Refining Method

The refining method stabilizes slag discharge by adjusting slag amount and composition, using microwave level meters to control forming height ratios, addressing the challenge of inconsistent slag removal in converter-type containers for high-purity steel production.

JP7568923B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021000488
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-05
Publication Date
2024-10-17
Estimated Expiration
2041-01-05

AI Technical Summary

Technical Problem

Existing refining methods for high-purity steel production in converter-type containers face challenges in stably discharging large amounts of slag during intermediate slag removal, leading to variations in slag composition and reduced productivity due to slopping and insufficient slag discharge.

Method used

A refining method that involves adjusting the slag amount to 20-40 kg/t-STEEL or 20-70 kg/t-STEEL, controlling the Si concentration to 0.28% by mass or less, setting the CaO concentration to 0.8-1.5, and using a microwave level meter to measure the forming height, with specific forming height ratios defined by equations (1) and (2) to ensure stable slag discharge.

Benefits of technology

Stable discharge of large amounts of slag is achieved, reducing variations in slag composition and improving productivity by minimizing slag remaining in the furnace, thereby maintaining consistent refining conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568923000003
    Figure 0007568923000003
  • Figure 0007568923000004
    Figure 0007568923000004
  • Figure 0007568923000005
    Figure 0007568923000005
Patent Text Reader

Abstract

To stably discharge a large amount of slag in intermediate deslagging in refining of molten metal in a converter type vessel.SOLUTION: The inventive refining method includes a first step for subjecting molten iron to at least an Si removal treatment, a second step for storing the molten metal having undergone the first step and slag in a converter type vessel and adjusting an amount of slag to be in a predetermined range, a third step for spraying acid into the converter type vessel to subject the molten metal to a P removal treatment, foaming the slag, a fourth step for performing intermediate deslagging to discharge slag out of the throat of the converter type vessel, and a fifth step for adding flux into the converter type vessel after intermediate deslagging, to subject the molten metal to a C removal treatment. At the finish of the first step, an Si content of the molten metal is 0.28 mass% or less. At the time when acid spraying is stopped in the third step, the slag has a basicity of 0.8-1.5. In the third step, a height of foaming is measured. At the time when acid spraying is stopped before intermediate deslagging, the height of foaming satisfies a formula (1).SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a refining method. [Background technology]

[0002] The refining process of molten pig iron in a converter-type vessel, typified by a converter, is a method in which blast furnace molten pig iron is charged into the converter-type vessel, and the molten pig iron is subjected to desiliconization (Si), dephosphorization (P), and decarburization (C) processes by adding a flux mainly consisting of quicklime and blowing oxygen (acid blowing) to produce steel. In recent years, in order to produce high-purity steel such as low-P steel and to reduce the amount of steelmaking slag generated as a by-product of converter refining, a converter-type vessel refining method (hereinafter abbreviated as "converter refining method") in which the desiliconization and dephosphorization processes are separated from the decarbonization process has been used.

[0003] Among the converter refining processes as described above, a widely used converter refining process (the so-called MURC process) is one in which, after de-Si and de-P processes (hereinafter abbreviated as "de-Si / P process"), the molten iron after the process is not discharged outside the converter, but the slag is discharged from the throat by tilting the converter (hereinafter referred to as "intermediate slag discharge"). Next, the molten iron in the converter is continuously subjected to de-C process.

[0004] The MURC process is characterized by the fact that the blowing process is divided into two processes, the de-Si / P process and the de-C process, with intermediate slag removal in between, which allows the slag composition and blowing conditions to be optimized separately for the de-Si / P process and the de-C process. This makes it possible to produce high-purity steel and reduce the amount of slag generated, compared to the converter refining process (so-called one-blow blowing), which performs the de-Si, de-P, and de-C processes all at once.

[0005] In addition, in the MURC process, the molten metal is not dumped outside the furnace during intermediate draining, but the slag is drained by tilting the furnace body, making it possible to quickly separate the molten metal and slag after treatment. This contributes to improved productivity compared to the converter refining process, in which the molten metal is once dumped outside the furnace after the de-Si / P treatment and then recharged into the converter for the de-C treatment.

[0006] In the MURC process, the slag composition and the oxygen blowing conditions are controlled during the desilicon / phosphorus treatment to perform intermediate slag removal, and the CO and CO generated by the reaction between the injected oxygen and the carbon in the molten iron are reduced. 2 The MURC process utilizes a phenomenon called foaming, in which the slag expands due to the foaming process. In the MURC process, the slag is expanded appropriately by foaming, and then the converter is tilted, making it possible to discharge only the slag from the furnace.

[0007] However, if excessive foaming occurs during the Si / P removal process, it will cause slopping, in which slag bubbles up from the furnace throat, resulting in reduced productivity.

[0008] For this reason, various techniques have been disclosed in the past, such as a technique for measuring the foaming height (also called the foaming level) in a converter to prevent slopping, and a method for desiliconizing the slag up to a foaming height where intermediate slag removal is easy.

[0009] For example, the following Patent Document 1 discloses a microwave measuring device for measuring the forming height in a furnace and a measurement method using the measuring device.

[0010] Furthermore, the following Patent Document 2 discloses a molten iron pretreatment method in which desiliconization and dephosphorization of molten iron are carried out continuously using a single converter-type refining furnace, with a slag removal process in between, in which a microwave level meter is used to terminate the desiliconization process at a predetermined height, thereby suppressing the accidental outflow of slag (slopping) during the slag removal process after desiliconization, and quickly removing a targeted, predetermined amount of desiliconized slag from the furnace in a short period of time.

[0011] In addition, the following Patent Document 3 discloses a technique for refining molten pig iron by using a single converter-type refining furnace to continuously perform a primary blowing process and a secondary blowing process with a slag removal process in between, and measuring the foaming height in the primary refining process with a microwave level meter and using the measured height for processing. More specifically, the following Patent Document 3 discloses a method for performing blowing until the foaming height ratio (the ratio of the slag height to the freeboard in the converter) is 0.6 or more, controlling the foaming height by introducing a foaming suppressant when it is 0.6 to less than 0.8, and terminating the primary refining process when the height ratio is 0.5 to 0.7, thereby suppressing the sudden outflow of slag in the primary blowing process and enabling the targeted predetermined amount of slag to be quickly discharged out of the furnace in a short time in the slag removal process after the primary blowing process.

[0012] Furthermore, in the following Patent Document 4, in a method for refining molten pig iron in which a single converter-type refining furnace is used to continuously perform a primary blowing process and a secondary blowing process of molten pig iron with a slag removal process in between, the primary blowing process is terminated when the slag height ratio in the furnace is 0.3 or more and less than 0.6, and then bottom blown gas is maintained for 1 minute or more and 5 minutes or less, and then slag discharge is initiated when the slag height ratio is 0.3 or more and less than 0.6, thereby making it possible to prevent the removed slag from foaming in a slag pot, and thereby to quickly discharge a targeted predetermined amount of slag in the furnace outside the furnace in a short period of time.

[0013] Thus, currently, there are disclosed techniques for monitoring the foaming state in the furnace, techniques for suppressing sudden slag outflow during refining by utilizing the foaming state in the furnace, foaming control techniques, and techniques for quickly discharging slag during intermediate slag discharge. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2018-87364 A [Patent Document 2] International Publication No. 2014 / 115526 [Patent Document 3] JP 2016-29212 A [Patent Document 4] JP 2017-133060 A Summary of the Invention [Problem to be solved by the invention]

[0015] However, although Patent Document 1 discloses a method for monitoring the forming state in the furnace, it does not disclose any technology for avoiding slopping or for keeping the amount of discharged slag constant.

