Solid composition, circuit board, and method for producing solid composition

A perfluorinated fluororesin and anisotropic filler combination with silane treatment addresses the issues of high linear expansion and moldability in circuit boards, providing a solid composition with improved mechanical and electrical properties for high-frequency applications.

JP7568957B2Active Publication Date: 2024-10-17DAIKIN INDUSTRIES LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023050459
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-03-27
Publication Date
2024-10-17
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing materials for circuit boards face challenges with high linear expansion coefficients and poor moldability, particularly when using fluororesin, which limits their performance in high-speed communication equipment.

Method used

A solid composition comprising perfluorinated fluororesin and anisotropic fillers treated with a silane coupling agent, such as talc or boron nitride, with controlled terminal groups and low Mohs hardness, is used to achieve low linear expansion and improved moldability.

Benefits of technology

The composition exhibits a low coefficient of linear expansion, reduced voids, enhanced mechanical and electrical properties, and improved moldability, making it suitable for high-frequency circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568957000001
    Figure 0007568957000001
  • Figure 0007568957000002
    Figure 0007568957000002
  • Figure 0007568957000003
    Figure 0007568957000003
Patent Text Reader

Abstract

To provide a solid composition having a low linear expansion coefficient and excellent moldability, a circuit board, and a method for producing a solid composition.SOLUTION: A solid composition contains a perfluoro-based fluororesin and an anisotropic filler that is surface-treated using a silane coupling agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid composition, a circuit board, and a method for making the solid composition. [Background technology]

[0002] As communication speeds increase, low dielectric and low loss materials are required for circuit boards used in electrical devices, electronic devices, communication devices, etc. Fluorine resins have been considered as such materials, but one of the issues with using fluororesins is how to reduce the linear expansion coefficient.

[0003] Patent Document 1 describes a resin composition for dielectrics that contains an inorganic substance dispersed in a thermoplastic resin and / or a thermosetting resin.

[0004] Patent Document 2 describes a dispersion liquid containing a tetrafluoroethylene-based polymer powder, an anisotropic filler, and a liquid dispersion medium. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-40296 A [Patent Document 2] International Publication No. 2021 / 112164 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present disclosure is to provide a solid composition having a low linear expansion coefficient and good moldability, a circuit board, and a method for producing the solid composition. [Means for solving the problem]

[0007] This disclosure (1) The solid composition contains a perfluoro-based fluororesin and an anisotropic filler that has been surface-treated with a silane coupling agent (hereinafter, also referred to as "the solid composition of the present disclosure").

[0008] This disclosure (2) The solid composition according to the present disclosure (1), wherein the anisotropic filler is talc and / or boron nitride.

[0009] This disclosure (3) The anisotropic filler is a solid composition according to the present disclosure (1) or (2) having a Mohs hardness of 4 or less.

[0010] This disclosure (4) The silane coupling agent is the solid composition according to any one of the present disclosure (1) to (3), which has at least one group selected from the group consisting of a fluorine-containing group, an amino group, a vinyl group, and an epoxy group.

[0011] This disclosure (5) The perfluoro-based fluororesin has an unstable terminal group having a carbon number of 1×10 6 Less than 50 pieces per piece, The solid composition according to any one of the present disclosures (1) to (4), wherein the unstable terminal group is at least one selected from the group consisting of -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH present at the main chain terminal of the perfluoro-based fluororesin.

[0012] This disclosure (6) The perfluoro-based fluororesin is at least one selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer, and tetrafluoroethylene / hexafluoropropylene copolymer, in the solid composition according to any one of the present disclosures (1) to (5).

[0013] This disclosure (7) In image analysis using a laser microscope, voids with a width of 30 μm or more were found to be 1 mm 2The solid composition according to any one of the present disclosures (1) to (6), wherein the number of particles per unit area is 30 or less.

[0014] This disclosure (8) The solid composition according to any one of the present disclosures (1) to (7), wherein the reduction rate of the linear expansion coefficient of the solid composition at 20°C to 200°C relative to the linear expansion coefficient of the perfluoro-based fluororesin at 20°C to 200°C is 25% or more.

[0015] This disclosure (9) The solid composition according to any one of the present disclosures (1) to (8) has a dielectric loss tangent at 25° C. and 10 GHz of 0.003 or less.

[0016] This disclosure (10) The solid composition according to any one of the present disclosure (1) to (9) is in the form of a film or sheet.

[0017] This disclosure (11) The solid composition according to any one of (1) to (10) of the present disclosure is an insulating material for a circuit board.

[0018] This disclosure (12) The insulating material of the circuit board is a solid composition according to the present disclosure (11), which is a low dielectric material.

[0019] This disclosure (13) The present invention relates to a circuit board (hereinafter also referred to as "the circuit board of the present disclosure") having a solid composition according to any one of (1) to (12) of the present disclosure and a conductive layer.

[0020] This disclosure (14) The circuit board according to the present disclosure (13), wherein the conductive layer is a metal.

[0021] This disclosure (15) In the circuit board according to the present disclosure (14), the metal has a surface roughness Rz of 2.0 μm or less on the surface on the side of the solid composition.

[0022] This disclosure (16) The circuit board according to the present disclosure (14) or (15), wherein the metal is copper.

[0023] This disclosure (17) The circuit board according to any one of the present disclosures (13) to (16) is a printed circuit board, a multilayer circuit board, or a high-frequency board.

