Cutting tool and manufacturing method thereof

A cutting tool with a multilayer structure of cubic crystal hard particles addresses thermal cracking and peeling issues, enhancing wear resistance and tool life in milling high-hardness, heat-resistant stainless steel.

JP7568076B2Active Publication Date: 2024-10-16SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023517110
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-30
Filing Date
2022-03-04
Publication Date
2024-10-16
Estimated Expiration
2042-03-04

AI Technical Summary

Technical Problem

Existing cutting tools fail to provide adequate tool life when milling high-hardness, heat-resistant stainless steel due to thermal cracks, delamination, and peeling at the interface of nanocomposite coatings.

Method used

A cutting tool with a multilayer structure of hard particles, where first and second unit layers are alternately stacked, each composed of cubic crystal structures made from specific metal elements, silicon, carbon, nitrogen, and oxygen, with controlled silicon atom percentages, and optionally including a base, intermediate, and surface layers to enhance adhesion and wear resistance.

Benefits of technology

The cutting tool exhibits improved wear resistance, reduced thermal cracking, and extended tool life during milling of high-hardness, heat-resistant stainless steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568076000009
    Figure 0007568076000009
  • Figure 0007568076000010
    Figure 0007568076000010
  • Figure 0007568076000011
    Figure 0007568076000011
Patent Text Reader

Abstract

A cutting tool including a substrate, and a coating disposed on the substrate, wherein the coating comprises a hard particle layer composed of hard particles. The hard particles include a multi-layer structure in which a first unit layer and a second unit layer are alternately stacked. The first unit layer is composed of a first compound having a cubic crystal structure, and the second unit layer is composed of a second compound having a cubic crystal structure. Each of the first compound and the second compound is composed of at least one metal element selected from the group consisting of group 4 elements, group 5 elements, and group 6 elements of the periodic table, silicon, and at least one element selected from the group consisting of carbon, nitrogen, boron and oxygen. The percentage of the number of atoms of the silicon to the total number of atoms of the metal element and the silicon in the first unit layer is different from the percentage of the number of atoms of the silicon to the total number of atoms of the metal element and the silicon in the second unit layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a cutting tool and a manufacturing method thereof. This application claims priority to Japanese Patent Application No. 2021-078030, filed on April 30, 2021. The entire contents of the Japanese patent application are incorporated herein by reference. [Background technology]

[0002] Conventionally, in order to improve the wear resistance of cutting tools, cutting tools having a substrate on which a TiSiCN film is formed have been developed.

[0003] Patent Document 1 describes a TiC produced by thermal CVD. x N 1-x Nanocrystalline layer and amorphous SiC x N y A nanocomposite coating is disclosed that includes a second phase of

[0004] Patent Document 2 discloses at least one nanocomposite layer including a first nanocrystalline phase made of cubic titanium oxycarbonitride produced by a thermal CVD method and a second amorphous phase made of silicon oxycarbonitride or silicon oxycarbide.

[0005] Non-Patent Document 1 discloses a TiSiCN coating film having a nanocomposite structure formed by a PVD method. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2015-505902

[0007] [Patent Document 2] Special Publication No. 2020-507679 [Non-patent literature]

[0008] [Non-Patent Document 1] Shinya Imamura et al., “Properties and cutting performance of AlTiCrN / TiSiCN bilayer coatings deposited by cathodic-arc ion plating”, Surface and Coatings Technology, 202, (2007), 820-825 Summary of the Invention

[0009] The cutting tool of the present disclosure comprises: 1. A cutting tool comprising a substrate and a coating disposed on the substrate, the coating includes a hard particle layer made of hard particles, The hard particles include a multilayer structure in which first unit layers and second unit layers are alternately laminated, the first unit layer is made of a first compound having a cubic crystal structure, the second unit layer is made of a second compound having a cubic crystal structure, Each of the first compound and the second compound is one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; Silicon and one or more elements selected from the group consisting of carbon, nitrogen, boron, and oxygen; A cutting tool, wherein the percentage of the number of silicon atoms relative to the total number of atoms of the metal element and the silicon in the first unit layer is different from the percentage of the number of silicon atoms relative to the total number of atoms of the metal element and the silicon in the second unit layer.

[0010] The method of manufacturing a cutting tool according to the present disclosure includes: A method for manufacturing the cutting tool, comprising the steps of: A first step of preparing a substrate; A second step of forming a coating on the substrate to obtain a cutting tool, The second step includes a 2a step of forming a hard particle layer made of hard particles by a CVD method, The 2a step includes a 2a-1 step of ejecting a first source gas, a second source gas, and a third source gas toward a surface of the substrate, the first source gas contains one or more elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; The second source gas is SiCl4, the third source gas contains one or more elements selected from the group consisting of carbon, nitrogen, boron, and oxygen; The first source gas is ejected from a plurality of first injection holes provided in a nozzle, the second source gas is ejected from a plurality of second injection holes provided in the nozzle, the third source gas is ejected from a plurality of third injection holes provided in the nozzle, In the step 2a-1, the nozzle rotates, the plurality of second injection holes include a 2-1 injection hole and a 2-2 injection hole, A method for manufacturing a cutting tool, wherein a diameter r1 of the 2-1 ejection hole is different from a diameter r2 of the 2-2 ejection hole. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic view showing an example of a cross section of a cutting tool according to a first embodiment. [Diagram 2] FIG. 2 is a schematic view showing another example of a cross section of the cutting tool according to the first embodiment. [Diagram 3] FIG. 3 is a schematic view showing another example of a cross section of the cutting tool according to the first embodiment. [Figure 4] FIG. 4 is a schematic view showing another example of a cross section of the cutting tool according to the first embodiment. [Diagram 5] FIG. 5 is a bright-field scanning electron microscope (BF-SEM) image of a cross section of the hard phase particle layer of the cutting tool according to the first embodiment. [Figure 6] FIG. 6 is an electron diffraction image taken within the region A shown in FIG. [Figure 7] FIG. 7 is a graph showing the change in the percentage of the number of silicon atoms ASi, {ASi / (ASi+AM)}×100, relative to the sum of the number of metal elements (titanium) atoms AM and the number of silicon atoms ASi along the direction of the arrows shown in FIG. 5. [Figure 8] FIG. 8 is a Fourier transform image obtained by performing a Fourier transform on the region A shown in FIG. [Figure 9] FIG. 9 is a graph showing the intensity profile within the rectangular frame of the Fourier transform image in FIG. [Figure 10] FIG. 10 is a schematic cross-sectional view of an example of a CVD apparatus used in manufacturing the cutting tool according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Problem that this disclosure aims to solve] In recent years, there has been an increasing demand for improved tool life, particularly in the milling of high-hardness, heat-resistant stainless steel.

[0013] Therefore, an object of the present invention is to provide a cutting tool that has a long tool life even when milling high-hardness, heat-resistant stainless steel. [Effects of this disclosure]

[0014] According to the present disclosure, it is possible to provide a cutting tool that can have a long tool life even when milling high-hardness heat-resistant stainless steel.

[0015] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. (1) The cutting tool of the present disclosure comprises: 1. A cutting tool comprising a substrate and a coating disposed on the substrate, the coating includes a hard particle layer made of hard particles, The hard particles include a multilayer structure in which first unit layers and second unit layers are alternately laminated, the first unit layer is made of a first compound having a cubic crystal structure, the second unit layer is made of a second compound having a cubic crystal structure, Each of the first compound and the second compound is one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; Silicon and one or more elements selected from the group consisting of carbon, nitrogen, boron, and oxygen; A cutting tool, wherein the percentage of the number of silicon atoms relative to the total number of atoms of the metal element and the silicon in the first unit layer is different from the percentage of the number of silicon atoms relative to the total number of atoms of the metal element and the silicon in the second unit layer.

