Microcrosslinked modified polyamino acid derivative and thickening composition

A slightly crosslinked modified polyamino acid derivative with balanced hydrophilic and hydrophobic groups addresses viscosity instability and enhances thickening properties, ensuring stability and effectiveness in cosmetic applications.

JP7568175B1Active Publication Date: 2024-10-16DIC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024534449
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2024-01-29
Publication Date
2024-10-16
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

Existing polyamino acid derivatives, such as crosslinked polyaspartic acid, suffer from insufficient thickening effect and viscosity instability, particularly in weakly acidic conditions common in skin care products, and there is a lack of a well-balanced structure that maintains viscosity while enhancing thickening properties.

Method used

A slightly crosslinked modified polyamino acid derivative is developed with a specific ratio of hydrophilic and hydrophobic groups and a trace amount of crosslinked structure, achieved through a controlled crosslinking process using polyfunctional amines, to maintain viscosity and stability.

Benefits of technology

The derivative achieves both high thickening power and storage stability by promoting hydrophobic-hydrophobic interactions, maintaining viscosity over time even in weakly acidic conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568175000001
    Figure 0007568175000001
  • Figure 0007568175000002
    Figure 0007568175000002
  • Figure 0007568175000003
    Figure 0007568175000003
Patent Text Reader

Abstract

By introducing a hydroxyl group as a hydrophilic group and a long-chain alkyl group as a hydrophobic group, having a certain hydroxyl value, and introducing a trace amount of crosslinked structure, it is possible to provide a slightly crosslinked modified polyamino acid derivative that has a higher viscosity and maintains a certain level of viscosity for a longer period of time, and that achieves both thickening power and storage stability. The slightly crosslinked modified polyamino acid derivative of the present invention contains a monomer unit AU represented by the following general formula (1), a monomer unit BU represented by the following general formula (2), and a monomer unit Crosslink-U represented by the following general formula (3). The ratio (AU) / (BU) of the molar percentage of the monomer unit AU to the molar percentage of the monomer unit BU is 40 / 60 to 60 / 40. The hydroxyl value is 80 to 170 mgKOH / g, and the crosslinking amount is 0.1 to 2.0 mol%. [C1] TIFF0007568175000017.tif44170 (In the formula, R1 represents a hydrocarbon group having 3 to 22 carbon atoms. R2 represents a hydroxyalkyl group having 2 to 8 carbon atoms. The wavy lines represent crosslinking sites.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a slightly crosslinked modified polyamino acid derivative and a thickening composition. This application claims priority based on Japanese Patent Application No. 2023-047050, filed on March 23, 2023, the contents of which are incorporated herein by reference. [Background technology]

[0002] Carbomer, a polyacrylic acid-based thickener, is the most widely used cosmetic thickener on the market. Carbomer has features not found in other thickeners, including extremely high viscosity and a refreshing feel when applied to the skin. Polyaspartic acid has a similar chemical structure to polyacrylic acid and may be able to exhibit similar functions. In addition, because it is biodegradable, it is expected to be an alternative material with less environmental impact. For example, a nonionic polyamino acid derivative has been reported that does not lose its thickening or foaming effect even in the presence of salt (Patent Document 1). On the other hand, polyamino acid derivatives having a crosslinked structure in the polyamino acid main chain have been reported (Patent Documents 2 and 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4546158 [Patent Document 2] JP 2002-179791 A [Patent Document 3] International Publication No. 2006 / 062207 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the thickening effect of Patent Document 1 is insufficient. In addition, in Patent Document 2, the non-derivatized crosslinked polyaspartic acid is easily hydrolyzed in water, making it difficult to maintain viscosity. When the crosslinked polyaspartic acid of Patent Document 2 is used as a thickener, there is a problem that the viscosity decreases over time when it is mixed in water to prepare a thickened solution. The decrease in viscosity is particularly remarkable in the weak acid range that is common in skin care products. On the other hand, in Patent Document 3, the purpose of providing a crosslinked structure to the polyamino acid main chain is to increase the molecular weight, thereby strengthening the film when used as a forming agent for hair styling products, etc., and to obtain a resin with high setting power. There was no disclosure of focusing on the relationship between the crosslinked structure and the non-crosslinked structure of the polyamino acid main chain and designing them in a well-balanced manner in order to maintain viscosity stability while increasing the thickening effect.

[0005] The present invention has been made to solve the above-mentioned problems, and aims to provide a micro-crosslinked modified polyamino acid derivative and a thickening composition which exhibit thickening properties due to hydrophobic-hydrophobic interactions caused by long-chain alkyl groups in the side chains, while simultaneously achieving both a thickening effect and viscosity stability by introducing a certain amount of hydrophilic side chains and a micro-crosslinked structure. [Means for solving the problem]

[0006] The present disclosure includes the following embodiments [1] to [9]. [1] A slightly crosslinked modified polyamino acid derivative comprising an α- or β-polyaspartic acid monomer unit AU represented by the following general formula (1), an α- or β-polyaspartic acid monomer unit BU represented by the following general formula (2), and a crosslinking portion Crosslink-U represented by the following general formula (3): In the slightly crosslinked modified polyamino acid derivative, the ratio (AU) / (BU) of the molar percentage of the monomer unit AU to the molar percentage of the monomer unit BU is 40 / 60 to 60 / 40; The hydroxyl value of the slightly crosslinked modified polyamino acid derivative is 80 to 170 mgKOH / g; The slightly crosslinked modified polyamino acid derivative has a crosslinking amount of 0.1 to 2.0 mol %. [ka] (In the formula, R1 represents a hydrocarbon group having 3 to 22 carbon atoms.) [ka] (In the formula, R2 represents a hydroxyalkyl group having 2 to 8 carbon atoms. The hydroxyalkyl group may contain a heteroatom. In addition, in the formula, -NH-R2 may be -NR2-R3, where R3 is a hydrocarbon group having 1 to 6 carbon atoms. In addition, the -NR2-R3 may be a cyclic amino group in which R2 and R3 are covalently bonded.) [ka] (In the formula, the wavy lines indicate crosslinking sites.) [2] Contains a succinimide monomer unit CU represented by the following general formula (4): The slightly crosslinked modified polyamino acid derivative according to [1], wherein the ratio of the molar percentage of the monomer unit CU to the total molar percentage of the monomer unit AU and the monomer unit BU, [(AU)+(BU)] / (CU), is 80 / 20 to 99 / 1. [ka] [3] The slightly crosslinked modified polyamino acid derivative according to [1] or [2], wherein the amount of crosslinking of the slightly crosslinked modified polyamino acid derivative is 0.5 to 1.8 mol %, and the hydroxyl value of the slightly crosslinked modified polyamino acid derivative is 90 to 130 mgKOH / g. [4] The crosslinking portion Crosslink-U represented by the general formula (3) is a structure containing a structure derived from a crosslinking agent, The slightly cross-linked modified polyamino acid derivative according to any one of [1] to [3], wherein the cross-linking agent is a polyfunctional amine. [5] The slightly cross-linked modified polyamino acid derivative according to [4], wherein the cross-linking agent is an ether-based diamine or a tris(2-aminoalkyl)amine. [6] The slightly crosslinked modified polyamino acid derivative according to [4] or [5], wherein the crosslinking agent is at least one selected from the group consisting of 1,2-bis(2-aminoethoxy)ethane (AEE), bis[2-(3-aminopropoxy)ethyl ether (APEE), and tris(2-aminoethyl)amine (TREN). [7] A thickening composition comprising the slightly crosslinked modified polyamino acid derivative according to any one of [1] to [6]. [8] The thickening composition according to [7], further comprising water. [9] A thickening composition according to [7] or [8], A cosmetic active ingredient, A cosmetic composition comprising: Effect of the Invention

