Method for producing silicon single crystals
By adjusting Ar gas flow rate and furnace pressure during counter-doping, the method prevents dislocations in silicon single crystals, ensuring uniform resistivity and low oxygen concentration, addressing the incorporation issue of solid dopants in the silicon melt.
Patent Information
- Application Number
- JP2022553849
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-29
- Filing Date
- 2021-09-21
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-09-21
AI Technical Summary
The incorporation of solid dopants into a silicon melt before complete dissolution causes dislocations in the silicon single crystal during counter-doping, particularly in the production of silicon single crystals for IGBTs where reduced Ar gas flow rates are used to minimize oxygen content.
A method involving controlled adjustments of Ar gas flow rate and furnace pressure during the crystal pulling process, including increasing the Ar gas flow rate and reducing the furnace pressure during sub-dopant addition to prevent unmelted dopants from reaching the solid-liquid interface.
Prevents dislocations in the silicon single crystal by ensuring complete dissolution of dopants, maintaining uniform resistivity, and achieving low oxygen concentration and narrow resistivity ranges.
Smart Images

Figure 0007567929000001 
Figure 0007567929000002 
Figure 0007567929000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a silicon single crystal by the Czochralski method (CZ method), and in particular to a method for additionally supplying a dopant during a crystal pulling process. [Background technology]
[0002] Most of the silicon single crystals used as substrate materials for semiconductor devices are manufactured by the CZ method. In the CZ method, a seed crystal is immersed in molten silicon contained in a quartz crucible, and the seed crystal is gradually pulled up while rotating the seed crystal and the quartz crucible, growing a single crystal with a large diameter below the seed crystal. The CZ method makes it possible to manufacture high-quality silicon single crystals with a high yield.
[0003] In the growth of silicon single crystals, various dopants are used to adjust the electrical resistivity (hereinafter simply referred to as resistivity) of the single crystal. Typical dopants include boron (B), phosphorus (P), arsenic (As), and antimony (Sb). Usually, these dopants are put into a quartz crucible together with the polycrystalline silicon raw material, and melted together with the polycrystalline silicon by heating with a heater. This produces a silicon melt containing a specified amount of dopant.
[0004] However, since the dopant concentration in the silicon single crystal changes in the direction of the pulling axis due to segregation, it is difficult to obtain a uniform resistivity in the direction of the pulling axis. To solve this problem, a method of supplying dopants during the pulling of the silicon single crystal is effective. For example, adding a p-type dopant to the silicon melt during the pulling of an n-type silicon single crystal can suppress the decrease in the resistivity of the silicon single crystal caused by the segregation of the n-type dopant. This method of additionally supplying a secondary dopant of the opposite conductivity type to the primary dopant is called counter doping.
[0005] Regarding the counter doping technology, for example, Patent Document 1 describes adding a dopant so that the rate of addition of a dopant of the opposite type (e.g., p-type) to the type (e.g., n-type) initially added satisfies a predetermined relational expression. Patent Document 2 describes a method of controlling the axial resistivity of a grown silicon single crystal by inserting a rod-shaped silicon crystal containing a secondary dopant into a raw material melt. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 3-247585 [Patent Document 2] JP 2016-216306 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, counterdoping, in which granular dopant is dropped into the silicon melt in a quartz crucible, has the problem that the solid dopant is captured at the solid-liquid interface before it is completely dissolved in the melt, causing dislocations in the silicon single crystal. This problem of dislocations is prominent in the pulling of silicon single crystals for IGBTs, in which the flow rate of Ar gas introduced into the pulling furnace is reduced to reduce the oxygen content of the single crystal, and improvement is required.
[0008] Therefore, an object of the present invention is to provide a method for producing a silicon single crystal that is capable of preventing dislocations from occurring in the single crystal in a counter doping method in which a secondary dopant is added during the crystal pulling process. [Means for solving the problem]
[0009] In order to solve the above problems, the method for producing a silicon single crystal according to the present invention comprises a melting step of producing a silicon melt containing a main dopant, and a crystal pulling step of pulling a silicon single crystal from the silicon melt, the crystal pulling step including at least one additional doping step of dropping a secondary dopant into the silicon melt, wherein the flow rate of Ar gas supplied into the pulling furnace during a first period in which the secondary dopant is not dropped is set to a first flow rate, and the flow rate of the Ar gas supplied into the pulling furnace during a second period including the period in which the secondary dopant is dropped is set to a second flow rate greater than the first flow rate.