[0024] This disclosure (18) A method for producing a solid composition according to any one of the present disclosure (1) to (12), comprising melt-kneading the perfluoro-based fluororesin and the anisotropic filler to obtain the solid composition (hereinafter also referred to as the "production method of the present disclosure"). Effect of the Invention

[0025] According to the present disclosure, it is possible to provide a solid composition having a low linear expansion coefficient and good moldability, a circuit board, and a method for producing the solid composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] As used herein, "organic group" means a group containing one or more carbon atoms or a group formed by removing a hydrogen atom from an organic compound. Examples of the "organic group" are: an alkyl group which may have one or more substituents; an alkenyl group optionally having one or more substituents; an alkynyl group optionally having one or more substituents; a cycloalkyl group optionally having one or more substituents, a cycloalkenyl group optionally having one or more substituents, a cycloalkadienyl group optionally having one or more substituents, an aryl group which may have one or more substituents; an aralkyl group optionally having one or more substituents; a non-aromatic heterocyclic group optionally having one or more substituents, a heteroaryl group optionally having one or more substituents, Cyano group, Formyl group, RaO-, RaCO-, RaSO2-, RaCOO-, RaNRaCO-, RaCONRa-, RaOCO-, RaOSO2- and RaNRbSO2- (In these formulas, Ra is independently an alkyl group which may have one or more substituents; an alkenyl group optionally having one or more substituents; an alkynyl group optionally having one or more substituents; a cycloalkyl group optionally having one or more substituents, a cycloalkenyl group optionally having one or more substituents, a cycloalkadienyl group optionally having one or more substituents, an aryl group which may have one or more substituents; an aralkyl group optionally having one or more substituents; a non-aromatic heterocyclic group optionally having one or more substituents, or a heteroaryl group optionally having one or more substituents, Rb is independently H or an alkyl group which may have one or more substituents. Includes: The organic group is preferably an alkyl group which may have one or more substituents.

[0027] The present disclosure will now be described in detail.

[0028] The solid composition of the present disclosure contains a perfluoro-based fluororesin and an anisotropic filler that has been surface-treated with a silane coupling agent. The solid composition of the present disclosure contains the anisotropic filler, and therefore has a low linear expansion coefficient and good moldability, despite containing a perfluoro-based fluororesin. In addition, by incorporating the anisotropic filler, the solid composition of the present disclosure has fewer internal voids when pelletized, which improves the mechanical properties of films and sheets formed from the pellets. Furthermore, by blending the anisotropic filler, the electrical properties can be improved. In addition, as described in Patent Document 1, when an anisotropic filler and a fluororesin are melt-kneaded, a strong stress is usually required, and the properties of the anisotropic filler (such as the effect of improving electrical properties) may be impaired, but since the anisotropic filler is surface-treated with a silane coupling agent, the properties can be maintained even when melt-kneaded with the fluororesin. Furthermore, by performing melt-kneading, the anisotropic filler can be well dispersed in the fluororesin, and the electrical properties can be improved. Furthermore, the solid composition of the present disclosure has the advantage that, since it is a solid, it requires fewer production steps and can be easily formed into a thick film, as compared with the dispersion described in Patent Document 2. In addition, since the solid composition of the present disclosure uses a perfluoro-based fluororesin, better electrical properties can be obtained compared to other fluororesins such as ethylene / tetrafluoroethylene copolymer (ETFE).

[0029] The above-mentioned perfluoro-based fluororesin is a copolymer mainly composed of a fluorine-containing monomer such as a perfluoromonomer, and is a fluorine resin having very few hydrogen atoms bonded to carbon atoms in the repeating units constituting the main chain, and may have hydrogen atoms bonded to carbon atoms in the repeating units other than those constituting the main chain, such as terminal structures. In addition, as long as the content of the fluorine-containing monomer in the resin is 90 mol% or more, a monomer other than the fluorine-containing monomer may be copolymerized. The content of the fluorine-containing monomer is preferably 95 mol% or more, more preferably 99 mol% or more, and may be 100 mol%. As the perfluoro-based fluororesin, a polymer of tetrafluoroethylene [TFE], which is a perfluoromonomer, or a copolymer of TFE and a copolymerizable monomer that can be copolymerized therewith can be used. In this specification, the term "perfluoromonomer" refers to a monomer in which all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms.

[0030] The copolymerizable monomer is not particularly limited as long as it is copolymerizable with TFE and does not contain a hydrogen atom bonded to a carbon atom constituting the main chain. For example, hexafluoropropylene [HFP], fluoroalkyl vinyl ether, fluoroalkyl ethylene, and fluoroalkyl ethylene represented by the general formula (100): CH2=CFRf 101 (In the formula, Rf 101 Examples of the fluoromonomer include a fluoromonomer represented by a straight-chain or branched fluoroalkyl group having 1 to 12 carbon atoms, and a fluoroalkyl allyl ether. Examples of monomers other than the fluoromonomer include itaconic anhydride, citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, and maleic anhydride. The above copolymerizable monomers may be used alone or in combination of two or more.

[0031] Examples of the fluoroalkyl vinyl ether include General formula (110): CF2=CF-ORf 111 (In the formula, Rf 111 represents a perfluoro organic group; General formula (120): CF2=CF-OCH2-Rf 121 (In the formula, Rf 121 is a perfluoroalkyl group having 1 to 5 carbon atoms), General formula (130): CF2=CFOCF2ORf 131 (In the formula, Rf 131 is a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a linear or branched perfluorooxyalkyl group having 2 to 6 carbon atoms and containing 1 to 3 oxygen atoms, General formula (140): CF2=CFO(CF2CF(Y 141 )O)m (CF2) n F (In the formula, Y 141 represents a fluorine atom or a trifluoromethyl group; m is an integer of 1 to 4; and n is an integer of 1 to 4. General formula (150): CF2=CF-O-(CF2CFY 151 -O) n -(CFY 152 ) m -A 151 (In the formula, Y 151 represents a fluorine atom, a chlorine atom, a -SO2F group, or a perfluoroalkyl group. The perfluoroalkyl group may contain an etheric oxygen and a -SO2F group. n represents an integer of 0 to 3. n Y 151 may be the same or different. Y 152 represents a fluorine atom, a chlorine atom, or a -SO2F group. m represents an integer of 1 to 5. m Y 152 may be the same or different. A 151 -SO2X 151 , -COZ 151 or -POZ 152 Z 153 Represents X. 151 is F, Cl, Br, I, -OR 151 or -NR 152 R 153 Represents Z. 151 , Z 152 and Z 153 are the same or different, -NR 154 R 155 -OR 156 Represents R 151 , R 152 , R 153 , R 154 , R 155 and R 156 are the same or different and represent H, ammonium, an alkali metal, an alkyl group which may contain a fluorine atom, an aryl group, or a sulfonyl-containing group. It is preferable that the material is at least one selected from the group consisting of:

[0032] In this specification, the term "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.

