Refining Method
By controlling slag forming behavior through specific concentration adjustments and using a microwave level meter, the refining method stabilizes slag discharge, addressing the challenge of inconsistent slag removal and reducing flux usage in high-purity steel production.
Patent Information
- Application Number
- JP2021000481
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-05
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-01-05
AI Technical Summary
Existing refining methods for high-purity steel production in converter-type containers face challenges in stably discharging a large amount of slag during intermediate slag removal, leading to variations in slag remaining in the furnace, which affects subsequent refining processes and increases flux usage.
A refining method that controls the slag forming behavior by adjusting the Si concentration, CaO and Al2O3 concentrations, and using a microwave level meter to measure the forming height, ensuring the foaming height ratio falls within specific ranges defined by equations (1) or (2) to stabilize slag discharge.
Stable and large-scale slag discharge is achieved, reducing variations in slag remaining in the furnace, thereby improving the efficiency of subsequent refining processes and minimizing flux usage.
Smart Images

Figure 0007568922000003 
Figure 0007568922000004 
Figure 0007568922000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a refining method. [Background technology]
[0002] The refining process of molten pig iron in a converter-type vessel, typified by a converter, is a method in which blast furnace molten pig iron is charged into the converter-type vessel, and the molten pig iron is subjected to desiliconization (Si), dephosphorization (P), and decarburization (C) processes by adding a flux mainly consisting of quicklime and blowing oxygen (acid blowing) to produce steel. In recent years, in order to produce high-purity steel such as low-P steel and to reduce the amount of steelmaking slag generated as a by-product of converter refining, a converter-type vessel refining method (hereinafter abbreviated as converter refining method) in which the desiliconization and dephosphorization processes are separated from the decarbonization process has been used.
[0003] Among the converter refining processes as described above, a widely used converter refining process (the so-called MURC process) is one in which, after de-Si and de-P processes (hereinafter abbreviated as "de-Si / P process"), the molten iron after the process is not discharged outside the converter, but the slag is discharged from the throat by tilting the converter (hereinafter referred to as intermediate slag discharge), and then, continuously, de-C process is performed on the molten iron in the converter.
[0004] The MURC process is characterized by the fact that the blowing process is divided into two processes, the de-Si / P process and the de-C process, with intermediate slag removal in between, which allows the slag composition and blowing conditions to be optimized separately for the de-Si / P process and the de-C process. This makes it possible to produce high-purity steel and reduce the amount of slag generated, compared to the converter refining process (so-called one-blow blowing), which performs the de-Si, de-P, and de-C processes all at once.
[0005] In addition, in the MURC process, the molten metal is not dumped outside the furnace during intermediate draining, but the slag is drained by tilting the furnace body, making it possible to quickly separate the molten metal and slag after treatment. This contributes to improved productivity compared to the converter refining process, in which the molten metal is once dumped outside the furnace after the de-Si / P treatment and then recharged into the converter for the de-C treatment.
[0006] The MURC process utilizes a phenomenon called foaming, in which the slag expands with the CO and CO2 generated by the reaction between the charged oxygen and the carbon in the molten iron by controlling the slag composition and the acid blowing conditions during the de-Si / P treatment to perform intermediate slag removal. The MURC process uses foaming to expand the slag appropriately, and then tilts the converter, making it possible to remove only the slag from the furnace.
[0007] However, if excessive foaming occurs during the Si / P removal process, it will cause slopping, in which slag bubbles up from the furnace throat, resulting in reduced productivity.
[0008] For this reason, various techniques have been disclosed in the past, such as a technique for measuring the foaming height (also called the foaming level) in a converter to prevent slopping, and a method for desiliconizing the slag up to a foaming height where intermediate slag removal is easy.
[0009] For example, the following Patent Document 1 discloses a microwave measuring device for measuring the forming height in a furnace and a measurement method using the measuring device.
[0010] Furthermore, the following Patent Document 2 discloses a molten iron pretreatment method in which desiliconization and dephosphorization of molten iron are carried out continuously using a single converter-type refining furnace, with a slag removal process in between, in which a microwave level meter is used to terminate the desiliconization process at a predetermined height, thereby suppressing the accidental outflow of slag (slopping) during the slag removal process after desiliconization, and quickly removing a targeted, predetermined amount of desiliconized slag from the furnace in a short period of time.
[0011] In addition, the following Patent Document 3 discloses a technique for refining molten pig iron by using a single converter-type refining furnace to continuously perform a primary blowing process and a secondary blowing process with a slag removal process in between, and measuring the foaming height in the primary refining process with a microwave level meter and using the measured height for processing. More specifically, the following Patent Document 3 discloses a method for performing blowing until the foaming height ratio (the ratio of the slag height to the freeboard in the converter) is 0.6 or more, controlling the foaming height by introducing a foaming suppressant when it is 0.6 to less than 0.8, and terminating the primary refining process when the height ratio is 0.5 to 0.7, thereby suppressing the sudden outflow of slag in the primary blowing process and enabling the targeted predetermined amount of slag to be quickly discharged out of the furnace in a short time in the slag removal process after the primary blowing process.
[0012] Furthermore, in the following Patent Document 4, in a method for refining molten pig iron in which a single converter-type refining furnace is used to continuously perform a primary blowing process and a secondary blowing process of molten pig iron with a slag removal process in between, the primary blowing process is terminated when the slag height ratio in the furnace is 0.3 or more and less than 0.6, and then bottom blown gas is maintained for 1 minute or more and 5 minutes or less, and then slag discharge is initiated when the slag height ratio is 0.3 or more and less than 0.6, thereby making it possible to prevent the removed slag from foaming in a slag pot, and thereby to quickly discharge a targeted predetermined amount of slag in the furnace outside the furnace in a short period of time.
[0013] Thus, currently, there are disclosed techniques for monitoring the foaming state in the furnace, techniques for suppressing sudden slag outflow during refining by utilizing the foaming state in the furnace, foaming control techniques, and techniques for quickly discharging slag during intermediate slag discharge. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] JP 2018-87364 A [Patent Document 2] International Publication No. 2014 / 115526 [Patent Document 3] JP 2016-29212 A [Patent Document 4] JP 2017-133060 A Summary of the Invention [Problem to be solved by the invention]
[0015] However, although Patent Document 1 discloses a method for monitoring the forming state in the furnace, it does not disclose any technology for avoiding slopping or for keeping the amount of discharged slag constant.
[0016] Furthermore, the above Patent Documents 2 to 4 disclose techniques for preventing slopping and quickly discharging slag. However, as a result of verification by the present inventors, it was found that when the techniques disclosed in Patent Documents 2 to 4 are used to properly form slag in a furnace with a small amount of slag, it becomes difficult to sufficiently discharge the slag during intermediate slag discharge. This causes problems such as a reduction in the effect of the flux supplied to the molten metal in the refining process after intermediate slag discharge.
[0017] Furthermore, as a result of the inventor's investigation, it has become clear that in the techniques of Patent Documents 2 to 4, the amount of slag remaining in the furnace after intermediate slag removal varies depending on the initial molten iron composition and slag amount in the furnace. If such a phenomenon occurs, the variation in the slag amount causes problems in the refining process after intermediate slag removal. For example, if the refining process after intermediate slag removal is a decarburization process, the amount of rephosphorization during decarburization varies, leading to a situation where excessive use of CaO to suppress the variation in the amount of rephosphorization cannot be suppressed.