[0010] According to the present invention, it is possible to prevent dislocations in a silicon single crystal caused by a secondary dopant dropped into a silicon melt reaching the solid-liquid interface in an unmolten state and being incorporated into the silicon single crystal.
[0011] In the present invention, the increase in the second flow rate relative to the first flow rate is preferably 40 L / min or more and 300 L / min or less in terms of the converted flow rate at room temperature and atmospheric pressure. If it is less than 40 L / min, the effect is small, and if it exceeds 300 L / min, the liquid surface temperature is lowered, which may cause dislocations in the single crystal. In particular, the increase in the second flow rate relative to the first flow rate is preferably 80 L / min or more and 160 L / min or less. Moreover, the second flow rate is preferably 120 L / min or more in terms of the converted flow rate at room temperature and atmospheric pressure, and is preferably 1.5 times or more and 5 times or less of the first flow rate, and particularly preferably 2 times or more and 3 times or less. This makes it possible to prevent dislocations in the silicon single crystal caused by the unmelted secondary dopant being taken into the solid-liquid interface.
[0012] In the present invention, it is preferable that the additional doping step increases the flow rate of the Ar gas to the second flow rate before starting to drop the secondary dopant, and returns the flow rate of the Ar gas to the first flow rate after the drop of the secondary dopant is completed, thereby further reducing the probability that the dopant dropped into the silicon melt is taken into the solid-liquid interface in an unmelted state.
[0013] In the present invention, it is preferable that the pressure in the pulling furnace is set to a first furnace pressure during the first period, and the pressure in the pulling furnace is set to a second furnace pressure lower than the first furnace pressure during the second period. By changing the furnace pressure simultaneously with the Ar gas flow rate, the probability of dislocations occurring can be further reduced.
[0014] In the present invention, the reduction amount of the second furnace pressure relative to the first furnace pressure is preferably 1 Torr or more and 10 Torr or less. Generally, the first furnace pressure is often several tens of Torr, and if the reduction amount of the second furnace pressure exceeds 10 Torr, the second furnace pressure becomes too low and may cause dislocations in the single crystal being pulled. In addition, if the reduction amount of the second furnace pressure is less than 1 Torr, the second furnace pressure is almost the same as the first furnace pressure, making it difficult to obtain the effect of reducing the probability of dislocations. On the other hand, if the reduction amount of the second furnace pressure relative to the first furnace pressure is 1 Torr or more and 10 Torr or less, the probability of dislocations in the single crystal can be further reduced.
[0015] In the method for producing a silicon single crystal according to the present invention, it is preferable to arrange a substantially cylindrical heat shielding member above the silicon melt so as to surround the silicon single crystal pulled up from the silicon melt, and to pull up the silicon single crystal while controlling the flow rate of the Ar gas passing through the gap between the lower end of the heat shielding member and the melt surface. When pulling up a silicon single crystal with a low oxygen concentration in a furnace in which a heat shielding member is installed, it is necessary to precisely control the flow rate of the Ar gas flowing through the gap between the lower end of the heat shielding member and the melt surface. According to the present invention, by increasing the flow rate of Ar gas during counter doping, the flow rate of Ar gas flowing from the center side of the silicon single crystal to the outside near the liquid surface of the silicon melt can be increased, and unmelted dopant can be prevented from approaching the solid-liquid interface. In particular, when the auxiliary dopant is dropped closer to the quartz crucible than the lower end of the heat shielding member, the flow rate of the Ar gas passing through the gap between the lower end of the heat shielding member and the melt surface from the central axis side of the silicon single crystal toward the outside can be increased, which is effective in preventing unmelted dopant from approaching the solid-liquid interface.
[0016] In the present invention, the oxygen concentration in the silicon single crystal is 6×10 17 atoms / cm 3 (ASTM F-121, 1979) or less, and 4 × 10 17 atoms / cm 3 (ASTM F-121,1979) or less. The electrical resistivity of the silicon single crystal is preferably 10 Ωcm or more and 1000 Ωcm or less, and more preferably 20 Ωcm or more and 100 Ωcm or less. In this way, when pulling a silicon single crystal having a low oxygen concentration and a narrow resistivity range, it is necessary to reduce the Ar gas flow rate in the furnace during the crystal pulling process, and when counterdoping is performed under conditions of a low Ar gas flow rate, the probability of dislocations in the silicon single crystal increases. However, when the Ar gas flow rate is increased only during the counterdoping process as in the present invention, the probability of dislocations in the silicon single crystal can be reduced.
