Method for producing perfluoroalkyne compound

The method optimizes catalysts like fluorinated chromium oxide and controlled water content to enhance perfluoroalkyne production efficiency by improving conversion rates and reducing by-product formation and catalyst deterioration.

JP7568937B2Active Publication Date: 2024-10-17DAIKIN INDUSTRIES LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021131386
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-16
Filing Date
2021-08-11
Publication Date
2024-10-17
Estimated Expiration
2039-10-08

AI Technical Summary

Technical Problem

Existing methods for producing perfluoroalkyne compounds suffer from low reaction conversion rates, high production of fluoroalkene by-products, and catalyst deterioration, limiting their efficiency and longevity.

Method used

A method involving the use of specific catalysts, such as fluorinated chromium oxide, fluorinated alumina, and fluorinated silica alumina, with optimized pore volumes and contact times, along with controlled water content in the reaction system, to enhance the selectivity and reduce catalyst deterioration during the isomerization of perfluoroalkadiene to perfluoroalkyne.

Benefits of technology

The method achieves high conversion rates and high selectivity for perfluoroalkyne production while minimizing fluoroalkene by-products and reducing catalyst degradation, thereby increasing the catalyst's lifespan and economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568937000023
    Figure 0007568937000023
  • Figure 0007568937000024
    Figure 0007568937000024
  • Figure 0007568937000025
    Figure 0007568937000025
Patent Text Reader

Abstract

To provide a method which gives high reaction conversion, can give a perfluoroalkyne compound with high selectivity, and hardly produces a fluoroalkene compound as a byproduct, and also to provide a method for producing a perfluoroalkyne compound which can reduce deterioration of a catalyst.SOLUTION: A method comprises: setting a contact time of a catalyst and the perfluoroalkadiene compound to 30 seconds or less using a catalyst which comprises a catalyst selected from (a) a catalyst containing a prescribed element(s), (b) a catalyst containing at least two kinds of prescribed elements, (c) a fluorinated prescribed metal oxide(s) whose pore volume is in a prescribed range, (d) a metal oxide(s) fluorinated by a prescribed compound(s), and (e) a catalyst obtained by fluorinating a prescribed metal oxide(s) whose pore volume is in a prescribed range, or a prescribed element(s): or setting a moisture content in the reaction system in a prescribed range at at least one point from the start of the reaction to the end of the reaction.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to a method for producing perfluoroalkyne compounds. [Background technology]

[0002] Perfluoroalkyne compounds are compounds that are expected to be used as dry etching gases for semiconductors, as well as various refrigerants, foaming agents, heat transfer media, etc., and are compounds that contain one carbon-carbon triple bond. It is a thing.

[0003] A known method for producing this perfluoroalkyne compound is the isomerization reaction of hexafluorobutadiene. For example, in Patent Document 1, hexafluorobutyne is obtained by isomerizing hexafluorobutadiene using halogenated alumina. In addition, in Patent Document 2, hexafluorobutyne is obtained from hexafluorocyclobutene using sodium fluoride or a mixture containing sodium fluoride as an isomerization catalyst. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2012-001448 [Patent Document 2] Japanese Patent Application Laid-Open No. 2014-058488 Summary of the Invention [Problem to be solved by the invention]

[0005] The present disclosure aims to provide a method for producing a perfluoroalkyne compound with high conversion and high selectivity, while minimizing the by-production of a fluoroalkene compound. Another object of the present disclosure is to provide a method for producing a perfluoroalkyne compound with reduced catalyst degradation. [Means for solving the problem]

[0006] The present disclosure encompasses the following configurations.

[0007] Item 1. A method for producing a perfluoroalkyne compound, A step of reacting a perfluoroalkadiene compound in the presence of a catalyst to obtain a perfluoroalkyne compound. The following (A) to (G): (A) The catalyst contains at least one catalyst selected from the group consisting of catalysts containing transition metal elements and catalysts containing at least two elements belonging to Groups 3 to 14 of the periodic table; (B) The catalyst contains at least one element belonging to Groups 3 to 14 of the periodic table. death, the contact time between the catalyst and the perfluoroalkadiene compound is 30 seconds or less; (C) The catalyst comprises a fluorinated chromium oxide having a pore volume of 0.08 mL / g or more, a fluorinated alumina having a pore volume of 0.35 mL / g or more, and a fluorinated silica having a pore volume of 0.50 mL / g or more. containing at least one catalyst selected from the group consisting of silica and alumina, (D) the catalyst contains a fluorinated metal oxide having a pore volume of 0.35 mL / g or more; (E) The catalyst is a hydrofluorocarbon, a hydrochlorofluorocarbon, and a chlorofluorocarbon. At least one compound selected from the group consisting of fluorocarbons and a metal oxide containing a metal oxide fluorinated by reacting (F) The catalyst is a chromium oxide having a pore volume of 0.10 mL / g or more, an alkali metal ion having a pore volume of 0.45 mL / g or more, At least one selected from the group consisting of lumina, and silica alumina having a pore volume of 0.50 mL / g or more. containing at least one fluorinated metal oxide catalyst, (G) Perfluoroalkadiene at least partially from the start of the reaction to the end of the reaction The mass of the compound is used as the standard (100 mass%), and the water content in the reaction system is 30 mass ppm or less. reacting the perfluoroalkadiene compound; A manufacturing method that satisfies any of the above.

[0008] Item 2. The perfluoroalkyne compound is represented by the general formula (1): CR 1 2nd Round 2 -C≡C-CR 3 R 4 2(1) [In the formula, R 1 ~R 4 and are the same or different and represent a fluorine atom or a perfluoroalkyl group.

[0009] Item 3. The perfluoroalkadiene compound is General formula (2): CR 1 2=CR 2 -CR 3 =CR 4 2(2) [In the formula, R 1 ~R 4 and are the same or different and represent a fluorine atom or a perfluoroalkyl group.

[0010] Item 4. A catalyst that satisfies the above (A) or (B) and contains at least one transition metal element belonging to Groups 4 to 6 of the periodic table, and a catalyst that contains at least one transition metal element belonging to Groups 4 to 6 and Groups 13 to 14 of the periodic table. 4. The method according to any one of items 1 to 3, wherein the catalyst is at least one selected from the group consisting of catalysts containing at least two elements belonging to the group A, B, C, and D.

[0011] Item 5. The production method according to any one of Items 1 to 4, wherein the condition (A) or (B) is satisfied and the catalyst is at least one catalyst selected from the group consisting of an optionally fluorinated chromium oxide catalyst, an optionally fluorinated titanium oxide catalyst, an optionally fluorinated zirconia catalyst, and an optionally fluorinated silica-alumina catalyst.

[0012] Item 6. The above (D) is satisfied, and the metal constituting the fluorinated metal oxide is Item 4. The method according to any one of Items 1 to 3, wherein at least one element belonging to Groups 3 to 14 of the periodic table is contained.

[0013] Item 7. The method according to any one of Items 1 to 3, wherein the condition (E) is satisfied and the pore volume of the metal oxide before fluorination is 0.45 mL / g or more.

[0014] Item 8. A metal that satisfies (E) and constitutes the metal oxide before being fluorinated Item 8. The method according to Item 1, 2, 3 or 7, wherein the metal oxide contains at least one element belonging to Groups 3 to 14 of the periodic table.

[0015] Item 9. The production method according to any one of Items 1 to 3, wherein the condition (G) is satisfied and the catalyst contains at least one element belonging to Groups 3 to 14 of the periodic table.

[0016] Item 10. The method according to any one of Items 1 to 9, wherein the reaction of the perfluoroalkadiene compound is carried out in a gas phase.

[0017] Item 11. Item 1, wherein the reaction of the perfluoroalkadiene compound is carried out at 170°C or higher. The manufacturing method according to any one of items 1 to 10.

[0018] Item 12. The production method according to any one of Items 1 to 11, wherein a perfluorocycloalkene compound is also produced in addition to the perfluoroalkyne compound by the reaction of the perfluoroalkadiene compound.

[0019] Item 13. The perfluorocycloalkene compound, Formula (3):

[0020] [ka]

[0021] [In the formula, R 1 ~R 4 is the same as above.] Item 13. The method according to item 12, wherein the compound is a perfluorocycloalkene compound represented by the formula:

[0022] Item 14. A method for producing a perfluoroalkyne compound, Item 14. A production method comprising a step of obtaining the perfluoroalkadiene compound by using a perfluorocycloalkene compound produced as a by-product by the production method according to Item 12 or 13 as a substrate.

[0023] Item 15. The perfluoroalkyne compound is represented by the general formula (1): CR 1 2nd Round 2 -C≡C-CR 3 R 4 2(1) [In the formula, R 1 ~R 4 and are the same or different and represent a fluorine atom or a perfluoroalkyl group.

[0024] Section 16. General formula (1): CR 1 2nd Round 2 -C≡C-CR 3 R 4 2(1) [In the formula, R 1 ~R 4 and each may be the same or different and represent a fluorine atom or a perfluoroalkyl group. General formula (3):

[0025] [ka]

[0026] [In the formula, R 1 ~R 4 is the same as above.] A composition containing a perfluorocycloalkene compound represented by the formula: The total amount of the composition is taken as 100 mol %, and the perfluoroalkyne compound represented by the general formula (1) The content of the composition is 40 to 99.999 mol %.

[0027] Item 17. The composition according to Item 16, which is used as an etching gas or a building block for organic synthesis.

[0028] Item 18. A catalyst used to react a perfluoroalkadiene compound to obtain a perfluoroalkyne compound, comprising the following (C) to (D): (C) Fluorinated chromium oxide with a pore volume of 0.08 mL / g or more, and a pore volume of 0.35 mL / g or more Contains at least one selected from the group consisting of fluorinated alumina and fluorinated silica alumina having a pore volume of 0.50 mL / g or more; (D) containing a fluorinated metal oxide having a pore volume of 0.35 mL / g or more; A catalyst that satisfies one of the following criteria.

[0029] Item 19. The above (D) is satisfied, and the metal constituting the fluorinated metal oxide is Item 19. The catalyst according to item 18, comprising at least one element belonging to groups 3 to 14 of the periodic table.

[0030] Item 20. A method for producing a catalyst used to react a perfluoroalkadiene compound to obtain a perfluoroalkyne compound, comprising the following (E) to (F): (E) Hydrofluorocarbons, hydrochlorofluorocarbons and chlorofluorocarbons and reacting at least one compound selected from the group consisting of carbon and a metal oxide. fluorinating the metal oxide by (F) chromium oxide having a pore volume of 0.10 mL / g or more, alumina having a pore volume of 0.45 mL / g or more, and At least one metal selected from the group consisting of silica alumina having a pore volume of 0.50 mL / g or more Fluorinating the oxide A manufacturing method comprising:

[0031] Item 21. The method according to Item 20, wherein (E) is satisfied and the pore volume of the metal oxide before fluorination is 0.45 mL / g or more.

[0032] Item 22. A metal oxide that satisfies (E) and is not fluorinated. Item 22. The method according to item 20 or 21, wherein the group includes at least one element belonging to groups 3 to 14 of the periodic table. [Effects of the Invention]

[0033] According to the present disclosure, it is possible to provide a production method that is less likely to produce a fluoroalkene compound as a by-product, has a high reaction conversion rate, and is capable of obtaining a perfluoroalkyne compound with high selectivity. Furthermore, according to the present disclosure, it is also possible to provide a production method for a perfluoroalkyne compound that is capable of reducing catalyst degradation. [Brief explanation of the drawings]

[0034] [Figure 1] 1 shows the relationship between reaction time and conversion when a fluorinated alumina catalyst is used. [Figure 2] 1 shows the relationship between the pore volume before fluorination and the deterioration rate when a fluorinated alumina catalyst is used. [Figure 3] 1 shows the relationship between the pore volume after fluorination and the deterioration rate when a fluorinated alumina catalyst is used. DETAILED DESCRIPTION OF THE INVENTION

[0035] In this specification, the term "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of." Furthermore, in this specification, when a numerical range is expressed as "A to B," it means A or more and B or less.

[0036] 1. Catalyst and its manufacturing method The catalyst of the present disclosure is a catalyst used to react a perfluoroalkadiene compound to obtain a perfluoroalkyne compound, and is selected from the following (C) to (D): (C) Fluorinated chromium oxide with a pore volume of 0.08 mL / g or more, and a pore volume of 0.35 mL / g or more Contains at least one selected from the group consisting of fluorinated alumina and fluorinated silica alumina having a pore volume of 0.50 mL / g or more; (D) containing a fluorinated metal oxide having a pore volume of 0.35 mL / g or more; Satisfy one of the following.

[0037] [1-1] Catalyst and its manufacturing method (Part 1) In the present disclosure, catalyst 1 (hereinafter sometimes referred to as "isomerization catalyst 1") used to obtain a perfluoroalkyne compound by reacting (isomerization reaction) a perfluoroalkadiene compound contains at least one selected from the group consisting of fluorinated chromium oxide having a pore volume of 0.08 mL / g or more, fluorinated alumina having a pore volume of 0.35 mL / g or more, and fluorinated silica-alumina having a pore volume of 0.50 mL / g or more. Satisfies requirement (C). The pore volume is the smallest among the conventionally used isomerization catalysts. It is not optimized, and it is unclear what pore volume is being used. In the present disclosure, by using fluorinated metal oxides each having a specific pore volume, the conversion rate of the reaction can be increased, it is easy to reduce the deterioration of the catalyst, and the deterioration of the catalyst can be suppressed even when the isomerization reaction is carried out for a long time. Therefore, when the catalyst of the present disclosure is adopted, the replacement frequency can be lengthened, which is economical.

