Composite semipermeable membrane
The composite semipermeable membrane with a pleated structure and specific thickness ratios addresses abrasion issues, ensuring high water permeability and durability under pressure.
Patent Information
- Application Number
- JP2022175059
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-22
- Filing Date
- 2022-10-31
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-04-22
AI Technical Summary
Conventional composite semipermeable membranes suffer from degradation due to abrasion during use, particularly when rubbed against channel materials, leading to reduced performance.
A composite semipermeable membrane design featuring a support membrane with a separation functional layer that includes a pleated structure with specific thickness and protrusion ratios, enhancing abrasion resistance and water permeability.
The membrane maintains excellent water permeability and scratch resistance even under high-pressure operation, preventing damage from rubbing against other membranes.
Smart Images

Figure 0007567890000004 
Figure 0007567890000005 
Figure 0007567890000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite semipermeable membrane useful for selectively separating a liquid mixture. The composite semipermeable membrane obtained by the present invention can be suitably used, for example, for desalinizing seawater or brackish water. [Background technology]
[0002] Regarding the separation of mixtures, there are various technologies for removing substances (e.g., salts) dissolved in a solvent (e.g., water), but in recent years, the use of membrane separation methods has expanded as a process for saving energy and resources. Membranes used in membrane separation methods include microfiltration membranes, ultrafiltration membranes, nanofiltration membranes, and reverse osmosis membranes, and these membranes are used, for example, to obtain drinking water from seawater, brackish water, and water containing harmful substances, to produce ultrapure water for industrial use, to treat wastewater, and to recover valuable materials.
[0003] In particular, composite semipermeable membranes having crosslinked polyamide as a separation active layer have been proposed as reverse osmosis membranes and nanofiltration membranes. Methods for producing composite semipermeable membranes having crosslinked polyamide as a separation active layer include a method of polymerization in the presence of an organic additive (Patent Documents 1 and 2), a method of polymerization in the presence of a monofunctional acid halide (Patent Document 3), and a method of polymerization in the presence of a partially hydrolyzed acid halide (Patent Document 4). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 08-224452 [Patent Document 2] Japanese Patent Application Publication No. 6-47260 [Patent Document 3] Japan Special Publication No. 2014-521499 [Patent Document 4] International Publication No. 2010 / 120326 Summary of the Invention [Problem to be solved by the invention]
[0005] Conventional composite semipermeable membranes are generally used in layers, and a flow path material is inserted between the membranes. This causes friction between the membrane and the flow path material or other composite semipermeable membranes during use, which reduces the performance of the membrane, and therefore there is room for improvement in the surface structure of the membrane. The present invention has been made in view of the above, and an object of the present invention is to provide a composite semipermeable membrane which has excellent abrasion resistance and, at the same time, excellent water permeability even during high-pressure operation. [Means for solving the problem]
[0006] In order to achieve the above object, the present invention has the following configuration. [1] A composite semipermeable membrane comprising a support membrane and a separation functional layer provided on the support membrane, the separation functional layer includes a thin film, the thin film forming a pleated structure including a plurality of protrusions having a height of 10 nm or more; A composite semipermeable membrane having a pleated structure, in which the ratio (T100 / T25) of the thickness T25 of the thin film in a region that is 0 to 25% of the height of the protrusions to the thickness T100 of the thin film in a region that is 50 to 100% of the height of the protrusions is less than 0.95. [2] The composite semipermeable membrane according to [1], wherein the thickness T25 of the thin film in a region that is 0 to 25% of the height of the protrusions is 13 nm or more and less than 24 nm. [3] The composite semipermeable membrane according to [2], wherein the actual length L of the thin film per 1 μm length of the support membrane in a cross-sectional direction perpendicular to the membrane surface is 3.0 μm or more. [4] The composite semipermeable membrane according to [3], wherein in the pleated structure, the ratio of the number of protrusions having a height of 200 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 2 or less. [5] The composite semipermeable membrane according to [3] or [4], wherein in the pleated structure, the ratio of the number of protrusions having a height of 400 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 5 or less. Effect of the Invention
[0007] According to the present invention, it is possible to provide a membrane that has excellent abrasion resistance and also exhibits excellent water permeability even during high-pressure operation. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view of a composite semipermeable membrane according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the separation functional layer, and is a schematic diagram showing the pleated structure. [Diagram 3] FIG. 3 is an enlarged cross-sectional view of a protrusion in a pleated structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these in any way. In this specification, "weight" and "mass", and "wt %" and "mass %" are treated as synonyms. A numerical range expressed using "~" means that the range includes the numerical values before and after "~" as the lower and upper limits.
[0010] 1.Composite semipermeable membrane (1-1) Support membrane The support membrane does not substantially have a separation function for ions, etc., and provides strength to the separation functional layer that substantially has a separation function. The size and distribution of the pores of the support membrane are not particularly limited, but it is preferable that the support membrane has, for example, uniform and fine pores, or fine pores that gradually increase in size from the surface on which the separation functional layer is formed to the other surface, and the size of the fine pores on the surface on which the separation functional layer is formed is 0.1 nm to 100 nm.
[0011] The material used for the support membrane and its shape are not particularly limited. For example, the support membrane may be a composite membrane having a substrate 2 and a porous support layer 3 provided on the substrate 2, as shown in FIG. 1, or it may be a membrane consisting of only one layer.
[0012] The substrate may be, for example, a fabric containing at least one material selected from polyester and aromatic polyamide as a main component. As the fabric, a long fiber nonwoven fabric or a short fiber nonwoven fabric can be preferably used.
[0013] The thickness of the substrate is preferably in the range of 10 μm or more and 200 μm or less, and more preferably in the range of 30 μm or more and 120 μm or less.
[0014] The porous support layer may contain at least one polymer selected from the group consisting of, for example, polysulfone; polyethersulfone; polyamide; polyester; cellulosic polymers such as cellulose acetate and cellulose nitrate; vinyl polymers such as polyethylene, polypropylene, polyvinyl chloride and polyacrylonitrile; homopolymers such as polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfone and polyphenylene oxide, and copolymers thereof.
[0015] Among them, polysulfone, cellulose acetate, polyvinyl chloride, or a mixture thereof is preferably used for the porous support layer, and it is particularly preferable to use polysulfone which has high chemical, mechanical and thermal stability.