[0007] According to the present invention, by introducing a hydroxyl group as a hydrophilic group and a long-chain alkyl group as a hydrophobic group, and by introducing a small amount of crosslinked structure into a microcrosslinked modified polyamino acid derivative having a certain hydroxyl value, it is possible to provide a microcrosslinked modified polyamino acid derivative and a thickening composition which have a higher viscosity and maintain a certain level of viscosity for a longer period of time, thereby achieving both thickening power and storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in more detail below. Note that the present invention is not limited to the following embodiments.

[0009] "~" means greater than or equal to the value before the "~", and less than or equal to the value after the "~".

[0010] (Slightly cross-linked modified polyamino acid derivative) A slightly crosslinked modified polyamino acid derivative according to one embodiment of the present invention comprises an α- or β-polyaspartic acid monomer unit AU represented by the following general formula (1), an α- or β-polyaspartic acid monomer unit BU represented by the following general formula (2), and a crosslinking portion Crosslink-U represented by the following general formula (3). The crosslinking portion Crosslink-U preferably comprises a structure derived from a crosslinking agent (this will be described in detail in the synthesis method below). The term "slightly cross-linked modified polyamino acid derivative" refers to a modified polyamino acid derivative having a cross-linking amount of 0.1 to 2.0 mol %. The term "slightly cross-linked" is distinguished from normal "cross-linked" having a cross-linking amount of more than 2.0 mol %.

[0011] [ka] (In the formula, R1 represents a hydrocarbon group having 3 to 22 carbon atoms.)

[0012] [ka] (In the formula, R2 represents a hydroxyalkyl group having 2 to 8 carbon atoms. The hydroxyalkyl group may contain a heteroatom. In addition, in the formula, -NH-R2 may be -NR2-R3, where R3 is a hydrocarbon group having 1 to 6 carbon atoms. In addition, the -NR2-R3 may be a cyclic amino group in which R2 and R3 are covalently bonded.)

[0013] [ka] (In the formula, the wavy lines indicate crosslinking sites.)

[0014] Furthermore, the slightly crosslinked modified polyamino acid derivative of the present invention preferably contains, in addition to the monomer units AU, BU, and Crosslink-U, a succinimide monomer unit CU represented by the following general formula (4) as a repeating unit.

[0015] [ka]

[0016] In the general formula (1), R1 is not particularly limited as long as it is a group containing a hydrocarbon group having 3 to 22 carbon atoms, and the hydrocarbon group having 3 to 22 carbon atoms may be saturated or unsaturated. Examples of the hydrocarbon group having 3 to 22 carbon atoms include linear alkyl groups such as propyl group, butyl group, pentyl group, hexyl group, octyl group, dodecyl group, and octadecyl group; branched alkyl groups such as isopropyl group, isobutyl group, isopentyl group, and isohexyl group; cycloalkyl groups such as cyclobutyl group, cyclopentyl group, and cyclohexyl group; cycloalkylalkyl groups such as cyclobutylmethyl group, cyclopentylmethyl group, cyclohexylmethyl group, cyclobutylethyl group, cyclopentylethyl group, cyclohexylethyl group, cyclobutylpropyl group, cyclopentylpropyl group, cyclohexylpropyl group, cyclobutylbutyl group, cyclopentylbutyl group, and cyclohexylbutyl group; and alkenyl groups such as propenyl group, butenyl group, pentenyl group, and hexenyl group. Of these, alkyl groups are preferred.

[0017] The number of carbon atoms in the hydrocarbon group having 3 to 22 carbon atoms is preferably 6 to 20, and more preferably 8 to 18. The hydrocarbon group having 3 to 22 carbon atoms may be branched or linear, and is preferably linear.

[0018] In the general formula (2), R2 is not particularly limited as long as it is a hydroxyalkyl group having 2 to 8 carbon atoms. Examples of the hydroxyalkyl group include a hydroxyethyl group, a hydroxypropyl group, a hydroxybutyl group, a hydroxypentyl group, a hydroxyhexyl group, a hydroxyheptyl group, and a hydroxyoctyl group.

[0019] In addition, the hydroxyalkyl group having 2 to 8 carbon atoms in R2 may contain a heteroatom, which may be one or more selected from the group consisting of a nitrogen atom, an oxygen atom, and a sulfur atom. Examples of the hydroxyalkyl group having 2 to 8 carbon atoms and containing a heteroatom include the above-mentioned hydroxyalkyl group having 2 to 8 carbon atoms in which one or more hydrogen atoms are substituted with a substituent containing a heteroatom. The substituent containing a heteroatom includes one or more selected from the group consisting of a hydroxy group (-OH), an amino group (-NH2), and a thiol group (-SH). Examples of hydroxyalkyl groups having 2 to 8 carbon atoms substituted with a heteroatom-containing substituent include dihydroxyalkyl groups such as dihydroxyethyl groups, dihydroxypropyl groups, and dihydroxybutyl groups; and polyhydroxyalkyl groups such as groups obtained by removing the amino group (-NH2-) from D-glucamine. In addition, examples of the hydroxyalkyl group having 2 to 8 carbon atoms and containing a heteroatom include the above-mentioned hydroxyalkyl group having 2 to 8 carbon atoms interrupted by a heteroatom. The interrupted heteroatom may be one or more selected from the group consisting of -O-, -N-, and -S-. Specific examples of the hydroxyalkyl group having 2 to 8 carbon atoms interrupted by a heteroatom include hydroxyalkoxyalkyl groups such as a hydroxyethoxyethyl group (-CH2CH2OCH2CH2OH), a hydroxyethoxypropyl group (-CH2CH2CH2OCH2CH2OH), a hydroxyethoxybutyl group (-CH2CH2CH2CH2OCH2CH2OH), a hydroxyethoxypentyl group (-CH2CH2OCH2CH2CH2OCH2CH2OH), a hydroxypropoxypropyl group (-CH2CH2CH2OCH2CH2CH2OH), and a hydroxypropoxybutyl group (-CH2CH2CH2CH2OCH2CH2CH2OH).