[0033] The fluoromonomer represented by the general formula (110) is Rf 111 An example of a fluoromonomer is a perfluoroalkyl group having 1 to 10 carbon atoms. The perfluoroalkyl group preferably has 1 to 5 carbon atoms.

[0034] Examples of the perfluoro organic group in the general formula (110) include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group. The fluoromonomer represented by the general formula (110) further includes a fluoromonomer represented by the general formula (110) in which Rf 111 is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, Rf 111 is the following formula:

[0035] [ka] (wherein m represents 0 or an integer of 1 to 4), Rf 111 is the following formula:

[0036] [ka] (wherein n represents an integer of 1 to 4).

[0037] As the fluoromonomer represented by the general formula (110), perfluoro(alkyl vinyl ether) [PAVE] is preferable. General formula (160): CF2=CF-ORf 161 (In the formula, Rf 161Rf represents a perfluoroalkyl group having 1 to 10 carbon atoms. 161 is preferably a perfluoroalkyl group having 1 to 5 carbon atoms.

[0038] The fluoroalkyl vinyl ether is preferably at least one selected from the group consisting of fluoromonomers represented by the general formulas (160), (130) and (140).

[0039] The fluoromonomer (PAVE) represented by general formula (160) is preferably at least one selected from the group consisting of perfluoro(methyl vinyl ether) [PMVE], perfluoro(ethyl vinyl ether) [PEVE], and perfluoro(propyl vinyl ether) [PPVE], and more preferably at least one selected from the group consisting of perfluoro(methyl vinyl ether) and perfluoro(propyl vinyl ether).

[0040] The fluoromonomer represented by general formula (130) is preferably at least one selected from the group consisting of CF2=CFOCF2OCF3, CF2=CFOCF2OCF2CF3, and CF2=CFOCF2OCF2CF2OCF3.

[0041] The fluoromonomer represented by general formula (140) is preferably at least one selected from the group consisting of CF2=CFOCF2CF(CF3)O(CF2)3F, CF2=CFO(CF2CF(CF3)O)2(CF2)3F, and CF2=CFO(CF2CF(CF3)O)2(CF2)2F.

[0042] The fluoromonomer represented by general formula (150) is preferably at least one selected from the group consisting of CF2=CFOCF2CF2SO2F, CF2=CFOCF2CF(CF3)OCF2CF2SO2F, CF2=CFOCF2CF(CF2CF2SO2F)OCF2CF2SO2F and CF2=CFOCF2CF(SO2F)2.

[0043] The fluoromonomer represented by the general formula (100) is Rf 101 is a linear fluoroalkyl group, and Rf 101 More preferred is a fluoromonomer in which Rf is a straight-chain perfluoroalkyl group. 101 The number of carbon atoms is preferably 1 to 6. Examples of the fluoromonomer represented by the general formula (100) include CH2=CFCF3, CH2=CFCF2CF3, CH2=CFCF2CF2CF3, CH2=CFCF2CF2CF2H, CH2=CFCF2CF2CF2CF3, CHF=CHCF3 (E form), CHF=CHCF3 (Z form), and the like, and among these, 2,3,3,3-tetrafluoropropylene represented by CH2=CFCF3 is preferred.

[0044] The fluoroalkyl ethylenes include: General formula (170): CH2=CH-(CF2) n -X 171 (In the formula, X 171 is H or F, and n is an integer of 3 to 10.) is preferred, and CH2=CH-C4F9 and CH2=CH-C6F 13 It is more preferable that the material is at least one selected from the group consisting of:

[0045] Examples of the fluoroalkyl allyl ether include General formula (170): CF2=CF-CF2-ORf 111 (In the formula, Rf 111 represents a perfluoro organic group.

[0046] Rf of general formula (170) 111 is Rf in general formula (110). 111 is the same as Rf 111is preferably a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoroalkoxyalkyl group having 1 to 10 carbon atoms. As the fluoroalkyl allyl ether represented by the general formula (170), at least one selected from the group consisting of CF2=CF-CF2-O-CF3, CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9 is preferable, at least one selected from the group consisting of CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9 is more preferable, and CF2=CF-CF2-O-CF2CF2CF3 is even more preferable.

[0047] As the copolymerization monomer, a monomer having a perfluorovinyl group is preferred in that it can reduce deformation of the solid composition and can lower the linear expansion coefficient, and at least one selected from the group consisting of perfluoro(alkyl vinyl ether) (PAVE), hexafluoropropylene (HFP), and perfluoroallyl ether is more preferred, and at least one selected from the group consisting of PAVE and HFP is even more preferred, with PAVE being particularly preferred in that it can suppress deformation of the solid composition during solder processing.

[0048] The perfluoro-based fluororesin contains the copolymerized monomer units in a total amount of preferably 0.1% by mass or more, more preferably 1.0% by mass or more, and even more preferably 1.1% by mass or more of the total monomer units. The total amount of the copolymerized monomer units is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less of the total monomer units. The amount of the copolymerized monomer unit is 19 Measured by F-NMR.

[0049] As the perfluoro-based fluororesin, from the viewpoint of reducing deformation of the solid composition and lowering the linear expansion coefficient, at least one selected from the group consisting of polytetrafluoroethylene (PTFE), tetrafluoroethylene (TFE) / perfluoro(alkyl vinyl) ether (PAVE) copolymer (PFA) and tetrafluoroethylene (TFE) / hexafluoropropylene (HFP) copolymer (FEP) is preferred, at least one selected from the group consisting of PFA and FEP is more preferred, and PFA is even more preferred.

[0050] When the perfluoro-based fluororesin is a PFA containing TFE units and PAVE units, it preferably contains 0.1 to 12 mass% of PAVE units based on the total polymerized units. The amount of PAVE units is more preferably 0.3 mass% or more based on the total polymerized units, even more preferably 0.7 mass% or more, even more preferably 1.0 mass% or more, particularly preferably 1.1 mass% or more, and more preferably 8.0 mass% or less, even more preferably 6.5 mass% or less, particularly preferably 6.0 mass% or less. The amount of PAVE units is as follows: 19 Measured by F-NMR.

