Polypropylene polymer composition having high stiffness properties

A blend of polypropylene polymers with controlled xylene solubles content and molecular weight distribution addresses the challenge of achieving high stiffness and toughness in polypropylene, enabling efficient production of self-supporting articles with minimal wall thickness and maintaining catalyst activity.

JP7568637B2Active Publication Date: 2024-10-16WR GRACE & CO CONN
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021557664
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-05
Filing Date
2020-04-03
Publication Date
2024-10-16
Estimated Expiration
2040-04-03

AI Technical Summary

Technical Problem

Existing polypropylene polymers face challenges in achieving high stiffness without compromising toughness and catalyst activity, often leading to increased production costs and processing difficulties due to high crystallinity.

Method used

A polypropylene polymer composition comprising a blend of two polypropylene polymers with controlled xylene solubles content and molecular weight distribution, produced using a non-phthalate Ziegler-Natta catalyst, to achieve high stiffness and toughness while maintaining catalytic activity.

Benefits of technology

The composition exhibits excellent stiffness and toughness properties, allowing for efficient processing and the production of self-supporting articles with minimal wall thickness, while maintaining high catalytic activity and reducing material usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568637000011
    Figure 0007568637000011
  • Figure 0007568637000001
    Figure 0007568637000001
  • Figure 0007568637000002
    Figure 0007568637000002
Patent Text Reader

Abstract

Disclosed is a polypropylene polymer composition having excellent stiffness properties. The polypropylene polymer composition is made by combining a first polypropylene polymer with a second polypropylene polymer. The combination of polymers has been found to produce a composition having high stiffness properties in addition to excellent toughness properties. In addition, the polymer composition has good flow properties for molding into various products and articles. Among other advantages, the different polypropylene polymers can be produced with relatively high catalytic activity, especially compared to previously produced highly crystalline polymers.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (Related Applications) This application is based on and claims priority to U.S. Provisional Patent Application No. 62 / 830,007, filed April 5, 2019, which is incorporated herein by reference. [Background technology]

[0002] One important property of many polymeric materials is stiffness. Stiffness refers to the rigidity property of a material and can be measured by determining the flexural modulus of the material. Flexural modulus relates to the ability of a material to bend, or in other words, its resistance to bending when a force is applied perpendicular to a molded plaque formed from the polymer.

[0003] Polymers made with increased stiffness provide various advantages when molded into products and articles. For example, high stiffness polymers generally do not deform when subjected to external forces. Therefore, free-standing and shape-retaining products can be made from high stiffness polymers. For example, by increasing the stiffness of polymers, the wall thickness of various polymeric articles, such as containers, can be minimized while still having sufficient rigidity and shape-conforming properties.

[0004] In the past, various efforts have been made to increase the stiffness of polypropylene polymers. For example, in the past, the stiffness of polypropylene polymers was increased by increasing the crystallinity of the material. Increasing the crystallinity of the material provided the desired increase in stiffness. However, various problems arose.

[0005] For example, increasing the crystallinity of a polypropylene polymer can reduce the toughness of the polymer, resulting in brittleness of the final product. In addition, highly crystalline polypropylene can be somewhat difficult to process. For example, increasing the crystallinity of a polypropylene polymer can shorten the operating window for melt processing the polymer, which increases the difficulty of forming the product.

[0006] Additionally, highly crystalline polypropylene can be somewhat expensive to produce. For example, by increasing the crystallinity of the polymer, the effectiveness of the catalyst used to produce the polymer can decrease. For example, Ziegler-Natta catalysts have a lower catalytic activity as the crystallinity of the polymer increases. As a result, more catalyst is needed to produce the polymer, which can significantly increase the cost of making the polymer. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above, there is a need for a polypropylene polymer composition having relatively high stiffness and high toughness properties. There is also a need for a process for producing a polypropylene polymer composition having high stiffness properties without reducing catalyst activity.

[0008] In general, the present disclosure is directed to polypropylene polymer compositions having relatively high stiffness properties. The polymer compositions of the present disclosure can be produced without sacrificing catalytic activity and with a broad molecular weight distribution. The broad molecular weight distribution improves the processability of the composition.

[0009] In one embodiment, the present disclosure is directed to a polypropylene polymer composition comprising a first polypropylene polymer together with a second polypropylene polymer. The first polypropylene polymer has a melt flow rate of greater than about 0.1 g / 10 min and less than about 3 g / 10 min. The first polypropylene polymer has a xylene solubles content of greater than about 1 wt%, for example greater than about 2.5 wt%, for example greater than about 3 wt%, for example greater than about 3.5 wt%, and generally less than about 8 wt%, for example less than about 7 wt%. In one aspect, the xylene solubles content is greater than about 5 wt%, for example greater than about 6 wt%. In another aspect, the xylene solubles content is less than about 4 wt%. The first polypropylene polymer may generally have a polydispersity index of greater than about 4 and less than about 10.

[0010] The second polypropylene polymer added to the first polypropylene polymer may have a melt flow rate of more than about 5 g / 10 min and less than about 100 g / 10 min. The second polypropylene polymer may have a xylene solubles content of more than about 1 wt%, for example more than about 2.5 wt%, for example more than about 3 wt%, for example more than about 4 wt%, and generally less than about 8 wt%, for example less than about 7 wt%. The second polypropylene polymer may have a polydispersity index of more than about 4 and less than about 5.5.

[0011] In one embodiment, one of the polypropylene polymers has a xylene solubles content greater than about 5 wt.%, such as greater than about 6 wt.%, and the other polypropylene polymer has a xylene solubles content less than about 4 wt.%.

[0012] The first polypropylene polymer may be present in the polypropylene polymer composition in a weight ratio of about 5:95 to about 80:20, such as about 30:70 to about 67:33, relative to the second polypropylene polymer. In a particular embodiment, the first low melt flow rate polypropylene polymer is present in a lesser amount than the second polypropylene polymer. For example, in one embodiment, the weight ratio of the first polypropylene polymer to the second polypropylene polymer may be about 5:95 to about 45:55. The overall polypropylene polymer composition may generally have a melt flow rate of greater than about 0.5 g / 10 min, such as greater than about 0.7 g / 10 min, such as greater than about 1 g / 10 min, and generally less than about 30 g / 10 min, such as less than about 25 g / 10 min, such as less than about 20 g / 10 min. In one embodiment, for example, the melt flow rate may be from about 0.5 g / 10 min to about 3 g / 10 min. In an alternative embodiment, the melt flow rate may be from about 5 g / 10 min to about 20 g / 10 min.

[0013] The polypropylene polymer composition may generally have a total xylene solubles content greater than about 3 wt%, such as less than about 3.5 wt%, for example greater than about 4 wt%, and generally less than about 8 wt%, such as less than about 7 wt%, for example less than about 6.8 wt%. The polypropylene polymer composition may have an overall polydispersity index greater than about 5 and less than about 10.

[0014] As noted above, the polypropylene polymer composition of the present disclosure has relatively high stiffness properties. For example, the polypropylene polymer composition may have a flexural modulus (ASTM test D790) according to the following equation: 2072*XS -0.18 wherein XS is the xylene solubles content of the polypropylene polymer composition, and the xylene solubles content of the polypropylene polymer composition may be from about 2.5% to about 8% by weight.

[0015] For example, the polypropylene polymer composition of the present disclosure may have a flexural modulus of greater than about 1500 MPa, such as greater than about 1550 MPa, such as greater than about 1600 MPa, such as greater than about 1650 MPa, such as greater than about 1700 MPa, and generally less than about 2500 MPa. In addition to having excellent stiffness properties, the polypropylene polymer composition may also display an IZOD impact resistance of greater than about 40 J / m, such as greater than about 45 J / m, such as greater than about 55 J / m, and generally less than about 90 J / m.

[0016] In one embodiment, the first polypropylene polymer and the second polypropylene polymer can both comprise a polypropylene homopolymer, hi an alternative embodiment, at least one of the polypropylene polymers can be a copolymer, such as a copolymer containing ethylene units.

[0017] The polypropylene polymer composition of the present disclosure can be formed in a process in which a propylene polymer is polymerized in the presence of a Ziegler-Natta catalyst that is non-phthalate, in one embodiment. The Ziegler-Natta catalyst can have a catalytic activity of greater than about 50 kg / g to produce the polypropylene polymer composition. The polypropylene polymer can be produced in a gas phase reactor or in a bulk phase reactor. In one embodiment, each of the first and second polypropylene polymers are formed in separate processes and then combined. Alternatively, the first and second polypropylene polymers can be formed sequentially in a series of reactors.

[0018] The polypropylene polymer composition of the present disclosure can be used to form any kind of molded article. In one embodiment, the polymer composition can be used to manufacture any kind of molded article using any suitable thermoforming or molding process. For example, the article can be manufactured using extrusion blow molding, injection molding, rotational molding, extrusion, etc. The polypropylene polymer composition can also be used to manufacture biaxially oriented polypropylene films. Articles that can be made according to the present disclosure include storage or packaging containers, such as food containers.