[0016] According to the present disclosure, it is possible to provide a cutting tool that can have a long tool life even when milling high-hardness heat-resistant stainless steel.

[0017] (2) It is preferable that the first unit layer and the second unit layer have the same crystal orientation, which makes it possible to minimize the interfacial energy and makes it difficult for the hardness to decrease even when exposed to a high-temperature environment.

[0018] (3) In each of the first unit layer and the second unit layer, the percentage of the number of silicon atoms to the total number of the metal elements and the silicon atoms is preferably 0.5% or more and 10% or less, which improves the heat crack resistance of the coating and the adhesion between the hard particle layer and the adjacent layer in a well-balanced manner.

[0019] (4) The thickness of the hard particle layer is 3 μm or more and 15 μm or less, The thickness of the coating is preferably 3 μm or more and 30 μm or less.

[0020] This improves the wear resistance and chipping resistance of the coating in a well-balanced manner.

[0021] (5) The number A of atoms of the metal element in the first unit layerM and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M )}×100, and the number A of atoms of the metal element in the second unit layer M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M )}×100 is preferably 0.5% or more and 10% or less. This improves the hardness of the coating.

[0022] (6) The coating includes a base layer disposed between the substrate and the hard particle layer, the underlayer is made of a third compound, The third compound is One or more elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and aluminum in the periodic table; and one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen.

[0023] This improves the adhesion between the coating and the substrate, and also improves the abrasion resistance.

[0024] (7) The coating includes a base layer disposed directly on the substrate, The underlayer is preferably made of at least one layer selected from the group consisting of a TiN layer, a TiC layer, a TiCN layer, a TiBN layer, and an Al2O3 layer.

[0025] By placing a TiN layer, TiC layer, TiCN layer, or TiBN layer directly on the substrate as an underlayer, the adhesion between the substrate and the coating can be improved. Also, by using an Al2O3 layer as an underlayer, the oxidation resistance of the coating can be improved.

[0026] (8) The coating has a surface layer disposed on its outermost surface, the surface layer is made of a fourth compound, The fourth compound is One or more elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and aluminum in the periodic table; and one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen.

[0027] This improves the thermal cracking resistance and abrasion resistance of the coating.

[0028] (9) The coating is a layer including the underlayer and the hard particles. layer It is preferable to have an intermediate layer disposed between the coating and the base material, which improves the abrasion resistance of the coating.

[0029] (10) A method for manufacturing a cutting tool according to the present disclosure includes: A method for manufacturing the cutting tool, comprising the steps of: A first step of preparing a substrate; A second step of forming a coating on the substrate to obtain a cutting tool, The second step includes a 2a step of forming a hard particle layer made of hard particles by a CVD method, The 2a step includes a 2a-1 step of ejecting a first source gas, a second source gas, and a third source gas toward a surface of the substrate, the first source gas contains one or more elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; The second source gas is SiCl4, the third source gas contains one or more elements selected from the group consisting of carbon, nitrogen, boron, and oxygen; The first source gas is ejected from a plurality of first injection holes provided in a nozzle, the second source gas is ejected from a plurality of second injection holes provided in the nozzle, the third source gas is ejected from a plurality of third injection holes provided in the nozzle, In the step 2a-1, the nozzle rotates, the plurality of second injection holes include a 2-1 injection hole and a 2-2 injection hole, A method for manufacturing a cutting tool, wherein a diameter r1 of the 2-1 ejection hole is different from a diameter r2 of the 2-2 ejection hole.

[0030] According to the present disclosure, it is possible to provide a cutting tool that can have a long tool life even when milling high-hardness heat-resistant stainless steel.

[0031] [Details of the embodiment of the present disclosure] In order to develop a cutting tool having a long tool life even when milling high-hardness, heat-resistant stainless steel, the present inventors milled high-hardness, heat-resistant stainless steel using a conventional cutting tool and observed the damage state of the tool.

[0032] When high-hardness heat-resistant stainless steel was milled using the tools of Patent Documents 1 and 2, it was confirmed that thermal cracks caused by the thermal load during cutting progressed at the interface between the nanocomposite coating and the underlayer, resulting in interfacial peeling. This is presumably due to insufficient interface consistency between the crystalline underlayer and the nanocomposite coating.

[0033] When high-hardness heat-resistant stainless steel was milled using the tool described in Non-Patent Document 1, the TiSiCN coating was found to self-destruct. This is presumably because the TiSiCN coating has a large compressive residual stress due to being formed by the PVD method.

[0034] As a result of intensive research based on the above findings, the present inventors have obtained a cutting tool having a long tool life even in milling high-hardness heat-resistant stainless steel. Specific examples of the cutting tool and its manufacturing method of the present disclosure will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference symbols represent the same or corresponding parts. In addition, dimensional relationships such as length, width, thickness, and depth have been appropriately changed to clarify and simplify the drawings, and do not necessarily represent actual dimensional relationships.

[0035] In this specification, the expression in the form "A to B" means the upper and lower limits of a range (i.e., greater than or equal to A and less than or equal to B). When no unit is specified for A and a unit is specified only for B, the unit of A and the unit of B are the same.

[0036] In this specification, when a compound is expressed by a chemical formula, unless the atomic ratio is particularly limited, it is intended to include any conventionally known atomic ratio and is not necessarily limited to the stoichiometric range. For example, when "TiSiCN" is written, the ratio of the number of atoms constituting TiSiCN includes any conventionally known atomic ratio.

[0037] In the present disclosure, when one or more numerical values ​​are described as the lower limit and the upper limit of a numerical range, a combination of any one numerical value described as the lower limit and any one numerical value described as the upper limit is also disclosed. For example, when a1 or more, b1 or more, and c1 or more are described as the lower limit, and a2 or less, b2 or less, and c2 or less are described as the upper limit, a1 or more and a2 or less, a1 or more and b2 or less, a1 or more and c2 or less, b1 or more and a2 or less, b1 or more and b2 or less, b1 or more and c2 or less, c1 or more and a2 or less, c1 or more and b2 or less, and c1 or more and c2 or less are disclosed.

[0038] [Embodiment 1: Cutting tool] A cutting tool according to an embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") includes: 1. A cutting tool comprising a substrate and a coating disposed on the substrate, The coating includes a hard particle layer made of hard particles, The hard particles include a multilayer structure in which first unit layers and second unit layers are alternately laminated, the first unit layer is made of a first compound having a cubic crystal structure, the second unit layer is made of a second compound having a cubic crystal structure, Each of the first compound and the second compound is one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; Silicon and one or more elements selected from the group consisting of carbon, nitrogen, boron, and oxygen; The cutting tool has a percentage of the number of silicon atoms relative to the total number of atoms of the metal element and the silicon in the first unit layer that is different from a percentage of the number of silicon atoms relative to the total number of atoms of the metal element and the silicon in the second unit layer.

[0039] As used herein, the Group 4 elements of the periodic table include titanium (Ti), zirconium (Zr) and hafnium (Hf), the Group 5 elements include vanadium (V), niobium (Nb) and tantalum (Ta), and the Group 6 elements include chromium (Cr), molybdenum (Mo) and tungsten (W).

[0040] The cutting tool of this embodiment has a long tool life even in milling high-hardness heat-resistant stainless steel. The reason for this is not clear, but is presumed to be as follows: (i) to (iii).