[0018] As described above, even if the techniques disclosed in Patent Documents 2 to 4 above are used, there is still room for improvement in terms of stably discharging a large amount of slag during intermediate draining of the slag generated after molten iron pretreatment (desiliconization treatment and dephosphorization treatment) in a converter.
[0019] The present invention has been made in view of the above problems, and an object of the present invention is to provide a refining method capable of stably discharging a large amount of slag during intermediate slag discharge produced after molten iron pretreatment in a converter-type vessel. [Means for solving the problem]
[0020] In order to solve the above problems, the present inventors conducted further studies and discovered that it was necessary to focus on the foaming behavior of slag in a converter-type vessel, leading to the completion of the present invention described below. The gist of the present invention, which was completed based on these findings, is as follows.
[0021] [1] A refining method in a top-blowing refining process for refining steel using a converter-type vessel, comprising the steps of: a first step of charging molten pig iron into the converter-type vessel; a second step of adding a lime-based flux into the converter-type vessel and blowing acid into the converter-type vessel to desiliconize and dephosphorize the molten pig iron and form slag; a third step of performing intermediate slag discharging by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel; and a fourth step of adding flux into the converter-type vessel after the intermediate slag discharging and performing top-blowing refining. and a step of: a Si concentration of the molten iron at the start of the second step is 0.6 mass% or less; and the slag at the time when the acid blowing is stopped in the second step has an Al2O3 concentration of 0.5 mass% or more and 5.0 mass% or less and a basicity obtained by dividing the CaO concentration (unit: mass%) by the SiO2 concentration (unit: mass%) of 0.8 or more and 1.5 or less, and in the second step, a height of the foaming is measured, and the height of the foaming at the time when the acid blowing is stopped before the intermediate slag removal satisfies the following formula (1): 0.6-0.3 × (Si concentration in molten iron at the start of the second process (unit: mass%)) ≦ foaming height ratio at the end of acid blowing Equation (1) Here, in the above formula (1), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel. [2] A refining method in a top blowing refining process for refining steel using a converter-type vessel, comprising the steps of: charging molten pig iron into the converter-type vessel in a first step; adding a lime-based flux into the converter-type vessel and blowing acid therein to subject the molten pig iron to a desiliconization treatment and a dephosphorization treatment, and foaming slag; and mold container a third step of performing intermediate slag discharge by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel; and a fourth step of adding flux into the converter-type vessel after the intermediate slag discharge and performing a top-blowing refining process, wherein the slag at the time when the acid blowing is stopped in the second step has an Al2O3 concentration of 0.5 mass% or more and 5.0 mass% or less and a basicity obtained by dividing the CaO concentration (unit: mass%) by the SiO2 concentration (unit: mass%) of 0.8 or more and 1.5 or less, and the height of the foaming at the time when the acid blowing is stopped before the intermediate slag discharge satisfies the following formula (2): 0.6-0.3 × (Si concentration in molten iron at the start of the second process (unit: mass%)) ≦ foaming height ratio when acid blowing is stopped ≦ 0.8-0.3 × (Si concentration in molten iron at the start of the second process (unit: mass%)) Equation (2) Here, in the above formula (2), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel. [3] The refining method according to [1] or [2], wherein a microwave level meter is used to measure the height of the foam in the second step. [4] The refining method according to any one of [1] to [3], wherein the fourth step is a step of performing decarburization refining, and a portion of the molten slag generated after the decarburization refining is left in the furnace, and the left molten slag is used as a portion or all of the lime-based flux in the second step of the next charge. [5] The refining method according to any one of [1] to [3], wherein the fourth step is a step of performing decarburization refining, and the solidified slag obtained by cooling and solidifying the molten slag generated after the decarburization refining is used as part or all of the lime-based flux in the second step of another charge. Effect of the Invention
[0022] As described above, according to the present invention, when the slag generated after the hot metal pretreatment in the converter-type vessel is discharged in the intermediate slag removal step, it is possible to stably discharge a large amount of slag. Furthermore, since it is possible to stably discharge a large amount of slag during the intermediate slag removal step, it is possible to suppress the variation in the amount of slag remaining in the converter. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is an explanatory diagram showing a schematic flow of a refining method in a top-blowing refining process that is the focus of an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining the tilting angle of a converter-type vessel. [Diagram 3] FIG. 1 is a graph showing the relationship between the molten iron Si concentration and the tilting angle at the start of intermediate slag removal. [Figure 4A] FIG. 2 is an explanatory diagram showing a schematic diagram of a microwave level meter used in the embodiment. [Figure 4B] FIG. 2 is an explanatory diagram showing a schematic diagram of a microwave level meter used in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0025] (About the inventor's investigations and findings) Prior to describing the refining method according to the embodiment of the present invention, the investigations conducted by the present inventors and the findings that led to the conception of the refining method according to the present embodiment will be specifically described with reference to Figs. 1 to 3. Fig. 1 is an explanatory diagram showing a flow of a refining method in a top-blowing refining process that is the focus of this embodiment. Fig. 2 is a schematic diagram for explaining the tilting angle of a converter-type vessel. Fig. 3 is a graph showing the relationship between the molten iron Si concentration and the tilting angle at the start of intermediate slag removal.
[0026] The refining method in the top-blowing refining process, which is the focus of the present embodiment described in detail below, includes the following steps, as shown in Fig. 1: a first step of charging molten iron into a converter-type vessel, a second step of subjecting the molten iron to desiliconization and dephosphorization, a third step of performing intermediate slag removal by tilting the converter-type vessel to remove slag from the throat of the converter-type vessel, and a fourth step of performing top-blowing refining. As shown in Fig. 1, the molten iron after the top-blowing refining process in the fourth step is tapped out of the furnace from the tapping hole of the converter-type vessel (fifth step).
[0027] <1st process> The first step is a step of charging molten iron into a converter-type vessel as shown in Fig. 1. Here, Fig. 1 focuses on a case where a top-blown converter is used as an example of a converter-type vessel and refining is performed by supplying oxygen from a top-blowing lance inserted into the top-blown converter, but the same as described below can also be applied to a case where a converter-type vessel other than a top-blown converter is used and oxygen is supplied by a different acid blowing method.
[0028] In the first step, molten iron is charged from a container such as a ladle into a converter-type vessel in which molten slag that was left in the furnace in the previous charge and solidified slag that was cooled and solidified are present. By having such slag present in the converter-type vessel, it is possible to reduce the amount of lime-based flux used in the second step, which is the subsequent stage, and thus to reduce flux costs. The amount of molten iron charged into the converter-type vessel is not particularly specified, and is appropriately set depending on the size of the converter-type vessel to be used, etc.
[0029] The chemical composition of the molten iron subjected to the first step is not particularly limited, but generally, the molten iron has a chemical composition containing 0.3 to 1.2 mass% Si, 0.08 to 0.18 mass% P, and the remainder being Fe and impurities.
