Method for manufacturing a composite structure comprising a thin layer made of monocrystalline SiC on a carrier substrate made of SiC
The method addresses the challenges of bonding c-SiC on p-SiC substrates by using epitaxial growth, implantation, and controlled CVD to create a high-quality composite structure with improved conductivity and reduced defects, facilitating reliable vertical power components.
Patent Information
- Application Number
- JP2022554256
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-27
- Filing Date
- 2021-01-12
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-01-12
AI Technical Summary
Existing methods for producing composite structures with monocrystalline silicon carbide (c-SiC) thin layers on polycrystalline SiC substrates face challenges such as high cost, complexity, and poor quality due to difficulties in bonding and the formation of amorphous layers, which affect vertical electrical conduction and component reliability.
A method involving epitaxial growth of a donor layer with reduced crystal defects, implantation of light entities to create a buried brittle plane, and successive chemical vapor deposition of carrier layers at controlled temperatures to form a high-quality composite structure with a conductive interface, followed by mechanical and chemical treatments to refine the surface and thickness.
The method produces a high-quality composite structure with improved electrical conductivity and reduced defect density, enabling the fabrication of reliable vertical power components with enhanced performance and reduced manufacturing costs.
Smart Images

Figure 0007568736000001 
Figure 0007568736000002 
Figure 0007568736000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of semiconductor materials for microelectronic components. In particular, the present invention relates to a method for manufacturing a composite structure comprising a thin layer made of monocrystalline silicon carbide on a carrier substrate made of silicon carbide. [Background technology]
[0002] Interest in silicon carbide (SiC) has grown significantly in recent years due to the increased ability of this semiconducting material to process energy. SiC is being used more and more extensively to manufacture innovative power devices that meet the needs of rising sectors in electronics, especially electric vehicles.
[0003] Power devices and integrated power supply systems based on monocrystalline silicon carbide can manage much higher power densities and can do so with smaller active zone dimensions compared to conventional power devices and integrated power supply systems made of silicon. To further limit the dimensions of power devices on SiC, it is advantageous to manufacture vertical components instead of lateral ones. To do so, the SiC structure must allow vertical electrical conduction between electrodes arranged on the front and back sides of the SiC structure.
[0004] However, single-crystal SiC substrates intended for the microelectronics industry are still expensive and difficult to supply in large sizes. It is therefore advantageous to use thin layer transfer solutions to prepare composite structures, typically comprising a thin layer made of single-crystal SiC, on a lower-cost carrier substrate. One well-known thin layer transfer solution is the Smart Cut™ process, based on the implantation of light ions and on assembly by direct bonding. With such a process it is possible to produce composite structures, for example comprising a thin layer made of single-crystal SiC (c-SiC), taken from a donor substrate made of c-SiC, in direct contact with a carrier substrate made of polycrystalline SiC (p-SiC), allowing electrical conduction in the vertical direction. However, producing a good quality direct bond by molecular adhesion between two c-SiC and p-SiC substrates remains difficult due to the complex control of the surface condition and roughness of said substrates.
[0005] Various methods derived from this process are also known from the prior art. For example, F. Mu et al. (ECS Transactions, 86(5), 3-21, 2018) use direct bonding after activating the surfaces to be assembled by bombardment with argon (SAB: "Surface Activation Bonding"), such a treatment prior to bonding creates a very high density of side bonds that promotes the formation of covalent bonds at the assembly interface and thus high bond energy. However, this method has the drawback of creating an amorphous layer on the surface of the donor substrate made of monocrystalline SiC, which has an unfavorable effect on the vertical electrical conduction between the thin layer made of c-SiC and the carrier substrate made of p-SiC.
[0006] Solutions have been proposed to solve this problem, notably in document EP 3 168 862, which uses the implantation of dopant entities into the amorphous layer in order to restore its electrical properties. The main drawback of this approach is its complexity and therefore its cost.
[0007] Furthermore, document US Pat. No. 8,436,363 is known, which describes a method for producing a composite structure with a thin layer made of c-SiC arranged on a metal carrier substrate, the thermal expansion coefficient of the composite structure matching that of the thin layer. This production method comprises: forming a buried brittle plane in a c-SiC donor substrate, the buried brittle plane defining a thin layer between the buried brittle plane and a front surface of the donor substrate; - depositing a metal layer, for example made of tungsten or molybdenum, on the front surface of the donor substrate to form a carrier substrate having a sufficient thickness to act as a reinforcement; Separation along the embedded brittle plane in order to form, on the one hand, a composite structure comprising a metal carrier substrate and a thin layer made of c-SiC, and, on the other hand, the remaining part of the donor substrate made of c-SiC. Includes.
