Spunbond nonwoven fabrics and laminated nonwoven fabrics

A spunbond nonwoven fabric with a polymer combination of A and B, having a 30°C melting temperature difference, addresses the challenge of bulkiness and flexibility, ensuring high productivity and stability for sanitary materials.

JP7567478B2Active Publication Date: 2024-10-16TORAY INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020540357
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-16
Filing Date
2020-07-10
Publication Date
2024-10-16
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Existing spunbond nonwoven fabrics face challenges in achieving high bulkiness and flexibility while maintaining productivity and stability, particularly for sanitary material applications, due to complex manufacturing processes and reduced bulkiness from consolidation and embossing.

Method used

A spunbond nonwoven fabric using a specific combination of polymers A and B, where polymer B has a melting temperature 30°C higher than polymer A, with side-by-side fibers and connection parts containing polymer A, resulting in high bulkiness and stability with a simpler process.

Benefits of technology

The fabric achieves excellent productivity and stability with high bulkiness, suitable for sanitary materials like disposable diapers and sanitary napkins, offering a soft feel and improved morphological stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567478000002
    Figure 0007567478000002
  • Figure 0007567478000001
    Figure 0007567478000001
Patent Text Reader

Abstract

The present invention relates to a spun-bonded nonwoven fabric that contains a long fiber. The long fiber contains a polymer A and a polymer B. The melting temperature of polymer B is higher than the melting temperature of polymer A by at least 30°C. The apparent density of the span-bonded nonwoven fabric is 0.050 g / cm3 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a spunbond nonwoven fabric that is pleasant to the touch and is particularly suitable for use as a sanitary material. [Background technology]

[0002] In general, nonwoven fabrics for sanitary materials such as disposable diapers and sanitary napkins are required to have excellent bulkiness and softness in order to improve the texture when worn. Bulkiness is particularly required for surface members that come into direct contact with the skin.

[0003] Conventionally, as the surface material of sanitary materials, so-called air-through nonwoven fabrics, which are made by carding short fibers into a sheet and then subjecting the sheet to self-fusion by hot air treatment, have been suitably used. Air-through nonwoven fabrics are characterized by excellent bulkiness and flexibility, and therefore have an excellent soft feel, and are widely used, but have the disadvantages of a complicated manufacturing process and a slow production speed.

[0004] On the other hand, spunbonded nonwoven fabrics are characterized by their high productivity and low cost due to their manufacturing process, but the manufacturing process of spunbonded nonwoven fabrics is a manufacturing process that tends to result in a structure in which the constituent long fibers are oriented in the plane direction, making it difficult to obtain spunbonded nonwoven fabrics with excellent bulkiness and softness.

[0005] Therefore, studies are being conducted to improve the soft feel by imparting crimps to long fibers to obtain high bulkiness.

[0006] For example, Patent Document 1 proposes a crimped conjugate fiber composed of two component polymers whose melting temperatures differ by 10° C. or more.

[0007] Furthermore, Patent Document 2 proposes a technique in which a web made of two component polymers is heated to give it shrinkage, then cooled, and subsequently fused by hot air treatment.

[0008] Furthermore, Patent Document 3 proposes a technique in which a web made of two component polymers is first consolidated and embossed, and then fused by hot air treatment. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent No. 5484564 [Patent Document 2] Japan Special Publication No. 2005-514528 [Patent Document 3] Japanese Patent Application Publication No. 2018-024965 Summary of the Invention [Problem to be solved by the invention]

[0010] According to the technology disclosed in Patent Document 1, it is possible to improve the bulkiness by the crimping during spinning. However, since the shape is fixed by embossing, which involves heat fusion while compressing, it is not possible to obtain sufficient bulkiness.

[0011] According to the technology disclosed in Patent Document 2, bulkiness is improved by inducing shrinkage through heat treatment after spinning and then fusing with hot air. However, since heat treatment needs to be performed twice, there are problems in that the productivity is poor and the bulkiness is insufficient.