[0030] <Second process> The second step is a step of subjecting the molten iron in the furnace to desiliconization and dephosphorization. The desiliconization and dephosphorization are carried out by adding various lime-based fluxes (slag forming agents) to the converter-type vessel furnace and blowing (blowing) an oxygen-containing gas (e.g., oxygen gas, oxidizing gas such as air, etc.) from a top blowing lance. In the second step, the slag generated by the acid blowing is foamed. The lime-based flux used here is not particularly specified, but various CaO sources such as quicklime, limestone, and various recycled slags including decarburized slag are used. The lime-based flux may be added before the start of acid blowing or during acid blowing, as long as the desired refining purpose is achieved.
[0031] Here, performing desiliconization and dephosphorization on molten pig iron using acid blowing means supplying oxygen to the molten pig iron to oxidize the Si in the molten pig iron to SiO2, and convert the Si in the molten pig iron into slag (i.e., desiliconization). In addition, acid blowing for the purpose of desiliconization inevitably causes the removal of P in the molten pig iron (dephosphorization). Therefore, if acid blowing is used for the purpose of dephosphorization, desiliconization is also unavoidably caused. In addition, dephosphorization using acid blowing is generally performed as a preliminary treatment for molten pig iron. By such acid blowing, substances that have oxidation properties similar to those of Si and P are oxidized and removed from the molten pig iron. For example, according to the commonly known Ellingham diagram, elements that are often treated as impurities, such as Mg, Li, Ti, Mn, Cr, Zn, and Sn, can be removed from the molten pig iron.
[0032] The amount of oxygen blown from the top blowing lance is not particularly specified either, and is set appropriately depending on the chemical composition and volume of the molten iron to be treated.
[0033] The degree of foaming of the slag generated in the second step (more specifically, the height of the foaming) can be measured by a known measuring device such as a microwave level meter. Based on the measurement results of such a measuring device, the height of the foaming of the slag can be grasped.
[0034] It is useful to express such foaming height as a percentage of a certain reference height. In the following, the height of the in-furnace freeboard in a converter-type vessel is taken as the reference, and the ratio of the foaming height of the slag to the in-furnace freeboard height is treated as the foaming height ratio.
[0035] More specifically, with the converter-type vessel standing upright, the molten metal bath surface (the top surface of the molten metal) is taken as the reference position, and the vertical height to the throat of the converter-type vessel is taken as the in-furnace freeboard height.Then, the ratio of the slag height (the position of the top surface of the foamed slag) from the measured reference position to the in-furnace freeboard height is calculated to obtain the foaming height ratio.
[0036] <3rd process> The third step is a step of performing intermediate slag discharge by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel. Here, the tilting angle of the converter-type vessel is defined as the angle between the center line of the furnace when the converter-type vessel is upright (standing vertically) (the center line when the furnace is down in FIG. 2) and the center line of the furnace when the converter-type vessel is tilted (the center line when tilted in FIG. 2). This tilting angle is defined as zero degrees when the converter-type vessel is upright, and increases as the converter-type vessel is tilted, until the tilting angle reaches 90° when the throat is facing horizontally.
[0037] As shown in FIG. 2, inside the converter-type vessel at the end of the second process, the molten metal that has been subjected to the desiliconization and dephosphorization processes is located at the bottom of the furnace, and above that, the liquefied slag is present, and above the liquefied slag, the foamed slag is present. When the converter-type vessel is tilted to a certain tilt angle, the foamed slag is discharged from the throat to the outside of the system. The tilt angle at which the foamed slag starts to be discharged from the throat is hereinafter referred to as the tilt angle at the start of intermediate slag discharge. Since the liquefied slag has high viscosity, it is difficult to discharge it from the throat even if the converter-type vessel is tilted. Only by foaming the slag to reduce its viscosity, can the slag in the furnace be discharged to the outside of the system.
[0038] <4th process> The fourth step is a step of adding flux into the converter-type vessel after the intermediate slag removal and performing a top-blowing refining process. The top-blowing refining process performed in the fourth step is not particularly limited, and may be a de-C process or a de-P process aimed at producing low-phosphorus steel, for example, in which the phosphorus concentration in the molten steel is 100 ppm or less. By the fourth step, the molten metal to be treated is further subjected to a top-blowing refining process, and a molten metal (molten steel) in a desired state can be obtained.
[0039] <Contents of study by the inventor> In the top blowing refining process carried out in the above-mentioned manner, the present inventors have conducted extensive research in order to solve the problems that arise during intermediate slag removal as mentioned above. The present inventors have conducted extensive research into the causes of insufficient slag removal volume and variations in the amount of slag remaining in a converter-type vessel when intermediate draining of the slag generated after molten iron pretreatment (de-Si treatment and de-P treatment) in a converter, and have discovered that attention should be focused on the foaming behavior of the slag.
[0040] As explained above, for intermediate slag removal, it is important that the slag is properly formed, and the tilt angle at the start of intermediate slag removal (hereinafter, simply referred to as the intermediate slag removal start angle) depends on the height of the slag forming. Therefore, it was presumed that if the height of the slag forming in the converter-type vessel varies for each treatment charge, it will cause variations in the amount of slag remaining in the furnace for each treatment charge, and also cause a shortage of slag discharge. Based on this idea, the inventor carried out an operation with a constant height of the slag forming, but the variation in the height of the slag forming could not be suppressed. Therefore, the inventor conducted a detailed investigation into the relationship between the actual state of slag forming in the above-mentioned second process and the intermediate slag removal start angle in the third process (intermediate slag removal process).
[0041] As a result, it became clear that the angle at which intermediate slag removal starts varies even when the forming height is kept constant. Furthermore, it was found that the tilting angle at the start of intermediate slag removal correlates with the Si concentration of the molten iron (before the start of molten iron pretreatment). An example of such a survey result is shown below with reference to Figure 3.
[0042] Figure 3 is a graph in which the horizontal axis represents the Si concentration (mass%) in the molten iron (before the start of molten iron pretreatment) and the vertical axis represents the intermediate slag drainage start angle (degrees). In the investigation shown in Figure 3, the foaming height at the time when acid blowing was stopped in the second process was controlled to be constant at a foaming height ratio of 0.6 to 0.7, and the Al2O3 concentration in the slag at the time when acid blowing was stopped was in the range of 0.1 to 0.3 mass%.
[0043] As shown in Fig. 3, even if the forming height ratio is controlled to be constant at 0.6 to 0.7, the intermediate slag draining start angle fluctuates in the range of approximately 55° to 73°. In addition, when plotting the molten iron Si concentration on the horizontal axis, it can be seen that the intermediate slag draining start angle can be plotted with a strong correlation to the molten iron Si concentration.
[0044] For example, when the molten iron Si concentration is a low value of 0.6 mass% or less, although there is some scatter in the plot, it is understood that intermediate slag removal cannot be started unless the converter-type vessel is tilted to about 65° or more. It is considered that when the oxygen blowing is stopped, gas is released from the bubbles in the foamed slag, and the height of the foaming starts to decrease. In other words, it is presumed that when the molten iron Si concentration is a low value of 0.6 mass% or less, the foaming of the slag is significantly calmed down. Based on the above findings suggested by Figure 3, the inventors have come up with the idea that the rate of decrease in the foaming height changes depending on the molten iron Si concentration.