[0016] Furthermore, the above Patent Documents 2 to 4 disclose techniques for preventing slopping and quickly discharging slag. However, as a result of verification by the present inventors, it was found that when the techniques disclosed in Patent Documents 2 to 4 are used to properly form slag in a furnace with a small amount of slag, for example, 20 to 40 kg / t-steel, it becomes difficult to sufficiently discharge the slag during intermediate slag discharge. This causes problems such as a reduction in the effect of the flux supplied to the molten metal in the refining process after intermediate slag discharge.

[0017] Furthermore, as a result of the study by the present inventors, it has become clear that in the case of a general range of slag amounts, such as 20 to 70 kg / t-steel, in the techniques of Patent Documents 2 to 4, the amount of slag remaining in the furnace after intermediate slag removal varies depending on the initial molten iron composition and slag amount in the furnace. If such a phenomenon occurs, problems will occur in the refining process after intermediate slag removal due to the variation in the slag amount. For example, if the refining process after intermediate slag removal is a decarburization process, the amount of rephosphorization during decarburization will vary, leading to a state in which excessive use of CaO to suppress the variation in the amount of rephosphorization cannot be suppressed.

[0018] As described above, even if the techniques disclosed in Patent Documents 2 to 4 above are used, there is still room for improvement in terms of stably discharging a large amount of slag during intermediate draining of the slag generated after molten iron pretreatment (desiliconization treatment and dephosphorization treatment) in a converter.

[0019] The present invention has been made in view of the above problems, and an object of the present invention is to provide a refining method capable of stably discharging a large amount of slag during intermediate slag discharge generated by the refining process of molten metal in a converter-type vessel. [Means for solving the problem]

[0020] In order to solve the above problems, the present inventors conducted further studies and discovered that it was necessary to focus on the foaming behavior of slag in a converter-type vessel, leading to the completion of the present invention described below. The gist of the present invention, which was completed based on these findings, is as follows.

[0021] [1] A refining method in a top blowing refining process for refining molten pig iron using a converter-type vessel, comprising: a first step of supplying an oxidizing agent to the molten pig iron to perform at least a desiliconization treatment on the molten pig iron; a second step of storing the molten pig iron and slag that have undergone the first step in the converter-type vessel and adjusting the amount of the slag to 20 to 40 kg / t-steel; and a second step of blowing acid into the converter-type vessel to perform a dephosphorization treatment on the molten pig iron and foam the slag. a third step, a fourth step of performing intermediate slag discharge by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel, and a fifth step of performing a top blowing refining process to perform a decarbonization process on the molten metal by adding flux into the converter-type vessel after the intermediate slag discharge, wherein the Si concentration of the molten metal at the end of the first step is 0.28 mass% or less, and the CaO concentration (unit: mass%) of the slag at the time when the acid blowing in the third step is stopped is 0.50 mass% or less. 2a basicity divided by a concentration (unit: mass%) is set to 0.8 or more and 1.5 or less, and in the third step, a height of the foaming is measured, and the height of the foaming at the time when the acid blowing is stopped before the intermediate slag discharge satisfies the following formula (1): 0.65-2.90 × (amount of slag before starting acid blowing in the third process (unit: kg / t-steel)) / 1000 ≦ foaming height ratio when acid blowing is stopped Formula (1) Here, in the above formula (1), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel. [2] A refining method in a top-blowing refining process for refining molten pig iron using a converter-type vessel, comprising: a first step of supplying an oxidizing agent to the molten pig iron to perform at least a desiliconization treatment on the molten pig iron; a second step of storing the molten metal and slag from the first step in the converter-type vessel and adjusting the amount of the slag to 20 to 70 kg / t-steel; a third step of blowing oxygen into the converter-type vessel to perform a dephosphorization treatment on the molten metal and foam the slag; a fourth step of performing intermediate slag discharge by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel; and a fifth step of performing a top-blowing refining treatment in which flux is added into the converter-type vessel after the intermediate slag discharge to perform a decarbonization treatment on the molten metal. Including, The Si concentration of the molten metal at the end of the first step is 0.28 mass% or less, and the CaO concentration (unit: mass%) of the slag at the time when the acid blowing in the third step is stopped is SiO 2 a basicity divided by a concentration (unit: mass%) is set to 0.8 or more and 1.5 or less, and in the third step, a height of the foaming is measured, and the height of the foaming at the time when the acid blowing is stopped before the intermediate slag discharge satisfies the following formula (2): 0.65-2.90×(amount of slag before starting acid blowing in the third process (unit: kg / t-STEEL)) / 1000 ≦ foaming height ratio when acid blowing is stopped ≦ 0.87-2.90×(amount of slag before starting acid blowing in the third process (unit: kg / t-STEEL)) / 1000 ··· formula (2) Here, in the above formula (2), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel. [3] The refining method according to [1] or [2], wherein a microwave level meter is used to measure the height of the foam in the third step. [4] A refining method according to any one of [1] to [3], in which a portion of the molten slag generated after the fifth step is left in the furnace, and the remaining molten slag is used to adjust the amount of the slag in the second step of the next charge. [5] A refining method according to any one of [1] to [3], wherein the solidified slag obtained by cooling and solidifying the molten slag produced after the fifth step is used to adjust the amount of the slag in the second step of another charge. Effect of the Invention

[0022] As described above, according to the present invention, when the slag generated by the refining process of the molten metal in the converter-type vessel is discharged in the intermediate slag discharge, it is possible to stably discharge a large amount of slag. Furthermore, since it is possible to stably discharge a large amount of slag during the intermediate slag discharge, it is possible to suppress the variation in the amount of slag remaining in the converter. [Brief description of the drawings]

[0023] [Figure 1] FIG. 2 is an explanatory diagram showing a schematic flow of a refining method in a top-blowing refining process that is the focus of an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining the tilting angle of a converter-type vessel. [Diagram 3] FIG. 1 is a graph showing the relationship between the amount of slag and the tilting angle at the start of intermediate slag removal. [Figure 4A] FIG. 2 is an explanatory diagram showing a schematic diagram of a microwave level meter used in the embodiment. [Figure 4B] FIG. 2 is an explanatory diagram showing a schematic diagram of a microwave level meter used in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.

[0025] (About the inventor's investigations and findings) Prior to describing the refining method according to the embodiment of the present invention, the investigations conducted by the present inventors and the findings that led to the conception of the refining method according to the present embodiment will be specifically described with reference to Figs. 1 to 3. Fig. 1 is an explanatory diagram showing a flow of a refining method in a top-blowing refining process that is the focus of this embodiment. Fig. 2 is a schematic diagram for explaining the tilting angle of a converter-type vessel. Fig. 3 is a graph showing the relationship between the amount of slag and the tilting angle at the start of intermediate slag discharge.

[0026] The refining method in the top-blowing refining process, which is the focus of the present embodiment described in detail below, includes the following steps as diagrammatically shown in FIG. 1: a first step of supplying an oxidizing agent to the molten pig iron to at least de-Si the molten pig iron; a second step of storing the molten metal and slag that have undergone the first step in a converter-type vessel and adjusting the amount of slag in the vessel to a predetermined amount; a third step of blowing oxygen into the converter-type vessel to de-P the molten metal and form the slag; a fourth step of performing intermediate slag dumping, in which the slag is dumped from the throat of the converter-type vessel by tilting the converter-type vessel; and a fifth step of performing top-blowing refining, in which flux is added into the converter-type vessel after the intermediate slag dumping and the molten metal is de-C treated.

[0027] <1st process> The first step is a step of at least desiliconizing the molten iron by supplying an oxidizing agent to the molten iron as described above. Here, in Fig. 1, for the sake of convenience, a top-blown converter is used as an example of a converter-type vessel, and attention is focused on a case where desiliconizing is performed by supplying oxygen from a top-blowing lance inserted in the top-blown converter, but the same as described below can be applied to a case where a converter-type vessel other than a top-blown converter is used (for example, a case where a torpedo car is used to transport the molten iron to the converter-type vessel).