[0008] However, such a manufacturing method is not compatible when the material forming the carrier substrate is p-SiC and requires deposition at temperatures above 1200° C. (the usual temperature for manufacturing p-SiC). In particular, at these high temperatures, the growth kinetics of the cavities present in the embedded brittle planes is faster than that of the layer made of p-SiC, and the thickness required for the reinforcement effect is not reached until the appearance of a blistering phenomenon associated with the deformation of the layer directly above the cavities.
[0009] Whatever the layer transfer technique used, the problem of providing a composite structure comprising a thin layer made of c-SiC of very high quality is additionally posed, in particular one free of extended defects (or exhibiting a very low density of defects), which are a cause of affecting the performance quality and reliability of the power devices intended to be prepared on said thin layer. Summary of the Invention
[0010] The present invention relates to an alternative solution to the prior art solutions, aiming at overcoming the above mentioned drawbacks completely or partially.The present invention relates in particular to a method for manufacturing a composite structure comprising a thin layer made of high quality c-SiC arranged on a carrier substrate made of polycrystalline SiC.
[0011] The present invention relates to a method for manufacturing a composite structure comprising a thin layer made of monocrystalline silicon carbide arranged on a carrier substrate made of silicon carbide, the method comprising the steps of: a) providing a donor substrate made of monocrystalline silicon carbide, the donor substrate comprising a donor layer produced by epitaxial growth on an initial substrate, the donor layer exhibiting a density of crystal defects lower than the density of crystal defects of the initial substrate; b) ion-implanting light entities into the donor layer to form a buried brittle plane, the buried brittle plane defining a thin layer between said buried brittle plane and a free surface of the donor layer; c) n successive steps for forming a plurality of carrier layers, n being 2 or more, the n carrier layers being disposed one after the other on the donor layer to form a carrier substrate, each forming step comprising chemical vapor deposition at a temperature between 400° C. and 1100° C. to form a carrier layer made of polycrystalline silicon carbide, the n successive steps comprising chemical vapor deposition at n different temperatures; d) forming, on the one hand, a composite structure comprising the thin layer on the carrier substrate and, on the other hand, a separation along the embedded brittle plane in order to form the remaining part of the donor substrate; e) subjecting the composite structure to (one or more) mechanical and / or chemical treatments in order to smooth the free surfaces of the thin layers and / or to modify the thickness uniformity of the composite structure; Includes.
[0012] According to other advantageous non-limiting features of the present invention taken alone or in any technically attainable combination, The deposition of step c) is carried out at a temperature between 600° C. and 900° C., more preferably between 700° C. and 800° C., The deposition of step c) is based on an atmospheric pressure chemical vapor deposition technique, a low pressure chemical vapor deposition technique or a plasma enhanced chemical vapor deposition technique, n depositions of step c) are carried out at n increasing temperatures; n depositions of step c) are carried out at n decreasing temperatures, At least two of the n carrier layers deposited in step c) exhibit different doping levels, As a result of the deposition of step c), the carrier substrate exhibits a thickness of 50 microns or more, exhibits a thickness of 100 microns or more, and even exhibits a thickness of 200 microns or more, step a) comprises forming a monocrystalline conversion layer on the initial substrate prior to epitaxial growth of the donor layer in order to convert basal plane dislocation type defects of the initial substrate into threading edge dislocation type defects; In step a), epitaxial growth of the donor layer is carried out at a temperature higher than 1200° C., preferably between 1500° C. and 1650° C., In step c), at least one of the n steps for forming the plurality of carrier layers includes an annealing step performed after the chemical vapor deposition of that step, the temperature of the annealing being higher than the deposition temperature and lower than the separation temperature that results in the achievement of the separation of step d); Between steps c) and d), the free surface of the carrier substrate is subjected to chemical etching, mechanical lapping and / or chemical-mechanical polishing, After the detachment of step d), a new chemical vapor deposition is carried out to thicken the carrier substrate, Step e) includes simultaneously chemically mechanically polishing the front and back surfaces of the composite structure; The manufacturing method includes a step of recovering the remaining portion of the donor substrate for reuse as an initial substrate or as a donor substrate.
[0013] Other features and advantages of the present invention will become apparent from the following detailed description of the invention, which proceeds with reference to the accompanying drawings. [Brief description of the drawings]
[0014] [Figure 1] 1 shows a composite structure prepared according to a manufacturing method according to the invention; [Figure 2a] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2b] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2c(i)] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2c(ii)] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2c(iii)] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2d] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2e] 1 illustrates steps of a manufacturing method according to the invention; [Figure 2f] 1 illustrates steps of a manufacturing method according to the invention; [Figure 3a] 1 illustrates steps of a manufacturing method according to the invention; [Figure 3b] 1 illustrates steps of a manufacturing method according to the invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In the description, the same reference numbers of the figures may be used for the same types of elements. The figures are schematic and not to scale for ease of reading. In particular, the thickness of layers along the z-axis is not to scale relative to the lateral dimensions along the x- and y-axes, nor are the relative thicknesses of layers with respect to each other necessarily to scale in the figures.