[0017] Furthermore, the method for producing a silicon single crystal according to the present invention includes a melting step for producing a silicon melt containing a primary dopant, and a crystal pulling step for pulling a silicon single crystal from the silicon melt, the crystal pulling step including at least one additional doping step for dropping a secondary dopant into the silicon melt, and is characterized in that the pressure in the pulling furnace is set to a first furnace pressure during a first period in which the secondary dopant is not dropped, and the pressure in the pulling furnace is set to a second furnace pressure lower than the first furnace pressure during a second period including a period in which the secondary dopant is dropped.
[0018] According to the present invention, it is possible to prevent dislocations in a silicon single crystal caused by a secondary dopant dropped into a silicon melt reaching the solid-liquid interface in an unmolten state and being incorporated into the silicon single crystal.
[0019] In the present invention, the reduction amount of the second furnace pressure relative to the first furnace pressure is preferably 1 Torr or more and 10 Torr or less. Generally, the first furnace pressure is often several tens of Torr, and if the reduction amount of the second furnace pressure exceeds 10 Torr, the second furnace pressure becomes too low and may cause dislocations in the single crystal being pulled. In addition, if the reduction amount of the second furnace pressure is less than 1 Torr, the second furnace pressure is almost the same as the first furnace pressure, making it difficult to obtain the effect of reducing the probability of dislocations. On the other hand, if the reduction amount of the second furnace pressure relative to the first furnace pressure is 1 Torr or more and 10 Torr or less, the probability of dislocations in the single crystal can be further reduced. Effect of the Invention
[0020] According to the present invention, it is possible to provide a method for producing a silicon single crystal that is capable of preventing dislocations from occurring in the single crystal in a counter doping method in which a secondary dopant is added during the crystal pulling process. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the configuration of a single crystal manufacturing apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow chart for explaining the method for producing a silicon single crystal according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a flow chart for explaining the body portion growing step S16 including the counter doping step. [Figure 4] FIG. 4 is a graph showing the relationship between the dopant dropping period and the Ar gas flow rate and the furnace pressure. [Diagram 5] FIG. 5 is a graph showing the change in resistivity in a silicon single crystal when counterdoping is performed twice. [Figure 6] FIG. 6 is a graph showing the results of measuring the resistivity of the silicon single crystal according to the embodiment by the four-probe method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0023] FIG. 1 is a schematic cross-sectional view showing the configuration of a single crystal manufacturing apparatus according to an embodiment of the present invention.
[0024] As shown in FIG. 1, the single crystal manufacturing apparatus 1 includes a chamber 10 constituting a pulling furnace for a silicon single crystal 2, a quartz crucible 12 installed in the chamber 10, a graphite susceptor 13 supporting the quartz crucible 12, a shaft 14 supporting the susceptor 13 so that it can be raised and lowered and rotated, a heater 15 arranged around the susceptor 13, a heat shielding member 16 arranged above the quartz crucible 12, a single crystal pulling wire 17 arranged above the quartz crucible 12 and coaxially with the shaft 14, a wire winding mechanism 18 arranged above the chamber 10, a dopant supply device 20 that supplies a dopant raw material 5 into the quartz crucible 12, and a control unit 30 that controls each part.
[0025] The chamber 10 is composed of a main chamber 10a, a top chamber 10b that covers the upper opening of the main chamber 10a, and a long and thin cylindrical pull chamber 10c that is connected to the upper opening of the top chamber 10b, and a quartz crucible 12, a susceptor 13, a heater 15, and a heat shielding member 16 are provided inside the main chamber 10a. The susceptor 13 is fixed to the upper end of a shaft 14 that is provided vertically penetrating the center of the bottom of the chamber 10, and the shaft 14 is raised and lowered and rotated by a shaft driving mechanism 19.