[0038] The chromium oxide catalyst is not particularly limited, but when chromium oxide is represented as CrO m it is preferably 1 < m < 3, more preferably 1.2 < m < 2, and even more preferably 1.3 < m < 1.8. Also, when chromium oxide is represented as CrO m ·nH2O, it may be hydrated so that the value of n is 3 or less, particularly 1 to 1.5.

[0039] An example of a method for synthesizing a chromium oxide catalyst is shown below.

[0040] First, a precipitate of chromium hydroxide can be obtained by mixing an aqueous solution of a chromium salt (chromium nitrate, chromium chloride, chrome alum, chromium sulfate, etc.) and aqueous ammonia. The physical properties of chromium hydroxide can be controlled by the reaction rate of the precipitation reaction at this time. The reaction rate is preferably fast. The reaction rate depends on the reaction solution temperature, the method of mixing aqueous ammonia (mixing rate), the stirring state, etc.

[0041] After filtering and washing this precipitate, it can be dried. Drying can be carried out, for example, in air at 70 to 200 °C for 1 to 100 hours. The catalyst at this stage may be referred to as the state of chromium hydroxide. Next, this catalyst can be crushed. From the viewpoints of pellet strength, catalyst activity, etc., the crushed powder (for example, the particle size is 1000 μm or less, particularly 95% of the particle size product of 46 to 1000 μm) It is preferable to adjust the precipitation reaction rate so that the powder density is 0.6 to 1.1 g / ml, preferably 0.6 to 1.0 g / ml. The specific surface area of ​​the powder (specific surface area by the BET method) is, for example, 100 m under degassing conditions at 200°C for 80 minutes. 2 / g or more is preferable, and 120m 2 The upper limit of the specific surface area is, for example, 220 m 2 / g.

[0042] This chromium hydroxide powder can be mixed with 3% by weight or less of graphite, if necessary, and formed into pellets using a tablet press. The size and strength of the pellets can be adjusted as needed.

[0043] The molded catalyst can be calcined in an inert atmosphere, for example, in a nitrogen stream, to form amorphous chromium oxide. The calcination temperature is preferably 360° C. or higher, and from the viewpoint of suppressing crystallization, a temperature of 380 to 460° C. The calcination time can be, for example, 1 to 5 hours.

[0044] The specific surface area of ​​the calcined catalyst is, for example, 170 m 2 / g or more is preferable , 180m 2 / g or more is more preferable, and 200m 2 The upper limit of the specific surface area is usually 240 m 2 / g is preferable, and 220m 2 / g is more preferable.

[0045] Examples of the alumina catalyst include α-alumina and activated alumina. Lumina includes ρ-alumina, χ-alumina, κ-alumina, η-alumina, and pseudo-γ-alumina. Examples of suitable alumina include alumina, γ-alumina, σ-alumina, and θ-alumina.

[0046] A silica-alumina catalyst can also be used as a composite oxide. The silica-alumina catalyst is a composite oxide catalyst containing silica (SiO2) and alumina (Al2O3). For example, the silica content is 20 to 90 mass%, particularly 50 to 80 mass%, based on the total amount of alumina being 100 mass%. % by weight of catalyst can be used.

[0047] In the present disclosure, the above-described metal oxide catalyst is fluorinated to obtain a fluorinated metal oxide catalyst. Fluorination not only enhances activity but also reduces catalyst degradation, and adjusting the pore volume can suppress catalyst degradation even when the isomerization reaction is carried out over a long period of time. Therefore, the metal oxide catalyst is used as a fluorinated metal oxide catalyst. The method for fluorinating a metal oxide catalyst will be described later.

[0048] The catalyst of the present disclosure has a large pore volume, which reduces catalyst deterioration and can suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Specifically, the pore volume of each metal oxide catalyst is 0.05 mL / g or more (particularly 0.075 to 1.5 mL / g) for fluorinated chromium oxide, 0.35 mL / g or more (particularly 0.40 to 2.0 mL / g) for fluorinated alumina, and 0.5 mL / g or more (particularly 0.5 mL / g to 1.5 mL / g) for fluorinated alumina. The pore volume of the oxidized silica alumina is 0.50 ml / g or more (especially 0.55 to 2.0 ml / g). If the pore volume is smaller than this range, the pores where the active sites of the catalyst are present will be covered with carbon, a by-product of the reaction, or the adhered carbon will impair gas diffusion within the pores, resulting in a decrease in catalytic activity, i.e., catalyst deterioration. Furthermore, if the pore volume is too large, the catalyst manufacturing method will become complicated and the manufacturing cost will increase.

[0049] The catalyst of the present disclosure has a large pore volume as described above. The pore volume can be adjusted by the degree of fluorination of the catalyst, that is, the content of fluorine atoms. Therefore, the content of fluorine atoms is preferably 5.0 to 50 atomic %, and more preferably 10 to 25 atomic %, based on 100 atomic % of the total amount of the catalyst of the present disclosure.

[0050] As a method for fluorinating a metal oxide catalyst, for example, a metal oxide may be reacted with a fluorinating agent. Specifically, for example, the fluorination can be performed by passing a fluorinating agent through the metal oxide. The metal oxide in this case may be the metal oxide that constitutes the above-mentioned fluorinated metal oxide.

[0051] A large pore volume is preferred for the metal oxide catalyst before fluorination, because it increases the pore volume of the metal oxide catalyst after fluorination, thereby increasing the reaction conversion rate and reducing catalyst degradation. This facilitates the suppression of catalyst degradation even when the isomerization reaction is carried out over a long period of time. Specifically, suitable pore volumes for each metal oxide catalyst before fluorination include, for example, 0.05 mL / g or more (especially 0.075 to 1.5 mL / g) for chromium oxide, 0.45 mL / g or more (especially 0.50 to 2.5 mL / g) for alumina, and 0.40 mL / g or more (especially 0.50 to 2.0 mL / g) for silica-alumina. By maintaining the pore volume within this range, the active sites of the catalyst are less likely to be covered by carbon, a by-product of the reaction, and the deposited carbon is less likely to inhibit gas diffusion within the pores. This maintains the catalytic activity, i.e., inhibits catalyst degradation, and simplifies the catalyst production process.

[0052] In this case, the fluorinating agent may be, for example, hydrofluorocarbon (R23: trifluorocarbon Examples of fluorinating agents include chlorofluoromethane (R32: difluoromethane, R41: monofluoromethane), hydrochlorofluorocarbons (R22: chlorodifluoromethane, R21: dichloromonofluoromethane), and chlorofluorocarbons (R13: chlorotrifluoromethane, R11: trichloromonofluoromethane). Compared to hydrogen fluoride, these fluorinating agents tend to increase the pore volume of the fluorinated metal oxide catalyst, making it easier to reduce catalyst deterioration and to inhibit catalyst deterioration when the isomerization reaction is carried out over a long period of time. These fluorinating agents can be used alone or in combination of two or more.

[0053] The fluorination conditions are not particularly limited, but from the viewpoint of easily reducing catalyst deterioration and easily suppressing catalyst deterioration even when the above isomerization reaction is carried out for a long period of time, the temperature is preferably 50 to 600°C ( The pressure is preferably 0 to 1000 kPa (particularly 0.1 to 500 kPa), and the time is preferably The time is preferably 0.1 to 24 hours (particularly 1 to 12 hours), and it is preferable to adjust the content of fluorine atoms in this way so that it falls within the above range.

[0054] The perfluoroalkyne compound to be produced may be, for example, a compound represented by the general formula (1): CR 1 2nd Round 2 -C≡C-CR 3 R 4 2(1) [In the formula, R 1 ~R 4 are the same or different and represent a fluorine atom or a perfluoroalkyl group.] is preferred.

[0055] In general formula (1), R 1 ~R 4 There are no particular restrictions on the perfluoroalkyl group represented by the formula: Examples of the alkyl group include perfluoroalkyl groups having 1 to 6 carbon atoms (particularly 1 to 4 carbon atoms), such as trifluoromethyl and pentafluoroethyl groups.

[0056] In general formula (1), R 1 ~R 4 The conversion rate of the reaction, the amount of perfluoroalkyl groups obtained, From the viewpoint of the yield and selectivity of the fluorine compound, it is preferable that both of them are fluorine atoms. 1 ~R 4 may be the same or different.

[0057] From the above, the perfluoroalkyne compound represented by general formula (1) to be produced is For example, CF3C≡CCF3, CF3C≡CCF2CF3, CF3C≡CCF(CF3)2, CF3C≡CC(CF3)3, CF3CF2C≡CCF2CF3, CF3CF2C≡CCCF(CF3)2, CF3CF2C≡CC(CF3)3, (CF3)2CFC≡CCCF(CF3)2, (CF3)2CFC≡CC(CF3)3, (CF3)3CC≡CC(CF3)3, etc.

[0058] The perfluoroalkadiene compound as the substrate is, for example, a compound represented by the general formula (2): CR 1 2=CR 2 -CR 3 =CR 4 2(2) [In the formula, R 1 ~R 4 are the same or different and represent a fluorine atom or a perfluoroalkyl group.] is preferred.

[0059] In general formula (2), R 1 ~R 4 There are no particular restrictions on the perfluoroalkyl group represented by the formula: Examples of the alkyl group include perfluoroalkyl groups having 1 to 6 carbon atoms (particularly 1 to 4 carbon atoms), such as trifluoromethyl and pentafluoroethyl groups.

[0060] In general formula (2), R 1 ~R 4 The conversion rate of the reaction, the amount of perfluoroalkyl groups obtained, From the viewpoint of the yield and selectivity of the fluorine compound, it is preferable that both of them are fluorine atoms. 1 ~R 4 may be the same or different.

[0061] The perfluoroalkadienes represented by the general formula (2) that satisfy the above conditions are , For example, CF2=CFCF=CF2, CF2=CFCF=CFCF3, CF3CF=CFCF=CFCF3, CF(CF3)=CFCF=CF2, C(CF3)2=CFCF=CF2, CF(CF3)=CFCF=CF(CF3), C(CF3)2=CFCF=CF(CF3), C(CF3)2=CFCF=C(CF3)2, CF2=C(CF3)C(CF3)=CF2, etc. Lucadienes can be used alone or in combination of two or more.

[0062] The perfluoroalkadiene compounds described above can be publicly known or commercially available products, or can be synthesized according to the conventional method disclosed in JP-A-2001-192345.

[0063] [1-2] Catalyst and its manufacturing method (part 2) In the present disclosure, catalyst 2 (hereinafter sometimes referred to as "isomerization catalyst 2") used to obtain perfluoroalkyne compounds by reacting (isomerization reaction) perfluoroalkadiene compounds contains a fluorinated metal oxide having a pore volume of 0.35 mL / g or more. This catalyst satisfies the above-mentioned requirement (D). Conventionally used isomerization catalysts include In the case of the catalyst, the pore volume is not optimized, and it is unclear what pore volume is being used. In the present disclosure, by using a fluorinated metal oxide and increasing its pore volume to 0.35 mL / g or more, the conversion rate of the reaction is increased and catalyst deterioration is easily reduced, making it possible to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Therefore, when the catalyst of the present disclosure is used, the replacement frequency can be increased, which is economical.

[0064] The catalyst of the present disclosure is not particularly limited, but from the viewpoint of increasing the conversion rate of the reaction, easily reducing catalyst deterioration, and easily suppressing catalyst deterioration even when the isomerization reaction is carried out over a long period of time, the metal constituting the fluorinated metal oxide is preferably at least one element belonging to Groups 3 to 14 of the periodic table, more preferably at least one element belonging to Groups 4 to 6 and Groups 13 to 14 of the periodic table, and more preferably chromium, titanium, silicon, or the like. More preferably, the catalyst is at least one of the above-mentioned metals, aluminum, zirconium, etc. Only one type of metal element may be contained, or two or more types may be contained.

[0065] As the catalyst of the present disclosure, a fluorinated titanium oxide catalyst, a fluorinated alumina catalyst, a fluorinated silica-alumina catalyst, a fluorinated zirconia catalyst, or the like is particularly preferred, from the viewpoints that the activity of the isomerization reaction of a perfluoroalkadiene compound to a perfluoroalkyne compound is high, the conversion rate of the reaction is increased, catalyst deterioration is easily reduced, and catalyst deterioration is easily suppressed even when the isomerization reaction is carried out over a long period of time.

[0066] The titanium oxide catalyst may contain titanium dioxide as the main component, and may contain one or more non-volatile substances such as other metal oxides, hydroxides, sulfates, nitrates, phosphates, sulfides, etc. Titanium dioxide should account for 70 mass% or more of the titanium oxide catalyst. is preferred.

[0067] As titanium dioxide, anatase type titanium dioxide is particularly preferred, and the specific surface area is 5 to 100 m 2 Preferably, the catalyst has a viscosity of 1000 s / g and a pore volume of 0.2 to 0.4 ml / g. The catalyst is preferably molded into a spherical shape. Specifically, commercially available catalysts under the trade names CS-200, CS-300, CS-950, etc. (manufactured by Sakai Chemical Industry Co., Ltd.) can be suitably used.

[0068] As the alumina catalyst and silica-alumina catalyst, those described in the above [1-1] Catalyst and its production method (part 1) can be used.

[0069] The zirconia catalyst is not particularly limited as long as it contains zirconium oxide as the main component, and may contain one or more non-volatile substances such as other metal oxides, hydroxides, sulfates, nitrates, phosphates, sulfides, etc. The zirconia catalyst preferably contains 70 mass% or more of zirconia.

[0070] In the present disclosure, the above-described metal oxide catalyst is fluorinated to obtain a fluorinated metal oxide catalyst. Fluorination not only enhances activity but also reduces catalyst degradation, and adjusting the pore volume can suppress catalyst degradation even when the isomerization reaction is carried out over a long period of time. Therefore, the metal oxide catalyst is used as a fluorinated metal oxide catalyst. The method for fluorinating a metal oxide catalyst will be described later.