[0028] Here, the chemical composition of the molten iron subjected to the first step is not particularly limited, but generally, the molten iron has a chemical composition containing 0.3 to 1.2 mass% Si, 0.08 to 0.18 mass% P, and the balance being Fe and impurities.

[0029] In the first step, it is sufficient that at least the desiliconization reaction is proceeding, and the dephosphorization reaction may also proceed together with the desiliconization reaction. Here, supplying oxygen to the molten iron to perform the desiliconization treatment means supplying oxygen to the molten iron to oxidize the Si in the molten iron to produce SiO 2 This means that the Si in the molten iron is converted into slag (i.e., desiliconized). The oxidizing agent is not particularly limited as long as it is a material that can oxidize and remove the Si in the molten iron, and examples of such an oxidizing agent include gaseous oxygen and iron oxide sources such as dust, iron ore, and sintered ore. The first step produces at least the molten iron that has been subjected to the desiliconization treatment, and slag. The slag contains not only the slag produced by the desiliconization reaction, but also a slag former containing CaO.

[0030] <Second process> The second step is a step of storing the molten metal and slag from the first step in a converter-type vessel and adjusting the amount of slag in the converter-type vessel to a predetermined amount. Here, in the second step, the amount of slag in the converter-type vessel is adjusted so that the amount of slag is suitable for the deP treatment performed in the third step. The adjustment of the amount of slag in the converter-type vessel can be achieved by reducing the amount of slag (i.e., discarding a part of it) or adding new flux when storing the molten metal and slag from the first step in the converter-type vessel. Also, if the amount of slag happens to be appropriate, it may be possible to omit reducing or adding it. As the flux, various lime-based fluxes (slag formers) can be used so that the slag composition is suitable for the deP treatment performed in the third step. Although not particularly specified, various CaO sources such as quicklime, limestone, various recycled slags including decarburization slag, etc. are used.

[0031] <3rd process> The third step is a step of dephosphorizing the molten metal by blowing acid into the converter-type vessel and foaming the slag. This dephosphorization is performed by blowing (blowing) an oxygen-containing gas (e.g., an oxidizing gas such as oxygen gas or air) from a top blowing lance into the converter-type vessel that stores the molten metal and the slag whose amount was adjusted in the second step. In the third step, the slag is foamed by blowing the acid.

[0032] Here, performing deP treatment on molten pig iron (molten metal) by acid blowing means supplying oxygen to the molten pig iron to oxidize the P in the molten pig iron and turn the P in the molten pig iron into slag (i.e., deP). In addition, acid blowing for the purpose of deP treatment inevitably causes the removal of Si in the molten pig iron (desiliconization treatment). Therefore, if acid blowing is performed for the purpose of deP treatment, desiliconization is also inevitably caused. In addition, deP treatment by acid blowing is generally performed as a preliminary treatment of molten pig iron. By such acid blowing treatment, substances that have the same oxidation properties as Si and P are oxidized and removed from the molten pig iron. For example, according to the commonly known Ellingham diagram, elements that are often treated as impurities, such as Mg, Li, Ti, Mn, Cr, Zn, and Sn, can be removed from the molten pig iron.

[0033] The amount of oxygen blown from the top blowing lance is not particularly specified either, and is set appropriately depending on the chemical composition and volume of the molten iron to be treated.

[0034] The degree of foaming of the slag generated in the third step (more specifically, the height of the foaming) can be measured by a known measuring device such as a microwave level meter. Based on the measurement results of such a measuring device, the height of the foaming of the slag can be grasped.

[0035] It is useful to express such foaming height as a percentage of a certain reference height. In the following, the height of the in-furnace freeboard in a converter-type vessel is taken as the reference, and the ratio of the foaming height of the slag to the in-furnace freeboard height is treated as the foaming height ratio.

[0036] More specifically, with the converter-type vessel standing upright, the molten metal bath surface (the top surface of the molten metal) is taken as the reference position, and the vertical height to the throat of the converter-type vessel is taken as the in-furnace freeboard height.Then, the ratio of the slag height (the position of the top surface of the foamed slag) from the measured reference position to the in-furnace freeboard height is calculated to obtain the foaming height ratio.

[0037] <4th process> The fourth step is an intermediate slag discharge step in which the converter-type vessel is tilted to discharge the slag from the throat of the converter-type vessel. Here, the tilting angle of the converter-type vessel is defined as the angle between the center line of the furnace when the converter-type vessel is upright (standing vertically) (the center line when the furnace is down in Fig. 2) and the center line of the furnace when the converter-type vessel is tilted (the center line when tilted in Fig. 2). This tilting angle is defined as zero degrees when the converter-type vessel is upright, and increases as the converter-type vessel is tilted, until the tilting angle reaches 90° when the throat is facing horizontally.

[0038] As shown in FIG. 2, inside the converter-type vessel at the end of the third process, the molten metal that has been subjected to the desiliconization and dephosphorization processes is located at the bottom of the furnace, and above that, the liquefied slag is present, and above the liquefied slag, the foamed slag is present. When the converter-type vessel is tilted to a certain tilt angle, the foamed slag is discharged from the throat to the outside of the system. The tilt angle at which the foamed slag starts to be discharged from the throat is hereinafter referred to as the tilt angle at the start of intermediate slag discharge. Note that the liquefied slag has high viscosity, so it is difficult to discharge it from the throat even if the converter-type vessel is tilted. Only by foaming the slag to reduce its viscosity can the slag in the furnace be discharged to the outside of the system.

[0039] <5th process> The fifth step is a step of adding flux into the converter-type vessel after the intermediate slag removal and performing a top-blowing refining process to decarbonize the molten metal. By the fifth step, the molten metal to be treated is further subjected to a top-blowing refining process (i.e., a decarbonization process), and a molten metal (molten steel) in a desired state can be obtained. The flux may be added before the start of acid blowing or during acid blowing, as long as the desired refining purpose is achieved.

[0040] <Contents of study by the inventor> In the top blowing refining process carried out in the above-mentioned manner, the present inventors have conducted extensive research in order to solve the problems that arise during intermediate slag removal as mentioned above. The present inventors have conducted extensive research into the causes of insufficient slag removal volume and variations in the amount of slag remaining in a converter-type vessel when intermediate draining of the slag generated after molten iron pretreatment (de-Si treatment and de-P treatment) in a converter, and have discovered that attention should be focused on the foaming behavior of the slag.

[0041] As explained above, for intermediate slag removal, it is important that the slag is appropriately formed, and the tilt angle at the start of intermediate slag removal (hereinafter, simply referred to as the intermediate slag removal start angle) during intermediate slag removal depends on the height of the slag forming. Therefore, it was presumed that if the height of the slag forming in the converter-type vessel varies for each treatment charge, it will cause variations in the amount of slag remaining in the furnace for each treatment charge, and also cause a shortage of slag discharge. Based on this idea, the inventor carried out an operation with the slag forming height constant while keeping the Si concentration of the molten pig iron approximately constant at 0.28 mass% or less, but the variation in the slag forming height could not be suppressed. Therefore, the inventor conducted a detailed investigation into the relationship between the actual state of slag forming in the above-mentioned third step and the intermediate slag removal start angle in the fourth step (intermediate slag removal step).

[0042] As a result, it became clear that the angle at which intermediate slag discharge starts varies even when the forming height is kept constant. Furthermore, it became clear that the tilt angle at the start of intermediate slag discharge correlates with the amount of slag before the start of deP treatment (the third process). An example of such a survey result is shown below with reference to Figure 3.