[0045] When the molten pig iron Si concentration is low, 0.6 mass% or less, even if tilting of the converter-type vessel is started after the acid blowing is stopped in the second process, the foaming height decreases at a relatively fast rate, so that slag discharge does not start until the converter-type vessel is tilted to about 65° or more. Furthermore, since the slag whose foaming height has decreased becomes liquefied slag (high-density slag from which gas has been removed) and is in a highly viscous state, it is not as easy to discharge as foamed slag even if the tilting angle is increased, and it was presumed that a large amount of liquefied slag will remain in the furnace when the discharge of the molten metal begins (at the completion of intermediate slag discharge).
[0046] In addition, it is relatively common for the Si concentration of the molten iron to vary for each charge being treated, and estimating from past operational results that the Si concentration of the molten iron can vary, for example, between 0.1 and 1.2 mass% (frequently between 0.3 and 1.2 mass%). Therefore, it was presumed that the foaming height reduction rate varies for each charge being treated, and as a result, the amount of slag remaining in the converter-type vessel varies for each charge being treated.
[0047] Based on the above findings, the present inventors came up with the idea of reducing the rate at which the foaming height of the slag decreases and weakening the dependency of the rate at which the foaming height decreases on the Si concentration in the molten iron. They discovered that the Al2O3 concentration in the slag, which has not received much attention in the past, can be considered as an operational factor that can achieve such a situation.
[0048] Furthermore, as a result of further investigation based on the above findings, the inventors have come up with a method that, by focusing on the height of slag foaming, enables stable discharge of large amounts of slag during intermediate slag discharge in the treatment of multiple charges, including cases where the molten iron Si concentration is low, at or below 0.6 mass%, and cases where the molten iron Si concentration is high, exceeding 0.6 mass%.
[0049] Based on the above findings, in the first embodiment of the present invention shown below, a refining method capable of stably discharging a large amount of slag when the molten pig iron Si concentration is low, ie, 0.6 mass% or less, during intermediate slag disposal will be described. In the second embodiment of the present invention shown below, a refining method capable of stably discharging a large amount of slag when the molten pig iron Si concentration is low, ie, 0.6 mass% or less, during intermediate slag disposal will be described.
[0050] (First embodiment) In the first embodiment described below, a refining method in which the molten iron Si concentration (molten iron Si concentration at the start of the second step) is 0.6 mass% or less will be described in detail. The lower limit of the Si concentration of the molten iron is not particularly specified, but is usually about 0.1 mass%.
[0051] The refining method according to the first embodiment of the present invention is a refining method in a top-blowing refining process in which steel is refined using a converter-type vessel. As shown in Fig. 1, the refining method includes a first step of charging molten pig iron into the converter-type vessel, a second step of adding a lime-based flux into the converter-type vessel and blowing acid therein to desiliconize and dephosphorize the molten pig iron and form slag, a third step of performing intermediate slag discharging by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel, and a fourth step of adding flux into the converter-type vessel after the intermediate slag discharging and performing top-blowing refining.
[0052] As explained above, when the Si concentration of the molten iron (molten iron before the acid blowing treatment in the second process) was 0.6 mass% or less, the foaming height reduction rate was large, and a large amount of slag tended to remain inside the converter-type vessel even after intermediate slag removal.
[0053] However, in the refining method according to the present embodiment, as described in detail below, the Al2O3 concentration and the basicity, calculated by dividing the CaO concentration (unit: mass %) by the SiO2 concentration (unit: mass %) of the slag at the end of the second step are set within predetermined ranges, and the foaming height in the second step is controlled to satisfy specific conditions, so that a large amount of slag can be stably discharged during intermediate slag discharge.
[0054] <Chemical composition of slag when acid blowing in the second process is stopped> In the blowing method according to this embodiment, the Al2O3 concentration of the slag at the time when the acid blowing in the second step is stopped is set to a range of 0.5 mass % or more and 5.0 mass % or less, and the basicity is set to a range of 0.8 to 1.5.
[0055] [Basicity] In the second step of the refining method according to the present embodiment, foaming of the slag by blowing acid is an important factor. Here, in order to generate a desired amount of foaming of the slag with a normally applied amount of blowing acid, in the refining method according to the present embodiment, the basicity of the slag, which is the value obtained by dividing the CaO concentration (unit: mass%) by the SiO2 concentration (unit: mass%), is set to a range of 0.8 to 1.5. If the basicity of the slag is less than 0.8, the foamed slag tends to cause slopping (the foamed slag overflowing from the converter-type vessel), which is not preferable. The basicity of the slag at the end of the second step is preferably 0.9 or more, more preferably 1.0 or more.
[0056] On the other hand, if the basicity of the slag exceeds 1.5, the slag is not sufficiently slag-formed, and foaming is difficult to occur, which is undesirable. The basicity of the slag is preferably 1.4 or less, and more preferably 1.3 or less.
[0057] [Al2O3 concentration] According to the findings of the present inventors, the foaming occurring in the second step calms down after the acid blowing is stopped, and the height of the foaming decreases during the time from the stop of the acid blowing to the start of intermediate slag draining (usually about 0.5 to 10 minutes). If the decrease in the height of the foaming is not approximately constant, as mentioned above, the angle at which intermediate slag draining starts will not be constant and will vary, which will cause variations in the amount of slag remaining in the furnace.
[0058] According to the verification by the inventors as mentioned above, it was found that the rate of decrease in foam height tends to be affected by the Al2O3 concentration of the slag, which has not been focused on in the past.
[0059] Specifically, when the Al2O3 concentration is less than 0.5 mass%, Al2O3 may be unevenly distributed in the slag. As a result, depending on the position of the slag in the furnace where the forming is performed, there are some places where the rate of decrease in the forming height is high, while other places have a low rate of decrease in the forming height, resulting in variation in the rate of decrease in the forming height. This causes the rate of decrease in the forming height for each treated charge to become inconsistent. From this perspective, the Al2O3 concentration in the slag at the end of the second process is set to 0.5 mass% or more. The Al2O3 concentration in the slag at the end of the second process is preferably 1.0 mass% or more. By setting the Al2O3 concentration to 1.0 mass% or more, it is possible to more significantly suppress the variation in the rate of decrease in the forming height.
[0060] As a result of the verification by the inventors, it is possible to further reduce the rate of decrease in the forming height with an increase in the Al2O3 concentration. Here, at an Al2O3 concentration of about 4.0 mass%, the effect of suppressing the variation in the rate of decrease in the forming height as described above begins to saturate, and at an Al2O3 concentration of 5.0 mass%, the increase in the effect is no longer noticeable. From this perspective, the Al2O3 concentration in the slag at the end of the second step is set to 5.0 mass% or less.
[0061] The upper limit of the Al2O3 concentration that does not inhibit the dephosphorization action is about 6 mass%. Generally, the Al2O3 concentration in slag is controlled by adding a slag former, but from the viewpoint of cost reduction, it is desirable for the Al2O3 concentration to be low.
[0062] As described above, by setting the Al2O3 concentration in the slag at the end of the second step to 0.5 mass% or more and 5.0 mass% or less, it is possible to reduce the rate at which the foaming height decreases, and it is possible to achieve the desired foaming amount with the amount of acid blowing that is normally applied.
[0063] In addition to the above components, the slag often contains about 10 to 40% iron oxide in terms of Fe concentration, and may further contain other components. However, in order to obtain the effects of the refining method according to this embodiment, the above-mentioned range of components is sufficient, and the detailed concentrations are not specified.