[0019] Other features and aspects of the present disclosure are discussed in more detail below. [Brief description of the drawings]

[0020] A full and enabling disclosure of the present disclosure is more particularly set forth in the remainder of the specification, including reference to the accompanying drawings, in which: [Figure 1] FIG. 1 is a graphical representation of the results obtained in the examples below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Repeat use of reference characters in the present specification and drawings is intended to represent same or analogous features or elements of the invention. Definitions and Test Procedures

[0022] As used herein, the term "polypropylene homopolymer" is a homopolymer that contains propylene monomer units.

[0023] As used herein, the term "propylene-ethylene copolymer" is a copolymer that contains a majority weight percent of propylene monomer with ethylene monomer as the secondary constituent. A "propylene-ethylene copolymer" (also called polypropylene random copolymer, PPR, PP-R, RCP, or RACO) is a polymer that has individual repeat units of ethylene monomer present in a random or statistical distribution within the polymer chain.

[0024] As used herein, melt flow rate (MFR) is measured according to ASTM D 1238 test method at 230° C. using a propyne-based polymer weighing 2.16 kg.

[0025] Xylene soluble (XS) is defined as the weight percent of resin remaining in solution after dissolving a sample of polypropylene random copolymer resin in hot xylene and allowing the solution to cool to 25°C. This is also referred to as the gravimetric XS method according to ASTM D5492-06 using a 90 minute precipitation time, also referred to herein as the "wet method". XS can also be measured according to the Viscotek method as follows: 0.4 g of polymer is dissolved in 20 mL of xylene with stirring at 130°C for 60 minutes. The solution is then cooled to 25°C and after 60 minutes the insoluble polymer fraction is filtered off. The resulting filtrate is analyzed by flow injection polymer analysis using a Viscotek ViscoGEL H-100-3078 column with a THF mobile phase flowing at 1.0 mL / min. The column is connected to a Viscotek Model 302 Triple Detector Array with light scattering, viscometer, and refractometer detectors operating at 45°C. Instrument calibration is maintained using Viscotek PolyCAL™ polystyrene standards. A polypropylene (PP) homopolymer such as biaxially oriented polypropylene (BOPP) grade Dow 5D98 is used as a reference material to ensure that Viscotek instruments and sample preparation procedures provide consistent results by using a polypropylene homopolymer such as 5D98 as a control to verify method performance. Values ​​for reference polypropylene homopolymer such as 5D98 are first derived from testing using the ASTM method identified above.

[0026] The above-mentioned ASTM D5492-06 method may be adapted to determine the xylene soluble portion. In general, the procedure consists of weighing 2 g of sample and dissolving it in 200 mL of o-xylene in a 400 mL flask with a 24 / 40 joint. The flask is connected to a water-cooled condenser, the contents are stirred and heated to reflux under nitrogen (N2), and then maintained at reflux for an additional 30 minutes. The solution is then cooled in a temperature-controlled water bath at 25° C. for 90 minutes to crystallize the xylene insoluble fraction. Once the solution has cooled and the insoluble fraction has precipitated from the solution, separation of the xylene soluble portion (XS) from the xylene insoluble portion (XI) is achieved by filtration through a 25 micron filter paper. 100 mL of the filtrate is collected in a pre-weighed aluminum pan, and the o-xylene is evaporated from this 100 mL filtrate under a stream of nitrogen. Once the solvent has evaporated, the pan and contents are placed in a 100°C vacuum oven for 30 minutes or until dry. The pan is then allowed to cool to room temperature and weighed. The xylene soluble portion is calculated as XS (wt%) = [(m3-m2) * 2 / m1] * 100, where m1 is the original weight of the sample used, m2 is the weight of the empty aluminum pan, and m3 is the weight of the pan and residue (asterisk * indicates that the specified term or value is multiplied, both here and elsewhere in this disclosure.

[0027] The ethylene content is mainly determined by 13It is measured using Fourier Transform Infrared (FTIR), which correlates with the ethylene value determined using C NMR. The relationship and agreement between measurements performed using the two methods is described, for example, in J.R. Paxson, J.C. Sandall, "Quantitative Measurement of Ethylene Incorporation into Propylene Copolymers by Carbon-13 Nuclear Magnetic Resonance and Infrared Spectroscopy", Analytical Chemistry, Vol. 50, No. 13, Nov. 1978, 1777-1780.

[0028] Flexural modulus is determined according to ASTM 3641 and using Type 1 specimens molded according to ASTM D4101, according to ASTM D790-10 Method A at 1.3 mm / min.

[0029] The polydispersity index is measured by small amplitude oscillatory shear (SAOS). The test is carried out according to the method described in Zeichner GR, Patel PD (1981) "A comprehensive Study of Polypropylene Melt Rheology" Proc. (the 2nd ndThe measurements are performed using a stress controlled dynamic spectrometer, ARES G2 (TA instrument), manufactured by TA Instruments, using the method according to the World Congress of Chemical Eng., Montreal, Canada. An ETC oven is used to control the temperature at 180°C ± 0.1°C. Nitrogen is used to purge the inside of the oven to protect the samples from degradation by oxygen and moisture. The sample holder is a parallel plate with a diameter of 25 mm. The samples were compression molded at 230°C with a diameter of 25 mm and a thickness of 2 mm. An oscillation frequency sweep is used to obtain the storage modulus (G'), loss modulus (G'') at 190°C under nitrogen atmosphere. The crossover of G' and G'' at 190°C, Gc, is used to calculate the polydispersity (PDI) using the following equation: PDI=10 5 / Gc Test methods are also generally described in US Pat. No. 9,045,570, which uses different sample sizes and cone-plate rheometry.

[0030] IZOD impact strength is measured according to ASTM D 256 and D4101.

[0031] Detailed Description Those skilled in the art will appreciate that this discussion is a description of exemplary embodiments only, and is not intended to limit the broader aspects of the disclosure.

[0032] In general, the present disclosure is directed to polyolefin polymer compositions having a unique blend of physical properties. For example, in one embodiment, the polymer compositions can be formulated to have relatively high stiffness properties along with excellent toughness properties. In addition, the polymer compositions can be formulated to have good flow properties. Thus, the polymer compositions are particularly well suited for forming molded articles, such as thermoformed products and injection molded articles. In one embodiment, for example, the polymer compositions can be used to form containers. The stiffness and toughness properties of the polymer compositions allow containers and other articles with internal volumes to be formed with minimal wall thickness. In this way, the polymer articles can be efficiently formed using minimal amounts of the polymer compositions.

[0033] Among other advantages, the polypropylene polymer compositions of the present disclosure have high stiffness properties while also having broad molecular weight distributions and can be formulated using catalyst systems that maintain high catalytic activity during the polymerization process. For example, non-phthalate Ziegler-Natta catalysts can be used during polymerization of the polymers of the present disclosure that maintain activity greater than about 50 kg / g, greater than about 55 kg / g, e.g., greater than about 60 kg / g during the formation of the polymer composition.

[0034] Generally, the polypropylene polymer composition of the present disclosure comprises a blend of polymers. More specifically, the polymer composition comprises a first polypropylene polymer combined with a second polypropylene polymer. The first polypropylene polymer has a relatively low melt flow rate compared to the second polypropylene polymer. Unexpectedly, it has been discovered that a relatively small amount of a low melt flow rate polymer is required in combination with the second polypropylene polymer to obtain a polymer composition with desired high stiffness properties. In fact, the low melt flow rate polypropylene polymer can be present in an amount of less than 50% by weight, such as less than 40% by weight, such as less than 30% by weight, such as less than 20% by weight, and still provide an overall polymer composition with excellent stiffness properties. These results are dramatic and unexpected.

[0035] In addition, as noted above, polypropylene polymer compositions can be produced having a relatively broad molecular weight distribution, which significantly enhances the processability of the composition.

[0036] Additionally, the xylene solubles content of the first and second polypropylene polymers is selectively controlled to maximize stiffness while maintaining high catalytic activity during production of the polymer. For example, the resulting polymer composition may exhibit a flexural modulus according to the following equation: 2072*XS -0.18 In the formula, XS is the xylene solubles content of the polypropylene polymer composition. The xylene solubles content of the polypropylene polymer composition can be, for example, about 2.5% by weight to about 8%.

[0037] For example, in one embodiment, the polypropylene polymer composition of the present disclosure may have a flexural modulus greater than about 1500 MPa, such as greater than about 1550 MPa, such as greater than about 1600 MPa, such as greater than about 1650 MPa, such as greater than about 1700 MPa, such as greater than about 1750 MPa, and generally less than about 2500 MPa, such as less than about 2000 MPa. For example, in one embodiment, the polypropylene polymer composition may have a flexural modulus greater than about 1525 MPa and less than about 2000 MPa, including all 25 MPa increments therebetween.