[0016] The thickness of the porous support layer is preferably in the range of 10 to 200 μm, more preferably in the range of 20 to 100 μm. When the thickness of the porous support layer is 10 μm or more, good pressure resistance can be obtained and a uniform support membrane without defects can be obtained, and a composite semipermeable membrane including such a porous support layer can exhibit good salt removal performance. When the thickness of the porous support layer is 200 μm or less, the amount of unreacted substances remaining during production does not increase, and a decrease in chemical resistance due to a decrease in the amount of permeated water can be prevented.
[0017] In order for the composite semipermeable membrane to have sufficient mechanical strength and packing density, the thickness of the support membrane is preferably in the range of 30 to 300 μm, and more preferably in the range of 50 to 250 μm.
[0018] The morphology of the support membrane can be observed by a scanning electron microscope, a transmission electron microscope, an atomic force microscope, etc. For example, when observing the morphology of the support membrane by a scanning electron microscope, the porous support layer is peeled off from the substrate, and then cut by freeze fracturing to obtain a sample for cross-sectional observation. This sample is thinly coated with preferably platinum, platinum-palladium, or ruthenium tetrachloride, more preferably ruthenium tetrachloride, and observed by a high-resolution field emission scanning electron microscope (UHR-FE-SEM) at an accelerating voltage of 3 to 6 kV.
[0019] The thickness of the substrate, the porous support layer, and the composite semipermeable membrane can be measured by a digital thickness gauge. In addition, since the thickness of the separation functional layer described later is very thin compared to the support membrane, the thickness of the composite semipermeable membrane can also be considered as the thickness of the support membrane. Therefore, the thickness of the composite semipermeable membrane can be measured by a digital thickness gauge, and the thickness of the porous support layer can be calculated simply by subtracting the thickness of the substrate from the thickness of the composite semipermeable membrane. When using a digital thickness gauge, it is preferable to measure the thickness at 20 points and calculate the average value.
[0020] The thickness of the substrate, the porous support layer, and the composite semipermeable membrane may be measured by the above-mentioned microscope. The thickness is measured from an electron microscope photograph of a cross section observed at any five points for one sample, and the thickness is obtained by calculating the average value. Note that the thickness and pore size in this embodiment refer to the average value.
[0021] (1-2) Separation functional layer In the composite semipermeable membrane, it is the separation functional layer that has the substantial ability to separate ions, etc. In the cross-sectional view of the composite semipermeable membrane shown in Fig. 1, the separation functional layer is indicated by the reference numeral "4". In the separation functional layer, the thin film 11 forms a pleated structure including a plurality of protrusions, as shown in Fig. 2.
[0022] The separation functional layer preferably contains polyamide as a main component. In the case of a separation functional layer mainly containing polyamide, the polyamide can be formed, for example, by interfacial polycondensation of a polyfunctional amine and a polyfunctional acid halide. Here, it is preferable that at least one of the polyfunctional amine and the polyfunctional acid halide contains a compound having three or more functional groups.
[0023] The thickness of the separating functional layer is usually within the range of 0.01 to 1 μm, and preferably within the range of 0.1 to 0.5 μm, in order to obtain sufficient separation performance and permeate amount.
[0024] Here, the polyfunctional amine refers to an amine having at least two primary amino groups and / or secondary amino groups in one molecule, at least one of which is a primary amino group. Examples of the polyfunctional amine include aromatic polyfunctional amines such as phenylenediamine, xylylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 3-aminobenzylamine, and 4-aminobenzylamine, in which two amino groups are bonded to a benzene ring at the ortho, meta, or para position, aliphatic amines such as ethylenediamine and propylenediamine, and alicyclic polyfunctional amines such as 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, 4-aminopiperidine, and 4-aminoethylpiperazine.
[0025] Among them, considering the selective separation property, permeability and heat resistance of the membrane, aromatic polyfunctional amines having 2 to 4 primary amino groups and / or secondary amino groups in one molecule are preferable. As such polyfunctional aromatic amines, for example, m-phenylenediamine, p-phenylenediamine, 1,3,5-triaminobenzene, etc. are preferably used. Among them, m-phenylenediamine (hereinafter referred to as m-PDA) is more preferably used because of its easy availability and ease of handling. These polyfunctional amines may be used alone or two or more kinds may be used simultaneously. When two or more kinds are used simultaneously, the above amines may be combined with each other, or the above amine may be combined with an amine having at least two secondary amino groups in one molecule. Examples of amines having at least two secondary amino groups in one molecule include piperazine and 1,3-bispiperidylpropane.
[0026] Polyfunctional acid halide refers to an acid halide having at least two halogenated carbonyl groups in one molecule. For example, trifunctional acid halide can be, for example, trimesic acid chloride, 1,3,5-cyclohexane tricarboxylic acid trichloride, 1,2,4-cyclobutane tricarboxylic acid trichloride, etc., and bifunctional acid halide can be, for example, aromatic bifunctional acid halide such as biphenyl dicarboxylic acid dichloride, azobenzene dicarboxylic acid dichloride, terephthalic acid chloride, isophthalic acid chloride, naphthalenedicarboxylic acid chloride, etc., aliphatic bifunctional acid halide such as adipoyl chloride, sebacoyl chloride, etc., cyclopentane dicarboxylic acid dichloride, cyclohexane dicarboxylic acid dichloride, tetrahydrofuran dicarboxylic acid dichloride, etc., alicyclic bifunctional acid halide can be, for example,
[0027] Considering the reactivity with polyfunctional amine, the polyfunctional acid halide is preferably a polyfunctional acid chloride, and considering the selective separation property and heat resistance of the membrane, it is preferably a polyfunctional aromatic acid chloride having 2 to 4 carbonyl chloride groups in one molecule. Among them, it is more preferable to use trimesoyl chloride as the polyfunctional acid halide from the viewpoint of easy availability and ease of handling. These polyfunctional acid halides may be used alone or in combination of two or more kinds.
[0028] In addition, in the separation functional layer, the thin film forms a pleated structure having multiple recesses and protrusions, and has multiple protrusions with a height of 10 nm or more, as shown in Figure 2. Hereinafter, "protrusion" and "recess" refer to relatively protruding and recessed parts in the thin film, and in particular, the part above (away from the support film) the reference line A described below is called the protrusion, and the part below (towards the support film) is called the recess.