[0064] In addition, the contents of components such as Al2O3, CaO, and SiO2 in the slag can be determined by a known measurement method such as ICP (Inductivity Coupled Plasma) emission spectroscopy.
[0065] <Height of slag foam when acid blowing is stopped in the second process> According to the findings of the present inventors, as explained above, the rate at which the foam height decreases is related to the Si concentration in the molten iron in addition to the Al2O3 concentration.
[0066] In the second process, the silicon in the molten iron is almost entirely oxidized by the acid blowing, generating SiO2 according to the silicon concentration, which becomes part of the slag. The slag generated during acid blowing consists of SiO2, which is the oxidized silicon, as well as iron oxide, manganese oxide, and phosphoric acid produced by the acid blowing, and the total amount of these components is about 70% of the slag after acid blowing is stopped. The CaO source, a refining material, is usually determined according to the silicon concentration of the molten iron, and the amount of slag in the furnace is generally determined according to the silicon concentration of the molten iron.
[0067] From the above viewpoint, when Fig. 3 is viewed, it can be seen that even if the foaming height of the slag is the same, the rate of decrease in foaming height varies depending on the amount of slag in the furnace (corresponding to the horizontal axis). Note that in Fig. 3, the basicity is in the range of 0.8 to 1.5, and the CaO source is 100% in terms of CaO, and quicklime (powdered CaO) mixed with 0 to 70 mass% of converter decarburization slag is used, and the effect of the origin of CaO on the intermediate slag discharge start angle could not be confirmed.
[0068] As mentioned previously, it has been found that when the molten iron Si concentration is 0.6 mass% or less, the rate of decrease in the foaming height is so large that a large amount of slag remains in the furnace after intermediate slag removal.
[0069] Therefore, as in the present embodiment, when the molten iron Si concentration is 0.6 mass% or less, it is necessary to realize a relatively high foaming height after the acid blowing refining in the second step, on the premise that the foaming height decreases at a high rate, and then perform the intermediate slag removal in the third step. This allows a large amount of foaming slag to be removed from the system before it liquefies, making it possible to reduce the amount of slag remaining in the furnace.
[0070] In this way, in the second step, it is important to constantly grasp the height of the slug and to specify the degree of forming. Therefore, in the second step according to the present embodiment, the height of the forming is measured.
[0071] [Measuring forming height] Here, in the second step according to the present embodiment, it is preferable to use a microwave level meter as shown in Fig. 4A and Fig. 4B in order to measure the forming height. This makes it possible to measure the forming height in a non-contact manner, and it is possible to further improve the convenience of the operation.
[0072] The device configuration and usage of the microwave level meter are briefly described below. The device configurations shown in Figures 4A and 4B are merely examples, and the microwave level meter used in this embodiment is not limited to those shown in Figures 4A and 4B.
[0073] The microwave level meter is a device that uses microwaves to measure the height of the slag surface in a converter-type vessel. As shown in FIG. 4A, the microwave level meter has an antenna unit and a device body that controls the antenna unit. As shown in FIG. 4B, the antenna unit has a transmitting antenna that irradiates microwaves into the furnace and a receiving antenna that receives microwaves from the furnace. A lens unit is provided at each tip of the transmitting antenna and the receiving antenna to increase the antenna gain (increase the signal strength), and a heat insulating plate is provided on the furnace body side of the lens unit to prevent heat from the furnace. As shown in FIG. 4A and FIG. 4B, the antenna unit of the microwave level meter is attached to an opening for inserting a sublance, which is provided in an exhaust hood above the furnace mouth.
[0074] Using such a microwave level meter, microwaves with a frequency exceeding 10 [GHz] and not exceeding 90 [GHz] are transmitted from a transmitting antenna into the converter-type vessel, and the microwaves reflected from the formed slag surface and received by a receiving antenna are measured, thereby determining the time from microwave transmission to reception. Half of the distance traveled by the microwave during the determined time corresponds to the distance to the slag surface. From this relationship, the height of the formed slag can be determined.
[0075] By using such a microwave level meter, the forming height can be quickly determined even when the material is hot, which can lead to a reduction in the amount of residual slag and suppression of variation in the amount of residual slag.
[0076] [Conditions that forming height must meet] Based on the above findings, the inventors conducted a detailed investigation into the correlation between the molten iron Si concentration, the slag foaming height ratio, and the amount of slag remaining in the furnace at the time of intermediate slag draining, and were able to determine the boundary line, on a coordinate plane defined by the molten iron Si concentration and the slag foaming height ratio, between a region where the amount of slag remaining in the furnace at the time of intermediate slag draining is preferable and a region where the amount of slag remaining in the furnace at the time of intermediate slag draining is unpreferable.
[0077] More specifically, operations are performed while changing the silicon concentration of the molten iron, and for each operation, the slag foaming height ratio is identified, and it is determined whether the amount of slag remaining in the furnace at the time of intermediate slag removal is in a desirable state or not. The obtained results are plotted on a coordinate plane defined by the silicon concentration of the molten iron and the foaming height ratio of the slag, using markers corresponding to desirable states and markers corresponding to undesirable states. Using the obtained plot, a straight line representing the boundary between the two regions can be determined by the linear least squares method, and an equation representing the boundary line can be obtained.
[0078] As described above, the inventor was able to obtain the following equation (1) which represents the boundary line between the region in which the amount of slag remaining in the furnace during intermediate slag discharge is desirable and the region in which the amount of slag remaining in the furnace during intermediate slag discharge is undesirable.
[0079] 0.6-0.3 × (Si concentration in molten iron at the start of the second process (unit: mass%)) ≦ foaming height ratio at the end of acid blowing Equation (1)
[0080] That is, in the refining method according to the present embodiment, by controlling the foaming height ratio of the slag when the acid blowing is stopped in the second step so as to satisfy the above formula (1), it becomes possible to stably discharge a large amount of slag during intermediate slag discharge. Furthermore, by making it possible to stably discharge a large amount of slag during intermediate slag discharge, it becomes possible to suppress the variation in the amount of slag remaining in the converter.
[0081] From the viewpoint of reducing the amount of slag remaining in the converter-type vessel, it is not necessary to set an upper limit for the foaming height ratio when the acid blowing is stopped. However, since the occurrence of slopping can be suppressed to enable smooth refining operations, it is preferable that the foaming height ratio when the acid blowing is stopped is 1.0 or less.
[0082] <End point temperature of molten iron in the second process> In the second step, the end temperature of the molten iron is preferably in the range of 1280 to 1380°C. By setting the end temperature of the molten iron to 1280°C or higher, it is possible to ensure that the progress levels of the desiliconization reaction and the dephosphorization reaction of the molten iron are in an appropriate state. In order to further advance these reactions, the end temperature of the molten iron is preferably set to 1300°C or higher, and more preferably set to 1310°C or higher. On the other hand, by setting the end temperature of the molten iron to 1380°C or lower, it is possible to advance these reactions while suppressing the decrease in the desiliconization efficiency and the dephosphorization efficiency. The end temperature of the molten iron is preferably set to 1360°C or lower, and more preferably set to 1350°C or lower.