[0071] The catalyst of the present disclosure is preferably made large in pore volume because it is easy to reduce catalyst deterioration and to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Specifically, the pore volume of the metal oxide catalyst after fluorination is 0.35 mL / g or more, preferably 0.40 to 2.0 mL / g. The preferred pore volume of each metal oxide catalyst is, for example, The fluorinated alumina is 0.35 mL / g or more (especially 0.40 to 2.0 mL / g), and the fluorinated silica alumina is The pore volume is in this range. This makes it difficult for the active sites of the catalyst to be covered by carbon, a by-product of the reaction, and the adhered carbon is unlikely to inhibit gas diffusion within the pores, which maintains the activity of the catalyst, i.e., makes it easy to suppress catalyst deterioration, and also simplifies the method for producing the catalyst.

[0072] The degree of fluorination (i.e., the content of fluorine atoms), fluorination method, fluorinating agent, fluorination conditions, etc. of the catalyst of the present disclosure can be those described in the above [1-1] Catalyst and production method thereof (part 1).

[0073] The metal oxide catalyst before fluorination preferably has a large pore volume because it can increase the pore volume of the metal oxide catalyst after fluorination, thereby increasing the conversion rate of the reaction and easily reducing catalyst deterioration, and it is easy to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Specifically, the pore volume of the metal oxide catalyst before fluorination is preferably 0.45 mL / g or more, more preferably 0.50 to 2.5 mL / g. Note that, Suitable pore volumes are, for example, 0.45 mL / g or more (particularly 0.50 to 2.5 mL / g) for alumina, and 0.50 to 2.5 mL / g for silica. The lumina is 0.40 mL / g or more (particularly 0.50 to 2.0 mL / g). By doing so, the active sites of the catalyst are less likely to be covered by carbon, a by-product of the reaction, and the adhered carbon is less likely to inhibit gas diffusion within the pores. This makes it easier to maintain the activity of the catalyst, i.e., to suppress catalyst deterioration, and also simplifies the method for producing the catalyst.

[0074] The perfluoroalkyne compound to be produced and the perfluoroalkadiene compound as the substrate may be those described in the above [1-1] Catalyst and its production method (part 1).

[0075] 2. Catalyst manufacturing method The method for producing a catalyst according to the present disclosure is a method for producing a catalyst used to obtain a perfluoroalkyne compound by reacting a perfluoroalkadiene compound, and includes the following steps (E) to (F): (E) Hydrofluorocarbons, hydrochlorofluorocarbons and chlorofluorocarbons and reacting at least one compound selected from the group consisting of carbon and a metal oxide. fluorinating the metal oxide by (F) chromium oxide having a pore volume of 0.10 mL / g or more, alumina having a pore volume of 0.45 mL / g or more, and At least one metal selected from the group consisting of silica alumina having a pore volume of 0.50 mL / g or more Fluorinating the oxide It has one of the following.

[0076] [2-1] Catalyst manufacturing method (part 3) In the present disclosure, a perfluoroalkadiene compound is reacted (isomerized) to form a perfluoroalkadiene. Catalyst manufacturing method 3 used to obtain a fluoroalkyne compound (hereinafter referred to as "isomerization reaction") The catalyst manufacturing method (sometimes called "3") is and a metal oxide. The method includes a step of fluorinating the metal oxide by reacting the metal oxide with the catalyst. This catalyst satisfies the above-mentioned requirement (E). The pore volume is the optimum value for a catalyst for isomerization reaction that has been conventionally used. The catalyst used in the present disclosure has not been fluorinated, and it is unclear what pore volume is used. In the present disclosure, fluorination with the specific compound described above adjusts the pore volume to a predetermined range, thereby increasing the conversion rate of the reaction and facilitating a reduction in catalyst deterioration, making it possible to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Therefore, when the catalyst of the present disclosure is used, the replacement frequency can be increased, which is economical.

[0077] The metal oxide is not particularly limited, but from the viewpoint of increasing the conversion rate of the reaction, easily reducing catalyst deterioration, and easily suppressing catalyst deterioration even when the isomerization reaction is carried out over a long period of time, it is preferable that the constituent metal is, for example, an element belonging to Groups 3 to 14 of the periodic table. At least one element is preferably selected from the group 4 to 6 and the group 13 to 14 of the periodic table. At least one of these is more preferable, and examples thereof include chromium, titanium, silicon, aluminum, zirconium, etc. At least one kind is more preferable. The metal oxide may contain only one kind of the above-mentioned metal elements, or may contain two or more kinds of them.

[0078] As such metal oxides, chromium oxide catalysts, titanium oxide catalysts, alumina catalysts, silica-alumina catalysts, zirconia catalysts, and the like are particularly preferred, from the viewpoints that fluorination as described above increases the activity of the isomerization reaction from perfluoroalkadiene compounds to perfluoroalkyne compounds, further increasing the conversion rate of the reaction, and making it easy to reduce catalyst deterioration, even when the isomerization reaction is carried out over a long period of time.

[0079] As the chromium oxide catalyst, alumina catalyst, and silica-alumina catalyst, those described in the above [1-1] Catalyst and its manufacturing method (part 1) can be used, and as the titanium oxide catalyst and zirconia catalyst, those described in the above [1-2] Catalyst and its manufacturing method (part 2) can be used.

[0080] The metal oxide catalyst before fluorination as described above can have a larger pore volume after fluorination, which increases the conversion rate of the reaction and also reduces catalyst deterioration, making it easier to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Specifically, the pore volume of the metal oxide catalyst before fluorination is preferably 0.45 mL / g or more, more preferably 0.50 to 2.5 mL / g. Note that, before fluorination, Suitable pore volumes for each of the metal oxide catalysts include, for example, 0.05 mL / g or more (particularly 0.075 to 1.5 mL / g) for chromium oxide, 0.45 mL / g or more (particularly 0.50 to 2.5 mL / g) for alumina, and 0.40 mL / g or more (particularly 0.50 to 2.0 mL / g) for silica alumina. By setting the pore volume within this range, the active sites of the catalyst are less likely to be covered by carbon, a by-product of the reaction, and the adhered carbon is less likely to inhibit gas diffusion within the pores, maintaining the activity of the catalyst; in other words, catalyst deterioration is easily suppressed, and the catalyst production method is also simple.

[0081] In the present disclosure, the above-described metal oxide catalyst is fluorinated with a specific compound to obtain a fluorinated metal oxide catalyst. Fluorination not only enhances activity but also reduces catalyst degradation, and by adjusting the pore volume, catalyst degradation can be suppressed even when the above-described isomerization reaction is carried out over a long period of time. Therefore, the fluorinated metal oxide catalyst is used.

[0082] In the present disclosure, the method for fluorinating a metal oxide catalyst involves reacting the metal oxide with a fluorinating agent. Specifically, for example, a fluorinating agent is passed through the metal oxide to generate fluorine. It can be made into

[0083] In this disclosure, the fluorinating agent used is a hydrofluorocarbon (R23: trifluoromethane). At least one compound selected from the group consisting of chlorofluoromethane (R32: difluoromethane, R41: monofluoromethane), hydrochlorofluorocarbons (R22: chlorodifluoromethane, R21: dichloromonofluoromethane), and chlorofluorocarbons (R13: chlorotrifluoromethane, R11: trichloromonofluoromethane) is used. Compared with hydrogen chloride, the pore volume of the fluorinated metal oxide catalyst is larger, which reduces catalyst deterioration and prevents catalyst deterioration when the isomerization reaction is carried out for a long period of time. These fluorinating agents can be used alone or in combination of two or more.

[0084] The fluorination conditions are not particularly limited, but from the viewpoint of easily reducing catalyst deterioration and easily suppressing catalyst deterioration even when the above isomerization reaction is carried out for a long period of time, the temperature is preferably 50 to 600°C ( The pressure is preferably 0 to 1000 kPa (particularly 0.1 to 500 kPa), and the time is preferably The time is preferably 0.1 to 24 hours (particularly 1 to 12 hours).

[0085] The catalyst obtained in this manner has a large pore volume, which reduces catalyst deterioration, and can suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Specifically, the pore volume of the metal oxide catalyst after fluorination is preferably 0.35 mL / g or more, more preferably 0.40 to 2.0 mL / g. It is preferable that the pore volume of each metal oxide catalyst is, for example, 0.05 mL / g or more (particularly 0.075 to 1.5 mL / g) for fluorinated chromium oxide, 0.35 mL / g or more (particularly 0.40 to 2.0 mL / g) for fluorinated alumina, and 0.50 mL / g or more (particularly 0.55 to 2.0 mL / g) for fluorinated silica-alumina. By setting the pore volume within this range, the active sites of the catalyst are less likely to be covered by carbon, a by-product of the reaction, and the gas diffusion within the pores is less likely to be hindered by the deposited carbon, maintaining the activity of the catalyst, i.e., easily suppressing catalyst deterioration, and also simplifying the method of producing the catalyst.

[0086] The catalyst obtained in this manner has a large pore volume, but the pore volume can also be adjusted by the degree of fluorination of the catalyst, that is, the content of fluorine atoms. Therefore, the total amount of the catalyst obtained after fluorination is taken as 100 atomic %, and the content of fluorine atoms is 5.0 to 50 atomic %. % is preferable, and 10 to 25 atomic % is more preferable.

[0087] The perfluoroalkyne compound to be produced and the perfluoroalkadiene compound as the substrate may be those described in the above [1-1] Catalyst and its production method (part 1).

[0088] [2-2] Catalyst manufacturing method (part 4) In the present disclosure, a method for producing a catalyst (hereinafter referred to as "method for producing a catalyst for isomerization reaction") is described. The catalyst manufacturing method (sometimes called "catalyst manufacturing method 4") is a method in which the metal oxide before fluorination is The method includes a step of fluorinating at least one metal oxide selected from the group consisting of chromium oxide having a pore volume of 0.10 mL / g or more, alumina having a pore volume of 0.45 mL / g or more, and silica-alumina having a pore volume of 0.5 mL / g or more. This catalyst satisfies the above-mentioned requirement (F). The pore volume of the catalyst used for the isomerization reaction is not optimized, and it is unclear what pore volume is used. In the present disclosure, by fluorinating metal oxides each having a specific pore volume, the conversion rate of the reaction is increased and catalyst deterioration is easily reduced, making it possible to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Therefore, when the catalyst of the present disclosure is used, the replacement frequency can be increased, which is economical.

[0089] As the chromium oxide catalyst, alumina catalyst and silica-alumina catalyst, those described in the above [1-1] Catalyst and its production method (part 1) can be used.

[0090] The metal oxide catalysts described above before fluorination are preferably those with large pore volumes, because this increases the pore volume of the resulting metal oxide catalyst after fluorination, thereby increasing the conversion rate of the reaction and reducing catalyst degradation. This prevents catalyst degradation even when the isomerization reaction is carried out over a long period of time. Specifically, the preferred pore volumes for each metal oxide catalyst before fluorination are 0.05 mL / g or more (especially 0.075 to 1.5 mL / g) for chromium oxide, 0.45 mL / g or more (especially 0.50 to 2.5 mL / g) for alumina, and 0.40 mL / g or more (especially 0.50 to 2.0 mL / g) for silica-alumina. If the pore volumes are smaller than these ranges, the pores containing the active sites of the catalyst may be covered by carbon, a by-product of the reaction, or the deposited carbon may impair gas diffusion within the pores, resulting in a decrease in catalytic activity, i.e., catalyst degradation. Moreover, if the pore volume is too large, the production method of the catalyst becomes complicated and the production cost increases.

[0091] In the present disclosure, the above-described metal oxide catalyst is fluorinated to obtain a fluorinated metal oxide catalyst. Fluorination not only enhances activity but also reduces catalyst degradation, and by adjusting the pore volume, catalyst degradation can be suppressed even when the above-described isomerization reaction is carried out over a long period of time. Therefore, the fluorinated metal oxide catalyst is used.

[0092] The fluorination method, fluorinating agent, and fluorination conditions can be those explained in the above [1-1] Catalyst and production method thereof (part 1).

[0093] The catalyst obtained in this manner has a large pore volume, which reduces catalyst deterioration and can suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time. Specifically, the pore volume of each metal oxide catalyst is, for example, 0.05 mL / g or more (particularly, 0.075 to 1.5 mL / g) for fluorinated chromium oxide, 0.35 mL / g or more (particularly, 0.40 to 2.0 mL / g) for fluorinated alumina, The fluorinated silica alumina preferably has a pore size of 0.50 ml / g or more (particularly 0.55 to 2.0 ml / g). By setting the volume within this range, the active sites of the catalyst are less likely to be covered by carbon, a by-product of the reaction, and the adhered carbon is less likely to inhibit gas diffusion within the pores. This maintains the activity of the catalyst, i.e., makes it easier to suppress catalyst deterioration, and also simplifies the method for producing the catalyst.

[0094] The catalyst obtained in this manner has a large pore volume, but the pore volume can also be adjusted by the degree of fluorination of the catalyst, that is, the content of fluorine atoms. Therefore, the total amount of the catalyst obtained after fluorination is taken as 100 atomic %, and the content of fluorine atoms is 5.0 to 50 atomic %. % is preferable, and 10 to 25 atomic % is more preferable.

[0095] The perfluoroalkyne compound to be produced and the perfluoroalkadiene compound as the substrate may be those described in the above [1-1] Catalyst and its production method (part 1).