[0051] When the perfluororesin is an FEP containing TFE units and HFP units, the mass ratio of the TFE units to the HFP units (TFE / HFP) is preferably 70-99 / 1-30 (mass%), and more preferably 85-95 / 5-15 (mass%). The FEP contains HFP units in an amount of 1% by mass or more, and preferably 1.1% by mass or more, of the total monomer units.

[0052] The FEP preferably contains perfluoro(alkyl vinyl ether) [PAVE] units in addition to TFE and HFP units. Examples of the PAVE unit contained in the FEP include the same PAVE unit constituting the PFA described above, and among these, PPVE is preferred. The above-mentioned PFA does not contain HFP units and, in that respect, differs from FEP, which contains PAVE units.

[0053] When the FEP contains TFE units, HFP units, and PAVE units, the mass ratio (TFE / HFP / PAVE) is preferably 70-99.8 / 0.1-25 / 0.1-25 (mass%). When the mass ratio is within the above range, the heat resistance and chemical resistance are excellent. The above mass ratio (TFE / HFP / PAVE) is more preferably 75 to 98 / 1.0 to 15 / 1.0 to 10 (% by mass). The FEP contains HFP units and PAVE units in a total amount of 1% by mass or more, preferably 1.1% by mass or more, of all monomer units.

[0054] In the FEP containing the TFE unit, the HFP unit, and the PAVE unit, the HFP unit preferably accounts for 25 mass % or less of the total monomer units. When the content of the HFP units is within the above range, a solid composition having excellent heat resistance can be obtained. The content of the HFP unit is more preferably 20% by mass or less, further preferably 18% by mass or less, and particularly preferably 15% by mass or less. The content of the HFP unit is preferably 0.1% by mass or more, more preferably 1% by mass or more, and particularly preferably 2% by mass or more. The HFP unit content is as follows: 19 It can be measured by F-NMR.

[0055] The content of the PAVE unit is more preferably 20% by mass or less, further preferably 10% by mass or less, and particularly preferably 3% by mass or less. The content of the PAVE unit is preferably 0.1% by mass or more, and more preferably 1% by mass or more. The content of the PAVE unit is 19 It can be measured by F-NMR.

[0056] The FEP may further contain other ethylenic monomer (α) units. The other ethylenic monomer (α) units are not particularly limited as long as they are monomer units copolymerizable with TFE, HFP, and PAVE, and examples thereof include fluorine-containing ethylenic monomers such as vinyl fluoride [VF], vinylidene fluoride [VdF], and chlorotrifluoroethylene [CTFE], and non-fluorinated ethylenic monomers such as ethylene, propylene, and alkyl vinyl ethers.

[0057] When the FEP contains TFE units, HFP units, PAVE units, and other ethylenic monomer (α) units, the mass ratio (TFE / HFP / PAVE / other ethylenic monomer (α)) is preferably 70-98 / 0.1-25 / 0.1-25 / 0.1-10 (mass%). The FEP contains monomer units other than TFE units in a total amount of 1% by mass or more, preferably 1.1% by mass or more, of all monomer units.

[0058] The perfluoro-based fluororesin is preferably the PFA and the FEP. In other words, the PFA and the FEP can be mixed and used. The mass ratio of the PFA to the FEP (PFA / FEP) is preferably 90 / 10 to 30 / 70, and more preferably 90 / 10 to 50 / 50.

[0059] The PFA and FEP can be produced by a conventional method such as emulsion polymerization or suspension polymerization by appropriately mixing monomers that are constituent units thereof and additives such as a polymerization initiator.

[0060] The above perfluoro-based fluororesin has an unstable terminal group with a carbon number of 1×10 6 The number per unit is preferably less than 700, more preferably less than 300, even more preferably less than 100, and particularly preferably less than 50. There is no particular lower limit. Within the above range, the electrical properties are better. From the viewpoint of electrical properties (particularly, dielectric tangent), the unstable terminal group is preferably at least one selected from the group consisting of -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH present at the main chain terminal of the perfluoro-based fluororesin. These may be associated with water.

[0061] The above perfluoro-based fluororesin has a -CF2H end with a carbon number of 1×10 6 Preferably, the number per particle is less than 600, more preferably less than 200, even more preferably less than 100, and particularly preferably less than 30. There is no particular lower limit. Within the above range, the electrical properties (particularly, the dielectric loss tangent) are better.

[0062] The number of the unstable terminal groups can be reduced, for example, by subjecting the perfluoro-based fluororesin to a fluorination treatment. The fluorination treatment can be carried out by a known method, for example, by contacting a non-fluorination-treated fluororesin with a fluorine-containing compound. Furthermore, the fluorine-containing compound may be a fluorine radical source that generates fluorine radicals under fluorination treatment conditions, such as F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, and halogen fluorides (e.g., IF5, ClF3).

[0063] The number of unstable terminal groups can be measured by infrared spectroscopy. Specifically, first, a film-like sample made of the perfluoro-based fluororesin and having a thickness of 0.25 to 0.3 mm is prepared. This sample is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer, and a difference spectrum is obtained from a base spectrum that is completely fluorinated and has no unstable terminal groups. From the absorption peaks of specific unstable terminal groups that appear in this difference spectrum, the number of carbon atoms in the copolymer can be determined according to the following formula (A): 6 The number of unstable terminal groups per unit, N, is calculated. N=I×K / t (A) I: Absorbance K: Correction coefficient t: film (sample) thickness (mm)

[0064] The above samples were cut out from pellets or sheets obtained by molding the perfluoro-based fluororesin.

[0065] The perfluoro-based fluororesin preferably has a melting point of 240 to 340° C. This makes it easy to carry out melt kneading. The melting point of the perfluoro-based fluororesin is more preferably 318° C. or lower, still more preferably 315° C. or lower, and is more preferably 245° C. or higher, still more preferably 250° C. or higher. The melting point of a perfluoro-based fluororesin is the temperature corresponding to the maximum value on the heat of fusion curve when the temperature is increased at a rate of 10° C. / min using a differential scanning calorimeter (DSC).

