Acrylic rubber sheet with excellent storage stability and processability
By controlling molecular weight distribution and using specific anti-aging agents, the acrylic rubber sheet achieves enhanced storage stability and processability, addressing the limitations of existing acrylic rubber sheets in harsh environments.
Patent Information
- Application Number
- JP2021534584
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-19
- Filing Date
- 2020-06-05
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-05
AI Technical Summary
Acrylic rubber sheets face challenges with poor storage stability and processability, particularly under harsh environments, due to issues with gel formation and loss of reactive groups during polymerization, which affect mechanical strength and handling.
The development of an acrylic rubber sheet with controlled molecular weight distribution, specific anti-aging agents, and optimized manufacturing processes, including emulsion polymerization and extrusion techniques, to enhance storage stability and processability without compromising strength.
The resulting acrylic rubber sheet exhibits improved storage stability and processability, with reduced gel content and enhanced mechanical properties, suitable for applications requiring balanced performance in harsh conditions.
Smart Images

Figure 0007567792000005 
Figure 0007567792000006 
Figure 0007567792000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an acrylic rubber sheet having excellent storage stability and processability and a manufacturing method thereof, an acrylic rubber veil formed by laminating said acrylic rubber sheets, a rubber mixture formed by mixing said acrylic rubber sheets or acrylic rubber veils and a manufacturing method thereof, and a cross-linked rubber product formed by cross-linking the rubber mixture. [Background technology]
[0002] Acrylic rubber is a polymer whose main component is acrylic ester, and is generally known as a rubber having excellent heat resistance, oil resistance, and ozone resistance. It is widely used in fields such as automobiles, and is used with the addition of antioxidants as necessary.
[0003] For example, in Patent Document 1 (International Publication No. WO 2018 / 139466), a monomer component including ethyl acrylate, n-butyl acrylate, monobutyl fumarate, etc. is stirred with pure water, sodium lauryl sulfate, and polyoxyethylene dodecyl ether to obtain a monomer emulsion, and an aqueous solution of ferrous sulfate, sodium ascorbate, and potassium persulfate is continuously dropped over a period of 3 hours to obtain an emulsion polymerization liquid in which a polymerization conversion rate reaches 95%, and a 50% by weight aqueous dispersion of 3-(3,5-tert-butyl-4-hydroxyphenyl)stearyl propionate (50 parts of an aqueous solution of 0.2% by weight sodium lauryl sulfate and 50 parts of (3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate is added to the emulsion polymerization liquid. The method disclosed is to add 50 parts by weight of 2,4-bis[(octylthio)methyl]-6-methylphenol to 50 parts by weight of an aqueous solution of 0.2% by weight of sodium lauryl sulfate, and then heat the mixture to 85° C., coagulate with sodium sulfate to generate hydrous crumbs, wash the generated hydrous crumbs four times with industrial water, wash once with an acid of pH 3, and wash once with pure water, and then dry them in a hot air dryer at 160° C. for 10 minutes, thereby suppressing contamination of the polymerization apparatus during polymerization and producing crumb-like acrylic rubber having excellent initial mechanical strength. It is also disclosed that this method allows the hydrous crumbs washed in a screw-type extrusion dryer to be dried at 150° C. or higher. However, in addition to heat resistance, processability and storage stability under severe environments are also required.
[0004] Regarding the gel content of acrylic rubber, for example, Patent Document 2 (JP Patent No. 3599962) discloses an acrylic rubber having an acetone insoluble gel fraction of 5% by weight or less obtained by copolymerizing 95-99.9% by weight of alkyl acrylate or alkoxyalkyl acrylate with 0.1-5% by weight of a polymerizable monomer having two or more radically reactive unsaturated groups with different reactivity in the presence of a radical polymerization initiator, a reinforcing filler, and an acrylic rubber composition having excellent extrusion processability such as extrusion speed, die swell, and surface texture, which is composed of an organic peroxide-based vulcanizing agent. The acrylic rubber used here with a very small gel fraction is obtained by adjusting the polymerization solution to pH 6-8 with sodium bicarbonate or the like, as opposed to an acrylic rubber with a high gel fraction (60%) obtained in a normal acidic range (pH 4 before polymerization, pH 3.4 after polymerization). Specifically, water, sodium lauryl sulfate and polyoxyethylene nonylphenyl ether as emulsifiers, sodium carbonate, and boric acid were charged and adjusted to 75°C, then t-butyl hydroperoxide, Rongalite, disodium ethylenediaminetetraacetate, and ferrous sulfate were added (pH 7.1 at this time), and then the monomer components of ethyl acrylate and allyl methacrylate were added dropwise to carry out emulsion polymerization, and the resulting emulsion (pH 7) was salted out using an aqueous sodium sulfate solution, washed with water, and dried to obtain acrylic rubber. However, acrylic rubber, which is mainly composed of (meth)acrylic acid ester, has problems with handling, such as decomposition in the neutral to alkaline range and poor storage stability, and acrylic rubber that was emulsion polymerized at a pH of neutral to alkaline had problems with poor mechanical strength due to loss of reactive groups (crosslinking points) such as carboxyl groups, epoxy groups, and chlorine atoms.
[0005] In addition, Patent Document 3 (International Publication No. WO 2018 / 143101) discloses a technique for improving the extrusion moldability, particularly the discharge amount, discharge length, and surface texture, of a rubber composition containing a reinforcing agent and a crosslinking agent, by emulsion polymerization of a (meth)acrylic acid ester and an ion-crosslinkable monomer, using an acrylic rubber having a complex viscosity at 100 ° C. ([η]100 ° C.) of 3,500 Pa·s or less and a ratio ([η]100 ° C. / [η]60 ° C.) of the complex viscosity at 60 ° C. ([η]60 ° C.) to the complex viscosity at 100 ° C. ([η]100 ° C.) of 0.8 or less. The technique discloses that the gel content of the tetrahydrofuran insoluble content of the acrylic rubber used in the technique is 80% by weight or less, preferably 5 to 80% by weight, and preferably exists as much as possible within the range of 70% or less, and that the extrusion property deteriorates when the gel content is less than 5%. It is also described that the weight average molecular weight (Mw) of the acrylic rubber used is 200,000 to 1,000,000, and that if the weight average molecular weight (Mw) exceeds 1,000,000, the viscoelasticity of the acrylic rubber becomes too high, which is undesirable. However, there has been a demand for a highly balanced combination of high strength and processability during kneading such as Banbury mixing, and there has also been a demand for improved storage stability. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 139466 Brochure [Patent Document 2] Patent No. 3599962 [Patent Document 3] International Publication No. 2018 / 143101 Brochure Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide an acrylic rubber sheet having excellent storage stability and processability and a method for producing the same, an acrylic rubber veil formed by laminating the acrylic rubber sheets, a rubber mixture containing the acrylic rubber sheet or the acrylic rubber veil and a method for producing the same, and a cross-linked rubber product thereof. [Means for solving the problem]
[0008] The inventors of the present invention conducted intensive research in light of the above-mentioned problems and discovered that, while crumb-like acrylic rubber that uses a (meth)acrylic acid ester as a main component and has a specific molecular weight and an increased molecular weight distribution in the polymer region to improve strength characteristics has poor storage stability and processability, an acrylic rubber sheet that contains a specific antioxidant and is formed into a sheet with a specific amount of gel has highly excellent storage stability and processability without compromising strength characteristics.
[0009] The present inventors have also found that the effects of the present invention can be further enhanced by specifying the type of sheet, the shape, melting point, molecular weight and content of the specific antioxidant, and the complex viscosity at a specific temperature, pH and specific gravity.
[0010] The present inventors have also discovered that while it has been extremely difficult to improve the storage stability of acrylic rubber because it is extremely difficult to uniformly disperse an antioxidant in an emulsion polymerization liquid obtained by emulsion polymerizing a monomer component mainly composed of a (meth)acrylic acid ester, it is possible to produce an acrylic rubber sheet with excellent storage stability and processability by melt-kneading the phenol-based antioxidant and acrylic rubber in a substantially water-free state (specific moisture content) using a specific screw-type extruder after washing and extruding the mixture into a sheet.
[0011] The inventors have also discovered that when the polymerization conversion rate of the emulsion polymerization is increased in order to improve the strength properties of the acrylic rubber, the amount of gel rapidly increases, thereby worsening the processability of the acrylic rubber; however, by melt-kneading the washed hydrous crumbs in a substantially water-free state (specific moisture content) using a specific screw-type extruder and extruding them into a sheet, the amount of gel that rapidly increased during the emulsion polymerization disappears, and an acrylic rubber sheet with excellent processability can be produced.
[0012] The present inventors have also discovered that by emulsifying a specific antioxidant to be added to an emulsion polymerization liquid and specifying the production temperature and emulsifier concentration, as well as specifying the temperature of the water-containing crumb fed into a screw-type extruder, it is possible to dramatically improve the storage stability and processability of the obtained acrylic rubber sheet.
[0013] Based on these findings, the present inventors have completed the present invention.
[0014] Thus, according to the present invention, there is provided an acrylic rubber sheet comprising an acrylic rubber having a weight average molecular weight (Mw) of 100,000 to 5,000,000 and a ratio (Mz / Mw) of z-average molecular weight (Mz) to weight average molecular weight (Mw) of 1.3 or more, which contains a (meth)acrylic acid ester as a main component, which contains a phenol-based antiaging agent, and has a gel content of 50% by weight or less.
[0015] In the acrylic rubber sheet of the present invention, the acrylic rubber sheet is preferably a melt-kneaded sheet.
[0016] In the acrylic rubber sheet of the present invention, the gel amount is preferably 15% by weight or less.
[0017] In the acrylic rubber sheet of the present invention, the proportion of the acrylic rubber in the acrylic rubber sheet is preferably 85% by weight or more.
[0018] In the acrylic rubber sheet of the present invention, the ash content in the acrylic rubber sheet is preferably 0.8% by weight or less.
[0019] In the acrylic rubber sheet of the present invention, the content of at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus in the ash is preferably 60% by weight or more.
[0020] In the acrylic rubber sheet of the present invention, the phenol-based antioxidant is preferably a hindered phenol-based antioxidant.
[0021] In the acrylic rubber sheet of the present invention, the melting point of the phenol-based antioxidant is preferably 150° C. or lower.
[0022] In the acrylic rubber sheet of the present invention, the molecular weight of the phenol-based antioxidant is preferably in the range of 100 to 1,000.
[0023] In the acrylic rubber sheet of the present invention, the content of the phenol-based antioxidant is preferably 0.001 to 15% by weight.
[0024] The acrylic rubber sheet of the present invention preferably has a weight average molecular weight (Mw) in the range of 1,000,000 to 5,000,000.
[0025] In the acrylic rubber sheet of the present invention, the complex viscosity at 60° C. ([η]60° C.) is preferably 15,000 Pa·s or less.
[0026] In the acrylic rubber sheet of the present invention, the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is preferably 0.5 or more.
[0027] The acrylic rubber sheet of the present invention preferably has a pH of 6 or less.
[0028] The acrylic rubber sheet of the present invention preferably has a specific gravity of 0.7 or more.
[0029] In the acrylic rubber sheet of the present invention, the specific gravity is more preferably in the range of 0.8 to 1.4.
[0030] In the acrylic rubber sheet of the present invention, the Mooney viscosity (ML1+4, 100° C.) of the acrylic rubber sheet is preferably in the range of 10-150.
[0031] Thus, according to the present invention, there is also provided a method for producing an acrylic rubber sheet, which includes an emulsion polymerization step of emulsifying a monomer component mainly composed of a (meth)acrylic acid ester with water and an emulsifier, and emulsion-polymerizing the resulting emulsion polymerization liquid in the presence of a polymerization initiator until a polymerization conversion rate of 90% by weight or more, an antioxidant addition step of adding a phenol-based antioxidant to the resulting emulsion polymerization liquid, a coagulation step of contacting the emulsion polymerization liquid to which the antioxidant has been added with a coagulation liquid to produce water-containing crumbs, a washing step of washing the produced water-containing crumbs, and a dehydration, drying and molding step of extruding the washed water-containing crumbs into a sheet-like dried rubber having a water content of less than 1% by weight using a screw-type extruder equipped with a dehydration barrel having a dehydration slit, a drying barrel for drying under reduced pressure, and a die at its tip.
[0032] In the method for producing an acrylic rubber sheet of the present invention, the temperature of the water-containing crumbs fed into the screw-type extruder is preferably 40° C. or higher.
[0033] In the method for producing an acrylic rubber sheet of the present invention, the phenolic antioxidant to be added is preferably a phenolic antioxidant-containing emulsion emulsified with warm water and an emulsifier.
[0034] In the method for producing an acrylic rubber sheet of the present invention, the temperature of the warm water is preferably 40° C. or higher.
[0035] In the method for producing an acrylic rubber sheet of the present invention, the temperature of the warm water is preferably equal to or higher than the melting point of the phenolic antioxidant used.
[0036] In the method for producing an acrylic rubber sheet of the present invention, the emulsifier concentration of the phenol-based antioxidant-containing emulsion is preferably 1% by weight or more.
[0037] Thus, the present invention also provides an acrylic rubber veil formed by laminating the above acrylic rubber sheets.
[0038] According to the present invention, there is also provided a rubber mixture obtained by mixing the above-mentioned acrylic rubber sheet or acrylic rubber veil with a filler and a crosslinking agent.
[0039] According to the present invention, there is also provided a method for producing a rubber mixture, which comprises mixing a filler and a crosslinking agent with the above-mentioned acrylic rubber sheet or acrylic rubber veil using a mixer.
[0040] The present invention also provides a method for producing a rubber mixture, which comprises mixing the above-mentioned acrylic rubber sheet or acrylic rubber veil with a filler and then mixing a crosslinking agent therein.
[0041] According to the present invention, there is further provided a cross-linked rubber product obtained by cross-linking the above rubber mixture. Effect of the Invention
[0042] According to the present invention, there are provided an acrylic rubber sheet having excellent storage stability and processability and a method for producing the same, an acrylic rubber veil formed by laminating the acrylic rubber sheet, a rubber mixture formed by mixing the acrylic rubber sheet or the acrylic rubber veil and a method for producing the same, and a cross-linked rubber product formed by cross-linking the rubber mixture. [Brief description of the drawings]
[0043] [Figure 1] FIG. 1 is a diagram illustrating an example of an acrylic rubber production system used for producing an acrylic rubber sheet according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the configuration of the screw-type extruder in FIG. 1. [Diagram 3]FIG. 2 is a diagram showing the configuration of a transportable cooling device used as the cooling device in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0044] The acrylic rubber sheet of the present invention is characterized in that it comprises an acrylic rubber having a weight average molecular weight (Mw) of 100,000 to 5,000,000 and a ratio (Mz / Mw) of z-average molecular weight (Mz) to weight average molecular weight (Mw) of 1.3 or more, which is composed mainly of a (meth)acrylic acid ester, contains a phenol-based antiaging agent, and has a gel amount of 50% by weight or less.
[0045] <Monomer components> The acrylic rubber constituting the acrylic rubber sheet of the present invention is mainly composed of (meth)acrylic acid ester. The ratio of (meth)acrylic acid ester in the acrylic rubber is appropriately selected depending on the purpose of use, but is usually 50% by weight or more, preferably 70% by weight or more, and more preferably 80% by weight or more. In the present invention, "(meth)acrylic acid ester" is used as a general term for esters of acrylic acid and / or methacrylic acid.
[0046] It is preferable that the acrylic rubber constituting the acrylic rubber sheet of the present invention contains bonding units derived from at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, in order to highly improve the crosslinking properties of the acrylic rubber sheet.
[0047] The acrylic rubber constituting the acrylic rubber sheet of the present invention is preferably one containing a reactive group-containing monomer in its bonding units, since this can highly improve the heat resistance, compression set resistance, and the like.
[0048] A preferred specific example of the acrylic rubber constituting the acrylic rubber sheet of the present invention is one comprising at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and, if necessary, other copolymerizable monomers.
[0049] The (meth)acrylic acid alkyl ester is not particularly limited, but is usually a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 12 carbon atoms, preferably a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms, and more preferably a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 6 carbon atoms.
[0050] Specific examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred.
[0051] The (meth)acrylic acid alkoxyalkyl ester is not particularly limited, but is usually a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 12, preferably a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 8, and more preferably a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 6 carbon atoms.
[0052] Specific examples of the (meth)acrylic acid alkoxyalkyl ester include methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxymethyl (meth)acrylate, ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, etc. Among these, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, etc. are preferred, and methoxyethyl acrylate, ethoxyethyl acrylate, etc. are more preferred.
[0053] At least one (meth)acrylic acid ester selected from the group consisting of these (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters is used alone or in combination of two or more, and the ratio of the (meth)acrylic acid ester in the acrylic rubber is usually 50 to 99.99% by weight, preferably 70 to 99.9% by weight, more preferably 80 to 99.5% by weight, and most preferably 87 to 99% by weight. If the amount of the (meth)acrylic acid ester in the monomer component is excessively small, the weather resistance, heat resistance, and oil resistance of the obtained acrylic rubber may decrease, which is not preferable.
[0054] The reactive group-containing monomer is not particularly limited and may be appropriately selected depending on the intended use. In general, a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a halogen group, a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a chlorine atom is preferred, a monomer having an ion-reactive group such as a carboxyl group or an epoxy group is more preferred, and a monomer having a carboxyl group is particularly preferred.