[0012] According to the technology disclosed in Patent Document 3, bulkiness is improved by crimping during spinning. However, this is a complicated process in which the fibers are then compressed and then fused by embossing or hot air treatment, and the bulkiness is reduced by the compression, and there is also a problem in productivity.

[0013] Thus, conventionally, it has not been possible to obtain a spunbond nonwoven fabric that is excellent in productivity and stability and has a high level of bulkiness sufficient for use as a sanitary material.

[0014] Therefore, an object of the present invention has been made in consideration of the above circumstances, and is to provide a spunbonded nonwoven fabric which is excellent in productivity and stability and has a high level of bulkiness sufficient for use as a sanitary material. [Means for solving the problem]

[0015] Means for Solving the Problems The present inventors have conducted extensive research to achieve the above object, and as a result have discovered that by using a specific combination of polymers, the long fibers can maintain sufficient rigidity during the process of developing crimp and fusing the long fibers together, thereby making it possible to obtain a spunbonded nonwoven fabric having high bulkiness through a process simpler than that of the conventional manufacturing methods.

[0016] The present invention has been completed based on these findings, and provides the following inventions.

[0017] <1> A spunbond nonwoven fabric containing long fibers, The long fibers contain polymer A and polymer B, The melting temperature of the polymer B is 30° C. or more higher than the melting temperature of the polymer A, The apparent density of the spunbond nonwoven fabric is 0.050 g / cm 3 The following is a spunbond nonwoven fabric. <2> The polymer A is a polyolefin-based polymer, and the polymer B is a polyester-based polymer. <1> The spunbond nonwoven fabric according to claim 1. <3> The long fibers are side-by-side fibers. <1> or <2> The spunbond nonwoven fabric according to claim 1. <4> The long fiber has a plurality of connection parts connecting any two of the long fibers, At least one of the connecting parts includes the polymer A; <1> ~ <3> 13. The spunbond nonwoven fabric according to any one of claims 1 to 12. <5> The cross-sectional shape of the long fiber is dumbbell-shaped. <1> ~ <4> 13. The spunbond nonwoven fabric according to any one of claims 1 to 12. <6> At least the surface, <1> ~ <5> A laminated nonwoven fabric, which is a spunbond nonwoven fabric according to any one of claims 1 to 5. Effect of the Invention

[0018] According to the present invention, a spunbonded nonwoven fabric having excellent productivity, stability, and high bulkiness can be obtained. In particular, the spunbonded nonwoven fabric of the present invention is characterized by excellent productivity and excellent softness obtained from high bulkiness, and therefore can be suitably used for sanitary materials such as disposable diapers and sanitary napkins, which strongly require both high productivity and a comfortable touch. [Brief description of the drawings]

[0019] [Figure 1] Fig. 1 is a cross-sectional view of one embodiment of the long fiber used in the spunbonded nonwoven fabric of the present invention. The long fiber in Fig. 1 is a side-by-side fiber having a dumbbell-shaped cross-sectional shape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The spunbond nonwoven fabric of the present invention contains long fibers containing polymer A and polymer B, the melting temperature of polymer B is 30° C. or more higher than the melting temperature of polymer A, and the apparent density of the spunbond nonwoven fabric is 0.05 g / cm 3 The following is the result. The details of this are explained below.

[0021] [Polymer A and Polymer B] As the polymer A and the polymer B, for example, a thermoplastic resin can be used. Examples of thermoplastic resins include aromatic polyester polymers and copolymers thereof such as "polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyhexamethylene terephthalate"; aliphatic polyester polymers and copolymers thereof such as "polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, polyhydroxybutyrate-polyhydroxyvalerate copolymer, polycaprolactone"; aliphatic polyamide polymers and copolymers thereof such as "polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 12, polyamide 6-12"; polyolefin polymers and copolymers thereof such as "polypropylene, polyethylene, polybutene, polymethylpentene"; water-insoluble ethylene-vinyl alcohol copolymer polymers containing 25 mol% to 70 mol% ethylene units; polystyrene-based, polydiene-based, chlorine-based, polyolefin-based, polyester-based, polyurethane-based, polyamide-based, and fluorine-based elastomer polymers. At least two of these can be selected and used as polymer A and polymer B.