[0066] The perfluoro-based fluororesin preferably has a melt flow rate (MFR) of 0.1 to 100 g / 10 min at 372° C. This makes it easy to carry out melt kneading. The MFR is more preferably 0.5 g / 10 min or more, further preferably 1.5 g / 10 min or more, more preferably 80 g / 10 min or less, further preferably 40 g / 10 min or less. The MFR is a value obtained in accordance with ASTM D1238 using a melt indexer (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) as the mass of polymer flowing out per 10 minutes from a nozzle with an inner diameter of 2 mm and a length of 8 mm under a load of 5 kg at 372°C (g / 10 min).

[0067] The relative dielectric constant and dielectric loss tangent of the perfluoro-based fluororesin are not particularly limited, and at 25°C and a frequency of 10 GHz, the relative dielectric constant may be 4.5 or less, preferably 4.0 or less, more preferably 3.5 or less, and even more preferably 2.5 or less. The dielectric loss tangent may be 0.01 or less, preferably 0.008 or less, and more preferably 0.005 or less. The lower limits of these are not particularly limited, and for example, the relative dielectric constant may be 1.0 or more, and the dielectric loss tangent may be 0.0001 or more.

[0068] The content of the perfluoro-based fluororesin is preferably 40 to 90% by mass relative to the solid composition, more preferably 50% by mass or more, even more preferably 60% by mass or more, particularly preferably 70% by mass or more, and more preferably 85% by mass or less, more preferably 80% by mass or less.

[0069] The anisotropic filler is a particle having an anisotropic shape (having a different diameter depending on the direction), and examples thereof include carbon, mica, clay, talc, etc. Nitrides such as boron nitride and silicon nitride can also be used. Among these, talc and boron nitride are preferred, and talc is more preferred, in terms of good moldability. The anisotropic filler may be used alone or in combination of two or more kinds.

[0070] In view of good dispersibility, the anisotropic filler preferably has a Mohs hardness of 4 or less. The anisotropic filler more preferably has a Mohs hardness of 3 or less, and preferably has a Mohs hardness of 1 or more. The Mohs hardness is the old Mohs hardness scale, which is scaled from 1 to 10, and can be measured with a Mohs hardness scale.

[0071] The anisotropic filler preferably has an average particle size of 0.1 to 50 μm. The average particle size is more preferably 1 μm or more, even more preferably 3 μm or more, particularly preferably 5 μm or more, and more preferably 30 μm or less, even more preferably 20 μm or less, particularly preferably 15 μm or less. The above average particle size is a value measured by a laser diffraction / scattering method.

[0072] The anisotropic filler preferably has an aspect ratio of 1 to 5000. The lower limit of the aspect ratio is more preferably 10, and even more preferably 20. The upper limit of the aspect ratio is more preferably 1000, and even more preferably 200. The aspect ratio is a value obtained by dividing the average particle size of the anisotropic filler by the average minor axis (average value of the length in the short direction).

[0073] The shape of the anisotropic filler is not particularly limited, but examples thereof include scale-like, plate-like, needle-like, granular, spherical, columnar, cone-like, frustum-like, polyhedral, hollow, and the like.

[0074] The anisotropic filler is surface-treated with a silane coupling agent. The method of surface treatment is not particularly limited, and any commonly used method can be used. The silane coupling agents may be used alone or in combination of two or more.

[0075] From the viewpoint of enhancing affinity with the resin, the functional group of the silane coupling agent is preferably at least one selected from the group consisting of a fluorine-containing group, an amino group, a vinyl group and an epoxy group, more preferably at least one selected from the group consisting of a fluorine-containing group, an amino group and a vinyl group, and even more preferably a fluorine-containing group or an amino group.

[0076] The content of the anisotropic filler is preferably 10 to 60% by mass relative to the solid composition, more preferably 15% by mass or more, still more preferably 20% by mass or more, and more preferably 50% by mass or less, still more preferably 45% by mass or less.

[0077] The solid composition of the present disclosure may contain other components as necessary, such as additives such as fillers, crosslinking agents, antistatic agents, heat stabilizers, foaming agents, foam nucleating agents, antioxidants, surfactants, photopolymerization initiators, antiwear agents, surface modifiers, resins (excluding the above-mentioned modified fluororesins), and liquid crystal polymers.

[0078] The other components are preferably inorganic fillers other than the anisotropic fillers. By including an inorganic filler, the effect of improving the strength and the effect of reducing the linear expansion coefficient can be obtained.

[0079] Specific examples of the inorganic filler include inorganic compounds (except zinc oxide) such as zinc oxide, silica (more specifically, crystalline silica, fused silica, spherical fused silica, etc.), titanium oxide, zirconium oxide, tin oxide, silicon nitride, silicon carbide, boron nitride, calcium carbonate, calcium silicate, potassium titanate, aluminum nitride, indium oxide, alumina, antimony oxide, cerium oxide, magnesium oxide, iron oxide, and tin-doped indium oxide (ITO). In addition, minerals such as montmorillonite, talc, mica, boehmite, kaolin, smectite, zonolite, vermiculite, and sericite can be mentioned. Other inorganic fillers include carbon compounds such as carbon black, acetylene black, ketjen black, and carbon nanotubes; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; and various glasses such as glass beads, glass flakes, and glass balloons.

[0080] The inorganic filler may be of one type or of two or more types. The inorganic filler may be used as a powder as it is, or may be dispersed in a resin.

[0081] The inorganic filler is preferably one that has ultraviolet absorbing properties, which means that the absorbance of light having a wavelength of 355 nm is 0.1 or more. The light absorbance is a value measured in a reflection configuration using an ultraviolet-visible-near infrared spectrophotometer (e.g., "V-770" manufactured by JASCO Corporation) for the inorganic filler powder filled to a thickness of 100 μm.

[0082] Examples of the inorganic filler having ultraviolet absorbing properties include zinc oxide and titanium oxide, with zinc oxide being preferred.

[0083] The shape of the inorganic filler is not particularly limited, and may be the same as that of the anisotropic filler.