[0043] Figure 3 is a graph in which the horizontal axis represents the amount of slag in the furnace before the start of acid blowing in the third process (kg / t-steel: kg amount per ton of molten steel) and the vertical axis represents the intermediate slag drain start angle (degrees). In the survey shown in Figure 3, the foaming height at the end of acid blowing in the third process was controlled to be constant at a foaming height ratio of 0.6 to 0.7. 2 O 3 The concentration was 0.1 to 0.3 mass%, and the Si concentration in the molten metal was roughly constant at 0.28 mass% or less.

[0044] As shown in Fig. 3, even if the forming height ratio is constant at 0.6 to 0.7, the intermediate slag drainage start angle varies in the range of approximately 64° to 76°. In addition, when the amount of slag on the molten metal before the start of acid blowing in the third process is plotted on the horizontal axis, it can be seen that the intermediate slag drainage start angle can be plotted with a strong correlation to the amount of slag before the start of acid blowing in the third process.

[0045] For example, when the amount of slag on the molten metal is low, such as 20 to 40 kg / t-STEEL, the plots show some variation, but it is clear that intermediate slag removal cannot be started unless the converter is tilted at about 70° or more. It is considered that the foamed slag releases gas from the bubbles when the acid blowing is stopped, and the foaming height starts to decrease. In other words, it is presumed that when the slag amount is low, such as 20 to 40 kg / t-STEEL or less, the foaming of the slag subsides significantly. Based on the above findings suggested by FIG. 3, the inventors have come to the conclusion that the rate of decrease in the foaming height changes depending on the amount of slag in the furnace before the start of the third process.

[0046] Focusing on the case of 20-40 kg / t-STEEL, where the amount of slag in the furnace before the start of the third process is small, even if tilting of the converter-type vessel is started after the stop of the acid blowing in the third process, the rate of decrease in foaming height is relatively fast, so that slag discharge does not start until the converter-type vessel is tilted to about 70° or more. Furthermore, since the slag with a decreased foaming height becomes liquefied slag (high-density slag from which gas has been removed) and is in a highly viscous state, it is not as easy to discharge as foamed slag even if the tilting angle is increased, and it was inferred that a large amount of liquefied slag will remain in the furnace when the discharge of the molten metal begins (at the completion of intermediate slag discharge).

[0047] In addition, the amount of slag in the furnace before the start of the third process varies for each treated charge relatively frequently, and estimating from past operational results, the amount of slag in the furnace before the start of the third process can vary, for example, between 20 and 70 kg / t-steel. Therefore, it was presumed that the foaming height reduction rate varies for each treated charge, and as a result, the amount of slag remaining in the converter-type vessel varies for each treated charge.

[0048] Based on the above findings and on the fact that the time from the stop of acid blowing in the third process to the start of intermediate slag discharge is approximately 10 minutes at most, it has been discovered that when the amount of slag in the furnace, in which the rate of decrease in the foaming height is relatively fast, is small at 20 to 40 kg / t-steel, the foaming height can be set high in advance to avoid a decrease in the amount of intermediate slag discharge and to reduce the amount of slag in the furnace after intermediate slag discharge (after the end of the fourth process).

[0049] Furthermore, as a result of further investigation based on the above findings, the inventors have come up with a method that, by focusing on the height of slag foaming, enables a stable discharge of a large amount of slag during intermediate slag discharge in the treatment of multiple charges, including cases in which the amount of slag in the furnace before the start of the third process is as low as 20 to 40 kg / t-steel to cases in which the amount of slag in the furnace before the start of the third process is as high as more than 40 kg / t-steel.

[0050] Based on the above findings, in the first embodiment of the present invention shown below, a refining method capable of stably discharging a large amount of slag when intermediately discharging slag will be described when the amount of slag in the furnace before the start of the third step is as small as 20 to 40 kg / t-steel. In addition, in the second embodiment of the present invention shown below, a refining method capable of stably discharging a large amount of slag when intermediately discharging slag will be described, regardless of the amount of slag in the furnace before the start of the third step.

[0051] (First embodiment) In the first embodiment shown below, a refining method in which the amount of slag in the furnace before the start of the third step is small, such as 20 to 40 kg / t-steel, will be described in detail.

[0052] The refining method according to the first embodiment of the present invention is a refining method in a top-blowing refining process for refining steel using a converter-type vessel. As shown in Fig. 1, the refining method includes a first step of supplying an oxidizing agent to the molten pig iron to perform at least a desiliconization treatment on the molten pig iron, a second step of storing the molten iron and slag that have been subjected to the first step in a converter-type vessel and adjusting the amount of slag to 20 to 40 kg / t-steel, a third step of blowing oxygen into the converter-type vessel to perform a dephosphorization treatment on the molten iron and foam the slag, a fourth step of performing intermediate slag discharge by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel, and a fifth step of performing a top-blowing refining treatment by adding flux into the converter-type vessel after the intermediate slag discharge to perform a decarbonization treatment on the molten iron.

[0053] <Si concentration in molten metal after the first process> In the first step described above, in the refining method according to this embodiment, the de-siliconization treatment is carried out in the first step so that the Si concentration in the molten metal after the first step is 0.28 mass % or less.

[0054] If the Si concentration of the molten metal after the first step exceeds 0.28% by mass, the amount of oxygen consumed for desiliconization in the acid blowing for the purpose of deP treatment in the subsequent third step increases, and the P concentration of the molten metal after the deP treatment is likely to deviate from the desired concentration. In other words, if the Si concentration of the molten metal after the first step exceeds 0.28% by mass, the desiliconization reaction will proceed preferentially compared to the deP reaction.

[0055] By keeping the Si concentration of the molten metal after the first step to 0.28 mass% or less, it is possible to reduce the proportion of oxygen consumed for de-Si in the acid blowing for the purpose of de-P treatment in the subsequent third step, thereby making it possible to steadily progress the de-P treatment and achieve the desired P concentration.

[0056] However, the inventors have found that if the Si concentration of the molten metal after the first step is 0.28 mass% or less, there is no significant increase in the amount of slag in the furnace in the subsequent third step, and the slag cannot be sufficiently removed during intermediate slag removal after the deP treatment. Therefore, in the refining method according to this embodiment, the height of the slag foaming in the subsequent third step is appropriately controlled, as described in detail below, to achieve sufficient slag removal.

[0057] In addition, in the first step, as long as oxygen is supplied so that the Si concentration after the treatment is 0.28 mass % or less and the molten material after the treatment can be called a molten metal, the treatment conditions other than those described above are not particularly specified, and various methods can be used as appropriate.

[0058] <Adjustment of slag amount in the second process> In the second step of the refining method according to this embodiment, the molten metal after the first step, in which the Si concentration is reduced to 0.28 mass% or less as described above, and the slag generated by the desiliconization treatment in the first step are stored in a converter-type vessel, and the amount of the slag is adjusted to 20 to 40 kg / t-steel.

[0059] <Conditions for the third step> In the third step of the blowing method according to the present embodiment, the molten metal that has been through the second step is dephosphorized by blowing acid into a converter-type vessel, and the slag with the adjusted slag amount is foamed.

[0060] As described above, since the Si concentration in the molten metal after the first step is controlled to 0.28 mass% or less, in the third step according to this embodiment, it becomes possible to perform a sufficient de-P treatment on the molten metal.

[0061] On the other hand, the amount of slag in the furnace at the start of acid blowing in the third process is small at 20 to 40 kg / t-steel, and the amount of slag generated by acid blowing is also small because the Si concentration of the molten metal is controlled to 0.28 mass% or less. Therefore, as shown in Figure 3, even if the foaming height ratio is about 0.6 to 0.7, it is presumed that the intermediate slag discharge start angle becomes larger compared to when the amount of slag in the furnace is large, the liquefaction of the foaming slag progresses faster, and the foaming height decreases faster.