[0022] Here, as the polymer A, which is the low melting temperature component, it is preferable to select a polymer having a relatively low melting temperature among the above-mentioned thermoplastic resins, and it is preferable to use polyolefin-based polymers such as "polypropylene, polyethylene, polybutene, polymethylpentene" and copolymers thereof.

[0023] On the other hand, as polymer B, which is a high melting temperature component, it is preferable to use aromatic polyester-based polymers and copolymers thereof, such as "polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyhexamethylene terephthalate," or aliphatic polyester-based polymers and copolymers thereof, such as "polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, polyhydroxybutyrate-polyhydroxyvalerate copolymer, polycaprolactone."

[0024] In particular, aromatic polyesters such as "polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyhexamethylene terephthalate" are used as polymer B because they are easy to obtain spunbonded nonwoven fabrics with excellent strength and excellent fluff resistance. Polymers and their copolymers It is more preferable to use

[0025] As described above, the melting temperature of polymer B is at least 30° C. higher than the melting temperature of polymer A. The difference between the melting temperatures of polymer B and polymer A is preferably at least 60° C., more preferably at least 80° C. In this way, a spunbond nonwoven fabric having bulkiness suitable for sanitary material applications can be obtained.

[0026] The melting temperature of the polymer A and the melting temperature of the polymer B used in the present invention are preferably from 100° C. to 300° C., more preferably from 120° C. to 280° C. By setting the melting temperature to 100° C. or higher, it becomes easier to obtain heat resistance sufficient for practical use.

[0027] The melting temperatures of polymer A and polymer B are preferably 300° C. or lower, and more preferably 280° C. or lower. By setting the melting temperatures to 300° C. or lower, the yarn discharged from the spinneret can be easily cooled, fusion between the fibers can be suppressed, and the resulting spunbonded nonwoven fabric has fewer defects.

[0028] The melting temperature in the present invention refers to the peak top temperature of the endothermic peak measured using a differential scanning calorimeter (for example, "DSCQ2000" manufactured by TA Instruments) under a nitrogen atmosphere at a heating rate of 16°C / min.

[0029] Furthermore, additives such as antioxidants, weather resistance stabilizers, light resistance stabilizers, antistatic agents, spinning agents, antiblocking agents, nucleating agents, and pigments, or other polymers may be added to Polymer A and Polymer B as necessary, within the scope of not impairing the effects of the present invention.

[0030] [Long fiber] The long fibers contained in the spunbonded nonwoven fabric of the present invention contain the above-mentioned polymer A and polymer B, and are preferably long fibers made of polymer A and polymer B. In this long fiber, polymer A and polymer B each form a region, and polymer A and polymer B are bonded to each other via an interface. The long fiber can be selected from composite fibers in the form of side-by-side fibers, eccentric core-sheath fibers, etc.

[0031] Among them, from the viewpoint of obtaining a high degree of crimp, it is preferable to use side-by-side fibers as the long fibers because it is easy to control the positions and amounts of both polymers. In particular, it is more preferable to use dumbbell-shaped side-by-side fibers as shown in Figure 1 because it is easy to impart fine crimps.

[0032] On the other hand, when there is a difference between the melt viscosities of polymer A and polymer B, it is also a preferred embodiment to use eccentric core-sheath fibers as the long fibers from the viewpoint of spinnability. In the present invention, the difference in melt viscosity means that one of the two is 10% or more higher than the other in viscosity, extrapolated to a shear rate of zero from a viscosity curve measured at the spinning temperature using a dynamic viscoelasticity evaluation device (e.g., "Rheosol-G3000" manufactured by UBM).