[0029] A "protrusion" refers to the distance from the bottom of a recess to the bottom of the adjacent recess, i.e., from one convex portion to the bottoms of the recesses on both sides of the convex portion. In this specification, a protrusion refers to a protrusion having a height equal to or greater than one-fifth of the 10-point average surface roughness of the thin film.
[0030] In the present embodiment, the separation functional layer preferably has an actual thin film length L of 3.0 μm or more per 1 μm of support membrane length in the cross-sectional direction perpendicular to the membrane surface. When the actual thin film length L is 3.0 μm or more, the composite semipermeable membrane can obtain high water permeability. The actual thin film length L is more preferably 3.0 to 100 μm, and even more preferably 3.0 to 10 μm. In this specification, the term "cross-sectional direction perpendicular to the film surface" means a direction perpendicular to the film surface.
[0031] The actual length L of the thin film can be determined according to a general method for determining a surface area or a specific surface area. The method is not particularly limited, but examples thereof include a method using an electron microscope such as a scanning electron microscope (SEM, FE-SEM) or a transmission electron microscope (TEM).
[0032] An example of a method for measuring the actual length L of a thin film using a transmission electron microscope (TEM) is described below. First, to prepare an ultrathin section for TEM, the sample is embedded in a water-soluble polymer. Any water-soluble polymer can be used as long as it can maintain the shape of the sample, such as PVA.
[0033] Next, to facilitate cross-sectional observation, the sample is stained with OsO4, and cut with an ultramicrotome to prepare ultrathin sections. The obtained ultrathin sections are photographed using an electron microscope. The observation magnification may be appropriately determined depending on the film thickness of the separation functional layer, but in order to observe the cross-sectional shape of the separation functional layer and to prevent the measurement from being localized, if the thickness of the separation functional layer is about 10 to 100 nm, the observation magnification may be set to 50,000 to 100,000 times.
[0034] In any of 10 cross sections of 2.0 μm length in the cross-sectional photograph obtained above, the actual length of the thin film per 1 μm length of the support membrane in the cross-sectional direction perpendicular to the membrane surface is measured, and the arithmetic mean value is calculated as the actual length L of the thin film in the composite semipermeable membrane.
[0035] The ten-point average surface roughness of a thin film can be obtained by the following method. A cross section perpendicular to the film surface is observed using an electron microscope. The observation magnification is preferably 10,000 to 100,000 times. In the obtained cross-sectional image, the surface of the thin film (indicated by the reference symbol "11" in FIG. 2) appears as a curve, as shown in FIG. 2. A roughness curve defined based on ISO4287:1997 is obtained for this curve. The average line of the roughness curve is obtained, also based on ISO4287:1997. The average line is a straight line drawn so that the total area of the region enclosed by the average line and the roughness curve is equal above and below the average line.
[0036] In the image with a length of 2.0 μm in the direction of the average line obtained above, as shown in FIG. 2, the average line is set as a reference line A, and for the five convex parts from the highest convex part to the fifth highest, heights from the reference line (distances from the reference line to the apex of the convex part) H1 to H5 are measured and their average value is calculated. In addition, for the five concave parts from the deepest concave part to the fifth deepest, depths (distances from the reference line to the apex of the concave part) D1 to D5 are measured and their average value is calculated. The sum of the two average values obtained is the 10-point average surface roughness. The apex is the point on the convex part or concave part that is the greatest distance from the reference line.
[0037] The height of a protrusion is calculated as follows: For a protrusion that is at least one-fifth of the above-mentioned 10-point average surface roughness in a cross section 2.0 μm long in the direction of the above-mentioned average line, the sum of the average d of the depths d1 and d2 of the recesses on either side of the protrusion (the distance from the reference line to the apex of the recess) and the height h of the protrusion (the distance from the reference line to the apex of the protrusion) is calculated as the height Ph of the protrusion.
[0038] In the composite semipermeable membrane of the present embodiment, in any 10 cross sections having a length of 2.0 μm in the direction of the above-mentioned average line, the ratio (N / M) of the number N of protrusions having a height of 200 nm or more present on the 10 cross sections to the number M of protrusions having a height of 10 nm or more present on the 10 cross sections is preferably 1 / 20 or more and 1 / 2 or less. When N / M is 1 / 20 or more, the composite semipermeable membrane can obtain high water permeability. N / M is more preferably 1 / 10 or more. In addition, when N / M is 1 / 2 or less, high water permeability can be obtained while maintaining a high removal rate. N / M is more preferably 1 / 3 or less.
[0039] The total number of protrusions present in 10 cross sections means the sum of the number of protrusions contained in each cross section in all 10 cross sections and the total number of protrusions found in each cross section for all 10 cross sections.
[0040] It is also preferable that all protrusions present in any 10 cross sections having a length of 2.0 μm in the direction of the mean line have at least one protrusion with a height of 400 nm or more. It is also more preferable that the ratio (N1 / M) of the number of protrusions with a height of 400 nm or more present in the 10 cross sections N1 to the number of protrusions with a height of 10 nm or more present in the 10 cross sections M is 1 / 20 or more and 1 / 5 or less. By having protrusions with a height of 400 nm or more in the above range, high water permeability is obtained.
[0041] The height of the protrusions is preferably 70 nm or more, more preferably 90 nm or more. The height of the protrusions is preferably 1000 nm or less, more preferably 800 nm or less. When the height of the protrusions is 70 nm or more, a composite semipermeable membrane with sufficient water permeability can be easily obtained. When the height of the protrusions is 1000 nm or less, the protrusions are not crushed even when the composite semipermeable membrane is operated and used at high pressure, and stable membrane performance can be obtained.
[0042] The thickness of the thin film can be measured by TEM. The preparation of ultrathin sections for TEM is as described in the description of the measurement of the actual length L of the thin film. The cross section of the obtained ultrathin section is photographed by TEM. The observation magnification may be appropriately determined depending on the thickness of the separation functional layer. The obtained cross-sectional photograph can be analyzed using image analysis software.
