Wafer support boat, horizontal heat treatment furnace, wafer heat treatment method, and bonded wafer manufacturing method

The combination of a silicon carbide housing and quartz support section in the wafer support boat addresses oxide film adhesion and chipping issues, enhancing the quality of bonded wafers by reducing defects.

JP7567761B2Active Publication Date: 2024-10-16SUMCO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021198816
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-07
Publication Date
2024-10-16
Estimated Expiration
2041-12-07

AI Technical Summary

Technical Problem

Conventional wafer support boats made of silicon carbide suffer from issues such as oxide film adhesion, chipping, and defects during heat treatment processes, leading to poor bonding and increased defect rates, particularly in the formation of thick BOX layers.

Method used

A wafer support boat design with a silicon carbide housing and a quartz support section, featuring protrusions and a detachable configuration, which prevents oxide film adhesion and supports wafers effectively, reducing defects.

Benefits of technology

The design suppresses oxide film adhesion and chipping, minimizing defects like scratches, chips, and bonding failures, thereby improving the quality of bonded wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567761000001
    Figure 0007567761000001
  • Figure 0007567761000002
    Figure 0007567761000002
  • Figure 0007567761000003
    Figure 0007567761000003
Patent Text Reader

Abstract

To provide a wafer support boat capable of suppressing generation of various defects, a horizontal heat treatment furnace with the wafer support boat, a heat treatment method for a wafer using the water support boat, and a manufacturing method of a bonded wafer.SOLUTION: A wafer support boat is a wafer support boat for horizontal heat treatment furnace, a storage unit consists of silicon carbide, and a support unit consists of quartz. A horizontal heat treatment furnace comprises the wafer support boat. A heat treatment method for a wafer includes a heat treatment step of performing heat treatment using the wafer support boat. A manufacturing method of a bonded wafer includes a heat treatment step according to the heat treatment method for the wafer.SELECTED DRAWING: Figure 3A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wafer support boat for a horizontal heat treatment furnace, a horizontal heat treatment furnace equipped with the wafer support boat, a wafer heat treatment method using the wafer support boat, and a method for manufacturing bonded wafers. [Background technology]

[0002] Conventionally, a method of performing heat treatment on wafers using a horizontal heat treatment furnace equipped with a furnace core tube extending horizontally inside the furnace body and a wafer support boat on which multiple wafers can be placed horizontally has been known (for example, Patent Document 1).

[0003] Here, an SOI (Silicon on Insulator) wafer has a structure in which an insulating film such as silicon oxide (SiO2) and a single crystal silicon layer used as a device active layer are sequentially formed on a support substrate wafer. One of the representative manufacturing methods of an SOI wafer is a bonding method. In the bonding method, an oxide film is formed as a BOX (Buried Oxide) layer on at least one of the support substrate wafer and the active layer wafer, and then the support substrate wafer and the active layer wafer are bonded together via the oxide film to form a bonded wafer. Then, the bonded wafer is subjected to a heat treatment to strengthen the bond between the support substrate wafer and the active layer wafer, thereby manufacturing an SOI wafer.

[0004] Fig. 1A is a schematic front view of a conventional wafer support boat, and Fig. 1B is a schematic side view of the conventional wafer support boat. Among all the processes, the processes for performing heat treatment include a BOX (Buried Oxide) oxide film heat treatment process and a post-bonding heat treatment process performed after bonding. First, an active layer wafer and a support substrate wafer are prepared. Next, a BOX heat treatment process is performed to form an oxide film on the active layer wafer. In the BOX heat treatment process, as shown in Figures 1A and 1B, a wafer support boat on which active layer silicon wafers are placed is placed into a heat treatment furnace, and the active layer wafer is heat treated in an oxidizing atmosphere to form an oxide film on the active layer wafer.

[0005] Here, the wafer support boat used has multiple wafers aligned at equal intervals in the horizontal direction, and each wafer stands vertically (for example, Patent Document 2). As shown in Figures 1A and 1B, multiple wafer grooves 92 are provided at equal intervals in the horizontal direction in the wafer support boat 91. Although only one wafer W is shown in Figures 1A and 1B for simplification, multiple wafers W are actually placed in each of the multiple wafer grooves 92.