[0026] The heater 15 is used to melt the polycrystalline silicon raw material filled in the quartz crucible 12 to generate the silicon melt 3. The heater 15 is a resistance heating type heater made of carbon, and is provided so as to surround the quartz crucible 12 inside the susceptor 13. A heat insulating material 11 is provided on the outside of the heater 15. The heat insulating material 11 is disposed along the inner wall surface of the main chamber 10a, thereby improving the heat retention inside the main chamber 10a.
[0027] The heat shielding member 16 is provided to prevent the silicon single crystal 2 from being heated by radiant heat from the heater 15 and the quartz crucible 12, and to suppress temperature fluctuations in the silicon melt 3. The heat shielding member 16 is a substantially cylindrical member whose diameter decreases from top to bottom, and is provided to cover the upper part of the silicon melt 3 and surround the silicon single crystal 2 being grown. Graphite is preferably used as the material for the heat shielding member 16. An opening larger than the diameter of the silicon single crystal 2 is provided in the center of the heat shielding member 16, and a pulling path for the silicon single crystal 2 is secured. As shown in the figure, the silicon single crystal 2 is pulled upward through the opening. The diameter of the opening of the heat shielding member 16 is smaller than the diameter of the quartz crucible 12, and the lower end of the heat shielding member 16 is located inside the quartz crucible 12, so that even if the upper end of the rim of the quartz crucible 12 is raised above the lower end of the heat shielding member 16, the heat shielding member 16 will not interfere with the quartz crucible 12.
[0028] Although the amount of melt in the quartz crucible 12 decreases as the silicon single crystal 2 grows, by controlling the rise of the quartz crucible 12 so that the distance (gap) between the melt surface and the heat shielding member 16 is constant, it is possible to suppress temperature fluctuations in the silicon melt 3 and to control the amount of dopant evaporation from the silicon melt 3 by keeping constant the flow rate of the Ar gas flowing near the melt surface (purge gas guide path). Therefore, it is possible to improve the stability of the crystal defect distribution, oxygen concentration distribution, resistivity distribution, etc. in the pulling axial direction of the single crystal.
[0029] Above the quartz crucible 12, there is provided a wire 17 which is a pulling shaft for the silicon single crystal 2, and a wire winding mechanism 18 which winds up the wire 17. The wire winding mechanism 18 has a function of rotating the silicon single crystal 2 together with the wire 17. The wire winding mechanism 18 is disposed above the pull chamber 10c, and the wire 17 extends downward from the wire winding mechanism 18 through the pull chamber 10c, with the tip of the wire 17 reaching the internal space of the main chamber 10a. FIG. 1 shows a state in which the silicon single crystal 2 in the middle of growth is suspended from the wire 17. When pulling the single crystal, the seed crystal is immersed in the silicon melt 3, and the wire 17 is gradually pulled up while rotating the quartz crucible 12 and the seed crystal, respectively, to grow the single crystal.
[0030] A gas inlet 10d for introducing Ar gas (purge gas) into the chamber 10 is provided at the top of the pull chamber 10c, and a gas exhaust port 10e for exhausting the Ar gas from the chamber 10 is provided at the bottom of the main chamber 10a. Here, Ar gas means a gas whose main component (more than 50 vol.%) is argon, and may contain gases such as hydrogen and nitrogen.
[0031] An Ar gas supply source 31 is connected to a gas inlet 10d via a mass flow controller 32, and Ar gas from the Ar gas supply source 31 is introduced into the chamber 10 from the gas inlet 10d, with the amount of the Ar gas introduced being controlled by the mass flow controller 32. The Ar gas in the sealed chamber 10 is exhausted to the outside of the chamber 10 from a gas exhaust port 10e, so that the SiO gas and CO gas in the chamber 10 can be collected to keep the inside of the chamber 10 clean. The Ar gas flowing from the gas inlet 10d toward the gas exhaust port 10e passes through the opening of the heat shielding member 16, moves along the melt surface from the center of the pulling furnace to the outside, and then descends to reach the gas exhaust port 10e.
[0032] A vacuum pump 33 is connected to gas exhaust port 10e via piping, and the inside of chamber 10 is kept at a constant reduced pressure by sucking Ar gas from inside chamber 10 with vacuum pump 33 while controlling the flow rate with valve 34. The air pressure inside chamber 10 is measured by a pressure gauge, and the amount of Ar gas exhausted from gas exhaust port 10e is controlled so that the air pressure inside chamber 10 remains constant.