[0096] 3. Method for producing perfluoroalkyne compounds The method for producing a perfluoroalkyne compound of the present disclosure includes: A step of reacting a perfluoroalkadiene compound in the presence of a catalyst to obtain a perfluoroalkyne compound. The following (A) to (G): (A) The catalyst contains at least one catalyst selected from the group consisting of catalysts containing transition metal elements and catalysts containing at least two elements belonging to Groups 3 to 14 of the periodic table; (B) The catalyst contains at least one element belonging to Groups 3 to 14 of the periodic table. death, the contact time between the catalyst and the perfluoroalkadiene compound represented by the general formula (2) is 30 seconds or less; (C) The catalyst comprises a fluorinated chromium oxide having a pore volume of 0.08 mL / g or more, a fluorinated alumina having a pore volume of 0.35 mL / g or more, and a fluorinated silica having a pore volume of 0.50 mL / g or more. containing at least one catalyst selected from the group consisting of silica and alumina, (D) the catalyst contains a fluorinated metal oxide having a pore volume of 0.35 mL / g or more; (E) The catalyst is a hydrofluorocarbon, a hydrochlorofluorocarbon, and a chlorofluorocarbon. At least one compound selected from the group consisting of fluorocarbons and a metal oxide containing a metal oxide fluorinated by reacting (F) The catalyst is a chromium oxide having a pore volume of 0.10 mL / g or more, an alkali metal ion having a pore volume of 0.45 mL / g or more, A catalyst containing at least one fluorinated metal oxide selected from the group consisting of lumina and silica-alumina having a pore volume of 0.50 mL / g or more. (G) Perfluoroalkadiene at least partially from the start of the reaction to the end of the reaction The mass of the compound is used as the standard (100 mass%), and the water content in the reaction system is 30 mass ppm or less. reacting the perfluoroalkadiene compound; Satisfy one of the following.

[0097] As the perfluoroalkyne compound and perfluoroalkadiene compound, those explained in the above [1-1] Catalyst and its production method (part 1) can be used.

[0098] [3-1] Method for producing perfluoroalkyne compounds (part 1) A first method for producing a perfluoroalkyne compound of the present disclosure includes: A step of reacting a perfluoroalkadiene compound in the presence of a catalyst to obtain a perfluoroalkyne compound. The catalyst is a catalyst containing a transition metal element and an element belonging to groups 3 to 14 of the periodic table. The catalyst is at least one selected from the group consisting of catalysts including at least two of the following: This production method satisfies the above-mentioned requirement (A).

[0099] Conventionally, methods for producing perfluoroalkyne compounds have used catalysts containing only one Group 13 element, such as halogenated alumina or sodium fluoride, without containing any transition metal. Only examples using catalysts containing alkali metals or catalysts containing transition metal elements have been known. According to the present disclosure, by using catalysts containing unconventional transition metal elements or catalysts containing at least two elements belonging to Groups 3 to 14 of the periodic table, the reaction conversion rate is high and perfluoroalkyne compounds can be obtained with high yield and high selectivity, thereby broadening the range of options for synthesizing perfluoroalkyne compounds. In this way, by using catalysts containing highly active transition metal elements or catalysts containing at least two elements belonging to Groups 3 to 14 of the periodic table whose activity increases when made into composite oxides, the reaction conversion rate is high and perfluorocycloalkene compounds can be obtained with high selectivity. Moreover, according to the present disclosure, unlike conventional methods, fluoroalkene compounds are less likely to be by-produced, as described below.

[0100] In the present disclosure, catalysts containing transition metal elements and catalysts containing Group 3 of the periodic table are used as catalysts for isomerization reactions. A catalyst containing at least two elements belonging to Group 14 is used. Although not particularly limited, from the viewpoint of achieving a particularly high conversion rate in the reaction and obtaining a perfluoroalkyne compound in a higher yield and with a higher selectivity, a catalyst containing at least one transition metal element belonging to Groups 4 to 6 of the periodic table, or a catalyst containing at least one transition metal element belonging to Groups 4 to 6 and Groups 13 to 14 of the periodic table is preferred. Catalysts containing at least two of the above are preferred, and catalysts containing chromium, titanium, zirconium, etc. and catalysts containing silicon and aluminum are more preferred.

[0101] As a catalyst for such an isomerization reaction, perfluoroalkadiene compounds are highly active in the isomerization reaction of perfluoroalkyne compounds, and depending on the reaction conditions, perfluoroalkadiene compounds can be easily converted into perfluoroalkyne compounds. Like quinone compounds, they also have high activity in the reaction for producing perfluorocycloalkene compounds, which are expected to be used not only as dry etching gases for semiconductors but also as various refrigerants, foaming agents, heat transfer media, etc., and therefore, preferred are chromium oxide catalysts which may be fluorinated (chromium oxide catalyst or fluorinated chromium oxide catalyst), titanium oxide catalysts which may be fluorinated (titanium oxide catalyst or fluorinated titanium oxide catalyst), zirconia catalysts which may be fluorinated (zirconia catalyst or fluorinated zirconia catalyst), silica-alumina catalysts which may be fluorinated (silica-alumina catalyst or fluorinated silica-alumina catalyst), etc.

[0102] As the chromium oxide catalyst and silica alumina catalyst, those described in the above [1-1] Catalyst and its manufacturing method (part 1) can be used, and as the titanium oxide catalyst and zirconia catalyst, those described in the above [1-2] Catalyst and its manufacturing method (part 2) can be used.

[0103] In addition, when the catalyst is fluorinated, the degree of fluorination (content of fluorine atoms), fluorination method, fluorinating agent, and fluorination conditions can be those described in the above [1-1] Catalyst and production method thereof (part 1).

[0104] These isomerization catalysts can be used alone or in combination of two or more. It is also possible.

[0105] The amount of catalyst used in the above-mentioned isomerization reaction can be a catalytic amount and is not particularly limited. However, from the viewpoint of achieving a particularly high conversion rate in the reaction and obtaining a perfluoroalkyne compound in a higher yield and with a higher selectivity, for example, the weight ratio of catalyst to the hourly supply rate of perfluoroalkadiene compound (W / F) is preferably 0.1 to 200 g·sec. / cc, more preferably 0.5 to 150 g·sec. / cc. When multiple catalysts for the isomerization reaction are used, it is preferable to adjust the total amount so that it is within the above range. The above W / F is particularly important in determining the amount of catalyst in the case of a gas-phase reaction. However, even when a liquid phase reaction is employed, the amount of fluoride used can be a catalytic amount and can be adjusted appropriately.

[0106] In the production method of the present disclosure, when reacting a perfluoroalkadiene compound, in addition to the perfluoroalkadiene compound substrate and the catalyst for the isomerization reaction, metallic nickel (particularly metallic nickel beads), activated carbon, or the like may also be used for the purpose of improving heat transfer or diluting the catalyst concentration, so that the W / F is 0.1 to 200 g sec. / cc, particularly 0.5 to 150 g sec. / cc.

[0107] The production method of the present disclosure (particularly the reaction of a perfluoroalkadiene compound) can be carried out in a liquid phase, but is preferably carried out in a gas phase, particularly in a gas phase continuous flow system using a fixed-bed reactor. This allows for further simplification of the equipment, operation, etc. compared to when carried out in a liquid phase, and also allows for the production of a perfluoroalkyne compound in a higher yield and with a higher selectivity compared to when carried out in a batch system.

[0108] In the production method of the present disclosure, the reaction of the perfluoroalkadiene compound is preferably carried out under heating. Specifically, it is preferable to heat the system after adding the perfluoroalkadiene compound as a substrate and the catalyst for the isomerization reaction. The heating temperature at this time is preferably 170°C or higher (particularly 170 to 400°C), more preferably 180 to 280°C, from the viewpoint of achieving a particularly high conversion rate in the reaction and being able to obtain the perfluoroalkyne compound in a higher yield and with a higher selectivity. stomach.

[0109] In the production method of the present disclosure, the contact time (reaction time) between the catalyst and the perfluoroalkadiene compound is not particularly limited, and from the viewpoint of achieving a particularly high conversion rate in the reaction and obtaining the perfluoroalkyne compound in a higher yield and with a higher selectivity, the contact time is preferably 1 to 100 seconds, and more preferably 2 to 30 seconds. More preferable.

[0110] In the production method of the present disclosure, the atmosphere in which the perfluoroalkadiene compound is reacted is not particularly limited, and for example, the reaction atmosphere is preferably an inert gas atmosphere (nitrogen gas atmosphere, argon gas atmosphere, etc.).

[0111] In the production method of the present disclosure, not only perfluorocycloalkene compounds but also perfluorocycloalkene compounds can be produced. The perfluorocycloalkene compounds include those represented by the general formula (3):

[0112] [ka]

[0113] [In the formula, R 1 ~R 4 is the same as above.] The perfluorocycloalkene compound is represented by the following formula: The details of the perfluorocycloalkene compound will be described later.

[0114] Therefore, after the reaction is completed, if necessary, purification treatment can be carried out in accordance with a conventional method to obtain a perfluoroalkyne compound.

[0115] Furthermore, the perfluorocycloalkene compound produced as a by-product by the production method of the present disclosure can be purified according to a conventional method as needed, and then used as a substrate to produce a perfluoroalkyne compound. The method and conditions for this can be those described in Patent Document 2 (JP 2014-058488 A). Preferred specific examples can also be used.

[0116] Specifically, a perfluorocycloalkene compound can be used as a substrate and isomerized using an isomerization catalyst to obtain a perfluoroalkyne compound. This process can be carried out in a gas phase, particularly in a gas phase continuous flow system using a fixed bed reactor, but can also be carried out by a batch reaction.

[0117] As a catalyst for the isomerization reaction, it is preferable to use sodium fluoride, which has low hygroscopicity and is therefore easy to handle in the air, and which can provide high activity and high selectivity. When sodium fluoride itself is used as a catalyst, it may be in powder form, but pellet form is preferred for gas-phase continuous flow reactions. It is also possible to use sodium fluoride supported on a carrier such as alumina, porous aluminum fluoride, activated carbon, silica, or zeolite. It is also possible to use sodium fluoride mixed with other components.

[0118] The temperature of the isomerization reaction is usually preferably 200 to 800°C, more preferably 400 to 600°C.

[0119] Not only the perfluoroalkyne compounds obtained as described above, but also the perfluorocycloalkene compounds can be effectively used in a variety of applications, such as etching gases for forming cutting-edge microstructures in semiconductors, liquid crystals, etc., as well as building blocks for organic synthesis. The synthetic building blocks will be described in detail below.

[0120] [3-2] Method for producing perfluoroalkyne compounds (part 2) A second method for producing a perfluoroalkyne compound of the present disclosure includes: A step of reacting a perfluoroalkadiene compound in the presence of a catalyst to obtain a perfluoroalkyne compound. wherein the catalyst contains at least one element belonging to groups 3 to 14 of the periodic table, and the contact time between the catalyst and the perfluoroalkadiene compound is 30 seconds or less. This production method satisfies the above-mentioned requirement (B).

[0121] Conventionally, methods for producing perfluoroalkyne compounds have used catalysts containing only one Group 13 element, such as halogenated alumina or sodium fluoride, without containing any transition metal. There are examples of catalysts containing alkali metals, but when using a catalyst containing only one Group 13 element without a transition metal, there are only examples of long reaction times of 32 seconds or more. According to the present disclosure, by using a catalyst containing at least one element belonging to Groups 3 to 14 of the periodic table and setting the reaction time to 30 seconds or less, the reaction conversion rate is high, and perfluoroalkyne compounds can be obtained in high yield and with high selectivity, thereby broadening the range of options when synthesizing perfluoroalkyne compounds. This method also has a short reaction time, allowing the reaction to proceed economically. Moreover, according to the present disclosure, unlike conventional methods, fluoroalkene compounds are less likely to be by-produced, as will be described later.

[0122] In the present disclosure, a small amount of elements belonging to groups 3 to 14 of the periodic table is used as a catalyst for the isomerization reaction. The catalyst used is not particularly limited, but may be any of the following: From the viewpoint of being able to obtain a perfluoroalkyne compound with a particularly high conversion rate and a high selectivity, a catalyst containing a transition metal element or a small amount of an element belonging to Groups 3 to 14 of the periodic table is preferred. A catalyst containing at least two of the transition metal elements belonging to groups 4 to 6 of the periodic table is preferred. catalysts containing at least one of the elements belonging to groups 4 to 6 and groups 13 to 14 of the periodic table; Catalysts containing at least two of these are more preferred, and catalysts containing chromium, titanium, zirconium, etc., and catalysts containing ketone, etc. Catalysts containing silicon and aluminum are more preferred.

[0123] As a catalyst for such an isomerization reaction, a chromium oxide catalyst which may be fluorinated (chromium oxide catalyst or fluorinated chromium oxide catalyst), a titanium oxide catalyst which may be fluorinated (titanium oxide catalyst or fluorinated titanium oxide catalyst), a zirconia catalyst which may be fluorinated (zirconia catalyst or fluorinated zirconia catalyst), a silica-alumina catalyst which may be fluorinated (silica-alumina catalyst or fluorinated silica-alumina catalyst), etc. are preferred, since they have high activity in the isomerization reaction of perfluoroalkadiene compounds to perfluoroalkyne compounds and, depending on the reaction conditions, also have high activity in the reaction of producing perfluorocycloalkene compounds which are expected to be used as dry etching gases for semiconductors as well as various refrigerants, blowing agents, heat transfer media, etc., just like perfluoroalkyne compounds. In this embodiment, a fluorinated catalyst is preferably used as the catalyst containing one element belonging to Group 13 of the periodic table. Alternatively, an alumina catalyst may be used.

[0124] As the chromium oxide catalyst, alumina catalyst, and silica-alumina catalyst, those described in the above [1-1] Catalyst and its manufacturing method (part 1) can be used, and as the titanium oxide catalyst and zirconia catalyst, those described in the above [1-2] Catalyst and its manufacturing method (part 2) can be used.