[0016] The invention relates to a method for manufacturing a composite structure 1 (FIG. 1) comprising a thin layer 10 made of monocrystalline silicon carbide arranged on a carrier substrate 20 made of silicon carbide, which is advantageously polycrystalline (hereinafter, polycrystalline SiC will be referred to using "p-SiC").
[0017] The method first comprises the step a) of providing a donor substrate 111 made of monocrystalline silicon carbide. In the following description, "c-SiC" is used to refer to monocrystalline silicon carbide.
[0018] The donor substrate 111 comprises an initial substrate 11 made of c-SiC (Fig. 2a). The initial substrate 11 is preferably provided in the form of a wafer with a diameter of 100 mm, 150 mm, 200 mm, indeed even 300 mm or even 450 mm, and a typical thickness between 300 and 800 microns. Fig. 2a shows the front side 11a and the back side 11b. The surface roughness of the front side 11a is advantageously chosen to be less than 1 nm Ra (average roughness), measured by atomic force microscopy (AFM) on a scan of 20 microns x 20 microns.
[0019] The donor substrate 111 also comprises a donor layer 110 made of c-SiC, produced by epitaxial growth, on the initial substrate 11. The epitaxial growth step is performed such that the donor layer 110 exhibits a lower density of crystal defects than the density of crystal defects of the initial substrate 11.
[0020] As an example, the initial substrate 11 made of c-SiC exhibits an offcut angle of less than 4.0°±0.5° with respect to the <11-20> crystal axis and has a lattice constant of 5 / cm 2Below, in fact, even 1 / cm 2 The initial substrate 11 is of 4H or 6H polytype, exhibiting a density of threading dislocations (micropipes) of less than 0.015 ohm cm. Doped N (nitrogen) type, the initial substrate 11 exhibits a resistivity preferably between 0.015 ohm cm and 0.030 ohm cm. A low density of basal plane dislocations, i.e. BPD type defects, typically 3000 / cm. 2 An initial substrate 11 can be chosen that exhibits a defect density of 1500 / cm 2 c-SiC substrates exhibiting a BPD density of about 100 nm are reasonably available, which may facilitate the supply of c-SiC substrates.
[0021] In the case of the donor layer 110 from which the thin layer 10 made of c-SiC of the composite structure 1 is to be formed as a result of the method that is the subject of the present invention, it is desirable to exhibit a crystalline quality superior to that of the initial substrate 11 in order to meet the specifications required for the vertical components intended to be prepared on said thin layer 10. This is due to the presence of various types of extended defects in the layer or substrate made of c-SiC. These extended defects can affect the performance quality and reliability of the components. In particular, in the case of bipolar components, defects of the BPD type are fatal, especially Shockley stacking faults (SSFs), which are extended from dislocations when energy is available to recombine electron-hole pairs. The extension of SSF stacking faults inside the active area of the component leads to an increase in the pass-state resistance of the component.
[0022] Therefore, the donor layer made of c-SiC has a density of 1 / cm 2 It is prepared to show the density of defects for the following BPD types:
[0023] For that purpose, the epitaxial growth of the donor layer 110 is carried out at a temperature higher than 1200° C., preferably between 1500° C. and 1650° C. The precursors used are silane (SiH4), propane (C3H8) or ethylene (C2H4), and the carrier gas may be hydrogen with or without argon.
[0024] The donor layer 110 with a low content of BPD defects is obtained by supporting the conversion of BPD defects present in the initial substrate 11 into threading edge dislocations (TEDs).
[0025] According to a particular embodiment, step a) comprises the formation of a monocrystalline conversion layer 13, preferably made of c-SiC, on the initial substrate 11 prior to the growth of the donor layer 110. The purpose of the conversion layer 13 is to maximize the conversion of the BPD type defects of the initial substrate 11 into TED type defects (FIG. 3a). To that end, it is advantageous to choose a small cleavage angle close to 4° for the initial substrate 11 made of c-SiC in order to achieve a fast growth rate (typically higher than 5 μm / h), a high in situ etching carried out before the epitaxial growth, and finally to choose growth conditions for the monocrystalline conversion layer 13 with a C / Si ratio in the precursor stream close to 1.