[0020] Among these, R2 is preferably a branched or straight-chain hydroxyalkyl group, and more preferably a straight-chain hydroxyalkyl group.

[0021] In the compound of the present invention, the monomer unit represented by general formula (2) may contain one type alone or two or more types.

[0022] In addition, in the general formula (2), -NH-R2 may be -NR3-R2, and R3 is not particularly limited as long as it is a hydrocarbon group having 1 to 6 carbon atoms. Examples of R3 include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and among these, a methyl group is particularly preferable. Examples of --NR3-R2 include groups in which a hydrogen atom has been removed from the amino group of N-methylethanolamine and N-methyl-D-glucamine. In addition, -NR3-R2 may be a cyclic amino group in which R2 and R3 are covalently bonded, such as a group in which a hydrogen atom has been removed from the amino group of prolinol.

[0023] The monomer unit BU contained in the slightly crosslinked modified polyamino acid derivative may contain one type alone or two or more types.

[0024] The bonding form of the monomer units AU, BU, CU, and Crosslink-U may be any of random, block, and tapered. From the viewpoint of simultaneously improving the water solubility and viscosity of the polyamino acid derivative, the bonding form of the monomer units AU, BU, and CU is preferably linear.

[0025] In the slightly crosslinked modified polyamino acid derivative, the ratio of the molar percentage of the monomer unit AU to the molar percentage of the monomer unit BU (also represented as (AU) / (BU)) is 40 / 60 to 60 / 40, preferably 45 / 55 to 60 / 40, and more preferably 50 / 50 to 60 / 40. If it is within the above range, the compatibility with water is excellent and the viscosity is improved. In the present disclosure, the ratio is 1 The molecular weight is calculated from H NMR. 1 A detailed calculation method from 1 H NMR will be described in the Examples.

[0026] The (AU) / (BU) ratio can also be calculated from the amounts of the raw materials used. In this case, the ratio can be calculated by dividing the total number of moles of amine A added during synthesis by the total number of moles of amine B added during synthesis.

[0027] In the slightly crosslinked modified polyamino acid derivative, the ratio of the molar percentage of the monomer unit CU to the total molar percentage of the monomer unit AU and the monomer unit BU (also represented as [(AU)+(BU)] / (CU)) is 80 / 20 to 99 / 1, preferably 85 / 15 to 98 / 2, more preferably 90 / 10 to 97 / 3, and further preferably 90 / 10 to 95 / 5. In the present disclosure, the ratio is 1 The molecular weight is calculated from H NMR. 1 A detailed calculation method from 1 H NMR will be described in the Examples.

[0028] The mol% of the monomer unit AU in the slightly crosslinked modified polyamino acid derivative is preferably 40 mol% to 60 mol%, more preferably 43 mol% to 58 mol%, and even more preferably 45 mol% to 57 mol%. In the present disclosure, the mol% of the monomer unit AU in the slightly crosslinked modified polyamino acid derivative refers to the amount (mol%) of the monomer unit AU present in one molecule of the slightly crosslinked modified polyamino acid derivative. The mol% of AU can be adjusted by the blending amounts of amine A and other raw materials during synthesis, which will be described later.

[0029] The mol% of the monomer unit BU in the slightly crosslinked modified polyamino acid derivative is preferably 30 mol% to 60 mol%, more preferably 32 mol% to 50 mol%, and even more preferably 35 mol% to 45 mol%. In the present disclosure, the mol% of the monomer unit BU in the slightly crosslinked modified polyamino acid derivative refers to the amount (mol%) of the monomer unit BU present in one molecule of the slightly crosslinked modified polyamino acid derivative. The mol% of BU can be adjusted by the blending amount of amine B described later and other raw materials during synthesis.

[0030] Here, the mole percentages of the monomer units AU and BU in the slightly crosslinked modified polyamino acid derivative are, respectively, 1 It is calculated from H NMR. Specifically, it is calculated using the obtained NMR spectrum according to the following formula: Molar % of monomer unit AU=(peak integral value of methyl group of amine A / 3)×100 / ((peak integral value of methyl group of amine A / 3)+(peak integral value of methylene group of amine B / 2)+(peak integral value of methine group of succinimide)) Molar % of monomer unit BU=(peak integral value of methylene group of amine B / 2)×100 / ((peak integral value of methyl group of amine A / 3)+(peak integral value of methylene group of amine B / 2)+(peak integral value of methine group of succinimide))

[0031] The mole percentages of the monomer units AU and BU in the slightly crosslinked modified polyamino acid derivative can also be calculated from the amounts of the raw materials by the following formula. Molar % of monomer unit AU=(total number of moles of amine A added during synthesis / total number of moles of polysuccinimide (PSI) added during synthesis)×100 Molar % of monomer unit BU=(total number of moles of amine B added during synthesis / total number of moles of PSI added during synthesis)×100

[0032] The amount of crosslinking in the slightly crosslinked modified polyamino acid derivative (mol % of the crosslinked portion Crosslink-U in the slightly crosslinked modified polyamino acid derivative) is 0.1 to 2.0 mol %. For example, since the amount of crosslinking in the slightly crosslinked polymer is small, a solution of a given concentration does not gel and can maintain a certain fluidity.

[0033] The amount of crosslinking in the slightly crosslinked modified polyamino acid derivative (the mol % of the crosslinked portion Crosslink-U in the slightly crosslinked modified polyamino acid derivative) is preferably 0.1 mol % to 2.0 mol %, more preferably 0.3 mol % to 1.8 mol %, and even more preferably 0.5 mol % to 1.7 mol %. In the crosslinked portion Crosslink-U, the crosslinked portion preferably contains a structure derived from a crosslinking agent (described in detail in the manufacturing method described later). The amount of crosslinking can be adjusted by the amount of the crosslinking agent and other raw materials used during synthesis. The amount of crosslinking (mol%) can be calculated by (total number of moles of crosslinking agent added during synthesis / total number of moles of polysuccinimide (PSI) added during synthesis)×100.