[0043] The thickness of the thin film at the upper part and the lower part of the protrusion in the pleated structure is obtained as follows. As shown in FIG. 3, the average value d of the depths d1 and d2 from the reference line A to the apex of the recess on both sides of the protrusion is calculated. Below the reference line A (on the support membrane side), the position at a distance d from the reference line A is set to 0% height, and the apex of the protrusion is set to 100% height, and the thickness of the thin film is measured at 10 points in the region of 0 to 25% height and the region of 50 to 100% height. The same measurement is performed for five protrusions. The arithmetic mean value is calculated for the values of the thin film thickness at 50 points in the region of 0 to 25% height. This value is the lower thickness T25 of the thin film in the composite semipermeable membrane. The arithmetic mean value is also calculated in the same manner for the thickness of the thin film in the region of 50 to 100% height, and this is set to the upper thickness T100 of the thin film.
[0044] The lower thickness T25 is preferably 13 nm or more and less than 24 nm. When the lower thickness T25 is 13 nm or more, the composite semipermeable membrane can maintain its pleated structure even when operated and used at high pressure, so that the water permeability and salt rejection rate can be maintained. T25 is more preferably 14 nm or more, and even more preferably 16 nm or more. Furthermore, when T25 is less than 24 nm, sufficient water permeability can be maintained while ensuring a high salt rejection rate. T25 is more preferably 23 nm or less, and even more preferably 21 nm or less.
[0045] In the pleated structure of this embodiment, the ratio of the upper thickness T100 to the lower thickness T25 (T100 / T25) is less than 0.95. T100 / T25 is preferably 0.92 or less, more preferably 0.90 or less, and even more preferably 0.87 or less. Moreover, T100 / T25 is preferably 0.70 or more, more preferably 0.72 or more, and even more preferably 0.75 or more.
[0046] Composite semipermeable membranes are generally used in layers, with, for example, a flow path material inserted between the composite semipermeable membranes. When T100 / T25 satisfies the above range, the upper part of the protrusion is relatively thinner and more flexible than the lower part, and the lower part is thicker and stronger than the upper part, so that even if the protrusion rubs against the flow path material or another composite semipermeable membrane during use of the composite semipermeable membrane, the force field is dispersed to the lower part, reducing damage.
[0047] In particular, when T100 / T25 is less than 0.95 and T25 is preferably 13 nm or more, even if the protrusions of the thin film rub against the flow path material or another composite semipermeable membrane during use of the composite semipermeable membrane, damage to the lower parts of the protrusions and collapse of the pleated structure can be further suppressed.
[0048] 2. Manufacturing method An example of a method for producing the composite semipermeable membrane of the present embodiment described above will be described below. (2-1) Formation of separation functional layer The process of forming a separation functional layer on a support membrane will be described. In the following, an example will be given in which the support membrane has a substrate and a porous support layer. When the support membrane does not include a substrate, the "porous support layer surface" and "on the porous support layer" can be read as the "support membrane surface" and "on the support membrane", respectively.
[0049] The step of forming the separation functional layer includes a step of contacting a polyfunctional amine solution with a polyfunctional acid halide solution on the porous support layer to form a polyamide by an interfacial polycondensation reaction. More specifically, the step of forming the separation functional layer includes the steps of: (i) contacting a porous support layer with a multifunctional amine solution; (ii) After the above (i), the method includes a step of contacting the porous support layer with an organic solvent solution containing a polyfunctional acid halide to produce a polyamide on the porous support layer by interfacial polycondensation. Each production step will be described in detail below.
[0050] The polyfunctional amine solution is an aqueous solution, and the polyfunctional amine concentration in this solution is preferably in the range of 0.1 to 20% by weight, more preferably in the range of 0.5 to 15% by weight. When the polyfunctional amine concentration is in this range, a composite semipermeable membrane having sufficient salt removal performance and water permeability can be obtained.
[0051] The aqueous polyfunctional amine solution may contain a surfactant, an organic solvent, an alkaline compound, an antioxidant, and the like, so long as they do not interfere with the reaction between the polyfunctional amine and the polyfunctional acid halide.
[0052] Examples of the surfactant include compounds having a polyoxyalkylene structure, a fatty acid ester structure, or a hydroxyl group. Examples of the polyoxyalkylene structure include -(CH2CH2O) n -, -(CH2CH2(CH3)O) n -, -(CH2CH2CH2O) n -, -(CH2CH2CH2CH2O) n - and the like. Examples of the fatty acid ester structure include fatty acids having a long-chain aliphatic group. The long-chain aliphatic group may be either linear or branched, and examples of the fatty acid include stearic acid, oleic acid, lauric acid, palmitic acid, and salts thereof. Examples of fatty acid esters derived from fats and oils include beef tallow, palm oil, coconut oil, and the like. Examples of surfactants having a sulfo group include 1-hexanesulfonic acid, 1-octanesulfonic acid, 1-decanesulfonic acid, 1-dodecanesulfonic acid, perfluorobutanesulfonic acid, toluenesulfonic acid, cumenesulfonic acid, and octylbenzenesulfonic acid. Examples of surfactants having a hydroxyl group include ethylene glycol, propylene glycol, 2-propanediol, 1,4-butanediol, glycerin, sorbitol, glucose, and sucrose. The surfactant has the effect of improving the wettability of the porous support layer surface and reducing the interfacial tension between the amine aqueous solution and the nonpolar solvent.
[0053] Examples of the organic solvent include linear amide compounds and cyclic amide compounds. Examples of the linear amide compounds include N-methylformamide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, and N,N-diethylacetamide. Examples of the cyclic amide compounds include N-methylpyrrolidinone, γ-butyrolactam, and ε-caprolactam. The organic solvent may act as a catalyst for the interfacial polycondensation reaction, and the addition of the organic solvent may allow the interfacial polycondensation reaction to be carried out efficiently.
[0054] Examples of alkaline compounds include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, inorganic carbonates and bicarbonates such as sodium carbonate, sodium bicarbonate, potassium carbonate and potassium bicarbonate, and organic compounds such as tetramethylammonium hydroxide and tetraethylammonium hydroxide.