[0026] The epitaxial growth of a donor layer 110 on the conversion layer 13 can then be carried out (FIG. 3b). According to this particular embodiment, the 1 / cm 2 In fact, even less than 0.1 / cm 2 It is also possible to obtain a donor layer 110 made of c-SiC that exhibits a density of BPD type defects below 100 nm. Furthermore, as a result of the method according to the invention, the probability of bipolar degradation (probability of holes arriving below the BPD / TED conversion point) is negligible (less than 0.1%) and the monocrystalline conversion layer 13 is not intended to be transferred to the composite structure 1. Prior art aimed at reducing the bipolar degradation involves the incorporation of a recombination layer (1 E 18at / cm 3 This layer has a thickness of 10 μm and a thickness of 5 E 18 / cm 3In exchange for a concentration above 0.1%, the probability of holes being present can be reduced to 0.1% relative to the basic structure without this recombination layer. Since the monocrystalline conversion layer 13 is not transferred in the present invention, the probability of holes reaching the nucleation point of bipolar degradation (BPD-TED conversion point or any BPD point) is at a minimum less than 0.1%, and in practice even close to 0%.
[0027] It should be noted that a conventional cleaning or etching sequence of the initial substrate 11 aimed at removing all or part of any particulates, metallic or organic contaminants or native oxide layer potentially present on the front surface 11a of the initial substrate 11 can be carried out prior to the epitaxial growth.
[0028] The manufacturing method according to the invention further comprises a step b) of ion-implanting light entities into the donor layer 110 to a predetermined depth representing the desired thickness of the thin layer 10. It should be noted that this depth will always be kept below the thickness of the donor layer 110. This implantation produces a buried brittle plane 12 in the donor layer 110, which delimits the thin layer 10 between said buried brittle plane 12 and the free surface 11a of said donor layer 110 (Figure 2b).
[0029] The light entities implanted are preferably hydrogen, helium or a co-implantation of these two entities. As is well known with reference to the Smart-Cut™ process, these light entities will form microcavities distributed at approximately a predefined depth in a thin layer parallel to the free surface 11a of the donor layer 110, i.e. parallel to the (x,y) plane of the figure. This thin layer will be referred to for simplicity as the embedded brittle plane 12.
[0030] The energy for implanting the light entities is selected to reach a determined depth in the donor substrate 111. Typically, hydrogen ions are implanted at energies between 10 keV and 250 keV for 5 min to define a thin layer 10 exhibiting a thickness of the order of 100-1500 nm.E 16 / cm 2 and 1 E 17 / cm 2 The implantation is carried out at a dose between 0.01 and 0.1.
[0031] It should be noted that prior to the ion implantation step, a protective layer can be deposited on the free surface 11a of the donor layer 110. This protective layer can consist of a material such as, for example, silicon oxide or silicon nitride.
[0032] The method according to the invention subsequently comprises n successive steps for forming a plurality of carrier layers 20', where n is greater than or equal to 2 and advantageously greater than or equal to 3. The n carrier layers 20' are arranged one after the other on the free surface 11a of the donor layer 110 to form the carrier substrate 20. In other words, a first carrier layer 20' is in direct contact with the front surface 11a of the donor layer 110, then a second carrier layer 20' is in contact with the first carrier layer 20' and so on for the n carrier layers 20' until the carrier substrate 20 is obtained (Figures 2c(i), 2c(ii), 2c(iii)).
[0033] The individual forming steps include chemical vapor deposition (CVD) to form a carrier layer 20' made of polycrystalline silicon carbide.
[0034] The individual CVD depositions are carried out at temperatures between 400° C. and 1100° C., preferably between 600° C. and 900° C., and in practice even more advantageously between 700° C. and 800° C. The deposition of step c) is advantageously based on the atmospheric pressure chemical vapour deposition (APCVD) technique, the low pressure chemical vapour deposition (LPCVD) technique or the plasma enhanced chemical vapour deposition (PECVD) technique.
[0035] According to the invention, the n depositions of step c) are carried out at n different temperatures, which makes it possible to improve the quality of the carrier substrate 20 obtained by the superposition of n carrier layers 20', as will be explained below with reference to two embodiments.
[0036] Preferably, the individual carrier layers 20' exhibit a thickness of less than 150 microns, less than 100 microns, and indeed even less than 50 microns.
[0037] According to a first embodiment, the n depositions of step c) are carried out at n increasing temperatures. As an example, four successive depositions can be carried out at temperatures ranging from 700° C. to 1000° C. It is noted that the thickness of the carrier layer 20′ deposited during successive depositions can be exactly the same or different.
[0038] This embodiment has the advantage of limiting the thermal history applied to the donor substrate 111 at the start of the formation of the carrier layer 20', i.e. at a time when the reinforcing effect of these layers is not high, thus significantly reducing the risk of damage to the donor layer 110 due to blisters caused by the growth of cavities in the embedded brittle plane 12.