[0033] The dopant supply device 20 includes a dopant supply pipe 21 that is drawn into the chamber 10 from the outside thereof, a dopant hopper 22 that is installed outside the chamber 10 and connected to the upper end of the dopant supply pipe 21, and a seal cap 23 that seals an opening 10f of the top chamber 10b through which the dopant supply pipe 21 passes.
[0034] The dopant supply pipe 21 is a pipe that extends from the installation position of the dopant hopper 22 through the opening 10f of the top chamber 10b to directly above the silicon melt 3 in the quartz crucible 12. During the pulling of the silicon single crystal 2, the dopant raw material 5 is additionally supplied from the dopant supply device 20 to the silicon melt 3 in the quartz crucible 12. The dopant raw material 5 discharged from the dopant hopper 22 is supplied to the silicon melt 3 through the dopant supply pipe 21.
[0035] The dopant raw material 5 supplied from the dopant supply device 20 is granular silicon containing a secondary dopant. Such a dopant raw material 5 is produced by growing silicon crystals containing a high concentration of a secondary dopant by, for example, the CZ method, and then crushing the crystals into small pieces. However, the dopant raw material 5 used for counter doping is not limited to silicon containing a secondary dopant, and may be a simple dopant or a compound containing a dopant atom. The shape of the dopant raw material 5 is not limited to granular, and may be plate-like or rod-like.
[0036] FIG. 2 is a flow chart for explaining the method for producing a silicon single crystal according to the embodiment of the present invention.
[0037] 2, in the manufacture of silicon single crystal 2, first, polycrystalline silicon raw material is filled into quartz crucible 12 together with a main dopant (raw material filling step S11). When pulling n-type silicon single crystal, the main dopant is, for example, phosphorus (P), arsenic (As) or antimony (Sb), and when pulling p-type silicon single crystal, the main dopant is, for example, boron (B), aluminum (Al), gallium (Ga) or indium (In). Next, the polycrystalline silicon in quartz crucible 12 is heated and melted by heater 15 to generate silicon melt 3 containing the main dopant (melting step S12).
[0038] Next, the seed crystal attached to the tip of the wire 17 is lowered to make it contact with the silicon melt 3 (step S13). Thereafter, a crystal pulling process (steps S14 to S17) is performed in which the seed crystal is gradually pulled up while maintaining contact with the silicon melt 3 to grow a single crystal.
[0039] In the crystal pulling process, the following steps are carried out in order: necking step S14, in which a neck portion with a narrowed crystal diameter is formed to eliminate dislocations; shoulder portion growing step S15, in which a shoulder portion with a gradually enlarged crystal diameter is formed; body portion growing step S16, in which a body portion with a crystal diameter maintained at a specified diameter (e.g., about 300 mm); and tail portion growing step S17, in which a tail portion with a gradually reduced crystal diameter is formed. Finally, the single crystal is separated from the melt surface. This completes the silicon single crystal ingot.
[0040] The body portion growing step S16 preferably includes at least one counter doping step (additional doping step) in which a secondary dopant having a conductivity type opposite to that of the primary dopant contained in the silicon single crystal 2 is introduced into the silicon melt 3. This makes it possible to suppress a change in resistivity of the body portion of the silicon single crystal 2 in the crystal longitudinal direction.
[0041] The oxygen concentration in silicon single crystal for IGBT is 6×10 17 atoms / cm 3(ASTM F-121, 1979) or less, and 4 × 10 17 atoms / cm 3 (ASTM F-121, 1979) or less is particularly preferable. Furthermore, the resistivity of the silicon single crystal for IGBT is preferably 10 Ωcm or more and 1000 Ωcm or less, and particularly preferably 20 Ωcm or more and 100 Ωcm or less.
[0042] In this way, when pulling silicon single crystals for IGBTs with low oxygen concentration and narrow resistivity range, it is preferable to slow down the flow rate of Ar gas along the melt surface from the central axis side of the pulling furnace to the outside, and when additional doping is performed under such furnace conditions, the probability of dislocations occurring in the silicon single crystal increases. However, when the furnace conditions during the counter doping step are changed as in this embodiment, the probability of dislocations occurring in the silicon single crystal can be reduced.
[0043] FIG. 3 is a flow chart for explaining the body portion growing step S16 including the counter doping step.