[0006] Next, the active layer wafer and the support substrate wafer are bonded together via the BOX layer. The active layer wafer and the support substrate wafer are bonded together with their notches aligned so that no air or foreign matter gets into the bonding interface between the active layer wafer and the support substrate wafer.

[0007] Next, in order to increase the bonding strength, a post-bonding heat treatment is performed. In this heat treatment, the wafer W, which is a bonded wafer of the active layer wafer and the support substrate wafer, is set upright in the wafer groove 92 of the wafer support boat 91, and the wafer support boat 91 is put into a heat treatment furnace and heat treated in an oxidizing atmosphere. Thereafter, the wafer support boat 91 is removed from the heat treatment furnace, and then the wafer W is removed from the wafer support boat 91.

[0008] Thereafter, the active layer wafer is subjected to processes such as chamfering, etching, grinding, and polishing until the active layer wafer has a predetermined thickness, thereby producing a bonded SOI wafer. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent Publication No. 2021-089993 [Patent Document 2] JP 2002-299423 A Summary of the Invention [Problem to be solved by the invention]

[0010] Conventionally, wafer support boats are often entirely made of silicon carbide (SiC). The reason for this is that in the BOX heat treatment process for forming the BOX layer, it is preferable to use a material that is resistant to thermal deformation and has heat resistance, taking into account the heat treatment temperature and time typically used. Also, in the post-bonding heat treatment process, high temperature and long-term heat treatment are required, and the wafer support port needs to support two bonded wafers with the same weight, so heat resistance and load resistance are required. As a material that has these properties, silicon carbide has often been used as the material for wafer support boats.

[0011] However, performing heat treatment using a silicon carbide wafer support boat has the following problems: Figures 2A to 2D are diagrams for explaining the BOX heat treatment and bonding using a conventional wafer support boat. In the BOX oxidation process, an oxide film Wa formed on the surface of a silicon wafer W by heat treatment and an oxide film 91a formed on the surface of a silicon carbide wafer support boat 91 may adhere to each other (FIG. 2A). At this time, when the silicon wafer W is removed from the silicon carbide wafer support boat 91, a part of the oxide film may be chipped due to adhesion of the wafer end surface to the silicon carbide wafer boat 91, generating silicon chips Wb (FIG. 2B). In addition, the chipped silicon chips Wb may remain in the wafer grooves 92 of the wafer support boat 91, and the next batch of wafers W to be subjected to heat treatment is placed on the silicon chips remaining in the wafer grooves 92 and heat-treated, which makes it easy for defects to occur on the wafer end surface. In addition, the silicon chips may adhere to the wafer surface (FIG. 2C), which makes it easy for bright spot defects to occur. In particular, the thicker the BOX film formed, the more likely the above phenomenon is to occur, and the higher the starting point defect rate and the higher the chip defect rate on the end surface tend to be.

[0012] In addition, even in the heat treatment process after bonding, chipping may occur in the end faces of the active layer wafer and the support substrate wafer at the bonding portion with the wafer support board. Furthermore, if the post-process etching is performed in a state where the oxide on the end faces is chipped, pits will occur on the end faces of the silicon wafer, resulting in defects.

[0013] Furthermore, in the bonding process, silicon pieces that adhered to the wafer surface during the BOX heat treatment could get caught between the wafer and the supporting substrate wafer, causing bonding defects when the silicon pieces got caught at the interface between the two wafers (Fig. 2D). In addition, silicon pieces getting caught at the wafer interface can also lead to defects such as air getting into the wafer interface. In the bonding process and heat treatment after bonding, the above phenomenon was more likely to occur and the defect rate was also higher, especially as the film thickness of the BOX increased.

[0014] In view of the above problems, an object of the present invention is to provide a wafer support boat, a horizontal heat treatment furnace having the wafer support boat, a wafer heat treatment method using the wafer support boat, and a bonded wafer manufacturing method, which are capable of suppressing the occurrence of the various defects described above. [Means for solving the problem]

[0015] The gist and configuration of the present invention are as follows. (1) A wafer support boat for a horizontal heat treatment furnace, comprising: the wafer support boat includes a container portion for accommodating wafers, and a support portion disposed at a bottom of the container portion for supporting the wafers; The support has a support body extending along a direction in which the wafers are arranged, and a plurality of protruding parts protruding upward from the support body and arranged along the direction in which the support body extends, and a wafer groove in which the wafer is placed is defined and formed between two adjacent protruding parts; The housing portion is made of silicon carbide, 4. A wafer support boat, wherein the support portion is made of quartz.