[0062] Therefore, as the present embodiment focuses on, when the amount of slag at the start of acid blowing in the third step is small, such as 20 to 40 kg / t-steel, the height of the slag foaming before the start of intermediate slag draining in the fourth step is set high in advance, which makes it possible to reduce the angle at which intermediate slag draining starts, and as a result, the slag in the furnace can be sufficiently drained.

[0063] [Chemical composition of slag when acid blowing is stopped in the third process] In the third step of the refining method according to the present embodiment, foaming of slag by acid blowing is an important factor. Here, in order to generate a desired amount of foaming of slag with a normally applied amount of acid blowing, in the refining method according to the present embodiment, the CaO concentration (unit: mass%) is adjusted to SiO 2The basicity of the slag, which is the value obtained by dividing the concentration (unit: mass%), is set to be within the range of 0.8 to 1.5. If the basicity of the slag is less than 0.8, the foamed slag is more likely to cause slopping (overflow of the foamed slag from the converter-type vessel), which is not preferable. The basicity of the slag at the end of the third step is preferably 0.9 or more, more preferably 1.0 or more.

[0064] On the other hand, if the basicity of the slag exceeds 1.5, the slag is not sufficiently slag-formed, and foaming is difficult to occur, which is undesirable. The basicity of the slag is preferably 1.4 or less, and more preferably 1.3 or less.

[0065] In addition, the slag contains CaO, SiO 2 In addition to phosphoric acid, iron oxide is often contained at 10 to 40% in terms of Fe concentration, and other components may also be contained. However, in order to obtain the effects of the refining method according to this embodiment, the above-mentioned range of components is sufficient, and the detailed concentrations are not specified.

[0066] In addition, CaO, SiO 2 The contents of the above components can be determined by known measurement methods such as ICP (Inductivity Coupled Plasma) emission spectroscopy.

[0067] <Height of slag foam when acid blowing is stopped in the third process> According to the findings of the present inventors, as explained above, the rate at which the foaming height decreases is related to the amount of slag in the furnace before the start of acid blowing in the third step.

[0068] In the third process, almost all of the Si in the molten iron is oxidized by acid blowing, and SiO 2 The slag generated during acid blowing is SiO 2In addition, iron oxide, manganese oxide, and phosphoric acid are produced by acid blowing, and the total amount of these components accounts for about 70% of the slag after acid blowing is stopped.

[0069] From the above viewpoint, when Fig. 3 is viewed, it can be seen that even if the foaming height of the slag is the same, the rate of decrease in foaming height varies depending on the amount of slag in the furnace. Note that Fig. 3 shows that the basicity is in the range of 0.8 to 1.5, the amount of CaO converted into CaO is 100%, and quicklime (powdered CaO) mixed with 0 to 70 mass% of converter decarburization slag is used, and the effect of the origin of CaO on the intermediate slag discharge start angle could not be confirmed.

[0070] As mentioned previously, it has been found that when the amount of slag in the furnace at the start of the acid blowing in the third process is small, such as 20 to 40 kg / t-steel, the rate of decrease in the foaming height is so large that a large amount of slag remains in the furnace after intermediate slag removal.

[0071] Therefore, as in the present embodiment, when the amount of slag in the furnace at the start of the acid blowing in the third step is small, such as 20 to 40 kg / t-steel, it is necessary to realize a relatively high foaming height in advance after the acid blowing refining in the third step, on the premise that the foaming height decreases at a high rate, and then perform the intermediate slag removal in the fourth step. This allows a large amount of foaming slag to be removed from the system before it liquefies, making it possible to reduce the amount of slag remaining in the furnace.

[0072] In this way, in the third step, it is important to constantly grasp the height of the slug and to specify the degree of forming. Therefore, in the third step according to the present embodiment, the height of the forming is measured.

[0073] [Measuring forming height] Here, in the third step according to the present embodiment, it is preferable to use a microwave level meter as shown in Fig. 4A and Fig. 4B in order to measure the forming height. This makes it possible to measure the forming height in a non-contact manner, and it is possible to further improve the convenience of operation.

[0074] The device configuration and usage of the microwave level meter are briefly described below. The device configurations shown in Figures 4A and 4B are merely examples, and the microwave level meter used in this embodiment is not limited to those shown in Figures 4A and 4B.

[0075] The microwave level meter is a device that uses microwaves to measure the height of the slag surface in a converter-type vessel. As shown in FIG. 4A, the microwave level meter has an antenna unit and a device body that controls the antenna unit. As shown in FIG. 4B, the antenna unit has a transmitting antenna that irradiates microwaves into the furnace and a receiving antenna that receives microwaves from the furnace. A lens unit is provided at each tip of the transmitting antenna and the receiving antenna to increase the antenna gain (increase the signal strength), and a heat insulating plate is provided on the furnace body side of the lens unit to prevent heat from the furnace. As shown in FIG. 4A and FIG. 4B, the antenna unit of the microwave level meter is attached to an opening for inserting a sublance, which is provided in an exhaust hood above the furnace mouth.

[0076] Using such a microwave level meter, microwaves with a frequency exceeding 10 [GHz] and not exceeding 90 [GHz] are transmitted from a transmitting antenna into the converter-type vessel, and the microwaves reflected from the formed slag surface and received by a receiving antenna are measured, thereby determining the time from microwave transmission to reception. Half of the distance traveled by the microwave during the determined time corresponds to the distance to the slag surface. From this relationship, the height of the formed slag can be determined.

[0077] By using such a microwave level meter, the forming height can be quickly determined even when the material is hot, which can lead to a reduction in the amount of residual slag and suppression of variation in the amount of residual slag.

[0078] [Conditions that forming height must meet] Based on the above findings, the inventors conducted a detailed investigation into the correlation between the amount of slag in the furnace at the start of acid blowing in the third step, the foaming height ratio of the slag, and the amount of slag remaining in the furnace at the time of intermediate slag draining, and were able to determine the boundary line between the region where the amount of slag remaining in the furnace at the time of intermediate slag draining is preferable and the region where the amount of slag remaining in the furnace at the time of intermediate slag draining is unpreferable on the coordinate plane defined by the amount of slag in the furnace at the start of acid blowing in the third step and the foaming height ratio of the slag.

[0079] More specifically, operations are performed while changing the amount of slag in the furnace at the start of the third step of acid blowing, and for each operation, the foaming height ratio of the slag is specified, and it is determined whether the amount of slag remaining in the furnace at the time of intermediate slag removal is in a desirable state or not. The obtained results are plotted on a coordinate plane defined by the amount of slag in the furnace at the start of the third step of acid blowing and the foaming height ratio of the slag, using markers corresponding to desirable states and markers corresponding to undesirable states. Using the obtained plot, a straight line representing the boundary between the two regions can be determined by the linear least squares method, and an equation representing the boundary line can be obtained.

[0080] As described above, the inventor was able to obtain the following equation (1) which represents the boundary line between the region in which the amount of slag remaining in the furnace during intermediate slag discharge is desirable and the region in which the amount of slag remaining in the furnace during intermediate slag discharge is undesirable.

[0081] 0.65-2.90 × (amount of slag before starting acid blowing in the third process (unit: kg / t-steel)) / 1000 ≦ foaming height ratio when acid blowing is stopped Formula (1)

[0082] That is, in the refining method according to the present embodiment, by controlling the foaming height ratio of the slag at the time of stopping the acid blowing in the third step so as to satisfy the above formula (1), it becomes possible to stably discharge a large amount of slag during intermediate slag discharge. Furthermore, by making it possible to stably discharge a large amount of slag during intermediate slag discharge, it becomes possible to suppress the variation in the amount of slag remaining in the converter.