[0041] (i) In the cutting tool of this embodiment, the coating comprises a hard particle layer made of hard particles. The hard particle layer can have a region made of granular structure in the thickness direction. This improves the toughness of the hard particle layer, and even if thermal cracks occur on the surface of the coating due to cutting, the progression of the cracks to the substrate is effectively suppressed. In addition, even if the coating includes layers other than the hard particle layer, the difference in crystallinity between the hard particle layer and the other layers can be reduced, so that the propagation of cracks at the interface between the hard particle layer and the other layers is suppressed, and film peeling is suppressed. Therefore, the cutting tool can have a long tool life.

[0042] (ii) In the cutting tool of this embodiment, the hard particles include a multilayer structure in which first and second unit layers having different compositions are alternately laminated. As a result, even if distortion occurs in the hard particles and cracks occur on the surface of the coating due to cutting, the progression of the cracks to the substrate is effectively suppressed. In addition, the hardness of the hard particles and the hard particle layer is increased, improving the wear resistance of the cutting tool. In addition, the cutting tool can have a long tool life.

[0043] (iii) in the cutting tool of this embodiment, each of the first compound and the second compound has a cubic crystal structure, one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; Silicon and and one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen. The first compound and the second compound have high hardness. Therefore, the hard particle layer including the first compound and the second compound has high hardness and excellent wear resistance. Therefore, the cutting tool can have a long tool life.

[0044] <Cutting tools> As shown in FIG. 1, the cutting tool 1 of this embodiment includes a substrate 10 and a coating 15 disposed on the substrate 10. FIG. 1 shows a case where the coating 15 is composed only of a hard particle layer 11. The coating 15 preferably covers at least a part of the substrate that is involved in cutting, and more preferably covers the entire substrate. The part of the substrate that is involved in cutting means a region on the substrate surface that is within 500 μm from the cutting edge. Even if a part of the substrate is not covered with this coating or the coating has a partially different configuration, this does not deviate from the scope of the present disclosure.

[0045] <Types of cutting tools> The cutting tool of the present disclosure may be, for example, a drill, an end mill (e.g., a ball end mill), an indexable cutting tip for a drill, an indexable cutting tip for an end mill, an indexable cutting tip for milling, an indexable cutting tip for turning, a metal saw, a gear cutting tool, a reamer, a tap, and the like.

[0046] <Base material> The substrate 10 includes a rake face and a flank face, and any of the substrates known in the art can be used. For example, the substrate is preferably any of cemented carbide (e.g., WC-based cemented carbide containing tungsten carbide and cobalt, which can contain carbonitrides of Ti, Ta, Nb, etc.), cermet (mainly composed of TiC, TiN, TiCN, etc.), high-speed steel, ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, etc.), cubic boron nitride sintered body, and diamond sintered body.

[0047] Among these various substrates, a substrate made of a cemented carbide containing tungsten carbide and cobalt, in which the content of cobalt in the cemented carbide is 6% by mass or more and 11% by mass or less, is preferred. This provides an excellent balance between hardness and strength at high temperatures, and has excellent characteristics as a substrate for cutting tools for the above-mentioned applications. When a WC-based cemented carbide is used as the substrate, the structure may contain free carbon and abnormal layers called η phase or ε phase.

[0048] Furthermore, the substrate may have a modified surface. For example, in the case of a cemented carbide, a de-β layer may be formed on the surface, and in the case of a cermet, a surface-hardened layer may be formed. The substrate may exhibit the desired effect even if the surface is modified.

[0049] When the cutting tool is an indexable cutting tip, the substrate may or may not have a chip breaker. The shape of the cutting edge ridge can be any of a sharp edge (the ridge where the rake face and the flank intersect), a honing (a sharp edge with an arc), a negative land (a chamfer), or a combination of a honing and a negative land.

[0050] <Coating> (Coating composition) The coating of the present embodiment includes a hard particle layer. The coating of the present embodiment may include other layers as long as it includes a hard particle layer.

[0051] For example, as shown in cutting tool 21 of FIG. 2, coating 25 can include, in addition to hard particle layer 11, underlayer 12 disposed between substrate 10 and hard particle layer 11.

[0052] As shown in the cutting tool 31 of FIG. 3, the coating 35 may include a surface layer 13 disposed on the hard particle layer 11 in addition to the hard particle layer 11 and the underlayer 12 .

[0053] As shown in the cutting tool 41 of FIG. 4 , the coating 45 may include, in addition to the hard particle layer 11 , the underlayer 12 , and the surface layer 13 , an intermediate layer 14 disposed between the underlayer 12 and the hard particle layer 11 .

[0054] The hard particle layer, underlayer, intermediate layer and surface layer will be described in detail later.

[0055] (Coating thickness) The thickness of the coating in this embodiment is preferably 3 μm or more and 30 μm or less. Here, the thickness of the coating means the thickness of the entire coating. When the thickness of the entire coating is 3 μm or more, it can have excellent wear resistance. On the other hand, when the thickness of the entire coating is 30 μm or less, it can suppress the occurrence of peeling or destruction of the coating when a large stress is applied between the coating and the substrate during cutting. The lower limit of the thickness of the entire coating is more preferably 5 μm or more, and more preferably 10 μm or more, from the viewpoint of improving wear resistance. The upper limit of the thickness of the entire coating is more preferably 25 μm or less, and more preferably 20 μm or less, from the viewpoint of suppressing the occurrence of peeling or destruction of the coating. The thickness of the entire coating is more preferably 5 μm or more and 25 μm or less, and more preferably 10 μm or more and 20 μm or less.

[0056] The thickness of the coating is measured, for example, by obtaining a cross-sectional sample parallel to the normal direction of the surface of the substrate and observing the sample with a scanning transmission electron microscope (STEM). eThe cross-sectional sample is a thin sample processed using an ion slicer or the like. An example of a scanning transmission electron microscope is JEM-2100F (trademark) manufactured by JEOL Ltd. The measurement conditions are an acceleration voltage of 200 kV and a current of 0.3 nA.

[0057] In this specification, the thickness means the average thickness. Specifically, the observation magnification of the cross-sectional sample is set to 10,000 times, and a rectangular measurement field of view of (100 μm in the direction parallel to the substrate surface) × (distance including the entire thickness of the coating) is set in the electron microscope image, and the thickness width is measured at 10 points in the field of view, and the average value is taken as the "thickness". The thickness (average thickness) of each layer described below is also measured and calculated in the same manner.

[0058] As long as measurements are performed on the same sample, there is almost no variation in the measurement results even if the measurement field of view is changed and performed multiple times, and it has been confirmed that setting the measurement field of view arbitrarily is not arbitrary.

[0059] <Hard particle layer> (Structure of hard particle layer) The hard particle layer of the present embodiment is made of hard particles, and the hard particles have a multilayer structure in which first unit layers and second unit layers are alternately laminated.

[0060] Even if the hard particle layer of this embodiment contains components other than hard particles as unavoidable impurities, such as an amorphous phase or an intermetallic compound (e.g., TiSi2, Co2Si, etc.), it does not deviate from the scope of the present disclosure as long as the effects of the present disclosure are exhibited.

[0061] (Thickness of hard particle layer) The thickness of the hard particle layer in this embodiment is preferably 3 μm or more and 15 μm or less. When the thickness of the hard particle layer is 3 μm or more, it can have excellent wear resistance. On the other hand, when the thickness of the hard particle layer is 15 μm or less, it can suppress the occurrence of peeling or destruction of the coating when a large stress is applied between the coating and the substrate during cutting. The lower limit of the thickness of the hard particle layer is more preferably 4 μm or more, and even more preferably 5 μm or more, from the viewpoint of improving wear resistance. The upper limit of the thickness of the hard particle layer is preferably 15 μm or less, and more preferably 10 μm or less, from the viewpoint of suppressing the occurrence of peeling or destruction of the coating. The thickness of the hard particle layer is more preferably 4 μm or more and 15 μm or less, and even more preferably 5 μm or more and 10 μm or less.

