Preparation method of BTO-PDMS fiber film
By modifying with vinylsilane coupling agents and using electrospinning technology, the problem of poor dispersion of barium titanate nanoparticles in polymers was solved, and BTO@PDMS fiber films with excellent piezoelectric properties were prepared, which are suitable for flexible piezoelectric sensors.
Patent Information
- Application Number
- CN202411144059.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-20
AI Technical Summary
In existing technologies, barium titanate nanoparticles exhibit poor dispersion in polymers, resulting in poor piezoelectric and mechanical properties. Furthermore, the preparation process is complex and energy-intensive, which hinders the application of flexible piezoelectric sensors.
Barium titanate nanoparticles were surface modified using a vinyl silane coupling agent, and the ordered arrangement of internal dipoles of barium titanate was achieved by electrospinning under a high voltage electric field. BTO@PDMS fiber films were then prepared by high-temperature crosslinking and curing.
The dispersibility of barium titanate in polymers was improved, enhancing piezoelectric properties, simplifying the preparation process, reducing energy consumption, and producing a flexible piezoelectric sensor material with low Young's modulus and excellent piezoelectric constant.
Smart Images

Figure CN118957884A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric films, and in particular to a method for preparing a BTO@PDMS fiber film. Background Art
[0002] With the rapid development of industrialization, the depletion of fossil energy has forced people to explore green energy to cope with the current energy crisis. Piezoelectric materials based on the piezoelectric effect have been widely studied in the field of mechanical energy collection because of their ability to convert mechanical energy into electrical energy. At present, extensive research focuses on the composite of piezoelectric materials with high piezoelectric properties with flexible polymers to achieve the purpose of combining the advantages of both to develop high-performance flexible piezoelectric sensors. Among them, barium titanate is considered to be an ideal filler for the preparation of flexible piezoelectric sensors because of its advantages such as high piezoelectric constant, low dielectric constant and non-toxicity. However, for now, directly doping piezoelectric nanoparticles into polymers will lead to problems such as agglomeration and uneven dispersion of piezoelectric nanoparticles. By chemically modifying piezoelectric nanoparticles and combining them with polymers through chemical bonds, the agglomeration problem can be effectively improved. It is not only conducive to achieving the flexibility of the film, but also conducive to improving its flexibility in wearable applications.
[0003] The Chinese patent with the authorization announcement number CN113150554B discloses a PDMS-based flexible energy storage composite membrane, which has PDMS as the matrix and inorganic dielectric nanoparticles or inorganic dielectric nanowires as fillers; the inorganic dielectric nanoparticles are barium titanate or barium strontium titanate nanoparticles, and the inorganic dielectric nanowires are barium titanate or barium strontium titanate nanowires; when the filler is inorganic dielectric nanoparticles, the mass ratio of the filler to the PDMS is 1:19~1:4; when the filler is inorganic dielectric nanowires, the mass ratio of the filler to the PDMS is 1:39~1:9. The flexible energy storage composite membrane obtained by using PDMS as the matrix and inorganic dielectric nanomaterials as fillers has the advantages of high energy storage density and ultra-high energy storage efficiency. In particular, when barium titanate nanoparticles are used as fillers, the energy storage density of PDMS is as high as 7.1J / cm 3 The energy storage efficiency can be as high as 99%; when barium strontium titanate nanowires are used as fillers, the energy storage density is as high as 11.7 J / cm 3 , while maintaining an ultra-high energy storage efficiency of 99%.
[0004] Although the above-mentioned PDMS-based flexible energy storage composite film has made certain progress in improving energy storage density and energy storage efficiency, there are still some problems in its practical application. For example, due to the poor dispersion of barium titanate nanoparticles in the PDMS matrix, the piezoelectric properties and mechanical properties of the composite film cannot reach the optimal level. In addition, the prior art does not fully consider the effect of surface modification of nanoparticles on the piezoelectric properties of the composite film, which limits the application potential of PDMS-based composite films in the development of high-performance flexible piezoelectric sensors. Barium titanate has three crystal structures: orthorhombic phase, tetragonal phase and cubic phase. Among them, the orthorhombic phase is a stable structure at room temperature, but has no piezoelectric effect. The tetragonal phase and cubic phase are high-temperature phases. The tetragonal phase will transform into the cubic phase near the Curie temperature of about 120°C, and the cubic phase mainly has ferroelectric properties and weak piezoelectric properties. Only barium titanate with a tetragonal phase crystal structure has excellent piezoelectric properties at room temperature. Therefore, the flexible piezoelectric sensor based on barium titanate with a tetragonal phase crystal structure can have high piezoelectric properties. The Chinese patent with publication number CN116330773A discloses a method for preparing a composite nanogenerator for an intelligent monitoring system, comprising the following steps: S1: preparing barium titanate nanowires (BTO Ncs) by a two-step hydrothermal method and performing a hydroxylation treatment to obtain hydroxylated barium titanate nanowires; S2: mixing the hydroxylated barium titanate nanowires obtained in step S1 with carboxylated carbon nanotubes, PVDF and PDMS, and preparing a PVDF / PDMS-BTO-CNT nanofiber film by electrospinning; S3: bonding a PI film, a copper tape and the PVDF / PDMS-BTO-CNT nanofiber film obtained in step S2 in sequence, and pasting the PI film inside a rubber hose to assemble the composite nanogenerator. The barium titanate nanowires in the electrospun nanofiber film are arranged coaxially around the carbon nanotubes. The charges generated by triboelectricity help promote the dipole polarization inside the nanofiber film, thereby enhancing the piezoelectric performance and the output of the composite nanogenerator. Therefore, the performance when used as a composite nanogenerator is better than the sum of the performance of the triboelectric nanogenerator and the piezoelectric nanogenerator.