[0055] The monomer having a carboxyl group is not particularly limited, but an ethylenically unsaturated carboxylic acid can be suitably used. Examples of the ethylenically unsaturated carboxylic acid include ethylenically unsaturated monocarboxylic acid, ethylenically unsaturated dicarboxylic acid, and ethylenically unsaturated dicarboxylic acid monoester, and among these, ethylenically unsaturated dicarboxylic acid monoester is particularly preferred because it can further improve the compression set resistance property when the acrylic rubber is made into a rubber cross-linked product.
[0056] The ethylenically unsaturated monocarboxylic acid is not particularly limited, but is preferably an ethylenically unsaturated monocarboxylic acid having 3 to 12 carbon atoms, and examples thereof include acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and cinnamic acid.
[0057] The ethylenically unsaturated dicarboxylic acid is not particularly limited, but is preferably an ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms, and examples thereof include butenedioic acids such as fumaric acid and maleic acid, itaconic acid, citraconic acid, etc. The ethylenically unsaturated dicarboxylic acid also includes those that exist as an anhydride.
[0058] The ethylenically unsaturated dicarboxylic acid monoester is not particularly limited, but is usually an ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms and an alkyl monoester having 1 to 12 carbon atoms, preferably an ethylenically unsaturated dicarboxylic acid having 4 to 6 carbon atoms and an alkyl monoester having 2 to 8 carbon atoms, and more preferably an alkyl monoester having 2 to 6 carbon atoms of butenedioic acid having 4 carbon atoms.
[0059] Specific examples of ethylenically unsaturated dicarboxylic acid monoesters include butenedioic acid monoalkyl esters such as monomethyl fumarate, monoethyl fumarate, mono-n-butyl fumarate, monomethyl maleate, monoethyl maleate, mono-n-butyl maleate, monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclohexenyl fumarate, monocyclopentyl maleate, and monocyclohexyl maleate; and itaconic acid monoalkyl esters such as monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, and monocyclohexyl itaconate; and among these, mono-n-butyl fumarate and mono-n-butyl maleate are preferred, and mono-n-butyl fumarate is particularly preferred.
[0060] Examples of the monomer having an epoxy group include epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate; epoxy group-containing vinyl ethers such as allyl glycidyl ether and vinyl glycidyl ether; and the like.
[0061] Examples of monomers having a halogen group include unsaturated alcohol esters of halogen-containing saturated carboxylic acids, (meth)acrylic acid haloalkyl esters, (meth)acrylic acid haloacyloxyalkyl esters, (meth)acrylic acid (haloacetylcarbamoyloxy)alkyl esters, halogen-containing unsaturated ethers, halogen-containing unsaturated ketones, halomethyl group-containing aromatic vinyl compounds, halogen-containing unsaturated amides, and haloacetyl group-containing unsaturated monomers.
[0062] Examples of unsaturated alcohol esters of halogen-containing saturated carboxylic acids include vinyl chloroacetate, vinyl 2-chloropropionate, and allyl chloroacetate. Examples of (meth)acrylic acid haloalkyl esters include chloromethyl (meth)acrylate, 1-chloroethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 1,2-dichloroethyl (meth)acrylate, 2-chloropropyl (meth)acrylate, 3-chloropropyl (meth)acrylate, and 2,3-dichloropropyl (meth)acrylate. Examples of (meth)acrylic acid haloacyloxyalkyl esters include 2-(chloroacetoxy)ethyl (meth)acrylate, 2-(chloroacetoxy)propyl (meth)acrylate, 3-(chloroacetoxy)propyl (meth)acrylate, and 3-(hydroxychloroacetoxy)propyl (meth)acrylate. Examples of (meth)acrylic acid (haloacetylcarbamoyloxy) alkyl esters include 2-(chloroacetylcarbamoyloxy) ethyl (meth)acrylate and 3-(chloroacetylcarbamoyloxy) propyl (meth)acrylate. Examples of halogen-containing unsaturated ethers include chloromethyl vinyl ether, 2-chloroethyl vinyl ether, 3-chloropropyl vinyl ether, 2-chloroethyl allyl ether, and 3-chloropropyl allyl ether. Examples of halogen-containing unsaturated ketones include 2-chloroethyl vinyl ketone, 3-chloropropyl vinyl ketone, and 2-chloroethyl allyl ketone. Examples of halomethyl group-containing aromatic vinyl compounds include p-chloromethylstyrene, m-chloromethylstyrene, o-chloromethylstyrene, and p-chloromethyl-α-methylstyrene. Examples of halogen-containing unsaturated amides include N-chloromethyl(meth)acrylamide. Examples of the haloacetyl group-containing unsaturated monomer include 3-(hydroxychloroacetoxy)propyl allyl ether and p-vinylbenzyl chloroacetic acid ester.
[0063] These reactive group-containing monomers may be used alone or in combination of two or more, and their proportion in the acrylic rubber is usually 0.01 to 20% by weight, preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and most preferably 1 to 3% by weight.
[0064] The other monomers used as necessary are not particularly limited as long as they are copolymerizable with the above-mentioned monomers, and examples thereof include aromatic vinyl, ethylenically unsaturated nitrile, acrylamide monomers, other olefin monomers, etc. Examples of aromatic vinyl include styrene, α-methylstyrene, divinylbenzene, etc. Examples of ethylenically unsaturated nitrile include acrylonitrile, methacrylonitrile, etc. Examples of acrylamide monomers include acrylamide, methacrylamide, etc. Examples of other olefin monomers include ethylene, propylene, vinyl acetate, ethyl vinyl ether, butyl vinyl ether, etc.
[0065] These other monomers may be used alone or in combination of two or more, and their proportion in the acrylic rubber is usually in the range of 0 to 30% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, and most preferably 0 to 10% by weight.
[0066] <Acrylic rubber> The acrylic rubber constituting the acrylic rubber sheet of the present invention is made of the above-mentioned monomer component and preferably has a reactive group.
[0067] The reactive group is not particularly limited and is appropriately selected depending on the purpose of use, but is preferably at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a halogen group, more preferably at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a chlorine atom, particularly preferably a carboxyl group or an epoxy group, and most preferably a carboxyl group, which is suitable for highly improving the crosslinked properties of the acrylic rubber sheet. In addition, the reactive group is preferably an ion-reactive group such as a carboxyl group or an epoxy group, which is suitable for particularly improving water resistance. The acrylic rubber having such a reactive group may be provided with a reactive group by a post-reaction, but is preferably one obtained by copolymerizing a reactive group-containing monomer.
[0068] The content of the reactive group may be appropriately selected depending on the purpose of use, but when the weight ratio of the reactive group itself is usually in the range of 0.001 wt % or more, preferably 0.001 to 5 wt %, more preferably 0.01 to 3 wt %, particularly preferably 0.05 to 1 wt %, and most preferably 0.1 to 0.5 wt %, it is suitable in that properties such as processability, strength properties, compression set resistance, oil resistance, cold resistance, and water resistance are highly balanced.
[0069] Specific examples of the acrylic rubber constituting the acrylic rubber sheet of the present invention include at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and other copolymerizable monomers as necessary. The proportions of each in the acrylic rubber are as follows: the bonding units derived from at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters are usually in the range of 50 to 99.99% by weight, preferably 70 to 99.9% by weight, more preferably 80 to 99.5% by weight, and particularly preferably 87 to 99% by weight; the bonding units derived from the reactive monomer are usually in the range of 0.01 to 20% by weight, preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and particularly preferably 1 to 3% by weight; and the bonding units derived from other monomers are usually in the range of 0 to 30% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, and particularly preferably 0 to 10% by weight. By setting the ratio of these monomers constituting the acrylic rubber within this range, the objects of the present invention can be achieved to a high degree, and when the acrylic rubber sheet is crosslinked, the water resistance and compression set resistance are significantly improved, which is preferable.
[0070] The weight average molecular weight (Mw) of the acrylic rubber constituting the acrylic rubber sheet of the present invention, in terms of absolute molecular weight measured by GPC-MALS, is preferably in the range of 100,000 to 5,000,000, preferably 500,000 to 5,000,000, more preferably 1,000,000 to 5,000,000, particularly preferably 1,100,000 to 3,500,000, and most preferably 1,200,000 to 2,500,000, which is suitable because the processability during mixing of the acrylic rubber sheet, strength properties, and compression set resistance properties are highly balanced.
[0071] The ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) of the acrylic rubber constituting the acrylic rubber sheet of the present invention, in terms of absolute molecular weight distribution with emphasis on the polymer region measured by GPC-MALS, is preferably 1.3 or more, preferably 1.4 to 5, and more preferably in the range of 1.5 to 2, which is suitable because it allows the processability and strength characteristics of the acrylic rubber veil to be highly balanced and also alleviates changes in physical properties during storage.
[0072] The glass transition temperature (Tg) of the acrylic rubber constituting the acrylic rubber sheet of the present invention is not particularly limited, but is usually 20° C. or lower, preferably 10° C. or lower, and more preferably 0° C. or lower. The lower limit of the glass transition temperature (Tg) is not particularly limited, but is usually −80° C. or higher, preferably −60° C. or higher, and more preferably −40° C. or higher. By setting the glass transition temperature to the lower limit or higher, the oil resistance and heat resistance can be improved, and by setting the glass transition temperature to the upper limit or lower, the cold resistance and processability can be improved.
[0073] The content of the acrylic rubber in the acrylic rubber sheet of the present invention is appropriately selected depending on the purpose of use, but is usually 85% by weight or more, preferably 90% by weight or more, more preferably 95% by weight or more, particularly preferably 97% by weight or more, and most preferably 98% by weight or more. The content of the acrylic rubber in the acrylic rubber sheet of the present invention is approximately equal to the total amount of the acrylic rubber sheet minus the amount of ash that was not completely removed from the emulsifier and coagulant used and the amount of the phenol-based anti-aging agent added and dispersed in the acrylic rubber sheet.
[0074] <Anti-aging agent> The acrylic rubber sheet of the present invention is characterized by containing a phenol-based antioxidant.
[0075] The phenolic antioxidant used is not particularly limited as long as it is one that is normally used as an antioxidant for rubber, but preferably, when it is a hindered phenolic antioxidant, it is suitable because it can achieve high storage stability and heat resistance effects. The hindered phenolic antioxidant refers to a phenolic antioxidant having a hindered structure, and the hindered structure is a structure having bulky substituents on both sides of the phenol group, and the bulky substituents on both sides are substituents with 3 or more carbon atoms, preferably 4, and specifically, includes an isobutyl group or a t-butyl group, and preferably a t-butyl group.
[0076] The melting point of the phenol-based anti-aging agent is not particularly limited, but a melting point of 150° C. or lower is usually preferred, preferably 100° C. or lower, more preferably 90° C. or lower, particularly preferably 80° C. or lower, and most preferably 70° C. or lower, since this provides excellent uniform fine dispersion with the acrylic rubber during melt-kneading and can highly improve the storage stability and heat resistance of the acrylic rubber sheet.
[0077] The molecular weight of the phenol-based antiaging agent is not particularly limited, but is usually 250 to 1,000, preferably 300 to 800, and more preferably 350 to 600, which is suitable because it provides excellent uniform and fine dispersion with the acrylic rubber and can highly improve the heat resistance and storage stability of the acrylic rubber sheet.
[0078] Examples of the hindered phenol-based antioxidants include 2,6-di-t-butylphenol, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-α-dimethylamino-p-cresol, butyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, hexyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, octyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, and 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid. decyl, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate dodecyl, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate octadecyl, 3-(4-hydroxy-3,5-diisopropylphenyl)propionate heptyl, 3-(4-hydroxy-3,5-diisopropylphenyl)propionate octyl, 3-(4-hydroxy-3,5-diisopropylphenyl)propionate dodecyl, 3-(4-hydroxy-3,5-diisopropylphenyl)propionate octadecyl, 4,4'-methyl Examples of the tert-butyl phenol include 2,6-di-t-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, and the like. Preferred are 3-(4-hydroxy-3,5-di-t-butylphenyl)butyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl)hexyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl)octyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl)decyl propionate, dodecyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate and octadecyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate are more preferably octyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, decyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, dodecyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate and octadecyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate.
[0079] Examples of phenol-based antioxidants other than the hindered phenol-based antioxidants include styrenated phenols such as butyl hydroxyanisole and mono (or di, or tri) (α-methylbenzyl) phenol. 2,2'-methylene-bis (6-α-methyl-benzyl-p-cresol), 2,2'-methylene-bis (4-methyl-6-t-butylphenol), alkylated bisphenols, 2,4-bis [(octylthio) methyl] -6-methylphenol, 2,2'-thiobis (4-methyl-6-t-butylphenol), 4,4'-thiobis (6-t-butyl-o-cresol), and the like, with 2,4-bis [(octylthio) methyl] -6-methylphenol being preferred.
[0080] These phenol-based antiaging agents can be used alone or in combination of two or more. The content of the phenol-based antiaging agent in the acrylic rubber sheet is not particularly limited, but is usually in the range of 0.001 to 15% by weight, preferably 0.01 to 10% by weight, more preferably 0.1 to 5% by weight, particularly preferably 0.3 to 3% by weight, and most preferably 0.5 to 2% by weight.
[0081] The acrylic rubber sheet of the present invention may contain antioxidants other than the phenol-based antioxidants, provided the antioxidants do not impair the object of the present invention.
[0082] <Acrylic rubber sheet> The acrylic rubber sheet of the present invention is characterized in that it is made of the above-mentioned acrylic rubber, contains the above-mentioned antioxidant, and has a specific gel amount.
[0083] The thickness of the acrylic rubber sheet of the present invention is not particularly limited, but is preferably in the range of usually 1 to 40 mm, preferably 2 to 35 mm, more preferably 3 to 30 mm, and most preferably 5 to 25 mm, since workability, storage stability, and productivity are well balanced. In particular, in the case where the productivity is significantly improved to produce an inexpensive acrylic rubber sheet, the thickness is usually in the range of 1 to 30 mm, preferably 2 to 25 mm, more preferably 3 to 15 mm, and particularly preferably 4 to 12 mm.
[0084] The width of the acrylic rubber sheet of the present invention is appropriately selected depending on the purpose of use, but is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm, which is particularly suitable for ease of handling.
[0085] The length of the acrylic rubber sheet of the present invention is not particularly limited, but is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm, which is particularly suitable for ease of handling.
[0086] The acrylic rubber sheet of the present invention has a gel content of 50% by weight or less, preferably 30% by weight or less, more preferably 20% by weight or less, even more preferably 15% by weight or less, particularly preferably 10% by weight or less, and most preferably 5% by weight or less, in terms of insoluble matter in methyl ethyl ketone. The gel content of the methyl ethyl ketone in the acrylic rubber veil is related to the processability during kneading in a Banbury kneader, but the characteristics of the gel content differ depending on the solvent used, and there is no correlation with the gel content insoluble in THF (tetrahydrofuran), in particular.
[0087] The ash content of the acrylic rubber sheet of the present invention is not particularly limited, but is usually 0.8% by weight or less, preferably 0.5% by weight or less, more preferably 0.3% by weight or less, particularly preferably 0.2% by weight or less, and most preferably 0.15% by weight or less, which is suitable in terms of excellent storage stability and water resistance.
[0088] The lower limit of the ash content of the acrylic rubber sheet of the present invention is not particularly limited, but an ash content of usually 0.0001% by weight or more, preferably 0.0005% by weight or more, more preferably 0.001% by weight or more, particularly preferably 0.005% by weight or more, and most preferably 0.01% by weight or more is preferable because it suppresses metal adhesion and provides excellent workability.
[0089] The ash content, which provides a high balance between storage stability, water resistance, and workability of the acrylic rubber sheet of the present invention, is usually in the range of 0.0001 to 0.8% by weight, preferably 0.0005 to 0.5% by weight, more preferably 0.001 to 0.3% by weight, particularly preferably 0.005 to 0.2% by weight, and most preferably 0.01 to 0.15% by weight.
[0090] The content (total amount) of at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus in the ash of the acrylic rubber sheet of the present invention is not particularly limited, but when the content (total amount) of the at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus is, relative to the total ash content, usually at least 30% by weight, preferably 50% by weight or more, more preferably 60% by weight or more, particularly preferably 70% by weight or more, and most preferably 80% by weight or more, the storage stability and water resistance are highly excellent and suitable.
[0091] The total amount of sodium and sulfur in the ash of the acrylic rubber sheet of the present invention is not particularly limited, but when the total amount of sodium and sulfur is 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 80% by weight or more, the storage stability and water resistance are highly excellent and suitable.
[0092] The ratio of sodium to sulfur in the ash of the acrylic rubber sheet of the present invention ([Na] / [S]) is not particularly limited by weight, but when it is in the range of usually 0.4 to 2.5, preferably 0.6 to 2, preferably 0.8 to 1.7, and more preferably 1 to 1.5, water resistance is highly excellent and it is suitable.
[0093] The total amount of magnesium and phosphorus in the ash of the acrylic rubber sheet of the present invention is not particularly limited, but when the total amount of magnesium and phosphorus is 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 80% by weight or more, the storage stability and water resistance are highly excellent and suitable.