[0034] The hydroxyl value of the slightly crosslinked modified polyamino acid derivative is 80 mgKOH / g to 170 mgKOH / g, preferably 90 mgKOH / g to 130 mgKOH, and more preferably 95 mgKOH / g to 110 mgKOH. The hydroxyl value can be adjusted by the blending amounts of the below-described amine A and amine B. The method for calculating the hydroxyl value will be described in the Examples.

[0035] The weight average molecular weight (Mw) of the slightly crosslinked modified polyamino acid derivative is not particularly limited, but is preferably 80,000 or more, more preferably 100,000 or more, and even more preferably 120,000 or more. Also, it is preferably 800,000 or less, more preferably 700,000 or less, and even more preferably 600,000 or less. For example, it is 80,000 or more and 800,000 or less, 100,000 or more and 700,000 or less, or 120,000 or more and 600,000 or less. The weight average molecular weight can be adjusted by the molecular weight of the polysuccinimide used in the synthesis and the types of amine A and amine B described later. The weight average molecular weight here refers to a converted value measured by the GPC method (differential refractometer) using polystyrene as a standard substance, and specifically refers to the weight average molecular weight measured using a G1000HHR column, a G4000HHR column, and a GMHHR-H column (TSKgel (registered trademark), manufactured by Tosoh Corporation) using dimethylformamide containing 10 mM lithium bromide as an eluent.

[0036] In the slightly crosslinked modified polyamino acid derivative of this embodiment, the monomer units AU, BU, and CU are structural units derived from amine A, amine B, and succinimide, respectively (described in detail in the production method described below).

[0037] The slightly crosslinked modified polyamino acid derivative containing the monomer units AU and BU is obtained by ring-opening polysuccinimide (PSI) using a monoamine. The monomer unit CU is formed by remaining unreacted imide rings. The slightly crosslinked modified polyamino acid derivative is obtained by further crosslinking the monoamine modified polyamino acid derivative obtained by ring-opening polysuccinimide (PSI) using a monoamine with a trace amount of a crosslinking agent.

[0038] The "slightly cross-linked modified polyamino acid derivative" of the present invention means a modified polyamino acid derivative with a cross-linking amount of 0.1 to 2.0 mol%. "Slightly cross-linked" is distinguished from normal "cross-linked" with a cross-linking amount of more than 2.0 mol%. For example, since the cross-linking amount of a slightly cross-linked polymer is small, a solution of a given concentration does not gel and can maintain a certain fluidity. The method for calculating the cross-linking amount of a slightly cross-linked modified polyamino acid derivative will be described in the Examples.

[0039] [Polysuccinimide (PSI)] The polysuccinimide (PSI) according to this embodiment is a polymer represented by the following formula (2).

[0040] [ka] (In the formula, n=10~10000)

[0041] There is no particular limitation on the method for producing polysuccinimide (PSI), but for example, aspartic acid is heated in a vacuum at 170 to 190°C in the presence of phosphoric acid, and dehydration condensation is performed. In order to obtain a polysuccinimide (PSI) having a higher molecular weight, the polysuccinimide (PSI) obtained as described above may be treated with a condensing agent such as dicyclohexylcarbodiimide. There is no particular limitation on the molecular weight of polysuccinimide (PSI). For example, the weight average molecular weight is preferably 20,000 or more, more preferably 50,000 or more, and even more preferably 70,000 or more. The molecular weight of polysuccinimide (PSI) is preferably 500,000 or less, and more preferably 200,000 or less. The weight average molecular weight in this case is a conversion value obtained by the GPC method using polystyrene as a standard substance.

[0042] [Crosslinking Agent] The crosslinking agent according to the present embodiment is not particularly limited as long as it can form the bond. A specific example of a crosslinking agent that is preferable for forming an amide bond used in the crosslinking portion is a polyfunctional amine.

[0043] The polyfunctional amine according to this embodiment is preferably an amine having at least two primary and / or secondary amino groups. Examples of the diamine compound include aliphatic diamines such as ethylenediamine and hexamethylenediamine, and aliphatic diamines containing aromatic rings such as xylenediamine; alicyclic diamines such as norbornenediamine; ether-based diamines such as 1,2-bis(2-aminoethoxy)ethane (AEE), diethylene glycol bis(3-aminopropyl)ether (bis[2-(3-aminopropoxy)ethyl ether (APEE)), polyoxyethylenediamine, and polyoxypropylenediamine; amino acids and derivatives thereof having amino groups in the side chains such as lysine and ornithine; and monoamino compounds linked by disulfide bonds such as cystine and cystamine, and derivatives thereof. The polyfunctional amine according to the present embodiment is preferably free of the above amino acids and derivatives thereof. The polyfunctional amine according to the present embodiment is preferably an ether-based diamine from the viewpoint of being less likely to generate bumps during the crosslinking reaction due to its flexible structure and being easy to control the crosslinking reaction.

[0044] Examples of polyfunctional amine compounds other than diamines include tris(2-aminoalkyl)amines (wherein the alkyl carbon atom number is preferably 1 to 5, and more preferably 2 to 4), such as tris(2-aminoethyl)amine (TREN) and tris(3-aminopropyl)amine; diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine.

[0045] Preferred examples of the polyfunctional amine according to this embodiment include 1,2-bis(2-aminoethoxy)ethane (AEE), bis[2-(3-aminopropoxy)ethyl ether (APEE), and tris(2-aminoethyl)amine (TREN).

[0046] The reaction between polysuccinimide and polyfunctional amine can be carried out in an organic solvent, for example. The reaction will be described below using an example in which the polyfunctional amine according to the present embodiment is a diamine. In the method of reacting polysuccinimide with diamine in an organic solvent, polysuccinimide is dissolved in an aprotic polar organic solvent such as dimethylformamide (DMF), dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylimidazolidinone (DMI), dimethylsulfoxide (DMSO), sulfolane, etc., and then diamine or a solution of diamine in the organic solvent is dropped. At this time, the amount of the organic solvent used to dissolve polysuccinimide is not particularly limited, but it is usually used at a polymer concentration of 1 to 50 mass%.

[0047] The temperature at which the polysuccinimide and the diamine are reacted is not particularly limited, but is, for example, room temperature to 80°C.

[0048] The reaction conditions (such as reaction temperature, reaction time, reaction concentration, and amount of diamine used) are not particularly limited, but it is preferable to set the reaction conditions such that the entire reaction solution does not gel.