[0005] The disadvantage of the above-mentioned prior art is that, although the preparation method of the composite nanogenerator improves the piezoelectric performance to a certain extent, its preparation process is complicated and involves the mixing of multiple materials and multi-step processing, which not only increases the production cost but also reduces the production efficiency. In addition, due to the composite of multiple materials, compatibility problems between materials may occur, affecting the stability and reliability of the composite nanogenerator. At present, the polarization methods for making flexible piezoelectric films have piezoelectric effect mainly include electric field polarization, pressure polarization, thermal polarization, etc. Among them, pressure polarization and thermal polarization are relatively simple, but they will cause stress concentration in the film, film damage or interface defects. Electric field polarization is highly controllable, efficient and does not introduce stress to cause damage, so it is widely used, but the corona polarization method based on electric field has problems such as high energy consumption, long time consumption, and easy electrical breakdown of the film. Summary of the invention
[0006] The problem to be solved by the present invention is to provide a method for preparing a BTO@PDMS fiber film in view of the above-mentioned deficiencies existing in the prior art. The method mainly aims at the shortcomings that limit further application, such as poor dispersion of piezoelectric particles in flexible polymers, large energy consumption for high-voltage polarization, and complicated steps. Vinyl silane coupling agent is used to surface modify barium titanate nanoparticles to improve their dispersibility in polydimethylsiloxane, and the high-voltage electric field in electrostatic spinning is used to complete the one-step polarization of the internal dipoles of barium titanate from disordered to ordered arrangement during the preparation process of the film, thereby obtaining a BTO@PDMS fiber film with piezoelectric properties.
[0007] The above-mentioned object of the present invention is achieved through the following technical solutions: A method for preparing a BTO@PDMS fiber film comprises the following steps: S1, in hydrogen peroxide, tetragonal barium titanate nanoparticles undergo hydroxylation reaction, and after the reaction, surface hydroxylated barium titanate nanoparticles are obtained by post-treatment; S2: in an ethanol solution, the surface hydroxylated barium titanate nanoparticles obtained in S1 are subjected to surface modification under the action of a vinyl silane coupling agent, and after the modification, the surface hydroxylated barium titanate nanoparticles are subjected to post-treatment to obtain vinyl modified barium titanate nanoparticles; S3: ultrasonically dispersing the polydimethylsiloxane prepolymer and the vinyl-modified barium titanate nanoparticles obtained in S2 in n-hexane, and reacting them in the presence of tetrahydrofuran and a polydimethylsiloxane curing agent to obtain a BTO@PDMS core material solution; S4: mixing anhydrous ethanol and polyvinyl pyrrolidone to obtain a PVP shell solution; S5: coaxially electrospinning the BTO@PDMS core material solution obtained in S3 and the PVP shell solution obtained in S4, and collecting them with aluminum foil to obtain a PVP / BTO@PDMS fiber film; S6: After the PVP / BTO@PDMS fiber film obtained in S5 is peeled off from the aluminum foil, it is subjected to high-temperature cross-linking curing and washed with anhydrous ethanol in sequence to obtain a BTO@PDMS fiber film.
[0008] Furthermore, in the S1, the concentration of hydrogen peroxide is 70-80 wt%, and the dosage ratio of hydrogen peroxide to tetragonal barium titanate nanoparticles is controlled to be 150-250 mL: 10-20 g.
[0009] Furthermore, in S1, the tetragonal barium titanate nanoparticles are first ultrasonically dispersed in hydrogen peroxide, and the dispersion time is controlled to be 25-35 minutes, and then a hydroxylation reaction occurs, and the reaction temperature is controlled to be 100-110°C, the stirring speed is 700-900 r / min, and the reaction time is 5-7 hours.
[0010] Furthermore, in S2, the concentration of the ethanol solution is 70-80wt%, and the dosage ratio of the ethanol solution, hydroxylated barium titanate nanoparticles and vinyl silane coupling agent is controlled to be 40-80mL: 2.0-3.0g: 1.5-2.5g.
[0011] Furthermore, in the S2, the hydroxylated barium titanate nanoparticles and the vinyl silane coupling agent are first ultrasonically dispersed in an ethanol solution, and the dispersion time is controlled to be 25-35 minutes, and then the surface modification is carried out, and the reaction temperature is controlled to be 70-80°C, the stirring speed is 700-900 r / min, and the reaction time is 15-17 hours.
[0012] Furthermore, in S1 and S2, the post-treatment includes centrifugal washing with anhydrous ethanol for 2 to 3 times, and vacuum drying.
[0013] Furthermore, in S3, the dosage ratio of polydimethylsiloxane prepolymer, vinyl-modified barium titanate nanoparticles, polydimethylsiloxane curing agent and tetrahydrofuran is controlled to be 4.0-6.0 g: 0.50-0.60 g: 0.40-0.60 g: 0.4-0.6 mL, and the concentration of the BTO@PDMS core material solution is 8-12 wt %.
[0014] Furthermore, in S3, the dispersion time is first controlled to be 25-35 min, and then the reaction temperature is controlled to be 30-50° C., the stirring speed is 500-700 r / min, and the reaction time is 1-2 h.
[0015] Furthermore, in S4, the molecular weight of polyvinyl pyrrolidone is 1200-1400 kDa, the dosage ratio of anhydrous ethanol and polyvinyl pyrrolidone is controlled to be 15-20 mL: 1.5-2.0 g, and the concentration of the PVP shell solution is 12-18 wt %.
[0016] Furthermore, in S4, the mixing temperature is controlled to be 60-80° C., the stirring speed is 700-900 r / min, and the stirring time is 1-3 h.
[0017] Furthermore, in S5, the distance between the coaxial electrospinning needle and the roller collector is controlled to be 15 cm, the injection rate of the BTO@PDMS core solution is 0.8~1.2 mL / h, the injection rate of the PVP shell solution is 2.0~2.8 mL / h, the rotation speed of the roller collector is 100~150 r / min, the positive electrode of the electrospinning machine is applied with a voltage of +13 kV, the negative electrode is applied with a voltage of -2 kV, the electrospinning temperature is 20~40°C, and the ambient humidity is 40~50%.