[0094] The ratio of magnesium to phosphorus in the ash of the acrylic rubber sheet of the present invention ([Mg] / [P]) is not particularly limited by weight, but is preferably in the range of usually 0.4 to 2.5, preferably 0.4 to 1.3, more preferably 0.4 to 1, particularly preferably 0.45 to 0.75, and most preferably 0.5 to 0.7, in which case storage stability and water resistance are highly excellent.
[0095] The specific gravity of the acrylic rubber sheet of the present invention is not particularly limited, but is usually 0.7 or more, preferably 0.8 to 1.4, more preferably 0.9 to 1.3, particularly preferably 0.95 to 1.25, and most preferably 1.0 to 1.2, and is therefore suitable since it has excellent storage stability.
[0096] The pH of the acrylic rubber sheet of the present invention is not particularly limited, but is usually 6 or less, preferably 2 to 6, more preferably 2.5 to 5.5, and particularly preferably 3 to 5, and is therefore suitable since storage stability is highly improved.
[0097] The complex viscosity at 60°C ([η]60°C) of the acrylic rubber sheet of the present invention is not particularly limited, but when it is usually in the range of 15,000 Pa·s or less, preferably 2,000 to 10,000 Pa·s, more preferably 2,500 to 7,000 Pa·s, and most preferably 2,700 to 5,500 Pa·s, the sheet will be excellent in processability, oil resistance, and shape retention.
[0098] The complex viscosity of the acrylic rubber sheet of the present invention at 100°C ([η]100°C) is not particularly limited, but a value in the range of usually 1,500 to 6,000 Pa·s, preferably 2,000 to 5,000 Pa·s, more preferably 2,500 to 4,000 Pa·s, and most preferably 2,500 to 3,500 Pa·s is suitable in terms of excellent processability, oil resistance, and shape retention.
[0099] The ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) of the acrylic rubber sheet of the present invention is not particularly limited, but is usually 0.5 or more, preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.83 or more. In addition, when the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) of the acrylic rubber sheet of the present invention is usually in the range of 0.5 to 0.99, preferably 0.6 to 0.98, more preferably 0.75 to 0.95, particularly preferably 0.8 to 0.94, and most preferably 0.83 to 0.93, the processability, oil resistance, and shape retention are highly balanced and are suitable.
[0100] The water content of the acrylic rubber sheet of the present invention is not particularly limited, but when it is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less, the crosslinking characteristics are optimized and the properties such as heat resistance and water resistance are highly excellent, which is preferable.
[0101] The Mooney viscosity (ML1+4, 100°C) of the acrylic rubber sheet of the present invention is not particularly limited, but when it is in the range of usually 10 to 150, preferably 20 to 100, and more preferably 25 to 70, the processability and strength properties are highly balanced and it is suitable.
[0102] The type of the acrylic rubber sheet of the present invention is not particularly limited, but examples thereof include a blown sheet produced by a hollow molding method, a cast sheet produced by a solution casting method, and a melt-kneaded sheet produced by a melt extrusion method. Among these, the melt-kneaded sheet is preferred in terms of enabling the storage stability effect of the phenol-based antiaging agent to be maximized.
[0103] <Method of manufacturing acrylic rubber sheet> The method for producing the acrylic rubber sheet of the present invention is not particularly limited, but the acrylic rubber sheet can be easily produced by, for example, including an emulsion polymerization step of emulsifying a monomer component mainly composed of a (meth)acrylic acid ester with water and an emulsifier, and emulsion-polymerizing the monomer component in the presence of a polymerization initiator until a polymerization conversion rate of 90% by weight or more is reached to obtain an emulsion polymerization liquid, an antioxidant addition step of adding a phenol-based antioxidant to the obtained emulsion polymerization liquid, a coagulation step of contacting the emulsion polymerization liquid to which the antioxidant has been added with a coagulation liquid to produce water-containing crumbs, a washing step of washing the produced water-containing crumbs, and a dehydration, drying, and molding step of extruding the washed water-containing crumbs into a sheet-like dry rubber having a water content of less than 1% by weight using a screw-type extruder equipped with a dehydration barrel having a dehydration slit, a drying barrel for drying under reduced pressure, and a die at the tip.
[0104] (Emulsion polymerization process) The emulsion polymerization step in the method for producing an acrylic rubber sheet of the present invention is characterized in that a monomer component mainly composed of a (meth)acrylic acid ester is emulsified with water and an emulsifier, and emulsion-polymerized in the presence of a polymerization initiator to a polymerization conversion rate of 90% by weight or more to obtain an emulsion polymerization liquid.
[0105] The monomer components used are the same as those exemplified as the monomer components and those described above as the preferred ranges, and the amount used may be appropriately selected so as to obtain the monomer composition of the acrylic rubber constituting the acrylic rubber sheet.
[0106] The emulsifier used in the emulsion polymerization is not particularly limited, but examples thereof include anionic emulsifiers, cationic emulsifiers, and nonionic emulsifiers, and is preferably anionic emulsifiers.
[0107] The anionic emulsifier is not particularly limited, and examples thereof include salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid; alkylbenzenesulfonates such as sodium dodecylbenzenesulfonate; sulfates such as sodium lauryl sulfate, and phosphates such as polyoxyalkylene alkyl ether phosphates; and alkylsulfosuccinates. Among these anionic emulsifiers, phosphates and sulfates are preferred, and phosphates are particularly preferred. Suitable examples of phosphates include sodium lauryl phosphate, potassium lauryl phosphate, and sodium polyoxyalkylene alkyl ether phosphate. Suitable examples of sulfates include sodium lauryl sulfate, ammonium lauryl sulfate, sodium myristyl sulfate, sodium laureth sulfate, sodium polyoxyethylene alkyl sulfate, and sodium polyoxyethylene alkylaryl sulfate, and among these, sodium lauryl sulfate is particularly preferred. These anionic emulsifiers can be used alone or in combination of two or more.
[0108] Examples of the cationic emulsifier include alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride.
[0109] The nonionic emulsifier is not particularly limited, but examples thereof include polyoxyalkylene fatty acid esters such as polyoxyethylene stearate ester; polyoxyalkylene alkyl ethers such as polyoxyethylene dodecyl ether; polyoxyalkylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether; polyoxyethylene sorbitan alkyl esters; and the like. Polyoxyalkylene alkyl ethers and polyoxyalkylene alkylphenol ethers are preferred, and polyoxyethylene alkyl ethers and polyoxyethylene alkylphenol ethers are more preferred.
[0110] These emulsifiers can be used alone or in combination of two or more. The amount used is usually 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 1 to 3 parts by weight, per 100 parts by weight of the monomer component.
[0111] The method for mixing the monomer component, water, and emulsifier may be a conventional method, and examples thereof include a method in which the monomer, emulsifier, and water are stirred using a stirrer such as a homogenizer or a disk turbine. The amount of water used is usually 1 to 1,000 parts by weight, preferably 5 to 500 parts by weight, more preferably 10 to 300 parts by weight, particularly preferably 15 to 150 parts by weight, and most preferably 20 to 80 parts by weight, relative to 100 parts by weight of the monomer component.
[0112] The polymerization catalyst used is not particularly limited as long as it is one that is usually used in emulsion polymerization. For example, a redox catalyst consisting of a radical generator and a reducing agent can be used.
[0113] Examples of the radical generator include peroxides and azo compounds, and preferably peroxides. As the peroxide, inorganic peroxides and organic peroxides can be used.
[0114] Examples of inorganic peroxides include sodium persulfate, potassium persulfate, hydrogen peroxide, and ammonium persulfate. Among these, potassium persulfate, hydrogen peroxide, and ammonium persulfate are preferred, and potassium persulfate is particularly preferred.
[0115] The organic peroxide is not particularly limited as long as it is a known peroxide used in emulsion polymerization, and examples thereof include 2,2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane, 1-di-(t-hexylperoxy)cyclohexane, 1,1-di-(t-butylperoxy)cyclohexane, 4,4-di-(t-butylperoxy)n-butyl valerate, 2,2-di-(t-butylperoxy)butane, t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, and paramenthane hydroperoxide. oxide, benzoyl peroxide, 1,1,3,3-tetraethylbutyl hydroperoxide, t-butylcumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide, dibenzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzyl) peroxydicarbonate, diisobutyryl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethyl t-butylperoxy-2-ethylhexanate, t-hexylperoxy-2-ethylhexanate, t-butylperoxy-3,5,5-trimethylhexanate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxybenzoate, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and among these, diisopropylbenzene hydroperoxide, cumene hydroperoxide, paramenthane hydroperoxide, benzoyl peroxide, and the like are preferred.
[0116] Examples of azo compounds include azobisisoptylonitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane, 2,2'-azobis(propane-2-carboxamidine), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide], 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2,2'-azobis(1-imino-1-pyrrolidino-2-methylpropane), and 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide}.
[0117] These radical generators can be used alone or in combination of two or more kinds. The amount of the radical generator used is usually in the range of 0.0001 to 5 parts by weight, preferably 0.0005 to 1 part by weight, and more preferably 0.001 to 0.5 parts by weight, per 100 parts by weight of the monomer component.
[0118] The reducing agent can be any reducing agent that is used in a redox catalyst for emulsion polymerization, but in the present invention, it is particularly preferable to use at least two reducing agents. As the at least two reducing agents, for example, a combination of a metal ion compound in a reduced state and another reducing agent is preferable.
[0119] The reduced metal ion compound is not particularly limited, but examples thereof include ferrous sulfate, sodium iron hexamethylenediaminetetraacetate, and cuprous naphthenate, among which ferrous sulfate is preferred. These reduced metal ion compounds can be used alone or in combination of two or more, and the amount used is usually in the range of 0.000001 to 0.01 parts by weight, preferably 0.00001 to 0.001 parts by weight, and more preferably 0.00005 to 0.0005 parts by weight, relative to 100 parts by weight of the monomer component.
[0120] The reducing agent other than these metal ion compounds in a reduced state is not particularly limited, and examples thereof include ascorbic acid or a salt thereof, such as ascorbic acid, sodium ascorbate, and potassium ascorbate; erythorbic acid or a salt thereof, such as erythorbic acid, sodium erythorbate, and potassium erythorbate; sulfinates, such as sodium hydroxymethanesulfinate; sulfites, such as sodium sulfite, potassium sulfite, sodium hydrogen sulfite, aldehyde sodium hydrogen sulfite, and potassium hydrogen sulfite; Examples of suitable phosphorous acids include pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium hydrogen pyrosulfite, and potassium hydrogen pyrosulfite; thiosulfates such as sodium thiosulfate and potassium thiosulfate; phosphorous acid or a salt thereof such as phosphorous acid, sodium phosphite, potassium phosphite, sodium hydrogen phosphite, and potassium hydrogen phosphite; pyrophosphorous acid or a salt thereof such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite, and potassium hydrogen pyrophosphite; sodium formaldehyde sulfoxylate, etc. Among these, ascorbic acid or a salt thereof, sodium formaldehyde sulfoxylate, etc. are preferred, and ascorbic acid or a salt thereof is particularly preferred.
[0121] These reducing agents other than metal ion compounds in a reduced state can be used alone or in combination of two or more kinds, and the amount used is usually in the range of 0.001 to 1 part by weight, preferably 0.005 to 0.5 parts by weight, and more preferably 0.01 to 0.3 parts by weight, per 100 parts by weight of the monomer component.
[0122] A preferred combination of a metal ion compound in a reduced state and another reducing agent is ferrous sulfate and ascorbic acid or a salt thereof and / or sodium formaldehyde sulfoxylate, more preferably ferrous sulfate and an ascorbate and / or sodium formaldehyde sulfoxylate, and most preferably ferrous sulfate and an ascorbate. In this case, the amount of ferrous sulfate used is usually 0.000001 to 0.01 parts by weight, preferably 0.00001 to 0.001 parts by weight, more preferably 0.00005 to 0.0005 parts by weight, relative to 100 parts by weight of the monomer component, and the amount of ascorbic acid or a salt thereof and / or sodium formaldehyde sulfoxylate used is usually 0.001 to 1 part by weight, preferably 0.005 to 0.5 parts by weight, more preferably 0.01 to 0.3 parts by weight, relative to 100 parts by weight of the monomer component.
[0123] The amount of water used in the emulsion polymerization reaction may be only that used during emulsification of the monomer components, but is adjusted to be in the range of usually 10 to 1,000 parts by weight, preferably 50 to 500 parts by weight, more preferably 80 to 400 parts by weight, and most preferably 100 to 300 parts by weight, relative to 100 parts by weight of the monomer components used in the polymerization.
[0124] The emulsion polymerization reaction may be carried out according to a conventional method, and may be any of batch, semi-batch, and continuous. The polymerization temperature and polymerization time are not particularly limited and may be appropriately selected depending on the type of polymerization initiator used. The polymerization temperature is usually in the range of 0 to 100°C, preferably 5 to 80°C, and more preferably 10 to 50°C, and the polymerization time is usually 0.5 to 100 hours, and preferably 1 to 10 hours.
[0125] The polymerization conversion rate of the emulsion polymerization reaction is not particularly limited, but is usually 80% by weight or more, preferably 90% by weight or more, and more preferably 95% by weight or more, which is suitable for producing an acrylic rubber sheet having excellent strength characteristics and no monomer odor. A polymerization terminator may be used to terminate the polymerization.
[0126] (Anti-aging agent addition process) The antioxidant addition step in the method for producing an acrylic rubber sheet of the present invention is characterized by adding a phenol-based antioxidant to the emulsion polymerization liquid after the above-mentioned emulsion polymerization.
[0127] The amount of the phenol-based antiaging agent used may be appropriately selected so as to achieve the content of the phenol-based antiaging agent in the acrylic rubber sheet of the present invention, and is usually in the range of 0.001 to 15 parts by weight, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, particularly preferably 0.3 to 3 parts by weight, and most preferably 0.5 to 2 parts by weight, per 100 parts by weight of the monomer component.
[0128] The method of adding the phenol-based antiaging agent to the emulsion polymerization liquid is not particularly limited, but for example, by emulsifying the phenol-based antiaging agent with an emulsifier and water and adding it as a phenol-based antiaging agent-containing emulsion, the antiaging agent can be easily dispersed in the acrylic rubber and further finely dispersed in the screw extruder, maximizing the antiaging effect, which is preferable.
[0129] The method for emulsifying the phenol-based anti-aging agent is not particularly limited, but the phenol-based anti-aging agent can usually be produced by preparing an emulsion of water and an emulsifier, adding the phenol-based anti-aging agent, and stirring until the emulsion is uniformly dispersed.
[0130] The water for emulsifying the phenol-based antiaging agent is preferably warm water, and when the temperature of the water is usually 40° C. or higher, preferably 50 to 90° C., and more preferably 60 to 80° C., it is suitable because it enables easy emulsification of the phenol-based antiaging agent and uniform dispersion.
[0131] The temperature of the water for emulsifying the phenolic antioxidant is preferably equal to or higher than the melting point of the phenolic antioxidant used, more preferably equal to or higher than the melting point + 5°C, and more preferably equal to or higher than the melting point + 10°C, which allows easy emulsification of the phenolic antioxidant and enables uniform dispersion.
[0132] The emulsifier for emulsifying the phenolic antioxidant is not particularly limited, but it is preferable to use the same emulsifier as that used when emulsifying the monomer component, since this ensures stability in isolating the acrylic rubber in the subsequent step.Specific examples of the emulsifier include anionic emulsifiers, cationic emulsifiers, and nonionic emulsifiers, and preferably anionic emulsifiers, more preferably phosphate ester salts and sulfate ester salts, and particularly preferably phosphate ester salts.
[0133] The amount of emulsifier used to emulsify the phenol-based antiaging agent may be appropriately selected depending on the molecular weight, melting point, SP value, etc. of the antiaging agent used, but when the amount is in the range of usually 1% by weight or more, preferably 2 to 40% by weight, more preferably 3 to 30% by weight, particularly preferably 4 to 20% by weight, and most preferably 5 to 15% by weight, relative to the emulsion of water and emulsifier, this is suitable because it enables easy emulsification of the phenol-based antiaging agent and uniform dispersion.
[0134] The stirring time for emulsifying the phenol-based antiaging agent is not particularly limited as long as it is the time required for the antiaging agent to be uniformly dispersed, but is usually in the range of 1 hour or more, preferably 1 to 5 hours, preferably 1 to 4 hours, and more preferably 1 to 3 hours.
[0135] In the phenolic antioxidant-containing emulsion thus obtained, which is added to the emulsion polymerization liquid, the phenolic antioxidant is uniformly dispersed. The uniform dispersion of the phenolic antioxidant in the phenolic antioxidant-containing emulsion can be judged, for example, as follows. A glass container once filled with the phenolic antioxidant-containing emulsion and then emptied is left standing, and the wall of the glass container after the attached phenolic antioxidant-containing emulsion has dripped down is observed. If it is not dirty, it is judged as good uniform dispersion, and if white powder is attached, it is judged as poor uniform dispersion. The phenolic antioxidant-containing emulsion once uniformly dispersed rarely re-solidifies even when left standing, but if it becomes poorly dispersed, it can be used by stirring again and readjusting.
[0136] The content of the phenolic antioxidant in the phenolic antioxidant-containing emulsion is appropriately selected depending on the purpose of use, but it is usually suitable when it is 10 to 80% by weight, preferably 20 to 60% by weight, and more preferably 30 to 45% by weight, because this highly improves the storage stability and heat resistance of the acrylic rubber sheet.