[0083] From the viewpoint of reducing the amount of slag remaining in the converter-type vessel, it is not necessary to set an upper limit for the foaming height ratio when the acid blowing is stopped. However, since the occurrence of slopping can be suppressed to enable smooth refining operations, it is preferable that the foaming height ratio when the acid blowing is stopped is 1.0 or less.

[0084] <End point temperature of molten steel in the third process> The end point temperature of the molten steel in the third step is not particularly limited and may be set appropriately, but is preferably set within a range of 1280 to 1380°C, for example. By setting the end point temperature of the molten steel at 1280°C or higher, it is possible to ensure that the progress level of the deP reaction of the molten steel is at an appropriate state. In order to further advance this reaction, the end point temperature of the molten steel is preferably set at 1300°C or higher, and more preferably set at 1310°C or higher. On the other hand, by setting the end point temperature of the molten steel at 1380°C or lower, it is possible to advance the deP reaction while suppressing a decrease in the deP efficiency. The end point temperature of the molten steel is preferably set at 1360°C or lower, and more preferably set at 1350°C or lower.

[0085] In the third step, the oxygen supply time (acid blowing time) is not particularly limited, but it is preferable that the oxygen supply time (acid blowing time) is within the range of, for example, 1 to 6 minutes.

[0086] <Regarding the 4th and 5th steps> In the refining method according to this embodiment, the fourth step is not particularly limited, and the fourth step may be carried out in the manner previously described with reference to FIG.

[0087] Also, in the fifth step, the decarbonization process may be carried out by adding flux to the converter-type vessel after intermediate slag removal in the same manner as previously described with reference to FIG.

[0088] Here, the end temperature of the molten steel in the fifth step is not particularly specified and may be set appropriately, but is preferably set within the range of 1560 to 1750°C, for example. By setting the end temperature of the molten steel at 1560°C or higher, it is possible to ensure that the progress level of the deC reaction of the molten steel is at an appropriate state. In order to further advance this reaction, the end temperature of the molten steel is preferably set to 1580°C or higher, and more preferably set to 1590°C or higher. On the other hand, by setting the end temperature of the molten steel at 1750°C or lower, even if work that causes a decrease in the molten steel temperature, such as an alloy addition process subsequent to the deC process, is performed, the decrease in the molten steel temperature after tapping from the converter can be suppressed, and an excessive increase in the molten steel temperature can be avoided.

[0089] In the fifth step, the oxygen supply time (acid blowing time) is not particularly limited, but it is preferable that the oxygen supply time (acid blowing time) is within the range of, for example, 7 to 25 minutes.

[0090] In the fifth step, a part or all of the molten slag generated in the decarbonization process may be left in the converter-type vessel and used to adjust the amount of slag in the second step of the next charge. By adopting such a method of using the molten slag, it is possible to reduce the flux cost in the second step.

[0091] In addition, in the fifth step, a part or all of the slag generated and discharged in the decarbonization process may be cooled and solidified, and recovered, and the solidified slag obtained may be used to adjust the amount of slag in the second step of another charge. By adopting such a method of using the solidified slag, it is possible to reduce the flux cost in the second step.

[0092] The refining method according to the first embodiment of the present invention has been described in detail above.

[0093] As described above, according to the refining method of the first embodiment of the present invention, when the slag generated after the refining process (e.g., de-P process) of the molten metal in the converter type vessel is discharged, a large amount of slag can be discharged. As a result, it is possible to further reduce the amount of rephosphorization during the de-C process carried out after the intermediate slag discharge.

[0094] In addition, by using this refining method, it is possible to reduce the average amount of slag remaining when multiple charges are processed.

[0095] Second embodiment In the first embodiment described above, a refining method for eliminating a large amount of slag remaining after intermediate slag removal when the amount of slag in the furnace before the start of the third process is small, such as 20 to 40 kg / t-steel, has been described. By using this refining method, it is possible to reduce the average amount of slag remaining when multiple charges are processed.

[0096] However, in consideration of the variation in the P concentration of the molten metal to be dephosphorized, the amount of slag material charged into the furnace may increase, and according to past operational results, the amount of slag in the furnace may vary within the range of 20 to 70 kg / t-steel. If multiple charge treatment is assumed under such a premise, the amount of residual slag may vary even though it is a low value, which may cause variation in the amount of rephosphorization in the refining process after intermediate slag removal.

[0097] In the second embodiment shown below, a refining method capable of suppressing the variation in the amount of residual slag among a plurality of charges, regardless of the amount of slag in the furnace before the start of the third process, will be described in detail.

[0098] The refining method according to the second embodiment of the present invention is a refining method in a top-blowing refining process for refining steel using a converter-type vessel. As shown in Fig. 1, the refining method includes a first step of supplying an oxidizing agent to the molten pig iron to perform at least a desiliconization treatment on the molten pig iron, a second step of storing the molten iron and slag that have been subjected to the first step in a converter-type vessel and adjusting the amount of slag to 20 to 70 kg / t-steel, a third step of blowing oxygen into the converter-type vessel to perform a dephosphorization treatment on the molten iron and foam the slag, a fourth step of performing intermediate slag discharge by tilting the converter-type vessel to discharge the slag from the throat of the converter-type vessel, and a fifth step of performing a top-blowing refining treatment by adding flux into the converter-type vessel after the intermediate slag discharge to perform a decarbonization treatment on the molten iron.

[0099] Here, in the refining method according to this embodiment, the first step, the fourth step, and the fifth step are similar to those in the refining method according to the first embodiment, and therefore detailed explanations thereof will be omitted below.

[0100] <Amount of slag in the furnace in the second process> In the second step of the refining method according to this embodiment, the amount of slag in the furnace is adjusted to within a range of 20 to 70 kg / t-STEEL, taking into consideration the variation in the amount of slag in the furnace as described above. Since the second step is the same as that in the first embodiment except that the target value of the amount of slag in the furnace is different from that in the first embodiment, detailed description will be omitted below.

[0101] <3rd process> [Chemical composition of slag when acid blowing is stopped] In the blowing method according to this embodiment, similarly to the first embodiment, the basicity of the slag at the time of stopping the acid blowing in the third step is set to 0.8 to 1.5. The reason for setting the basicity of the slag within this range and the effects obtained by setting it within this range are similar to those in the first embodiment, and therefore detailed explanations will be omitted below.

[0102] [Slag forming height] In the multi-charge process of this embodiment, the amount of slag remaining in the furnace varies in each charge, which causes the rate of reduction of the foaming height to vary. One of the main causes of such variation is the amount of slag remaining in the furnace in each charge. Therefore, if the setting value of the foaming height is set to a numerical range according to the amount of slag in the furnace, it is possible to suppress the variation in the amount of slag remaining in the furnace after intermediate slag removal in each charge due to the variation in the amount of slag in the furnace.

[0103] More specifically, in the refining method according to this embodiment, when the amount of slag in the furnace is large and the rate of decrease in the foaming height is slow, the foaming height is set relatively low and the start position of the foaming height decrease is set low. On the other hand, when the amount of slag in the furnace is small and the rate of decrease in the foaming height is fast, the foaming height is set relatively high and the start position of the foaming height decrease is set high, as in the first embodiment. This makes it possible to suppress the variation in the amount of slag remaining in the furnace at the end of intermediate slag removal.

[0104] Based on this policy, the inventors conducted research to identify an equation that represents the boundary between the region in which the amount of slag remaining in the furnace during intermediate slag removal is favorable and the region in which the amount of slag remaining in the furnace during intermediate slag removal is unfavorable, as in the first embodiment. As a result, the equation that represents the boundary was identified, and the condition expressed by the following equation (2) was obtained.