[0018] Furthermore, in S5, after the electrospinning starts, a Taylor cone-shaped micro jet can be observed under a direct light. After the jet is stabilized, the direct light is turned off and the electrospinning is continued for 2 to 3 hours.
[0019] Furthermore, in S6, the cross-linking curing temperature is controlled to be 100-120° C., and the cross-linking curing time is 10-15 hours.
[0020] Specifically, the method comprises the following steps: S1: First, add 10-20 g of tetragonal barium titanate nanoparticles (BTO NPs) to 150-250 mL of 70-80 wt% hydrogen peroxide (reaction solvent), perform ultrasonic dispersion for 25-35 min, then build a reflux reaction device, control the oil bath temperature to 100-110 ° C, the stirring speed to 700-900 r / min, and the reaction time to 5-7 h. After the reaction, wash with anhydrous ethanol by centrifugation for 2-3 times, and vacuum dry to obtain surface hydroxylated barium titanate nanoparticles (BTO-OH NPs); S2: First, add 2.0-3.0 g of the hydroxylated barium titanate nanoparticles (BTO-OH NPs) obtained in S1 and 1.5-2.5 g of a vinyl silane coupling agent (KH-171, vinyl trimethoxysilane) to a 40-80 mL, 70-80 wt% ethanol solution (reaction solvent), perform ultrasonic dispersion for 25-35 min, then build a reflux reaction device, control the oil bath temperature to 70-80 ° C, the stirring speed to 700-900 r / min, and the reaction time to 15-17 h. After the reaction is completed, wash with anhydrous ethanol by centrifugation for 2-3 times, and vacuum dry to obtain vinyl-modified barium titanate nanoparticles (BTO NPs@SCA); S3: First, 0.50-0.60 g of the vinyl-modified barium titanate nanoparticles (BTO NPs@SCA) obtained in S2 and 1.0-2.0 mL of n-hexane (dispersant) are added to 4.0-6.0 g of polydimethylsiloxane prepolymer (PDMS prepolymer, which is not limited to, for example, high molecular weight terminal vinyl polydimethylsiloxane), and ultrasonic dispersion is performed for 25-35 min. Then, 0.40-0.60 g of polydimethylsiloxane curing agent (PDMS curing agent, which is not limited to, for example, DBP) and 0.4-0.6 mL of tetrahydrofuran (THF, reaction solvent) are added. Then, a stirring reaction device is built, and the oil bath temperature is controlled to be 30-50° C., the stirring speed is 500-700 r / min, and the reaction time is 1-2 h. After the reaction is completed, a 10 wt% BTO@PDMS core material solution is obtained. S4: First, add 1.5-2.0 g of 1200-1400 kDa polyvinyl pyrrolidone (PVP) powder to 15-20 mL of anhydrous ethanol (AE, reaction solvent), then build a stirring and mixing device, and control the oil bath temperature to 60-80 ° C, the stirring speed to 700-900 r / min, and the stirring time to 1-3 h to obtain a PVP shell solution; S5 first uses a 5mL syringe to absorb the 8~12wt% BTO@PDMS core material solution obtained in S3 and the 12~18wt% PVP shell solution obtained in S4, and the syringe is equipped with a 15G / 21G coaxial electrospinning needle. Then the syringe is installed on the fixed table of the electrospinning machine. The drum collector end of the electrospinning machine is collected with aluminum foil, and the distance between the coaxial electrospinning needle and the drum collector is controlled to be 15cm. The injection speed of the BTO@PDMS core material solution is 0.8~1.2mL / h, and the injection speed of the PVP shell solution is 2.0 ~2.8mL / h, the speed of the drum collector is 100~150r / min, +13kV voltage is applied to the positive electrode of the electrospinning machine, -2kV voltage is applied to the negative electrode, the electrospinning temperature is 20~40℃, the ambient humidity is 40~50%, and then electrospinning is started, and Taylor cone-shaped micro-jets can be observed under direct light. After the jet is stable (there are three main forms of instability in electrospinning: viscous instability, axisymmetric varicose instability, and non-axisymmetric tortuosity instability), the direct light is turned off, and electrospinning is performed for 2~3h to obtain PVP / BTO@PDMS fiber film; S6: After peeling the PVP / BTO@PDMS fiber film obtained in S5 from the aluminum foil, it is placed in an oven and baked at 100-120°C for 10-15h to ensure that the polydimethylsiloxane (PDMS) can be fully cross-linked and cured. The cured PVP / BTO@PDMS fiber film is then washed with anhydrous ethanol for multiple times until the PVP shell layer is removed to obtain a BTO@PDMS fiber film.