[0062] The first unit layer is made of a first compound having a cubic crystal structure. The second unit layer is made of a second compound having a cubic crystal structure. When the first compound and the second compound have a cubic crystal structure, it is possible to achieve both excellent wear resistance and high toughness. The fact that the first compound and the second compound have a cubic crystal structure can be confirmed by pattern analysis of electron beam diffraction using a selected area.

[0063] Each of the first compound and the second compound is one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; Silicon and and one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen. Here, the composition of the first compound is different from the composition of the second compound, more specifically, the percentage of the number of silicon atoms relative to the total number of metal elements and silicon atoms in the first compound is different from the percentage of the number of silicon atoms relative to the total number of metal elements and silicon atoms in the second compound.

[0064] Even if the first compound and the second compound of the present embodiment contain inevitable impurities, they do not depart from the scope of the present disclosure as long as they exhibit the effects of the present disclosure.

[0065] Each of the first compound and the second compound is, for example, TiSiC, TiSiN, TiSiCN, TiSiNO, TiSiCNO, TiSiBN, TiSiBNO, TiSiCBN, ZrSiC, ZrSiO2, HfSiC, HfSiN, TiCrSiN, TiZrSiN, CrSiN, VSiN 、Zr Examples of the impurities include SiCN, ZrSiCNO, ZrSiN, NbSiC, NbSiN, and NbSiCN. Note that the first compound and the second compound may contain unavoidable impurities without departing from the scope of the present disclosure.

[0066] Whether the hard particles contain a multilayer structure in which first unit layers and second unit layers are alternately laminated can be confirmed by the following methods (A1) to (A6).

[0067] (A1) A cutting tool is used to cut out the substrate along the normal line with a diamond wire, exposing a cross section of the hard particle layer. The exposed cross section is subjected to focused ion beam processing (hereinafter also referred to as "FIB processing") to make the cross section mirror-finished.

[0068] (A2) The FIB-machined cross section is observed using a bright-field scanning electron microscope (BF-SEM) to identify one hard particle. Next, a BE-STEM image of the identified hard particle is obtained. Figure 5 shows an example of a BF-STEM image of one hard particle in the cutting tool of this embodiment.

[0069] (A3) In the above BF-STEM image, the measurement area (size: 100 nm × 100 nm) is set so as to include the area where 10 or more layers of the white layers and the black layers are stacked. In Figure 5, the square area surrounded by a white frame corresponds to the measurement area.

[0070] In FIG. 5, the layers shown in black are regions with a high silicon content, and the layers shown in white are regions with a low silicon content.

[0071] (A4) In the measurement region in the BF-STEM image, the stacking direction of the layer shown in white (hereinafter also referred to as the "white layer") and the layer shown in black (hereinafter also referred to as the "black layer") is identified. Specifically, the electron beam diffraction pattern of the selected visual field region is superimposed on the stacking orientation of the white layer and the black layer, and the stacking orientation is identified from the orientation indicated by the diffraction spot. An electron diffraction image taken in region A shown in Figure 5 is shown in Figure 6. In Figure 5, the stacking direction is indicated by a white arrow.

[0072] (A5) In the measurement area in the BF-STEM image, line analysis is performed along the stacking direction using an SEM-attached EDX (Energy Dispersive X-ray Spectroscopy) to measure the composition. The beam diameter of the line analysis is 0.5 nm or less, the scan interval is 0.5 nm, and the length of the line analysis is 50 nm.

[0073] (A6) When the results of the line analysis satisfy the following (a1) to (a2), it is confirmed that the hard particles include a multilayer structure in which first unit layers and second unit layers are alternately laminated.

[0074] (a1) The measurement region contains one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table, and one or more elements selected from the group consisting of silicon, carbon, nitrogen, boron, and oxygen.

[0075] (a2) The results of the line analysis are shown with the X-axis representing the distance from the measurement start point and the Y-axis representing the number of atoms of the metal element, A. M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M A graph is created in a coordinate system where {A )}×100 in the measurement area. Si / (A Si +A M )}×100 (hereinafter, also referred to as "average") is calculated. As the distance from the measurement start point increases, the average value of {ASi / (A Si +A M )}×100, there are alternating areas with large and small areas.

[0076] An example of the above graph in this embodiment is shown in Fig. 7. Fig. 7 shows the atomic number A of a metal element (titanium) along the arrow direction. M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M 7 is a graph showing the change in {A )}×100. In FIG. 7, the X-axis shows the distance from the measurement start point along the direction of the arrow, and the Y-axis shows the change in {A Si / (A Si +A M )}×100. In FIG. 7, {A Si / (A Si +A M )}×100 average is shown by dotted line L1.

[0077] In Fig. 7, as the distance from the measurement start point increases, the average value of {A Si / (A Si +A M )}×100}×100 is alternately present in an area S1 and an area S2 in which it is small. Therefore, it is confirmed that the hard particle shown in FIG 5 includes a multilayer structure in which the first unit layers and the second unit layers are alternately laminated.

[0078] As long as the measurement is performed on the same sample, even if the hard particles specified in (A2) above are changed and the measurement is performed multiple times, there is almost no variation in the measurement results, and it has been confirmed that the measurement points can be set arbitrarily without being arbitrary.

[0079] It has been confirmed that the effects of the present disclosure are exhibited as long as it is confirmed by the above method that the hard particles include a multilayer structure in which first unit layers and second unit layers are alternately laminated.

[0080] In the following, for ease of understanding, the above (a2) "{ASi / (A Si +A M )}×100 average, Si / (A Si +A M The area where {A )}×100 is large is also referred to as the "first unit layer," and the area where {A Si / (A Si +A M )}×100 average, Si / (A Si +A M )}×100" is also referred to as the "second unit layer."

[0081] (Composition of the first unit layer and the second unit layer) In each of the first unit layer and the second unit layer, the number of atoms of the metal element A M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M )}×100 is preferably 0.5% or more and 10% or less. This improves the thermal crack resistance of the hard particle layer and the adhesion between the hard particle layer and the adjacent layer in a well-balanced manner. Si / (A Si +A M The lower limit of {A )}×100 is preferably 0.5% or more, more preferably 0.7% or more, more preferably 1.0% or more, and even more preferably 1.2% or more. Si / (A Si +A M The upper limit of {A )}×100 is preferably 10.0% or less, more preferably 8.0% or less, more preferably 7.2% or less, more preferably 7% or less, and still more preferably 5% or less. Si / (A Si +A M )}×100 is preferably 0.5% or more and 8.0% or less, more preferably 0.5% or more and 7.2% or less, more preferably 0.7% or more and 7% or less, and more preferably 1.0% or more and 5.0% or less.

[0082] Number of metal atoms in the first unit layer A M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M The lower limit of the number of atoms A of the metal element in the first unit layer is preferably 1% or more, more preferably 1.5% or more, more preferably 2.0% or more, more preferably 5.3% or more, and even more preferably 6.0% or more. M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M The upper limit of the number of atoms A of the metal element in the first unit layer is preferably 10.0% or less, more preferably 9.0% or less, and even more preferably 8.0% or less. M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M From the viewpoint of improving heat resistance, the above {A )}×100 is preferably 1% or more and 10% or less, more preferably 1.5% or more and 9.0% or less, more preferably 2.0% or more and 8.0% or less, more preferably 5.3% or more and 10.0% or less, and more preferably 6.0% or more and 10.0% or less. When the first unit layer has a structure in which the composition changes in the thickness direction, the above {A Si / (A Si +A M )}×100 means the average value in the first unit layer.