[0039] Furthermore, even if the crystalline quality of the deposited first carrier layer 20' decreases (as a result of a lower deposition temperature), the crystalline quality can be restored (at least in part) by a subsequent deposition carried out at an elevated temperature and / or the crystallinity of the first deposition(s) can be improved.
[0040] The maximum temperature, i.e. the temperature applied during the last deposition n, is preferably less than the temperature that will be applied in the subsequent step d) for performing the separation.
[0041] According to a second embodiment, the n depositions of step c) are carried out at n descending temperatures. By way of example, between 3 and 5 successive depositions can be carried out at temperatures ranging from 1000° C. to 700° C.
[0042] Advantageously, the maximum temperature, ie the temperature applied during the first deposition, is less than the temperature that will be applied in the subsequent step d) for carrying out the separation.
[0043] The aim of this second embodiment is to form a first carrier layer 20' on a donor layer 110 of very good crystalline quality and to improve the electrical conductivity of the interface between these two layers. The quality of the subsequent carrier layer 20' will potentially be poorer (in view of the lower deposition temperature), but the lower deposition temperature can limit the growth of cavities in the embedded brittle plane 12 until the desired thickness of the carrier substrate 20 is reached. It can also be considered that the carrier layer 20' deposited at a lower temperature generates lower thermomechanical stresses during cooling to ambient temperature.
[0044] Optionally, in any one of the described embodiments, at least one of the n steps for forming the carrier layers 20′ comprises an annealing step carried out after the chemical vapor deposition. The annealing temperature is advantageously selected to be higher than the deposition temperature but lower than the separation temperature to be applied during the subsequent step d) of separation along the embedded brittle plane 12.
[0045] Generally, regardless of which embodiment is adopted, the thermal budget applied to the stack 211 during any one of the n steps of forming the carrier layer 20' is less than the thermal budget that would result in the growth of cavities in the embedded brittle plane 12, which would deform the thin layer 10 and the n carrier layer(s) 20' formed thereon.
[0046] Furthermore, the total thermal budget applied to the stack 211 during the n steps for forming the plurality of carrier layers 20 ′ remains less than the thermal budget that would result in spontaneous separation along the embedded brittle planes 12 .
[0047] Step c) of the method advantageously defines a non-insulating interface between the donor layer 110 and the first carrier layer 20′ deposited during the first CVD deposition. In other words, step c) is performed such that, at least in the final composite structure 1, the interface between the donor layer 110 and the first carrier layer 20′ is capable of forming a conductive interface, e.g. typically below 1 milliohm cm 2 A specific interface resistance of less than 100 nm is to be targeted. To ensure electrical conductivity at the interface, removal of the native oxide present on the free surface 11 a of the donor layer 110 is advantageously carried out by HF (hydrofluoric acid) deoxidation, either by wet or dry route.
[0048] Prior to deoxidation and / or prior to formation of the first carrier layer 20′, the donor substrate 111 may be subjected to a cleaning sequence to remove all or part of any particulate, metallic or organic contaminants potentially present on the free surface of the donor substrate 111.
[0049] To further improve the electrical conductivity at the interface with the donor substrate 111, it is advantageous for the deposited carrier layer 20' to exhibit a high doping level during the first CVD deposition. Typically, the deposited first carrier layer 20' has a doping level of 1 E 14 / cm 3 and 1 E 22 / cm 3 , n) or p) may exhibit a concentration of N-type or P-type dopant between them. Subsequent carrier layers 20' that are deposited may exhibit different concentrations and / or different types of dopants. Thus, at least two carrier layers 20' of the n carrier layers 20' deposited in step c) may exhibit entirely different doping levels.
[0050] The deposition parameters of step c) are such that said carrier substrate 20 exhibits good electrical conductivity, i.e. less than 0.03 ohm cm, in fact even less than 0.01 ohm cm, and high thermal conductivity, i.e. less than 150 W.m -1 .K -1 Above, in fact even 200W.m -1 .K -1or greater and has a thermal expansion coefficient similar to that of the thin layer 10, i.e., typically 3.8 at ambient temperature. E -6 / K and 4.2 E It is advantageously determined to exhibit a thermal expansion coefficient between 0.1 and 0.2 kPa (-6 / K). To obtain these properties, the carrier substrate 20 preferably exhibits the following structural features: polycrystalline structure, grains of 3C SiC type, 111 orientation, average size in the plane of the substrate between 1 and 50 μm, and N-type doping for a final resistivity of less than or equal to 0.03 ohm cm.
[0051] As a result of step c), the carrier substrate 20 exhibits a thickness of 10 microns or more, exhibits a thickness of 50 microns or more, exhibits a thickness of 100 microns or more, indeed even exhibits a thickness of 200 microns or more. The stack 211 obtained by step c) comprises the carrier substrate 20 arranged on the donor substrate 111.