[0021] Preferably, the method comprises the following steps, S1: First, 15 g of tetragonal barium titanate nanoparticles (BTONPs) were added to 200 mL of 75 wt% hydrogen peroxide (reaction solvent), and ultrasonic dispersion was performed for 30 min. Then, a reflux reaction device was built, and the oil bath temperature was controlled to be 105 ° C, the stirring speed was 800 r / min, and the reaction time was 6 h. After the reaction, the mixture was washed by centrifugation with anhydrous ethanol for 3 times and vacuum dried to obtain surface hydroxylated barium titanate nanoparticles (BTO-OH NPs). S2: First, 2.5 g of the hydroxylated barium titanate nanoparticles (BTO-OH NPs) obtained in S1 and 2 g of a vinyl silane coupling agent (KH-171, vinyl trimethoxysilane) were added to a 50 mL, 80 wt% ethanol solution (reaction solvent), and ultrasonic dispersion was performed for 30 min. A reflux reaction device was then built, and the oil bath temperature was controlled to be 75 ° C. The stirring speed was 800 r / min and the reaction time was 16 h. After the reaction was completed, the anhydrous ethanol was centrifuged and washed three times, and vacuum dried to obtain vinyl-modified barium titanate nanoparticles (BTONPs@SCA); S3: First, 0.55 g of the vinyl-modified barium titanate nanoparticles (BTO NPs@SCA) obtained in S2 and 1.5 mL of n-hexane (dispersant) were added to 5 g of polydimethylsiloxane prepolymer (PDMS prepolymer, which may be, for example, high molecular weight end-vinyl polydimethylsiloxane without limitation), and ultrasonic dispersion was performed for 30 min. Then, 0.5 g of polydimethylsiloxane curing agent (PDMS curing agent, which may be, for example, DBP without limitation) and 0.5 mL of tetrahydrofuran (THF, reaction solvent) were added. Then, a stirring reaction device was built, and the oil bath temperature was controlled to be 40° C., the stirring speed was 600 r / min, and the reaction time was 1 h. After the reaction was completed, a 10 wt% BTO@PDMS core material solution was obtained. The mass volume ratio of the polydimethylsiloxane prepolymer, the polydimethylsiloxane curing agent and tetrahydrofuran is controlled to be 10 g: 1 g: 1 mL; S4: First, add 1.8 g of 1300 kDa polyvinyl pyrrolidone (PVP) powder to 16 mL of anhydrous ethanol (AE, reaction solvent), then build a stirring and mixing device, and control the oil bath temperature to 70 °C, the stirring speed to 800 r / min, and the stirring time to 2 h to obtain a PVP shell solution; S5 first uses a 5mL syringe to absorb the 10wt% BTO@PDMS core material solution obtained in S3 and the 15wt% PVP shell solution obtained in S4, and the syringe is equipped with a coaxial electrospinning needle of model 15G / 21G, and then the syringe is installed on the fixed table of the electrospinning machine. The drum collector end of the electrospinning machine is collected with aluminum foil, and the distance between the coaxial electrospinning needle and the drum collector is controlled to be 15cm. The injection speed of the BTO@PDMS core material solution is 1.0mL / h, and the injection speed of the PVP shell solution is 2.0mL / h. .4mL / h, the speed of the drum collector is 120r / min, +13kV voltage is applied to the positive electrode of the electrospinning machine, -2kV voltage is applied to the negative electrode, the electrospinning temperature is 30℃, the ambient humidity is 40-50%, and then electrospinning is started, and Taylor cone-shaped micro-jets can be observed under direct light. After the jet is stable (there are three main forms of instability in electrospinning: viscous instability, axisymmetric varicose instability, and non-axisymmetric tortuosity instability), the direct light is turned off, and electrospinning is performed for 2h to obtain PVP / BTO@PDMS fiber film; S6: After peeling the PVP / BTO@PDMS fiber film obtained in S5 from the aluminum foil, it is placed in an oven and baked at 110°C for 12 hours to ensure that the polydimethylsiloxane (PDMS) can be fully cross-linked and cured. The cured PVP / BTO@PDMS fiber film is then washed with anhydrous ethanol for multiple times until the PVP shell layer is removed to obtain a BTO@PDMS fiber film.
[0022] Preferably, in the BTO@PDMS fiber film, the BTO@PDMS fibers are uniform in thickness and show a 3D mesh structure unique to electrospinning. A three-dimensional multi-space structure is built between the fibers in the BTO@PDMS fibers, which is beneficial to stress concentration between the fibers when loaded and is beneficial to the output of piezoelectric charges.
[0023] In summary, the beneficial technical effects of the present invention are: The present invention uses a vinyl silane coupling agent to perform surface modification on barium titanate nanoparticles, thereby improving their dispersibility in polydimethylsiloxane; By using the coaxial electrospinning technology containing 10wt% BTO@PDMS core material solution and 15wt% PVP shell solution, the present invention realizes the orderly arrangement of the internal dipoles of barium titanate under the action of a high voltage electric field, thereby completing the polarization process in one step and significantly enhancing the piezoelectric properties of the BTO@PDMS fiber film. The PVP shell layer is removed through a high-temperature cross-linking curing reaction and anhydrous ethanol cleaning process. The BTO@PDMS fiber film prepared by the present invention exhibits a low Young's modulus, an excellent piezoelectric constant and excellent piezoelectric properties, and becomes an ideal material for preparing flexible piezoelectric sensors. The BTO@PDMS fiber film prepared by the present invention can be directly coated with electrodes and packaged into a piezoelectric flexible sensor that does not require an additional power source, and has a very wide range of application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a SEM image of the PVP / BTO@PDMS fiber film prepared in Example 2 of the present invention; Figure 2 is a SEM image of the BTO@PDMS fiber film prepared in Example 2 of the present invention; Figure 3 FTIR spectra of the PVP / BTO@PDMS fiber film and the BTO@PDMS fiber film prepared in Example 2 of the present invention; Figure 4 is a statistical diagram of the piezoelectric coefficient of the BTO@PDMS fiber film prepared in Example 2 of the present invention; Figure 5 This is a diagram of the butterfly piezoelectric response amplitude of the BTO@PDMS fiber film prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0025] In order to make the technical means, creative features, objectives and functions achieved by the present invention clearer and easier to understand, the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.
[0026] Example 1: A method for preparing a BTO@PDMS fiber film disclosed in the present invention comprises the following steps: S1, in hydrogen peroxide, tetragonal barium titanate nanoparticles undergo hydroxylation reaction, and after the reaction, surface hydroxylated barium titanate nanoparticles are obtained by post-treatment; S2: in an ethanol solution, the surface hydroxylated barium titanate nanoparticles obtained in S1 are subjected to surface modification under the action of a vinyl silane coupling agent, and after the modification, post-treatment is performed to obtain vinyl-modified barium titanate nanoparticles; S3 ultrasonically disperses the polydimethylsiloxane prepolymer and the vinyl-modified barium titanate nanoparticles obtained in S2 in n-hexane, and reacts them in the presence of tetrahydrofuran and a polydimethylsiloxane curing agent to obtain a BTO@PDMS core material solution; S4: mixing anhydrous ethanol and polyvinyl pyrrolidone to obtain a PVP shell solution; S5 performs coaxial electrospinning on the BTO@PDMS core material solution obtained in S3 and the PVP shell solution obtained in S4, and collects the mixture using aluminum foil to obtain a PVP / BTO@PDMS fiber film; S6 peels the PVP / BTO@PDMS fiber film obtained in S5 from the aluminum foil, and then performs high-temperature cross-linking curing and anhydrous ethanol washing in sequence to obtain a BTO@PDMS fiber film.