[0083] Number of metal atoms in the second unit layer A M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M The lower limit of the number of atoms A of the metal element in the second unit layer is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.5% or more. M and the number of silicon atoms, ASi The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M The upper limit of the number of atoms A of the metal element in the second unit layer is preferably 2.0% or less, more preferably 1.5% or less, still more preferably 1.2% or less, and still more preferably 1.0% or less. M and the number of silicon atoms, A Si The number of silicon atoms, A, relative to the total Si Percentage of {A Si / (A Si +A M From the viewpoint of improving adhesion, the above {A )}×100 is preferably 0.1% or more and 2.0% or less, more preferably 0.5% or more and 2.0% or less, more preferably 0.2% or more and 1.5% or less, more preferably 0.5% or more and 1.5% or less, and more preferably 0.5% or more and 1.0% or less. When the second unit layer has a structure in which the composition changes in the thickness direction, the above {A Si / (A Si +A M )}×100 means the average value in the second unit layer.

[0084] In the first unit layer, {A Si / (A Si +A M )}×100 and {A Si / (A Si +A M )}×100 is preferably 0.5% or more and 10% or less, more preferably 1% or more and 9% or less, more preferably 2% or more and 8% or less, and even more preferably 4% or more and 8% or less, from the viewpoint of improving hardness.

[0085] The first unit layer and the second unit layer may each have a single composition in the thickness direction, or may each have a composition that varies. In this case, the {A Si / (A Si +A M )}×100 is the average of {A Si / (A Si +A M)}×100. In addition, the average of {A Si / (A Si +A M )}×100 is the average of {A Si / (A Si +A M )}×100.

[0086] As long as the measurement is performed on the same sample, even if the hard particles specified in (A2) above are changed and the measurement is performed multiple times, there is almost no variation in the measurement results, and it has been confirmed that the measurement points can be set arbitrarily without being arbitrary.

[0087] ( Many Average composition of layer structure) Many The average composition of the layer structure can be obtained by calculating the average composition of the region where the line analysis was carried out based on the results of the line analysis in (A5) above.

[0088] In the area where the line analysis was performed, Si / (A Si +A M )}×100 is preferably 1% or more and 8% or less, more preferably 1.5% or more and 7.5% or less, and even more preferably 2% or more and 5% or less, from the viewpoint of improving heat resistance.

[0089] In this specification, the above {A Si / (A Si +A M ) × 100 means the average of the values ​​obtained by performing line analysis on three adjacent hard particles.

[0090] (Crystal orientation of the first unit layer and the second unit layer) The first and second unit layers preferably have the same crystal orientation, which reduces the interfacial energy. Examples of the crystal orientation include {311}, {211}, {110}, {100}, and {111}. In the crystallographic descriptions in this specification, {} indicates a collection plane.

[0091] Whether the first unit layer and the second unit layer have the same crystal orientation can be confirmed by the following procedure: An electron diffraction image as shown in Fig. 6 is obtained by the same method as (A1) to (A4) above. If the electron diffraction image is a diffraction image from a single crystal, it is determined that the first unit layer and the second unit layer have the same crystal orientation.

[0092] ( Many Periodic width of layer structure) In this embodiment Many From the viewpoint of maintaining the distortion between unit layers and improving the resistance to defects, the average periodic width of the layer structure is preferably 2 nm or more and 20 nm or less, more preferably 4.1 nm or more and 17.7 nm or less, more preferably 3 nm or more and 15 nm or less, and more preferably 5 nm or more and 10 nm or less. Many The periodic width of the layer structure refers to the distance from one first unit layer to another first unit layer adjacent to the one first unit layer across a second unit layer adjacent to the one first unit layer, where this distance is the distance connecting the midpoints of the first unit layer and the other first unit layer in the thickness direction. Many The average periodic width of the layer structure is the average of all the periodic widths measured within the measurement area set in (A3) above. Many It means the average periodic width of the layer structure.

[0093] In this specification, the method for measuring the periodic width of silicon concentration is as follows. A measurement region is set in the same manner as in (A1) to (A3) above. A Fourier transform is performed on the measurement region to obtain a Fourier transform image. FIG. 8 shows a Fourier transform image obtained by performing a Fourier transform on region A shown in FIG. 5. In the Fourier transform image, the periodicity in the measurement region appears as spots. The periodic width is calculated by calculating the reciprocal of the distance between the spots and the center of the image showing the maximum intensity in the Fourier transform image.

[0094] As long as measurements are performed on the same sample, there is almost no variation in the measurement results even if the measurement points are changed and repeated multiple times, and it has been confirmed that setting measurement points arbitrarily is not arbitrary.

[0095] The number of layers (total number of layers) of the first and second unit layers constituting the multi-layer structure layer is not particularly limited, but is preferably, for example, 10 layers or more and 1000 layers or less. When the number of layers is 10 layers or more, coarsening of crystal grains in each unit layer is suppressed, and the hardness of the hard particles can be maintained. On the other hand, when the number of layers is 1000 layers or less, the thickness of each unit layer can be sufficiently secured, and mixing of the unit layers can be suppressed.

[0096] <Underlayer> The coating includes an underlayer disposed between the substrate and the hard particle layer, the underlayer being made of a third compound, the third compound being: One or more elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and aluminum in the periodic table; and preferably one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen. This improves the adhesion between the coating and the substrate, and also improves the abrasion resistance.

[0097] By disposing a TiN layer, a TiC layer, a TiCN layer, or a TiBN layer directly on the substrate as the underlayer, the adhesion between the substrate and the coating can be improved. By using an Al2O3 layer as the underlayer, the oxidation resistance of the coating can be improved. The underlayer preferably has an average thickness of 0.1 μm or more and 20 μm or less. This allows the coating to have excellent wear resistance and chipping resistance.

[0098] <Surface layer> The coating has a surface layer disposed on the outermost surface thereof, the surface layer being made of a fourth compound, the fourth compound being One or more elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and aluminum in the periodic table; and preferably one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen, which improves the thermal crack resistance and wear resistance of the coating.

[0099] The surface layer is the layer that is disposed on the outermost surface side of the coating. However, the surface layer may not be formed on the cutting edge. The surface layer is disposed directly on the hard particle layer when no other layer is formed on the hard particle layer.

[0100] Examples of surface layers include TiN layers and Al2O3 layers. The TiN layer has a clear color (golden color), so when used as a surface layer, it has the advantage that it is easy to identify the corners of the cutting tip after cutting (identify the used parts). By using an Al2O3 layer as a surface layer, the oxidation resistance of the coating can be improved.

[0101] The surface layer preferably has an average thickness of 0.05 μm or more and 1 μm or less, which improves the adhesion between the surface layer and the adjacent layers.

[0102] <Middle Class> The intermediate layer is a layer disposed between the underlayer and the hard particle layer. When the underlayer is a TiN layer, the intermediate layer is preferably a TiCN layer. The TiCN layer has excellent wear resistance, and can impart more suitable wear resistance to the coating. The intermediate layer preferably has an average thickness of 1 μm or more and 20 μm or less.

[0103] [Embodiment 2: Manufacturing method of cutting tool] The method for manufacturing the cutting tool of this embodiment will be described with reference to Fig. 10. Fig. 10 is a schematic cross-sectional view of an example of a CVD apparatus used in manufacturing the cutting tool of this embodiment.