[0137] The emulsifier concentration of the phenol-based anti-aging agent-containing emulsion is not particularly limited, but is usually 1% by weight or more, preferably 1 to 30% by weight, more preferably 2 to 20% by weight, particularly preferably 3 to 15% by weight, and most preferably in the range of 5 to 10% by weight, which is suitable in order to achieve a high level of balance between the storage stability, heat resistance, and water resistance of the acrylic rubber sheet.
[0138] The pH of the emulsion containing a phenol-based antioxidant is not particularly limited, but when it is usually 6 or less, preferably in the range of 2 to 6, and more preferably in the range of 3 to 6, the storage stability and heat resistance of the acrylic rubber sheet are highly excellent and suitable.
[0139] The method for adding the phenolic antioxidant or the emulsion containing the phenolic antioxidant to the emulsion polymerization liquid is not particularly limited, and may be any conventional method.
[0140] (solidification process) The coagulation step in the method for producing acrylic rubber of the present invention is a step in which the emulsion polymerization liquid to which the phenol-based antioxidant has been added is brought into contact with a coagulation liquid to produce water-containing crumbs.
[0141] The solids concentration of the emulsion polymerization liquid used in the coagulation step is not particularly limited, but is usually adjusted to within the range of 5 to 50% by weight, preferably 10 to 45% by weight, and more preferably 20 to 40% by weight.
[0142] The coagulant used is not particularly limited, but a metal salt is usually used. Examples of the metal salt include alkali metals, salts of metals in Group 2 of the periodic table, and other metal salts, and are preferably alkali metal salts and salts of metals in Group 2 of the periodic table, more preferably salts of metals in Group 2 of the periodic table, and particularly preferably magnesium salts.
[0143] Examples of alkali metal salts include sodium salts such as sodium chloride, sodium nitrate, and sodium sulfate; potassium salts such as potassium chloride, potassium nitrate, and potassium sulfate; and lithium salts such as lithium chloride, lithium nitrate, and lithium sulfate. Among these, sodium salts are preferred, and sodium chloride and sodium sulfate are particularly preferred.
[0144] Examples of the salt of a metal of Group 2 of the periodic table include magnesium chloride, calcium chloride, magnesium nitrate, calcium nitrate, magnesium sulfate, and calcium sulfate, and preferably calcium chloride and magnesium sulfate.
[0145] Examples of other metal salts include zinc chloride, titanium chloride, manganese chloride, iron chloride, cobalt chloride, nickel chloride, aluminum chloride, tin chloride, zinc nitrate, titanium nitrate, manganese nitrate, iron nitrate, cobalt nitrate, nickel nitrate, aluminum nitrate, tin nitrate, zinc sulfate, titanium sulfate, manganese sulfate, iron sulfate, cobalt sulfate, nickel sulfate, aluminum sulfate, and tin sulfate.
[0146] These coagulants can be used alone or in combination of two or more, and the amount used is usually 0.01 to 100 parts by weight, preferably 0.1 to 50 parts by weight, and more preferably 1 to 30 parts by weight, relative to 100 parts by weight of the monomer component. When the coagulant is in this range, it is preferable because it can sufficiently coagulate the acrylic rubber while highly improving the compression set resistance and water resistance when the acrylic rubber sheet is crosslinked.
[0147] The coagulant concentration of the coagulation liquid used is usually in the range of 0.1 to 20% by weight, preferably 0.5 to 15% by weight, more preferably 1 to 10% by weight, and particularly preferably 1.5 to 5% by weight, which is suitable for concentrating the particle size of the generated hydrous crumbs uniformly in a specific region.
[0148] The temperature of the coagulation liquid is not particularly limited, but when it is usually 40°C or higher, preferably 40 to 90°C, more preferably in the range of 50 to 80°C, uniform water-containing crumbs are preferably formed.
[0149] The contact between the emulsion polymerization liquid and the coagulation liquid is not particularly limited, and examples thereof include a method of adding the emulsion polymerization liquid to the coagulation liquid being stirred, and a method of adding the coagulation liquid to the emulsion polymerization liquid being stirred. The method of adding the emulsion polymerization liquid to the coagulation liquid being stirred is preferable because the shape and diameter of the water-containing crumbs produced can be made uniform and the crumbs can be concentrated in a specific area, thereby significantly improving the washing efficiency of the emulsifier and coagulation agent.
[0150] The stirring speed (rotation speed) of the stirred coagulation liquid, that is, in the present invention, is represented by the rotation speed of the stirring blade of the stirring device provided in the coagulation bath, and is usually 100 rpm or more, preferably 200 to 1,000 rpm, more preferably 300 to 900 rpm, and particularly preferably in the range of 400 to 800 rpm.
[0151] Regarding this rotation speed, a rotation speed at which the coagulation liquid is stirred vigorously to some extent is preferable, since the particle size of the hydrous crumbs produced can be made small and uniform. By setting the rotation speed above the lower limit, the generation of crumbs with excessively large and small particle sizes can be suppressed, and by setting the rotation speed below the upper limit, the coagulation reaction can be more easily controlled.
[0152] The peripheral speed of the stirred coagulation liquid is expressed by the linear speed of the outer circumference of the stirring blade of the stirring device installed in the coagulation bath, and it is preferable to stir vigorously to a certain extent so that the particle size of the water-containing crumbs produced can be made small and uniform, and the peripheral speed is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. On the other hand, the upper limit of the peripheral speed is not particularly limited, but it is preferable that it is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less, because it is easy to control the coagulation reaction.
[0153] By setting the above conditions of the coagulation reaction in the coagulation step (contact method, solids concentration of the emulsion polymerization liquid, concentration and temperature of the coagulation liquid, rotation speed and peripheral speed during stirring of the coagulation liquid, etc.) within specific ranges, the shape and diameter of the generated water-containing crumbs are uniform and concentrated in a specific region, and removal of the emulsifier and coagulant during washing and dehydration is significantly improved, which is preferable.
[0154] (Cleaning process) The washing method is not particularly limited and may be any conventional method, for example, by mixing the produced water-containing crumbs with a large amount of water.
[0155] The amount of water used is not particularly limited, but when the amount of water used per one water wash is usually 50 parts by weight or more, preferably 50 to 15,000 parts by weight, more preferably 100 to 10,000 parts by weight, and particularly preferably 150 to 5,000 parts by weight, relative to 100 parts by weight of the monomer component, it is suitable because the ash content in the acrylic rubber can be effectively reduced.
[0156] The temperature of the water used for washing is not particularly limited, but is usually 40° C. or higher, preferably 40 to 100° C., more preferably 50 to 90° C., and most preferably 60 to 80° C., since this significantly improves the washing efficiency.
[0157] By setting the temperature of the washing water to the lower limit or higher, the emulsifier and coagulant are released from the water-containing crumbs, and the washing efficiency is further improved.
[0158] The washing time is not particularly limited, but is usually in the range of 1 to 120 minutes, preferably 2 to 60 minutes, and more preferably 3 to 30 minutes.
[0159] The number of washings is not particularly limited and is usually 1 to 10 times, preferably multiple times, and more preferably 2 to 3 times. From the viewpoint of reducing the amount of residual coagulant in the finally obtained acrylic rubber sheet, it is desirable to wash with water more frequently, but the number of washings can be significantly reduced by specifying the shape and diameter of the water-containing crumbs and / or setting the washing temperature within the above range.
[0160] (Dehydration, drying, molding process) The dehydrating / drying / molding step in the method for producing an acrylic rubber sheet of the present invention is characterized in that the washed water-containing crumbs are dehydrated in the dehydrating barrel using a dehydrating barrel having a dehydrating slit, a drying barrel under reduced pressure, and a screw-type extruder having a die at the tip thereof to a moisture content of 1 to 40% by weight, and then dried in the drying barrel to a moisture content of less than 1% by weight, and a sheet-like dried rubber is extruded through the die.
[0161] In the present invention, the water-containing crumbs to be supplied to the screw-type extruder are preferably those from which free water has been removed (drained) after washing.
[0162] Draining process In the method for producing an acrylic rubber sheet of the present invention, it is preferable to provide a draining step in which free water is separated from the water-containing crumbs after washing with a draining machine after the above-mentioned washing step and before the dehydrating, drying and molding steps, in order to increase the dehydration efficiency.
[0163] Any known draining machine can be used without any particular limitation, and examples thereof include wire mesh, screens, and electric sifters, with wire mesh and screens being preferred.
[0164] The opening of the drainer is not particularly limited, but is usually in the range of 0.01 to 5 mm, preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm, which is suitable for minimizing loss of water-containing crumb and enabling efficient draining.
[0165] The moisture content of the hydrous crumbs after draining, i.e., the moisture content of the hydrous crumbs input to the dehydration, drying and molding process, is not particularly limited, but is usually in the range of 50 to 80% by weight, preferably 50 to 70% by weight, and more preferably 50 to 60% by weight.
[0166] The temperature of the hydrous crumbs after draining, i.e., the temperature of the hydrous crumbs fed into the dehydrating / drying / molding steps, is not particularly limited, but is usually in the range of 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, particularly preferably 55 to 85°C, and most preferably 60 to 80°C, which is suitable for efficiently dehydrating and drying hydrous crumbs such as the acrylic rubber of the present invention, which has a high specific heat of 1.5 to 2.5 KJ / kg K and is difficult to raise in temperature, in a screw-type extruder.
[0167] Dehydration of crumbs (dehydration barrel section) The dehydration of the hydrous crumb is carried out in a dehydration barrel having a dehydration slit provided in a screw-type extruder. The opening of the dehydration slit may be appropriately selected depending on the conditions of use, but it is usually in the range of 0.01 to 5 mm, preferably 0.1 to 1 mm, more preferably 0.2 to 0.6 mm, which is suitable for minimizing hydrous crumb loss and efficiently dehydrating the hydrous crumb.
[0168] The number of dehydration barrels in the screw extruder is not particularly limited, but it is generally suitable to have multiple barrels, preferably 2 to 10 barrels, and more preferably 3 to 6 barrels, in order to efficiently dehydrate the viscous acrylic rubber.
[0169] There are two ways to remove water from the wet crumb in the dewatering barrel: in liquid form (wastewater) through the dewatering slit, and in vapor form (exhaust steam). In the present invention, the wastewater is defined as dewatering, and the exhaust steam is defined as preliminary drying.
[0170] When a screw-type extruder equipped with a plurality of dehydration barrels is used, a combination of drainage and exhaust steam can be used to efficiently dehydrate the viscous acrylic rubber and reduce its moisture content, which is preferable.Whether each barrel of a screw-type extruder equipped with three or more dehydration barrels is a drainage type dehydration barrel or an exhaust steam type dehydration barrel can be selected appropriately according to the intended use, but generally, when the ash content in the acrylic rubber sheet to be produced is reduced, the number of drainage type barrels is increased, and when the moisture content is reduced, the number of exhaust steam type barrels is increased.
[0171] The set temperature of the dehydration barrel is appropriately selected depending on the monomer composition, ash content, water content, and operating conditions of the acrylic rubber, but is usually in the range of 60 to 150° C., preferably 70 to 140° C., and more preferably 80 to 130° C. The set temperature of the dehydration barrel for dehydration in a drainage state is usually in the range of 60 to 120° C., preferably 70 to 110° C., and more preferably 80 to 100° C. The set temperature of the dehydration barrel for pre-drying in an exhaust steam state is usually in the range of 100 to 150° C., preferably 105 to 140° C., and more preferably 110 to 130° C.
[0172] The moisture content of the crumb after dehydration in the drainage dehydration in which the moisture is squeezed out of the hydrous crumb, i.e., after passing through a drainage dehydration barrel, is not particularly limited, but is usually 1 to 45% by weight, preferably 1 to 40% by weight, more preferably 5 to 35% by weight, particularly preferably 10 to 35% by weight, and most preferably 15 to 35% by weight, which is suitable since it provides a high balance between productivity and ash removal efficiency.
[0173] When sticky acrylic rubber is dehydrated using a centrifuge or the like, the acrylic rubber adheres to the dehydration slits and it is virtually impossible to dehydrate it (the moisture content reaches approximately 45 to 55% by weight). However, in the present invention, by using a screw-type extruder that has a dehydration slit and is forcibly squeezed by a screw, it is possible to reduce the moisture content to this extent.
[0174] When a drainage type dehydration barrel and a steam exhaust type dehydration barrel are provided, the moisture content of the hydrous crumb after dehydration in the drainage type dehydration barrel is usually 5 to 45% by weight, preferably 10 to 40% by weight, and more preferably 15 to 35% by weight, and the moisture content after preliminary drying in the steam exhaust type dehydration barrel is usually 1 to 30% by weight, preferably 3 to 20% by weight, and more preferably 5 to 15% by weight.
[0175] By setting the water content after dehydration to above the lower limit, the dehydration time can be shortened and deterioration of the acrylic rubber can be suppressed, whereas by setting it to below the upper limit, the ash content can be sufficiently reduced.
[0176] Drying of moist crumbs (drying barrel section) The drying of the water-containing crumbs after the dehydration is carried out in a drying barrel under reduced pressure.
[0177] The degree of reduced pressure in the drying barrel may be appropriately selected, but is usually 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa, which is suitable for efficiently drying the water-containing crumbs.
[0178] The set temperature of the drying barrel may be appropriately selected, but is usually suitable within the range of 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C, since this allows efficient drying without discoloration or deterioration of the acrylic rubber and reduces the amount of gel in the acrylic rubber sheet.
[0179] The number of drying barrels in the screw extruder is not particularly limited, but is usually more than one, preferably 2 to 10, more preferably 3 to 8. When there are more than one drying barrels, the degree of reduced pressure may be similar for all drying barrels or may be different. When there are more than one drying barrels, the set temperatures may be similar for all drying barrels or may be different, but it is preferable to make the temperature of the discharge part (closer to the die) higher than the temperature of the introduction part (closer to the dehydration barrel) in order to increase the drying efficiency.
[0180] The water content of the dried rubber after drying is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less. In the present invention, the phenolic antioxidant and the acrylic rubber are melt-kneaded and extruded in a screw-type extruder when the water content of the dried rubber is at this value (in a state where almost all water has been removed), which is particularly preferable since it allows the production of an acrylic rubber sheet with highly improved storage stability and heat resistance. In the present invention, the acrylic rubber is melt-kneaded in a state where almost all water has been removed, which is also preferable since it reduces the amount of gel of the methyl ethyl ketone-insoluble portion of the acrylic rubber sheet and significantly improves the processability of the acrylic rubber sheet.
[0181] Drying rubber (die part) The dried rubber dehydrated and dried in the screw section of the dehydrating barrel and the drying barrel is sent to the screw-free straightening die section. A breaker plate or wire mesh may or may not be provided between the screw section and the die section.
[0182] The dried rubber to be extruded is preferably extruded in a sheet form using a die having a substantially rectangular shape, which results in less air entrapment, a high specific gravity, and excellent storage stability.
[0183] The resin pressure in the die section is not particularly limited, but when it is in the range of usually 0.1 to 10 MPa, preferably 0.5 to 5 MPa, and more preferably 1 to 3 MPa, it is suitable since it reduces air entrainment (high specific gravity) and provides excellent productivity.
[0184] Screw type extruder and operating conditions The screw length (L) of the screw type extruder used may be appropriately selected depending on the purpose of use, but is usually in the range of 3,000 to 15,000 mm, preferably 4,000 to 10,000 mm, and more preferably 4,500 to 8,000 mm.
[0185] The screw diameter (D) of the screw type extruder used may be appropriately selected depending on the purpose of use, but is usually in the range of 50 to 250 mm, preferably 100 to 200 mm, and more preferably 120 to 160 mm.
[0186] The ratio (L / D) of the screw length (L) to the screw diameter (D) of the screw extruder used is not particularly limited, but is usually in the range of 10 to 100, preferably 20 to 80, and more preferably 30 to 60, which is suitable since the moisture content can be reduced to less than 1% by weight without causing a decrease in the molecular weight of the dried rubber or scorching.
[0187] The rotation speed (N) of the screw-type extruder used may be appropriately selected depending on various conditions, but a rotation speed of usually 10 to 1,000 rpm, preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm is suitable because it allows the water content and gel amount of the acrylic rubber to be efficiently reduced.
[0188] The extrusion rate (Q) of the screw extruder used is not particularly limited, but is usually in the range of 100 to 1,500 kg / hr, preferably 300 to 1,200 kg / hr, more preferably 400 to 1,000 kg / hr, and most preferably 500 to 800 kg / hr.
[0189] The ratio (Q / N) of the extrusion rate (Q) to the rotation speed (N) of the screw extruder used is not particularly limited, but is usually in the range of 2 to 10, preferably 3 to 8, and more preferably 4 to 6.
[0190] Dry rubber sheet The dried rubber extruded from the screw extruder is in the form of a sheet, which is preferable because it has a high specific gravity and highly improved storage stability without air being entrained in. The dried rubber sheet extruded from the screw extruder is preferably cut after cooling and used as an acrylic rubber sheet.