[0027] Example 2: A method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 1 in that it includes the following steps: S1 first added 15g of tetragonal barium titanate nanoparticles to 200mL of 75wt% hydrogen peroxide, and ultrasonically dispersed them for 30min. Then, a reflux reaction device was built, and the oil bath temperature was controlled to be 105℃, the stirring speed was 800r / min, and the reaction time was 6h. After the reaction, the mixture was centrifuged and washed 3 times with anhydrous ethanol, and vacuum dried to obtain surface hydroxylated barium titanate nanoparticles. S2 first added 2.5g of hydroxylated barium titanate nanoparticles obtained in S1 and 2g of vinyl silane coupling agent KH-171 into 50mL, 80wt% ethanol solution, and ultrasonically dispersed for 30min. Then, a reflux reaction device was built, and the oil bath temperature was controlled to 75°C, the stirring speed was 800r / min, and the reaction time was 16h. After the reaction was completed, the anhydrous ethanol was centrifuged and washed 3 times, and vacuum dried to obtain vinyl-modified barium titanate nanoparticles. S3 first added 0.55g of vinyl-modified barium titanate nanoparticles obtained in S2 and 1.5mL of n-hexane to 5g of polydimethylsiloxane prepolymer, and ultrasonically dispersed for 30min, then added 0.5g of polydimethylsiloxane curing agent and 0.5mL of tetrahydrofuran, and then built a stirring reaction device, and controlled the oil bath temperature to 40°C, the stirring speed to 600r / min, and the reaction time to 1h. After the reaction, a 10wt% BTO@PDMS core material solution was obtained; The mass volume ratio of the polydimethylsiloxane prepolymer, the polydimethylsiloxane curing agent and tetrahydrofuran is controlled to be 10 g: 1 g: 1 mL; S4: First, add 1.8 g of 1300 kDa polyvinyl pyrrolidone powder to 16 mL of anhydrous ethanol, then build a stirring and mixing device, and control the oil bath temperature to 70 ° C, the stirring speed to 800 r / min, and the stirring time to 2 h to obtain a PVP shell solution; S5 first used a 5 mL syringe to absorb the 10 wt% BTO@PDMS core solution obtained in S3 and the 15 wt% PVP shell solution obtained in S4, and installed a 15G / 21G coaxial electrospinning needle in the syringe. Then, the syringe was installed on the fixed table of the electrospinning machine. The roller collector end of the electrospinning machine was collected with aluminum foil, and the distance between the coaxial electrospinning needle and the roller collector was controlled to be 15 cm. The injection speed of the BTO@PDMS core solution was 1.5 times that of the PDMS core solution. The concentration was 1.0 mL / h, the injection speed of the PVP shell solution was 2.4 mL / h, the rotation speed of the drum collector was 120 r / min, +13 kV voltage was applied to the positive electrode of the electrospinning machine, -2 kV voltage was applied to the negative electrode, the electrospinning temperature was 30 ° C, the ambient humidity was 40-50%, and then electrospinning was started, and Taylor cone-shaped micro-jets could be observed under direct light. After the jet was stable, the direct light was turned off, and electrospinning was performed for 2 hours to obtain PVP / BTO@PDMS fiber film. S6: After peeling the PVP / BTO@PDMS fiber film obtained in S5 from the aluminum foil, it is placed in an oven and baked at 110°C for 12 hours to ensure that the polydimethylsiloxane can be fully cross-linked and cured. The cured PVP / BTO@PDMS fiber film is then washed with anhydrous ethanol for multiple times until the PVP shell layer is removed to obtain a BTO@PDMS fiber film.
[0028] The PVP / BTO@PDMS fiber film and BTO@PDMS fiber film prepared by the above steps were tested for performance respectively: 1. The surface morphology of the prepared PVP / BTO@PDMS fiber film was tested using a scanning electron microscope (SEM). The results are as follows: Figure 1 As shown, it was found that PVP / BTO@PDMS fibers were evenly distributed and exhibited a 3D network structure; 2. The surface morphology of the prepared BTO@PDMS fiber film was tested using a scanning electron microscope (SEM). Figure 2 As shown, it was found that the BTO@PDMS fibers were denser and exhibited a 3D network structure; 3. The PVP / BTO@PDMS fiber film and BTO@PDMS fiber film were tested by FTIR infrared spectroscopy. The results are as follows Figure 3 As shown in the figure, it can be seen that the PVP / BTO@PDMS fiber film has a -1 and 1652cm -1Characteristic vibration peaks appear at 2 The OH stretching and C=O stretching vibrations occurred, and the BTO@PDMS fiber film obtained after washing with anhydrous ethanol had a wavelength of 3410 cm -1 and 1652cm -1 The peak disappeared, and the PDMS absorption peak was strengthened, indicating that the PVP shell layer was completely removed; 4. Cut five pieces of 2cm×2cm BTO@PDMS fiber films, place them on the quasi-static instrument, select five points for testing, record the test data, and then take the average value to obtain the piezoelectric constant D 33 The value of Figure 4 As shown in the figure, it can be seen that the D of the BTO@PDMS fiber film prepared by coaxial electrospinning 33 The value is maintained at 5~6pC / N; 5. Cut a 1cm×1cm piece of BTO@PDMS fiber film for piezoelectric force microscopy (PFM) test. Use the conductive probe of the atomic force microscope to detect the electrostatic variables of the BTO@PDMS fiber film under an applied excitation voltage. The results are as follows: Figure 5 As shown in the figure, the piezoelectric response amplitude of BTO@PDMS fiber film presents a typical butterfly-shaped curve in the range of -6V~6V. This result once again verifies that BTO@PDMS fiber film has piezoelectric properties and is expected to be widely used in piezoelectric flexible sensors, tactile sensors and other fields.