[0052] The method according to the invention subsequently comprises a step d) of separation along the embedded brittle plane 12 in order to form, on the one hand, the composite structure 1 and, on the other hand, the remaining part 111' of the donor substrate (FIG. 2d).
[0053] According to an advantageous embodiment, the separation step d) is carried out by subjecting the stack 211 to a heat treatment at a separation temperature higher than the temperature of the deposition and the annealing (if performed) of step c), as the microcavities present in the buried brittle plane 12 follow a growth kinetics until a breaking wave is generated that propagates over the entire extent of the buried brittle plane 12, resulting in a separation between the composite structure 1 and the remainder of the initial substrate 111'. In practice, the temperature may be between 950°C and 1200°C, preferably between 1000°C and 1200°C, as a function of the implantation conditions of step b).
[0054] According to an alternative embodiment, the separation step d) is performed by applying a mechanical stress to the stack 211. The stress can for example be applied by inserting a tool (for example in the form of a blade or bevel) close to the embedded weak plane 12. By way of example, the separation stress can be of the order of a few GPa, preferably more than 2 GPa.
[0055] It should be noted that it is optionally possible to plan to carry out at least one new CVD deposition after the separation in step d) in order to thicken the carrier substrate 20 further.
[0056] After step d), a composite structure 1 is obtained comprising a thin layer 10 made of monocrystalline silicon carbide arranged on a carrier substrate 20 made of polycrystalline silicon carbide.
[0057] As can be seen, as a result of the separation step d), the free surface 10a of the thin layer 10 of the composite structure 1 exhibits a surface roughness of between 5 nm RMS and 100 nm RMS (measured by atomic force microscope (AFM) with a scan of 20 microns x 20 microns).
[0058] Step e) of subjecting the composite structure 1 to (one or more) mechanical and / or chemical treatments is therefore provided in order to smooth the free surface 10a of the thin layer 10 and / or to modify the thickness uniformity of said structure 1 (Figure 2e).
[0059] Step e) may include a chemical mechanical polishing (CMP) of the free surface 10a of the thin layer 10, typically removing around 50 nm to 1000 nm of material to obtain a final roughness of less than 0.5 nm RMS (with an AFM field of view of 20x20 μm), in practice even less than 0.3 nm. Step e) may also include a chemical or plasma (cleaning or etching) treatment to further improve the quality of the free surface 10a of the thin layer 10, for example cleaning of SC1 / SC2 (standard cleaning 1, standard cleaning 2) and / or HF (hydrofluoric acid) type, or N2, Ar, CF4, etc., plasmas.
[0060] Furthermore, step e) may comprise a chemical mechanical polishing (CMP) and / or a chemical (etching or cleaning) and / or a mechanical (grinding) treatment of the back surface 20b of the carrier substrate 20. Such treatments may improve the thickness uniformity of the carrier substrate 20 and also the roughness of the back surface 20b of the carrier substrate 20. A roughness of less than 0.5 nm RMS (measured by atomic force microscope (AFM) in a field of view of 20 microns x 20 microns) is desirable for preparing vertical components, where at least one metal electrode will be present on the back surface 20b of the composite substrate 1.
[0061] It should be noted that these treatments applied to the back surface 20b of the carrier substrate 20 can also be optionally carried out just before the separation step d), i.e. before the front surface 10a of the composite structure 1 is exposed, thereby making it possible to limit contamination of the front surface 10a, in particular during contamination or limiting processes such as chemical etching or mechanical lapping (or mechanical grinding).
[0062] Polishing or grinding of the edges of the composite structure 1 can also be carried out during this step e) in order to make the shape of the circular profile of the composite structure 1 and the shape of the edge waste compatible with the requirements of the microelectronic manufacturing process.
[0063] According to an advantageous embodiment, step e) of chemical mechanical processing comprises simultaneous polishing (CMP) of the front surface 10a and the back surface 20b of the composite structure 1 in order to smooth the thickness of said structure 1 and improve the thickness uniformity. The polishing parameters may be different between the front surface 10a and the back surface 20b. Different consumables are usually required for the smoothing of c-SiC and p-SiC surfaces. If the carrier substrate 20 is made of p-SiC, the mechanical component of polishing is preferred, especially for the back surface 20b, in order to limit the preferential attack of the grain boundaries by the chemical component of polishing. As an example, the polishing parameters such as the rotation speed (plate and polishing head), pressure, concentration and physical properties of the abrasive (i.e. the diameter of diamond nanoparticles between approximately 10 nm and 1 μm) can be modified to enhance the effect of the mechanical component.