[0049] [Monoamines] The monoamine in this embodiment uses a monoamine represented by the following general formula (6) (sometimes referred to as hydrophobic amine A or amine A) and a monoamine represented by the following general formula (7) or general formula (8) (sometimes referred to as hydrophilic amine B or amine B). R1-NH2(6) (In the formula, R1 represents a hydrocarbon group having 3 to 22 carbon atoms.) R2-NH2(7) (wherein R2 represents a hydroxyalkyl group having 2 to 8 carbon atoms. The hydroxyalkyl group may contain a heteroatom.) R2-NH-R3(8) (In the formula, R2 is a hydroxyalkyl group having 2 to 8 carbon atoms. The hydroxyalkyl group may contain a heteroatom. In addition, in the formula, R3 is a hydrocarbon group having 1 to 6 carbon atoms. Furthermore, R2 and R3 may be covalently bonded to form a cyclic amine.)

[0050] The explanation for R1 in general formula (1) is incorporated herein by reference for R1 in general formula (6). In addition, the explanation for R2 and R3 in general formula (7) and general formula (8) is incorporated herein by reference for R2 and R3 in general formula (2). The monoamines represented by the general formulae (6) to (8) may be commercially available products, or may be prepared by a known method.

[0051] [Method for producing slightly cross-linked modified polyamino acid derivatives] The method for producing the slightly crosslinked modified polyamino acid derivative according to the present embodiment includes, for example, a method of ring-opening reaction of polysuccinimide (PSI) using polysuccinimide (PSI), a crosslinking agent such as a trace amount of a polyfunctional amine compound, and a monoamine. The order of addition of the crosslinking agent and the monoamine is not particularly limited. The monoamine may be added first and then the crosslinking agent, or the monoamine and the crosslinking agent may be added simultaneously, or the crosslinking agent may be added first and then the monoamine. From the viewpoint of easy control of the amount of crosslinking, it is preferable to add the crosslinking agent first and then add the monoamine after the crosslinking reaction has progressed.

[0052] For example, when a polyfunctional amine compound is used as a crosslinking agent, polysuccinimide (PSI) is reacted with a crosslinking agent such as a trace amount of a polyfunctional amine compound, and then a monoamine is added to perform a ring-opening reaction of polysuccinimide (PSI) by reacting with the monoamine. After reacting polysuccinimide (PSI) with a crosslinking agent such as a trace amount of a polyfunctional amine compound, polysuccinimide (PSI) is reacted with the monoamine, and the imide ring of polysuccinimide (PSI) is opened. In addition, since a trace amount of a crosslinking agent such as a polyfunctional amine compound is used, the obtained polyamino acid derivative has a crosslinked structure of a trace amount. The total amount of the crosslinking agent and the monoamine used may be less than 1 equivalent to the equivalent of the monomer unit of polysuccinimide (PSI) to perform the ring-opening reaction, and unreacted imide rings may remain, or may be more than 1 equivalent to perform the ring-opening reaction, and no unreacted imide rings may remain.

[0053] In the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment, the monoamine preferably contains a monoamine represented by the above general formula (6) (sometimes referred to as hydrophobic amine A) and a monoamine represented by the general formula (7) or general formula (8) (sometimes referred to as hydrophilic amine B), and the molar ratio of the hydrophobic amine A to the hydrophilic amine B used as raw materials is 45 / 55 to 60 / 40. It is more preferable that the monoamine contains a hydrophobic amine A and a hydrophilic amine B, and the molar ratio of the hydrophobic amine A to the hydrophilic amine B is 50 / 55 to 55 / 45.

[0054] In the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment, the monoamine may contain a hydrophobic amine A and a hydrophilic amine B, or may contain a monoamine other than the hydrophobic amine A and the hydrophilic amine B. In this case, the total molar amount of the hydrophobic amine A and the hydrophilic amine B in the monoamine is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more. The monoamine may be the hydrophobic amine A and the hydrophilic amine B.

[0055] The unreacted imide ring may remain as it is, or may be further subjected to a ring-opening reaction using another monoamine, or, if desired, the unreacted imide ring may be opened with a substituted amine such as cysteamine or dibutylamine.

[0056] "Organic solvent" In the method for producing the slightly crosslinked modified polyamino acid derivative according to this embodiment, the organic solvent is not particularly limited as long as it substantially dissolves the polysuccinimide (PSI), the crosslinking agent, and the monoamine, and / or does not substantially inhibit the progress of the reaction.

[0057] Specific examples of the organic solvent include aprotic polar organic solvents such as dimethylformamide (DMF), dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylimidazolidinone (DMI), dimethylsulfoxide (DMSO), and sulfolane, which may be used alone or in combination.

[0058] "Amount of crosslinking agent used" The amount of the crosslinking agent used in this embodiment is not particularly limited, as long as it is sufficient to obtain a micro-crosslinked modified polyamino acid derivative with a small amount of crosslinking structure introduced to such an extent that gelation does not occur. For example, in the final synthesis of the micro-crosslinked modified polyamino acid derivative represented by the above general formula (1), the amount of crosslinking may be 0.1 to 2.0 mol%. It is preferably 0.3 to 1.8 mol%, more preferably 0.4 to 1.7 mol%, and even more preferably 0.5 to 1.5 mol%. For example, when a polyfunctional amine is used as the crosslinking agent, the amount of the polyfunctional amine used is 0.1 to 2.0 mol, preferably 0.2 to 1.5 mol, more preferably 0.3 to 1.3 mol, and even more preferably 0.4 to 1.0 mol, relative to the total mole number of 100 mol of polysuccinimide added during synthesis. When the amount of the polyfunctional amine used is 2 mol relative to the total mole number of 100 mol of polysuccinimide added during synthesis, it is simply referred to as "the amount of the polyfunctional amine used is 2 mol%". When the amount of polyfunctional amine used is within the range of 0.1 to 2.0 mol %, a thickening composition can achieve a high thickening effect and maintain a certain level of viscosity for a longer period of time. In this disclosure, the "total number of moles of polysuccinimide (PSI) added during synthesis" means the weight of polysuccinimide added during the synthesis of the slightly crosslinked modified polyamino acid derivative divided by the molecular weight of the repeating unit of polysuccinimide.

[0059] "Monoamine usage" The total amount of the monoamine used according to the present embodiment is not particularly limited as long as it is substantially soluble in the organic solvent and / or does not substantially inhibit the progress of the reaction. The amount of the monoamine used is generally 0.1 to 10 times equivalent, preferably 0.1 to 1.0 times equivalent, relative to the equivalent of the monomer unit of polysuccinimide (PSI).