[0038] In addition to the excellent stiffness properties, the polypropylene polymer composition of the present disclosure also has excellent toughness properties. For example, the polypropylene polymer composition of the present disclosure may have an IZOD impact strength of more than about 40 J / m, such as more than about 50 J / m, such as more than about 55 J / m, such as more than about 60 J / m, such as more than about 65 J / m. The IZOD impact strength is generally less than about 90 J / m, such as less than about 80 J / m.

[0039] As described above, the polypropylene polymer composition of the present disclosure includes a first polypropylene polymer blended with a second polypropylene polymer. The first polypropylene polymer generally has a low melt flow rate and contributes significantly to the stiffness properties of the resulting composition. For example, the first polypropylene polymer may have a melt flow rate of less than about 3 g / 10 min, such as less than about 1 g / 10 min, such as less than about 0.8 g / 10 min, such as less than about 0.5 g / 10 min, and generally greater than about 0.01 g / 10 min, such as greater than about 0.1 g / 10 min. The first polypropylene polymer has a low melt flow rate, but generally has a xylene solubles content of greater than about 2.5 wt%, such as greater than about 3 wt%, such as greater than about 3.5 wt%, such as greater than about 4 wt%, such as greater than about 4.5 wt%, and generally less than about 8 wt%, less than about 7 wt%. The first polypropylene polymer may be formed using a Ziegler-Natta catalyst and may have a relatively broad molecular weight distribution. In one embodiment, the first polypropylene polymer has a polydispersity index greater than about 4, and generally less than about 10, such as less than about 8.5, such as less than about 7, such as less than about 5.5.

[0040] The second polypropylene polymer combined with the first polypropylene polymer generally has a higher melt flow rate. For example, the second polypropylene polymer may generally have a melt flow rate of more than about 5 g / 10 min, such as more than about 7 g / 10 min, such as more than about 9 g / 10 min. The melt flow rate is generally less than about 100 g / 10 min, such as less than about 40 g / 10 min, such as less than about 30 g / 10 min, such as less than about 25 g / 10 min. The xylene soluble content of the second polypropylene polymer is similar to that of the first polypropylene polymer. For example, the xylene soluble content of the second polypropylene polymer is generally more than about 1 wt%, such as more than about 2 wt%, such as more than about 2.5 wt%, such as more than about 3 wt%, such as more than about 4 wt%. In certain embodiments, the xylene solubles content of the second polypropylene polymer can be greater than about 5 wt%, such as greater than about 6 wt%, such as greater than about 6.5 wt%. The xylene solubles content of the second polypropylene polymer is generally less than about 10 wt%, such as less than about 9 wt%, such as less than about 8 wt%, such as less than about 7.5 wt%.

[0041] The second polypropylene polymer may also be formed using a Ziegler-Natta catalyst that maintains high catalytic activity during polymerization. The second polypropylene polymer may have a relatively broad molecular weight distribution, with a polydispersity index greater than about 4 and generally less than about 10, such as less than about 8.5, such as less than about 7, such as less than about 5.5.

[0042] The first polypropylene polymer and the second polypropylene polymer, in one embodiment, can both be polypropylene homopolymers. In an alternative embodiment, one of the polypropylene polymers can be a copolymer. For example, the first polypropylene polymer can be a homopolymer while the second polypropylene polymer can be a copolymer. Alternatively, the first polypropylene polymer can be a copolymer and the second polypropylene polymer can be a homopolymer. In yet another embodiment, the first polypropylene polymer and the second polypropylene polymer are both copolymers. When present as a copolymer, one or both of the polypropylene polymers can include a small amount of a comonomer, such as ethylene. For example, ethylene can be present in an amount less than about 1.5% by weight, such as less than 1% by weight. The copolymer can be a random copolymer, such as a mini-random copolymer.

[0043] According to the present disclosure, a first polypropylene polymer is blended with a second polypropylene polymer to produce a polypropylene polymer composition. The weight ratio between the first polypropylene polymer and the second polypropylene polymer in the final composition is generally about 5:95 to about 80:20, for example about 30:70 to about 67:33. In one embodiment, the first polypropylene polymer or the low melt flow rate polypropylene polymer can be present in a lesser amount than the second polypropylene polymer, but still have the desired stiffness properties. For example, based on the weight of the two polypropylene polymers present, the first polypropylene polymer can be present in an amount less than about 50% by weight, for example less than about 45% by weight, for example less than about 40% by weight, for example less than about 35% by weight, for example less than about 30% by weight, for example less than about 25% by weight, for example less than about 20% by weight, and generally more than about 5% by weight, for example more than about 10% by weight, for example more than about 15% by weight, for example more than about 20% by weight. In one embodiment, the first polypropylene polymer is present in the polymer composition in an amount of about 30% to about 66% by weight, such as about 30% to about 50% by weight, for example, about 30% to about 45% by weight.

[0044] The resulting polypropylene polymer composition not only has good stiffness properties, but also is well suited for molding processes, such as thermoforming and injection molding processes, for producing various articles, especially due to the broad molecular weight distribution. For example, the composition may have a melt flow rate of more than about 0.5 g / 10 min, such as more than about 0.7 g / 10 min, such as more than about 1 g / 10 min, such as more than about 2 g / 10 min, such as more than about 3 g / 10 min, such as more than about 5 g / 10 min, such as more than about 8 g / 10 min, such as more than about 10 g / 10 min, such as more than about 12 g / 10 min, such as more than about 15 g / 10 min. The melt flow rate is generally less than about 30 g / 10 min, such as less than about 25 g / 10 min, such as less than about 20 g / 10 min. In one embodiment, the melt flow rate of the polypropylene composition may be relatively low, and may be from about 0.5 g / 10 min to about 3 g / 10 min. Alternatively, the melt flow rate can be higher, typically from about 5 g / 10 min to about 20 g / 10 min. The melt flow rate can be adjusted by adjusting the relative amounts of different polymers to produce a polymer composition having desired physical properties in combination with desired flow characteristics.

[0045] The total xylene solubles content of the polypropylene polymer composition is generally greater than about 2 wt%, such as greater than about 2.5 wt%, such as greater than about 3 wt%, such as greater than about 3.5 wt%. The total xylene solubles content is generally less than about 10 wt%, such as less than about 8 wt%, such as less than about 7 wt%, such as less than about 6.8 wt%. The polydispersity index of the polymer composition is generally greater than about 4, such as greater than about 5, such as greater than about 6, and generally less than about 10, such as less than about 9, such as less than about 8.

[0046] In addition to the first and second polypropylene polymers, the polypropylene polymer compositions of the present disclosure may contain various other additives and components.

[0047] For example, the polypropylene composition may contain nucleating agents, release agents, slip agents, antiblocking agents, UV stabilizers, heat stabilizers (e.g., DSTDP), colorants / dyes, and the like. In one embodiment, the polymer composition may contain an antioxidant, such as a hindered phenolic antioxidant. The polymer composition may also contain an acid scavenger. Each of the additives may generally be present in the polymer composition in an amount less than about 3 wt%, such as less than about 2 wt%, such as less than about 1 wt%, such as less than about 0.5 wt%, and generally greater than about 0.001 wt%.

[0048] For example, in one embodiment, the polymer composition may optionally contain a nucleating agent, such as an alpha-nucleating agent. The nucleating agent may be present in an amount generally greater than about 0.001% by weight, and generally less than about 1% by weight, such as less than about 0.5% by weight, for example less than about 0.3% by weight.

[0049] In one embodiment, an inorganic nucleating agent such as talc may be used. Other nucleating agents include polymeric nucleating agents such as sodium benzoate, or partial metal salts of rosin acids.

[0050] In another embodiment, the nucleating agent may be selected from the group of phosphorus-based nucleating agents, such as phosphate ester metal salts represented by the formula: [ka] In the formula, R1 is oxygen, sulfur, or a hydrocarbon group of 1 to 10 carbon atoms, each of R2 and R3 is hydrogen or a hydrocarbon group of 1 to 10 carbon atoms, R2 and R3 can be the same as or different from each other, two of R2, two of R3, or R2 and R3 can be bonded together to form a ring, M is a monovalent to trivalent metal atom, n is an integer from 1 to 3, and m is either 0 or 1, with the proviso that n>m.