[0055] Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. Examples of the phenol-based antioxidants (including hindered phenol-based antioxidants) include 2,6-di-tert-butyl-4-methylphenol, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), and tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane. Examples of the amine-based antioxidants include phenyl-β-naphthylamine, α-naphthylamine, N,N'-di-sec-butyl-p-phenylenediamine, phenothiazine, and N,N'-diphenyl-p-phenylenediamine.
[0056] Examples of sulfur-based antioxidants include dilauryl 3,3'-thiodipropionate, distearyl thiodipropionate, lauryl stearyl thiodipropionate, and dimyristyl 3,3'-thiodipropionate. Examples of phosphorus-based antioxidants include triphenyl phosphite, octadecyl phosphite, and trinonylphenyl phosphite. Examples of other antioxidants include ascorbic acid or an alkali metal salt thereof, sterically hindered phenolic compounds such as dibutylhydroxytoluene and butylhydroxyanisole, isopropyl citrate, dl-α-tocopherol, nordihydroguaiaretic acid, and propyl gallate.
[0057] The contact of the aqueous polyfunctional amine solution with the porous support layer is preferably carried out uniformly and continuously on the surface of the porous support layer.Specific examples of the method include a method of applying the aqueous polyfunctional amine solution to the porous support layer, or a method of immersing the porous support layer in the aqueous polyfunctional amine solution.The contact time between the porous support layer and the aqueous polyfunctional amine solution is preferably within a range of 1 to 10 minutes, and more preferably within a range of 1 to 3 minutes.
[0058] After the polyfunctional amine aqueous solution is brought into contact with the porous support layer, it is preferable to thoroughly drain the solution so that no droplets remain on the membrane. By thoroughly draining the solution, it is possible to prevent the remaining droplets from becoming membrane defects after membrane formation, which leads to a decrease in membrane performance. As a method for draining the solution, for example, as described in Japanese Patent Application Laid-Open No. 2-78428, a method in which the support membrane after contact with the polyfunctional amine aqueous solution is held vertically to allow excess aqueous solution to flow naturally, or a method in which an air current such as nitrogen is blown from an air nozzle to forcibly drain the solution can be used. In addition, after draining, the membrane surface can be dried to remove some of the water content of the aqueous solution.
[0059] Step (ii) will now be described. Step (ii) is a step of producing a polyamide on the porous support layer by contacting the porous support layer with a polyfunctional acid halide or an organic solvent solution containing a polyfunctional acid halide through interfacial polycondensation.
[0060] In step (ii), a layer of the polyfunctional acid halide solution is formed on the layer of the aqueous amine solution on the porous support layer formed in step (i). The method of contacting the polyfunctional acid halide solution with the porous support layer includes coating or dripping. Hereinafter, "coating" includes other contact methods unless otherwise specified.
[0061] The concentration of the polyfunctional acid halide in the organic solvent solution is preferably within the range of 0.01 to 10% by weight, more preferably within the range of 0.02 to 2.0% by weight. By setting the concentration of the polyfunctional acid halide to 0.01% by weight or more, a sufficient reaction rate can be obtained, and by setting the concentration to 10% by weight or less, the occurrence of side reactions can be suppressed.
[0062] The organic solvent is preferably one that is immiscible with water, dissolves the polyfunctional acid halide, and does not destroy the support film, and is inactive against the polyfunctional amine compound and the polyfunctional acid halide. Preferred examples of the organic solvent include hydrocarbon compounds such as n-hexane, n-octane, n-nonane, n-decane, n-undecane, n-dodecane, isodecane, and isododecane.
[0063] The polyfunctional acid halide solution preferably further contains water. In addition, it is preferable to provide a concentration gradient in the layer of the polyfunctional acid halide solution formed on the layer of the aqueous amine solution on the porous support layer, in which the water content decreases closer to the porous support layer. When the polyfunctional acid halide solution contains water and the water content in the layer of the polyfunctional acid halide solution has the above-mentioned gradient, the upper and lower thicknesses of the thin film in the pleated structure can be changed. As a result, the abrasion resistance of the composite semipermeable membrane can be improved, and a composite semipermeable membrane having both abrasion resistance and water permeability can be obtained.
[0064] The method for forming a concentration gradient in the water content of the layer of the multifunctional acid halide solution is not limited to a specific form, but for example, a multifunctional acid halide solution with a low water content (first multifunctional acid halide solution) may be first applied to the porous support layer, and then a multifunctional acid halide solution with a high water content (second multifunctional acid halide solution) may be applied.
[0065] The water content of the first polyfunctional acid halide solution is preferably 500 ppm or less. By making the water content of the first polyfunctional acid halide solution 500 ppm or less, the reactivity with amine is improved, and the lower thickness of the thin film can be increased. The water content of the first polyfunctional acid halide solution is more preferably 200 ppm or less, and even more preferably 150 ppm or less. In addition, the water content of the first polyfunctional acid halide solution is preferably greater than 0 ppm, more preferably 5 ppm or more, and even more preferably 40 ppm or more.
[0066] The water content of the second polyfunctional acid halide solution is preferably more than that of the first polyfunctional acid halide solution and is 500 ppm or less, more preferably 300 ppm or less, and even more preferably 150 ppm or less. The water content of the second polyfunctional acid halide solution is preferably more than that of the first polyfunctional acid halide solution and is 0 ppm or more, more preferably 20 ppm or more, and even more preferably 40 ppm or more.
[0067] The number of times that the polyfunctional acid halide solution is applied to the porous supporting layer is preferably from 2 to 6 times, and more preferably 2 times.
[0068] More preferably, the polyfunctional acid halide solution contains a compound represented by the following chemical formula (I) (hereinafter, referred to as compound (I)).
[0069] [ka]
[0070] In the above formula, R1 and R2 are each independently an alkyl group having one or more carbon atoms.
[0071] Compound (I) is preferably an aromatic ester, and particularly preferably a phthalate ester.Specific examples of phthalate ester include dibutyl phthalate, dibutylbenzyl phthalate, diethylhexyl phthalate, diisodecyl phthalate, diisonoyl phthalate, dioctyl phthalate, diisobutyl phthalate, diethyl phthalate, dimethyl phthalate, diisooctyl phthalate, dipropyl phthalate, dicyclohexyl phthalate, dinonyl phthalate, dipentyl phthalate, dihexyl phthalate, dibenzyl phthalate, diphenyl phthalate, and bis(2-ethylhexyl) phthalate.