[0104] A method for manufacturing a cutting tool according to the present embodiment is the method for manufacturing the cutting tool according to the first embodiment, A first step of preparing a substrate; A second step of forming a coating on the substrate to obtain a cutting tool, The second step includes a step 2a of forming a hard particle layer made of hard particles by a CVD method, The step 2a includes a step 2a-1 of ejecting a first source gas, a second source gas, and a third source gas toward a surface of the substrate, the first source gas contains one or more elements selected from the group consisting of Group 4 elements, Group 5 elements, and Group 6 elements of the periodic table; The second source gas is SiCl4, the third source gas contains one or more elements selected from the group consisting of carbon, nitrogen, boron, and oxygen; the first source gas is ejected from a plurality of first injection holes provided in a nozzle, the second source gas is ejected from a plurality of second injection holes provided in the nozzle, the third source gas is ejected from a plurality of third injection holes provided in the nozzle, In the step 2a-1, the nozzle rotates, the plurality of second injection holes include a 2-1 injection hole and a 2-2 injection hole, A method for manufacturing a cutting tool, wherein a diameter r1 of the 2-1 ejection hole is different from a diameter r2 of the 2-2 ejection hole.

[0105] (1st step) In the first step, a substrate is prepared. Details of the substrate are described in the first embodiment, and therefore the description will not be repeated.

[0106] (2nd process) Next, in the second step, a coating is formed on the substrate to obtain a cutting tool. The coating is formed, for example, by using a CVD apparatus shown in FIG. 10. A plurality of substrate setting jigs 52 holding substrates 10 can be installed in the CVD apparatus 50, which are covered by a reaction vessel 53 made of heat-resistant alloy steel. A temperature control device 54 is disposed around the reaction vessel 53, and the temperature control device 54 can control the temperature inside the reaction vessel 53.

[0107] A nozzle 56 having three inlets 55, 57 (the other inlet is not shown) is disposed in the CVD apparatus 50. The nozzle 56 is disposed so as to penetrate the area in which the substrate setting jig 52 is disposed. A plurality of injection holes (a first injection hole 61, a second injection hole 62, and a third injection hole (not shown)) are formed in a portion of the nozzle 56 near the substrate setting jig 52.

[0108] 10, the gases introduced into nozzle 56 from inlets 55, 57, and another inlet (not shown) are not mixed in nozzle 56 either, and are introduced into reaction vessel 53 via different injection holes. Nozzle 56 can rotate about its axis. An exhaust pipe 59 is provided in CVD apparatus 50, and exhaust gas can be discharged to the outside from exhaust port 60 of exhaust pipe 59. Fixtures and the like in reaction vessel 53 are usually made of graphite.

[0109] When the coating includes an undercoat layer, an intermediate layer and / or a surface layer, these layers can be formed by a conventionally known method.

[0110] (Step 2a) The second step includes a 2a step of forming a hard particle layer made of hard particles by a CVD method, and the 2a step includes a 2a-1 step of ejecting a first source gas, a second source gas, and a third source gas toward the surface of the substrate.

[0111] The first source gas includes one or more elements selected from the group consisting of Group 4, Group 5, and Group 6 elements of the periodic table. The first source gas is, for example, a chloride gas of Group 4, Group 5, or Group 6 element of the periodic table. More specifically, TiCl4, ZrCl4, VCl4, CrCl3, and a mixed gas containing two or more of these can be mentioned. The second source gas is SiCl4. The third source gas is, for example, CH3CN, CH4, N2, NH3, BCl3, H2O, and a mixed gas containing two or more of these.

[0112] The first source gas is ejected from a plurality of first injection holes provided in the nozzle, the second source gas is ejected from a plurality of second injection holes provided in the nozzle, and the third source gas is ejected from a plurality of third injection holes provided in the nozzle. Specifically, the first source gas is introduced into the nozzle 56 from the inlet 55 of the nozzle and ejected from the plurality of first injection holes 61. The second source gas is introduced into the nozzle 56 from the inlet 57 of the nozzle and ejected from the plurality of second injection holes 62. The third source gas is introduced into the nozzle 56 from an inlet (not shown) of the nozzle and ejected from a plurality of third injection holes (not shown).

[0113] In the second a-1 step, the nozzle rotates, and the plurality of second injection holes include a second-1 injection hole and a second-2 injection hole, and the diameter r1 of the second-1 injection hole is different from the diameter r2 of the second-2 injection hole. According to this, the hard particles have a multilayer structure including a first unit layer and a second unit layer, and the percentage of the number of silicon atoms to the total number of metal element and silicon atoms in the first unit layer is different from the percentage of the number of silicon atoms to the total number of metal element and silicon atoms in the second unit layer. A multilayer structure can be included. Hereinafter, for ease of understanding, it will be described with r1 < r2.

[0114] The diameter r1 of the second-1 injection hole is preferably 0.5 mm or more and 3 mm or less, more preferably 1 mm or more and 2.5 mm or less, and still more preferably 1.5 mm or more and 2 mm or less. The diameter r2 of the second-2 injection hole is preferably 1 mm or more and 4 mm or less, more preferably 1.5 mm or more and 3.5 mm or less, and still more preferably 2 mm or more and 3 mm or less.

[0115] The lower limit of the ratio r1 / r2 of the diameter r1 of the second-1 injection hole to the diameter r2 of the second-2 injection hole is preferably 0.125 or more, more preferably 0.2 or more, and still more preferably 0.5 or more. The upper limit of r1 / r2 is preferably less than 1, preferably 0.8 or less, and preferably 0.6 or less. r1 / r2 is preferably 0.125 or more and less than 1, preferably 0.2 or more and 0.8 or less, and preferably 0.5 or more and 0.6 or less.

[0116] In this step, the temperature of the substrate in the reaction vessel is preferably in the range of 700 to 900°C, and the pressure in the reaction vessel is preferably 0.1 to 13 kPa. In addition, H2 gas, N2 gas, Ar gas, etc. can be used as the carrier gas. The composition of the first unit layer and the second unit layer can be controlled by the mixing ratio of the raw material gas and the ratio r1 / r2 of the diameter r1 of the 2-1 injection hole and the diameter r2 of the 2-2 injection hole. The thickness of the hard particle layer can be controlled by adjusting the flow rate of the raw material gas and the film formation time. The thickness of each of the first unit layer and the second unit layer, the lamination period thereof, and the number of laminations thereof can be controlled by adjusting the rotation speed of the nozzle and the film formation time.

[0117] During the formation of the hard particle layer, the total gas flow rate of the reactive gas can be, for example, 70 to 90 L / min. Here, the "total gas flow rate" refers to the total volumetric flow rate introduced into the CVD furnace per unit time, assuming that the gas under standard conditions (0°C, 1 atm) is an ideal gas.

[0118] (Other processes) Next, the substrate 10 on which the coating has been formed is cooled. The cooling rate does not exceed, for example, 5° C. / min, and the cooling rate becomes slower as the temperature of the substrate 10 decreases.

[0119] In addition to the above steps, a heat treatment step such as annealing, and a surface treatment step such as surface grinding and shot blasting may be carried out.

[0120] The cutting tool of the first embodiment can be obtained by the above-described manufacturing method. EXAMPLES

[0121] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.

[0122] <Preparing the substrate (first step)> Substrate A shown in Table 1 below was prepared. Specifically, first, raw material powders having the composition (mass%) shown in Table 1 were uniformly mixed to obtain a mixed powder. "Remainder" in Table 1 indicates that WC occupies the remainder of the composition (mass%). Next, the mixed powder was pressure-molded into the shape of SEMT13T3AGSR-G (a replaceable cutting tip manufactured by Sumitomo Electric Hardmetal Corporation), and then sintered at 1300 to 1500°C for 1 to 2 hours to obtain substrate A made of cemented carbide. Substrate A had the shape of SEMT13T3AGSR-G.