[0191] The thickness of the sheet-like dry rubber extruded from the screw extruder is not particularly limited, but is preferably in the range of usually 1 to 40 mm, preferably 2 to 35 mm, more preferably 3 to 30 mm, and most preferably 5 to 25 mm, which is excellent in workability and productivity. In particular, when the thermal conductivity of the sheet-like dry rubber is as low as 0.15 to 0.35 W / mK and the cooling efficiency is increased to significantly improve the productivity, the thickness of the sheet-like dry rubber is usually in the range of 1 to 30 mm, preferably 2 to 25 mm, more preferably 3 to 15 mm, and particularly preferably 4 to 12 mm.
[0192] The width of the sheet-like dry rubber extruded from the screw extruder is appropriately selected depending on the intended use, but is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm.
[0193] The temperature of the dried rubber extruded from the screw extruder is not particularly limited, but is usually in the range of 100 to 200°C, preferably 110 to 180°C, and more preferably 120 to 160°C.
[0194] The moisture content of the dry rubber extruded from the screw-type extruder is not particularly limited, but is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less.
[0195] The complex viscosity at 100°C of the dry rubber sheet extruded from the screw extruder ([η]100°C) is not particularly limited, but is usually in the range of 1,500 to 6,000 Pa·s, preferably 2,000 to 5,000 Pa·s, more preferably 2,500 to 4,000 Pa·s, and most preferably 2,500 to 3,500 Pa·s, which is suitable for achieving a high balance between extrudability as a sheet and shape retention. That is, by setting the viscosity at or above the lower limit, the extrudability can be made superior, and by setting the viscosity at or below the upper limit, deformation or breakage of the dry rubber sheet can be suppressed.
[0196] The sheet-like dried rubber extruded from the screw-type extruder may be folded as it is for use, but is preferably cut for use.
[0197] There are no particular limitations on the cutting of the sheet-like dried rubber, but since the acrylic rubber of the acrylic rubber sheet of the present invention has strong adhesiveness, it is preferable to cool the sheet-like dried rubber before cutting in order to cut it continuously without entraining air.
[0198] The cutting temperature of the dry rubber sheet is not particularly limited, but a temperature of usually 60° C. or less, preferably 55° C. or less, and more preferably 50° C. or less provides a high balance between cuttability and productivity, and is therefore suitable.
[0199] The complex viscosity of the dry rubber sheet at 60°C ([η]60°C) is not particularly limited, but is usually 15,000 Pa·s or less, preferably 2,000 to 10,000 Pa·s, more preferably 2,500 to 7,000 Pa·s, and most preferably 2,700 to 5,500 Pa·s, which allows continuous cutting without entraining air.
[0200] The ratio ([η]100°C / [η]60°C) of the complex viscosity of the dry rubber sheet at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is not particularly limited, but is usually 0.5 or more, preferably 0.6 to 0.98, more preferably 0.75 to 0.95, particularly preferably 0.8 to 0.94, and most preferably 0.83 to 0.93, which is suitable since it reduces air entrapment and provides a high balance between cutting and productivity.
[0201] The cooling method for the dry rubber sheet is not particularly limited, and the sheet may be left at room temperature. However, since the thermal conductivity of the dry rubber sheet is very low at 0.15 to 0.35 W / mK, forced cooling such as air cooling using ventilation or cooling, water spraying by spraying water, or immersion in water is preferred in order to increase productivity, and air cooling using ventilation or cooling is particularly preferred.
[0202] In the air-cooling method of the sheet-like dry rubber, for example, the sheet-like dry rubber is extruded from a screw-type extruder onto a conveyor such as a belt conveyor, and conveyed and cooled while blowing cold air. The temperature of the cold air is not particularly limited, but is usually in the range of 0 to 25°C, preferably 5 to 25°C, and more preferably 10 to 20°C. The length to be cooled is not particularly limited, but is usually in the range of 5 to 500m, preferably 10 to 200m, and more preferably 20 to 100m. The cooling speed of the sheet-like dry rubber is not particularly limited, but is usually 50°C / hr or more, more preferably 100°C / hr or more, and more preferably 150°C / hr or more, which is particularly easy to cut and is therefore suitable.
[0203] The cut length of the dry rubber sheet is not particularly limited and may be appropriately selected depending on the intended use, but is usually in the range of 100 to 800 mm, preferably 200 to 500 mm, and more preferably 250 to 450 mm.
[0204] The acrylic rubber sheet thus obtained is superior in handling and storage stability to crumb-like acrylic rubber, and can be used as is or after lamination into a bale.
[0205] <Acrylic rubber veil> The acrylic rubber veil of the present invention is characterized in that it is formed by laminating and integrating the above-mentioned acrylic rubber sheets. The number of laminations is appropriately selected depending on the size or weight of the acrylic rubber veil.
[0206] The size of the acrylic rubber veil of the present invention is not particularly limited, but the width is usually in the range of 100 to 800 mm, preferably 200 to 500 mm, and more preferably 250 to 450 mm, the length is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm, and the height is usually in the range of 50 to 500 mm, preferably 100 to 300 mm, and more preferably 150 to 250 mm.
[0207] The characteristic values of the acrylic rubber veil of the present invention, namely, reactive group content, water content, ash content, amount and ratio of components in the ash, specific gravity, gel content, pH, complex viscosity at 60°C ([η]60°C), complex viscosity at 100°C ([η]100°C), ratio of complex viscosity at 100°C ([η]100°C) to complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C), and Mooney viscosity (ML1+4,100°C), are the same as the respective characteristic values of the above-mentioned acrylic rubber sheet.
[0208] The method for producing the acrylic rubber veil of the present invention is not particularly limited, but it can be easily produced by cooling the dried sheet-like rubber extruded from the above-mentioned screw-type extruder, cutting it, and then laminating it.
[0209] The lamination temperature of the dry rubber sheet is not particularly limited, but is usually 30° C. or higher, preferably 35° C. or higher, and more preferably 40° C. or higher, which allows air entrapped during lamination to escape. The number of layers may be appropriately selected depending on the size or weight of the acrylic rubber veil. In the acrylic rubber veil of the present invention, the layered dry rubber sheets are integrated by their own weight.
[0210] The acrylic rubber veil of the present invention thus obtained is superior in handling properties as well as in storage stability and water resistance compared to crumb-like acrylic rubber, and the acrylic rubber veil can be used as is or by cutting into the required amount and feeding into a mixer such as a Banbury mixer or roll mixer.
[0211] <Rubber mixture> The rubber mixture of the present invention is characterized in that it is obtained by mixing the acrylic rubber sheet or acrylic rubber veil with a filler and a crosslinking agent.
[0212] The filler is not particularly limited, but examples thereof include reinforcing fillers and non-reinforcing fillers, with reinforcing fillers being preferred.
[0213] Examples of reinforcing fillers include carbon blacks such as furnace black, acetylene black, thermal black, channel black, and graphite; silicas such as wet silica, dry silica, and colloidal silica; etc. Examples of non-reinforcing fillers include quartz powder, diatomaceous earth, zinc oxide, basic magnesium carbonate, activated calcium carbonate, magnesium silicate, aluminum silicate, titanium dioxide, talc, aluminum sulfate, calcium sulfate, barium sulfate, etc.
[0214] These fillers can be used alone or in combination of two or more kinds. The amount of filler to be added is appropriately selected within a range that does not impair the effects of the present invention, and is usually in the range of 1 to 200 parts by weight, preferably 10 to 150 parts by weight, and more preferably 20 to 100 parts by weight, per 100 parts by weight of the acrylic rubber sheet or acrylic rubber veil.
[0215] The crosslinking agent may be appropriately selected according to the type of reactive group contained in the acrylic rubber constituting the acrylic rubber sheet or acrylic rubber veil and the purpose, but is not particularly limited as long as it can crosslink the acrylic rubber sheet or acrylic rubber veil, and for example, conventionally known crosslinking agents such as polyamine compounds such as diamine compounds and carbonates thereof, sulfur compounds, sulfur donors, triazine thiol compounds, polyepoxy compounds, organic ammonium carboxylate salts, organic peroxides, polycarboxylic acids, quaternary onium salts, imidazole compounds, isocyanuric acid compounds, organic peroxides, and triazine compounds can be used. Among these, polyamine compounds, ammonium carboxylate salts, metal dithiocarbamate salts, and triazine thiol compounds are preferred, and hexamethylenediamine carbamate, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, ammonium benzoate, and 2,4,6-trimercapto-1,3,5-triazine are particularly preferred.
[0216] When the acrylic rubber sheet or acrylic rubber veil used is composed of a carboxyl group-containing acrylic rubber, it is preferable to use a polyamine compound or a carbonate thereof as the crosslinking agent. Examples of the polyvalent amine compound include aliphatic polyvalent amine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine; and aromatic polyvalent amine compounds such as 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, and 1,3,5-benzenetriamine. Among these, hexamethylenediamine carbamate, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, and the like are preferred.
[0217] When the acrylic rubber sheet or acrylic rubber veil used is composed of an epoxy group-containing acrylic rubber, examples of the crosslinking agent that can be used include aliphatic polyamine compounds, such as hexamethylenediamine and hexamethylenediamine carbamate, and carbonates thereof; aromatic polyamine compounds, such as 4,4'-methylenedianiline; ammonium carboxylates, such as ammonium benzoate and ammonium adipate; metal dithiocarbamate salts, such as zinc dimethyldithiocarbamate; polycarboxylic acids, such as tetradecanedioic acid; quaternary onium salts, such as cetyltrimethylammonium bromide; imidazole compounds, such as 2-methylimidazole; and isocyanuric acid compounds, such as ammonium isocyanurate. Among these, ammonium carboxylates and metal dithiocarbamate salts are preferred, and ammonium benzoate is more preferred.
[0218] When the acrylic rubber sheet or acrylic rubber veil used is composed of a halogen atom-containing acrylic rubber, it is preferable to use sulfur, a sulfur donor, or a triazine thiol compound as a crosslinking agent. Examples of sulfur donors include dipentamethylene thiuram hexasulfide and triethyl thiuram disulfide. Examples of triazine compounds include 6-trimercapto-s-triazine, 2-anilino-4,6-dithiol-s-triazine, 1-dibutylamino-3,5-dimercaptotriazine, 2-dibutylamino-4,6-dithiol-s-triazine, 1-phenylamino-3,5-dimercaptotriazine, 2,4,6-trimercapto-1,3,5-triazine, and 1-hexylamino-3,5-dimercaptotriazine, and among these, 2,4,6-trimercapto-1,3,5-triazine is preferred.
[0219] These crosslinking agents can be used alone or in combination of two or more, and the amount of the crosslinking agent is usually 0.001 to 20 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight, per 100 parts by weight of the acrylic rubber sheet or acrylic rubber veil. By setting the amount of the crosslinking agent within this range, it is possible to obtain excellent mechanical strength as a crosslinked rubber product while ensuring sufficient rubber elasticity, which is preferable.
[0220] The rubber mixture of the present invention may contain rubber components other than the acrylic rubber sheet or acrylic rubber veil, if necessary.
[0221] Other rubber components used as necessary are not particularly limited, and examples thereof include natural rubber, polybutadiene rubber, polyisoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, silicone rubber, fluororubber, olefin-based elastomer, styrene-based elastomer, vinyl chloride-based elastomer, polyester-based elastomer, polyamide-based elastomer, polyurethane-based elastomer, polysiloxane-based elastomer, etc. The shape of the other rubber components is not particularly limited, and may be, for example, any of powder, pellet, crumb, sheet, veil, etc.
[0222] These other rubber components may be used alone or in combination of two or more. The amount of these other rubber components used is appropriately selected within a range that does not impair the effects of the present invention.
[0223] The rubber mixture of the present invention may contain an antioxidant as required. Examples of the antioxidant include, but are not limited to, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butylphenol, butylhydroxyanisole, 2,6-di-t-butyl-α-dimethylamino-p-cresol, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, styrenated phenol, 2,2'-methylene-bis(6-α-methyl-benzyl-p-cresol), 4,4'-methylenebis( Other phenols such as 2,6-di-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, 2,2'-thiobis-(4-methyl-6-t-butylphenol), 4,4'-thiobis-(6-t-butyl-o-cresol), 2,6-di-t-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, Phenolic antioxidants; phosphorous ester antioxidants such as tris(nonylphenyl)phosphite, diphenylisodecylphosphite, and tetraphenyldipropylene glycol diphosphite; sulfur ester antioxidants such as dilauryl thiodipropionate; phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonylamido)-diphenylamine, and 4,4'-(α,α-dimethylbenzyl)diphenylamine. Examples of the antioxidant include amine-based antioxidants such as amine, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and butyraldehyde-aniline condensate; imidazole-based antioxidants such as 2-mercaptobenzimidazole; quinoline-based antioxidants such as 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline; and hydroquinone-based antioxidants such as 2,5-di-(t-amyl)hydroquinone. Among these, amine-based antioxidants are particularly preferred. The antioxidant used here may be the same as or different from the antioxidant used in the emulsion polymerization step.
[0224] These antioxidants can be used alone or in combination of two or more kinds. The amount of the antioxidant to be added is in the range of 0.01 to 15 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 1 to 5 parts by weight, per 100 parts by weight of the acrylic rubber sheet or acrylic rubber veil.
[0225] The rubber mixture of the present invention contains the above-mentioned acrylic rubber sheet or acrylic rubber veil of the present invention, a filler, a crosslinking agent, and if necessary, other rubber components and antiaging agents, and further, if necessary, other additives normally used in the technical field can be arbitrarily blended, such as crosslinking aids, crosslinking accelerators, crosslinking retarders, silane coupling agents, plasticizers, processing aids, lubricants, pigments, colorants, antistatic agents, foaming agents, etc. These other compounding agents can be used alone or in combination of two or more, and the blending amounts thereof are appropriately selected within a range that does not impair the effects of the present invention.
[0226] <Method of manufacturing rubber mixture> The method for producing the rubber mixture of the present invention includes a method of mixing the acrylic rubber sheet or acrylic rubber veil of the present invention with the filler, crosslinking agent, and the other rubber components, antioxidants, and other compounding ingredients that can be contained as necessary, and any means conventionally used in the field of rubber processing can be used for mixing, such as an open roll, a Banbury mixer, various kneaders, etc. That is, the acrylic rubber sheet or acrylic rubber veil can be used to directly mix, preferably by directly kneading, the filler, crosslinking agent, etc.
[0227] In this case, the acrylic rubber sheet or acrylic rubber veil may be used as is or after being divided (cut, etc.).
[0228] The mixing procedure of each component is not particularly limited, but for example, two-stage mixing is preferred in which components that do not easily react or decompose when heated are thoroughly mixed, and then components that easily react or decompose when heated, such as crosslinking agents, are mixed for a short time at a temperature at which they do not react or decompose. Specifically, it is preferred to mix the acrylic rubber sheet or acrylic rubber veil and the filler in the first stage, and then mix the crosslinking agent in the second stage. Other rubber components and antiaging agents are usually mixed in the first stage, the crosslinking accelerator in the second stage, and other compounding agents may be selected as appropriate.
[0229] The Mooney viscosity (ML1+4, 100°C; compound Mooney) of the rubber mixture of the present invention thus obtained is not particularly limited, but is usually in the range of 10-150, preferably 20-100, more preferably 25-80.
[0230] <Rubber cross-linked products> The cross-linked rubber of the present invention is obtained by cross-linking the above-mentioned rubber mixture.
[0231] The cross-linked rubber product of the present invention can be produced by using the rubber mixture of the present invention, molding it into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, or a roll, and heating it to carry out a cross-linking reaction and fix the shape as a cross-linked rubber product. In this case, cross-linking may be carried out after molding in advance, or may be carried out simultaneously with molding. The molding temperature is usually 10 to 200°C, preferably 25 to 150°C. The cross-linking temperature is usually 100 to 250°C, preferably 130 to 220°C, more preferably 150 to 200°C, and the cross-linking time is usually 0.1 minutes to 10 hours, preferably 1 minute to 5 hours. As the heating method, a method used for cross-linking rubber, such as press heating, steam heating, oven heating, and hot air heating, may be appropriately selected.
[0232] The cross-linked rubber of the present invention may be further heated to carry out secondary cross-linking depending on the shape, size, etc. of the cross-linked rubber. The secondary cross-linking is preferably carried out for 1 to 48 hours, although it varies depending on the heating method, cross-linking temperature, shape, etc. The heating method and heating temperature may be appropriately selected.
[0233] The cross-linked rubber product of the present invention is suitably used, for example, as sealing materials such as O-rings, packings, diaphragms, oil seals, shaft seals, bearing sheaths, mechanical seals, well head seals, seals for electric and electronic devices, and seals for air compressors; various gaskets such as a rocker cover gasket attached to the joint between a cylinder block and a cylinder head, an oil pan gasket attached to the joint between an oil pan and a cylinder head or a transmission case, a gasket for a fuel cell separator attached between a pair of housings that sandwich a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and a gasket for the top cover of a hard disk drive; cushioning materials, vibration-proof materials; wire covering materials; industrial belts; tubes and hoses; sheets; and the like.
[0234] The cross-linked rubber product of the present invention can also be suitably used as extrusion molded products and mold cross-linked products for automotive applications, for example, various hoses such as fuel oil hoses for fuel tanks, such as fuel hoses, filler neck hoses, vent hoses, paper hoses and oil hoses, air hoses, such as turbo air hoses and mission control hoses, radiator hoses, heater hoses, brake hoses and air conditioner hoses.