[0084] When the solid composition of the present disclosure contains the inorganic filler, the content of the inorganic filler is preferably 0.01 to 5.0% by mass relative to the solid composition, more preferably 0.1% by mass or more, even more preferably 0.3% by mass or more, and more preferably 4.0% by mass or less, even more preferably 3.0% by mass or less.

[0085] The inorganic filler preferably has an average particle size of 0.01 to 20 μm. When the average particle size is within the above range, aggregation is reduced and good surface roughness can be obtained. The lower limit of the average particle size is more preferably 0.02 μm, and even more preferably 0.03 μm. The upper limit of the average particle size is more preferably 5 μm, and even more preferably 2 μm. The above average particle size is a value measured by a laser diffraction / scattering method.

[0086] The inorganic filler may be surface-treated, for example, with a silicone compound. By treating the surface with the silicone compound, the dielectric constant of the inorganic filler can be reduced. The silicone compound is not particularly limited, and any conventionally known silicone compound can be used. For example, it is preferable to use at least one selected from the group consisting of a silane coupling agent and an organosilazane. The amount of the silicone compound used for surface treatment is the amount of the surface treatment agent reacting with the inorganic filler surface per unit surface area (nm 2 It is preferable that the number of particles per 100 particles is 0.1 to 10, and more preferably 0.3 to 7.

[0087] In the solid composition of the present disclosure, when imaged by a laser microscope, voids having a width of 30 μm or more are found to be 1 mm 2 It is preferable that the number of voids is 30 or less per area. The number of voids is more preferably 25 or less, further preferably 20 or less, and may be 0. Within the above range, the moldability (particularly, sheet moldability and strand take-up stability) will be better. The image analysis by the above-mentioned laser microscope observation was carried out on a cross section of a pellet made from the solid composition of the present disclosure.

[0088] The solid composition of the present disclosure has a linear expansion coefficient at 20° C. to 200° C. of preferably 160 ppm / ° C. or less, more preferably 120 ppm / ° C. or less. The lower limit is not particularly limited, but may be, for example, 100 ppm / ° C. The linear expansion coefficient of the solid composition of the present disclosure at 20° C. to 200° C. is preferably reduced by 25% or more, more preferably 40% or more, and even more preferably 50% or more, relative to the linear expansion coefficient of the perfluoro-based fluororesin at 20° C. to 200° C. The upper limit is not particularly limited, and may be, for example, 60%.

[0089] The solid composition of the present disclosure has a relative dielectric constant at 25° C. and 10 GHz of preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.5 or less. There is no particular lower limit, but it may be, for example, 1.0. If it is within the above range, it can be suitably used for circuit boards.

[0090] The solid composition of the present disclosure has a dielectric loss tangent at 25° C. and 10 GHz of preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.0015 or less. The lower limit is not particularly limited, but may be, for example, 0.0001. If it is within the above range, it can be suitably used for circuit boards.

[0091] The shape of the solid composition of the present disclosure is not particularly limited, and examples thereof include pellets, films, sheets, etc. When used for circuit boards, films and sheets are preferred. Pellets can be used as molding materials.

[0092] The solid composition of the present disclosure can be suitably produced by a production method in which the perfluoro-based fluororesin and the anisotropic filler are melt-kneaded to obtain the solid composition. The present disclosure also provides the production method. The solid composition of the present disclosure may be produced by a method other than the above-mentioned production method, for example, injection molding, blow molding, inflation molding, vacuum / pressure molding, etc. Also, if it is in a state of being dispersed or dissolved in a solvent, it may be produced by a paste extrusion method, a casting method, etc.

[0093] The apparatus used for the melt kneading is not particularly limited, and a twin-screw extruder, a single-screw extruder, a multi-screw extruder, a tandem extruder, or the like can be used.

[0094] The melt kneading time is preferably 1 to 1800 seconds, more preferably 60 to 1200 seconds. If the time is too long, the fluororesin may deteriorate, and if the time is too short, the zinc oxide may not be sufficiently dispersed. The melt-kneading temperature may be equal to or higher than the melting points of the perfluoro fluororesin and the anisotropic filler, and is preferably 240 to 450°C, and more preferably 260 to 400°C.

[0095] The present inventors have found that the solid composition of the present disclosure, which contains a perfluoro-based fluororesin and an anisotropic filler, has a low linear expansion coefficient, excellent moldability, and good dispersibility. These properties make it suitable for use as a circuit board material. That is, the solid composition of the present disclosure is suitably used as an insulating material (particularly, a low dielectric material) and a thermally conductive material for circuit boards. In this specification, the term "low dielectric material" refers to a material having a dielectric constant of 5.0 or less at 25° C. and 10 GHz and a dielectric loss tangent of 0.003 or less at 25° C. and 10 GHz, more preferably a material having a dielectric constant of 4.0 or less at 25° C. and 10 GHz and a dielectric loss tangent of 0.002 or less at 25° C. and 10 GHz, and even more preferably a material having a dielectric constant of 3.5 or less at 25° C. and 10 GHz and a dielectric loss tangent of 0.0012 or less at 25° C. and 10 GHz.

[0096] The circuit board of the present disclosure comprises the solid composition of the present disclosure described above and a conductive layer.

[0097] The conductive layer is preferably made of a metal. Examples of the metal include copper, stainless steel, aluminum, iron, silver, gold, ruthenium, etc. Furthermore, alloys of these metals can also be used. Among these, copper is preferred.

[0098] As the copper, rolled copper, electrolytic copper, etc. can be used.

[0099] The metal preferably has a surface roughness Rz of 2.0 μm or less on the surface facing the solid composition, which results in good transmission loss when the solid composition and the metal are joined together. The surface roughness Rz is more preferably 1.8 μm or less, and further preferably 1.5 μm or less, and is more preferably 0.3 μm or more, and further preferably 0.5 μm or more. The surface roughness Rz is a value (maximum height roughness) calculated by the method of JIS C 6515-1998.

[0100] The conductive layer may have a thickness of, for example, 2 to 200 μm, and preferably has a thickness of 5 to 50 μm.