[0029] Examples 3 to 6 are methods for preparing a BTO@PDMS fiber film disclosed in the present invention. The difference from Example 2 is that in S1, the amount of tetragonal barium titanate nanoparticles is controlled to be 10 g, 12 g, 18 g, and 20 g, respectively.
[0030] By comparing Example 2 and Examples 3 to 6, as the amount of tetragonal barium titanate nanoparticles increases, the surface hydroxylation effect is limited, and the van der Waals force between the barium titanate nanoparticles increases, resulting in an enhanced attraction between the particles and agglomeration.
[0031] Examples 7 to 10: In S2, a method for preparing a BTO@PDMS fiber film disclosed in the present invention is different from Example 2 in that the amount of hydroxylated barium titanate nanoparticles is controlled to be 2.0, 2.3, 2.8, and 3.0 g, respectively, and the amount of vinyl silane coupling agent is controlled to be 1.5, 1.8, 2.3, and 2.5 g, respectively.
[0032] By comparing Example 2 and Examples 7 to 10, as the amount of vinyl silane coupling agent KH-171 increases, the modification effect gradually increases, so that the compatibility between barium titanate nanoparticles and polydimethylsiloxane is improved; however, when the amount of coupling agent exceeds 2.5 g, the excessive use of the coupling agent causes part of the coupling agent to fail to fully react with the barium titanate nanoparticles, but instead forms tiny agglomerates in the fiber film, affecting the uniformity and mechanical properties of the fiber.
[0033] Examples 11 to 14 are a method for preparing a BTO@PDMS fiber film disclosed in the present invention. The difference from Example 2 is that in S3, the concentration of the BTO@PDMS core material solution is controlled to be 8, 9, 11, and 12 wt%, respectively; in S4, the concentration of the PVP shell layer solution is controlled to be 12, 14, 16, and 18 wt%.
[0034] By comparing Example 2 and Examples 11 to 14, the tensile fracture rate of the BTO@PDMS fiber film decreases with the increase of the BTO doping amount. The reason for this may be that the modified BTO reacts with a part of the silicon-hydrogen bonds in the PDMS prepolymer, resulting in insufficient silicon-hydrogen bonds for cross-linking reaction after adding the same amount of curing agent. By comparing Example 2 and Examples 11 to 14, as the concentration of the PVP shell layer increases, the uncured BTO@PDMS core material solution is effectively coated under the drive of the PVP spinning Taylor cone, and BTO@PDMS fibers with uniform diameters are obtained after high-temperature curing of the structure in the later stage; In addition, the BTO@PDMS fiber film prepared based on PVP with a molecular weight of 1500 kDa has a good balance between mechanical properties and porosity, while too high or too low molecular weight is not conducive to the comprehensive performance of the BTO@PDMS fiber film.
[0035] Examples 15 to 18: In S5, a method for preparing a BTO@PDMS fiber film disclosed in the present invention is different from Example 2 in that the injection rates of the BTO@PDMS core material solution are 0.8, 0.9, 1.1, and 1.2 mL / h, respectively, and the injection rates of the PVP shell layer solution are 2.0, 2.3, 2.6, and 2.8 mL / h, respectively.
[0036] By comparing Example 2 and Examples 15 to 18, the injection speed of the BTO@PDMS core solution is controlled to be 0.8, 0.9, 1.1, and 1.2 mL / h, respectively. As the injection speed increases, the PVP shell layer cannot form a coating on the core solution, and the core solution may leak, increasing the degree of adhesion between the fibers, resulting in an increase in the Young's modulus of the BTO@PDMS fiber film and a decrease in piezoelectricity.
[0037] By comparing Example 2 and Examples 15 to 18, the injection speed of the PVP shell solution is controlled to be 2.0, 2.3, 2.6, and 2.8 mL / h, respectively. As the injection speed of the PVP shell solution increases, incomplete evaporation of the solvent may occur, and an effective coating cannot be formed on the BTO@PDMS core solution, which has a certain impact on the morphology of the BTO@PDMS fiber film.