[0033] [Spunbond nonwoven fabric] The spunbond nonwoven fabric of the present invention has a tensile strength per unit area of ​​0.3 (N / 5cm) / (g / m 2 ) or more 10.0(N / 5cm) / (g / m 2 ) or less.

[0034] The tensile strength per unit weight is 0.3 (N / 5cm) / (g / m 2 ) or more, the fabric can withstand the process of manufacturing paper diapers and the like and can withstand use as a product. The tensile strength per unit area is preferably 0.4 (N / 5cm) / (g / m 2 ) or more, more preferably 0.5 (N / 5cm) / (g / m 2 )That's all.

[0035] On the other hand, the tensile strength per unit area is 10.0 (N / 5cm) / (g / m 2 ) or less, the flexibility of the spunbonded nonwoven fabric can be improved. The tensile strength per unit area is more preferably 8.0 (N / 5cm) / (g / m 2 ) or less, more preferably 6.0 (N / 5cm) / (g / m 2 ) or less.

[0036] The tensile strength per unit area weight can be controlled by the above-mentioned thermoplastic resin, additives, fiber diameter, and / or the spinning speed, area weight, apparent density, and bonding method described below.

[0037] The tensile strength per unit area weight of the spunbond nonwoven fabric in the present invention is the average of the tensile strengths (strength at the time the sample breaks) in two perpendicular directions in a tensile test performed in accordance with "6.3.1 Standard time" of "6.3 Tensile strength and elongation (ISO method)" of JIS L1913:2010 "Testing methods for general nonwoven fabrics" with a gripping distance of at least 5 cm, divided by the area weight measured by the method described below.

[0038] The spunbond nonwoven fabric of the present invention preferably has a thickness of 0.05 mm or more and 1.50 mm or less.

[0039] When the thickness is 0.05 mm or more, the spunbond nonwoven fabric has an appropriate cushioning property. The thickness is more preferably 0.07 mm or more, and further preferably 0.09 mm or more.

[0040] On the other hand, when the thickness is 1.50 mm or less, the spunbonded nonwoven fabric has excellent bending flexibility. The thickness is more preferably 0.14 mm or less, and further preferably 0.13 mm or less.

[0041] The thickness of the spunbond nonwoven fabric in the present invention is not particularly limited, but refers to the thickness under no load measured, for example, with a shape measuring machine (for example, "VR3050" manufactured by Keyence Corporation).

[0042] The spunbond nonwoven fabric of the present invention has a basis weight of 10 g / m 2 More than 100g / m 2 It is preferable that:

[0043] The weight of the spunbond nonwoven fabric is 10g / m 2 Due to the above, the spunbond nonwoven fabric can be easily made to a thickness suitable for use as a sanitary material, and can have mechanical strength sufficient for practical use.

[0044] On the other hand, the basis weight of spunbond nonwoven fabric is 100 g / m 2 By setting the weight per unit area of ​​the spunbond nonwoven fabric to 80 g / m or less, it is possible to obtain a spunbond nonwoven fabric having excellent breathability and flexibility. The weight per unit area of ​​the spunbond nonwoven fabric is preferably 80 g / m or less. 2 Less than 60 g / m, more preferably 2 The following is the result.

[0045] In addition, the basis weight (g / m 2 ) is based on "6.2 Mass per unit area" of JIS L1913:2010, and is calculated by taking 3 test pieces of 20cm x 25cm per 1m width of the sample, measuring the mass (g) of each piece under standard conditions, and averaging the masses per unit area of ​​1m. 2 This refers to the mass per unit.

[0046] The spunbond nonwoven fabric of the present invention has an apparent density of 0.050 g / cm 3 The following is the result.

[0047] The apparent density of spunbond nonwoven fabric is 0.050 g / cm 3 By setting the apparent density to 0.045 g / cm or less, it is easy to obtain a spunbonded nonwoven fabric having excellent breathability and flexibility, and it is easy to feel high bulkiness. The apparent density of the spunbonded nonwoven fabric is preferably 0.045 g / cm or less. 3Less than or equal to 0.040 g / cm 3 The following is the result.