[0016] (2) The wafer support boat according to (1) above, wherein the support body has a thickness of 2 to 30 mm.

[0017] (3) The wafer support boat according to (1) or (2) above, wherein the bottom of the accommodation section is configured to support the support section body by surface support.

[0018] (4) The wafer support boat according to (1) or (2) above, wherein the bottom of the accommodation section is configured to support the support section body by point support at a plurality of locations.

[0019] (5) The wafer support boat according to any one of (1) to (4) above, wherein the support portion is detachably attached to the container portion.

[0020] (6) A horizontal heat treatment furnace equipped with the wafer support boat according to any one of (1) to (5) above.

[0021] (7) A method for heat treating a wafer, comprising a heat treatment step of performing a heat treatment using the wafer support boat according to any one of (1) to (5) above.

[0022] (8) A method for producing a bonded wafer, comprising a heat treatment step using the wafer heat treatment method according to (7) above.

[0023] (9) The method for producing a bonded wafer according to the above (7), wherein at least one of a BOX heat treatment step and a post-bonding heat treatment step is performed as the heat treatment step. Effect of the Invention

[0024] According to the present invention, it is possible to provide a wafer support boat, a horizontal heat treatment furnace having the wafer support boat, a wafer heat treatment method using the wafer support boat, and a bonded wafer manufacturing method, which are capable of suppressing the occurrence of the various defects described above. [Brief description of the drawings]

[0025] [Figure 1A] FIG. 1 is a schematic front view of a conventional wafer support boat. [Figure 1B] FIG. 1 is a schematic side view of a conventional wafer support boat. [Figure 2A] 1A and 1B are diagrams for explaining a BOX heat treatment and bonding using a conventional wafer support boat. [Figure 2B] 1A and 1B are diagrams for explaining a BOX heat treatment and bonding using a conventional wafer support boat. [Figure 2C] 1A and 1B are diagrams for explaining a BOX heat treatment and bonding using a conventional wafer support boat. [Figure 2D] 1A and 1B are diagrams for explaining a BOX heat treatment and bonding using a conventional wafer support boat. [Figure 3A] 1 is a schematic front view of a wafer support boat according to an embodiment of the present invention, on which one wafer is placed. [Figure 3B] FIG. 2 is a schematic side view of a wafer support boat with one wafer placed thereon according to one embodiment of the present invention. [Figure 3C] FIG. 2 is a schematic top view of a wafer support boat according to an embodiment of the present invention. [Figure 4A] FIG. 1 is a schematic diagram showing the state of a conventional silicon carbide wafer support boat before heat treatment. [Figure 4B] FIG. 1 is a diagram showing a schematic view of a conventional silicon carbide wafer support boat after heat treatment. [Figure 5A] FIG. 13 is a diagram showing a schematic view of a wafer support made of quartz before heat treatment. [Figure 5B] 13 is a diagram showing a schematic view of a state after heat treatment in the case where quartz is used for the wafer support portion. FIG. [Figure 6A] FIG. 13 is a schematic top view of a modified example of a wafer support boat according to an embodiment of the present invention, on which one wafer is placed. [Figure 6B] FIG. 13 is a schematic side view of a modified example of the wafer support boat according to the embodiment of the present invention. [Figure 7] 13A and 13B are diagrams for explaining a thickness of a support main body. [Figure 8A] 13A and 13B are views showing surface support of the support body by the bottom of the storage section. [Figure 8B] 13A and 13B are diagrams showing point support of the support body by the bottom of the storage section. [Figure 9] 1 is a cross-sectional view of a horizontal heat treatment furnace according to an embodiment of the present invention. [Figure 10A] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10B] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10C] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10D] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10E] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10F] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10G] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 10H] 1A to 1C are diagrams showing steps of a method for manufacturing a bonded wafer according to an embodiment of the present invention. [Figure 11A] FIG. 13 is a diagram showing the results of quality evaluation of a wafer end face in a comparative example. [Figure 11B] FIG. 13 is a diagram showing the results of quality evaluation of the wafer end face of an example of the present invention. [Figure 12A] FIG. 13 is a diagram showing the results of bright spot observation on the wafer surface of a comparative example. [Figure 12B] FIG. 13 is a diagram showing the results of observing bright spots on the surface of a wafer according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.