[0044] As shown in Fig. 3, at the start of the body portion growing step S16, the Ar gas flow rate and the furnace pressure are set to values suitable for growing silicon single crystals (step S21). For example, in the case of silicon single crystals for IGBTs, low resistivity and low interstitial oxygen concentration are required. To grow such silicon single crystals, the Ar gas flow rate needs to be smaller than that for silicon single crystals for general semiconductor devices. The Ar gas flow rate and the furnace pressure required for the normal body portion growing step S16 are set to a first flow rate F1 and a first furnace pressure P1, respectively.
[0045] Since the dopant concentration in the silicon single crystal increases as the crystal is pulled up, it falls outside the desired resistivity range. Therefore, when the counter-doping is required during the process, the counter-doping is started (steps S22Y, S23 to S25).
[0046] In counter doping, a dopant raw material 5 containing a secondary dopant is dropped into the silicon melt 3 (step S24). The secondary dopant when pulling up an n-type silicon single crystal is, for example, boron (B), aluminum (Al), gallium (Ga), or indium (In), and the secondary dopant when pulling up a p-type silicon single crystal is, for example, phosphorus (P), arsenic (As), or antimony (Sb).
[0047] During the dopant dropping period, the Ar gas flow rate and the furnace internal pressure are each changed to values suitable for counter doping. The Ar gas flow rate F2 (second flow rate) during the dopant dropping period (second period) is set to a value larger than the Ar gas flow rate F1 (first flow rate) during the normal crystal pulling period (first period) (F2 > F1). Also, the furnace internal pressure P2 (second furnace internal pressure) during the counter doping period is set to a value lower than the furnace internal pressure P1 (first furnace internal pressure) during the normal crystal pulling period (P2 < P1). Note that the dopant dropping period, in a narrow sense, is the period when the dopant raw material 5 is actually dropped, but in a broad sense, it refers to the period required until the dopant dropped into the silicon melt is completely melted and no problem of dislocations occurs.
[0048] The increase amount of the Ar gas flow rate F2 with respect to the Ar gas flow rate F1 is preferably 40 L / min or more and 300 L / min or less in terms of the converted flow rate at room temperature and atmospheric pressure. Also, the Ar gas flow rate F2 is preferably 120 L / min or more in terms of the converted flow rate at room temperature and atmospheric pressure, and preferably 1.5 times or more and 5 times or less of the Ar gas flow rate F1. Thereby, it is possible to prevent the dislocation of the silicon single crystal due to the unmolten secondary dopant being incorporated into the solid-liquid interface.
[0049] The decrease amount of the furnace internal pressure P2 with respect to the furnace internal pressure P1 is preferably 1 Torr or more and 10 Torr or less. By changing the furnace internal pressure simultaneously with the Ar gas flow rate, the probability of dislocation can be further reduced.
[0050] When the counterdoping is completed, the Ar gas flow rate F1 and the furnace pressure P1 during the normal crystal pulling period (first period) are restored, and the growth of the body portion is continued (steps S25, S26).
[0051] The counter doping process is repeated according to the desired crystal length (steps S27Y, S22Y, S23 to S25). After counter doping is completed, the growth of the straight body portion continues, and when the time comes when counter doping is required again, counter doping is started. The number of times counter doping is repeated is predetermined, and counter doping is repeated until the specified number of times is completed. During each counter doping, the Ar gas flow rate and the furnace pressure are changed to values (F2, P2) suitable for counter doping, respectively. In this way, by pulling up a silicon single crystal of the desired length while performing counter doping the specified number of times, it is possible to increase the yield of silicon single crystals with small changes in resistivity in the direction of the pulling axis.
[0052] FIG. 4 is a graph showing the relationship between the dopant dropping period and the Ar gas flow rate and the furnace pressure.
[0053] As shown in Fig. 4, during the dopant dropping period, the Ar gas flow rate is increased and the furnace pressure is decreased. For example, the Ar gas flow rate during the dopant dropping period (second period) is set to twice the Ar gas flow rate during the normal pulling period (first period) when no dopant is dropped. Also, the furnace pressure during the dopant dropping period (second period) is set to 80% of the furnace pressure during the normal pulling period (first period).