[0072] By incorporating compound (I) into the polyfunctional acid halide solution, it is possible to increase the actual length of the thin film in the separation functional layer and to increase the thickness of the thin film, thereby achieving both the water permeability and salt rejection properties of the composite semipermeable membrane.
[0073] Although the details of the action of compound (I) are unknown, it is believed that in the interfacial polycondensation of a polyfunctional amine and a polyfunctional acid halide, when the amine diffuses from the polyfunctional amine aqueous solution side to the organic solvent containing the polyfunctional acid halide side, the presence of compound (I) makes the amine concentration gradient gentler, resulting in a sufficiently long formation time for the protrusions of the separation functional layer, making it easier for the protrusion structure to form, and increasing both the surface area and thickness of the protrusions.
[0074] Furthermore, when forming the separation functional layer, it is preferable that the polyfunctional acid halide solution to which the compound (I) is added further contains water, which causes the concentration gradient from the amine aqueous solution side to the polyfunctional acid halide solution side to vary in the membrane surface direction, and therefore the height and angle of the protrusions are also changed.
[0075] The concentration of compound (I) in the polyfunctional acid halide solution can be changed depending on the type of compound (I) to be added, but is preferably within the range of 5 ppm to 500 ppm. It is also preferable to add 10 ppm or more of water to the polyfunctional acid halide solution.
[0076] The polyfunctional acid halide solution may further contain, as an additive, a monofunctional acid halide or trimesoyl chloride in which one acid chloride group has been hydrolyzed (hereinafter, monohydrolyzed TMC), or trimesoyl chloride in which two acid chloride groups have been hydrolyzed (hereinafter, dihydrolyzed TMC).
[0077] Examples of the monofunctional acid halide include at least one compound selected from the group consisting of benzoyl fluoride, benzoyl chloride, benzoyl bromide, methanoyl fluoride, methanoyl chloride, methanoyl bromide, ethanoyl fluoride, ethanoyl chloride, ethanoyl bromide, propanoyl fluoride, propanoyl chloride, propanoyl bromide, propenoyl fluoride, propenoyl chloride, propenoyl bromide, butanoyl fluoride, butanoyl chloride, butanoyl bromide, butenoyl fluoride, butenoyl chloride, and butenoyl bromide.
[0078] The temperature of the membrane surface immediately after contacting the polyfunctional amine aqueous solution with the polyfunctional acid halide solution is preferably within the range of 25 to 60°C, more preferably within the range of 30 to 50°C. By setting the membrane surface temperature at 25°C or higher, the pleated structure in the separation functional layer becomes larger, improving the permeation flux. In addition, by setting the membrane surface temperature at 60°C or lower, a composite semipermeable membrane with a high rejection rate can be obtained.
[0079] The method of applying temperature to the membrane surface may be to heat the support membrane or to contact the membrane with a heated organic solvent solution of the polyfunctional acid halide. The temperature of the membrane surface immediately after contacting the aqueous polyfunctional amine solution with the polyfunctional acid halide solution can be measured by a non-contact thermometer such as a radiation thermometer.
[0080] As described above, after contacting the organic solvent solution of the polyfunctional acid halide to carry out interfacial polycondensation and forming a separation functional layer containing a crosslinked polyamide on the porous support layer, it is advisable to drain off the excess solvent. For example, the method of draining can be a method of holding the membrane vertically and removing the excess organic solvent by gravity. In this case, the time for holding vertically is preferably 1 to 5 minutes, more preferably 1 to 3 minutes. If this time is 1 minute or more, a sufficient amount of polyamide can be formed as the separation functional layer, and if it is 5 minutes or less, the organic solvent does not evaporate too much, and the occurrence of defects in the membrane can be suppressed.
[0081] (2-2) Formation of the support membrane The support film may be a commercially available filter. Alternatively, a support film having a substrate and a porous support layer may be formed by applying a polymer solution onto a substrate and then solidifying the polymer, or by applying a polymer solution onto a substrate such as glass, then solidifying the polymer, and peeling the polymer off from the substrate.
[0082] For example, when forming a support membrane using polysulfone, polysulfone is dissolved in N,N-dimethylformamide (hereinafter referred to as DMF) to obtain a polymer solution, which is applied to a substrate to a certain thickness and then wet-coagulated in water. This method makes it possible to obtain a porous support layer in which most of the surface has fine pores with diameters of several tens of nanometers or less.
[0083] (2-3) Other processing The composite semipermeable membrane after the separation functional layer is formed can have improved salt removal performance and water permeability by adding a process of hot water treatment at preferably 50 to 150°C, more preferably 70 to 130°C, preferably for 1 second to 10 minutes, more preferably 1 minute to 8 minutes.
[0084] In addition, the salt rejection rate can be further improved by including a step of contacting the composite semipermeable membrane with a compound (A) that reacts with a primary amino group on the separation functional layer after the hot water treatment to produce a diazonium salt or a derivative thereof, and then contacting it with a water-soluble compound (B) that is reactive with the compound (A).
[0085] Examples of the compound (A) that reacts with a primary amino group to generate a diazonium salt or a derivative thereof include aqueous solutions of nitrous acid and its salts, nitrosyl compounds, etc. Since aqueous solutions of nitrous acid and nitrosyl compounds generate gas and are easily decomposed, it is preferable to sequentially generate nitrous acid, for example, by reacting a nitrite with an acidic solution. In general, nitrite reacts with hydrogen ions to generate nitrous acid (HNO2), which can be efficiently generated when the pH of the aqueous solution is preferably 7 or less, more preferably 5 or less, and even more preferably 4 or less. Among these, an aqueous solution of sodium nitrite reacted with hydrochloric acid or sulfuric acid in an aqueous solution is particularly preferable from the viewpoint of ease of handling.
[0086] When the compound (A) that reacts with the primary amino group to generate a diazonium salt or a derivative thereof is, for example, sodium nitrite, the concentration of sodium nitrite is preferably in the range of 0.01 to 1% by weight. When the sodium nitrite is within the above range, the effect of generating a sufficient diazonium salt or a derivative thereof is obtained, and the solution is easy to handle.