[0083] In the second step, the oxygen supply time (acid blowing time) is not particularly specified as long as the slag basicity, Al2O3 concentration, and foaming height ratio satisfy the above conditions. However, in order to more stably achieve the desired amount of slag foaming, it is preferable that the oxygen supply time (acid blowing time) is within the range of 1 to 6 minutes.
[0084] The second step in the refining method according to this embodiment has been described in detail above.
[0085] <Other processes> In the refining method according to this embodiment, the first and third steps are not particularly limited, and each step may be carried out in the manner previously described with reference to FIG.
[0086] As for the fourth step, flux may be added to the converter-type vessel after intermediate slag removal in the manner previously described with reference to FIG. 1, and top-blowing refining processes such as decarbonization and dephosphorization may be performed.
[0087] Here, the end point temperature of the molten steel in the fourth step is not particularly specified and may be appropriately set depending on the target treatment, but for example, in the case of deP treatment, it is preferable to set it within the range of 1300 to 1380°C. By setting the end point temperature of the molten steel to 1300°C or more, it is possible to ensure that the progress level of the deP reaction of the molten steel is in an appropriate state. In order to further advance the deP reaction, the end point temperature of the molten steel is preferably set to 1320°C or more, and more preferably set to 1330°C or more. On the other hand, by setting the end point temperature of the molten steel to 1380°C or less, it is possible to advance these reactions while suppressing a decrease in the deP efficiency. The end point temperature of the molten steel is preferably set to 1360°C or less, and more preferably set to 1350°C or less.
[0088] Furthermore, in the fourth step, for example, in the case of deC treatment, the end point temperature of the molten steel is preferably in the range of 1560 to 1750°C. By setting the end point temperature of the molten steel at 1560°C or higher, it is possible to ensure that the progress level of the deC reaction of the molten steel is appropriate. In order to further advance the deC reaction, the end point temperature of the molten steel is preferably set to 1580°C or higher, and more preferably set to 1600°C or higher. On the other hand, by setting the end point temperature of the molten steel at 1750°C or lower, even if an operation that causes a decrease in the molten steel temperature, such as an alloy addition process subsequent to the deC treatment, is performed, it is possible to suppress a decrease in the molten steel temperature after tapping from the converter, and to avoid an excessive increase in the molten steel temperature.
[0089] In the fourth step, the oxygen supply time (acid blowing time) is not particularly specified, but it is preferable that the oxygen supply time (acid blowing time) is within a range of 1 to 6 minutes for deP treatment and within a range of 7 to 25 minutes for deC treatment.
[0090] In addition, when decarbonizing the molten steel in the fourth step, a part or all of the molten slag generated in the decarbonizing process may be left in the converter-type vessel and used as a lime-based flux in the second step of the next charge. By adopting such a method of using the molten slag, it is possible to reduce the flux cost in the second step.
[0091] In addition, when decarbonization of molten steel is performed as the fourth step, a part or all of the slag generated and discharged in the decarbonization process may be cooled, solidified, and collected, and the solidified slag obtained may be used as a lime-based flux in the second step of another charge. By adopting such a method of using the solidified slag, it is possible to reduce the flux cost in the second step.
[0092] The refining method according to the first embodiment of the present invention has been described in detail above.
[0093] As described above, according to the refining method of the first embodiment of the present invention, it is possible to discharge a large amount of slag during intermediate slag draining, which is generated after molten iron pretreatment (de-Si treatment and de-P treatment) in a converter.
[0094] This makes it possible to reduce the amount of rephosphorization during decarbonization, for example, when the treatment after intermediate slag removal (i.e., the fourth step) is a decarbonization treatment. Also, when the treatment after intermediate slag removal is a dephosphorization treatment, the amount of quicklime introduced into the furnace in the fourth step is small, and the dephosphorization effect can be obtained.
[0095] In addition, by using this refining method, it is possible to reduce the average amount of slag remaining when multiple charges are processed.
[0096] Second Embodiment In the first embodiment described above, a refining method for eliminating a large amount of slag remaining after intermediate slag removal when the molten iron Si concentration is low, ie, 0.6 mass% or less, has been described. By using this refining method, it is possible to reduce the average amount of slag remaining when multiple charges are processed.
[0097] Here, when multiple charge processing is considered, although the amount of residual slag is low, there may be variation, which may cause variation in the refining process after intermediate slag removal, such as variation in the amount of rephosphorization (in the case of decarbonization processing) and variation in the amount of dephosphorization (in the case of dephosphorization processing).
[0098] In the second embodiment described below, a refining method capable of suppressing the variation in the amount of residual slag among a plurality of charges regardless of the Si concentration of the molten iron will be described in detail. The lower limit of the Si concentration of the molten iron is not particularly specified, but may be about 0.1 mass%, and is usually about 0.3 mass%. Similarly, the upper limit of the Si concentration of the molten iron is not particularly specified, but is usually about 1.2 mass%.
[0099] The refining method according to the second embodiment of the present invention is a refining method in a top-blowing refining process in which steel is refined using a converter-type vessel. As also shown in Fig. 1, the refining method includes a first step of charging molten pig iron into the converter-type vessel, a second step of adding a lime-based flux into the converter-type vessel and blowing acid therein to perform de-Si and de-P treatment on the molten pig iron and form slag, a third step of performing intermediate slag discharge by tilting the converter-type vessel to discharge slag from the throat of the converter-type vessel, and a fourth step of adding flux into the converter-type vessel after the intermediate slag discharge and performing top-blowing refining.
[0100] <Chemical composition of slag at the end of the second process> In the blowing method according to this embodiment, as in the first embodiment, the Al2O3 concentration of the slag at the end of the second step is set to a range of 0.5% by mass to 5.0% by mass, and the basicity is set to a range of 0.8 to 1.5.
[0101] The reasons for setting the slag basicity and Al2O3 concentration within the above ranges and the effects obtained by setting them within these ranges are the same as those in the first embodiment, so detailed explanations will be omitted below.
[0102] <Height of slag foam when acid blowing is stopped in the second process> In the multi-charge process of this embodiment, the amount of slag remaining in the furnace varies in each charge, which causes the rate of reduction of the forming height to vary, and one of the main causes of such variation is the molten pig iron Si concentration in each charge. Therefore, by setting the forming height to a value range corresponding to the molten pig iron Si concentration, it is possible to suppress the variation in the amount of slag remaining in the furnace in each charge due to the variation in the molten Si concentration.
[0103] More specifically, in the refining method according to this embodiment, when the molten pig iron Si concentration is high and the rate of decrease in the foaming height is slow, the foaming height is set relatively low and the start position of the foaming height decrease is set low. On the other hand, when the molten pig iron Si concentration is low and the rate of decrease in the foaming height is fast, the foaming height is set relatively high and the start position of the foaming height decrease is set high, as in the first embodiment. This makes it possible to suppress the variation in the amount of slag remaining in the furnace at the end of intermediate slag removal.
[0104] Based on this policy, the inventors conducted research to identify an equation that represents the boundary between the region in which the amount of slag remaining in the furnace during intermediate slag removal is favorable and the region in which the amount of slag remaining in the furnace during intermediate slag removal is unfavorable, as in the first embodiment. As a result, the equation that represents the boundary was identified, and the condition expressed by the following equation (2) was obtained.