[0235] <Device configuration used for manufacturing acrylic rubber sheets> Next, the configuration of the equipment used in the production of the acrylic rubber sheet according to one embodiment of the present invention will be described. Fig. 1 is a diagram showing a schematic diagram of an example of an acrylic rubber production system having an equipment configuration used in the production of the acrylic rubber sheet according to one embodiment of the present invention. For example, the acrylic rubber production system 1 shown in Fig. 1 can be used to produce the acrylic rubber sheet according to the present invention.
[0236] The acrylic rubber production system 1 shown in FIG. 1 is composed of an emulsion polymerization reactor, a coagulation device 3, a washing device 4, a draining machine 43, a screw-type extruder 5, a cooling device 6, and a baling device 7, all of which are not shown.
[0237] The emulsion polymerization reactor is configured to carry out the treatment related to the emulsion polymerization step described above. Although not shown in FIG. 1, this emulsion polymerization reactor has, for example, a polymerization reaction tank, a temperature control unit for controlling the reaction temperature, and a stirring device equipped with a motor and a stirring blade. In the emulsion polymerization reactor, the monomer components for forming the acrylic rubber are mixed with water and an emulsifier, emulsified while being appropriately stirred with a stirrer, and emulsion-polymerized in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid. The addition of the phenolic antioxidant or the emulsion containing the phenolic antioxidant to the emulsion polymerization liquid can be carried out directly in the emulsion polymerization reactor. The emulsion polymerization reactor may be any of a batch type, a semi-batch type, and a continuous type, and may be any of a tank type reactor and a tubular type reactor.
[0238] The solidification device 3 shown in Fig. 1 is configured to perform the above-mentioned solidification step. As shown in Fig. 1, the solidification device 3 includes, for example, a stirring tank 30, a heating unit 31 for heating the inside of the stirring tank 30, a temperature control unit (not shown) for controlling the temperature inside the stirring tank 30, a stirring device 34 equipped with a motor 32 and a stirring blade 33, and a drive control unit (not shown) for controlling the number of revolutions and the rotation speed of the stirring blade 33. In the solidification device 3, the emulsion polymerization liquid obtained in the emulsion polymerization reactor is brought into contact with the coagulation liquid and solidified to produce water-containing crumbs.
[0239] In the coagulation device 3, for example, the emulsion polymerization liquid is brought into contact with the coagulation liquid by adding the emulsion polymerization liquid to the coagulation liquid being stirred. That is, the stirring tank 30 of the coagulation device 3 is filled with the coagulation liquid, and the emulsion polymerization liquid is added to and brought into contact with the coagulation liquid to coagulate the emulsion polymerization liquid, thereby generating water-containing crumbs.
[0240] The heating unit 31 of the solidification device 3 is configured to heat the solidification liquid filled in the stirring tank 30. The temperature control unit of the solidification device 3 is configured to control the heating operation by the heating unit 31 while monitoring the temperature in the stirring tank 30 measured by a thermometer, thereby controlling the temperature in the stirring tank 30. The temperature of the solidification liquid in the stirring tank 30 is controlled by the temperature control unit to be usually 40°C or higher, preferably in the range of 40 to 90°C, and more preferably 50 to 80°C.
[0241] The agitator 34 of the solidification device 3 is configured to agitate the solidification liquid filled in the agitation tank 30. Specifically, the agitator 34 includes a motor 32 that generates rotational power, and an agitator blade 33 that spreads in a direction perpendicular to the rotation axis of the motor 32. The agitator blade 33 can cause the solidification liquid filled in the agitation tank 30 to flow by rotating around the rotation axis by the rotational power of the motor 32. The shape, size, and number of the agitator blades 33 to be installed are not particularly limited.
[0242] The drive control unit of the solidification device 3 is configured to control the rotation drive of the motor 32 of the agitation device 34 to set the number of rotations and the rotation speed of the agitation blade 33 of the agitation device 34 to a predetermined value. The rotation of the agitation blade 33 is controlled by the drive control unit so that the agitation speed of the solidification liquid is, for example, usually 100 rpm or more, preferably 200 to 1,000 rpm, more preferably 300 to 900 rpm, and particularly preferably 400 to 800 rpm. The rotation of the agitation blade 33 is controlled by the drive control unit so that the peripheral speed of the solidification liquid is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. Furthermore, the rotation of the agitation blade 33 is controlled by the drive control unit so that the upper limit of the peripheral speed of the solidification liquid is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less.
[0243] The cleaning device 4 shown in Fig. 1 is configured to perform the treatment related to the above-mentioned cleaning step. As shown in Fig. 1, the cleaning device 4 has, for example, a cleaning tank 40, a heating unit 41 that heats the inside of the cleaning tank 40, and a temperature control unit (not shown) that controls the temperature inside the cleaning tank 40. In the cleaning device 4, the water-containing crumbs generated in the solidifying device 3 are mixed with a large amount of water and washed, thereby making it possible to effectively reduce the amount of ash in the finally obtained acrylic rubber sheet.
[0244] The heating unit 41 of the cleaning device 4 is configured to heat the inside of the cleaning tank 40. The temperature control unit of the cleaning device 4 is configured to control the heating operation by the heating unit 41 while monitoring the temperature inside the cleaning tank 40 measured by a thermometer, thereby controlling the temperature inside the cleaning tank 40. As described above, the temperature of the cleaning water inside the cleaning tank 40 is controlled to be usually in the range of 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, and most preferably 60 to 80°C.
[0245] The water-containing crumb washed in the washing device 4 is supplied to a screw-type extruder 5 which performs a dehydration step and a drying step. At this time, the water-containing crumb after washing is preferably supplied to the screw-type extruder 5 through a drainer 43 capable of separating free water. For the drainer 43, for example, a wire net, a screen, an electric sieve, or the like can be used.
[0246] In addition, when the washed wet crumbs are supplied to the screw-type extruder 5, the temperature of the wet crumbs is preferably 40° C. or higher, more preferably 60° C. or higher. For example, the temperature of the water used for washing in the washing device 4 may be set to 60° C. or higher (e.g., 70° C.) so that the temperature of the wet crumbs when supplied to the screw-type extruder 5 can be maintained at 60° C. or higher, or the wet crumbs may be heated to a temperature of 40° C. or higher, preferably 60° C. or higher, when conveyed from the washing device 4 to the screw-type extruder 5. This makes it possible to effectively perform the subsequent dehydration and drying steps, and to significantly reduce the moisture content of the finally obtained dried rubber.
[0247] The screw-type extruder 5 shown in Fig. 1 is configured to perform the processes related to the dehydration step and the drying step described above. Although the screw-type extruder 5 is shown in Fig. 1 as a suitable example, a centrifuge or a squeezer may be used as a dehydrator that performs the process related to the dehydration step, and a hot air dryer, a reduced pressure dryer, an expander dryer, a kneader dryer, etc. may be used as a dryer that performs the process related to the drying step.
[0248] The screw-type extruder 5 is configured to mold the dried rubber obtained through the dehydration process and the drying process into a predetermined shape and discharge it. Specifically, the screw-type extruder 5 is equipped with a dehydration barrel section 53 having a function as a dehydrator for dehydrating the wet crumbs washed in the washing device 4, and a drying barrel section 54 having a function as a dryer for drying the wet crumbs, and further equipped with a die 59 downstream of the screw-type extruder 5 having a molding function for molding the wet crumbs.
[0249] Hereinafter, the configuration of the screw-type extruder 5 will be described with reference to Fig. 2. Fig. 2 shows the configuration of a specific example suitable for the screw-type extruder 5 shown in Fig. 1. By using this screw-type extruder 5, the above-mentioned dehydration and drying process can be suitably carried out.
[0250] The screw-type extruder 5 shown in Fig. 2 is a twin-screw type extrusion dryer having a pair of screws (not shown) in a barrel unit 51. The screw-type extruder 5 has a drive unit 50 that rotates and drives the pair of screws in the barrel unit 51. The drive unit 50 is attached to the upstream end (left end in Fig. 2) of the barrel unit 51. The screw-type extruder 5 also has a die 59 at the downstream end (right end in Fig. 2) of the barrel unit 51.
[0251] The barrel unit 51 has, from the upstream side to the downstream side (from the left side to the right side in FIG. 2), a supply barrel section 52, a dewatering barrel section 53, and a drying barrel section .
[0252] The supply barrel section 52 is made up of two supply barrels, that is, a first supply barrel 52a and a second supply barrel 52b.
[0253] The dehydration barrel section 53 is made up of three dehydration barrels, that is, a first dehydration barrel 53a, a second dehydration barrel 53b, and a third dehydration barrel 53c.
[0254] The drying barrel section 54 is composed of eight drying barrels, namely, a first drying barrel 54a, a second drying barrel 54b, a third drying barrel 54c, a fourth drying barrel 54d, a fifth drying barrel 54e, a sixth drying barrel 54f, a seventh drying barrel 54g, and an eighth drying barrel 54h.
[0255] In this manner, the barrel unit 51 is configured by connecting the divided 13 barrels 52a to 52b, 53a to 53c, and 54a to 54h from the upstream side to the downstream side.
[0256] The screw-type extruder 5 also has heating means (not shown) for individually heating each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h to heat the water-containing crumbs in each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h to a predetermined temperature. The number of heating means corresponds to each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h. As such a heating means, for example, a configuration in which high-temperature steam is supplied from a steam supply means to a steam circulation jacket formed in each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h is adopted, but is not limited thereto. The screw-type extruder 5 also has temperature control means (not shown) for controlling the set temperature of each heating means corresponding to each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h.
[0257] The number of supply barrels, dewatering barrels, and drying barrels constituting each of barrel portions 52, 53, and 54 in barrel unit 51 is not limited to the embodiment shown in FIG. 2, and can be set to a number depending on factors such as the moisture content of the moisture-containing acrylic rubber crumbs to be dried.
[0258] For example, the number of supply barrels installed in supply barrel section 52 is, for example, 1 to 3. The number of dehydration barrels installed in dehydration barrel section 53 is, for example, preferably 2 to 10, and more preferably 3 to 6, since this allows efficient dehydration of the water-containing crumbs of sticky acrylic rubber. The number of drying barrels installed in drying barrel section 54 is, for example, preferably 2 to 10, and more preferably 3 to 8.
[0259] The pair of screws in the barrel unit 51 are rotated by a driving means such as a motor housed in the drive unit 50. The pair of screws extend from the upstream side to the downstream side in the barrel unit 51, and are rotated to convey the wet crumb supplied to the supply barrel section 52 to the downstream side while mixing them. The pair of screws is preferably a twin-shaft intermeshing type in which the peaks and valleys are intermeshed with each other, which can increase the dewatering and drying efficiency of the wet crumb.
[0260] The rotation directions of the pair of screws may be the same or different, but from the viewpoint of self-cleaning performance, it is preferable that the screws rotate in the same direction. The screw shape of the pair of screws is not particularly limited as long as it is a shape required for each of the barrel portions 52, 53, and 54.
[0261] The supply barrel section 52 is a region for supplying the wet crumbs into the barrel unit 51. The first supply barrel 52a of the supply barrel section 52 has a feed port 55 for supplying the wet crumbs into the barrel unit 51.
[0262] The dewatering barrel section 53 is a region where liquid (serum water) containing a coagulant and the like is separated from the water-containing crumbs and discharged.
[0263] The first to third dewatering barrels 53a to 53c constituting the dewatering barrel section 53 each have a dewatering slit 56a, 56b, 56c for discharging moisture from the wet crumb to the outside. A plurality of dewatering slits 56a, 56b, 56c are formed in each of the dewatering barrels 53a to 53c.
[0264] The slit width, i.e., mesh size, of each dewatering slit 56a, 56b, 56c may be appropriately selected depending on the conditions of use, and is typically 0.01 to 5 mm. From the viewpoints of minimizing loss of moist crumb and enabling efficient dewatering of the moist crumb, the width is preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm.
[0265] The removal of moisture from the wet crumb in each of the dehydration barrels 53a to 53c of the dehydration barrel section 53 can be done in two ways: in liquid form through the dehydration slits 56a, 56b, and 56c, and in vapor form. In the dehydration barrel section 53 of this embodiment, the removal of moisture in liquid form is defined as drainage, and the removal of moisture in vapor form is defined as exhaust steam, and are distinguished between these.
[0266] In the dehydration barrel section 53, the combination of drainage and exhaust steam is suitable because it can efficiently reduce the moisture content of the viscous acrylic rubber. In the dehydration barrel section 53, which of the first to third dehydration barrels 53a to 53c is used for drainage or steam exhaust may be appropriately set according to the purpose of use, but when the amount of ash in the acrylic rubber to be produced is usually reduced, it is preferable to increase the number of dehydration barrels for drainage. In that case, for example, as shown in FIG. 2, drainage is performed in the first and second dehydration barrels 53a and 53b on the upstream side, and steam exhaust is performed in the third dehydration barrel 53c on the downstream side. In addition, for example, when the dehydration barrel section 53 has four dehydration barrels, it is possible to consider an embodiment in which drainage is performed in three dehydration barrels on the upstream side and steam exhaust is performed in one dehydration barrel on the downstream side. On the other hand, when the moisture content is reduced, it is preferable to increase the number of dehydration barrels for steam exhaust.
[0267] As described above in the dehydrating / drying process, the set temperature of the dehydrating barrel section 53 is usually in the range of 60 to 150°C, preferably 70 to 140°C, and more preferably 80 to 130°C. The set temperature of the dehydrating barrel for dehydrating in a drainage state is usually in the range of 60 to 120°C, preferably 70 to 110°C, and more preferably 80 to 100°C. The set temperature of the dehydrating barrel for dehydrating in an exhaust steam state is usually in the range of 100 to 150°C, preferably 105 to 140°C, and more preferably 110 to 130°C.
[0268] The drying barrel section 54 is a region where the dehydrated water-containing crumbs are dried under reduced pressure. Among the first to eighth drying barrels 54a to 54h constituting the drying barrel section 54, the second drying barrel 54b, the fourth drying barrel 54d, the sixth drying barrel 54f and the eighth drying barrel 54h each have a vent port 58a, 58b, 58c, 58d for degassing. The vent ports 58a, 58b, 58c, 58d are each connected to a vent pipe (not shown).
[0269] A vacuum pump (not shown) is connected to the end of each vent pipe, and the pressure inside the drying barrel portion 54 is reduced to a predetermined level by operation of the vacuum pumps. The screw-type extruder 5 has a pressure control means (not shown) that controls the operation of the vacuum pumps to control the degree of reduced pressure inside the drying barrel portion 54.
[0270] The degree of reduced pressure in the drying barrel section 54 may be appropriately selected, but as described above, it is usually set to 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa.
[0271] The temperature set within the drying barrel section 54 may be appropriately selected, but as described above, it is usually set to 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C.
[0272] In each of the drying barrels 54a to 54h that make up the drying barrel section 54, the set temperatures in all of the drying barrels 54a to 54h may be similar or different, but it is preferable to set the temperature on the downstream side (die 59 side) higher than the temperature on the upstream side (dehydration barrel section 53 side), as this improves drying efficiency.
[0273] The die 59 is a metal mold disposed at the downstream end of the barrel unit 51, and has an outlet of a predetermined nozzle shape. The acrylic rubber dried in the drying barrel section 54 passes through the outlet of the die 59, and is extruded into a shape corresponding to the predetermined nozzle shape. In the present invention, the acrylic rubber passing through the die 59 can be extruded into a sheet shape by making the nozzle shape of the die 59 approximately rectangular. A breaker plate or a wire mesh may or may not be provided between the screw and the die 59.
[0274] According to the screw-type extruder 5 of this embodiment, the water-containing crumbs of the raw acrylic rubber are extruded into a sheet-like dry rubber in the following manner.
[0275] The hydrous crumbs of the acrylic rubber obtained through the washing process are supplied to the supply barrel section 52 from the feed port 55. The hydrous crumbs supplied to the supply barrel section 52 are transferred from the supply barrel section 52 to the dehydration barrel section 53 by the rotation of the pair of screws in the barrel unit 51. In the dehydration barrel section 53, the hydrous crumbs are dehydrated by draining water contained in the hydrous crumbs and discharging steam from the dehydration slits 56a, 56b, and 56c provided in the first to third dehydration barrels 53a to 53c, respectively, as described above.
[0276] The water-containing crumbs dewatered in the dewatering barrel section 53 are sent to the drying barrel section 54 by the rotation of a pair of screws in the barrel unit 51. The water-containing crumbs sent to the drying barrel section 54 are plasticized and mixed to become a melt, and are transported downstream while generating heat and increasing in temperature. Then, the water contained in the acrylic rubber melt vaporizes, and the water (steam) is discharged to the outside through vent pipes (not shown) connected to each of the vent ports 58a, 58b, 58c, and 58d.
[0277] As described above, by passing through the drying barrel section 54, the water-containing crumb is dried and becomes a molten acrylic rubber. The acrylic rubber is supplied to the die 59 by the rotation of the pair of screws in the barrel unit 51 and is extruded from the die 59 as a sheet-like dried rubber.
[0278] Here, an example of operating conditions for the screw-type extruder 5 according to this embodiment will be given.
[0279] The rotation speed (N) of the pair of screws in barrel unit 51 may be appropriately selected depending on various conditions, and is usually set to 10 to 1,000 rpm. From the viewpoint of efficiently reducing the water content and gel amount in the acrylic rubber sheet, the rotation speed is preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm.