[0038] Example 19: A method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 1 in that it includes the following steps: S1: First, 10 g of tetragonal barium titanate nanoparticles were added to 150 mL of 70 wt% hydrogen peroxide, and ultrasonic dispersion was performed for 25 min. Then, a reflux reaction device was built, and the oil bath temperature was controlled to be 100 ° C, the stirring speed was 700 r / min, and the reaction time was 5 h. After the reaction, the mixture was centrifuged and washed twice with anhydrous ethanol, and vacuum dried to obtain surface hydroxylated barium titanate nanoparticles. S2 first added 2.0g of hydroxylated barium titanate nanoparticles obtained in S1 and 1.5g of vinyl silane coupling agent KH-171 into 40mL, 70wt% ethanol solution, and ultrasonically dispersed for 25min. Then, a reflux reaction device was built, and the oil bath temperature was controlled to 70°C, the stirring speed was 700r / min, and the reaction time was 15h. After the reaction, the anhydrous ethanol was centrifuged and washed twice, and vacuum dried to obtain vinyl-modified barium titanate nanoparticles. S3: First, 0.500 g of vinyl-modified barium titanate nanoparticles obtained in S2 and 1.0 mL of n-hexane were added to 4.0 g of polydimethylsiloxane prepolymer, and ultrasonic dispersion was performed for 25 min. Then, 0.40 g of polydimethylsiloxane curing agent and 0.4 mL of tetrahydrofuran were added. Then, a stirring reaction device was built, and the oil bath temperature was controlled to be 30 ° C, the stirring speed was 500 r / min, and the reaction time was 1 h. After the reaction was completed, a 10 wt% BTO@PDMS core material solution was obtained. S4: First, add 1.5 g of 1200 kDa polyvinyl pyrrolidone powder to 15 mL of anhydrous ethanol, then build a stirring and mixing device, and control the oil bath temperature to 60 ° C, the stirring speed to 700 r / min, and the stirring time to 1 h to obtain a PVP shell solution; S5 first uses a 5mL syringe to absorb the 8wt% BTO@PDMS core material solution obtained in S3 and the 12wt% PVP shell solution obtained in S4, and the syringe is equipped with a 15G / 21G coaxial electrospinning needle. Then the syringe is installed on the fixed table of the electrospinning machine. The roller collector end of the electrospinning machine is collected with aluminum foil, and the distance between the coaxial electrospinning needle and the roller collector is controlled to be 15cm. The BTO@PDMS core material solution is injected The speed was 0.8 mL / h, the injection speed of the PVP shell solution was 2.0 mL / h, the rotation speed of the drum collector was 100 r / min, +13 kV voltage was applied to the positive electrode of the electrospinning machine, -2 kV voltage was applied to the negative electrode, the electrospinning temperature was 20 ° C, the ambient humidity was 40%, and then electrospinning began, and Taylor cone-shaped micro-jets could be observed under direct light. After the jet was stable, the direct light was turned off, and electrospinning was performed for 2 hours to obtain PVP / BTO@PDMS fiber film; S6: After peeling the PVP / BTO@PDMS fiber film obtained in S5 from the aluminum foil, it is placed in an oven and baked at 100°C for 10 hours to ensure that the polydimethylsiloxane can be fully cross-linked and cured. The cured PVP / BTO@PDMS fiber film is then washed with anhydrous ethanol for multiple times until the PVP shell layer is removed to obtain a BTO@PDMS fiber film.
[0039] Example 20: A method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 1 in that it includes the following steps: S1: First, add 20g of tetragonal barium titanate nanoparticles into 250mL of 80wt% hydrogen peroxide, and ultrasonically disperse for 35min. Then, build a reflux reaction device, and control the oil bath temperature to 110℃, the stirring speed to 900r / min, and the reaction time to 7h. After the reaction, wash with anhydrous ethanol by centrifugation for 3 times, and vacuum dry to obtain surface hydroxylated barium titanate nanoparticles. S2 first added 3.0g of hydroxylated barium titanate nanoparticles obtained in S1 and 2.5g of vinyl silane coupling agent KH-171 into 80mL, 80wt% ethanol solution, and ultrasonically dispersed for 35min. Then, a reflux reaction device was built, and the oil bath temperature was controlled to 80°C, the stirring speed was 900r / min, and the reaction time was 17h. After the reaction was completed, the anhydrous ethanol was centrifuged and washed 3 times, and vacuum dried to obtain vinyl-modified barium titanate nanoparticles. S3: First, 0.60 g of vinyl-modified barium titanate nanoparticles obtained in S2 and 2.0 mL of n-hexane were added to 6.0 g of polydimethylsiloxane prepolymer, and ultrasonic dispersion was performed for 35 min. Then, 0.60 g of polydimethylsiloxane curing agent and 0.6 mL of tetrahydrofuran were added. Then, a stirring reaction device was built, and the oil bath temperature was controlled to 50 ° C, the stirring speed was 700 r / min, and the reaction time was 2 h. After the reaction was completed, a 10 wt% BTO@PDMS core material solution was obtained; S4: First, add 2.0 g of 1400 kDa polyvinyl pyrrolidone powder to 20 mL of anhydrous ethanol, then build a stirring and mixing device, and control the oil bath temperature to 80 ° C, the stirring speed to 900 r / min, and the stirring time to 3 h to obtain a PVP shell solution; S5 first uses a 5mL syringe to absorb the 12wt% BTO@PDMS core material solution obtained in S3 and the 18wt% PVP shell solution obtained in S4, and the syringe is equipped with a 15G / 21G coaxial electrospinning needle. Then the syringe is installed on the fixed table of the electrospinning machine. The roller collector end of the electrospinning machine is collected with aluminum foil, and the distance between the coaxial electrospinning needle and the roller collector is controlled to be 15cm. The BTO@PDMS core material solution is injected The speed was 1.2 mL / h, the injection speed of the PVP shell solution was 2.8 mL / h, the rotation speed of the drum collector was 150 r / min, +13 kV voltage was applied to the positive electrode of the electrospinning machine, -2 kV voltage was applied to the negative electrode, the electrospinning temperature was 40 ° C, the ambient humidity was 50%, and then electrospinning began, and Taylor cone-shaped micro-jets could be observed under direct light. After the jet was stable, the direct light was turned off, and electrospinning was performed for 3 hours to obtain PVP / BTO@PDMS fiber film; S6: After peeling the PVP / BTO@PDMS fiber film obtained in S5 from the aluminum foil, it is placed in an oven and baked at 120°C for 15 hours to ensure that the polydimethylsiloxane can be fully cross-linked and cured. The cured PVP / BTO@PDMS fiber film is then washed with anhydrous ethanol for multiple times until the PVP shell layer is removed to obtain a BTO@PDMS fiber film.
[0040] Comparative Example 1 is a method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 2 in that, in S1, barium titanate nanowires (BTO Ncs) are used instead of tetragonal barium titanate nanoparticles (BTO NPs).
[0041] Since barium titanate nanowires have a large aspect ratio, they are easily semi-embedded in the PDMS fiber membrane during electrospinning, resulting in uneven morphology of the PDMS fiber membrane and affecting the output of piezoelectric performance.
[0042] Comparative Example 2 is a method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 2 in that, in S2, no vinyl silane coupling agent is used.
[0043] Without the use of vinyl silane coupling agent, the surface hydroxylated barium titanate nanoparticles cannot undergo hydrolysis reaction to graft vinyl groups onto the BTO surface, thus affecting the dispersibility of BTO in PDMS.