[0048] The lower limit of the apparent density of the spunbond nonwoven fabric is not particularly limited, but is, for example, 0.01 g / cm 3 By satisfying the above, shape stability sufficient for practical use is easily obtained.

[0049] The apparent density of the spunbonded nonwoven fabric in the present invention is the value obtained by dividing the basis weight by the thickness.

[0050] The spunbond nonwoven fabric of the present invention preferably has a plurality of connection parts connecting any two of the long fibers, and at least one of the connection parts contains the polymer A, since this provides high dimensional stability.

[0051] The connection containing polymer A means that a certain long fiber and an adjacent long fiber are partially fused to each other by polymer A, and means that there are essentially no areas where the long fibers are fused to each other in a continuous manner to form a film having a certain width.

[0052] [Manufacturing method of spunbond nonwoven fabric] Next, a preferred embodiment of the method for producing the spunbonded nonwoven fabric of the present invention will be specifically described. In the spunbonding process for producing spunbonded nonwoven fabrics, the raw thermoplastic resins (polymer A, polymer B) are melted, spun from a spinneret, and cooled to solidify to obtain threads. The resulting threads are then pulled and stretched by an ejector to obtain long fibers. The long fibers are then collected on a moving net to form a nonwoven fiber web, which is then thermally bonded to obtain the spunbonded nonwoven fabric.

[0053] The shape of the spinneret and ejector to be used may be various, such as round or rectangular. Among them, a combination of a rectangular spinneret and a rectangular ejector is preferably used, from the viewpoints of using a relatively small amount of compressed air and preventing fusion or abrasion between the yarns.

[0054] As an example of a preferred method for producing the long fibers used in the present invention, polymer A and polymer B are melted and metered in separate extruders, respectively, and fed to a side-by-side or eccentric core-sheath type composite spinneret to be spun into long fibers. In this case, it is preferable that polymer A, which is a low melting temperature component, is exposed on the surface, since this makes it easier to bond the long fibers together in the thermal bonding step described below.

[0055] In the present invention, the spinning temperature is preferably set to (melting temperature of the thermoplastic resin as raw material + 10°C) or more (melting temperature of the thermoplastic resin as raw material + 100°C) or less. By setting the spinning temperature within the above range, a stable molten state can be achieved, and excellent spinning stability can be obtained.

[0056] The spun long fiber yarn is then cooled, and the cooling method for the spun yarn may be, for example, a method of forcibly blowing cold air onto the yarn, a method of naturally cooling the yarn at the ambient temperature around the yarn, a method of adjusting the distance between the spinneret and the ejector, etc. Alternatively, a combination of these methods may be used. The cooling conditions may be appropriately adjusted taking into consideration the discharge rate per hole of the spinneret, the spinning temperature, the ambient temperature, etc.

[0057] Next, the cooled and solidified yarn is pulled and stretched by compressed air jetted from an ejector.

[0058] The spinning speed is preferably 2000 m / min or more, more preferably 3000 m / min or more, and further preferably 4000 m / min or more. By setting the spinning speed at 2000 m / min or more, high productivity is achieved, and the orientation and crystallization of the fibers progresses, making it possible to obtain long fibers with high strength.

[0059] The obtained long fibers are then collected on a moving net to form a nonwoven fiber web. In the present invention, since the fibers are drawn at a high spinning speed, the fibers discharged from the ejector are collected on the net under a controlled condition of a high-speed air flow, and a nonwoven fiber web with less fiber entanglement and high uniformity can be obtained.

[0060] Although such a nonwoven fiber web can be made into a spunbonded nonwoven fabric using only one nonwoven fiber web, it is also preferred in that productivity can be increased by arranging multiple spinning equipment in the process direction to stack multiple webs to obtain a spunbonded nonwoven fabric.

[0061] In addition, the raw materials and process conditions can be changed for each nonwoven fiber web. Furthermore, laminating layers of melt-blown nonwoven fabrics to obtain a laminated nonwoven fabric is also a preferred embodiment. In the present invention, these laminates are also collectively referred to as "nonwoven fiber webs."