[0064] According to a further advantageous embodiment, step e) is followed by a step e') of heat treatment at a temperature between 1000° C. and 1800° C. for approximately one hour and up to several hours. The purpose of this step is to stabilize the composite structure 1 by repairing structural or surface defects still present in and / or on the thin layer 10 and, if appropriate, by changing the crystalline configuration of the carrier substrate 20, so that the structure 1 is compatible with the subsequent high-temperature heat treatments necessary for the manufacture of components on the thin layer 10.
[0065] The method according to the invention can include a step f) of epitaxially growing an additional layer 10' of monocrystalline silicon carbide on the thin layer 10 of the composite structure 1 (Fig. 2f). Such a step is applied when a relatively thick working layer 100 is required to manufacture the component, typically with a thickness of the order of 5-50 microns. The epitaxy conditions can be optionally selected in the same way as the epitaxy conditions of step a), with epitaxy at a lower temperature being preferred in order to limit the stresses induced in the working layer 100 (corresponding to the assembly of the thin layer 10 and the additional layer 10') as a result of the heterogeneous material of the composite structure 1.
[0066] Finally, the manufacturing method may include a step of regenerating the remaining part 111' of the donor substrate for reuse as the initial substrate 11 or as the donor substrate 111. Such a regeneration step is based on one or more treatments of the face 110' (FIG. 2d) by chemical-mechanical polishing of the surface or edge, and / or mechanical grinding, and / or dry or wet chemical etching. The thickness of the donor layer 110 formed in step a) is preferably defined so that the remaining part 111' of the donor substrate 111 can be reused at least twice as the donor substrate 111. If a conversion layer 13 is present, care must be taken to keep said layer intact, i.e. a part of the donor layer 10 is preferably always kept on top of the remaining part 111' of the donor substrate. Thus, if that part of the donor layer 10 is insufficient for preparing the composite structure 1, only the step of epitaxially growing the donor layer 10 is necessary, without the preceding step of growing the conversion layer 13.
[0067] (Example) According to a non-limiting exemplary embodiment, the initial substrate 11 is a wafer of c-SiC of the 4H polytype, oriented at 4.0°±0.5° relative to the <11-20> axis, with a diameter of 150 mm and a thickness of 350 μm.
[0068] Prior to the epitaxial growth of a donor layer 110 made of c-SiC, the initial substrate 11 is subjected to a conventional cleaning sequence of the RCA type (Standard Clean 1 + Standard Clean 2), then Caro's acid (a mixture of sulfuric acid and hydrogen peroxide), then HF (hydrofluoric acid).
[0069] The growth is carried out in an epitaxy chamber at a temperature of 1650° C. using precursors such as silane (SiH4) and propane (C3H8) or ethylene (C2H4), producing a 30 micron thick donor layer 110 made of c-SiC (growth rate: 10 microns / h). The donor layer has a thickness of 1 / cm 2 The density of BPD defects is shown.
[0070] The energy was 150 keV, and the entire free surface of the donor layer 110 was 6 E 16H + / cm 2 Thus, a buried brittle plane 12 is created at a depth of approximately 800 nm in the donor layer 110.
[0071] To remove potential contaminants on the free surface of the donor layer 110, a RCA+Caro's acid type cleaning sequence is performed on the donor substrate 111.
[0072] To achieve a thickness of 50 microns for the first carrier layer 20', a first LPCVD deposition is performed on the donor layer 110 using a methylsilane (MS) (CH3SiH3) precursor at a temperature of 700° C. and a pressure of 3.7 Torr for 60 minutes. Under these conditions, the support layer 20' is constructed of polycrystalline SiC.
[0073] To achieve a thickness of 100 microns for the second carrier layer 20' made of p-SiC, a second LPCVD deposition is performed on the first carrier layer 20' at a temperature of 800° C. using MS precursors under a pressure of 4 Torr for 30 minutes.
[0074] To achieve a thickness of 250 microns for the third carrier layer 20' made of p-SiC, a third LPCVD deposition is performed on the second carrier layer 20' at a temperature of 850° C. using MS precursors under a pressure of 4 Torr for 45 minutes.
[0075] The carrier substrate 20 formed by the superposition of three carrier layers 20' exhibits a thickness of 400 microns.
[0076] Subsequently, the stack 211 formed by the donor substrate 111 and the carrier substrate 20 is subjected to an anneal at 1000° C. for 50 minutes. During said anneal, separation is carried out at the level of the embedded brittle plane 12. As a result of this separation step d), the composite structure 1 formed by the thin layer 10 and the carrier substrate 20 is separated from the remaining part 111′ of the donor substrate.