[0101] The conductive layer may be provided on only one side or on both sides of the layer containing the solid composition of the present disclosure.

[0102] The film thickness of the layer containing the solid composition of the present disclosure may be, for example, 1 μm to 1 mm, and is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more, and is preferably 800 μm or less, and more preferably 600 μm or less. When forming a film from the dispersion described in Patent Document 2, it is usually difficult to achieve a film thickness of 50 μm or more. However, when forming a film from the solid composition of the present disclosure, it is easy to achieve a film thickness of 50 μm or more.

[0103] The circuit board of the present disclosure may be one in which a resin other than the perfluoro-based fluororesin is further laminated on the solid composition of the present disclosure and the conductive layer.

[0104] As the resin other than the perfluoro-based fluororesin, a thermosetting resin can be suitably used. The thermosetting resin is preferably at least one selected from the group consisting of polyimide, modified polyimide, epoxy resin, and thermosetting modified polyphenylene ether, more preferably epoxy resin, modified polyimide, and thermosetting modified polyphenylene ether, and even more preferably epoxy resin and thermosetting modified polyphenylene ether.

[0105] The resin other than the perfluoro-based fluororesin may be a resin other than a thermosetting resin. The resin other than the thermosetting resin is preferably at least one selected from the group consisting of liquid crystal polymers, polyphenylene ethers, thermoplastic modified polyphenylene ethers, cycloolefin polymers, cycloolefin copolymers, polystyrene, and syndiotactic polystyrene.

[0106] The thickness of the resin other than the perfluoro-based fluororesin is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 2000 μm or less, more preferably 1500 μm or less. The resin other than the perfluoro-based fluororesin is preferably in the form of a sheet having a substantially uniform thickness. However, if the perfluoro-based fluororesin has portions with different thicknesses, the thickness is determined by measuring the thicknesses at 10 points that are equally spaced apart in the longitudinal direction of the perfluoro-based fluororesin, and averaging these thicknesses.

[0107] The thickness of the circuit board of the present disclosure is preferably 20 μm or more, more preferably 30 μm or more, and is preferably 5000 μm or less, more preferably 3000 μm or less. The circuit board of the present disclosure is preferably in the form of a sheet having a substantially uniform thickness. However, if the board has portions of differing thickness, the board is divided into 10 equally spaced portions along the length, and the thicknesses are measured at these portions and the average is calculated.

[0108] The circuit board of the present disclosure is suitable for use as a printed circuit board, a laminated circuit board (multilayer board), or a high-frequency board.

[0109] The high-frequency circuit board is a circuit board that can operate in a high-frequency band. The high-frequency band may be a band of 1 GHz or more, preferably a band of 3 GHz or more, and more preferably a band of 5 GHz or more. There is no particular upper limit, but it may be a band of 100 GHz or less.

[0110] The circuit board of the present disclosure is preferably a sheet, and the thickness of the circuit board of the present disclosure is preferably 10 to 3500 μm, and more preferably 20 to 3000 μm.

[0111] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES

[0112] The present disclosure will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.

[0113] The materials used in the examples are as follows: (Perfluoro fluororesin) PFA1 (TFE / PAVE (mass%): 97.9 / 2.1, fluorine-containing monomer content: 100 mol%, melting point: 304°C, MFR: 29 g / 10 min, relative dielectric constant (25°C, 10 GHz): 2.1, dielectric loss tangent (25°C, 10 GHz): 0.0003) PFA2 (TFE / PAVE (mass%): 97.9 / 2.1, Fluorine-containing monomer content: 100 mol%, Melting point: 303°C, MFR: 29 g / 10 min, Relative dielectric constant (25°C, 10 GHz): 2.0, Dielectric loss tangent (25°C, 10 GHz): 0.001) FEP (TFE / HFP / PAVE (mass%): 87.5 / 11.5 / 1.0, Fluorine-containing monomer content: 100 mol%, Melting point: 255°C, MFR: 24 g / 10 min, Relative dielectric constant (25°C, 10 GHz): 2.1, Dielectric loss tangent (25°C, 10 GHz): 0.0008) (Filler) Talc 1 (average particle size: 7 μm, aspect ratio: 45 to 50, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with fluorine silane (fluorine-containing silane coupling agent)) Talc 2 (average particle size: 7 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with fluorine silane (fluorine-containing silane coupling agent)) Talc 3 (average particle size: 7 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with aminosilane (amino group-containing silane coupling agent)) Talc 4 (average particle size: 7 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with vinyl silane (vinyl group-containing silane coupling agent)) Talc 5 (average particle size: 5 μm, aspect ratio: 30, Mohs hardness (old Mohs hardness): 1, surface treatment: treated with fluorine silane (fluorine-containing silane coupling agent)) Talc 6 (average particle size: 7 μm, aspect ratio: 45 to 50, Mohs hardness (old Mohs hardness): 1, surface treatment: none) Zinc oxide (average particle size: 0.035 μm, surface treatment: none, UV absorption: yes (absorbance of 355 nm light is 0.1 or more))

[0114] The number of unstable terminal groups in the perfluororesin is shown in the following table. The measurement was performed using film-like samples cut out from pellets and sheets made of perfluororesin prepared in the same manner as in the Examples described later.

[0115] [Table 1]

[0116] Examples and Comparative Examples <Pelletizing method other than Example 2> The perfluoro-based fluororesin and the filler were melt-kneaded in the ratio (mass%) shown in the table below using a twin-screw extruder at a temperature of 360°C, and then cooled in a water bath. The resulting solid composition (strands) were cut and pelletized. <Pelletizing method of Example 2> The perfluoro-based fluororesin and the filler were melt-kneaded (time: 600 seconds, temperature: 350°C) in the ratio (mass%) shown in the table below using a Labo Plastomill Mixer, and then naturally cooled to obtain a solid composition. The obtained solid composition was crushed and pelletized.