[0060] "Basic catalyst" In the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment, a catalyst may not be used, or a basic catalyst may be used. The optional basic catalyst is not particularly limited as long as it substantially accelerates the reaction rate. Specific examples of the basic catalyst include aliphatic tertiary amines such as trimethylamine, triethylamine, tripropylamine, tributylamine, diisopropylethylamine (DIEA), triethanolamine, and triethylenediamine (DABCO), alicyclic tertiary amines such as N-methylmorpholine, aromatic tertiary amines such as dimethylaniline and diethylaniline, and tetramethylguanidine, which may be used alone or in combination.

[0061] "Amount of basic catalyst used" In the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment, the amount of the basic catalyst used is not particularly limited as long as it substantially accelerates the reaction rate. The amount of the basic catalyst used is generally 0 to 2 times the equivalent of the monoamine.

[0062] "Reaction temperature" In the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment, the reaction temperature is not particularly limited as long as the reaction progress can be substantially maintained. The reaction temperature is generally selected from a temperature range of 5 to 150°C. The reaction temperature can also be selected optimally from the viewpoints of the monoamine used, shortening the reaction time, improving the reaction rate, etc. The method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment preferably includes a crosslinking reaction step in which a crosslinking agent is added first and a monoamine reaction step in which a monoamine is added thereafter. In this case, the temperature of the crosslinking reaction and the temperature of the monoamine reaction may be the same or different. It is preferable that the temperature of the crosslinking reaction is lower than the reaction temperature after the addition of the monoamine. In the crosslinking reaction step in which a crosslinking agent is added to polysuccinimide (PSI) and a crosslinking reaction proceeds, the reaction temperature may be 120°C or lower, or 100°C or lower. It may also be 20°C or higher. For example, when the crosslinking agent is an ether-based diamine or tris(2-aminoalkyl)amine, the reaction temperature in the crosslinking reaction step is preferably 100°C or lower, more preferably 80°C or lower, further preferably 60°C or lower, and may be 50°C or lower. It may also be 20°C or higher. In the crosslinking reaction step, if the reaction temperature is within the above range, crosslinking can proceed uniformly. As a result, the thickening composition containing the microcrosslinked modified polyamino acid derivative obtained by the above production method can achieve both thickening power and storage stability.

[0063] "Concentration of reaction system" The concentration of the reaction system employed in the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment is not particularly limited as long as the progress of the reaction can be substantially maintained. The concentration of the reaction system is selected based on the concentration of polysuccinimide (PSI), and generally, the polysuccinimide (PSI) concentration is selected from a concentration range of 1 to 50% by weight. The concentration of the reaction system can also be selected from a polysuccinimide (PSI) concentration range of 1 to 50% by weight, so that the optimum concentration for the monoamine used is selected.

[0064] <Method for isolating slightly cross-linked modified polyamino acid derivatives> In the method for producing a slightly crosslinked modified polyamino acid derivative according to the present embodiment, the method for isolating the polymer produced from the reaction solution after the reaction is completed is not particularly limited as long as the reaction product can be substantially isolated with a desired purity. The isolation method may be any known or publicly used method. Generally, known or publicly used isolation procedures such as concentration, recrystallization, or reprecipitation are used.

[0065] A specific example of the isolation method is a method in which, after the completion of the reaction, at an appropriate temperature, an excess of a poor solvent (e.g., ethyl acetate, methyl alcohol, ethyl alcohol, isopropyl alcohol, etc.) is added to the reaction solution in which the reaction product is dissolved, and the precipitated reaction product is isolated by decantation, filtration, suction filtration, etc., and the crystals are thoroughly washed with a poor solvent that does not dissolve the crystals, followed by drying, etc. Another specific example is a method in which, after the completion of the reaction, at an appropriate temperature, the reaction solution in which the reaction product is dissolved is added to the same excess of a poor solvent as above, and the precipitated reaction product is isolated, washed, and dried in the same manner as above, etc.

[0066] In the method for producing the slightly cross-linked modified polyamino acid derivative according to the present embodiment, the obtained slightly cross-linked modified polyamino acid derivative is not isolated, and the mixture after the reaction can be used as it is. Also, if necessary, only a part of the unreacted raw materials other than the solvent can be removed, and the composition described below can be added. Also, the solvent of the mixture can be increased or decreased to adjust the concentration.

[0067] (Thickening composition) The thickening composition according to this embodiment contains at least a slightly crosslinked modified polyamino acid derivative, and may optionally contain water. The water may be, for example, ion-exchanged water. The water content may be 40% by mass to 99.99% by mass, 60% by mass to 99.95% by mass, or 80% by mass to 99.9% by mass, relative to 100% by mass of the total thickening composition including water.

[0068] <Other ingredients> The thickening composition of the present embodiment may further contain other ingredients, such as cosmetic active ingredients, and additives commonly used in cosmetics, such as surfactants, stabilizers, and moisturizers.

[0069] <Method of preparing thickening composition> A method for preparing the thickening composition of this embodiment can be, for example, a method in which a predetermined amount of the micro-crosslinked modified polyamino acid derivative of this embodiment described above is weighed out, and if necessary, a predetermined amount of water or other components is added and stirred to prepare the thickening composition. When the cosmetic composition of the present embodiment contains water, an aqueous dispersion of the slightly crosslinked modified polyamino acid derivative of the present embodiment may be prepared first, and then mixed with other components, if necessary. When the cosmetic composition of the present embodiment does not contain water, a predetermined amount of solid micro-crosslinked modified polyamino acid derivative may be weighed out, and if necessary, mixed with other solid components. Alternatively, a dispersion containing micro-crosslinked modified polyamino acid derivative and water may be prepared first, and if necessary, mixed with other components to prepare a mixed liquid, which may then be dried before preparation. The preparation temperature is not particularly limited, but heating to 60 to 80° C. will speed up dispersion and dissolution in water.

[0070] (Cosmetic composition) The cosmetic composition according to this embodiment contains the thickening composition and a cosmetic active ingredient. Examples of the cosmetic active ingredient include higher alcohols, lower alcohols, polyhydric alcohols, pH adjusters, surfactants, sequestering agents, antioxidants, physical and chemical sunscreens, vitamins, skin protectants, oils and fats, hydrocarbon oils, moisturizers, antiperspirants, detergents, fragrances, cosmetic colorants, antibacterial agents, germicides, texture improvers and foam stabilizers, other thickeners, etc. The cosmetic composition according to this embodiment may further contain water. When the cosmetic composition according to this embodiment contains water, the content of the micro-crosslinked modified polyamino acid derivative according to this embodiment is preferably 0.05 to 10 mass%, more preferably 0.1 to 7.0 mass%, even more preferably 0.3 to 5.0 mass%, and particularly preferably 0.5 to 3.0 mass%, relative to 100 mass% of the total cosmetic composition.