[0027] (wafer support boat) 3A is a schematic front view of a wafer support boat according to an embodiment of the present invention with one wafer placed thereon, FIG. 3B is a schematic side view of a wafer support boat according to an embodiment of the present invention with one wafer placed thereon, and FIG. 3C is a schematic top view of a wafer support boat according to an embodiment of the present invention.

[0028] The wafer support boat 1 of this embodiment is a wafer support boat for a horizontal heat treatment furnace, and is configured to align multiple wafers W (in this example, silicon wafers) in one horizontal direction so that the multiple wafers W can be heat-treated simultaneously.

[0029] As shown in FIGS. 3A to 3C, the wafer support boat 1 has a storage section 2 and a support section 3. The storage section 2 and support section 3 are arranged in a row direction.

[0030] In the following description, the direction perpendicular to the paper surface in FIG. 3A is the front-rear direction, the left-right direction on the paper surface is the horizontal direction, and the up-down direction on the paper surface is the vertical direction. The storage section 2 has a bottom 21, a side section 22 connected to the bottom section 21 and extending vertically upward, and an upper section 23 connected to the side section 22 and extending laterally.

[0031] In the illustrated example, the bottom portion 21 is a single plate-like member extending in the horizontal direction. Also, the side portion 22 is made up of two plate-like members having a substantially U-shape as shown in FIG. 3B. The upper portion 23 is connected to the upper end of the side portion 22 and is made up of two plate-like members extending in the horizontal direction. The upper portion 23 is provided with a plurality of wafer grooves 231 into which the wafers W are inserted, and the plurality of wafer grooves 231 are aligned in the horizontal direction.

[0032] Next, the support part 3 is disposed on the upper surface of the bottom part 21 of the storage part 2, and is configured to support a wafer. The support part 3 is attached to the storage part 2 in a detachable manner. The support 3 has a support body 31 extending along the direction in which the wafers are lined up (the horizontal direction in FIG. 3A), and a plurality of protrusions 32 protruding upward from the support body 31 and lined up along the direction in which the support body 31 extends. A wafer groove 33 in which the wafer W is placed is defined between two adjacent protrusions 32. In the illustrated example, a plurality of wafer grooves 33 are arranged in the horizontal direction. The protrusions 32 are configured to be able to support the lower side surface of the wafer W.

[0033] In this embodiment, the housing portion 21 is made entirely of silicon carbide, and the support portion 3 is made of quartz. The functions and effects of the wafer support boat of this embodiment will be described below. Fig. 4A is a diagram showing a typical state before heat treatment in the case of a conventional silicon carbide wafer support boat. Fig. 4B is a diagram showing a typical state after heat treatment in the case of a conventional silicon carbide wafer support boat. Fig. 5A is a diagram showing a typical state before heat treatment in the case of using quartz for the wafer support portion. Fig. 5B is a diagram showing a typical state after heat treatment in the case of using quartz for the wafer support portion.

[0034] When a silicon wafer is heat-treated in an oxygen atmosphere, the Si on the surface of the silicon wafer reacts with the O2 in the atmosphere to form an oxide film. Furthermore, O2 diffuses into the oxide film grown on the silicon surface and reacts with the Si at the oxide film-silicon interface to form an additional oxide film (SiO2). As shown in Figures 4A and 4B, when the support (support body 131 and protruding portion 132) is a silicon carbide member, Si on the surface of the silicon carbide member reacts with O2 in the atmosphere to form a thermal oxide film. Furthermore, O2 diffuses into the oxide film grown on the silicon surface and reacts with Si at the oxide film and silicon carbide interface to further form an oxide film (SiO2) as indicated by the diagonal lines in Figure 4B. For this reason, in a silicon carbide wafer support boat, in the portion where the silicon carbide member and the silicon wafer come into contact with each other, the oxide film on the wafer side and the oxide film on the wafer support boat side are bonded to each other as the oxide film growth on both sides progresses. On the other hand, as shown in Figures 5A and 5B, when the support (support body 31 and protrusion 32) is made of quartz (SiO2), the SiO2 member does not have Si to bond with even if O2 diffuses into the SiO2, so SiO2 is not formed on the surface. For this reason, in the case of a quartz wafer support boat, the oxide film grows on the wafer side and an oxide film (SiO2) is formed as shown by the diagonal lines in Figure 5B, but since no oxide film is formed on the wafer support boat side, bonding of the oxide film does not occur.