[0123] [Table 1]

[0124] <Formation of coating (second process)> A coating was formed on the surface of the substrate A obtained above. Specifically, using the CVD apparatus shown in FIG. 10, the substrate was set in a substrate setting jig, and a thermal CVD method was performed to form a coating on the substrate. The composition of the coating for each sample is shown in Table 2. A column marked with "-" in Table 2 indicates that no layer was present.

[0125] [Table 2]

[0126] The underlayer (TiN layer), intermediate layer (TiCN layer) and surface layer (Al2O3 layer) shown in Table 2 are layers formed by a conventionally known CVD method, and the deposition conditions are as shown in Table 3. For example, the "TiN (underlayer)" row in Table 3 shows the deposition conditions for the TiN layer as the underlayer. The description of the TiN layer (underlayer) in Table 3 means that the substrate is placed in a reaction vessel of a CVD apparatus (pressure in reaction vessel 6.7 kPa, substrate temperature 915°C), and a mixed gas consisting of 2.0 vol% TiCl4 gas, 39.7 vol% N2 gas and the remaining (58.3 vol%) H2 gas is sprayed into the reaction vessel at a flow rate of 63.8 L / min to form a TiN layer. The thickness of each layer formed under each deposition condition was controlled by the time for spraying each reaction gas.

[0127] [Table 3]

[0128] Coating condition A in the hard particle layer column of Table 2 、D ~G, X and Y are the deposition conditions A in Table 4. 、D 1 to G, which correspond to the deposition conditions X and Y in Table 5. For example, the hard particle layer of sample 1 is a layer formed under deposition condition A in Table 4, and the numerical value in parentheses means that the thickness of the hard particle layer is 4.5 μm.

[0129] [Table 4]

[0130] (Deposition conditions A 、 Film formation conditions D~ G) Film formation condition A 、 Film formation conditions D~ In G, a hard particle layer is formed using the CVD apparatus shown in FIG. 10. The nozzle of the CVD apparatus is provided with a first injection hole, a second injection hole (2-1 injection hole and 2-2 injection hole), and a third injection hole. The diameter φr1 of the 2-1 injection hole and the diameter φr2 of the 2-2 injection hole in the nozzle of the CVD apparatus used under each film formation condition are shown in the "Injection hole diameter φ (mm) r1 / r2" column of Table 4. For example, under film formation condition A, the diameter φr1 of the 2-1 injection hole is 1.5 mm, and the diameter φr2 of the 2-2 injection hole is 2.5 mm. The nozzle rotates during film formation.

[0131] Film formation condition A 、 Film formation conditions D~ In G, first, the pressure in the reaction vessel of the CVD apparatus is set to the pressure shown in the "Pressure (kPa)" column of Table 4, and the substrate temperature is set to the temperature shown in the "Temperature (°C)" column of Table 4. For example, in film formation condition A, the pressure in the reaction vessel of the CVD apparatus is set to 9.0 kPa, and the substrate temperature is set to 800°C.

[0132] Next, a reaction gas containing the components shown in the "Reaction gas composition (volume %)" column of Table 4 is introduced into the reaction vessel to form a hard particle layer on the substrate. "Remainder" in Table 4 indicates that H2 gas occupies the remainder of the reaction gas composition (volume %). Among the reaction gases, TiCl4, ZrCl4, VCl4, and CrCl3 are the first source gas, SiCl4 is the second source gas, and CH3CN and BCl3 are the third source gas. H2 is mixed into the third source gas to adjust the total gas flow rate.

[0133] Film formation condition A 、 Film formation conditions D~ In G, the total gas flow rate of the reactive gas is 80 L / min. The "total gas flow rate" refers to the total volumetric flow rate introduced into the CVD furnace per unit time, assuming that the gas is an ideal gas under standard conditions (0°C, 1 atm). For example, the reactive gas used in film formation condition A consists of 1 vol% SiCl4 gas, 1 vol% TiCl4 gas, 0.5 vol% CH3CH gas, and H2 gas (the remainder, 97.5 vol%).

[0134] The rotation speed of the nozzle during film formation is as shown in the "Rotation speed (rpm)" column in Table 4. For example, under film formation condition A, the rotation speed of the nozzle is 2.0 rpm.

[0135] The substrate is then cooled.

[0136] (Film forming condition X) Under film-forming condition X, a hard particle layer is formed using a conventional CVD apparatus. The nozzles of the CVD apparatus all have the same injection hole diameter φ of 10 mm. The nozzles do not rotate during film formation.

[0137] In the film formation condition X, the pressure inside the reaction chamber of the CVD apparatus is initially set to 6 kPa, and the substrate temperature is initially set to 800°C.

[0138] Next, a reaction gas (SiCl4: 0.84 vol%, TiCl4: 0.17 vol%, CH3CN: 0.32 vol%, H2: remainder) containing the components listed in the "Reaction gas composition (vol%)" column of Table 5 is introduced into the reaction vessel to form a TiSiCN layer (hard particle layer) on the substrate. The total gas flow rate of the reaction gas is 80 L / min. The substrate is then cooled.

[0139] (Film forming condition Y) In the deposition condition Y, the hard particle layer is formed by a conventional PVD method. Specific conditions of the deposition condition Y are as shown in the column of “Deposition condition Y” in Table 5.

[0140] From the above, Sample 1 , Sample 4 to Sample 15 (corresponding to the working example) and cutting tools of Samples 1-1 to 1-4 (corresponding to the comparative examples) were obtained.

[0141] [Table 5]

[0142] <Characteristics of the hard particle layer> (Structure of hard particle layer) Film formation condition A 、 Film formation conditions D~ When the hard particle layer of the coating obtained under G was observed with a bright field scanning electron microscope (BF-SEM), it was confirmed that the hard particle layer was composed of a plurality of hard particles and that a multi-layer structure was present within the hard particles. 、 Film formation conditions D~ It was confirmed that the multilayer structure of the hard particle layer obtained by G was formed by alternating layers (first unit layer) in which the percentage of the number of silicon atoms to the total number of metal elements and silicon atoms is large, and layers (second unit layer) in which the percentage of the number of silicon atoms to the total number of metal elements and silicon atoms is small.

[0143] Film formation condition A 、 Film formation conditions D~ It was confirmed that the first unit layer and the second unit layer in the hard particle layer obtained by G had the same crystal orientation.

[0144] When the hard particle (TiCN) layer obtained under film formation condition X was observed with a bright-field scanning electron microscope (BF-SEM), it was found to have a uniform structure and no periodic changes were observed.

[0145] When the hard particle layer obtained under the deposition condition Y was observed with a bright-field scanning electron microscope (BF-SEM), a nanocomposite structure was confirmed.

[0146] ( Many Average composition of layer structure, {A Si / (A Si +A M )}×100(%), {A Si / (A Si +A M )}×100(%)) Regarding the hard particle layers obtained under each deposition condition, Many The average composition of the layer structure, the percentage of the number of silicon atoms to the total number of metal elements and silicon atoms in the first unit layer (Si / Me+Si(%)), and the percentage of the number of silicon atoms to the total number of metal elements and silicon atoms in the second unit layer ({A Si / (A Si +A M )}×100(%)) was measured. The specific measurement method is as described in the first embodiment, and therefore the description thereof will not be repeated. The results are shown in Table 6 under the headings "Average composition," "First unit layer {A Si / (A Si +A M )}×100(%)" and "Second unit layer {A Si / (A Si +A M )}×100(%)" in the "Table 1" column. "-" indicates that the measurement was not performed.

[0147] (period width) The average periodic width of the multilayer structure was measured for the hard particle layers obtained under each film formation condition. The specific measurement method is as described in the first embodiment, and therefore the description will not be repeated. The results are shown in the "Average periodic width (nm)" column of Table 6. The notation "-" indicates that the measurement was not performed.