[0280] The extrusion rate (Q) of the acrylic rubber is not particularly limited, but is usually 100 to 1,500 kg / hr, preferably 300 to 1,200 kg / hr, more preferably 400 to 1,000 kg / hr, and most preferably 500 to 800 kg / hr.
[0281] In addition, the ratio (Q / N) of the extrusion amount (Q) of the acrylic rubber to the screw rotation speed (N) is not particularly limited, but is usually 1 to 20, preferably 2 to 10, more preferably 3 to 8, and particularly preferably 4 to 6.
[0282] The cooling device 6 shown in Fig. 1 is configured to cool the dried rubber obtained through the dehydration process using a dehydrator and the drying process using a dryer. As a cooling method using the cooling device 6, various methods can be adopted, including an air-cooling method using blowing air or air conditioning, a water-spraying method in which water is sprayed, and an immersion method in which the rubber is immersed in water. The dried rubber may also be cooled by leaving it at room temperature.
[0283] Hereinafter, as an example of the cooling device 6, a transportable cooling device 60 that cools the dry rubber sheet 10 formed into a sheet will be described with reference to FIG.
[0284] Fig. 3 shows the configuration of a conveyor-type cooling device 60 suitable for use as the cooling device 6 shown in Fig. 1. The conveyor-type cooling device 60 shown in Fig. 3 is configured to cool the sheet-like dry rubber 10 discharged from the discharge port of the die 59 of the screw-type extruder 5 by air cooling while conveying the sheet-like dry rubber 10. By using this conveyor-type cooling device 60, the sheet-like dry rubber discharged from the screw-type extruder 5 can be suitably cooled.
[0285] The conveying cooling device 60 shown in FIG. 3 is used by being directly connected to the die 59 of the screw-type extruder 5 shown in FIG.
[0286] The conveying type cooling device 60 has a conveyor 61 that conveys the sheet-like dried rubber 10 discharged from the die 59 of the screw-type extruder 5 in the direction of arrow A in Figure 3, and a cooling means 65 that blows cold air onto the sheet-like dried rubber 10 on the conveyor 61.
[0287] The conveyor 61 has rollers 62, 63, and a conveyor belt 64 that is wound around the rollers 62, 63 and on which the sheet-like dry rubber 10 is placed. The conveyor 61 is configured to continuously transport the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5 onto the conveyor belt 64 downstream (to the right in FIG. 3).
[0288] The cooling means 65 is not particularly limited, but may be, for example, a means configured to blow cooling air sent from a cooling air generating means (not shown) onto the surface of the sheet-like dried rubber 10 on the conveyor belt 64.
[0289] The length L1 of the conveyor 61 and the cooling means 65 of the transport-type cooling device 60 (the length of the part where cooling air can be blown) is not particularly limited, but is, for example, 10 to 100 m, and preferably 20 to 50 m. The transport speed of the sheet-like dry rubber 10 in the transport-type cooling device 60 may be appropriately adjusted depending on the length L1 of the conveyor 61 and the cooling means 65, the discharge speed of the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5, the target cooling speed and cooling time, and is, for example, 10 to 100 m / hr, and more preferably 15 to 70 m / hr.
[0290] According to the conveying type cooling device 60 shown in Figure 3, the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5 is conveyed by a conveyor 61 while cooling air is blown from a cooling means 65 onto the sheet-like dry rubber 10, thereby cooling the sheet-like dry rubber 10.
[0291] 3, the transportable cooling device 60 is not particularly limited to a configuration including one conveyor 61 and one cooling means 65, but may be configured to include two or more conveyors 61 and two or more corresponding cooling means 65. In that case, the total length of each of the two or more conveyors 61 and the cooling means 65 may be within the above range.
[0292] The baling apparatus 7 shown in Fig. 1 is configured to process the dried rubber that has been extruded from the screw-type extruder 5 and further cooled in the cooling apparatus 6 to produce a bale, which is a block. There are no particular limitations on the weight or shape of the acrylic rubber bales produced by the baling apparatus 7, but for example, an approximately rectangular parallelepiped acrylic rubber bale weighing about 20 kg is produced.
[0293] Furthermore, the sheet-like dried rubber 10 produced by the screw-type extruder 5 may be laminated to produce an acrylic rubber bale. For example, a cutting mechanism for cutting the sheet-like dried rubber 10 may be provided in the baling device 7 disposed downstream of the conveying cooling device 60 shown in FIG. 3. Specifically, the cutting mechanism of the baling device 7 is configured, for example, to continuously cut the cooled sheet-like dried rubber 10 at predetermined intervals to process it into cut sheet-like dried rubber 16 of a predetermined size. By laminating a plurality of cut sheet-like dried rubber 16 cut to a predetermined size by the cutting mechanism, an acrylic rubber bale in which the cut sheet-like dried rubber 16 is laminated can be produced.
[0294] When manufacturing an acrylic rubber veil in which cut sheet-like dry rubber 16 is laminated, it is preferable to laminate cut sheet-like dry rubber 16 at, for example, 40° C. or higher. By laminating cut sheet-like dry rubber 16 at 40° C. or higher, good air release is achieved by further cooling and compression due to its own weight. EXAMPLES
[0295] The present invention will be described in more detail below with reference to examples and comparative examples. In each example, "parts", "%" and "ratio" are by weight unless otherwise specified.
[0296] Various physical properties were evaluated according to the following methods.
[0297] [Monomer composition] Regarding the monomer composition of the acrylic rubber, the monomer composition of each monomer unit in the acrylic rubber was confirmed by H-NMR, and the remaining activity of reactive groups in the acrylic rubber and the content of each reactive group were confirmed by the following test methods.
[0298] The content ratio of each monomer unit in the acrylic rubber was calculated from the amount of each monomer used in the polymerization reaction and the polymerization conversion rate. Specifically, the polymerization reaction was an emulsion polymerization reaction, and the polymerization conversion rate was approximately 100%, with no unreacted monomers being confirmed, so the content ratio of each monomer unit was set to be the same as the amount of each monomer used.
[0299] [Reactive group content] The reactive group content of the acrylic rubber was measured in the acrylic rubber sheet or acrylic rubber veil by the following method. (1) The amount of carboxyl groups was calculated by dissolving an acrylic rubber sheet or acrylic rubber veil in acetone and performing potentiometric titration with a potassium hydroxide solution. (2) The amount of epoxy groups was calculated by dissolving an acrylic rubber sheet or acrylic rubber veil in methyl ethyl ketone, adding a specified amount of hydrochloric acid to it to react with the epoxy groups, and titrating the amount of residual hydrochloric acid with potassium hydroxide. (3) The amount of chlorine was calculated by completely burning an acrylic rubber sheet or acrylic rubber veil in a combustion flask, absorbing the chlorine generated in water, and titrating it with silver nitrate.
[0300] [Anti-aging agent content] The antioxidant content (%) in the acrylic rubber sheet or acrylic rubber veil was calculated based on the calibration curve of the same antioxidant by dissolving the acrylic rubber sheet or acrylic rubber veil in tetrahydrofuran and measuring with gel permeation chromatography (GPC).
[0301] [Ash content] The ash content (%) in the acrylic rubber sheet or acrylic rubber veil was measured in accordance with JIS K6228 Method A.
[0302] [Ash content] The amount (ppm) of each component in the acrylic rubber sheet or acrylic rubber veil ash was measured by pressing the ash sampled during the above ash content measurement onto a titration filter paper with a diameter of 20 mm and subjecting it to XRF measurement using a ZSX Primus (manufactured by Rigaku Corporation).
[0303] [Gel amount] The gel content (%) of the acrylic rubber sheet or acrylic rubber veil is the amount of insoluble matter in methyl ethyl ketone, and was determined by the following method.
[0304] Approximately 0.2 g of the acrylic rubber sheet or acrylic rubber veil was weighed out (Xg), immersed in 100 ml of methyl ethyl ketone and left to stand at room temperature for 24 hours, and then the components insoluble in methyl ethyl ketone were filtered off using an 80 mesh wire screen. The filtrate, i.e., the filtrate in which only the rubber components soluble in methyl ethyl ketone were dissolved, was evaporated, dried and solidified, and the dry solids (Yg) were weighed and calculated using the following formula.
[0305] Gel volume (%) = 100 × (XY) / X
[0306] [specific gravity] The specific gravity of the acrylic rubber sheet or acrylic rubber veil was measured in accordance with JIS K6268 crosslinked rubber - density measurement, method A.
[0307] [Glass transition temperature (Tg)] The glass transition temperature (Tg) of the acrylic rubber was measured using a differential scanning calorimeter (DSC, product name "X-DSC7000", manufactured by Hitachi High-Tech Science Corporation).
[0308] [pH] The pH of the acrylic rubber sheet or acrylic rubber veil was measured with a pH electrode after dissolving 6 g (±0.05 g) of the acrylic rubber sheet or acrylic rubber veil in 100 g of tetrahydrofuran, adding 2.0 ml of distilled water, and confirming complete dissolution.
[0309] [Water content] The water content (%) of the acrylic rubber sheet or acrylic rubber veil was measured in accordance with JIS K6238-1: Oven A (volatile matter measurement) method.
[0310] [Molecular weight and molecular weight distribution] The weight average molecular weight (Mw) and molecular weight distribution (Mz / Mw) of acrylic rubber are absolute molecular weight and absolute molecular weight distribution measured by GPC-MALS method using a solution of dimethylformamide with 0.05 mol / L lithium chloride and 0.01% 37% concentrated hydrochloric acid as a solvent. Specifically, a multi-angle laser light scattering photometer (MALS) and a differential refractometer (RI) were incorporated into a GPC (Gel Permeation Chromatography) device, and the light scattering intensity and refractive index difference of the molecular chain solution size-fractionated by the GPC device were measured over the elution time, and the molecular weight of the solute and its content were calculated sequentially. The measurement conditions and method using the GPC device are as follows. Column: 2 TSKgel α-M (φ7.8mm×30cm, Tosoh Corporation) Column temperature: 40℃ Flow rate: 0.8ml / mm Sample preparation: 5 ml of solvent was added to 10 mg of sample, and the mixture was gently stirred at room temperature (dissolution was visually confirmed).Then, the mixture was filtered using a 0.5 μm filter.
[0311] [Complex viscosity] The complex viscosity η of the acrylic rubber sheet or acrylic rubber veil was measured at 473% strain and 1 Hz using a dynamic viscoelasticity measuring device "Rubber Process Analyzer RPA-2000" (manufactured by Alpha Technology Co., Ltd.) to measure temperature dispersion (40 to 120°C) and obtain the complex viscosity η at each temperature. Here, the dynamic viscoelasticity at 60°C among the dynamic viscoelasticity described above was taken as the complex viscosity η(60°C), and the dynamic viscoelasticity at 100°C was taken as the complex viscosity η(100°C), and the values of η(100°C) / η(60°C) and η(60°C) / η(100°C) were calculated.
[0312] [Storage stability evaluation] The storage stability of the rubber samples was evaluated by placing the rubber mixture of the rubber sample in a constant temperature and humidity chamber at 45°C x 80% RH for 7 days, and then using the rubber sample before and after the test as a rubber mixture, a crosslinking test was performed at 180°C for 10 minutes using a rubber vulcanization tester (Moving Die Rheometer MDR; manufactured by Alpha Technology Co., Ltd.) to calculate the rate of change in crosslink density, which is the difference between the maximum torque (MH) and the minimum torque (ML) (MH-ML), and evaluating it with an index of 100 for Comparative Example 1 (the smaller the index, the better the storage stability).
[0313] [Processability evaluation] The processability of the rubber samples was evaluated by putting the rubber samples into a Banbury mixer heated to 50°C and masticating for 1 minute, then adding compounding ingredient A of the rubber mixture formulation shown in Table 2, and measuring the time until the rubber mixture in the first stage was integrated and showed the maximum torque value, i.e., the Black Incorporation Time (BIT), and evaluating it with an index of 100 for Comparative Example 1 (the smaller the index, the better the processability).
[0314] [Normal state physical property evaluation] The normal physical properties of the rubber samples were evaluated according to the following criteria by measuring the breaking strength, 100% tensile stress and breaking elongation of the cross-linked rubber samples in accordance with JIS K6251. (1) The breaking strength was evaluated as ⊚ when it was 10 MPa or more, and x when it was less than 10 MPa. (2) The 100% tensile stress was evaluated as ⊚ when it was 5 MPa or more, and x when it was less than 5 MPa. (3) The breaking elongation was evaluated as ⊚ when it was 150% or more, and x when it was less than 150%.
[0315] [Preparation of emulsion containing antioxidant] The antioxidant-containing emulsion to be added to the emulsion polymerization liquid after emulsion polymerization was prepared by preparing an emulsion liquid by charging a predetermined amount of water at a predetermined temperature into an adjustment tank with an agitator blade, adding a predetermined amount of emulsifier while stirring, and then adding 1 part of antioxidant to the emulsion and stirring for 2 hours, and measuring the pH, and if the pH was not within the range of 3 to 6, adjusting it to within the range with sulfuric acid or sodium hydroxide, based on the conditions shown in Table 1. The antioxidant-containing emulsion thus prepared was added in its entirety to the emulsion polymerization liquid after emulsion polymerization.
[0316] [Table 1]
[0317] [Example 1] A mixing vessel equipped with a homomixer was charged with 46 parts of pure water, 74.5 parts of ethyl acrylate, 17 parts of n-butyl acrylate, 7 parts of methoxyethyl acrylate, 1.5 parts of mono-n-butyl fumarate, and 1.8 parts of octyloxydioxyethylene phosphate sodium salt as an emulsifier, and the mixture was stirred to obtain a monomer emulsion.
[0318] Next, 170 parts of pure water and 3 parts of the monomer emulsion obtained above were put into a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to 12 ° C. under a nitrogen gas flow. Next, the remaining part of the monomer emulsion, 0.00033 parts of ferrous sulfate, 0.264 parts of sodium ascorbate, and 0.22 parts of potassium persulfate were continuously dropped into the polymerization reaction tank over 3 hours. Thereafter, the reaction was continued while maintaining the temperature inside the polymerization reaction at 23 ° C., and it was confirmed that the polymerization conversion rate reached approximately 100%, and hydroquinone was added as a polymerization terminator to terminate the polymerization reaction, and 1 part of the antioxidant emulsion (IRG1076) listed in Table 1, which was previously prepared as an antioxidant-containing emulsion, was added to obtain an antioxidant-added emulsion polymerization liquid.
[0319] In a coagulation tank equipped with a thermometer and agitator, the emulsion polymerization liquid containing the antioxidant was heated to 80°C and continuously added to a 2% magnesium sulfate aqueous solution (coagulation liquid) that had been heated to 80°C and vigorously stirred (600 rpm: peripheral speed 3.1 m / s), to coagulate the polymer, which was then filtered off to obtain hydrous crumbs.
[0320] Next, 194 parts of hot water (70°C) was added to the coagulation tank and stirred for 15 minutes, after which the water was discharged, and 194 parts of hot water (70°C) was added again and stirred for 15 minutes to wash the wet crumbs. The washed wet crumbs (wet crumb temperature 65°C) were fed to a screw-type extruder, dehydrated and dried, and extruded into a sheet-like dry rubber with a width of 300 mm and a thickness of 10 mm. Next, the sheet-like dry rubber was cooled at a cooling rate of 200°C / hr using a conveying-type cooling device directly connected to the screw-type extruder.
[0321] The screw extruder used in this Example 1 is composed of one supply barrel, three dehydration barrels (first to third dehydration barrels), and five drying barrels (first to fifth drying barrels). The first and second dehydration barrels discharge water, and the third dehydration barrel discharges steam. The operating conditions of the screw extruder were as follows.
[0322] Water content: Moisture content of wet crumbs after draining in the second dewatering barrel: 20% Moisture content of wet crumb after steaming in the third dewatering barrel: 10% Moisture content of wet crumb after drying in the fifth drying barrel: 0.4% Rubber Temperature: Temperature of wet crumbs fed into the first feed barrel: 65℃ -Temperature of rubber discharged from screw extruder: 140℃ Set temperature for each barrel: First dehydration barrel: 90℃ Second dehydration barrel: 100℃ ·Third dehydration barrel: 120℃ ·First drying barrel: 120℃ Second drying barrel: 130℃ ·Third drying barrel: 140℃ ·Fourth drying barrel: 160℃ · Fifth drying barrel: 180℃ Operating conditions: Diameter of the screw in the barrel unit (D): 132mm Total length of the screw in the barrel unit (L): 4620mm Length / Depth:35 - Rotation speed of the screw in the barrel unit: 135 rpm -Rubber extrusion rate from die: 700kg / hr Die resin pressure: 2MPa
[0323] The extruded dry rubber sheet was cooled to 50°C and then cut with a cutter to obtain an acrylic rubber sheet (A). The reactive group content, ash content, ash component content, specific gravity, gel content, glass transition temperature (Tg), pH, antioxidant content, water content, molecular weight, molecular weight distribution, and complex viscosity of the obtained acrylic rubber sheet (A) were measured and are shown in Tables 3-1 and 3-2.