[0105] 0.6-0.3 × (Si concentration in molten iron at the start of the second process (unit: mass%)) ≦ foaming height ratio when acid blowing is stopped ≦ 0.8-0.3 × (Si concentration in molten iron at the start of the second process (unit: mass%)) Equation (2)
[0106] The above formula (2) specifies the upper and lower limits of the foaming height ratio. For example, when the molten pig iron Si concentration is low, a higher foaming height ratio range is set according to the foaming height reduction rate indicating a fast value. On the other hand, when the molten pig iron Si concentration is high, a lower foaming height ratio range is set according to the foaming height reduction rate indicating a slow value. In the refining method according to this embodiment, even if the molten pig iron Si concentration varies, including the effect of slowing down the foaming height reduction rate due to the chemical composition of the slag, the variation in the foaming state (foaming ratio) of the slag in the furnace at the end of intermediate slag removal is largely suppressed. As a result, the refining method according to this embodiment makes it possible to suppress the variation in the amount of slag remaining in the furnace.
[0107] That is, in the refining method according to the present embodiment, by controlling the foaming height ratio of the slag at the time of stopping the acid blowing in the second step so as to satisfy the above formula (2), even if the molten iron Si concentration fluctuates, the variation in the amount of slag remaining in the furnace is reduced, and it becomes possible to stably discharge a large amount of slag during intermediate slag draining. Furthermore, by making it possible to stably discharge a large amount of slag during intermediate slag draining, it becomes possible to suppress the variation in the amount of slag remaining in the converter. In addition, by controlling so as to satisfy the above formula (2), it becomes possible to suppress the variation in the amount of slag remaining among multiple charges.
[0108] In the refining method according to this embodiment, it is preferable to use a microwave level meter to measure the height of the forming, as in the first embodiment. The device configuration and method of use of the microwave level meter, and the effects obtained thereby are the same as those in the first embodiment, so detailed explanations will be omitted below.
[0109] <Other conditions in the second step> In the second step, other conditions such as the end temperature of the molten iron and the acid blowing time are also similar to those in the first embodiment, and therefore detailed description thereof will be omitted below.
[0110] The second step in the refining method according to this embodiment has been described in detail above.
[0111] <Other processes> In the refining method according to this embodiment, the first and third steps are not particularly limited, and each step may be carried out in the manner previously described with reference to FIG.
[0112] As for the fourth step, flux may be added to the converter-type vessel after intermediate slag removal in the manner previously described with reference to FIG. 1, and top-blowing refining processes such as decarbonization and dephosphorization may be performed.
[0113] Here, other conditions such as the end temperature of the molten steel and the acid blowing time in the fourth step are also similar to those in the first embodiment, and therefore detailed description thereof will be omitted below.
[0114] In addition, when decarbonization of molten steel is performed as the fourth step, a part or all of the molten slag generated in the decarbonization may be left in the converter-type vessel and used as a lime-based flux in the second step of the next charge, or a part or all of the slag generated and discharged in the decarbonization may be cooled and solidified, recovered, and the solidified slag obtained may be used as a lime-based flux in the second step of another charge. By adopting such a method of using the slag, it is possible to reduce the flux cost in the second step.
[0115] The refining method according to the second embodiment of the present invention has been described in detail above.
[0116] As described above, according to the refining method of the second embodiment of the present invention, it is possible to discharge a large amount of slag when intermediate draining of the slag generated after molten iron preliminary treatment (de-Si treatment and de-P treatment) in a converter-type vessel is performed, regardless of the level of the Si concentration of the molten iron in the furnace, and it is also possible to suppress variation in the amount of slag remaining in the furnace after intermediate draining.
[0117] This makes it possible to suppress the variation in the amount of rephosphorization during deC treatment for each charge when the treatment after intermediate slag removal (i.e., the fourth step) is a deC treatment. Also, when the treatment after intermediate slag removal is a deP treatment, it makes it possible to stabilize the phosphorus concentration in the molten metal after the deP treatment, and it becomes possible to stably produce low-phosphorus steel with a P content of, for example, 100 ppm or less. EXAMPLES
[0118] The refining method according to the present invention will be specifically described below with reference to examples. Note that the following examples are merely examples of the refining method according to the present invention, and the refining method according to the present invention is not limited to the following examples.
[0119] As an example of a converter-type vessel, a top-and-bottom blown converter with a capacity of 350 tons was used. A plurality of double-pipe tuyeres were installed at the bottom of the converter. Molten pig iron was charged into the converter in an amount ranging from 300 to 330 tons (first step). The composition of the molten pig iron was as shown in Table 1 below, with the remainder being Fe and impurities.
[0120] After the hot metal was charged, the top blowing lance located above the throat was lowered to blow oxygen-containing gas such as oxygen gas or air into the hot metal. At the same time, auxiliary materials were added from the top of the converter, including iron oxide sources such as sintered ore, iron ore, and dust, refining agents such as limestone and quicklime, lime raw materials such as slag discharged and recovered in the decarbonization process, Al2O3 raw materials such as agglomerate slag and Al2O3 powder, and dolomite as a refractory protection material. At this time, to increase the reaction rate, oxidizing gases such as oxygen and air were blown from the inner tube at the bottom of the converter, and cooling gases such as LPG, nitrogen, and CO2 were blown from the outer tube, and the hot metal and molten steel in the converter were constantly stirred.
[0121] As a result, in the de-Si / P treatment, which is an example of the second process, the de-Si reaction proceeded in the furnace by blowing in oxygen, forming SiO2, which in turn reacted with the added CaO-based solvent agent to form slag. In addition, toward the end of the de-Si reaction, the de-P reaction started. At this time, some of the blown oxygen reacted with the C in the molten iron to generate CO and CO2 bubbles, and these bubbles caused the foaming of the slag to proceed at the end of the de-Si / P treatment.
[0122] The slag composition in the second process was adjusted to have a basicity between 0.8 and 1.5 and an Al2O3 concentration between 0.5% and 5% by adjusting the amount of Al2O3 sources such as added lime raw material and agglomerate slag. The specific values shown in Tables 1 and 2 below were measured by ICP atomic emission spectrometry.
[0123] In the second step, the height of the foamed slag was constantly measured using a microwave level meter installed in the sublance hole located at the top of the converter. When the foamed slag state satisfied the above formula (1) (in the case of Table 1 below) or formula (2) (in the case of Table 2 below), blowing was stopped and the top lance was raised. Then, intermediate slag draining was performed by tilting the converter to discharge the slag from the throat (third step). The slag was discharged into a slag pot installed under the converter. At this time, the angle at which the slag started to flow out after tilting the converter was recorded as the intermediate slag draining start angle. The furnace was returned to the vertical position just before the molten pig iron in the furnace flowed out, and the intermediate slag draining was completed.
[0124] After intermediate slag removal was completed, the top blowing lance was lowered again to blow in oxygen-containing gas, and at the same time, quicklime and limestone, which are refining agents, were added to make the slag basicity 3.0 or higher and perform decarbonization (4th process). After decarbonization, the converter was tilted and the molten steel was removed from the converter's tapping hole into a ladle, completing the refining process.