[0125] These isomerization catalysts can be used alone or in combination of two or more. It is also possible.

[0126] In addition, when the catalyst is fluorinated, the degree of fluorination (content of fluorine atoms), fluorination method, fluorinating agent, and fluorination conditions can be those described in the above [1-1] Catalyst and production method thereof (part 1).

[0127] The amount of catalyst used in the isomerization reaction can be the same as that explained in the above [3-1] Method for producing a perfluoroalkyne compound (part 1).

[0128] In the production method of the present disclosure, when reacting a perfluoroalkadiene compound, in addition to the perfluoroalkadiene compound substrate and the catalyst for the isomerization reaction, metallic nickel (particularly metallic nickel beads), activated carbon, or the like may also be used for the purpose of improving heat transfer or diluting the catalyst concentration, so that the W / F is 0.1 to 200 g sec. / cc, particularly 0.5 to 150 g sec. / cc.

[0129] The production method of the present disclosure (particularly the reaction of a perfluoroalkadiene compound) can be carried out in a liquid phase, but is preferably carried out in a gas phase, particularly in a gas phase continuous flow system using a fixed-bed reactor. This allows for further simplification of the equipment, operation, etc. compared to when carried out in a liquid phase, and also allows for the production of a perfluoroalkyne compound in a higher yield and with a higher selectivity compared to when carried out in a batch system.

[0130] In the production method of the present disclosure, the reaction temperature and reaction atmosphere in the reaction of the perfluoroalkadiene compound can be those described in the above [3-1] Production method of a perfluoroalkyne compound (part 1).

[0131] In the production method of the present disclosure, the contact time (reaction time) between the catalyst and the perfluoroalkadiene compound is 30 seconds or less, preferably 25 seconds or less. If the contact time (reaction time) exceeds 30 seconds, the yield of the perfluoroalkyne compound decreases. The lower limit of the contact time (reaction time) is not particularly limited, but is usually 1 second.

[0132] In the production method of the present disclosure, not only perfluorocycloalkene compounds but also perfluorocycloalkene compounds can be produced. The perfluorocycloalkene compounds include those represented by the general formula (3):

[0133] [ka]

[0134] [In the formula, R 1 ~R 4 is the same as above.] The perfluorocycloalkene compound is represented by the following formula: The details of the perfluorocycloalkene compound will be described later.

[0135] Therefore, after the reaction is completed, if necessary, purification treatment can be carried out in accordance with a conventional method to obtain a perfluoroalkyne compound.

[0136] In addition, the perfluorocycloalkene compound produced as a by-product by the production method of the present disclosure may be purified according to a conventional method as needed, and then the perfluorocycloalkene compound may be used as a by-product. It is also possible to obtain a perfluoroalkyne compound by using an ene compound as a substrate. The methods and conditions for this can be those described in the above [3-1] Method for producing a perfluoroalkyne compound (part 1).

[0137] Not only the perfluoroalkyne compounds obtained as described above, but also the perfluorocycloalkene compounds can be effectively used in a variety of applications, such as etching gases for forming cutting-edge microstructures in semiconductors, liquid crystals, etc., as well as building blocks for organic synthesis, etc. Details of building blocks for organic synthesis will be described later.

[0138] [3-3] Method for producing perfluoroalkyne compounds (part 3) A third method for producing a perfluoroalkyne compound of the present disclosure includes: A step of reacting a perfluoroalkadiene compound in the presence of a catalyst to obtain a perfluoroalkyne compound. The following (C) to (F): (C) The catalyst comprises a fluorinated chromium oxide having a pore volume of 0.08 mL / g or more, a fluorinated alumina having a pore volume of 0.35 mL / g or more, and a fluorinated silica having a pore volume of 0.50 mL / g or more. containing at least one catalyst selected from the group consisting of silica and alumina, (D) the catalyst contains a fluorinated metal oxide having a pore volume of 0.35 mL / g or more; (E) The catalyst is a hydrofluorocarbon, a hydrochlorofluorocarbon, and a chlorofluorocarbon. At least one compound selected from the group consisting of fluorocarbons and a metal oxide containing a metal oxide fluorinated by reacting (F) The catalyst is a chromium oxide having a pore volume of 0.10 mL / g or more, an alkali metal ion having a pore volume of 0.45 mL / g or more, A catalyst containing at least one fluorinated metal oxide selected from the group consisting of lumina and silica-alumina having a pore volume of 0.50 mL / g or more. Satisfy one of the following.

[0139] Requirement (C) is the present invention described in the above [1-1] Catalyst and its manufacturing method (part 1). Requirement (D) means that the catalyst 2 for the isomerization reaction of the present disclosure described in the above [1-2] Catalyst and its production method (part 2) is used. Requirement (E) means that in the above [2-1] catalyst production method (part 3), It is intended to use the catalyst obtained by the method for producing a catalyst for isomerization reaction of the present disclosure described above. Requirement (F) is satisfied by the method for producing a catalyst (part 4) described above in [2-2]. This means using a catalyst obtained by the method for producing an isomerization catalyst according to the present disclosure. The catalysts of the present disclosure can be used alone or in combination of two or more. Cut.

[0140] In the present disclosure, by using the catalyst of the present disclosure as described above, the conversion rate of the reaction can be increased and catalyst deterioration can be easily reduced, so that catalyst deterioration can be suppressed even when the isomerization reaction is carried out over a long period of time. Therefore, the replacement frequency of the catalyst of the present disclosure can be increased, which is an economical method.

[0141] The amount of the catalyst used in the present disclosure as described above can be a catalytic amount and is not particularly limited. However, from the viewpoint of achieving a particularly high conversion rate in the reaction, easily reducing catalyst deterioration, and easily suppressing catalyst deterioration even when the isomerization reaction is carried out over a long period of time, the catalyst weight ratio (W / F) to the hourly perfluoroalkadiene compound supply rate is preferably 0.1 to 200 g sec / cc, for example. In addition, when a plurality of catalysts according to the present disclosure are used, It is preferable to adjust the total amount to be within the above range. However, even when a liquid phase reaction is employed, the amount of catalyst used can be a catalytic amount and can be adjusted appropriately.

[0142] In the production method of the present disclosure, in addition to the perfluoroalkadiene compound as the substrate and the catalyst of the present disclosure, metallic nickel (particularly metallic nickel beads) or activated carbon, etc., can also be used in the isomerization reaction for the purpose of improving heat transfer or diluting the catalyst concentration, so that the W / F is 0.1 to 200 g sec. / cc, particularly 0.5 to 150 g sec. / cc.

[0143] In the production method of the present disclosure, the isomerization reaction can be carried out in a liquid phase, but is preferably carried out in a gas phase, particularly in a gas phase continuous flow system using a fixed bed reactor. This can further simplify the equipment, operation, etc. compared to when carried out in a liquid phase, and can obtain a perfluoroalkyne compound in a higher yield and with a higher selectivity compared to when carried out in a batch system. Furthermore, it is easy to reduce catalyst deterioration, and it is easy to suppress catalyst deterioration even when the isomerization reaction is carried out over a long period of time.

[0144] In the production method of the present disclosure, the isomerization reaction is preferably carried out under heating. Specifically, it is preferable to heat the system after adding the perfluoroalkadiene compound as the substrate and the catalyst of the present disclosure. The heating temperature at this time is preferably 170°C or higher (particularly 170 to 400°C), more preferably 180 to 280°C, from the viewpoints of particularly high reaction conversion, easy reduction in catalyst deterioration, and easy suppression of catalyst deterioration even when the isomerization reaction is carried out over a long period of time.

[0145] In the production method of the present disclosure, there is no particular limitation on the reaction time for the isomerization reaction, but the present disclosure is suitable for long-term reactions because it is easy to reduce catalyst deterioration and suppresses deterioration even when the isomerization reaction is carried out over a long period of time, and 10 to 200 hours is preferable, and 20 to 100 hours is more preferable.

[0146] In the production method of the present disclosure, the atmosphere in the isomerization reaction is not particularly limited, and for example, the reaction atmosphere is preferably an inert gas atmosphere (nitrogen gas atmosphere, argon gas atmosphere, etc.).

[0147] After the reaction is completed, if necessary, purification treatment is carried out according to a conventional method to obtain a perfluoroalkyne compound.

[0148] The perfluoroalkyne compounds obtained as described above can be effectively used in a variety of applications, such as as an etching gas for forming cutting-edge microstructures in semiconductors, liquid crystals, etc., as well as a building block for organic synthesis, etc. Details of the building block for organic synthesis will be described later.

[0149] [3-4] Method for producing perfluoroalkyne compounds (part 4) A fourth method for producing a perfluoroalkyne compound of the present disclosure includes: A step of reacting a perfluoroalkadiene compound in the presence of a catalyst to obtain a perfluoroalkyne compound. and, during at least a part of the period from the start of the reaction to the end of the reaction, the amount of water in the reaction system is 30 ppm by mass or less, based on the mass of the perfluoroalkadiene compound (100% by mass). The reaction of the perfluoroalkadiene compound is carried out.

[0150] As a method for producing a perfluoroalkyne compound, a method of isomerizing a perfluoroalkadiene compound by reacting it in the presence of a catalyst is known, but no method capable of reducing catalyst deterioration is known. According to the present disclosure, by keeping the amount of water in the reaction system at 30 mass ppm or less, based on the mass of the perfluoroalkadiene compound (100 mass%), at least part of the time from the start of the reaction to the end of the reaction, catalyst deterioration can be reduced and the conversion rate of the reaction can be maintained. In this case, it is possible to suppress catalyst deterioration even when the above isomerization reaction is carried out for a long time. In this case, the catalyst deterioration rate also varies depending on the catalyst weight ratio (W / F) to the perfluoroalkadiene compound supply rate per hour, and increasing W / F, that is, increasing the perfluoroalkadiene compound supply rate per hour, Slowing the supply rate of the perfluoroalkadiene compound can further suppress catalyst deterioration, and therefore, when the production method of the present disclosure is adopted, the catalyst replacement frequency can be increased, making it an economical method.

[0151] As will be described in detail later, according to the present disclosure, the amount of water present in the reaction system is kept low. This makes it possible to effectively prevent the active sites of the catalyst from being crushed by water and thereby causing deterioration. In other words, regardless of the type of catalyst used, it is possible to prevent the active sites of the catalyst from being crushed by water, and to effectively reduce catalyst deterioration. The catalyst for the isomerization reaction is not particularly limited, but from the viewpoint that reducing the amount of water in the reaction system makes it easy to reduce catalyst deterioration and makes it easy to suppress deterioration even when the isomerization reaction is carried out over a long period of time, for example, a catalyst containing at least one element belonging to Groups 3 to 14 of the periodic table is preferred, and a catalyst containing at least one element belonging to Groups 4 to 6 and Groups 13 to 14 of the periodic table is also preferred. More preferably, the catalyst contains at least one of chromium, titanium, silicon, aluminum, etc. The catalyst may contain only one of the above metal elements, or may contain two or more of them.

[0152] As the catalyst for such an isomerization reaction, from the viewpoints of high activity in the isomerization reaction of a perfluoroalkadiene compound to a perfluoroalkyne compound, easy reduction in catalyst deterioration by reducing the amount of water in the reaction system, and easy suppression of deterioration even when the isomerization reaction is carried out over a long period of time, particularly preferred are chromium oxide catalysts which may be fluorinated (chromium oxide catalyst or fluorinated chromium oxide catalyst), titanium oxide catalysts which may be fluorinated (titanium oxide catalyst or fluorinated titanium oxide catalyst), alumina catalysts which may be fluorinated (alumina catalyst or fluorinated alumina catalyst), silica-alumina catalysts which may be fluorinated (silica-alumina catalyst or fluorinated silica-alumina catalyst), and the like.

[0153] As the chromium oxide catalyst, alumina catalyst, and silica-alumina catalyst, those described in the above [1-1] Catalyst and its manufacturing method (part 1) can be used, and as the titanium oxide catalyst and zirconia catalyst, those described in the above [1-2] Catalyst and its manufacturing method (part 2) can be used.

[0154] These isomerization catalysts can be used alone or in combination of two or more. It is also possible.

[0155] In addition, when the catalyst is fluorinated, the degree of fluorination (content of fluorine atoms), fluorination method, fluorinating agent, and fluorination conditions can be those described in the above [1-1] Catalyst and production method thereof (part 1).

[0156] The amount of catalyst used in the isomerization reaction can be the same as that explained in the above [3-1] Method for producing a perfluoroalkyne compound (part 1).

[0157] In the production method of the present disclosure, in the isomerization reaction (reaction of a perfluoroalkadiene compound), in addition to the perfluoroalkadiene compound substrate and the catalyst for the isomerization reaction, metallic nickel (particularly metallic nickel beads), activated carbon, or the like may also be used for the purpose of improving heat transfer or diluting the catalyst concentration, so that the W / F is 0.1 to 200 g sec. / cc, particularly 0.5 to 150 g sec. / cc.

[0158] In the production method of the present disclosure, the isomerization reaction (reaction of a perfluoroalkadiene compound) is carried out under conditions where the amount of water in the reaction system is 30 ppm by mass or less, preferably 20 ppm by mass or less, based on the mass of the perfluoroalkadiene compound (100% by mass), at least partly from the start of the reaction to the end of the reaction. The lower limit of the amount of water can be 1 ppb by mass. In the present disclosure, the amount of water in the reaction system can be controlled, for example, by using an inert gas atmosphere as the reaction atmosphere, as described below. The moisture content can be adjusted by supplying a perfluoroalkadiene compound having a specific moisture content under the atmosphere.