[0035] In this embodiment, first, since the accommodation portion 2 is made of silicon carbide, the wafer support boat 1 as a whole has excellent heat resistance and load resistance. On the other hand, since the support portion 3 that supports the load of the silicon wafer W is made of quartz, as described above, it is possible to suppress adhesion due to oxidation between the silicon wafer W and the wafer support boat 1. Even if a high-temperature and long-time heat treatment (for example, an oxidation treatment with an oxide film thickness of 1 μm or more) is performed in the BOX heat treatment process, the post-bonding heat treatment process, or the like, it is possible to suppress adhesion due to oxidation between the silicon wafer W and the wafer support boat 1. Therefore, even when the silicon wafers W are removed from the silicon wafer support boat 1 after the oxidation heat treatment, the occurrence of scratches or chips on the end faces of the silicon wafers W can be suppressed, and the adhesion of silicon chips Wb, oxides, and the like to the surfaces of the silicon wafers W can also be suppressed. This makes it possible to suppress the occurrence of scratches and chips on the end face of the silicon wafer W (or bonded wafer) and to suppress the occurrence of defects such as pits. It is also possible to suppress bonding defects caused by silicon pieces being caught at the wafer interface during wafer bonding. In this manner, the wafer support boat 1 of the present embodiment can suppress the occurrence of the various defects described above.

[0036] 6A and 6B are schematic top and side views of a modified example of a wafer support boat according to an embodiment of the present invention, in which one wafer is placed. 3A and 3B, the wafer W is supported by the protruding parts 32 aligned in a row, but the wafer W can be supported at multiple points by the protruding parts aligned in multiple rows. For example, as shown in Figures 6A and 6B, the wafer W can be supported at two points by the protruding parts aligned in two rows.

[0037] 7 is a diagram for explaining the thickness of the support body. The thickness t of the support body 31 is preferably 2 to 30 mm. By setting the thickness t to 2 mm or more, it is possible to form a wafer groove while maintaining the strength of the support. On the other hand, since quartz has a larger specific heat than silicon, by setting the thickness t to 30 mm or less, it is possible to suppress slip defects caused by the temperature difference generated between the wafer and the support during the heat treatment process.

[0038] Fig. 8A is a diagram showing surface support of the support body by the bottom of the storage unit. Fig. 8B is a diagram showing point support of the support body by the bottom of the storage unit. The bottom 21 of the storage unit 2 is preferably configured to support the support body 31 by surface support or point support at multiple points. 8A, the upper surface of the bottom 21 of the accommodation unit 2 and the lower surface of the support body 31 are in surface contact with each other, whereby the support body 31 is surface-supported by the bottom 21 of the accommodation unit 2. Such surface support makes it possible to stably support the wafer. 8B, a plurality of protrusions 211 are provided at equal intervals in the horizontal direction (the lateral direction in the figure) on the upper surface of the bottom 21 of the accommodation unit 2 in this example, the plurality of protrusions 211 are the same height, and the support body 31 is placed on the plurality of protrusions 211. In this way, the support body 31 is point-supported by the bottom 21 of the accommodation unit 2. Such point support reduces the thermal conduction from the bottom 21 of the accommodation unit 2 to the support body 31, suppresses a sudden temperature change from the accommodation unit 2 to the support 3, and suppresses the occurrence of slip defects caused by the temperature difference between the silicon wafer W and the support 3.

[0039] When the wafer is a silicon wafer, the support is made of quartz, and it is more preferable to use quartz glass since the higher the purity, the more effectively the above-mentioned effects can be obtained. On the other hand, if the wafer is not a silicon wafer, a different material can be used, for example, if the wafer is an alumina wafer, alumina (Al2O3) can be used as the support.