[0105] 0.65-2.90×(amount of slag before starting acid blowing in the third process (unit: kg / t-STEEL)) / 1000 ≦ foaming height ratio when acid blowing is stopped ≦ 0.87-2.90×(amount of slag before starting acid blowing in the third process (unit: kg / t-STEEL)) / 1000 ··· formula (2)

[0106] The above formula (2) specifies the upper and lower limits of the foaming height ratio. For example, when the amount of slag in the furnace is small, a higher range of the foaming height ratio is set according to the rate of decrease of the foaming height indicating a fast value. On the other hand, when the amount of slag in the furnace is large, a lower range of the foaming height ratio is set according to the rate of decrease of the foaming height indicating a slow value. In the refining method according to this embodiment, since the Si concentration of the molten metal is controlled to a low value of 0.28 mass% or less, the amount of slag in the furnace does not increase significantly even by acid blowing, and the main factor that changes the rate of decrease of the foaming height is the amount of slag in the furnace at the start of acid blowing in the third step. Even if the amount of slag in the furnace varies, the variation in the foaming state (foaming ratio) of the slag in the furnace at the end of intermediate slag removal is generally suppressed, so that the refining method according to this embodiment can suppress the variation in the amount of slag remaining in the furnace.

[0107] That is, in the refining method according to the present embodiment, considering that the time from the stop of the acid blowing in the third step to the start of the intermediate slag discharge in the fourth step is about 10 minutes at the longest (most frequently about 3 to 5 minutes), by controlling the foaming height ratio of the slag at the stop of the acid blowing in the second step to satisfy the above formula (2), even if the amount of slag in the furnace fluctuates, the variation in the amount of slag remaining in the furnace is reduced, and it becomes possible to stably discharge a large amount of slag when the slag is discharged intermediately. Furthermore, since it becomes possible to stably discharge a large amount of slag during intermediate slag discharge, it becomes possible to suppress the variation in the amount of slag remaining in the converter. In addition, by performing control to satisfy the above formula (2), it becomes possible to suppress the variation in the amount of slag remaining among a plurality of charges.

[0108] In the refining method according to this embodiment, it is preferable to use a microwave level meter to measure the height of the forming, as in the first embodiment. The device configuration and method of use of the microwave level meter, and the effects obtained thereby are the same as those in the first embodiment, so detailed explanations will be omitted below.

[0109] [Other conditions in the third step] In the third step, other conditions such as the end temperature of the molten iron and the acid blowing time are also similar to those in the first embodiment, and therefore detailed description thereof will be omitted below.

[0110] The refining method according to the second embodiment of the present invention has been described in detail above.

[0111] As described above, according to the refining method of the second embodiment of the present invention, it is possible to discharge a large amount of slag when performing intermediate draining of the slag generated after the refining process (e.g., de-P process) of the molten metal in the converter-type vessel, regardless of the amount of slag in the furnace before the start of the third step. As a result, it is possible to further reduce the amount of rephosphorization during the de-C process performed after the intermediate draining. In addition, it is possible to suppress the variation in the amount of slag remaining in the furnace after the intermediate draining.

[0112] This makes it possible to stabilize the phosphorus concentration in the molten metal after the de-P treatment, and makes it possible to stably produce low-phosphorus steel with a P content of, for example, 100 ppm or less. EXAMPLES

[0113] The refining method according to the present invention will be specifically described below with reference to examples. Note that the following examples are merely examples of the refining method according to the present invention, and the refining method according to the present invention is not limited to the following examples.

[0114] <When using a torpedo car> The molten iron was charged into a torpedo car, and a top-blowing lance was then inserted into the torpedo car, where the silicon concentration in the molten iron was reduced to 0.28% or less by injecting gaseous oxygen and quicklime powder. After the molten iron was desiliconized to a silicon concentration of 0.28% or less, the molten iron was tapped from the torpedo car into a molten iron ladle, and then charged from the molten iron ladle into a top-bottom blown converter-type refining furnace as shown in Figure 1. Before charging into the converter, the slag generated during the decarbonization process of the previous charge was left in the refining furnace, and the amount of slag in the furnace was adjusted to be within the range of 20 to 40 kg / t-STEEL or 20 to 70 kg / t-STEEL.

[0115] <When using a refining furnace> Molten iron was charged into a top-and-bottom blowing converter-type refining furnace as shown in Figure 1, and the top blowing lance located above the throat was lowered to blow oxygen-containing gas such as oxygen gas or air into the molten iron. At the same time, auxiliary raw materials were blown from the top of the converter, including sintered ore, iron ore, dust and other iron oxide sources, limestone and quicklime as refining agents, slag and other lime raw materials recovered after discharge in the decarbonization process, agglomerate slag and Al. 2 O 3 Aluminum powder etc. 2 O 3 Raw materials and dolomite, a refractory protection material, were added. At this time, in order to increase the reaction rate, oxidizing gases oxygen and air were blown in from the inner tube at the bottom of the converter, and cooling gases LPG, nitrogen, and CO were blown in from the outer tube. 2 The molten pig iron and molten steel in the converter were constantly stirred. The basicity was adjusted to within the range of 0.8 to 1.5, foaming was induced, and the refining furnace was tilted to drain the slag from the throat. The silicon concentration in the molten pig iron after slag draining was always kept below 0.28%. The amount of slag discharged during slag draining was measured in a slag drain ladle, and the amount of slag remaining in the furnace after slag draining was adjusted to be within the range of 20 to 40 kg / t-STEEL or 20 to 70 kg / t-STEEL.

[0116] In each of the above two patterns of the second process, a refining furnace with a capacity of 350 tons was used. A plurality of double-tube tuyeres were installed at the bottom of the refining furnace. Molten pig iron was charged into the refining furnace in an amount ranging from 300 to 330 tons. The composition of the molten pig iron was as shown in Table 1 below, with the remainder being Fe and impurities.

[0117] <3rd process> The molten metal and slag obtained by any of the above methods were subjected to a deP treatment by lowering a top blowing lance located above the furnace throat and blowing an oxygen-containing gas such as oxygen gas or air into the molten metal.

[0118] In the refining furnace, since the silicon concentration of the molten metal is low, the desiliconization and dephosphorization reactions proceed in the furnace by blowing oxygen, and the SiO 2 and P 2 O 5 At this time, some of the injected oxygen reacts with the C in the molten iron to form CO and CO 2 These bubbles caused foaming of the slag at the end of the phosphorus treatment.

[0119] The slag composition in the third process is the aluminum from the lime raw material and agglomerate slag added in the second process. 2 O 3 The basicity was adjusted to be between 0.8 and 1.5 by adjusting the amount of the source used. Note that the specific values ​​shown in Table 1 below were measured by ICP emission spectrometry.

[0120] In the third step, the height of the foamed slag was constantly measured using a microwave level meter installed in the sublance hole located at the top of the converter. When the foamed slag condition satisfied the above formula (1) (in the case of Table 1 below) or formula (2) (in the case of Table 2 below), blowing was stopped and the top lance was raised.

[0121] <4th process> After that, the refining furnace was tilted to discharge the slag from the throat, thereby carrying out intermediate slag draining. The slag was discharged into a slag pot installed under the refining furnace. The angle at which the slag started to flow out after tilting the refining furnace was recorded as the intermediate slag draining start angle. The furnace was returned to a vertical position just before the molten iron in the furnace flowed out, completing the intermediate slag draining.

[0122] <5th process> After intermediate slag removal was completed, the top blowing lance was lowered again to blow oxygen-containing gas into the molten metal, and at the same time, quicklime and limestone, which are refining agents, were added to make the slag basicity 3.0 or higher and perform the decarbonization process. After the decarbonization process, the refining furnace was tilted and the molten steel was removed from the tapping hole into a ladle, completing the refining process.

[0123] <Method for measuring the amount of slag remaining in the furnace> The amount of slag in the furnace was calculated based on the amount of flux added, the Si concentration in the molten iron, and the slag composition. The amount of slag discharged was obtained from a weighing scale installed in the slag ladle, and the amount of slag remaining in the furnace was calculated by calculating the difference between the calculated total slag amount and the value obtained from the weighing scale.