[0087] The temperature of the compound is preferably 15° C. to 45° C. If the temperature of the compound is within the above range, the reaction does not take too much time, and the decomposition of nitrous acid is not too rapid, making the compound easy to handle.
[0088] The contact time between the primary amino group and the compound may be long enough to generate a diazonium salt and / or its derivative, and while a short contact time is possible at high concentrations, a long contact time is required at low concentrations. Therefore, in the above-mentioned solution, the contact time is preferably within 10 minutes, more preferably within 3 minutes.
[0089] The method of contacting the primary amino group with the compound is not particularly limited, and the compound may be applied (coated) in a solution, or the composite semipermeable membrane may be immersed in the compound solution. Any solvent may be used to dissolve the compound, as long as the compound dissolves and the composite semipermeable membrane is not eroded. The compound solution may contain a surfactant, an acidic compound, an alkaline compound, or the like, as long as it does not interfere with the reaction between the primary amino group and the reagent.
[0090] Next, the composite semipermeable membrane in which the diazonium salt or its derivative is produced is contacted with a water-soluble compound (B) that reacts with the diazonium salt or its derivative. Examples of the water-soluble compound (B) that reacts with the diazonium salt or its derivative include chloride ions, bromide ions, cyanide ions, iodide ions, fluoroboric acid, hypophosphorous acid, sodium hydrogen sulfite, sulfite ions, aromatic amines, phenols, hydrogen sulfide, and thiocyanic acid.
[0091] When reacted with sodium hydrogen sulfite and sulfite ions, a substitution reaction occurs instantly, and amino groups are replaced with sulfo groups. In addition, when contacted with aromatic amines and phenols, a diazo coupling reaction occurs, making it possible to introduce aromatics onto the membrane surface. These compounds may be used alone or in combination, or may be contacted with different compounds multiple times. The compounds to be contacted are preferably sodium hydrogen sulfite and sulfite ions.
[0092] The concentration and time of contacting the water-soluble compound (B) that reacts with a diazonium salt or a derivative thereof with the composite semipermeable membrane in which a diazonium salt or a derivative of a diazonium salt is formed can be appropriately adjusted to obtain the desired effect. The temperature at which the water-soluble compound (B) that reacts with the diazonium salt or its derivative is brought into contact with the composite semipermeable membrane in which the diazonium salt or the diazonium salt derivative is formed is preferably 10 to 90° C. Within this temperature range, the reaction proceeds easily, while a decrease in the amount of permeated water due to shrinkage of the polymer does not occur.
[0093] In addition, the membrane before and after the treatment in this section (2-3) is referred to as a "composite semipermeable membrane", and the layer on the support membrane in the membrane before and after the treatment in this section (2-3) is referred to as a "separation functional layer".
[0094] (3) Use of composite separation membranes The composite semipermeable membrane of the present embodiment thus produced is wound around a cylindrical water collection pipe having a large number of holes, together with a raw water flow path material such as a plastic net, a permeate water flow path material such as tricot, and, if necessary, a film for increasing pressure resistance, and is suitably used as a spiral-type composite semipermeable membrane element. Furthermore, this element can also be connected in series or in parallel and housed in a pressure vessel to form a composite semipermeable membrane module.
[0095] Furthermore, the above-mentioned composite semipermeable membrane and its elements and modules can be combined with a pump that supplies raw water to them, a device that pretreats the raw water, etc. to form a fluid separation device. By using this separation device, raw water can be separated into permeated water such as drinking water and concentrated water that did not permeate the composite semipermeable membrane, thereby obtaining water suitable for the purpose.
[0096] The salt removal rate improves as the operating pressure of the fluid separation device increases; however, the energy required for operation also increases. Taking into consideration the durability of the composite semipermeable membrane, the operating pressure when passing the treated water through the composite semipermeable membrane is preferably 0.5 MPa or more and 10 MPa or less.
[0097] As the temperature of the feed water increases, the salt rejection rate decreases, but as the temperature decreases, the membrane permeation flux also decreases, so it is preferable that the temperature be 5° C. or higher and 45° C. or lower. Also, as the pH of the feed water increases, in the case of high-salt feed water such as seawater, there is a risk of magnesium scale formation, and there is also concern about membrane deterioration due to high pH operation, so operation in the neutral range is preferable.
[0098] Examples of raw water to be treated by the composite semipermeable membrane according to the present embodiment include liquid mixtures containing 50 mg / L to 100 g / L of salt (total dissolved solids), such as seawater, brackish water, and wastewater. In general, salt refers to the total dissolved solids content, and is expressed as "mass / volume" or "weight ratio." According to the definition, it can be calculated from the weight of the residue obtained by evaporating a solution filtered through a 0.45 μm filter at a temperature of 39.5 to 40.5° C., but it is more convenient to convert it from the practical salinity (S). EXAMPLES
[0099] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. In the examples and comparative examples, measurements were carried out as follows.
[0100] (measuring thin film parameters) The composite semipermeable membrane was embedded in polyvinyl alcohol (PVA), stained with OsO4, and cut with an ultramicrotome to prepare ultrathin sections. The obtained ultrathin sections were photographed using a transmission electron microscope. The cross-sectional photographs taken with the transmission electron microscope were imported into the image analysis software Image J. Using the methods described above, the actual length of the thin film, the thickness of the thin film at the protrusions, and the height of the protrusions (proportion of presence) were measured.
[0101] (Water content of polyfunctional acid halide solution) The water content of the polyfunctional acid halide solution was measured five times using a trace water content analyzer CA-05 manufactured by Mitsubishi Chemical Industries Co., Ltd., and the average value was calculated.
[0102] (Film abrasion resistance test) On the surface of the separation functional layer of the composite semipermeable membrane cut to A3 size, an 18cm x 16cm net (thickness: 550μm, pitch: 2.1mm x 2.1mm, fiber diameter: 0.28mm), an 18cm x 16cm acrylic plate, and a 3kg weight were placed in that order. A metal rod was attached to the end of the net, and the composite semipermeable membrane and the net were scraped by pulling the metal rod at 0.5cm / sec. The NaCl permeability of the composite semipermeable membrane before and after scraping and the membrane permeation flux after scraping were measured by the method shown below, and the NaCl permeability ratio was calculated. The results of the NaCl permeability ratio are shown in Table 1 as "SP ratio".