[0324] The obtained acrylic rubber sheets (A) were laminated to obtain 20 parts (20 kg) before the temperature dropped below 40° C., thereby obtaining an acrylic rubber veil (A). The reactive group content, ash content, ash component content, specific gravity, gel content, glass transition temperature (Tg), pH, antioxidant content, water content, molecular weight, molecular weight distribution and complex viscosity of the obtained acrylic rubber veil (A) were measured.
[0325] Next, 100 parts of acrylic rubber veil (A) and compounding ingredient A of "Compound 1" in Table 2 were added using a Banbury mixer and mixed at 50°C for 5 minutes. A processability test was then conducted and the results are shown in Table 3-2. The resulting mixture was then transferred to a roll at 50°C, and compounding ingredient B of "Compound 1" in Table 2 was added and mixed to obtain a rubber mixture. A crosslinking test of the resulting rubber mixture was conducted and the results are shown in Table 3-2. The crosslinking (vulcanization) conditions at this time were 10 minutes at 180°C for the primary vulcanization and 2 hours at 180°C for the secondary vulcanization.
[0326] [Table 2]
[0327] The mixture was laminated to 20 parts (20 kg) before the temperature dropped below 40°C, to obtain an acrylic rubber veil (A). The reactive group content, ash content, ash component content, specific gravity, gel content, glass transition temperature (Tg), pH, antioxidant content, water content, molecular weight, molecular weight distribution, and complex viscosity of the obtained acrylic rubber veil (A) were measured.
[0328] [Example 2] The same procedure as in Example 1 was repeated except that the monomer components were changed to 4.5 parts of ethyl acrylate, 64.5 parts of n-butyl acrylate, 29.5 parts of methoxyethyl acrylate, and 1.5 parts of mono n-butyl fumarate, the emulsifier was changed to nonylphenyloxyhexaoxyethylene phosphate sodium salt, and the antioxidant-containing emulsion was changed to antioxidant emulsion 2. An acrylic rubber sheet (B) and an acrylic rubber veil (B) were obtained and their properties were evaluated. The results for the acrylic rubber sheet (B) are shown in Tables 3-1 and 3-2.
[0329] [Example 3] The same procedure as in Example 1 was carried out except that the monomer components were changed to 48.25 parts of ethyl acrylate, 50 parts of n-butyl acrylate, and 1.75 parts of mono n-butyl fumarate, the emulsifier was changed to tridecyloxyhexaoxyethylene phosphate sodium salt, and the antioxidant-containing emulsion was changed to antioxidant emulsion 3. An acrylic rubber sheet (C) and an acrylic rubber veil (C) were obtained and their properties were evaluated (the compounding ingredients were changed to "Compound 2"). The results for the acrylic rubber sheet (C) are shown in Tables 3-1 and 3-2.
[0330] [Example 4] The temperature of the first dehydration barrel of the screw extruder was changed to 100°C, the temperature of the second dehydration barrel to 120°C, and drainage was performed only in the first dehydration barrel, and the moisture content of the water-containing crumb after drainage in the first dehydration barrel was changed to 30%, but the same procedure as in Example 3 was carried out to obtain an acrylic rubber sheet (D) and an acrylic rubber veil (D), and the properties were evaluated. The results for the acrylic rubber sheet (D) are shown in Tables 3-1 and 3-2.
[0331] [Example 5] The same procedure as in Example 4 was carried out except that the monomer components were changed to 28 parts of ethyl acrylate, 38 parts of n-butyl acrylate, 27 parts of methoxyethyl acrylate, 5 parts of acrylonitrile, and 2 parts of allyl glycidyl ether, and an acrylic rubber sheet (E) and an acrylic rubber veil (E) were obtained and their properties were evaluated (the compounding ingredients were changed to "Compound 3"). The results of the acrylic rubber sheet (E) are shown in Tables 3-1 and 3-2.
[0332] [Example 6] The same procedure as in Example 4 was carried out except that the monomer components were changed to 42.2 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile, and 1.3 parts of vinyl chloroacetate, and an acrylic rubber sheet (F) and an acrylic rubber veil (F) were obtained and their properties were evaluated (the compounding ingredients were changed to "Compound 4"). The results for the acrylic rubber sheet (F) are shown in Tables 3-1 and 3-2.
[0333] [Example 7] The same procedure as in Example 6 was carried out except that the antioxidant-containing emulsion was changed to Anti-Aging Emulsion 4, and an acrylic rubber sheet (G) and an acrylic rubber veil (G) were obtained and their properties were evaluated. The results for the acrylic rubber sheet (G) are shown in Tables 3-1 and 3-2.
[0334] [Example 8] The same procedure as in Example 6 was carried out except that the antioxidant-containing emulsion was changed to Anti-Aging Emulsion 5, and an acrylic rubber sheet (H) and an acrylic rubber veil (H) were obtained and their properties were evaluated. The results for the acrylic rubber sheet (H) are shown in Tables 3-1 and 3-2.
[0335] [Comparative Example 1] A mixing vessel equipped with a homomixer was charged with 46 parts of pure water, 42.2 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile, 1.3 parts of vinyl chloroacetate, 0.709 parts of sodium lauryl sulfate as an emulsifier, and 1.82 parts of polyoxyethylene dodecyl ether (molecular weight 1500), and the mixture was stirred to obtain a monomer emulsion.
[0336] Next, 170 parts of pure water and 3 parts of the monomer emulsion obtained above were put into a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to 12 ° C. under a nitrogen gas flow. Next, the remaining part of the monomer emulsion, 0.00033 parts of ferrous sulfate, 0.264 parts of sodium ascorbate, and 0.22 parts of potassium persulfate were continuously dropped into the polymerization reaction tank over 3 hours. Thereafter, the reaction was continued while maintaining the temperature in the polymerization reaction tank at 23 ° C., and it was confirmed that the polymerization conversion rate reached approximately 100%, and hydroquinone was added as a polymerization terminator to terminate the polymerization reaction, and the anti-aging emulsion 6 shown in Table 1 was added as an anti-aging agent-containing emulsion to obtain an emulsion polymerization liquid containing an anti-aging agent.
[0337] Next, the emulsion polymerization liquid was heated to 80°C, and then 0.7% sodium sulfate aqueous solution (coagulation liquid) was continuously added to coagulate the polymer, which was then filtered to obtain hydrous crumbs. 194 parts of industrial water was added to 100 parts of the obtained hydrous crumbs, and the mixture was stirred at 25°C for 5 minutes, after which the hydrous crumbs were washed 4 times by draining the water from the coagulation tank, and then 194 parts of a sulfuric acid aqueous solution of pH 3 was added and stirred at 25°C for 5 minutes, after which the water was drained from the coagulation tank and acid washed once, and then 194 parts of pure water was added and pure water washed once, and then the mixture was dried in a hot air dryer at 160°C to obtain a crumb-like acrylic rubber (I) with a water content of 0.4% by weight. The properties of the obtained crumb-like acrylic rubber (I) were evaluated and shown in Tables 3-1 and 3-2.
[0338] [Comparative Example 2] A crumb-like acrylic rubber (J) was obtained in the same manner as in Comparative Example 1, except that the antioxidant-containing emulsion was changed to Anti-Age Emulsion 7 in Table 1. The properties of the obtained crumb-like acrylic rubber (J) were evaluated and are shown in Tables 3-1 and 3-2.
[0339] [Table 3-1]
[0340] [Table 3-2]
[0341] From Tables 3-1 and 3-2, it can be seen that the acrylic rubber sheets (A) to (H) made of acrylic rubber having a weight average molecular weight (Mw) of 100,000 to 5,000,000 and a ratio (Mz / Mw) of z-average molecular weight (Mz) to weight average molecular weight (Mw) of 1.3 or more, which contain a (meth)acrylic acid ester of the present invention as a main component, contain a phenol-based antiaging agent, and have a gel amount of 50% by weight or less, have significantly improved storage stability and processability without impairing strength characteristics (Examples 1 to 8).
[0342] As for strength properties, the acrylic rubber sheets (A) to (H) and the crumb-like acrylic rubbers (I) to (J) produced under the conditions of the present examples and comparative examples have weight-average molecular weights (Mw) of absolute molecular weights measured by GPC-MALS exceeding 100,000, and the ratio (Mz / Mw) of the z-average molecular weight (Mz) and weight-average molecular weight (Mw) of the absolute molecular weight distribution with emphasis on the high molecular weight region measured by GPC-MALS exceeds 1.3, so that all of the normal state physical properties including the breaking strength are excellent, and it is understood that the workability and strength of the acrylic rubber sheets (A) to (H) of the present invention are maintained (Examples 1 to 6 and Comparative Example 1). On the other hand, it is also understood from Tables 3-1 and 3-2 that the crumb-like acrylic rubber (I) of Comparative Example 1 has insufficient storage stability and processability, and the crumb-like acrylic rubber (J) of Comparative Example 2 has extremely poor storage stability.
[0343] As for storage stability, since the antioxidant content of the acrylic rubber sheets (A) to (H) is the same as that of the crumb-like acrylic rubber (I), the acrylic rubber sheets (A) to (H) have an overwhelmingly smaller specific surface area and a larger specific gravity than the crumb-like acrylic rubber, and have a structure that does not contain air and is less susceptible to oxidation, and the phenol-based antioxidant is uniformly and finely dispersed in the acrylic rubber sheets (A) to (H), which is thought to be the reason for the difference in storage stability effect (comparison between Examples 1 to 8 and Comparative Example 1). Furthermore, after the storage stability test, no change in color was observed in the acrylic rubber sheets of the present invention, but the crumb-like acrylic sheets (I) to (J) of the Comparative Examples were yellowed.
[0344] Tables 3-1 and 3-2 also show that the storage stability of the acrylic rubber sheets (A) to (H) of the present invention can be significantly improved by making the phenolic antioxidant added to the emulsion polymerization liquid a phenolic antioxidant-containing emulsion containing water and an emulsifier, setting the emulsifier concentration of the phenolic antioxidant-containing emulsion to a predetermined level or higher, and setting the water temperature during emulsion preparation to a predetermined level or higher or equal to or higher than the melting point of the phenolic antioxidant (comparison of Examples 1 to 7 with Example 8).
[0345] Regarding processability, in the present invention, the polymerization conversion rate of emulsion polymerization is increased to improve the strength properties of the sheet, but as the polymerization conversion rate is increased, the amount of gel of methyl ethyl ketone insolubles increases rapidly, worsening the processability of the acrylic rubber, but the gel of methyl ethyl ketone insolubles that has rapidly increased disappears by drying to a state where there is essentially no moisture (water content less than 1%) in the screw-type extruder and melt-kneading it. However, it is difficult to make acrylic rubber, which has a large specific heat and reactive groups, substantially free of moisture, and this can be achieved by adjusting the temperature of the water-containing crumb to be fed and the various conditions of the screw-type extruder, as shown in the examples.
[0346] It is further seen from Tables 3-1 and 3-2 that the acrylic rubber sheets (A) to (H) which contain a phenol-based antioxidant having a specific melting point and have specific ranges for the specific gravity, gel amount, glass transition temperature (Tg), pH, antioxidant content, water content, weight average molecular weight (Mw), ratio of z-average molecular weight (Mz) to weight average molecular weight (Mw) (Mz / Mw), complex viscosity at 100°C η (100°C), complex viscosity at 60°C η (60°C), and ratio of complex viscosities at 100°C and 60°C (η100°C / η60°C) are excellent in storage stability and processability without impairing normal physical properties including strength characteristics (Examples 1 to 8).
[0347] The characteristic values of the acrylic rubber veils (A) to (H) of the present invention formed by laminating the acrylic rubber sheets (A) to (H) were all the same as the characteristic values of each of the acrylic rubber sheets to be laminated. [Explanation of symbols]
[0348] 1 Acrylic rubber manufacturing system 3 Coagulation device 4. Cleaning equipment 5 screw extruder 6 Cooling device 7 Baling Equipment
Claims
1. The acrylic rubber sheet comprises an acrylic rubber having a (meth)acrylic acid ester as a main component, having a reactive group, having a weight average molecular weight (Mw) of 100,000 to 5,000,000 and a ratio (Mz / Mw) of z-average molecular weight (Mz) to weight average molecular weight (Mw) of 1.3 or more, containing a phenol-based antiaging agent, and having a gel amount of methyl ethyl ketone-insoluble matter of 50% by weight or less.
2. 2. The acrylic rubber sheet according to claim 1, which is a melt-kneaded sheet.
3. An acrylic rubber sheet as described in claim 1 or 2, wherein the amount of gel insoluble in methyl ethyl ketone is 15 weight % or less.
4. The acrylic rubber sheet according to any one of claims 1 to 3, wherein the proportion of the acrylic rubber in the acrylic rubber sheet is 85% by weight or more.
5. 5. The acrylic rubber sheet according to claim 1, wherein the ash content in the acrylic rubber sheet is 0.8% by weight or less.
6. 6. The acrylic rubber sheet according to claim 1, wherein the ash contains at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus in an amount of 60% by weight or more.
7. The acrylic rubber sheet according to any one of claims 1 to 6, wherein the phenol-based antioxidant is a hindered phenol-based antioxidant.
8. The acrylic rubber sheet according to any one of claims 1 to 7, wherein the melting point of the phenol-based antioxidant is 150°C or lower.
9. 9. The acrylic rubber sheet according to any one of claims 1 to 8, wherein the molecular weight of the phenol-based antioxidant is in the range of 100 to 1,000.
10. 10. The acrylic rubber sheet according to claim 1, wherein the content of the phenol-based antioxidant is 0.001 to 15% by weight.
11. The acrylic rubber sheet according to any one of claims 1 to 10, having a weight average molecular weight (Mw) in the range of 1,000,000 to 5,000,000.
12. The acrylic rubber sheet according to any one of claims 1 to 11, having a complex viscosity at 60 ° C. ([η] 60 ° C.) of 15,000 Pa · s or less.
13. The acrylic rubber sheet according to any one of claims 1 to 12, wherein the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is 0.5 or more.
14. The acrylic rubber sheet according to any one of claims 1 to 13, which has a pH of 6 or less.
15. The acrylic rubber sheet according to any one of claims 1 to 14, having a specific gravity of 0.7 or more.
16. The acrylic rubber sheet according to any one of claims 1 to 15, having a specific gravity in the range of 0.8 to 1.
4.
17. The acrylic rubber sheet according to any one of claims 1 to 16, wherein the acrylic rubber sheet has a Mooney viscosity (ML1+4, 100°C) in the range of 10 to 150.
18. An emulsion polymerization process in which a monomer component containing a (meth)acrylic acid ester as a main component and a reactive group-containing monomer is emulsified with water and an emulsifier, and emulsion-polymerized in the presence of a polymerization initiator to a polymerization conversion rate of 90% by weight or more to obtain an emulsion polymerization liquid; an antioxidant addition step of adding a phenol-based antioxidant to the obtained emulsion polymerization liquid; a coagulation step of contacting the emulsion polymerization liquid containing the antioxidant with a coagulation liquid to produce water-containing crumbs; A washing step of washing the produced hydrous crumbs; and a dehydrating, drying and molding step of extruding the washed wet crumbs into a sheet-like dry rubber having a water content of less than 1% by weight using a screw-type extruder equipped with a dehydrating barrel having a dehydrating slit, a drying barrel for drying under reduced pressure, and a die at the tip.
19. The method for producing an acrylic rubber sheet according to claim 18, wherein the temperature of the water-containing crumbs fed into the screw-type extruder is 40°C or higher.
20. 20. The method for producing an acrylic rubber sheet according to claim 18 or 19, wherein the phenolic antioxidant to be added is a phenolic antioxidant-containing emulsion emulsified with warm water and an emulsifier.
21. The method for producing an acrylic rubber sheet according to claim 20, wherein the temperature of the hot water is 40°C or higher.
22. The method for producing an acrylic rubber sheet according to claim 20 or 21, wherein the temperature of the hot water is equal to or higher than the melting point of the phenol-based antioxidant used.
23. The method for producing an acrylic rubber sheet according to any one of claims 20 to 22, wherein the emulsifier concentration of the phenol-based antioxidant-containing emulsion is 1% by weight or more.
24. An acrylic rubber veil obtained by laminating the acrylic rubber sheet according to any one of claims 1 to 17.
25. A rubber mixture obtained by mixing the acrylic rubber sheet according to any one of claims 1 to 17 or the acrylic rubber veil according to claim 24 with a filler and a crosslinking agent.
26. A method for producing a rubber mixture, comprising mixing a filler and a crosslinking agent with the acrylic rubber sheet according to any one of claims 1 to 17 or the acrylic rubber veil according to claim 24 using a mixer.
27. A method for producing a rubber mixture, comprising mixing the acrylic rubber sheet according to any one of claims 1 to 17 or the acrylic rubber veil according to claim 24 with a filler, and then mixing a crosslinking agent.
28. A cross-linked rubber product obtained by cross-linking the rubber mixture according to claim 25.
Citation Information
Patent Citations
Method for recovery of polymer and recovering apparatus
JP2004131654A
ACRYLIC RUBBER COMPOSITION AND METHOD FOR MANUFACTURING ACRYLIC RUBBER
JP3599962B2
Acrylic rubber composition and rubber crosslinked product
WO2011093444A1
Method for producing acrylic rubber
WO2018139466A1
Acrylic rubber, acrylic rubber composition, and acrylic rubber crosslinked product
WO2018143101A1