[0071] When the cosmetic composition contains water, the pH value thereof is preferably in the range of 4.5-8.0, and more preferably in the range of 5-7. The method for adjusting the pH value is not particularly limited, and may be a method using an acidic or basic substance. Specific examples of acids include organic acids such as citric acid. Specific examples of bases include organic basic compounds such as ammonia and inorganic basic compounds such as sodium hydroxide. EXAMPLES

[0072] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.

[0073] (Synthesis Example 1) <Synthesis of polysuccinimide (PSI)> 160 parts of aspartic acid (manufactured by YIXING QIANCHENG BIO-ENGINEERING Co., Ltd.) and 83 parts of 85% phosphoric acid were mixed in a mortar, transferred to a tray, and reacted at 190°C and 1.3 kPa for 6 hours. The reaction mixture was pulverized, washed with distilled water until the filtrate became neutral, and vacuum dried at 80°C to obtain 115 parts of polysuccinimide (PSI) with a weight average molecular weight of 80,000.

[0074] <Measurement of weight-average molecular weight of polysuccinimide (PSI) and slightly cross-linked modified polyamino acid derivatives> The weight average molecular weight of polysuccinimide (PSI) was determined as a polystyrene equivalent value by the GPC method (differential refractometer). For the measurement, a G1000HHR column, a G4000HHR column, and a GMHHR-H column (TSKgel (registered trademark), Tosoh Corporation) were used. Dimethylformamide containing 10 mM lithium bromide was used as the eluent. The weight average molecular weight of the slightly crosslinked modified polyamino acid derivative described later was also measured by the same method.

[0075] Example 1 <Synthesis of slightly cross-linked modified polyamino acid derivative No. 1> 10.0g of PSI and 95.3g of DMF were placed in a reaction vessel and completely dissolved under heating at 60°C. After lowering the temperature to 40°C, a mixture of 0.229g of 1,2-bis(2-aminoethoxy)ethane (AEE) and 2.06g of DMF was added as a crosslinking agent and reacted for 7 hours. Next, 10.3g of n-dodecylamine was added as hydrophobic amine A and reacted for 30 minutes. Furthermore, 3.45g of 3-amino-1-propanol was added as hydrophilic amine B and reacted for 7 hours while maintaining the temperature in the reaction vessel at 60°C. The reaction vessel was then cooled and left to stand overnight at room temperature. The reaction liquid was then discharged into 1200mL of ethyl acetate while stirring to precipitate the reactant, and the solid was collected by filtration. The reaction was further washed in 600mL of ethyl acetate while stirring, and the solid was collected by filtration. The recovered solid was dried at 60° C. under reduced pressure for 12 hours to obtain 22.0 g of slightly crosslinked modified polyamino acid derivative No. 1 having a weight average molecular weight of 12,500. The crosslinking amount calculated by the above method was 1.5 mol%, and the hydroxyl value was 110 mgKOH / g. The ratio of the mol% of the monomer unit AU to the mol% of the monomer unit BU (AU) / (BU) was 54 / 46, and the ratio of the mol% of the monomer unit AU and the monomer unit BU combined to the mol% of the monomer unit CU [(AU)+(BU)] / (CU) was 92 / 8. The results are shown in Table 1.

[0076] (Examples 2 to 13, Comparative Examples 1 to 3) <Synthesis of slightly cross-linked modified polyamino acid derivatives No. 2-13, c1-c3> Based on Example 1, the hydrophobic amine A, the hydrophilic amine B, and the crosslinking agent were appropriately changed to obtain slightly crosslinked polyamino acid derivatives Nos. 2-13 and c1-c3 of Examples 2 to 13 and Comparative Examples 1 to 3. The results are shown in Table 1.

[0077] <Method of calculating the composition ratio of the slightly cross-linked modified polyamino acid derivative> The composition ratio (mol %) of the slightly crosslinked modified polyamino acid derivative was calculated from the obtained NMR spectrum according to the following formula. Ratio of the mole percent of monomer units AU to the mole percent of monomer units BU (AU) / (BU)=(peak integral value of methyl group of amine A / 3) / (peak integral value of methylene group of amine B / 2) Ratio of the mole percent of the total of the monomer units AU and BU to the mole percent of the monomer unit CU [(AU)+(BU)] / (CU)=[(peak integral value of the methyl group of amine A / 3)+(peak integral value of the methylene group of amine B / 2)] / (peak integral value of the methine group of succinimide)

[0078] <Calculation method for hydroxyl value of slightly crosslinked modified polyamino acid derivative> Next, the mole percentages of the monomer units AU and BU were calculated from the following formula, and the hydroxyl value was calculated based on the calculated mole percentages. Molar % of monomer unit AU=(integral value of methyl group of monoamine A / 3)×100 / ((integral value of methyl group of monoamine A / 3)+(integral value of methylene group of monoamine B / 2)+(integral value of methylene group of succinimide / 2)) Molar % of monomer unit BU=(integral value of methylene group of monoamine B / 2)×100 / ((integral value of methyl group of monoamine A / 3)+(integral value of methylene group of monoamine B / 2)+(integral value of methylene group of succinimide / 2)) Hydroxyl value=(mol % of monomer unit BU / 100)×56.11×1000 / [97+molecular weight of crosslinker×(mol % of crosslinker / 100)+molecular weight of amine A×(mol % of monomer unit AU / 100)+molecular weight of amine B×(mol % of monomer unit BU / 100)] In the above formula, "mol % of crosslinking agent" refers to the ratio (mol %) of the total number of moles of crosslinking agent added during synthesis to the total number of moles of PSI added during synthesis. In addition, the "total number of moles of PSI added during synthesis" in the above formula refers to the weight of PSI added during synthesis divided by the molecular weight of the repeating unit of PSI.

[0079] <Method for calculating the amount of crosslinking of slightly crosslinked modified polyamino acid derivatives> The crosslinking amount (mol %) of the slightly crosslinked modified polyamino acid derivative was calculated by (moles of added polyfunctional amine / moles of charged PSI)×100.