[0103] (Membrane performance evaluation under high pressure) (NaCl transmittance) Raw water for evaluation (NaCl concentration 3.2%, boron concentration approximately 5 ppm) adjusted to a temperature of 25°C and pH 6.5 was supplied to the composite semipermeable membrane at an operating pressure of 5.5 MPa and membrane filtration was carried out for 24 hours. The electrical conductivity of the supply water and the permeated water were then measured using a conductivity meter manufactured by Toa Denpa Kogyo Co., Ltd. to obtain the NaCl concentration of each. NaCl permeability (%) = 100 × (NaCl concentration in permeated water / NaCl concentration in feed water)
[0104] (membrane flux) In the test described above, the amount of water that passes through the membrane of the feed water (evaluation raw water) is expressed as the membrane permeation flux (m 3 / m 2 / day).
[0105] (Reference example 1) A support membrane was prepared by casting an 18 wt % solution of polysulfone in DMF onto a polyester nonwoven fabric made of long fibers at room temperature (25°C) to a thickness of 200 μm, and then immediately immersing the fabric in pure water for 5 minutes.
[0106] Example 1 The support membrane obtained in Reference Example 1 was immersed in an aqueous solution containing 4% by weight of m-phenylenediamine (m-PDA) for 2 minutes, and the support membrane was slowly pulled up vertically. After removing excess aqueous solution from the support membrane surface by blowing nitrogen from an air nozzle, a 0.12% by weight n-decane solution of trimesoyl chloride (TMC) was applied to the support membrane in this order as the first and second multifunctional acid halide solutions. The water content of the first and second multifunctional acid halide solutions is as shown in Table 1.
[0107] Next, it was heated in an oven at 100°C, and then in order to remove excess solution from the membrane, the membrane was vertically drained and dried by blowing air at 20°C using a blower. Finally, it was washed with pure water at 90°C to obtain a composite semipermeable membrane. The manufacturing conditions are shown in Table 1, and the actual length of the thin film, the thin film thickness (T25 and T100 / T25), the height of the protrusions (proportion of protrusions), and the membrane performance of the obtained composite semipermeable membrane are shown in Table 2.
[0108] (Examples 2 to 17) A composite semipermeable membrane was obtained in the same manner as in Example 1, except that the presence or absence of dioctyl phthalate and the amount of water in the first and second multifunctional acid halide solutions were changed to the concentrations shown in Table 1. The additive concentrations of dioctyl phthalate in the first and second multifunctional acid halide solutions are as shown in Table 1.
[0109] (Comparative Examples 1 to 3) A composite semipermeable membrane was obtained in the same manner as in Example 1, except that only the first multifunctional acid halide solution was applied to the support membrane. The water content of the first multifunctional acid halide solution is shown in Table 1.
[0110] (Comparative Examples 4 to 5) A composite semipermeable membrane was obtained in the same manner as in Example 1, except that the water content in the first and second polyfunctional acid halide solutions was changed to the concentrations shown in Table 1.
[0111] Comparative Example 6 The substrate used was a polyester nonwoven fabric similar to that used in Reference Example 1. A first polysulfone solution (14.0 wt % DMF solution) and a second polysulfone solution (17.0 wt % DMF solution) were prepared.
[0112] The first polysulfone solution and the second polysulfone solution were simultaneously discharged using a double slit die coater, and the first polysulfone solution was cast onto a substrate, and the second polysulfone solution was cast onto the first polysulfone solution. The first polysulfone solution was cast to a thickness of 180 μm, and the second polysulfone solution was cast to a thickness of 20 μm, and the solution was immediately immersed in pure water and left for 5 minutes to produce a support membrane.
[0113] A 2.8 wt% aqueous solution of m-PDA was applied to the support membrane obtained above and left to stand for 2 minutes, and then nitrogen was blown from an air nozzle to remove excess aqueous solution from the support membrane surface. Next, an n-decane solution containing 0.10 wt% trimesoyl chloride as a first multifunctional acid halide solution was applied to the support membrane so that the surface was completely wetted and left to stand for 10 seconds, and then the membrane was held vertically for 1 minute to remove excess solution from the membrane and drained. The membrane thus obtained was washed with hot water at 90 ° C for 2 minutes to obtain a composite semipermeable membrane. The water content of the first multifunctional acid halide solution is as shown in Table 1.
[0114] [Table 1]
[0115] [Table 2]
[0116] As shown in Tables 1 and 2, Examples 1 to 17 had higher water permeability and salt removal properties after abrasion than Comparative Examples 1 to 6.
[0117] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2021-072381) filed on April 22, 2021, the contents of which are incorporated herein by reference. [Industrial Applicability]
[0118] The composite semipermeable membrane of the present invention can be suitably used, particularly, for desalinizing seawater or brackish water.
Claims
[Claim 1] A method for producing a composite semipermeable membrane having a substrate, a porous support layer, and a separation functional layer, comprising the steps of: forming the separation functional layer on the porous support layer, The step of forming the separation functional layer includes: (i) contacting the porous support layer with a m-phenylenediamine solution; (ii) after the step (i), contacting the porous support layer with an organic solvent solution containing trimesoyl chloride to produce a polyamide on the porous support layer by interfacial polycondensation; having The step (ii) includes first applying a first organic solvent solution containing trimesoyl chloride to the porous support layer, and then applying a second organic solvent solution containing trimesoyl chloride to the porous support layer; The water content of the first organic solvent solution containing trimesoyl chloride is greater than 0 ppm and less than 200 ppm, The water content of the second organic solvent solution containing trimesoyl chloride is greater than the water content of the first organic solvent solution containing trimesoyl chloride, and is 40 ppm or more and 300 ppm or less. A method for producing a composite semipermeable membrane.
Citation Information
Patent Citations
Preparation method for ultra-low-pressure high-flux reverse osmosis membrane
CN104607067A
Production of thin composite film
JP1994047260A
Productionn of high permeable composite reverse osmosis membrane
JP1996224452A
Composite semipermeable membrane, method for producing the same, and element, fluid separation device, and water treatment method using the same
JP2008517737A
Polyamide-based reverse osmosis separation membrane with excellent initial permeate flow rate and method for producing the same
JP2014521499A