[0051] Preferred examples of alpha nucleating agents represented by the above formula include sodium-2,2'-methylene-bis(4,6 di-t-butyl-phenyl) phosphate, sodium-2,2'-ethylidene-bis(4,6 di-t-butylphenyl)-phosphate, lithium-2,2'-methylene-bis(4,6 di-t-butylphenyl) phosphate, lithium-2,2'-ethylidene-bis(4,6 di-t-butylphenyl) phosphate, sodium-2,2'-ethylidene-bis(4-i-propyl-6-t-butylphenyl) phosphate, lithium Lithium 2,2'-methylene bis(4-methyl-6-t-butylphenyl) phosphate, Lithium 2,2'-methylene bis(4-ethyl-6-t-butylphenyl) phosphate, Calcium bis[2,2'-thiobis(4-methyl-6-t-butylphenyl)phosphate], Calcium bis[2,2'-thiobis(4-ethyl-6-t-butylphenyl)phosphate], Calcium bis[2,2'-thiobis(4,6-di-t-butylphenyl)phosphate], Magnesium bis[2,2'-thiobis(4,6-di-t-butyl phenyl) phosphate], magnesium bis[2,2'-thiobis(4-t-octylphenyl) phosphate], sodium 2,2'-butylidene-bis(4,6-dimethylphenyl) phosphate, sodium 2,2'-butylidene-bis(4,6-di-t-butyl-phenyl)-phosphate, sodium 2,2'-t-octylmethylene-bis(4,6-dimethyl-phenyl)-phosphate, sodium 2,2'-t-octylmethylene-bis(4,6-di-t-butylphenyl)-phosphate, calcium bis[2,2' -methylene-bis(4,6-di-t-butylphenyl)-phosphate], magnesium-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl)-phosphate], barium-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl)-phosphate], sodium-2,2'-methylene-bis(4-methyl-6-t-butylphenyl)-phosphate, sodium-2,2'-methylene-bis(4-ethyl-6-t-butylphenyl)phosphate, sodium (4,4'-dimethyl-5,6'-di-t-butyl-2,2'-biphenyl) phosphate, calcium-bis-[(4,4'-dimethyl-6,6'-di-t-butyl-2,2'-biphenyl) phosphate], sodium-2,2'-ethylidene-bis(4-m-butyl-6-t-butyl-phenyl) phosphate, sodium-2,2'-methylene-bis-(4,6-di-methylphenyl)-phosphate, sodium-2,2'-methylene-bis(4,6-di-t-ethyl-phenyl) phosphate, potassium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl)-phosphate, calcium Examples of such phosphates include mu-bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)-phosphate], magnesium-bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)-phosphate], barium-bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)-phosphate], aluminum-hydroxy-bis[2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate], and aluminum-tris[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)-phosphate].

[0052] A second group of phosphorus-based nucleating agents includes, for example, aluminum-hydroxy-bis[2,4,8,10-tetrakis(1,1-dimethylethyl)-6-hydroxy-12H-dibenzo-[d,g]-dioxa-phosphotin-6-oxidate] and blends thereof with Li-myristate or Li-stearate.

[0053] Among the phosphorus-based nucleating agents, sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate, or aluminum-hydroxy-bis[2,2'-methylene-bis(4,6-di-t-butyl-phenyl)-phosphate], or aluminum-hydroxy-bis-[2,4,8,10-tetrakis(1,1-dimethylethyl)-6-hydroxy-12H-dibenzo-[d,g]-dioxa-phosphotin-6-oxidate], or blends thereof with Li-myristate or Li-stearate, are particularly preferred.

[0054] Also, sorbitol-based nucleating agents such as optionally substituted dibenzylidene sorbitol (e.g., 1,3:2,4 dibenzylidene sorbitol, 1,3:2,4 di(methylbenzylidene) sorbitol, 1,3:2,4 di(ethylbenzylidene) sorbitol, 1,3:2,4 bis(3,4-dimethylbenzylidene) sorbitol, etc.) or rosin can be used as a nucleating agent.

[0055] Further suitable alpha-nucleating agents are polymeric nucleating agents selected from the group consisting of vinylcycloalkane polymers and vinylalkane polymers. Nucleation with these polymeric nucleating agents is achieved either by special reactor techniques where the catalyst is prepolymerized with a monomer such as vinylcyclohexane (VCH) or by blending a propylene polymer with a vinyl(cyclo)alkane polymer.

[0056] Nucleating agents such as ADK NA-11 (methylene-bis(4,6-di-t-butylphenyl)phosphate sodium salt) and ADK NA-21 (containing aluminum hydroxy-bis[2,4,8,10-tetrakis(1,1-dimethylethyl)-6-hydroxy-12H-dibenzo-[d,g]-dioxa-phosphotin-6-oxidate]) are commercially available from Asahi Denka Kokai and are examples of those that may be added to the polyolefin composition. Millad NX8000 (nonitol, 1,2,3-trideoxy-4,6:5,7-bis-O-[(4-propylphenyl)methylene)], Millad 3988 (3,4-dimethylbenzylidene sorbitol), Millad 3905, and Millad 3940 available from Milliken & Company are other examples of nucleating agents that may be utilized.

[0057] Further commercially available alpha-nucleating agents that can be used in the composition are, for example, Irgaclear XT 386 (N-[3,5-bis-(2,2-dimethyl-propionylamino)-phenyl]-2,2-dimethylpropionamide) from Ciba Specialty Chemicals, Hyperform HPN-68L and Hyperform HPN-20E from Milliken & Company.

[0058] According to one embodiment, the at least one alpha-nucleating agent is comprised of a polymeric nucleating agent selected from the group consisting of vinylcycloalkane polymers and vinylalkane polymers, preferably poly-vinylcyclohexane (pVCH).

[0059] According to further embodiments, the at least one alpha-nucleating agent is selected from the group consisting of aluminum hydroxy-bis[2,4,8,10-tetrakis(1,1-dimethylethyl)-6-hydroxy-12H-dibenzo-[d,g]-dioxa-phosphotin-6-oxidate]-based nucleating agents (e.g., ADK NA-21, NA-21 E, NA-21 F), sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate (ADK NA-11), aluminum-hydroxy-bis[2,2'-methylene-bis(4,6-di-t-butyl-phenyl)-phosphate], and sorbitol-based nucleating agents (e.g., Millad 3988, Millad 3905, and Millad 3940).

[0060] In one embodiment, the polypropylene composition may further comprise a clarifier. The clarifier may be added to further improve the transparency properties of the composition. The clarifier may, for example, include compounds capable of generating a gelling network within the composition.

[0061] In one embodiment, the clarification agent may include a sorbitol compound, such as a sorbitol acetal derivative. In one embodiment, for example, the clarification agent may include benzyl sorbitol.

[0062] With respect to the sorbitol acetal derivatives that can be used as additives in some embodiments, the sorbitol acetal derivatives are shown in formula (I): [ka] wherein R1-R5 comprise the same or different moieties selected from hydrogen and C1-C3 alkyl.

[0063] In some embodiments, R1-R5 are hydrogen such that the sorbitol acetal derivative is 2,4-dibenzylidene sorbitol ("DBS"). In some embodiments, R1, R4, and R5 are hydrogen and R2 and R3 are methyl groups such that the sorbitol acetal derivative is 1,3:2,4-di-p-methyldibenzylidene-D-sorbitol ("MDBS"). In some embodiments, R1-R4 are methyl groups and R5 is hydrogen such that the sorbitol acetal derivative is 1,3:2,4-bis(3,4-dimethylobenzylideno)sorbitol ("DMDBS"). In some embodiments, R2, R3, and R5 are propyl groups (-CH2-CH2-CH3) and R1 and R4 are hydrogen, such that the sorbitol acetal derivative is 1,2,3-trideoxy-4,6:5,7-bis-O-(4-propylphenylmethylene)nonitol ("TBPMN").

[0064] Other embodiments of clarification agents that may be used include: 1,3:2,4-dibenzylidene sorbitol, 1,3:2,4-bis(p-methylbenzylidene)sorbitol, Di(p-methylbenzylidene)sorbitol Di(p-ethylbenzylidene)sorbitol Bis(5',6',7',8'-tetrahydro-2-naphthylidene)sorbitol

[0065] In one embodiment, the clarification agent may also include a bisamide, such as benzenetriamide.The above clarification agents may be used alone or in combination.

[0066] When present in the polymer composition, one or more clarifiers are generally added in an amount of more than about 200 ppm, for example, more than about 1,800 ppm, for example, more than about 2,000 ppm, for example, more than about 2,200 ppm.One or more clarifiers are generally present in an amount of less than about 20,000 ppm, for example, less than about 15,000 ppm, for example, less than about 10,000 ppm, for example, less than about 8,000 ppm, for example, less than about 5,000 ppm.The amount of clarifier present in the composition can depend on various factors, including the type of clarifier used.