[0054] When the flow rate of Ar gas introduced into the chamber 10 is increased, the flow rate of the Ar gas along the melt surface flowing from the center side of the chamber 10 to the outside increases, so that it is possible to prevent the unmelted dopant floating near the melt surface from approaching the solid-liquid interface between the silicon single crystal 2 and the silicon melt 3. Similarly, when the furnace pressure is increased, the flow rate of the Ar gas along the melt surface flowing from the center side of the chamber 10 to the outside increases, so that it is possible to prevent the dopant from approaching the solid-liquid interface. Therefore, by temporarily changing the Ar gas flow rate and the furnace pressure, it is possible to prevent the single crystal from being dislocated due to the dopant being taken into the solid-liquid interface between the silicon single crystal 2 and the silicon melt 3.
[0055] FIG. 5 is a graph showing the change in resistivity in a silicon single crystal when counterdoping is performed twice, with the horizontal axis showing the crystal length (a relative value when the total length of the straight body portion is taken as 1) and the vertical axis showing the resistivity (relative value).
[0056] As shown in Figure 5, in the case of a silicon single crystal doped with phosphorus alone as the main dopant, the resistivity of the silicon single crystal is highest at the start of pulling and only gradually decreases as pulling proceeds, so that the resistivity falls outside the standard when the crystal length exceeds approximately 0.44.
[0057] However, by performing the first counterdoping at a position where the crystal length is approximately 0.44 and the second counterdoping at a position where the crystal length is 0.63, the length of the single crystal where the resistivity falls within the standard can be made as long as possible.
[0058] As described above, the method for producing a silicon single crystal according to this embodiment includes a step of dropping a secondary dopant of an opposite conductivity type to the main dopant of the silicon single crystal into the silicon melt during the silicon single crystal pulling step, and the Ar gas flow rate during the period when the secondary dopant is dropped is made larger than that during the period when the secondary dopant is not dropped, and the furnace pressure is made lower, thereby making it possible to prevent dislocations from occurring in the single crystal.
[0059] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present invention, and it goes without saying that these modifications are also included within the scope of the present invention. EXAMPLES
[0060] (Comparative Example) During the growth process of the straight body of n-type silicon single crystals using phosphorus (P) as the main dopant, counter doping was performed without changing the Ar gas flow rate or furnace pressure. In counter doping, the change in resistivity due to the segregation of P was predicted, and boron (B) was added as a secondary dopant just before the resistivity deviated from the standard. As a result, dislocations occurred in the silicon single crystal immediately after the secondary dopant was added.
[0061] (Example) Counterdoping was performed twice during the growth process of the straight body of n-type silicon single crystals using phosphorus (P) as the main dopant. During counterdoping, the Ar gas flow rate was increased to twice the normal flow rate, and this increased Ar gas flow rate was maintained for 15 minutes, after which the Ar gas flow rate was returned to the normal flow rate (see Figure 4). At the same time, the furnace pressure was reduced by 5 Torr from the normal flow rate, and this reduced furnace pressure was maintained for 15 minutes, after which the furnace pressure was returned to the normal flow rate (see Figure 4). It took 20 minutes to change (increase and decrease) the Ar gas flow rate and the furnace pressure. The secondary dopant was added during the period when the increased Ar gas flow rate and the reduced furnace pressure were maintained constant. As a result, the silicon single crystal was pulled to the end without dislocations.
[0062] In order to confirm the resistivity distribution in the longitudinal direction of the silicon single crystal obtained in this manner, a sample was obtained by cutting the crystal block vertically near the dopant injection position, and the sample was ground to a thickness of 1.0 mm. Furthermore, a donor killer treatment (heat treatment at 650°C for 40 minutes) was performed to measure the resistivity.
[0063] Next, the resistivity of the sample was measured using the four-point probe method. The measurement pitch for resistivity was 1 mm in the vicinity of the secondary dopant injection position, and 5 mm elsewhere. The results of continuous resistivity measurements are shown in Figure 6. As shown in the figure, the resistivity increased immediately after the dopant injection, and thereafter, the resistivity according to the segregation was obtained. The resistivity after the second injection of the secondary dopant was slightly lower than the target resistivity, but generally good results were obtained.