[0125] <Method for measuring the amount of slag remaining in the furnace> The amount of slag in the furnace was calculated based on the amount of flux added, the Si concentration in the molten iron, and the slag composition. The amount of slag discharged was obtained from a weighing scale installed in the slag ladle, and the amount of slag remaining in the furnace was calculated by calculating the difference between the calculated total slag amount and the value obtained from the weighing scale.
[0126] <Evaluation criteria in Table 1, which is a test example corresponding to the first embodiment> In Table 1, which is a test example corresponding to the first embodiment, a grade of "A" was given when the amount of slag remaining in the furnace was less than 26 kg / t, and a grade of "B" was given when the amount of slag remaining in the furnace was 26 kg / t or more.
[0127] The reason why the threshold value of 26 kg / t was adopted as the judgment criterion is as follows: In the present invention, the amount of slag before intermediate slag removal tends to be large because acid blowing is performed in a state where blast furnace slag may be mixed in and where the Si in the molten iron is oxidized, and therefore the amount of slag remaining in the furnace tends to be large. Therefore, the threshold value was adopted as 26 kg / t, which is a slightly large value.
[0128] <Evaluation criteria in Table 2, which is a test example corresponding to the second embodiment> In Table 2, which is a test example corresponding to the second embodiment, 20 charges of operation were performed within a specific range of molten iron composition, the amount of residual slag was measured, and the minimum and maximum values of the amount of residual slag were evaluated. The difference between the maximum and minimum values was then used as a representative value of the variation. If the obtained variation was 10 kg / t or less, a rating of "A" was given, and if the variation exceeded 10 kg / t, a rating of "B" was given.
[0129] The results obtained are summarized in Tables 1 and 2 below. In Table 2 below, the notation "xy" indicates that the numerical value in the corresponding column was within the range of "greater than or equal to x and less than or equal to y."
[0130] [Table 1]
[0131] As is clear from Table 1 above, for Nos. 1 to 7, which are within the range of the present invention, the amount of slag remaining in the furnace was less than 26 kg / t.
[0132] In addition, when the Al2O3 concentration of the slag composition similar to that of No. 5 (Al2O3 concentration of 5.0 mass% and residual slag of 20 kg / t) was increased to 6.0 mass%, the residual slag became 20 kg / t, similar to No. 5. As is clear from these results, the effect of increasing the Al2O3 concentration was not obtained.
[0133] On the other hand, in Nos. 8 to 10, where acid blowing was stopped when the foaming height ratio was below the lower limit of formula (1), the foaming height decreased significantly between the end of acid blowing and the start of intermediate slag removal, and an excessive amount of slag remained in the furnace.
[0134] In No. 11, where the basicity was below the lower limit of 0.8, excessive slopping occurred during blowing, and the planned blowing could not be carried out. In No. 12, where the basicity exceeded the upper limit of 1.5, the slag could not be foamed due to poor slag formation of the added flux, and the slag could not be removed even when intermediate slag removal was performed.
[0135] In No. 13, where the alumina concentration was less than the lower limit of 0.5 mass%, the rate at which foaming decreased varied within the furnace, with many areas where the rate at which foaming decreased was rapid, resulting in a decrease in the amount of intermediate slag discharged and an increase in the amount of slag remaining in the furnace.
[0136] [Table 2]
[0137] In addition, when the operation was carried out within the range shown in Table 2 above, regardless of the Si concentration range, as long as the slag composition and forming height ratio were within the ranges specified in the second embodiment, the difference between the maximum and minimum values was 10 kg / t or less, and the variation in the amount of slag remaining in the furnace after intermediate slag removal could be suppressed.
[0138] On the other hand, when the operation was stopped at a value where the foaming height ratio exceeded the upper limit value of formula (2), excessive slag was discharged in the intermediate slag discharge, and the difference between the maximum and minimum amounts of slag remaining in the furnace exceeded 10 kg / t, resulting in large variation.
[0139] In both Tables 1 and 2, the amount of rephosphorization and the amount of quicklime charged during decarburization were able to obtain the effects of the present invention according to the amount of residual slag and the degree of variation in the amount of residual slag.
[0140] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
Claims
1. A refining method in a top blowing refining process for refining steel using a converter-type vessel, comprising the steps of: A first step of charging molten iron into the converter-type vessel; a second step of adding a lime-based flux into the converter-type vessel and blowing acid therein to desiliconize and dephosphorize the molten iron and form slag; A third step of performing intermediate slag draining by tilting the converter-type vessel to drain the slag from a throat of the converter-type vessel; A fourth step of adding flux into the converter-type vessel after intermediate slag removal and performing top blowing refining; Including, The Si concentration of the molten iron at the start of the second step is 0.6 mass% or less, Regarding the slag at the time of stopping the acid blowing in the second step, Al 2 O 3 The concentration is 0.5 mass% or more and 5.0 mass% or less, and the CaO concentration (unit: mass%) is SiO 2 The basicity divided by the concentration (unit: mass%) is 0.8 or more and 1.5 or less, In the second step, a height of the foaming is measured, and the height of the foaming when the acid blowing is stopped before the intermediate slag removal satisfies the following formula (1): 0.6-0.3 x (Si concentration of molten iron at the start of the second process (unit: mass%)) ≦ foaming height ratio at the time of stopping acid blowing ... formula (1) Here, in the above formula (1), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel.
2. A refining method in a top blowing refining process for refining steel using a converter-type vessel, comprising the steps of: A first step of charging molten iron into the converter-type vessel; a second step of adding a lime-based flux into the converter-type vessel and blowing acid therein to desiliconize and dephosphorize the molten iron and form slag; A third step of performing intermediate slag draining by tilting the converter-type vessel to drain the slag from a throat of the converter-type vessel; A fourth step of adding flux into the converter-type vessel after intermediate slag removal and performing top blowing refining; Including, Regarding the slag at the time of stopping the acid blowing in the second step, Al 2 O 3 The concentration is 0.5 mass% or more and 5.0 mass% or less, and the CaO concentration (unit: mass%) is SiO 2 The basicity divided by the concentration (unit: mass%) is 0.8 or more and 1.5 or less, In the second step, a height of the foaming is measured, and the height of the foaming when the acid blowing is stopped before the intermediate slag removal satisfies the following formula (2): 0.6-0.3 x (Si concentration of molten iron at the start of the second process (unit: mass%)) ≦ foaming height ratio at the time of stopping acid blowing ≦ 0.8-0.3 x (Si concentration of molten iron at the start of the second process (unit: mass%)) ... formula (2) Here, in the above formula (2), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel.
3. The refining method according to claim 1 or 2, wherein a microwave level meter is used to measure the height of the foam in the second step.
4. The fourth step is a step of performing decarburization refining, The refining method according to any one of claims 1 to 3, wherein the molten slag generated after the decarburization refining is partially left in the furnace, and the left molten slag is used as a part or the whole of the lime-based flux in the second step of the next charge.
5. The fourth step is a step of performing decarburization refining, The refining method according to any one of claims 1 to 3, wherein the solidified slag obtained by cooling and solidifying the molten slag generated after the decarburization refining is used as a part or all of the lime-based flux in the second step of another charge.
Citation Information
Patent Citations
Steelmaking method in converter
JP1993140627A
Converter refining method
JP1995018318A
Method for dephosphorizing molten iron
JP2001115205A
Method for refining molten iron
JP2002047509A
Method for removing slag in converter
JP2004323959A