[0077] A thickness of about 50 microns is removed on the back surface 20b of the carrier substrate 20. Then, double-side polishing is performed to restore the surface roughness of the thin layer 10 and the surface roughness of the back surface 20b of the carrier substrate 20.
[0078] Naturally, the invention is not limited to the embodiments and to the examples described, and alternative embodiments can be introduced therein without departing from the scope of the invention as defined by the claims.
Claims
1. A method for manufacturing a composite structure (1) comprising a thin layer (10) made of monocrystalline silicon carbide arranged on a carrier substrate (20) made of silicon carbide, comprising: a) providing a donor substrate (111) made of monocrystalline silicon carbide, said donor substrate (111) comprising a donor layer (110) produced by epitaxial growth on an initial substrate (11), said donor layer (110) exhibiting a lower crystal defect density than the crystal defect density of said initial substrate (11); b) ion implantation of light entities into said donor layer (110) to form a buried brittle plane (12) that defines the thin layer (10) between said buried brittle plane (12) and a free surface of said donor layer (110); c) n successive steps for forming a plurality of carrier layers (20'), n being 2 or more, the n carrier layers (20') being arranged one after the other on the donor layer (110) to form the carrier substrate (20), each forming step comprising a chemical vapor deposition at a temperature between 400° C. and 1100° C., the n chemical vapor depositions being carried out at n different temperatures to form a carrier layer (20') made of polycrystalline silicon carbide; d) forming, on the one hand, a composite structure (1) comprising said thin layer (10) on said carrier substrate (20) and, on the other hand, a separation along said embedded brittle plane (12) in order to form the remaining part (111') of the donor substrate; e) subjecting said composite structure (1) to (one or more) mechanical and / or chemical treatments in order to smooth the free surface (10a) of said thin layer (10) and / or to modify the thickness uniformity of said composite structure (1); The method includes:
2. 2. A method according to claim 1, wherein said deposition of step c) is carried out at a temperature between 600°C and 900°C, more preferably between 700°C and 800°C.
3. The method according to claim 1 or 2, wherein said deposition in step c) is based on an atmospheric pressure chemical vapor deposition technique, a low pressure chemical vapor deposition technique or a plasma enhanced chemical vapor deposition technique.
4. Method according to any one of claims 1 to 3, wherein said n depositions of step c) are carried out at n increasing temperatures.
5. Method according to any one of claims 1 to 3, wherein said n depositions of step c) are carried out at n descending temperatures.
6. Method according to any one of the preceding claims, wherein at least two carrier layers (20') of the n carrier layers (20') deposited in step c) exhibit different doping levels.
7. The method according to any one of the preceding claims, wherein as a result of said deposition of step c), said carrier substrate (20) exhibits a thickness of 50 microns or more, exhibits a thickness of 100 microns or more, indeed even exhibits a thickness of 200 microns or more.
8. The method according to any one of claims 1 to 7, wherein step a) comprises forming a monocrystalline conversion layer (13) on the initial substrate (11) prior to the epitaxial growth of the donor layer (110) in order to convert basal plane dislocation type defects of the initial substrate (11) into threading edge dislocation type defects.
9. The method according to any one of the preceding claims, wherein in step a) the epitaxial growth of the donor layer (110) is performed at a temperature higher than 1200°C, preferably between 1500°C and 1650°C.
10. 10. The method according to claim 1, wherein in step c) at least one of the n steps for forming the plurality of carrier layers (20') comprises an annealing step carried out after the chemical vapor deposition of said step, the annealing temperature being higher than the deposition temperature and lower than a separation temperature resulting in the achievement of the separation of step d).
11. The method according to any one of the preceding claims, wherein between steps c) and d) the rear side (20b) of the carrier substrate (20) is subjected to chemical etching, mechanical lapping and / or chemical-mechanical polishing.
12. The method according to any one of the preceding claims, wherein after the detachment in step d) a new chemical vapor deposition is performed to thicken the carrier substrate (20).
13. The method according to any one of the preceding claims, wherein step e) comprises simultaneously chemically mechanically polishing the front (10a) and back (20b) faces of the composite structure (1).
14. The method according to any one of the preceding claims, comprising a step of reclaiming the remaining part (111') of the donor substrate for reuse as an initial substrate (11) or as a donor substrate (111).
Citation Information
Patent Citations
METHOD FOR PRODUCING SiC SUBSTRATE, SiC SUBSTRATE, AND SEMICONDUCTOR DEVICE
JP2007137689A
Manufacturing method of multilayer-structured silicon carbide substrate
JP2007273524A
Metallic carrier for layer transfer and methods for forming the same
JP2012178548A
Method for producing a film on a substrate having a non-planar surface
JP2021501477A
Metallic carrier for layer transfer and methods for forming the same
US20120199845A1