[0040] (Horizontal heat treatment furnace) Next, a horizontal heat treatment furnace according to one embodiment of the present invention will be described below. Fig. 9 is a cross-sectional view of the horizontal heat treatment furnace according to one embodiment of the present invention.

[0041] 9, this horizontal heat treatment furnace 100 includes a furnace core tube 102 extending horizontally inside a furnace body 101. The furnace core tube 102 is provided with an opening 103 and a door 104 for opening and closing the opening at one end, and a gas introduction pipe 105 at the other end. The horizontal heat treatment furnace 100 also includes a wafer support boat 1, which is shown simply in FIG. 9 but is the same as that described in the above embodiment of the wafer support boat. When silicon wafers W are to be heat-treated, the silicon wafers W are placed on the wafer support boat 1, inserted through the opening 103 of the furnace core tube 102 and set in the center. The door 104 is then closed to approximately seal the furnace, and a high-purity gas such as nitrogen, oxygen, argon, or the like is then fed through the gas inlet tube 105 and exhausted to the outside of the furnace through the gap between the opening 103 and the door 104. As an example, the horizontal heat treatment furnace 100 can be used for a BOX heat treatment process and a post-bonding heat treatment process in the manufacture of bonded SOI wafers, but is not limited to these heat treatments.

[0042] According to the horizontal heat treatment furnace 100 of the present embodiment, since the wafer support boat 1 of the above embodiment is used, it is possible to suppress the occurrence of the above-mentioned various defects for the same reasons as those described in the embodiment of the wafer support boat 1.

[0043] (Wafer Heat Treatment Method) A wafer heat treatment method according to one embodiment of the present invention includes a heat treatment step of performing heat treatment using the wafer support boat of the above embodiment. Examples of such a heat treatment step include, but are not limited to, a BOX heat treatment step and a post-bonding heat treatment step in the manufacture of a bonded SOI wafer. According to the wafer heat treatment method of the present embodiment, the wafer support boat of the above embodiment is used, and therefore, for the same reasons as those described in the embodiment of the wafer support boat, the occurrence of the above-mentioned various defects can be suppressed.

[0044] (Manufacturing method of bonded wafers) 10A to 10H are diagrams showing the steps of a method for producing a bonded wafer according to one embodiment of the present invention. As shown in FIG. 10, first, a wafer for an active layer and a wafer for a support substrate are prepared (FIG. 10A).

[0045] Next, a BOX heat treatment process is performed to form an oxide film on the active layer wafer (FIG. 10B). The BOX heat treatment process is an oxidation heat treatment process to form a BOX on the active layer wafer, which is performed before bonding the active layer wafer and the support substrate wafer. Specifically, silicon wafers are placed on a wafer support boat, which is then put into a heat treatment furnace and heat treated in an oxidizing atmosphere to form an oxide film on the silicon wafer. The oxide film is indicated by diagonal lines (same below).

[0046] Next, the active layer wafer with the BOX formed therein is bonded to the support substrate wafer (FIG. 10C). The active layer wafer and the support substrate wafer are bonded together with their notches aligned, so that no air or foreign matter gets into the bonding interface between the active layer wafer and the support substrate wafer.

[0047] Next, to increase the bonding strength, a post-bonding heat treatment is performed (FIG. 10D). The post-bonding heat treatment is an oxidation heat treatment process performed after bonding the active layer wafer and the support substrate wafer to strengthen the bond between the active layer wafer and the support substrate wafer. In this heat treatment, the wafer W, which is a bonded wafer of the active layer wafer and the support substrate wafer, is placed in the wafer groove of a wafer support boat and then placed in a heat treatment furnace together with the wafer support boat, where the heat treatment is performed in an oxidation atmosphere. The wafer support boat is then removed from the heat treatment furnace, and the wafer W is then removed from the wafer support boat. Thereafter, the active layer wafer is subjected to chamfering (FIG. 10E), etching (FIG. 10F), grinding (FIG. 10G), and polishing (FIG. 10H) processes until the active layer wafer has a predetermined thickness, thereby producing a bonded SOI wafer.

