is 1000 or more, the total number average molecular weight of the polymer blocks β is 1000 or more, and the total number average molecular weight of the polymer represented by the general formula (5) is 3500 or more.
8. The polymer according to claim 6 or 7, wherein the polymer block β is a polymer block containing at least one of structural units derived from a styrene derivative, a (meth)acrylic acid derivative, and an olefin derivative.
9. The polymer according to any one of claims 1 to 8, wherein the wavelength of the light is 280 nm or more and 480 nm or less.
10. A toner comprising the polymer according to any one of claims 1 to 9.
11. The toner according to claim 10, further comprising a binder resin.
12. The toner according to claim 11, wherein the binder resin comprises at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.
13. 13. An image forming method comprising: a step of forming a toner image made of the toner according to claim 10 on a recording medium; and a step of irradiating the toner image with light to soften the toner image.
14. The image forming method according to claim 13, wherein the wavelength of the light is 280 nm or more and 480 nm or less.
15. 15. The image forming method according to claim 13, further comprising a step of pressing the toner image.
16. The image forming method according to claim 15 , wherein the toner image is further heated in the pressurizing step.
17. 17. The image forming method according to claim 13, wherein in the step of irradiating the toner image with light to soften the toner image, the toner image is heated in addition to being irradiated with light.
18. A photoresponsive adhesive comprising the polymer according to any one of claims 1 to 9.
19. An optical switching material using the polymer according to any one of claims 1 to 9.
Citation Information
Patent Citations
Optical compensating sheet, its production and liquid crystal display element using same
JP1995098413A
Optical film, polarizing plate and liquid crystal display device
JP2002107539A
High-molecular compound and method for producing the same
JP2002194030A
Photoresponsive liquid crystal compound
JP2011256155A
Method for fluidizing / non-fluidizing compound with light
JP2011256291A