[0062] The resulting nonwoven fiber webs are then integrated by thermal bonding to obtain the intended spunbonded nonwoven fabric or laminated nonwoven fabric.

[0063] Examples of a method for integrating the nonwoven fiber webs by thermal bonding include a method of thermal bonding with heated air and a method of thermal bonding with a roll.

[0064] Examples of rolls used for thermal bonding include a thermal embossing roll consisting of a pair of upper and lower rolls, each of which has an engraving (uneven portion) on its surface; a thermal embossing roll consisting of a combination of one roll with a flat (smooth) surface and the other roll with an engraving (uneven portion) on its surface; and a thermal calendar roll consisting of a combination of a pair of upper and lower flat (smooth) rolls.

[0065] In the present invention, in order to obtain a high bulkiness, a method of thermal bonding using heated air, which does not involve the application of pressure by rolls, is preferred. In the method of thermal bonding using heated air, it is preferred to heat the air to a temperature between the melting temperature of polymer A and the melting temperature of polymer B, since this allows the shape to be fixed while maintaining the thickness.

[0066] [Laminated nonwoven fabric] At least the surface layer of the laminated nonwoven fabric of the present invention is the spunbonded nonwoven fabric of the present invention.

[0067] The laminated nonwoven fabric of the present invention is preferably a laminated nonwoven fabric in which the spunbonded nonwoven fabric of the present invention is laminated as a surface layer and a meltblown nonwoven fabric is laminated as an inner layer. By adopting such a constitution, it is possible to impart a level of water resistance required for a laminated nonwoven fabric for sanitary materials, particularly for waist gathering applications.

[0068] In a preferred embodiment of the laminated nonwoven fabric of the present invention, a layer (S) of a spunbonded nonwoven fabric is disposed as a surface layer, and a layer (M) of a meltblown nonwoven fabric is disposed as an inner layer. The number and combination of layers of the laminated nonwoven fabric can be any configuration depending on the purpose, such as SMS, SMMS, SSMMS, and SMSMS.

[0069] The basis weight of the laminated nonwoven fabric of the present invention is 10 g / m 2 More than 100g / m 2 It is preferable that:

[0070] The basis weight of the laminated nonwoven fabric is 10g / m 2 By adjusting the weight of the laminated nonwoven fabric to the above value, it is possible to obtain a laminated nonwoven fabric having a mechanical strength sufficient for practical use. The weight of the laminated nonwoven fabric is preferably 13 g / m 2 More preferably, 15 g / m 2 That's all.

[0071] On the other hand, the basis weight of the laminated nonwoven fabric is 100 g / m 2By setting the weight per unit area as below, a laminated nonwoven fabric having appropriate flexibility suitable for use as a nonwoven fabric for sanitary materials can be obtained. The weight per unit area of ​​the laminated nonwoven fabric is more preferably 50 g / m 2 Less than 35 g / m, more preferably 35 g / m 2 The following is the result.

[0072] In addition, the basis weight (g / m 2 ) is based on "6.2 Mass per unit area" of JIS L1913:2010, and is calculated by taking 3 test pieces of 20cm x 25cm per 1m width of the sample, measuring the mass (g) of each piece under standard conditions, and averaging the masses per unit area of ​​1m. 2 This refers to the mass per unit.

[0073] As described above, the spunbond nonwoven fabric and laminated nonwoven fabric of the present invention are characterized by excellent productivity and excellent softness resulting from high bulkiness, and therefore can be suitably used for sanitary materials such as disposable diapers and sanitary napkins, which strongly require both high productivity and a pleasant touch. The "soft feel" referred to in the present invention means a smooth feel when the surface is stroked and a moderate elasticity is felt in the thickness direction. EXAMPLES

[0074] Next, the present invention will be specifically described based on examples. However, the present invention is not limited to these examples. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was performed based on the above-mentioned method. However, the present invention is not limited to the description of these examples.