[0067] The first and second polypropylene polymers can be produced using a variety of different polymerization methods and procedures. In one embodiment, both of the polymers are formed from propylene monomer in the presence of a Ziegler-Natta catalyst. For example, the olefin polymerization can occur in the presence of a catalyst system, including a catalyst, an internal electron donor, a cocatalyst, and optionally an external electron donor and / or an activity limiting agent. The polymerization process used to produce the two polymers can be carried out using known techniques. For example, the polymers can be formed in a gas phase reactor or in a bulk phase reactor. Specifically, the polymers can be formed in a gas phase reactor using a fluidized bed or stirred bed reactor, or in a slurry phase using an inert hydrocarbon solvent or diluent or liquid monomer. For example, the first and second polypropylene polymers can both be formed in a gas phase reactor. Alternatively, the first and second polypropylene polymers can both be formed in a bulk (liquid propylene) phase reactor. In a further embodiment, one of the first and second polypropylene polymers is formed in a gas phase reactor and the other of the first and second polypropylene polymers is formed in a bulk phase reactor. For example, the first polypropylene polymer may be formed in a bulk phase reactor and the second polypropylene polymer may be formed in a gas phase reactor.

[0068] In one embodiment, the first polypropylene polymer and the second polypropylene polymer are produced in two different polymerization processes and then combined together. Alternatively, the first polypropylene polymer and the second polypropylene polymer can be produced sequentially in a process that includes a series of reactors. For example, one of the polypropylene polymers can be produced in a first reactor and then transferred to a second reactor where the other polypropylene polymer is produced.

[0069] In one embodiment of the present disclosure, the polymerization is carried out in the presence of a stereoregular olefin polymerization catalyst. For example, the catalyst can be a Ziegler-Natta catalyst. For example, in one embodiment, a catalyst sold under the trade name CONSISTA and available from W.R. Grace & Company can be used. In one embodiment, a phthalate-free electron donor is selected.

[0070] In one embodiment, the catalyst comprises a procatalyst composition containing a titanium moiety, such as titanium chloride, a magnesium moiety, such as magnesium chloride, and at least one internal electron donor.

[0071] The procatalyst precursor can include (i) magnesium, (ii) a transition metal compound from Groups IV to VII, (iii) a halide, oxyhalide and / or alkoxide, and / or the alkoxide of (i) or (i) and / or (ii), and (iv) a combination of (i), (ii) and (iii). Non-limiting examples of suitable procatalyst precursors include the halides, oxyhalides, alkoxides of magnesium, manganese, titanium, vanadium, chromium, molybdenum, zirconium, hafnium, and combinations thereof.

[0072] In one embodiment, the procatalyst precursor contains magnesium as the only metal component. Non-limiting examples include anhydrous magnesium chloride and / or its alcohol adducts, magnesium alkoxides and / or aryloxides, mixed magnesium alkoxyhalides, and / or carboxylated magnesium dialkoxides or aryloxides.

[0073] In one embodiment, the procatalyst precursor is an alcohol adduct of anhydrous magnesium chloride. The anhydrous magnesium chloride adduct is generally defined as MgCl2-nROH, where n has a total alcohol in the range of 1.5 to 6.0, preferably 2.5 to 4.0, and most preferably 2.8 to 3.5 moles. ROH is a C1 to C4 alcohol, straight or branched chain, or a mixture of alcohols. Preferably, ROH is ethanol, or a mixture of ethanol and a higher alcohol. When ROH is a mixture, the molar ratio of ethanol to higher alcohol is at least 80:20, preferably 90:10, and most preferably at least 95:5.

[0074] In one embodiment, the substantially spherical MgCl-nEtOH adduct may be formed by a spray crystallization process. In one embodiment, the spherical MgCl precursor has an average particle size (Malvern d) of about 15-150 microns, preferably 20-100 microns, and most preferably 35-85 microns. 50 ).

[0075] In one embodiment, the procatalyst precursor comprises a transition metal compound and a magnesium metal compound. The transition metal compound has the general formula TrX x wherein Tr is a transition metal and X is a halogen or C 1~10 Tr is a hydrocarboxyl or hydrocarbyl group, and x is the number of such X groups in the compound combined with the magnesium metal compound. Tr can be a Group IV metal, Group V metal, or Group VI metal. In one embodiment, Tr is preferably a Group IV metal, such as titanium. X can be chloride, bromide, C 1~4 It may be an alkoxide or a phenoxide, or a mixture thereof. In one embodiment, X is chloride.

[0076] The precursor composition may be prepared by chlorination of the aforementioned mixed magnesium compounds, titanium compounds, or mixtures thereof.

[0077] In one embodiment, the precursor composition has the formula Mg dTi(OR e ) f X g A mixed magnesium / titanium compound having the formula: e is an aliphatic or aromatic hydrocarbon radical having 1 to 14 carbon atoms or COR', where R' is an aliphatic or aromatic hydrocarbon radical having 1 to 14 carbon atoms, and each OR e The groups are the same or different; X is independently chlorine, bromine, or iodine; d is 0.5 to 56, or 2 to 4, or 3; f is 2 to 116, or 5 to 15; and g is 0.5 to 116, or 1 to 3.

[0078] According to the present disclosure, the procatalyst precursor described above is combined with at least one internal electron donor. The internal electron donor can include a substituted phenylene aromatic diester.

[0079] In one embodiment, the first internal electron donor comprises a substituted phenylene aromatic diester having the following structure (I): [ka] In the formula, R1~R 14 are the same or different. R1 to R 14 are each selected from hydrogen, a substituted hydrocarbyl group having 1 to 20 carbon atoms, an unsubstituted hydrocarbyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a heteroatom, and combinations thereof. 14 At least one of is not hydrogen.

[0080] In one embodiment, the substituted phenylene aromatic diester may be any of the substituted phenylene aromatic diesters disclosed in U.S. Patent Application No. 61 / 141,959, filed December 31, 2008, the entire contents of which are incorporated herein by reference.

[0081] In one embodiment, the substituted phenylene aromatic diester may be any of the substituted phenylene aromatic diesters disclosed in International Publication No. WO 12088028, filed December 20, 2011, the entire contents of which are incorporated herein by reference.

[0082] In one embodiment, at least one (or two, or three, or four) R groups of R1-R4 are selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, heteroatoms, and combinations thereof.

[0083] In one embodiment, R 14 At least one (or some, or all) of the R groups is selected from the group consisting of substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, heteroatoms, and combinations thereof. In another embodiment, at least one of R5-R9 and R 10 ~R 14 At least one of is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, heteroatoms, and combinations thereof.

[0084] In one embodiment, at least one of R1 to R4 and R5 to R 14 At least one of R1-R4, at least one of R5-R9, and R6 is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, heteroatoms, and combinations thereof. In another embodiment, at least one of R1-R4, at least one of R5-R9, and R 10 ~R 14At least one of them is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, heteroatoms, and combinations thereof.

[0085] In one embodiment, any successive R groups from R1 to R4, and / or any successive R groups from R5 to R9, and / or R 10 ~R 14 Any successive R groups may be linked to form a cyclic or intracyclic structure. The cyclic / intercyclic structure may be aromatic or non-aromatic. In one embodiment, the cyclic / intercyclic structure is a C5- or C6-membered ring.

[0086] In one embodiment, at least one of R1 through R4 is selected from a substituted hydrocarbyl group having 1 to 20 carbon atoms, an unsubstituted hydrocarbyl group having 1 to 20 carbon atoms, and combinations thereof. 14 At least one of R1 to R4, and / or R5 to R9, and / or R 10 ~R 14 may be linked to form cyclic structures or intra-cyclic structures. The cyclic structures and / or intra-cyclic structures may be aromatic or non-aromatic.

[0087] In one embodiment, R1 to R4, and / or R5 to R9, and / or R 10 ~R 14 Any successive R groups may be members of a C5-C6 membered ring.

[0088] In one embodiment, structure (I) includes R1, R3, and R4 as hydrogen. R2 is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, and combinations thereof. R5 to R 14 are the same or different, R5 to R 14Each of is selected from hydrogen, substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, halogen, and combinations thereof.

[0089] In one embodiment, R2 is selected from a C1-C8 alkyl group, a C3-C6 cycloalkyl group, or a substituted C3-C6 cycloalkyl group. R2 can be a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a t-butyl group, an isobutyl group, a sec-butyl group, a 2,4,4-trimethylpentan-2-yl group, a cyclopentyl group, and a cyclohexyl group.

[0090] In one embodiment, structure (I) comprises R2 which is methyl, and R5 through R 14 Each of is hydrogen.

[0091] In one embodiment, structure (I) includes R2 that is ethyl, and R5-R 14 Each of is hydrogen.

[0092] In one embodiment, structure (I) comprises R2 that is t-butyl, and R5 -R 14 Each of is hydrogen.

[0093] In one embodiment, structure (I) comprises R2 being ethoxycarbonyl, and R5-R 14 Each of is hydrogen.

[0094] In one embodiment, structure (I) includes R2, R3, and R4 each as hydrogen, and R1 is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, and combinations thereof. 14 are the same or different and each is selected from hydrogen, substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, halogen, and combinations thereof.

[0095] In one embodiment, structure (I) comprises R1 which is methyl, and R5 through R 14 Each of is hydrogen.