[0159] In the present disclosure, the amount of water in the reaction system is 30 mass ppm or less as described above. The amount of water in the reaction system may be 30 mass ppm or less at the start of the reaction, or may be increased during the reaction. The amount of water in the reaction system may be 30 ppm by mass or less, or the amount of water in the reaction system may be 30 ppm by mass or less at the end of the reaction. In other words, the amount of water in the reaction system is 30 ppm by mass or less at least partly (at least at any timing) from the start of the reaction to the end of the reaction. In particular, from the viewpoint of further suppressing catalyst deterioration, it is preferable that the amount of water in the reaction system is 30 ppm by mass or less (particularly 20 ppm by mass or less) at least at the start of the reaction, and it is particularly preferable that the amount of water in the reaction system is 30 ppm by mass or less (particularly 20 ppm by mass or less) throughout the entire period from the start of the reaction to the end of the reaction.

[0160] In the production method of the present disclosure, the reaction atmosphere in the isomerization reaction (reaction of a perfluoroalkadiene compound) is not particularly limited as long as the amount of water in the reaction system satisfies the above-mentioned range, and for example, an inert gas atmosphere (nitrogen gas atmosphere, argon gas atmosphere, etc.) is preferred. When the reaction atmosphere is an inert gas atmosphere, the amount of water in the reaction system should be 30 mass ppm or less. This can be essentially rephrased as meaning that the water content of the perfluoroalkadiene compound substrate is 30 mass ppm or less. In other words, the reaction atmosphere is an inert gas atmosphere. In this case, the production method of the present disclosure includes the step of producing a perfluorinated cellulose having a water content of 30 mass ppm or less in the presence of a catalyst. In other words, it is a method for obtaining a perfluoroalkyne compound by reacting a perfluoroalkadiene compound with a catalyst. In this case, the water content of the perfluoroalkyne compound may be 30 mass ppm or less immediately before the reaction, that is, immediately before contact with the catalyst. The water content of the fluoroalkyne compound may be 30 mass ppm or less, and the water content may be 100 ppm or less at the end of the reaction. The water content of the fluoroalkyne compound may be 30 mass ppm or less. The water content of the perfluoroalkyne compound may be 30 mass ppm or less at least partly (at any timing) from the start of the reaction to the end of the reaction. It is sometimes preferred that the water content of the perfluoroalkyne compound is 30 mass ppm or less, and It is particularly preferable that the water content of the perfluoroalkyne compound is 30 mass ppm or less throughout the entire reaction from the start to the end.

[0161] In the production method of the present disclosure, the isomerization reaction (reaction of perfluoroalkadiene compound) can be carried out in a liquid phase, but is preferably carried out in a gas phase, particularly in a gas phase continuous flow system using a fixed bed reactor. This allows the equipment, operation, etc. to be further simplified compared to when carried out in a liquid phase, and the perfluoroalkyne compound can be obtained in a higher yield and with a higher selectivity compared to when carried out in a batch system. Furthermore, by reducing the amount of water in the reaction system, catalyst deterioration can be easily reduced, and deterioration can be easily suppressed even when the isomerization reaction is carried out over a long period of time.

[0162] In the production method of the present disclosure, the reaction temperature in the reaction of the perfluoroalkadiene compound can be the same as that explained in the above [3-1] Production method of a perfluoroalkyne compound (part 1).

[0163] In the production method of the present disclosure, there is no particular restriction on the reaction time for the isomerization reaction (reaction of a perfluoroalkadiene compound), but the present disclosure is suitable for long-term reactions because it reduces the amount of water in the reaction system, which makes it easy to reduce catalyst deterioration and suppresses deterioration even when the isomerization reaction is carried out over a long period of time, and 10 to 200 hours is preferred, and 20 to 100 hours is more preferred.

[0164] After the reaction is complete, purification is carried out according to a conventional method as necessary to obtain the perfluoroalkyne. The compound can be obtained.

[0165] The perfluoroalkyne compounds obtained as described above can be effectively used in a variety of applications, such as as an etching gas for forming cutting-edge microstructures in semiconductors, liquid crystals, etc., as well as a building block for organic synthesis, etc. Details of the building block for organic synthesis will be described later.

[0166] 4. Perfluorocycloalkene composition As described above, a perfluoroalkyne compound can be obtained, but when the production method described in the above [3-1] Production method (part 1) of a perfluoroalkyne compound or the above [3-2] Production method (part 2) of a perfluoroalkyne compound is adopted, the compound may be obtained in the form of a perfluoroalkyne composition containing a perfluoroalkyne compound and a perfluorocycloalkene compound, as described above. Note that when the production method described in the above [3-3] Production method (part 3) of a perfluoroalkyne compound or the above [3-4] Production method (part 4) of a perfluoroalkyne compound is adopted, the selectivity of the obtained perfluoroalkyne compound is extremely high, and it is possible to drastically reduce the content of other additional compounds in the product.

[0167] When the perfluoroalkyne compound is obtained in the form of a perfluoroalkyne composition, the perfluoroalkyne compound is represented by the general formula (1): CR 1 2nd Round 2 -C≡C-CR 3 R 4 2(1) [In the formula, R 1 ~R 4 is the same as above.] The perfluorocycloalkene compound is preferably a perfluoroalkyne represented by the general formula (3):

[0168] [ka]

[0169] [In the formula, R 1 ~R 4 is the same as above.] In the perfluoroalkyne composition of the present disclosure, the perfluoroalkyne compound may be used alone or in combination of two or more kinds. The above can also be used in combination.

[0170] Examples of the perfluorocycloalkene compound include:

[0171] [ka]

[0172] The perfluorocycloalkene compounds may be used alone or in combination of two or more. The above can also be used in combination.

[0173] In the perfluoroalkyne composition of the present disclosure, the content of the perfluoroalkyne compound is 40 to 99.999 mol%, where the total amount of the perfluoroalkyne composition of the present disclosure is 100 mol%. Preferably, the content of the perfluorocycloalkene compound is 0.001 to 60 mol%, more preferably 0.002 to 50 mol%, and even more preferably 0.003 to 40 mol%, based on the total amount of the perfluoroalkyne composition of the present disclosure being 100 mol%.

[0174] Furthermore, according to the production method of the present disclosure, in addition to the perfluoroalkyne compounds and perfluorocycloalkene compounds, General formula (4A): CR 1 2=CR 2 -CFR 3 -CFR 4 2(4A) [In the formula, R 1 ~R 4 is the same as above.] and perfluoroalkene compounds represented by the formula: General formula (4B): CFR 1 2-CR 2 =CH-CFR 4 2(4B) [In the formula, R 1 ~R 4 is the same as above.] Fluoroalkene compounds represented by the formula: According to the production method of the present disclosure, the fluoroalkene compound represented by general formula (4B) is hardly produced as a by-product.

[0175] Therefore, the perfluoroalkyne composition of the present disclosure may also contain a perfluoroalkene compound represented by general formula (4A) or a fluoroalkene compound represented by general formula (4B). When the perfluoroalkyne composition of the present disclosure contains a perfluoroalkene compound represented by general formula (4A), the content thereof is preferably 0.0005 to 0.5 mol %, and more preferably 0.001 to 0.3 mol %, relative to the total amount of the perfluoroalkyne composition of the present disclosure as 100 mol %. When the perfluoroalkyne composition of the present disclosure contains a fluoroalkene compound represented by general formula (4B), the fluoroalkene compound represented by general formula (4B) is unlikely to be by-produced according to the production method of the present disclosure, and therefore the content thereof is preferably 0 to 0.3 mol %, and more preferably 0.01 to 0.28 mol %, relative to the total amount of the perfluoroalkyne composition of the present disclosure as 100 mol %.

[0176] According to the production method of the present disclosure, even when a perfluoroalkyne composition is obtained, the perfluoroalkyne compound can be obtained with a particularly high yield and high selectivity as described above, and therefore, components other than the perfluoroalkyne compound in the perfluoroalkyne composition can be easily obtained. Since it is possible to reduce the amount of the compound, the labor required for purification to obtain the perfluoroalkyne compound can be reduced.

[0177] The perfluoroalkyne composition of the present disclosure, like the perfluoroalkyne compound alone, can be effectively used in a variety of applications, such as as an etching gas for forming cutting-edge microstructures in semiconductors, liquid crystals, etc., as well as for organic synthesis building blocks. The term "organic synthesis building block" refers to a substance that can serve as a precursor for a compound having a highly reactive skeleton. For example, by reacting the perfluorocycloalkene composition of the present disclosure with a fluorine-containing organosilicon compound such as CF3Si(CH3)3, a fluoroalkyl group such as a CF3 group can be introduced to convert it into a substance that can be used as a cleaning agent or a fluorine-containing pharmaceutical intermediate.

[0178] Although the embodiments of the present disclosure have been described above, various changes in form and details are possible without departing from the spirit and scope of the claims. [Example]

[0179] Examples will be given below to clarify the features of the present disclosure, but the present disclosure is not limited to these examples.

[0180] [Example 1: Requirement (A) or (B)] In the following Example 1, the following catalyst was used. Chromia catalyst: Cr2O3 Fluorinated chromia catalyst (1): Cr2O3 was fluorinated by passing hydrogen fluoride through it at atmospheric pressure at 100 to 460°C for 3 to 4 hours. Titania catalyst: TiO2 Fluorinated titania catalyst: Circulate hydrogen fluoride at atmospheric pressure, room temperature to 300°C for 3 to 4 hours. TiO2 was fluorinated with Fluorinated zirconia catalyst: Fluorinated zirconia catalyst is produced by passing hydrogen fluoride through the catalyst at atmospheric pressure and at room temperature to 400°C for 3 to 4 hours. ZrO2 was fluorinated with Silica-alumina catalyst: SiO2 / Al2O3 = 80 / 10 to 60 / 20 (mass ratio).

[0181] Example 1-1: Fluorinated chromia catalyst; W / F = 30.0 g·sec. / cc; 200°C; 23.1 seconds The catalyst, fluorinated chromia catalyst (1) (chromia fluorinated with hydrogen fluoride), was packed into a metal tubular reactor. The reactor was heated to 200 °C and hexafluorobutadiene ( CF 2 =CFCF=CF 2) was supplied to the reaction tube, and the reaction was carried out for 23.1 seconds in a gas-phase continuous flow system. One hour after the end of the reaction, the outflow gas from the reaction tube was analyzed by gas chromatography. The conversion was 100 mol % and the selectivity of each component was 99.7 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.162 mol % for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-CF4F6), 0.0356 mol % (total amount of E- and Z-isomers) for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3), and a total of 0.0182 mol % for other by-products.

[0182] Example 1-2: Fluorinated chromia catalyst; W / F = 30.0 g·sec. / cc; 250°C; 23.1 seconds The reaction was carried out in the same manner as in Example 1-1, except that the heating temperature was 250°C and the reaction was carried out for 23.1 seconds. After 1 hour had passed since the end of the reaction, the gas flowing out of the reaction tube was analyzed by gas chromatography. The conversion was 100 mol % and the selectivity of each component was 97.2 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 97.2 mol % for 1,2,3,3,4,4-hexafluoro-1-cyclobutyne (CF3C≡CCF3), and Butene (c-C4F6) 2.47 mol%, 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) 0.0871 mol% (total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) 0.262 mol% (total amount of E- and Z-isomers), and other by-products totaling 0.0194 mol% It was.

[0183] Example 1-3: Fluorinated chromia catalyst; W / F = 90.0 g·sec. / cc; 200°C; 69.3 seconds The reaction was carried out in the same manner as in Example 1-1, except that the W / F was set to 90.0 g·sec. / cc and the reaction was carried out for 69.3 seconds. After 1 hour had passed since the end of the reaction, the gas flowing out of the reaction tube was analyzed by gas chromatography. Analysis by FT-IR showed that the conversion was 100 mol % and the selectivity of each component was 99.7 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 99.7 mol % for 1,2,3,3,4,4-hexafluoro-1-cyano Clobutene (c-C4F6) was 0.118 mol%, 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was 0.0254 mol% (total amount of E- and Z-isomers), and 1,1,1,2,4,4,4-heptafluoro-2-butene was 0.118 mol%. The amount of tetradecene (CF3CF=CHCF3) was 0.0911 mol % (total amount of E-isomer and Z-isomer), and the amount of other by-products was 0.0162 mol % in total.

[0184] Example 1-4: Fluorinated titania catalyst; W / F = 30.0 g sec. / cc; 200°C; 32.5 seconds The reaction was carried out in the same manner as in Example 1-1, except that a fluorinated titania catalyst (titania fluorinated with hydrogen fluoride) was used as the catalyst and the reaction was carried out for 32 seconds. After filtering, the gas effluent from the reaction tube was analyzed by gas chromatography, and the conversion was found to be 99.0 mol %. The selectivities for each component were 99.3 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.354 mol % for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), 0.0595 mol % (total amount of E- and Z-isomers) for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3), and 0.213 mol % in total for other by-products.

[0185] Example 1-5: Fluorinated titania catalyst; W / F = 30.0 g sec. / cc; 250°C; 32.5 seconds The reaction was carried out in the same manner as in Example 1-1, except that a fluorinated titania catalyst (titania fluorinated with hydrogen fluoride) was used as the catalyst, the heating temperature was set to 250°C, and the reaction was carried out for 32.5 seconds. One hour after the reaction was completed, the gas flowing out of the reaction tube was analyzed by gas chromatography. Analysis revealed that the conversion rate was 99.9 mol % and the selectivity of each component was 1,1,1,4,4,4-hexafluoropropane. 23.7 mol% fluoro-2-butyne (CF3C≡CCF3), 1,2,3,3,4,4-hexafluoro-1-cyclobutyne The content of the product was 76.0 mol% of c-CF, 0.00110 mol% of 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF=CFCFCF) (total amount of E- and Z-isomers), 0.00421 mol% of 1,1,1,2,4,4,4-heptafluoro-2-butene (CFCF=CHCF), and a total of 0.295 mol% of other by-products.