[0075] (Observation, Measurement) The following observations or measurements were made on the long fibers, polymers, or spunbond nonwoven fabrics, and the results are shown in Table 1.

[0076] (1) Cross section of long fiber Ten small samples were randomly taken from the obtained long fibers, and their cross sections were observed under a microscope to confirm their shapes.

[0077] (2) Melting temperature The melting temperatures of polymer A and polymer B were measured using a differential scanning calorimeter (TA Instruments' "DSCQ2000"). The melting temperature difference (°C) was calculated using the following formula. Melting temperature difference (℃) = Melting temperature of polymer B - Melting temperature of polymer A

[0078] (3) Metsuke Based on "6.2 Mass per unit area" of JIS L1913:2010, 20cm x 25cm test pieces were taken from the obtained spunbond nonwoven fabric, 3 pieces per 1m width, and the mass (g) of each was measured under standard conditions, and the mass per unit area was calculated from the average value. 2 The mass per unit was taken as the basis weight.

[0079] (4) Thickness The no-load thickness of the obtained spunbond nonwoven fabric was measured using a shape measuring machine (Keyence Corporation, "VR3050").

[0080] (5) Apparent density Based on "6.2 Mass per unit area" of JIS L1913:2010, 20cm x 25cm test pieces were taken from the obtained spunbond nonwoven fabric, 3 pieces per 1m width, and the mass (g) of each was measured under standard conditions, and the mass per unit area was calculated from the average value. 2 The mass per unit area was measured using a shape measuring instrument (Keyence Corporation, "VR3050") The obtained value was divided by the thickness of the spunbond nonwoven fabric under no load to obtain the apparent density.

[0081] (6) Tensile strength per unit area The tensile strength per unit area was calculated by averaging the tensile strength (the strength at which the spunbond nonwoven fabric breaks) in two perpendicular directions, using a tensile test with a gripping distance of at least 5 cm, in accordance with "6.3.1 Standard time" of "6.3 Tensile strength and elongation (ISO method)" of JIS L1913:2010 "Testing methods for general nonwoven fabrics." The tensile strength per unit area was calculated by dividing the average of the tensile strengths (the strength at which the spunbond nonwoven fabric breaks) in two perpendicular directions by the area weight.

[0082] (7) Softness (grade) Ten randomly selected panelists touched the obtained spunbond nonwoven fabrics with their hands and evaluated each of the spunbond nonwoven fabrics according to the following criteria. The average score of the evaluation results for each spunbond nonwoven fabric was regarded as the softness of the spunbond nonwoven fabric.

[0083] 5: Very comfortable, with a soft feel that I really liked (the surface felt smooth to the touch when stroked, and had a moderate amount of elasticity in the thickness direction). 4: Somewhat comfortable, with a soft feel that I somewhat liked. 3: The softness was not unpleasant but not comfortable, and was not something I disliked but did not like either. 2: Slightly uncomfortable, soft feeling that was somewhat disliked. 1: Very uncomfortable, very disliked soft feel (the surface felt rough when stroked, and either a strong rebound or the surface became floppy when pressed).

[0084] Example 1 Polyethylene (PE) as polymer A and polyethylene terephthalate (PET) as polymer B were melted in an extruder and formed into side-by-side composite fibers (mass ratio 1:1) at a spinning temperature of 290°C, and spun from a rectangular spinneret with holes with a hole diameter φ of 0.30 mm at a single-hole output rate of 0.6 g / min.

[0085] The spun yarn was cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, and collected on a moving net to obtain long fibers. The long fibers were then heated with hot air at 150°C to thermally bond the fibers to a basis weight of 20 g / m. 2 A spunbond nonwoven fabric of this type was obtained.

[0086] Example 2 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that eccentric core-sheath type conjugate fibers were formed instead of side-by-side type conjugate fibers.