[0148] [Table 6]

[0149] <Cutting test 1> Sample 1 , Sample 4 to Sample 10 Cutting was performed under the following cutting conditions using cutting tools of Sample 1-1 and Sample 1-3, and the cutting distance until the cutting edge of the tool was chipped was measured. The following cutting conditions apply to the milling (dry machining) of high-hardness heat-resistant stainless steel. The longer the cutting distance, the longer the tool life. The results are shown in Table 7.

[0150] <Cutting conditions> Workpiece: SUS630 / H900 block material (dimensions: 300mm x 150mm x 50mm) Cutter: WGX13100RS (Sumitomo Electric Hardmetal) Insert: SEMT13T3AGSR-G Cutting speed Vc:300m / min Feed per tooth Fz: 0.1mm / t Cutting depth Ap: 1.0mm Cutting width Ae:75mm Cutting fluid: None (Dry)

[0151] [Table 7]

[0152] (Rating 1) Sample 1 , Sample 4 to Sample 10 It was confirmed that the cutting distance and tool life of the (Example) was longer in the milling (dry milling) of high-hardness heat-resistant stainless steel than those of Sample 1-1 and Sample 1-3 (Comparative Example). , Sample 4 to Sample 10 It is presumed that the reason for this is that the hard particles contain a multilayer structure, which improves the thermal crack propagation resistance and peeling resistance.

[0153] <Cutting test 2> Sample 11 ~ Sample 15Cutting was performed under the following cutting conditions using cutting tools of Sample 1-2 and Sample 1-4, and the cutting distance until the tool tip was chipped was measured. The following cutting conditions apply to milling (wet machining) of high-hardness heat-resistant stainless steel. The longer the cutting distance, the better the heat resistance and the longer the tool life. The results are shown in Table 8.

[0154] <Cutting conditions> Workpiece: SUS640 / H900 block material (dimensions: 300mm x 150mm x 50mm) Cutter: WGX13100RS (Sumitomo Electric Hardmetal) Insert: SEMT13T3AGSR-G Cutting speed Vc:150m / min Feed per tooth fz: 0.3mm / t Cutting depth ap: 1.0mm Cutting width ae: 75mm Cutting fluid: WET

[0155] [Table 8]

[0156] (Rating 2) Sample 11 ~ Sample 15 It was confirmed that the cutting distance and tool life of the (Example) was longer in the milling (wet milling) of high-hardness heat-resistant stainless steel than those of Sample 1-2 and Sample 1-4 (Comparative Example). 15 It is presumed that the reason for this is that the hard particles contain a multilayer structure, which improves the thermal crack propagation resistance and peeling resistance.

[0157] Although the embodiments and examples of the present disclosure have been described above, it is intended from the outset that the configurations of the above-described embodiments and examples may be appropriately combined or modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered as limiting. The scope of the present invention is indicated by the claims, not by the embodiments and examples described above, and is intended to include the meaning equivalent to the claims and all modifications within the scope. [Explanation of symbols]

[0158] 1, 21, 31, 41 cutting tool, 10 substrate, 11 hard particle layer, 12 undercoat layer, 13 surface layer, 14 intermediate layer, 15, 25, 35, 45 coating, 50 CVD device, 52 substrate setting jig, 53 reaction vessel, 54 temperature control device, 55, 57 inlet, 56 nozzle, 59 exhaust pipe, 60 exhaust port, 61 first injection hole, 62 second injection hole

Claims

1. 1. A cutting tool comprising a substrate and a coating disposed on the substrate, the coating includes a hard particle layer made of hard particles, The hard particles include a multilayer structure in which first unit layers and second unit layers are alternately laminated, the first unit layer is made of a first compound having a cubic crystal structure, the second unit layer is made of a second compound having a cubic crystal structure, the first compound and the second compound are the same compound, the identical compound is TiSiCN, TiSiCBN, TiZrSiCN, TiVSiCN, or TiCrSiCN; The number A of atoms of the metal element in the first unit layer M and the number of silicon atoms A Si The number of silicon atoms A relative to the total Si Percentage of {A Si / (A Si +A M )} × 100 is 5.3% or more and 10.0% or less, The number A of atoms of the metal element in the second unit layer M and the number of silicon atoms A Si The number of silicon atoms A relative to the total Si Percentage of {A Si / (A Si +A M )} × 100 is 0.5% or more and 2.0% or less, The percentage {A Si / (A Si +A M )}×100, and the percentage {A Si / (A Si +A M )) × 100 is 4% or more and 8% or less, The number A of atoms of the metal element in the multilayer structure M and the number of silicon atoms A Si The number of silicon atoms A relative to the total Si Percentage of {A Si / (A Si +A M )} × 100 is 2% or more and 7% or less, A cutting tool, wherein the average periodic width of the multilayer structure is 5 nm or more and 10 nm or less.

2. The cutting tool according to claim 1 , wherein the first unit layer and the second unit layer have the same crystal orientation.

3. The thickness of the hard particle layer is 3 μm or more and 15 μm or less, 3. The cutting tool according to claim 1, wherein the coating has a thickness of 3 μm or more and 30 μm or less.

4. The coating includes a base layer disposed between the substrate and the hard particle layer, the underlayer is made of a third compound, The third compound is one or more elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and aluminum in the periodic table; The cutting tool according to claim 1 , further comprising one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen.

5. The coating includes an undercoat layer disposed directly over the substrate; The underlayer may be a TiN layer, a TiC layer, a TiCN layer, a TiBN layer, or an Al 2 O 3 The cutting tool according to claim 1 , comprising at least one layer selected from the group consisting of layers.

6. The coating has a surface layer disposed on its outermost surface, the surface layer is made of a fourth compound, The fourth compound is one or more elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and aluminum in the periodic table; and one or more elements selected from the group consisting of carbon, nitrogen, boron and oxygen.

7. The cutting tool according to claim 4 or 5, wherein the coating has an intermediate layer disposed between the base layer and the hard particle layer.

8. A method for manufacturing a cutting tool according to any one of claims 1 to 7, comprising the steps of: A first step of preparing a substrate; A second step of forming a coating on the substrate to obtain a cutting tool, The second step includes a 2a step of forming a hard particle layer made of hard particles by a CVD method, The 2a step includes a 2a-1 step of ejecting a first source gas, a second source gas, and a third source gas toward a surface of the substrate, the first source gas contains one or more elements selected from the group consisting of titanium, zirconium, vanadium, and chromium; The second source gas is SiCl 4 and the third source gas contains one or more elements selected from the group consisting of carbon, nitrogen, and boron; The first source gas is ejected from a plurality of first injection holes provided in a nozzle, the second source gas is ejected from a plurality of second injection holes provided in the nozzle, the third source gas is ejected from a plurality of third injection holes provided in the nozzle, In the 2a-1 step, the nozzle rotates, The plurality of second injection holes include a 2-1 injection hole and a 2-2 injection hole, A method for manufacturing a cutting tool, wherein a diameter r1 of the 2-1 injection hole is different from a diameter r2 of the 2-2 injection hole.

Citation Information

Patent Citations

  • Hard film coated member

    JP2006307323A

  • Hard material coatings of metals, hard metals, cermets or ceramics, and methods for manufacturing such objects.

    JP2015505902A

  • Surface-coated cubic boron nitride sintered tool

    JP2018094670A

  • Hard material coated body made of metal, cemented carbide, cermet or ceramic, and method for manufacturing said body

    JP2020507679A

  • Surface-coated cutting tool and process for producing same

    WO2019239654A1