[0096] In one embodiment, structure (I) includes R2 and R4 that are hydrogen, and R1 and R3 are the same or different. Each of R1 and R3 is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, and combinations thereof. 14 are the same or different, R5 to R 14 Each of is selected from substituted hydrocarbyl groups having 1 to 20 carbon atoms, unsubstituted hydrocarbyl groups having 1 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, halogens, and combinations thereof.

[0097] In one embodiment, structure (I) comprises R1 and R3, which are the same or different. Each of R1 and R3 is selected from a C1-C8 alkyl group, a C3-C6 cycloalkyl group, or a substituted C3-C6 cycloalkyl group. 14 are the same or different, and R5 to R 14 are each selected from hydrogen, a C1-C8 alkyl group, and halogen. Non-limiting examples of suitable C1-C8 alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, i-butyl, t-butyl, n-pentyl, i-pentyl, neopentyl, Examples of suitable C3-C6 cycloalkyl groups include cyclopentyl and cyclohexyl groups. In a further embodiment, R5-R 14 At least one of them is a C1 to C8 alkyl group or a halogen.

[0098] In one embodiment, structure (I) includes R1 which is a methyl group, and R3 which is a t-butyl group. R2, R4 and R5 through R 14 Each of is hydrogen.

[0099] In one embodiment, structure (I) includes R1 and R3 that are isopropyl groups. R2, R4 and R5-R 14 Each of is hydrogen.

[0100] In one embodiment, structure (I) comprises R, R, and R as methyl groups. 10 R2, R4, R6 to R9, and R 11 ~R 14 Each of is hydrogen.

[0101] In one embodiment, structure (I) comprises R, R, and R as methyl groups. 12 and R3 is a t-butyl group. 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0102] In one embodiment, structure (I) includes R1 as a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0103] In one embodiment, structure (I) comprises R, R, R, R, R as methyl groups. 10 , R 12 , and R 14 and R3 is a t-butyl group. 11 and R 13 Each of is hydrogen.

[0104] In one embodiment, structure (I) includes R1 as a methyl group and R3 is a t-butyl group. R5, R7, R9, R 10 , R 12 and R14 Each of R2, R4, R6, R8, R 11 and R 13 Each of is hydrogen.

[0105] In one embodiment, the substituted phenylene aromatic diester has structure (II) with R1 being a methyl group, and R3 being a t-butyl group. Each of R2 and R4 is hydrogen. R8 and R9 are members of a C6 membered ring to form a 1-naphthoyl moiety. 13 and R 14 is a member of a C6-membered ring and forms another 1-naphthoyl moiety. Structure (II) is provided below. [ka]

[0106] In one embodiment, the substituted phenylene aromatic diester has structure (III) with R1 being a methyl group, and R3 being a t-butyl group. Each of R2 and R4 is hydrogen. R6 and R7 are members of a C6 membered ring to form a 2-naphthoyl moiety. 12 and R 13 is a member of a C6-membered ring to form a 2-naphthoyl moiety. Structure (III) is provided below. [ka]

[0107] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0108] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0109] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0110] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0111] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0112] In one embodiment, structure (I) comprises R1 being a methyl group and R3 being a t-butyl group. 11 , and R 12 Each of R2, R4, R5, R8, R9, R 10 , R 13 , and R 14 Each of is hydrogen.

[0113] In one embodiment, structure (I) comprises R1 being a methyl group and R3 being a t-butyl group. 11 , and R 13 Each of R2, R4, R5, R7, R9, R 10 , R 12 , and R 14 Each of is hydrogen.

[0114] In one embodiment, structure (I) includes R1 which is a methyl group, and R3 is a t-butyl group. 14 Each of is a fluorine atom.

[0115] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0116] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 and R 14 Each of is hydrogen.

[0117] In one embodiment, R1 is a methyl group and R3 is a t-butyl group. 12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0118] In one embodiment, structure (I) includes R1 which is a methyl group and R3 is a t-butyl group.12 Each of R2, R4, R5, R6, R8, R9, R 10 , R 11 , R 13 , and R 14 Each of is hydrogen.

[0119] In one embodiment, structure (I) includes R1 which is a methyl group, and R3 is a 2,4,4-trimethylpentan-2-yl group. R2, R4 and R5 to R 14 Each of is hydrogen.

[0120] In one embodiment, structure (I) includes R1 and R3, each of which is a sec-butyl group. 14 Each of is hydrogen.

[0121] In one embodiment, the substituted phenylene aromatic diester has the structure (IV), where R1 and R2 are members of a C6 ring and form a 1,2-naphthalene moiety. 14 Each of is hydrogen. Structure (IV) is provided below. [ka]

[0122] In one embodiment, the substituted phenylene aromatic diester has the structure (V), where R2 and R3 are members of a C6 ring and form a 2,3-naphthalene moiety. 14 Each of is hydrogen. Structure (V) is provided below. [ka]

[0123] In one embodiment, structure (I) includes R1 and R4, each of which is a methyl group. R2, R3, R5-R9, and R 10 ~R 14 Each of is hydrogen.

[0124] In one embodiment, structure (I) includes R1 which is a methyl group. R4 is an i-propyl group. R2, R3, R5-R9, and R 10 ~R 14 Each of is hydrogen.

[0125] In one embodiment, structure (I) comprises R1, R3, and R4, each of which is an i-propyl group. 10 ~R 14 Each of is hydrogen.

[0126] In one embodiment, each of R1 and R4 is selected from a methyl group, an ethyl group, and a vinyl group. Each of R2 and R3 is selected from a hydrogen group, a secondary alkyl group, or a tertiary alkyl group, and R2 and R3 are not hydrogen at the same time. In other words, if R2 is hydrogen, then R3 is not hydrogen (and vice versa).

[0127] In one embodiment, a second internal electron donor may be used, which generally comprises a polyether capable of coordinating in a bidentate fashion. In one embodiment, the second internal electron donor is a substituted 1,3-diether of structure VI: [ka] In the formula, R1 and R2 are the same or different, methyl, C2-C 18 Straight or branched chain alkyl, C3-C 18 Cycloalkyl, C4-C 18 Cycloalkyl-Alkyl, C4-C 18 Alkyl-cycloalkyl, phenyl, organosilicon, C7-C 18 Aryl alkyl or C7-C 18 An alkylaryl radical, where R1 or R2 may also be a hydrogen atom.

[0128] In one embodiment, the second internal electron donor may comprise a cyclic or polycyclic 1,3-diether having structure VII: [ka] wherein R1, R2, R3, and R4 are as described for R1 and R2 in structure VI, or may be combined to form one or more C5-C7 fused aromatic or non-aromatic ring structures, optionally containing N, O, or S heteroatoms. Specific examples of second internal electron donors include: Examples of the fluorene include 4,4-bis(methoxymethyl)-2,6-dimethylheptane, 9,9-bis(methoxymethyl)fluorene, or a mixture thereof.

[0129] The precursor is converted to a solid procatalyst by further reaction (halogenation) with an inorganic halide compound, preferably a titanium halide compound, and incorporation of an internal electron donor.

[0130] One suitable method for halogenating the precursor is by reacting the precursor with a tetravalent titanium halide, optionally in the presence of a hydrocarbon or halogenated hydrocarbon diluent, at elevated temperature. A preferred tetravalent titanium halide is titanium tetrachloride.

[0131] The resulting procatalyst composition may generally contain titanium in an amount of about 0.5% to about 6% by weight, such as about 1.5% to about 5% by weight, such as about 2% to about 4% by weight. The solid catalyst may generally contain magnesium in an amount greater than about 5% by weight, such as greater than about 8% by weight, such as greater than about 10% by weight, such as greater than about 12% by weight, such as greater than about 14% by weight, such as greater than about 16% by weight. Magnesium is contained in the catalyst in an amount less than about 25% by weight, such as less than about 23% by weight, such as less than about 20% by weight. The internal electron donor may be present in the catalyst composition in an amount less than about 30% by weight, such as less than about 25% by weight, such as less than about 22% by weight, such as less than about 20% by weight, such as less than about 19% by weight. The internal electron donor is generally present in an amount greater than about 5% by weight, such as greater than about 9% by weight.

[0132] In one embodiment, the procatalyst composition is combined with a cocatalyst to form a catalyst system, which is a system that forms an olefin-based polymer when contacted with an olefin under polymerization conditions. The catalyst system may optionally include an external electron donor, an activity limiting agent, and / or various other components.