[0044] Comparative Example 3 is a method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 2 in that, in S4, polyvinylidene fluoride (PVDF) is used instead of polyvinyl pyrrolidone (PVP).
[0045] PVDF is an excellent piezoelectric polymer. Although using PVDF instead of PVP can improve the piezoelectric properties of fiber films, PVDF has a high Young's modulus, resulting in poor film elongation, which is not conducive to its application in wearable devices and limits its application scenarios.
[0046] Comparative Example 4 is a method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 2 in that, in S5, no PVP shell solution is used.
[0047] Since PDMS is a non-polar polymer, and the PDMS prepolymer and curing agent require high temperature and time to complete cross-linking and curing, electrospinning cannot be performed directly.
[0048] Comparative Example 5 is a method for preparing a BTO@PDMS fiber film disclosed in the present invention, which is different from Example 2 in that, in S6, high-temperature cross-linking and curing is not performed.
[0049] Without high-temperature cross-linking and curing, the uncured core material solution will be dissolved when anhydrous ethanol is used to remove the PVP shell layer, and the BTO@PDMS fiber will not form a film.
[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a BTO@PDMS fiber film, characterized in that: The following steps are included: S1 In hydrogen peroxide, tetragonal barium titanate nanoparticles undergo hydroxylation reaction, and after the reaction, surface hydroxylated barium titanate nanoparticles are obtained by post-treatment; S2: in an ethanol solution, the surface hydroxylated barium titanate nanoparticles obtained in S1 are subjected to surface modification under the action of a vinyl silane coupling agent, and after the modification, the surface hydroxylated barium titanate nanoparticles are subjected to post-treatment to obtain vinyl modified barium titanate nanoparticles; S3: ultrasonically dispersing the polydimethylsiloxane prepolymer and the vinyl-modified barium titanate nanoparticles obtained in S2 in n-hexane, and reacting them in the presence of tetrahydrofuran and a polydimethylsiloxane curing agent to obtain a BTO@PDMS core material solution; S4: mixing anhydrous ethanol and polyvinyl pyrrolidone to obtain a PVP shell solution; S5: coaxially electrospinning the BTO@PDMS core material solution obtained in S3 and the PVP shell solution obtained in S4, and collecting them with aluminum foil to obtain a PVP / BTO@PDMS fiber film; S6: After the PVP / BTO@PDMS fiber film obtained in S5 is peeled off from the aluminum foil, it is subjected to high-temperature cross-linking curing and washed with anhydrous ethanol in sequence to obtain a BTO@PDMS fiber film.
2. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S1, the concentration of hydrogen peroxide is 70-80 wt%, and the dosage ratio of hydrogen peroxide to tetragonal barium titanate nanoparticles is controlled to be 150-250 mL: 10-20 g.
3. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S1, the tetragonal barium titanate nanoparticles are first ultrasonically dispersed in hydrogen peroxide, and the dispersion time is controlled to be 25-35 minutes, and then a hydroxylation reaction occurs, and the reaction temperature is controlled to be 100-110° C., the stirring speed is 700-900 r / min, and the reaction time is 5-7 hours.
4. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S2, the concentration of the ethanol solution is 70-80wt%, and the dosage ratio of the ethanol solution, hydroxylated barium titanate nanoparticles and vinyl silane coupling agent is controlled to be 40-80mL: 2.0-3.0g: 1.5-2.5g.
5. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S2, the hydroxylated barium titanate nanoparticles and the vinyl silane coupling agent are first ultrasonically dispersed in an ethanol solution, and the dispersion time is controlled to be 25-35 minutes, and then the surface modification is carried out, and the reaction temperature is controlled to be 70-80°C, the stirring speed is 700-900 r / min, and the reaction time is 15-17 hours.
6. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In S3, the dosage ratio of polydimethylsiloxane prepolymer, vinyl-modified barium titanate nanoparticles, polydimethylsiloxane curing agent and tetrahydrofuran is controlled to be 4.0-6.0 g: 0.50-0.60 g: 0.40-0.60 g: 0.4-0.6 mL, and the concentration of the BTO@PDMS core material solution is 8-12 wt %.
7. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In S3, the dispersion time is first controlled to be 25-35 min, the reaction temperature is then controlled to be 30-50° C., the stirring speed is 500-700 r / min, and the reaction time is 1-2 h.
8. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S4, the molecular weight of polyvinyl pyrrolidone is 1200-1400 kDa, the dosage ratio of anhydrous ethanol and polyvinyl pyrrolidone is controlled to be 15-20 mL: 1.5-2.0 g, and the concentration of the PVP shell solution is 12-18 wt %.
9. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S5, the distance between the coaxial electrospinning needle and the roller collector is controlled to be 15 cm, the injection rate of the BTO@PDMS core solution is 0.8~1.2 mL / h, the injection rate of the PVP shell solution is 2.0~2.8 mL / h, the rotation speed of the roller collector is 100~150 r / min, the positive electrode of the electrospinning machine is applied with a voltage of +13 kV, the negative electrode is applied with a voltage of -2 kV, the electrospinning temperature is 20~40°C, and the ambient humidity is 40~50%.
10. The method for preparing a BTO@PDMS fiber film according to claim 1, characterized in that: In the S5, after the electrospinning starts, a Taylor cone-shaped micro jet can be observed under a direct light. After the jet is stabilized, the direct light is turned off and the electrospinning is continued for 2 to 3 hours.
Citation Information
Patent Citations
Composite nano-generator for intelligent monitoring system and preparation method and application of composite nano-generator
CN116330773A
Piezoelectric nano generator, preparation method thereof and wireless sensing system
CN117161378A
Piezoelectric composite film and preparation method and application thereof
CN117279475A
Cited By
Self-adhesion one-way water guide silica gel fiber membrane as well as preparation method and application thereof
CN119553428A
A self-adhesive unidirectional hydrophobic silica fiber membrane, its preparation method and application