[0186] Example 1-6: Fluorinated titania catalyst; W / F = 30.0 g sec. / cc; 300°C; 32.5 seconds The reaction was carried out in the same manner as in Example 1-1, except that a fluorinated titania catalyst (titania fluorinated with hydrogen fluoride) was used as the catalyst, the heating temperature was set to 300°C, and the reaction was carried out for 32.5 seconds. One hour after the reaction was completed, the gas flowing out of the reaction tube was analyzed by gas chromatography. Analysis revealed that the conversion was 100 mol%, and the selectivities for each component were 44.5 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 55.1 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-CF4F6), 0.00601 mol% (total amount of E- and Z-isomers) for 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3), 0.00200 mol% (total amount of E- and Z-isomers) for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3), and a total of 0.392 mol% for other by-products.

[0187] Example 1-7: Fluorinated zirconia catalyst; W / F = 30.0 g sec. / cc; 250°C; 14.9 seconds The reaction was carried out in the same manner as in Example 1-1, except that a fluorinated zirconia catalyst (zirconia fluorinated with hydrogen fluoride) was used as the catalyst, the heating temperature was set to 250°C, and the reaction was carried out for 14.9 seconds. After 1 hour had passed since the end of the reaction, the gas flowing out of the reaction tube was analyzed by gas chromatography. The conversion was 70.1 mol % and the selectivity of each component was 1,2,3,3,4,4-hexafluoropropane. 4.18 mol% of hexafluoro-1-cyclobutene (c-C4F6), 4.18 mol% of 1,1,1,4,4,4-hexafluoro-2- The content of 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was 0.00100 mol% (total of E- and Z-isomers), the content of 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.198 mol% (total of E- and Z-isomers), and the total content of other by-products was 0.0760 The molar percentage was

[0188] Example 1-8: Fluorinated zirconia catalyst; W / F = 30.0 g sec. / cc; 350°C; 14.9 seconds The reaction was carried out in the same manner as in Example 1-1, except that a fluorinated zirconia catalyst (zirconia fluorinated with hydrogen fluoride) was used as the catalyst, the heating temperature was set to 350°C, and the reaction was carried out for 14.9 seconds. After 1 hour had passed since the end of the reaction, the gas flowing out of the reaction tube was analyzed by gas chromatography. The conversion rate was 99.5 mol % and the selectivity of each component was 1,1,1,4,4,4-hexafluoropropanediol. The contents were 2.68 mol% trifluoro-2-butyne (CF3C≡CCF3), 96.3 mol% 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), 0.0127 mol% (total amount of E- and Z-isomers) of 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3), 0.118 mol% (total amount of E- and Z-isomers) of 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3), and a total of 0.274 mol% of other by-products.

[0189] Example 1-9: Fluorinated zirconia catalyst; W / F = 15.0 g sec. / cc; 350°C; 7.5 seconds The experiment was carried out using a fluorinated zirconia catalyst (zirconia fluorinated with hydrogen fluoride) as the catalyst, with the heating temperature set to 350°C, the W / F set to 15.0 g·sec. / cc, and the reaction time set to 7.5 seconds. The reaction was carried out in the same manner as in Example 1-1. After 1 hour had passed since the end of the reaction, the gas flowing out of the reaction tube was The conversion rate was 99.1 mol % when analyzed by gas chromatography. The selectivity was 3.71 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 95.3 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), and 1,1,2,3,3,4,4,4-octafluoro- 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0851 mol% (total amount of E- and Z-isomers), and The total amount of other by-products was 0.246 mol %.

[0190] The results of Examples 1-1 to 1-9 are shown in Table 1.

[0191] [Table 1]

[0192] Example 1-10: Fluorinated chromia catalyst; W / F = 15.0 g·sec. / cc; 200°C; 16.2 seconds The reaction was carried out in the same manner as in Example 1-1, except that the W / F was set to 15.0 g·sec. / cc and the reaction was carried out for 16.2 seconds. After 1 hour had passed since the end of the reaction, the gas flowing out of the reaction tube was analyzed by gas chromatography. Analysis by FT-IR showed that the conversion was 100 mol%, and the selectivity of each component was 99.8 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.0991 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was below the detection limit (ND; total amount of E- and Z-isomers), 0.0850 mol% for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) (total amount of E- and Z-isomers), and 0.0850 mol% for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3). The total was 0.0159 mol %.

[0193] Example 1-11: Chromia catalyst; W / F = 30.0 g·sec. / cc; 20°C; 25.1 seconds The reaction was carried out in the same manner as in Example 1-1, except that a chromia catalyst was used as the catalyst, the heating temperature was set to 20° C., and the reaction was carried out for 25.1 seconds. After 1 hour had passed since the end of the reaction, the flow rate from the reaction tube was Analysis of the outlet gas by gas chromatography revealed that the conversion was 100 mol %, and the selectivities for each component were as follows: 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3) was 99.8 mol %, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) was below the detection limit (ND), 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was 0.0257 mol % (total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0511 mol % (total amount of E- and Z-isomers), and a total of 0.0832 mol % for other by-products.

[0194] Example 1-12: Chromia catalyst; W / F = 14.0 g·sec. / cc; 20°C; 11.7 seconds The reaction was carried out using chromia catalyst at a W / F of 14.0 g·sec. / cc and a heating temperature of 20°C. The reaction was carried out in the same manner as in Example 1, except that the reaction was carried out for 11.7 seconds. One hour after the end of the reaction, the gas discharged from the reaction tube was analyzed by gas chromatography, and it was found that the conversion rate was 100%. The selectivity of each component was 99.8 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 99.8 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) was below the detection limit (ND), and 0.0187 mol% for 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) (E-isomer and The total amount of 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0544 moles. % (total amount of E-isomer and Z-isomer), and the total amount of other by-products was 0.0969 mol %.

[0195] Example 1-13: Chromia catalyst; W / F = 30.0 g·sec. / cc; 50°C; 25.1 seconds The reaction was carried out in the same manner as in Example 1-1, except that a chromia catalyst was used as the catalyst, the heating temperature was set to 50° C., and the reaction was carried out for 25.1 seconds. After 1 hour had passed since the end of the reaction, the flow rate from the reaction tube was Analysis of the outlet gas by gas chromatography revealed that the conversion was 100 mol %, and the selectivities for each component were as follows: 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3) was 99.9 mol %, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) was below the detection limit (ND), 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was 0.0201 mol % (total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0387 mol % (total amount of E- and Z-isomers), and a total of 0.0012 mol % for other by-products.

[0196] Example 1-14: Chromia catalyst; W / F = 6.0 g·sec. / cc; 150°C; 5.0 seconds The reaction was carried out using chromia catalyst at a W / F of 6.0 g·sec. / cc and a heating temperature of 150°C. The reaction was carried out in the same manner as in Example 1-1, except that the reaction was carried out for 5.0 seconds. One hour after the end of the reaction, the gas effluent from the reaction tube was analyzed by gas chromatography. The conversion was 100 mol % and the selectivity of each component was 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3 ) was 99.8 mol%, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) was 0.00311 mol%, 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was 0.0274 mol% (total amount of E-isomer and Z-isomer), and 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0477 mol% (total amount of E-isomer and Z-isomer), and the total amount of other by-products was 0.0818 mol %.

[0197] Example 1-15: Chromia catalyst; W / F = 30.0 g·sec. / cc; 150°C; 25.1 seconds The reaction was carried out for 25.1 seconds using chromia catalyst at a heating temperature of 150°C. The reaction was carried out in the same manner as in Example 1-1 except for the above. After 1 hour had passed since the end of the reaction, Analysis of the effluent gas by gas chromatography revealed that the conversion was 100 mol % and the selectivity of each component was 99.8 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.00154 mol % for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), and 0.00154 mol % for 1,1,2,3,3,4,4,4- Octafluoro-1-butene (CF2=CFCF2CF3) was 0.0272 mol% (total of E- and Z-isomers), and 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0364 mol% (total of E- and Z-isomers). Amount of methyl ...

[0198] Example 1-16: Chromia catalyst; W / F = 8.0 g·sec. / cc; 200°C; 6.7 seconds Chromia catalyst was used as the catalyst, and the reaction was carried out for 6.7 seconds at a W / F of 8.0 g·sec. / cc. The reaction was carried out in the same manner as in Example 1-1 except for the above. After 1 hour had passed since the end of the reaction, The effluent gas was analyzed by gas chromatography, and the conversion rate was found to be 99.9 mol %. The selectivity of each component was 99.6 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.00311 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-CF4F6), below the detection limit (ND; total amount of E- and Z-isomers) for 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3), 0.00111 mol% for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3), and a total of 0.416 mol% for other by-products.

[0199] Example 1-17: Chromia catalyst; W / F = 16.0 g·sec. / cc; 200°C; 13.3 seconds Chromia catalyst was used as the catalyst, and the reaction was carried out for 13.3 seconds at a W / F of 16.0 g·sec. / cc. The reaction was carried out in the same manner as in Example 1-1 except for the above. After 1 hour had passed since the end of the reaction, Analysis of the effluent gas from the reactor by gas chromatography revealed that the conversion was 100 mol %, and the selectivities for each component were as follows: 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3) was 99.9 mol %, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-CF4F6) was 0.00311 mol %, 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was below the detection limit (ND; total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.00101 mol % (total amount of E- and Z-isomers), and a total of 0.0959 mol % for other by-products.

[0200] Example 1-18: Titania catalyst; W / F = 10.0 g sec. / cc; 200°C; 11.1 seconds Titania catalyst was used as the catalyst, and the reaction was carried out for 11.1 seconds at a W / F of 10.0 g·sec. / cc. The reaction was carried out in the same manner as in Example 1-1 except for the above. After 1 hour had passed since the end of the reaction, The effluent gas was analyzed by gas chromatography, and the conversion rate was found to be 99.0 mol%. The selectivity of each component was 99.4 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.254 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), 0.059 mol% (ND; total amount of E- and Z-isomers) for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3), and 0.0341 mol% (E- and Z-isomers) for 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3). The total amount of other by-products was 0.213 mol %.

[0201] Example 1-19: Titania catalyst; W / F = 14.0 g sec. / cc; 200°C; 15.5 seconds Titania catalyst was used as the catalyst, and the reaction was carried out for 15.5 seconds at a W / F of 14.0 g·sec. / cc. The reaction was carried out in the same manner as in Example 1-1 except for the above. After 1 hour had passed since the end of the reaction, The effluent gas was analyzed by gas chromatography, and the conversion rate was found to be 99.0 mol%. The selectivity of each component was 99.3 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.362 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), and 0.0587 mol% for 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) (ND; the total amount of E- and Z-isomers). ), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0321 mol% (E isomer and Z isomer) The total amount of by-products was 0.247 mol %.

[0202] Example 1-20: Silica-alumina catalyst; W / F = 7.5 g sec. / cc; 20°C; 14.9 seconds The reaction was carried out in the same manner as in Example 1-1, except that a silica-alumina catalyst was used as the catalyst, the W / F was set to 7.5 g·sec. / cc, the heating temperature was set to 20°C, and the reaction was carried out for 14.9 seconds. After the time had passed, the gas effluent from the reaction tube was analyzed by gas chromatography, and it was found that the conversion rate was 100 mol % and the selectivity of each component was 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C ≡CCF3) was 99.4 mol%, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) was below the detection limit (ND), and 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was at the detection limit. less than ND (total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0909 mol% (total amount of E- and Z-isomers), and other by-products were 0.504 mol% in total. .

[0203] Example 1-21: Silica-alumina catalyst; W / F = 15.0 g sec. / cc; 20°C; 29.9 seconds A silica-alumina catalyst was used as the catalyst, and the W / F was set to 15.0 g·sec. / cc and the heating temperature to 20°C. The reaction was carried out in the same manner as in Example 1-1, except that the reaction was carried out for 29.9 seconds. One hour after the end of the reaction, the gas discharged from the reaction tube was analyzed by gas chromatography. The conversion rate was 100 mol %, and the selectivity of each component was 99.9 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), and 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) was detected. Below the limit (ND), 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was 0.00688 mol% (total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3 ) was 0.0555 mol % (total amount of E-isomer and Z-isomer), and the total amount of other by-products was 0.0374 mol %.

[0204] Example 1-22: Silica-alumina catalyst; W / F = 30.0 g sec. / cc; 20°C; 59.8 seconds The reaction was carried out in the same manner as in Example 1-1, except that a silica alumina catalyst was used as the catalyst, the heating temperature was set to 20°C, and the reaction was carried out for 59.8 seconds. After 1 hour had passed since the end of the reaction, Analysis of the effluent gas from the reactor by gas chromatography revealed that the conversion was 100 mol %, and the selectivities for each component were as follows: 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3) was 99.8 mol %, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-CF4F6) was below the detection limit (ND), 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was below the detection limit (ND; total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0804 mol % (total amount of E- and Z-isomers), and a total of 0.161 mol % for other by-products.

[0205] Example 1-23: Silica-alumina catalyst; W / F = 4.0 g sec. / cc; 100°C; 8.0 seconds A silica-alumina catalyst was used as the catalyst, and the W / F was set to 4.0 g·sec. / cc and the heating temperature to 100°C. The reaction was carried out in the same manner as in Example 1, except that the reaction was carried out for 8.0 seconds. After the reaction time, the gas effluent from the reaction tube was analyzed by gas chromatography. The conversion rate was 100 mol % and the selectivity of each component was 99.4 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.00121 mol % for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), and 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was below the detection limit (ND; E The content of 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.0909 mol % (total amount of E- and Z-isomers), and the total amount of other by-products was 0.503 mol %.