[0048] Here, the method for producing a bonded wafer according to one embodiment of the present invention includes a heat treatment step of performing a heat treatment using the wafer support boat of the above embodiment. The heat treatment step is at least one of a BOX heat treatment step for forming a BOX for an active layer wafer and a post-bonding heat treatment step for a bonded wafer.

[0049] According to the manufacturing method for a bonded wafer of the present embodiment, the wafer support boat of the above embodiment is used, and therefore, for the same reasons as those described in the embodiment of the wafer support boat, the occurrence of the above-mentioned various defects can be suppressed.

[0050] Examples of the present invention will be described below, but the present invention is not limited to the following examples in any way. EXAMPLES

[0051] As an example of the invention, a wafer support boat was produced in which the container portion was made of silicon carbide and the support portion was made of quartz glass, as shown in Figures 3A to 3C. As a comparative example, a wafer support boat entirely made of silicon carbide was prepared. A plurality of silicon wafers were placed in the plurality of wafer grooves of these wafer support boats, and a BOX heat treatment process was carried out at a heat treatment temperature of 1150° C. for 10 hours with an oxide film thickness of 2.5 μm, and quality evaluation was performed.

[0052] Fig. 11A is a diagram showing the results of quality evaluation of the wafer end face of the comparative example. Fig. 11B is a diagram showing the results of quality evaluation of the wafer end face of the inventive example. In the comparative example, scratches and chips were observed on the wafer end face. On the other hand, no scratches or chips were observed in the inventive example. Fig. 12A is a diagram showing the results of observing bright spots on the wafer surface of a comparative example. Fig. 12B is a diagram showing the results of observing bright spots on the wafer surface of an inventive example. In the comparative example, bright spots were confirmed at the edge when checking the vicinity of the wafer support part. On the other hand, in the inventive example, no bright spots were confirmed at the edge near the wafer support part. [Explanation of symbols]

[0053] 1: wafer support boat, 2: Storage section, 21: Bottom, 22: Side, 23: Upper part, 231: wafer groove, 3: Support part, 31: Support body, 32:Protrusion, 33: wafer groove, 100: Horizontal heat treatment furnace, W: Wafer

Claims

1. A wafer support boat for a horizontal heat treatment furnace, comprising: The wafer support boat includes a container having a bottom, a side portion connected to the bottom and extending vertically upward, and a top portion connected to the side portion and extending laterally, and a support portion disposed at the bottom of the container for supporting the wafers, The support portion has a support portion main body extending along a direction in which the wafers are arranged, and a plurality of protruding portions protruding upward from the support portion main body and arranged along the direction in which the support portion main body extends, and a wafer groove in which the wafer is placed is defined and formed between two adjacent protruding portions; The housing portion is made entirely of silicon carbide, 4. A wafer support boat, wherein the support portion is made of quartz.

2. 2. The wafer support boat according to claim 1, wherein the support body has a thickness of 2 to 30 mm.

3. The wafer support boat according to claim 1 , wherein the bottom of the container is configured to support the support body by surface support.

4. 3. The wafer support boat according to claim 1, wherein the bottom of the container is configured to support the support body by point support at a plurality of locations.

5. 5. The wafer support boat according to claim 1, wherein the support portion is detachably attached to the container portion.

6. A horizontal heat treatment furnace comprising the wafer support boat according to any one of claims 1 to 5.

7. A method for heat treating a wafer, comprising a heat treatment step of performing a heat treatment using the wafer support boat according to any one of claims 1 to 5.

8. A method for producing a bonded wafer, comprising a heat treatment step using the wafer heat treatment method according to claim 7.

9. 8. The method for producing a bonded wafer according to claim 7, wherein at least one of a BOX heat treatment step and a post-bonding heat treatment step is performed as the heat treatment step.

Citation Information

Patent Citations

  • Boat for semiconductor wafer

    JP1985022314A

  • Thermal treatment method of semiconductor wafer

    JP1993160053A

  • Boat for lateral heat-treatment oven and heat- treatment method

    JP2002299423A

  • Method for heat treating semiconductor wafer and horizontal heat treatment furnace

    JP2003100647A

  • Boat for heat treatment and wafer heat treatment method

    JP2009111271A