[0133] As used herein, a "cocatalyst" is a material capable of converting a procatalyst into an active polymerization catalyst. Cocatalysts may include hydrides, alkyls, or aryls of aluminum, lithium, zinc, tin, cadmium, beryllium, magnesium, and combinations thereof. In one embodiment, the cocatalyst is a hydrocarbyl aluminum cocatalyst represented by the formula R3Al, where each R is an alkyl, cycloalkyl, aryl, or hydride radical, at least one R is a hydrocarbyl radical, two or three R radicals can be bonded to a cyclic radical forming a heterocyclic ring structure, each R can be the same or different, and each R, which is a hydrocarbyl radical, has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms. In further embodiments, each alkyl radical can be straight or branched chain, and such hydrocarbyl radicals can be mixed radicals, i.e., the radicals can contain alkyl, aryl, and / or cycloalkyl groups. Non-limiting examples of suitable radicals are methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, 2-methylpentyl, n-heptyl, n-octyl, isooctyl, 2-ethylhexyl, 5,5-dimethylhexyl, n-nonyl, n-decyl, isodecyl, n-undecyl, n-dodecyl.

[0134] Non-limiting examples of suitable hydrocarbyl aluminum compounds are triisobutylaluminum, tri-n-hexylaluminum, diisobutylaluminum hydride, di-n-hexylaluminum hydride, isobutylaluminum dihydride, n-hexylaluminum dihydride, diisobutylhexylaluminum, isobutyldihexylaluminum, trimethylaluminum, triethylaluminum, tri-n-propylaluminum, triisopropylaluminum, tri-n-butylaluminum, tri-n-octylaluminum, tri-n-decylaluminum, tri-n-dodecylaluminum. In one embodiment, the preferred cocatalyst is selected from triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, diisobutylaluminum hydride, and di-n-hexylaluminum hydride, and the most preferred cocatalyst is triethylaluminum.

[0135] In one embodiment, the cocatalyst has the formula R n AIX 3-n where n=1 or 2, R is alkyl, and X is a halide or alkoxide. Non-limiting examples of suitable compounds are methylaluminoxane, isobutylaluminoxane, diethylaluminum ethoxide, diisobutylaluminum chloride, tetraethyldialuminoxane, tetraisobutyldialuminoxane, diethylaluminum chloride, ethylaluminum dichloride, methylaluminum dichloride, and dimethylaluminum chloride.

[0136] In one embodiment, the catalyst composition includes an external electron donor. As used herein, an "external electron donor" is a compound that is added independently of the procatalyst formation and contains at least one functional group that can donate a pair of electrons to a metal atom. Without being bound to a particular theory, it is believed that the external electron donor enhances the stereoselectivity of the catalyst (i.e., reduces xylene solubles in the formant polymer).

[0137] In one embodiment, the external electron donor may be selected from one or more of alkoxylates, amines, ethers, carboxylates, ketones, amides, carbamates, phosphines, phosphates, phosphites, sulfonates, sulfones, and / or sulfoxides.

[0138] In one embodiment, the external electron donor is an alkoxysilane. Alkoxysilanes have the general formula SiR m (OR') 4-m (I) wherein R is independently at each occurrence hydrogen or a hydrocarbyl or amino group optionally substituted with one or more substituents containing one or more Group 14, 15, 16 or 17 heteroatoms, and R' contains up to 20 atoms other than hydrogen and halogens, and R' is C 1~4 In one embodiment, R is an alkyl group, and m is 0, 1, 2, or 3. In one embodiment, R is 6~12 Aryl, alkyl or aralkyl, C 3~12 Cycloalkyl, C 3~12 Branched chain alkyl or C 3~12 R' is a cyclic or acyclic amino group, 1~4alkyl, and m is 1 or 2. Non-limiting examples of suitable silane compositions include dicyclopentyldimethoxysilane, di-tert-butyldimethoxysilane, methylcyclohexyldimethoxysilane, methylcyclohexyldiethoxysilane, ethylcyclohexyldimethoxysilane, diphenyldimethoxysilane, diisopropyldimethoxysilane, di-n-propyldimethoxysilane, diisobutyldimethoxysilane, diisobutyldiethoxysilane, isobutylisopropyldimethoxysilane, di-n-butyldimethoxysilane, cyclopentyltrimethoxysilane, isopropyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, ethyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, diethylaminotriethoxysilane, cyclopentylpyrrolidinodimethoxysilane, bis(pyrrolidino)dimethoxysilane, bis(perhydroisoquinolino)dimethoxysilane, and dimethyldimethoxysilane. In one embodiment, the silane composition is dicyclopentyldimethoxysilane (DCPDMS), methylcyclohexyldimethoxysilane (MChDMS), diisopropyldimethoxysilane (DIPDMS), n-propyltrimethoxysilane (NPTMS), diethylaminotriethoxysilane (DATES), or n-propyltriethoxysilane (PTES), and any combination thereof.

[0139] In one embodiment, the external donor can be a mixture of at least two alkoxysilanes. In further embodiments, the mixture can be dicyclopentyldimethoxysilane and methylcyclohexyldimethoxysilane, dicyclopentyldimethoxysilane and tetraethoxysilane, or dicyclopentyldimethoxysilane and n-propyltriethoxysilane.

[0140] In one embodiment, the external electron donor is selected from one or more of a benzoate and / or a diol ester. In another embodiment, the external electron donor is 2,2,6,6-tetramethylpiperidine. In yet another embodiment, the external electron donor is a diether.

[0141] In one embodiment, the catalyst composition includes an activity limiting agent (ALA). As used herein, an "activity limiting agent" ("ALA") is a substance that reduces catalyst activity at elevated temperatures (i.e., temperatures above about 85°C). The ALA inhibits or otherwise prevents polymerization reactor upsets and ensures that the polymerization process continues. Typically, the activity of Ziegler-Natta catalysts increases as the reactor temperature increases. Ziegler-Natta catalysts also typically maintain high activity at temperatures close to the melting point of the polymer produced. Heat generated by an exothermic polymerization reaction can cause polymer particle aggregates to form, which can ultimately interrupt the polymer production process. The ALA reduces catalyst activity at elevated temperatures, thereby preventing reactor upsets and reducing (or preventing) particle agglomeration, ensuring that the polymerization process continues.

[0142] The activity limiting agent may be a carboxylate ester, a diether, a poly(alkene glycol), a poly(alkene glycol) ester, a poly(alkene glycol) ester, a diol ester, and combinations thereof. The carboxylate ester may be an aliphatic or aromatic mono- or polycarboxylate ester. Non-limiting examples of suitable monocarboxylate esters include ethyl and methyl benzoate, ethyl p-methoxybenzoate, Included are methyl p-ethoxybenzoate, ethyl p-ethoxybenzoate, ethyl acrylate, methyl methacrylate, ethyl acetate, ethyl p-chlorobenzoate, hexyl p-aminobenzoate, isopropyl naphthenate, n-amyl toluate, ethyl cyclohexanoate, and propyl pivalate.

[0143] In one embodiment, the external electron donor and / or activity limiting agent may be added separately to the reactor. In another embodiment, the external electron donor and activity limiting agent may be premixed and then added to the reactor as a mixture. More than one external electron donor or more than one activity limiting agent may be used in the mixture. In one embodiment, the mixture includes dicyclopentyldimethoxysilane and isopropyl myristate, dicyclopentyldiethoxysilane and poly(ethylene glycol) laurate, dicyclopentyldimethoxysilane and isopropyl myristate and poly(ethylene glycol) dioleate, methylcyclohexyldimethoxysilane and isopropyl myristate, n-propyltrimethoxysilane and isopropyl myristate, dimethyldimethoxysilane and methylcyclohexyldimethoxysilane and isopropyl myristate, dicyclopentyldimethoxysilane and n-propyltriethoxysilane and isopropyl myristate, and dicyclopentyldimethoxysilane and tetraethoxysilane, isopropyl myristate, pentyl valerate, and combinations thereof.

[0144] In one embodiment, the catalyst composition comprises any of the aforementioned external electron donors in combination with any of the aforementioned activity limiting agents.

[0145] The first and second polypropylene polymers can each be formed from the catalyst system described above. The propylene polymers can be formed from the same non-phthalate Ziegler-Natta catalyst system or can be made from a different non-phthalate Ziegler-Natta catalyst system. It has been discovered that by using the catalyst system described above in conjunction with controlling the xylene solubles content of the propylene polymer, the first and second polypropylene polymers can be produced at relatively high catalytic activity while still producing a polypropylene polymer composition having excellent stiffness properties. For example, the first and second polypropylene polymers can be produced from the catalyst system described above during a process in which the catalytic activity is at least 50 kg / g, such as at least 55 kg / g, such as at least 60 kg / g, such as even greater than about 65 kg / g. The catalytic activity is generally less than about 100 kg / g. In accordance with the present disclosure, the two different polypropylene polymers are then combined to maximize stiffness properties without sacrificing toughness. Overall, the polypropylene polymer composition can be produced more efficiently than previously produced high stiffness polypropylene polymers. Furthermore, in addition to excellent stiffness and toughness properties, the polypropylene polymer compositions of the present disclosure also possess excellent thermoformable and moldable properties and can be easily formed into a variety of different articles and products.

[0146] For example, the polypropylene polymer compositions of the present disclosure are well suited for producing molded articles. The polypropylene compositions can be used, for example, in injection molding, blow molding, extrusion, and rotational molding applications.