[0206] Example 1-24: Silica-alumina catalyst; W / F = 4.0 g sec. / cc; 200°C; 8.0 seconds Using a silica-alumina catalyst, the reaction was carried out for 8.0 seconds at a W / F of 4.0 g·sec. / cc. The reaction was carried out in the same manner as in Example 1-1, except that the reaction was carried out in the same manner as in Example 1-1. Analysis of the gas effluent from the tube by gas chromatography revealed that the conversion was 100 mol % and the selectivity of each component was 99.5 mol % for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3). mol%, 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6) 0.0670 mol%, 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) below the detection limit (ND; total amount of E- and Z-isomers), 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) 0.0101 mol% (E- and Z-isomers). The total amount of the Z isomer and the Z isomer was 0.467 mol %.

[0207] Example 1-25: Silica-alumina catalyst; W / F = 8.0 g sec. / cc; 200°C; 16.0 seconds The reaction was carried out in the same manner as in Example 1-1, except that a silica-alumina catalyst was used as the catalyst, the W / F was set to 8.0 g sec / cc, and the reaction was carried out for 16.0 seconds. Analysis of the gas effluent from the reaction tube by gas chromatography revealed that the conversion was 100 mol%, and the selectivity of each component was 99.5 mol% for 1,1,1,4,4,4-hexafluoro-2-butyne (CF3C≡CCF3), 0.0611 mol% for 1,2,3,3,4,4-hexafluoro-1-cyclobutene (c-C4F6), and 1,1,2,3,3,4,4,4-octafluoro-1-butene (CF2=CFCF2CF3) was below the detection limit (ND; E- and Z-isomers). The content of 1,1,1,2,4,4,4-heptafluoro-2-butene (CF3CF=CHCF3) was 0.00921 mol % (total amount of E- and Z-isomers), and the total amount of other by-products was 0.480 mol %.

[0208] The results of Examples 1-1 and 1-10 to 1-17 are shown in Table 2, and the results of Examples 1-18 to 1-25 are shown in Table 3.

[0209] [Table 2]

[0210] [Table 3]

[0211] [Example 2: Requirements (C) to (F)] In the following Example 2, the following catalyst was used. Fluorinated chromia catalyst (1): Chromia fluorinated with hydrogen fluoride; pore volume 0.10 mL / g; Chromia (Cr2O3; pore volume 0.15 mL / g) was fluorinated by passing hydrogen fluoride through it at atmospheric pressure at 100 to 400°C for 6 hours. Fluorinated chromia catalyst (2): Chromia fluorinated with chlorodifluoromethane (R22) Chromia (Cr2O3; pore volume 0.15mL / g) was fluorinated by passing chlorodifluoromethane (R22) through it at atmospheric pressure at 100 to 500°C for 6 hours. Fluorinated silica-alumina catalyst (1): Silica-alumina fluorinated with hydrogen fluoride; pore volume 0.55 mL / g; For silica-alumina (pore volume 0.70 mL / g), 6 The mixture was fluorinated by passing hydrogen fluoride through it for 1 hour. Fluorinated silica-alumina catalyst (2): Silica fluorinated with chlorodifluoromethane (R22) Fluorination was carried out by passing chlorodifluoromethane (R22) through silica alumina (pore volume 0.70 mL / g) at atmospheric pressure at 100 to 500°C for 6 hours.

[0212] In addition, the fluorinated alumina catalysts were all fluorinated by passing hydrogen fluoride through the specified alumina at atmospheric pressure at 100 to 400°C for 6 hours. The details of the catalyst are shown in Table 4.

[0213] [Table 4]

[0214] Example 2-1: R22 fluorinated chromia catalyst; pore volume 0.13 mL / g The catalyst, fluorinated chromia catalyst (2) (chromia fluorinated with chlorodifluoromethane (R22)), was packed into a metal tubular reactor. The reactor was heated to 200 °C and hexafluorobutadiene ( CF 2 =CFCF=CF 2) was supplied to the reaction tube, and the reaction proceeded in a gas-phase continuous flow system. After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. The result showed that the catalyst degradation rate was -0.12% / hour. The catalyst degradation rate refers to the slope of a plot where the horizontal axis is reaction time and the vertical axis is conversion rate. The results are shown in Table 5.

[0215] [Table 5]

[0216] Example 2-2: R22 fluorinated silica-alumina catalyst; pore volume 0.69 mL / g The catalyst used was a fluorinated silica-alumina catalyst (2) (silica-alumina fluorinated with chlorodifluoromethane (R22)) instead of a fluorinated chromia catalyst (2). The reaction was carried out in the same manner as in Example 2-1. After a predetermined time had elapsed, the gas discharged from the reaction tube was analyzed by gas chromatography. As a result, the catalyst deterioration rate was -0.0014% / hour. The catalyst deterioration rate was calculated by plotting the reaction time on the horizontal axis and the conversion rate on the vertical axis. The results are shown in Table 6.

[0217] [Table 6]

[0218] Example 2-3: Fluorinated alumina catalyst; pore volume 1.33 mL / g The reaction was carried out in the same manner as in Example 2-1, except that the fluorinated alumina catalyst (1) was used instead of the fluorinated chromia catalyst (2). After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. The catalyst degradation rate was found to be -0.025% / hour. The catalyst degradation rate refers to the slope of a plot of reaction time on the horizontal axis and conversion rate on the vertical axis. The results are shown in Table 7.

[0219] [Table 7]

[0220] Example 2-4: Fluorinated alumina catalyst; pore volume 0.43 mL / g The reaction was carried out in the same manner as in Example 2-1, except that fluorinated alumina catalyst (2) was used instead of fluorinated chromia catalyst (2). After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. The catalyst degradation rate was found to be -0.026% / hour. The catalyst degradation rate refers to the slope of a plot of reaction time on the horizontal axis and conversion rate on the vertical axis. The results are shown in Table 8.

[0221] [Table 8]

[0222] Comparative Example 2-1: Fluorinated alumina catalyst; pore volume 0.22 mL / g The reaction was carried out in the same manner as in Example 2-1, except that the fluorinated alumina catalyst (3) was used instead of the fluorinated chromia catalyst (2). After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. As a result, the catalyst degradation rate was -0.65% / The catalyst degradation rate is the slope of a plot with reaction time on the horizontal axis and conversion rate on the vertical axis. The results are shown in Table 9.

[0223] [Table 9]

[0224] Example 2-5: Fluorinated alumina catalyst; pore volume 0.39 mL / g The reaction was carried out in the same manner as in Example 2-1, except that the fluorinated alumina catalyst (4) was used instead of the fluorinated chromia catalyst (2). The outflow gas was analyzed by gas chromatography. The results showed that the catalyst deterioration rate was -0.29% / The catalyst degradation rate is the slope of a plot with reaction time on the horizontal axis and conversion rate on the vertical axis. The results are shown in Table 10.

[0225] [Table 10]

[0226] Comparative Example 2-2: Fluorinated alumina catalyst; pore volume 0.23 mL / g The reaction was carried out in the same manner as in Example 2-1, except that the fluorinated alumina catalyst (5) was used as the catalyst instead of the fluorinated chromia catalyst (2). After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. As a result, the catalyst degradation rate was found to be -0.67% / hour. The catalyst degradation rate is the slope of a plot with reaction time on the horizontal axis and conversion rate on the vertical axis. The results are shown in Table 11.

[0227] [Table 11]

[0228] Of the results in Tables 7 to 11 above, the relationship between the elapsed time (contact time) and the conversion rate is shown in Figure 1, the relationship between the pore volume before fluorination and the deterioration rate is shown in Figure 2, and the relationship between the pore volume after fluorination and the deterioration rate is shown in Figure 3.

[0229] [Example 3: Requirement (G)] In the following Example 3, a chromia catalyst (Cr2O3) or an alumina catalyst (Al2O3) was used as the catalyst.

[0230] The water content of the hexafluorobutadiene was adjusted to a predetermined value by adding water or by dehydrating with a molecular sieve, and the water content was measured by the Karl Fischer method.

[0231] Example 3-1: Chromia catalyst; water content 20 ppm A metal tubular reactor was filled with nitrogen gas to create a nitrogen gas atmosphere, and then chromia catalyst was added as a catalyst. The reactor was heated to 200°C and hexafluorobutadiene ( CF 2 =CFCF=CF 2) was supplied to the reaction tube, and the reaction proceeded in a gas-phase continuous flow system. The water content of hexafluorobutadiene at the start of the reaction was 20 ppm by mass, and the water content in the reaction system was adjusted to 20 ppm from the start to the end of the reaction. After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. As a result, the catalyst deterioration rate was found to be -0.12% / hour. The catalyst deterioration rate refers to the slope when the horizontal axis is reaction time and the vertical axis is conversion rate. The results are shown in Table 12.

[0232] [Table 12]

[0233] Example 3-2: Chromia catalyst; water content 2 ppm At the start of the reaction, the water content of hexafluorobutadiene was 20 mass ppm. The water content of hexafluorobutadiene at the start of the reaction is 2 mass % instead of fluorobutadiene. The reaction system from the start to the end of the reaction using hexafluorobutadiene in ppm The reaction was carried out in the same manner as in Example 3-1, except that the water content in the reaction tube was adjusted to 2 ppm. After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. The catalyst deterioration rate was -0.12% / hour. The catalyst deterioration rate is shown on the horizontal axis as reaction time and on the vertical axis as The results are shown in Table 13.

[0234] [Table 13]

[0235] Example 3-3: Alumina catalyst; water content 20 ppm The reaction was carried out in the same manner as in Example 3-1, except that an alumina catalyst was used instead of a chromia catalyst. After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. As a result, the catalyst deterioration rate was -0.0302% / hour. The results are shown in Table 14.

[0236] [Table 14]

[0237] Example 3-4: Alumina catalyst; water content 2 ppm An alumina catalyst was used instead of a chromia catalyst, and the water content of the hexafluorobutadiene at the start of the reaction was 20 ppm by mass, but not hexafluorobutadiene at the start of the reaction. The reaction was carried out in the same manner as in Example 3-1, except that the amount of water in the reaction system was adjusted to 2 ppm from the start to the end of the reaction using hexafluorobutadiene having a water content of 2 ppm by mass. After a predetermined time had elapsed, the gas effluent from the reaction tube was analyzed by gas chromatography. As a result, the catalyst deterioration rate was found to be -0.08% / hour. The catalyst deterioration rate is the slope of a plot of reaction time on the horizontal axis and conversion rate on the vertical axis. The results are shown in Table 15.

[0238] [Table 15]

Claims

1. A method for producing a perfluoroalkyne compound, comprising the steps of: A process for obtaining a perfluoroalkyne compound by reacting a perfluoroalkadiene compound at 170 to 300°C in the presence of a catalyst. and the catalyst comprises at least one catalyst selected from the group consisting of catalysts containing at least one transition metal element belonging to Groups 4 to 6 of the periodic table and catalysts containing at least two elements belonging to Groups 4 to 6 and Groups 13 to 14 of the periodic table, and the contact time between the catalyst and the perfluoroalkadiene compound is 30 seconds or less.

2. The perfluoroalkyne compound is represented by the general formula (1): CR 1 2 R 2 -C≡C-CR 3 R 4 2 (1) [In the formula, R 1 ~R 4 and each of the formula (I) is the same or different and represents a fluorine atom or a perfluoroalkyl group.

3. The perfluoroalkadiene compound is General formula (2): CR 1 2 =CR 2 -CR 3 =CR 4 2 (2) [In the formula, R 1 ~R 4 and each of the formula (I) is the same or different and represents a fluorine atom or a perfluoroalkyl group.

4. The method according to any one of claims 1 to 3, wherein the catalyst is at least one catalyst selected from the group consisting of catalysts containing at least one of chromium, titanium, and zirconium, and catalysts containing silicon and aluminum.

5. The process according to any one of claims 1 to 4, wherein the catalyst is at least one catalyst selected from the group consisting of an optionally fluorinated chromium oxide catalyst, an optionally fluorinated titanium oxide catalyst, an optionally fluorinated zirconia catalyst, and an optionally fluorinated silica-alumina catalyst.

6. The process according to any one of claims 1 to 5, wherein the reaction of the perfluoroalkadiene compound is carried out in a gas phase.

7. The method according to any one of claims 1 to 6, wherein a perfluorocycloalkene compound is also produced in addition to the perfluoroalkyne compound by the reaction of the perfluoroalkadiene compound.

8. The perfluorocycloalkene compound is Formula (3): [Formula 1] [In the formula, R 1 ~R 4 and each of the formula (I) is the same or different and represents a fluorine atom or a perfluoroalkyl group.

9. A method for producing a perfluoroalkyne compound, comprising the steps of: The method for producing a perfluorocycloalkene compound in addition to the perfluoroalkyne compound according to claim 7 or 8, further comprising a step of producing the perfluorocycloalkene compound by the reaction of the perfluoroalkadiene compound, and then using the resulting perfluorocycloalkene compound as a substrate to obtain the perfluoroalkyne compound.

10. The perfluoroalkyne compound is represented by the general formula (1): CR 1 2 R 2 -C≡C-CR 3 R 4 2 (1) [In the formula, R 1 ~R 4 are the same or different and represent a fluorine atom or a perfluoroalkyl group. The method according to claim 9, wherein the perfluoroalkyne compound is represented by the formula:

Citation Information

Patent Citations

  • Method for preparing perfluorinated alkadiene and perfluorinated alkyne by gas phase isomerization

    CN107602340A

  • Method for producing perfluoroalkyne compound

    JP2004231562A

  • Method for producing 1,3,3,3-tetrafluoropropene

    JP2008019243A

  • Method for producing fluorine compound

    JP2012001448A

  • Method for producing 1,1,1,4,4,4-hexafluoro-2-butyne

    JP2014058488A