[0117] The pellets obtained above were press molded at 350° C. to obtain a sheet having a thickness of 100 μm. In Comparative Example 4, the flowability was low and molding into a sheet was not possible. In Example 10, the sheet obtained in Example 1 was laminated with Cu foil (electrolytic copper, thickness: 18 μm, surface roughness Rz of the side to be joined to the sheet: 1.4 μm) and pressed for 5 minutes at a heating temperature of 320° C. and a pressure of 15 kN to obtain a bonded body in which the sheet was bonded to one side of the copper foil.

[0118] (Strand take-up stability) The strand take-up stability during the formation of the above pellets was evaluated according to the following criteria. ◎: Stable 〇: Sometimes cuts off ×: Strand cannot be pulled

[0119] (Sheet formability) The moldability when forming the above-mentioned sheet was evaluated according to the following criteria. ◎: No bubbles ○: No bubbles in some areas

[0120] (Number of voids (image analysis of laser microscope observation)) 1mm in the following way: 2 The number of voids with a width of 30 μm or more per area was evaluated. The pellet was cut with a razor and the cross section was observed under a laser microscope. The number of voids was counted based on the area of ​​0.069 mm in an image measured at 50x magnification. 2 Count the number of voids per area (0.23 mm long, 0.3 mm wide) and calculate the number of voids per 1 mm 2 The numbers were converted to numbers per area.

[0121] (Coefficient of linear expansion (CTE) reduction rate) The linear expansion coefficient (linear expansion coefficient) of the above sheet was determined by TMA measurement in the following mode using a TMA-7100 (manufactured by Hitachi High-Tech Science Corporation). The same measurements were then carried out on the above perfluoro-based fluororesin, and the reduction rate relative to the linear expansion coefficient of the resin alone (linear expansion coefficient before the addition of the filler) was calculated using the following formula and evaluated according to the following criteria. [Tension mode measurement] A sample piece of extruded film 25 μm thick cut to a length of 20 mm and a width of 4 mm was used, and the linear expansion coefficient was calculated from the displacement of the sample at 20 to 200°C at a heating rate of 2°C / min while pulling with a load of 49 mN. [Calculation formula for reduction rate] (Decrease rate / %)=(B1-B2)×100 / B1 B1: Linear expansion coefficient before adding filler / ppm / ℃ B2: Linear expansion coefficient after adding filler / ppm / ℃ [standard] ◎: 50% or more ○: Less than 50%, 25% or more ×: Less than 25%

[0122] (Dielectric constant (Dk), dielectric tangent (Df)) The Dk and Df of the above-mentioned sheet were measured at 25° C. and 10 GHz using a split cylinder type dielectric constant / dielectric loss tangent measuring device (manufactured by EM Lab), and evaluated according to the following criteria. [Standards for relative dielectric constant] ◎: Less than 5 [Standard for dielectric tangent] ◎: Less than 0.0012 ○: 0.0012 or more and less than 0.003

[0123] (Peel test) A peel test (90 degree peel test) was carried out according to the method of JIS C 6481-1996. Approximately 1 cm of the resin at the end of the bonded body of Example 10 obtained above was peeled off, and the bonded body was clamped in the chuck of a tester, and the peel strength (unit: N / cm) was measured at a pulling speed (moving speed) of 50 mm / min, and evaluated according to the following criteria. ◎:10N / cm or more

[0124] [Table 2]

Claims

1. The present invention contains a perfluoro-based fluororesin and an anisotropic filler that has been surface-treated with a silane coupling agent, The perfluoro-based fluororesin has a melting point of 240 to 340° C. The anisotropic filler is talc (excluding talc having a multi-layer structure), The silane coupling agent has at least one group selected from the group consisting of a fluorine-containing group, an amino group, a vinyl group, and an epoxy group, The content of the perfluoro-based fluororesin is 40 to 90% by mass, A solid composition which is a film or sheet having a thickness of 50 μm or more.

2. 2. The solid composition according to claim 1, wherein the anisotropic filler has a Mohs hardness of 4 or less.

3. The perfluoro-based fluororesin has an unstable terminal group having a carbon number of 1×10 6 less than 50 per piece, The unstable terminal group is —CF 2 H, -COF, -COOH, -COOCH 3 , -CONH 2 and -CH 2 3. The solid composition according to claim 1, wherein the at least one member is selected from the group consisting of OH.

4. The solid composition according to claim 1 or 2, wherein the perfluoro-based fluororesin is at least one selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer, and tetrafluoroethylene / hexafluoropropylene copolymer.

5. In image analysis using a laser microscope, voids with a width of 30 μm or more were found to be 1 mm 2 3. The solid composition according to claim 1, wherein the number of particles per unit area is 30 or less.

6. 3. The solid composition according to claim 1, wherein the linear expansion coefficient of the solid composition at 20°C to 200°C is reduced by 25% or more relative to the linear expansion coefficient of the perfluoro-based fluororesin at 20°C to 200°C.

7. 3. The solid composition according to claim 1, which has a dielectric loss tangent at 25° C. and 10 GHz of 0.003 or less.

8. 3. The solid composition according to claim 1 or 2, which is an insulating material for a circuit board.

9. 9. The solid composition of claim 8, wherein the insulating material of the circuit board is a low dielectric material.

10. A circuit board comprising the solid composition according to claim 1 or 2 and a conductive layer.

11. 11. The circuit board of claim 10, wherein the conductive layer is a metal.

12. The circuit board according to claim 11 , wherein the metal has a surface roughness Rz of 2.0 μm or less on the surface facing the solid composition.

13. 12. The circuit board of claim 11, wherein the metal is copper.

14. The circuit board according to claim 10, which is a printed circuit board, a multilayer circuit board or a high-frequency board.

15. 3. The method for producing a solid composition according to claim 1, comprising melt-kneading the perfluoro-based fluororesin and the anisotropic filler to obtain the solid composition.

Citation Information

Patent Citations

  • Process for preparing filler-containing polytetrafluoroethylene powder for molding

    JP2002201287A

  • Composition, and method for producing foam molded material and electric wire

    JP2014224228A

  • Resin composition for dielectric and high-frequency dielectric device

    JP2015040296A

  • Gasket around engine and manufacturing method thereof

    JP2018080754A

  • Fluororesin film for agricultural use

    WO2010005085A1