[0147] The polypropylene polymer composition of the present disclosure can be used to make many different articles and products. The high stiffness and excellent flow properties, for example, allow the polypropylene polymer composition to be used to make all kinds of free-standing articles and products. The high stiffness properties allow the manufacture of articles with relatively thin walls while still having the desired shape retention properties. In addition, the high stiffness and toughness properties allow the products and articles made according to the present disclosure to withstand impact forces that may result from drops or other external events.

[0148] For example, the polypropylene polymer composition of the present disclosure is well suited for making any and all types of containers while minimizing the wall thickness and thus the amount of polymer required to make the article. Containers that can be made according to the present disclosure include, for example, storage containers, packaging containers, food containers, etc. Other containers can include cups and other beverage or liquid holding containers.

[0149] The present disclosure may be better understood with reference to the following examples. EXAMPLES

[0150] A variety of different polypropylene polymer compositions were made in accordance with the present disclosure and tested for stiffness and toughness. The samples were compared to a basic reactor grade polypropylene polymer.

[0151] The samples made according to the present disclosure included a first polypropylene polymer combined with a second polypropylene polymer to form a polypropylene polymer composition. All polypropylene polymers produced were polymerized in the presence of a non-phthalate Ziegler-Natta catalyst, as described above. In particular, the catalyst used was a CONSISTA catalyst marketed by W.R. Grace & Co. The polymers were produced in a gas phase reactor. In this example, only polypropylene homopolymers were produced.

[0152] In particular, polymer pellet samples were produced that were injection molded into test specimens. The test specimens were prepared according to ASTM test D4101 to produce specimens for testing flexural modulus and IZOD impact resistance.

[0153] The melt flow rate and xylene solubles content of each polypropylene polymer produced were measured, with the following results: [Table 1]

[0154] Figure 1 is a graphical representation of the results shown above. In particular, Figure 1 compares the flexural modulus of the polymers with the xylene solubles content. As shown, the polymers made according to the present disclosure had dramatically better stiffness properties than the comparative samples. In one aspect, the samples made according to the present disclosure can exhibit a flexural modulus according to the following equation: 2072*XS -0.18 In the formula, the xylene solubles content varies from 3% to 6.8% by weight.

[0155] These and other modifications and variations to the present invention may be implemented by those skilled in the art without departing from the spirit and scope of the present invention, as more particularly set forth in the appended claims. In addition, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Moreover, those skilled in the art will appreciate that the foregoing description is by way of example only, and is not intended to limit the invention as further set forth in such appended claims.

Claims

1. 1. A polypropylene polymer composition comprising: The polypropylene polymer composition comprises a first polypropylene polymer in combination with a second polypropylene polymer, the first polypropylene polymer having a melt flow rate of 0.1 g / 10 min to 3 g / 10 min and a xylene solubles content of 1.0 wt % to 7 wt %, the second polypropylene polymer having a melt flow rate of 5 g / 10 min to 100 g / 10 min and a xylene solubles content of 1 wt % to 7 wt %, and the polypropylene polymer composition has a flexural modulus according to the formula: FX≧2072*XS -0.18 wherein FX is the flexural modulus, XS is the xylene solubles content of the polypropylene polymer composition, the xylene solubles content of the polypropylene polymer composition being from 2.5% to 7% by weight; The melt flow rate is measured according to ASTM D 1238 test method at 230° C. using a 2.16 kg weight of the propyne-based polymer; and Flexural modulus is determined according to ASTM 3641 and using type 1 specimens molded according to ASTM D4101, according to ASTM D790-10 Method A at 1.3 mm / min; A polypropylene polymer composition.

2. 2. The polypropylene polymer composition of claim 1, wherein the first polypropylene polymer has a xylene solubles content of from 2.5% to 7% by weight and the second polypropylene polymer has a xylene solubles content of from 2.5% to 7% by weight.

3. 2. The polypropylene polymer composition of claim 1, wherein one of the polypropylene polymers has a xylene solubles content greater than 5 wt.% and the other polypropylene polymer has a xylene solubles content less than 4 wt.%.

4. 2. The polypropylene polymer composition of claim 1, wherein one of the polypropylene polymers has a xylene solubles content greater than 6 wt.% and the other polypropylene polymer has a xylene solubles content less than 4 wt.%.

5. 10. The polypropylene polymer composition of claim 1, wherein the first polypropylene polymer is present in the polymer composition in an amount less than 66% by weight and greater than 30%.

6. 10. The polypropylene polymer composition of claim 1, wherein the composition contains a nucleating agent.

7. 10. The polypropylene polymer composition of claim 1, wherein said composition does not contain a nucleating agent.

8. 2. The polypropylene polymer composition of claim 1, wherein said polypropylene polymer composition has a melt flow rate of 0.5 g / 10 min to 30 g / 10 min and a xylene solubles content of 3 wt% to 7 wt%.

9. 2. The polypropylene polymer composition of claim 1, wherein said polypropylene polymer composition has a polydispersity index of 5-10.

10. 2. The polypropylene polymer composition of claim 1, wherein the first polypropylene polymer has a polydispersity index from 4 to 5.5 and the second polypropylene polymer has a polydispersity index from 4 to 5.

5.

11. 2. The polypropylene polymer composition of claim 1, wherein a weight ratio between said first polypropylene polymer and said second polypropylene polymer is from 5:95 to 80:

20.

12. 10. The polypropylene polymer composition of claim 1, wherein the first polypropylene polymer and the second polypropylene polymer both comprise non-phthalate Ziegler-Natta catalyzed polypropylene polymers.

13. 10. The polypropylene polymer composition of claim 1, wherein said polypropylene polymer composition has a flexural modulus of 1,500 MPa to 2,500 MPa.

14. 10. The polypropylene polymer composition of claim 1, wherein said polypropylene polymer composition has a melt flow rate of from 0.5 g / 10 min to 3 g / 10 min.

15. 15. The polypropylene polymer composition of claim 14, wherein said composition has a xylene solubles content of from 3.5% to 7% by weight.

16. 10. The polypropylene polymer composition of claim 1, wherein said polypropylene composition has a melt flow rate of from 5 g / 10 min to 30 g / 10 min.

17. 10. The polypropylene polymer composition of claim 1, wherein said polypropylene polymer composition has an IZOD impact resistance greater than 40 J / m and less than 90 J / m.

18. 1. A method for producing a polypropylene polymer composition, the method comprising polymerizing propylene monomers in the presence of a non-phthalate Ziegler-Natta catalyst to form the polypropylene polymer composition; the polypropylene polymer composition comprises a first polypropylene polymer in combination with a second polypropylene polymer, the first polypropylene polymer having a melt flow rate of 0.1 g / 10 min to 3 g / 10 min and a xylene solubles content of 1.0 wt % to 7 wt %, and the second polypropylene polymer having a melt flow rate of 5 g / 10 min to 100 g / 10 min and a xylene solubles content of 1 wt % to 7 wt %, The polypropylene polymer composition has a flexural modulus according to the following formula: FX≧2072*XS -0.18 wherein FX is the flexural modulus, XS is the xylene solubles content of the polypropylene polymer composition, the xylene solubles content of the polypropylene polymer composition being from 2.5% to 7% by weight; The melt flow rate is measured according to ASTM D 1238 test method at 230° C. using a 2.16 kg weight of the propyne-based polymer; and Flexural modulus is determined according to ASTM 3641 and using type 1 specimens molded according to ASTM D4101, according to ASTM D790-10 Method A at 1.3 mm / min; method.

19. 20. The method of claim 18, wherein the first polypropylene polymer and the second polypropylene polymer are each formed in a gas phase reactor.

20. 20. The method of claim 18, wherein the first polypropylene polymer and the second polypropylene polymer are each formed in a bulk phase reactor.

21. 20. The method of claim 18, wherein one of the first polypropylene polymer and the second polypropylene polymer is formed in a gas phase reactor and the other of the first polypropylene polymer and the second polypropylene polymer is formed in a bulk phase reactor.

22. 22. The method of claim 21, wherein the first polypropylene polymer is formed in a bulk phase reactor and the second polypropylene polymer is formed in a gas phase reactor.

23. 20. The method of claim 18, wherein each of the first polypropylene polymer and the second polypropylene polymer are formed in a separate reactor and then combined together.

24. 20. The method of claim 18, wherein the first polypropylene polymer and the second polypropylene polymer are formed sequentially in a series of reactors.

Citation Information

Patent Citations

  • Polypropylene-based resin composition for oriented film and the resultant oriented film

    JP2002294010A

  • Impact resistant polyolefin composition

    JP2003509562A

  • Blow molded article based on a bimodal random copolymer

    JP2016535802A

  • Polypropylene-based resin composition

    JP2018135419A

  • Electron donors for polyolefin polymerization catalysts and their use