[0087] Example 3 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that the spinning was carried out under the following conditions. Shape of holes in rectangular base: A shape with a circle on each side of a rectangle Diameter of the circles on both sides of the rectangle: 0.30 mm Center distance between two circles on either side of a rectangle: 0.8mm Single hole discharge rate: 0.6g / min

[0088] Comparative Example 1 Polypropylene (PP) was melted in an extruder and formed into a single component fiber at a spinning temperature of 230°C. The fiber was then spun from a rectangular die having holes with a diameter φ of 0.30 mm at a single hole throughput rate of 0.6 g / min.

[0089] The spun yarn was cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, and collected on a moving net to obtain long fibers. The long fibers were then thermally bonded (linear pressure: 50 N / cm, thermal bonding temperature: 130°C) by a pair of upper and lower heat embossing rolls consisting of an upper roll and a lower roll, to obtain a basis weight of 20 g / m. 2 A spunbond nonwoven fabric of this type was obtained.

[0090] The upper roll was an embossed metal roll engraved with polka dots to a depth of 0.5 mm and with a bonding area ratio of 16%, and the lower roll was a flat metal roll.

[0091] Comparative Example 2 A spunbond nonwoven fabric was obtained in the same manner as in Comparative Example 1, except that copolymer PP was used as polymer A and PP was used as polymer B, each of which was melted in an extruder and formed into a side-by-side type composite fiber (mass ratio 1:1) at a spinning temperature of 230°C, and spun from a rectangular spinneret having holes with a hole diameter φ of 0.30 mm at a single-hole output rate of 0.6 g / min.

[0092] Comparative Example 3 A spunbond nonwoven fabric was obtained in the same manner as in Comparative Example 2, except that PE was used as the polymer A.

[0093] Comparative Example 4 A spunbonded nonwoven fabric was obtained in the same manner as in Comparative Example 1, except that the obtained long fibers were heated with hot air at 150° C. for thermal bonding.

[0094] [Table 1]

[0095] As shown in Table 1, the spunbond nonwoven fabrics of Examples 1 to 3 had sensory evaluation results of 4.0 to 5.0, which indicated excellent softness. Therefore, it was found that the spunbond nonwoven fabrics of Examples 1 to 3 had a satisfactory level of high bulkiness for use as sanitary materials.

[0096] The spunbonded nonwoven fabrics of Examples 1 to 3 are more productive than the air-through nonwoven fabrics, and furthermore, the spunbonded nonwoven fabrics of Examples 1 to 3 are fused and have a high level of bulkiness, and therefore have excellent shape stability.

[0097] On the other hand, in Comparative Examples 1 to 4, the sensory evaluation results were 2.0 or less, which indicated poor softness.

[0098] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2019-130840) filed on July 16, 2019, the contents of which are incorporated herein by reference. [Explanation of symbols]

[0099] A Polymer B Polymer

Claims

1. A spunbond nonwoven fabric containing long fibers, The long fiber contains polymer A and polymer B and is a side-by-side fiber, The polymer A is a polyolefin-based polymer, and the polymer B is polyethylene terephthalate or a copolymer thereof, The melting temperature of the polymer B is higher than the melting temperature of the polymer A by 30° C. or more, The apparent density of the spunbond nonwoven fabric is 0.050 g / cm 3 The following is a spunbond nonwoven fabric.

2. The long fiber has a plurality of connection portions each connecting any two of the long fiber, 2. The spunbond nonwoven fabric of claim 1, wherein at least one of the connections comprises the polymer A.

3. 3. The spunbond nonwoven fabric according to claim 1, wherein the cross-sectional shape of the long fibers is dumbbell-shaped.

4. A laminated nonwoven fabric, at least a surface layer of which is the spunbonded nonwoven fabric according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Novel butyrolactone derivative and its preparation

    JP1979084564A

  • Nonwoven filament cloth

    JP1992174753A

  • Nonwoven fabric having three-layer structure and its production

    JP1994128855A

  • Nonwoven fabric of polylactate-based filament and its production

    JP1997095847A

  • Laminated nonwoven fabric

    JP1997111635A