[0124] <Evaluation criteria in Table 1, which is a test example corresponding to the first embodiment> In Table 1, which is a test example corresponding to the first embodiment, a grade of "A" was given when the amount of residual slag in the furnace was less than 19 kg / t and the P concentration of the molten iron after the deP treatment was 0.03 mass% or less, and a grade of "B" was given when the amount of residual slag in the furnace was 19 kg / t or more or the P concentration of the molten iron after the deP treatment exceeded 0.03 mass%.

[0125] The reason for adopting the threshold value of 19 kg / t as the judgment criterion is as follows: In the present invention, the minimum value of the slag amount before intermediate slag disposal is set to a small value of 20 kg / t, and the smaller value of 19 kg / t is adopted as the threshold value.

[0126] <Evaluation criteria in Table 2, which is a test example corresponding to the second embodiment> In Table 2, which is a test example corresponding to the second embodiment, 20 charges of operation were carried out within a specific range of molten iron composition, the amount of residual slag was measured, and the minimum and maximum values ​​of the amount of residual slag were evaluated. The difference between the maximum and minimum values ​​was then taken as a representative value of the variation.

[0127] Since the variation depends on the amount of slag in the furnace before intermediate slag removal, the following two evaluation criteria were set according to the amount of slag in the furnace.

[0128] [When the amount of slag in the furnace before intermediate slag removal is 20-40kg / t or less] Rating "A": Variation is 25% or less of the amount of slag in the furnace before intermediate slag removal (the smallest amount among 20 charges) Grade "B": The variation exceeds 25% of the amount of slag in the furnace before intermediate draining (the smallest amount of 20 charges)

[0129] [When the amount of slag in the furnace before intermediate slag removal is more than 40kg / t and less than 70kg / t] Rating "A": Variation is 10kg / t or less Grade "B": Variation exceeds 10kg / t

[0130] The results obtained are summarized in Tables 1 and 2 below. In Table 2 below, the notation "xy" indicates that the numerical value in the corresponding column was within the range of "greater than or equal to x and less than or equal to y."

[0131] [Table 1]

[0132] As is clear from Table 1 above, for Nos. 1 to 8, which are within the range of the present invention, the amount of slag remaining in the furnace was less than 19 kg / t.

[0133] On the other hand, in No. 9, where the Si concentration in the molten iron exceeded 0.28%, the P concentration in the molten iron exceeded 0.03 when blowing was stopped, and the desired deP treatment could not be achieved.

[0134] In No. 10, where blowing was stopped when the foaming height ratio was below the lower limit, the foaming height decreased significantly between the end of blowing and the start of intermediate slag removal, and the amount of slag remaining in the furnace became excessive.

[0135] In No. 11, where the basicity was below the lower limit of 0.8, excessive slopping occurred during blowing, and the planned blowing could not be carried out. In No. 12, where the basicity exceeded the upper limit of 1.5, the slag could not be foamed due to poor slag formation of the added flux, and the slag could not be removed even when intermediate slag removal was performed.

[0136] [Table 2]

[0137] In addition, when the operation was carried out within the range shown in Table 2 above, regardless of the amount of slag, as long as it was within the range of the slag composition and forming height ratio specified in the second embodiment, the evaluation of the difference between the maximum value and the minimum value was graded "A," and the variation in the amount of slag remaining in the furnace after intermediate slag removal was suppressed.

[0138] On the other hand, when the operation was stopped at a value where the foaming height ratio exceeded the upper limit, excessive slag was removed in the intermediate slag removal, and the variation in the amount of slag remaining in the furnace was given a rating of "B," and the variation in the amount of slag remaining in the furnace could not be suppressed.

[0139] In both Tables 1 and 2, the amount of rephosphorization and the amount of quicklime charged during decarburization were able to obtain the effects of the present invention according to the amount of residual slag and the degree of variation in the amount of residual slag.

[0140] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.

Claims

1. A refining method in a top blowing refining process for refining molten iron using a converter-type vessel, comprising the steps of: A first step of supplying an oxidizing agent to the molten iron to perform at least a desiliconization treatment on the molten iron; a second step of storing the molten metal and slag from the first step in the converter-type vessel and adjusting the amount of the slag to 20 to 40 kg / t-steel; A third step of blowing oxygen into the converter-type vessel to dephosphorize the molten metal and foam the slag; A fourth step of performing intermediate slag removal by tilting the converter-type vessel to remove the slag from the throat of the converter-type vessel; A fifth step of performing a top-blowing refining process in which flux is added into the converter-type vessel after the intermediate slag removal and a decarbonization process is performed on the molten metal; Including, The Si concentration of the molten metal at the end of the first step is 0.28 mass% or less, The CaO concentration (unit: mass%) of the slag at the time of stopping the acid blowing in the third step was calculated by the following formula: 2 The basicity divided by the concentration (unit: mass%) is 0.8 or more and 1.5 or less, In the third step, a height of the foaming is measured, and the height of the foaming when the acid blowing is stopped before the intermediate slag removal satisfies the following formula (1): 0.65-2.90×(amount of slag before starting acid blowing in the third step (unit: kg / t-STEEL)) / 1000≦foaming height ratio when acid blowing is stopped (Equation (1)) Here, in the above formula (1), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel.

2. A refining method in a top blowing refining process for refining molten iron using a converter-type vessel, comprising the steps of: A first step of supplying an oxidizing agent to the molten iron to perform at least a desiliconization treatment on the molten iron; A second step of storing the molten metal and slag from the first step in the converter-type vessel and adjusting the amount of the slag to 20 to 70 kg / t-steel; A third step of blowing oxygen into the converter-type vessel to dephosphorize the molten metal and foam the slag; A fourth step of performing intermediate slag removal by tilting the converter-type vessel to remove the slag from the throat of the converter-type vessel; A fifth step of performing a top-blowing refining process in which flux is added into the converter-type vessel after the intermediate slag removal and a decarbonization process is performed on the molten metal; Including, The Si concentration of the molten metal at the end of the first step is 0.28 mass% or less, The CaO concentration (unit: mass%) of the slag at the time of stopping the acid blowing in the third step was calculated by the following formula: 2 The basicity divided by the concentration (unit: mass%) is 0.8 or more and 1.5 or less, In the third step, a height of the foaming is measured, and the height of the foaming when the acid blowing is stopped before the intermediate slag removal satisfies the following formula (2): 0.65-2.90×(amount of slag before starting acid blowing in the third step (unit: kg / t-STEEL)) / 1000≦foaming height ratio when acid blowing is stopped≦0.87-2.90×(amount of slag before starting acid blowing in the third step (unit: kg / t-STEEL)) / 1000 ...Equation (2) Here, in the above formula (2), the foaming height ratio is the ratio of the measured foaming height to the height of the in-furnace freeboard in the converter-type vessel.

3. The refining method according to claim 1 or 2, wherein a microwave level meter is used to measure the height of the foam in the third step.

4. The refining method according to any one of claims 1 to 3, wherein the molten slag generated after the fifth step is left partially in the furnace, and the left molten slag is used to adjust the amount of the slag in the second step of the next charge.

5. The refining method according to any one of claims 1 to 3, wherein the solidified slag obtained by cooling and solidifying the molten slag generated after the fifth step is used to adjust the amount of the slag in the second step of another charge.

Citation Information

Patent Citations

  • Converter refining method

    JP1995018318A

  • Method for removing slag in converter

    JP2004323959A

  • Method for manufacturing molten steel

    JP2014169492A

  • Refining method of molten iron

    JP2016029212A

  • Slag height measuring device, slag height measuring method and preliminary treatment method of hot pig iron

    JP2016180126A