[0064] The above-described counter-doped silicon single crystal pulling was carried out four times, and no dislocations were observed in any of the silicon single crystals, and good results were obtained. [Explanation of symbols]
[0065] 1. Single crystal manufacturing equipment 2. Silicon single crystal 3. Silicon melt 5 Dopant (co-dopant) 10. Chamber 10a Main Chamber 10b Top chamber 10c Pull Chamber 10d Gas Inlet 10e Gas exhaust port 10f opening 11. Insulation 12 Quartz crucible 13 Susceptor 14 Shaft 15 Heater 16 Heat shielding material 17 Wire 18 Wire winding mechanism 19 Shaft drive mechanism 20 Dopant supply device 21 Dopant supply tube 22 Dopant Hopper 23 Seal cap 30 Control section 31 Ar gas supply source 32 Mass Flow Controller 33 Vacuum Pump 34 Valve S11 Raw material filling process S12 Melting process S13 Liquid application process S14 Necking process S15 Shoulder part development process S16 Straight trunk growth process S17 Tail section development process
Claims
1. a melting step to produce a silicon melt containing a primary dopant; and a crystal pulling step of pulling a silicon single crystal from the silicon melt. The crystal pulling step includes at least one additional doping step of dropping a secondary dopant having an opposite conductivity type to the primary dopant into the silicon melt; A flow rate of Ar gas supplied into the pulling furnace during a first period in which the secondary dopant is not dropped is set to a first flow rate; A method for producing a silicon single crystal, characterized in that the flow rate of the Ar gas supplied into the pulling furnace during a second period including a period during which the secondary dopant is dropped is set to a second flow rate that is greater than the first flow rate.
2. 2. The method for producing a silicon single crystal according to claim 1, wherein an increase in the second flow rate with respect to the first flow rate is 40 L / min or more and 300 L / min or less in terms of a converted flow rate at room temperature and atmospheric pressure.
3. The method for producing a silicon single crystal according to claim 1 or 2, wherein the second flow rate is 120 L / min or more in terms of a converted flow rate at room temperature and atmospheric pressure.
4. The method for producing a silicon single crystal according to claim 1 , wherein the second flow rate is 1.5 to 5 times the first flow rate.
5. 5. The method for producing a silicon single crystal according to claim 1, wherein the additional doping step increases a flow rate of the Ar gas to the second flow rate before starting to drop the secondary dopant, and returns the flow rate of the Ar gas to the first flow rate after the drop of the secondary dopant is completed.
6. setting the pressure in the pulling furnace to a first furnace pressure during the first period; The method for producing a silicon single crystal according to claim 1 , wherein the pressure in the pulling furnace during the second period is set to a second furnace pressure lower than the first furnace pressure.
7. 7. The method for producing a silicon single crystal according to claim 6, wherein an amount of reduction in the second furnace pressure with respect to the first furnace pressure is 1 Torr or more and 10 Torr or less.
8. The method for producing a silicon single crystal according to claim 1 , further comprising disposing a substantially cylindrical heat shielding member above the silicon melt so as to surround the silicon single crystal pulled up from the silicon melt.
9. The oxygen concentration in the silicon single crystal is 6×10 17 atoms / cm 3 The method for producing a silicon single crystal according to any one of claims 1 to 8, wherein the silicon single crystal has a hardness of 100% or less than ASTM F-121, 1979.
10. The method for producing a silicon single crystal according to claim 1 , wherein the electrical resistivity of the silicon single crystal is 10 Ωcm or more and 1000 Ωcm or less.
11. a melting step to produce a silicon melt containing a primary dopant; and a crystal pulling step of pulling a silicon single crystal from the silicon melt. The crystal pulling step includes at least one additional doping step of dropping a secondary dopant having an opposite conductivity type to the primary dopant into the silicon melt; During a first period in which the secondary dopant is not dropped, the pressure in the pulling furnace is set to a first furnace pressure; A method for producing a silicon single crystal, comprising the steps of: setting the pressure in the pulling furnace to a second furnace pressure lower than the first furnace pressure during a second period including a period during which the secondary dopant is dropped.
12. 12. The method for producing a silicon single crystal according to claim 11, wherein an amount of reduction in the second furnace pressure with respect to the first furnace pressure is 1 Torr or more and 10 Torr or less.
Citation Information
Patent Citations
Crystal growing method
JP1991247585A
Silicon single crystal and single crystal growing method
JP2004307305A
Apparatus and method for pulling single crystal
JP2012206874A
Method for lifting silicon single crystal
JP2014125402A
Silicon ingot having multiple uniform dopants, and method and apparatus for producing the same.
JP2014511146A