[0080] [Table 1]

[0081] The meanings of the abbreviations in Table 1 are as follows: DDA: n-dodecylamine CCA: Coconut amine ("Farmin (registered trademark) CS" manufactured by Kao Corporation) 3-AP: 3-amino-1-propanol EA: Ethanolamine EEA: N-methylethanolamine PL: Prolinol AEE: 1,2-bis(2-aminoethoxy)ethane APEE: Bis[2-(3-aminopropoxy)ethyl ether TREN: Tris(2-aminoethyl)amine

[0082] (Examples 14 to 26, Comparative Examples 4 to 6) <Adjustment of thickening solution> In Examples 14 to 26 and Comparative Examples 4 to 6, for viscosity evaluation, 1.0 part of the microcrosslinked modified polyamino acid derivatives No. 1 to 13 and No. c1 to c3 obtained in Examples 1 to 13 and Comparative Examples 1 to 3, respectively, was mixed with 99 parts of ion-exchanged water and stirred at 60°C for 2 hours to obtain thickening compositions of Examples 14 to 26 and Comparative Examples 4 to 6. The shear viscosity and storage stability of each thickening composition were evaluated by the evaluation methods described below. The results are shown in Table 2.

[0083] [Table 2]

[0084] (Examples 27 to 39, Comparative Examples 7 to 9) <Adjustment of thickening solution> In Examples 27 to 39 and Comparative Examples 7 to 9, for the evaluation of storage stability, 1.5 parts of the microcrosslinked modified polyamino acid derivatives No. 1 to 13 and No. c1 to c3 obtained in Examples 1 to 13 and Comparative Examples 1 to 3 were mixed with 98.5 parts of ion-exchanged water, respectively, and then stirred at 60°C for 2 hours to obtain the thickening compositions of Examples 27 to 39 and Comparative Examples 7 to 9. The shear viscosity and storage stability of each thickening composition were evaluated by the evaluation methods described below. The results are shown in Table 3.

[0085] [Table 3]

[0086] (Evaluation method) <Viscosity evaluation> 1.0 part of the microcrosslinked modified polyamino acid derivative was mixed with 99 parts of ion-exchanged water, and then stirred for 2 hours at 60° C. The shear viscosity was measured using a rotational rheometer (R / Splus manufactured by Brookfield Corporation), and the viscosity at a shear rate of 5 (1 / sec) is shown in Table 1.

[0087] <Storage stability evaluation> 1.5 parts of the microcrosslinked modified polyamino acid derivative and 98.5 parts of ion-exchanged water were mixed and stirred for 2 hours at 60° C. The thickened solution was stored in a thermostatic chamber at 50° C. for 30 days, after which the viscosity at a shear rate of 5 (1 / sec) measured with a rotational rheometer (R / Splus manufactured by Brookfield) was evaluated as ◯ if it retained 70% or more of the viscosity before storage, and as × if it was less than 70%.

[0088] (Consideration) The effects of the present invention were confirmed from the results of Examples 1 to 13 and Comparative Examples 1 to 3 for the slightly crosslinked modified polyamino acid derivatives, and Examples 14 to 26 and Comparative Examples 4 to 6, and Examples 27 to 39 and Comparative Examples 7 to 9 for the thickening compositions. In other words, a small amount of cross-linking increases the apparent molecular weight (the molecule becomes larger). Furthermore, the number of hydrophobic-hydrophobic interaction points in one molecule increases, promoting interactions between molecules and increasing the thickening power. Also, a composition that maintains a delicate balance between whether or not it dissolves in water can achieve both the highest viscosity and stability. If there are many hydrophilic groups and the affinity to water is high, the viscosity will decrease due to hydrolysis of the main chain, and the stability will decrease. Furthermore, as the amount of hydrophobic groups decreases, the hydrophobic-hydrophobic interaction will weaken and the thickening power will also decrease. Also, if there are too many hydrophobic groups, there will be more interactions within the molecule, and a single molecule will form particles, resulting in a smaller thickening power.

Claims

1. A micro-crosslinked modified polyamino acid derivative comprising an α- or β-polyaspartic acid monomer unit A-U represented by the following general formula (1), an α- or β-polyaspartic acid monomer unit B-U represented by the following general formula (2), and a crosslinking portion Crosslink-U represented by the following general formula (3): In the slightly crosslinked modified polyamino acid derivative, the ratio (A-U) / (B-U) of the mole percent of the monomer unit A-U to the mole percent of the monomer unit B-U is 40 / 60 to 60 / 40; The slightly crosslinked modified polyamino acid derivative has a hydroxyl value of 80 to 170 mgKOH / g and a crosslinking amount of the slightly crosslinked modified polyamino acid derivative of 0.1 to 2.0 mol %. [Formula 1] (In the formula, R 1 represents a hydrocarbon group having 3 to 22 carbon atoms. [chemical 2] (In the formula, R 2 represents a hydroxyalkyl group having 2 to 8 carbon atoms. The hydroxyalkyl group may contain a heteroatom. 2 may be -NR-R, and R 3 is a hydrocarbon group having 1 to 6 carbon atoms. 2 and R 3 may be a cyclic amino group to which [C3] (In the formula, the wavy lines indicate crosslinking sites.)

2. Contains a succinimide monomer unit C-U represented by the following general formula (4): The slightly crosslinked modified polyamino acid derivative according to claim 1, wherein the ratio of the molar percentage of the monomer unit A-U and the monomer unit B-U to the molar percentage of the monomer unit C-U, [(A-U)+(B-U)] / (C-U), is 80 / 20 to 99 / 1. [C4]

3. the crosslinking amount of the slightly crosslinked modified polyamino acid derivative is 0.5 to 1.8 mol %, 3. The slightly crosslinked modified polyamino acid derivative according to claim 1, wherein the hydroxyl value of the slightly crosslinked modified polyamino acid derivative is 90 to 130 mgKOH / g.

4. The crosslinking portion Crosslink-U represented by the general formula (3) contains a structure derived from a crosslinking agent, 3. The slightly crosslinked modified polyamino acid derivative according to claim 1, wherein the crosslinking agent is a polyfunctional amine.

5. 5. The slightly cross-linked modified polyamino acid derivative according to claim 4, wherein the cross-linking agent is an ether-based diamine or a tris(2-aminoalkyl)amine.

6. The crosslinking agent is at least one selected from the group consisting of 1,2-bis(2-aminoethoxy)ethane (AEE), bis[2-(3-aminopropoxy)ethyl]ether (APEE), and tris(2-aminoethyl)amine (TREN).

7. A thickening composition comprising the slightly crosslinked modified polyamino acid derivative according to claim 1.

8. The thickened composition of claim 7 further comprising water.

9. A thickening composition according to claim 7 or 8, A cosmetic active ingredient, A cosmetic composition comprising:

Citation Information

Patent Citations

  • Polyasparagine derivative thickener with side chain containing linear alkyl chain and lysine

    CN115449074A

  • Copolymer and its production

    JP1999302378A

  • Production of crosslinked polymer

    JP2000191777A

  • Polyamino acid derivative composition having thickening, foaming or foam increasing action